Aluminum alloy sheet for can top

The aluminum alloy composition with controlled Si, Fe, Cu, Mn, and Mg content addresses the challenge of achieving high strength and toughness in can lids, facilitating the use of recycled materials and reducing CO2 emissions.

JP2024153464AActive Publication Date: 2024-10-29UACJ CORP
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2023067373
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Conventional aluminum alloy plates for can lids face challenges in achieving both high strength and toughness, particularly for positive pressure cans, while also requiring a high recycling rate to reduce CO2 emissions.

Method used

An aluminum alloy composition with specific ranges of Si, Fe, Cu, Mn, and Mg contents, along with optional Ti and Zn, is used to enhance solidus temperature, allowing for the incorporation of 3104 aluminum alloy scrap, thereby improving strength and toughness without the need for excessive new metal use.

Benefits of technology

The alloy achieves high strength and toughness, enabling the use of recycled materials, reducing CO2 emissions, and ensuring high formability for positive pressure can lids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153464000001
    Figure 2024153464000001
  • Figure 2024153464000002
    Figure 2024153464000002
Patent Text Reader

Abstract

To provide an aluminum alloy sheet for a can top having both high strength and high toughness while blending a scrap raw material derived from a can material.SOLUTION: An aluminum alloy sheet for a can top has a composition comprising 0.20 mass% or more and 0.47 mass% or less of Si, 0.30 mass% or more and 0.70 mass% or less of Fe, 0.11 mass% or more and 0.40 mass% or less of Cu, 0.70 mass% or more and 1.20 mass% or less of Mn, 1.1 mass% or more and 3.7 mass% or less of Mg, and the balance of Al and inevitable impurities, where a solidus line temperature is higher than a solid-solution temperature of Mg2Si.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an aluminum alloy sheet for can ends. [Background technology]

[0002] In recent years, with the rise in environmental awareness, there is a demand for aluminum alloy sheets with low CO2 emissions during the manufacturing process. In the aluminum manufacturing process, the compounding of new aluminum ingots in the casting process indirectly contributes greatly to CO2 emissions.

[0003] The production of primary aluminum ingots uses a large amount of electricity during the refining process, which leads to large amounts of CO2 emissions. Therefore, reducing the amount of primary aluminum ingots mixed and increasing the horizontal recycling rate will lead to a reduction in CO2 emissions in the production of aluminum alloy sheets.

[0004] It is generally said that CO2 emissions from remelting and casting aluminum scrap can be reduced to about one-thirtieth of that from producing new aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used around the world is extremely large, and further improving the horizontal recycling rate of these sheets has great significance in reducing the environmental impact.

[0005] Among these, can ends made of 5182 aluminum alloy (AA5182 alloy) have lower upper limits for the composition standards of Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to mix scrap derived from can materials that contain 3104 aluminum alloy.

[0006] For example, if can scrap (UBC: Used Beverage Can) generated in the city is mixed as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will easily exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.

[0007] Therefore, compared to aluminum alloy sheets for can bodies, aluminum alloy sheets for can ends use more virgin metal and have the composition adjusted to 5182 aluminum alloy, resulting in a low recycling rate. Therefore, by changing can ends to alloys whose composition is easily mixed with 3104 aluminum alloy, the usage rate of virgin metal for can ends can be significantly reduced.

[0008] Patent Documents 1 to 5 disclose aluminum alloy sheets for can ends that have compositions relatively close to those of 3104 aluminum alloy, which has excellent recyclability. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2001-73106 A [Patent Document 2] Japanese Patent Application Publication No. 9-070925 [Patent Document 3] Japanese Patent Application Publication No. 11-269594 [Patent Document 4] JP 2000-160273 A [Patent Document 5] JP 2016-160511 A Summary of the Invention [Problem to be solved by the invention]

[0010] The challenge in making the alloy for can lids closer to the 3104 aluminum alloy is that it reduces the pressure resistance of the can lids and the toughness of the material. The pressure resistance of a can lid is the internal pressure value when the can lid is inverted against the pressure inside the can, and is the resistance value when the internal pressure of the can increases unexpectedly due to a change in the external environment.

[0011] In particular, positive pressure cans for beer and carbonated beverages require high pressure resistance. Generally, the higher the material strength and the thicker the plate, the higher the pressure resistance. For this reason, high-strength 5182 aluminum alloy with a high magnesium content is used for the lids of positive pressure cans.

[0012] In contrast, if the conventional 3104 aluminum alloy is used for can lids, the pressure resistance is significantly reduced, and there is a high possibility that the lid will invert and leak contents if the internal pressure of the can suddenly increases. Also, if the plate thickness is increased to increase the pressure resistance, this will lead to an increase in the weight and cost of the lid.

[0013] Furthermore, the toughness of the material affects the formability and openability of the lid. If the material has low toughness, forming cracks may occur, especially in the rivet and countersink parts of the lid. Also, if the internal pressure of the can suddenly increases, cracks may occur in the score area, increasing the risk of the contents of the can leaking. In particular, these cracks occur along the rolling direction. Therefore, toughness against tensile stress and bending stress in the direction perpendicular to the rolling direction is required.

[0014] However, aluminum alloy sheets for can ends that have a composition relatively close to that of the conventional 3104 aluminum alloy do not satisfy either or both of the above two issues, namely, material strength (i.e., pressure resistance of the end) and toughness (i.e., formability and openability).

[0015] An object of one aspect of the present disclosure is to provide an aluminum alloy sheet for can ends that can achieve both high strength and high toughness while incorporating scrap raw material derived from can stock. [Means for solving the problem]

[0016] One embodiment of the present disclosure is an aluminum alloy sheet for can ends, having a silicon (Si) content of 0.20% by mass or more and 0.47% by mass or less, an iron (Fe) content of 0.30% by mass or more and 0.70% by mass or less, a copper (Cu) content of 0.11% by mass or more and 0.40% by mass or less, a manganese (Mn) content of 0.70% by mass or more and 1.20% by mass or less, a magnesium (Mg) content of 1.1% by mass or more and 3.7% by mass or less, with the balance being aluminum (Al) and unavoidable impurities, and having a solidus temperature higher than the solution temperature of MgSi.

[0017] According to this configuration, the solidus temperature of the aluminum alloy can be made higher than the solution temperature of the Mg2Si crystallized matter, and therefore, by subjecting the aluminum alloy ingot to a soaking treatment within this temperature range, it is expected that the Mg2Si crystallized matter, which causes cracks and unexpected openings during molding, can be suppressed.

[0018] As a result, it is possible to obtain both high strength and high toughness in an aluminum alloy sheet while blending scrap raw materials derived from can materials. In other words, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, thereby reducing the usage rate of new ingots and reducing CO2 emissions. Furthermore, it is possible to obtain an aluminum alloy sheet for can ends that has high formability and can be used for positive pressure can ends that require high pressure resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments to which the present disclosure is applied will be described. [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for can ends (hereinafter also simply referred to as "alloy sheet") of the present disclosure contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn) and magnesium (Mg).

[0020] The lower limit of the Si content is 0.20 mass%. The average Si content standard of 3104 aluminum alloy specified in JIS-H-4000:2014 is 0.30 mass%, and the average Si content standard of 5182 aluminum alloy specified in JIS-H-4000:2014 is 0.10 mass%. Therefore, by making the Si content 0.20 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0021] The upper limit of the Si content is 0.47% by mass, and preferably 0.39% by mass. If the Si content exceeds 0.47% by mass, the difference between the solution temperature of Mg2Si and the solidus temperature of the Al matrix becomes small, making it difficult to dissolve the Mg2Si present in the ingot in the homogenization process. In addition, coarse Mg2Si is newly precipitated during hot rolling. As a result, the strength and toughness of the alloy are reduced.

[0022] In addition, by setting the Si content to 0.39 mass% or less, Mg2Si can be easily dissolved in the homogenization process. Furthermore, the precipitation of coarse Mg2Si during hot rolling is suppressed, and good strength and toughness can be obtained without performing a heat treatment process after hot rolling.

[0023] The lower limit of the Fe content is 0.30% by mass. The average Fe content standard of 3104 aluminum alloy is 0.40% by mass, and the average Fe content standard of 5182 aluminum alloy is 0.18% by mass. Therefore, by making the Fe content 0.30% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0024] The upper limit of the Fe content is 0.70 mass%, preferably 0.59 mass%, and more preferably 0.51 mass%. If the Fe content exceeds 0.70 mass%, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., giant compounds) increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases. In addition, if the Fe content is 0.51 mass% or less, the crystallization of the above-mentioned coarse intermetallic compounds is suppressed, and strength and toughness can be compensated for by adding a large amount of Mg.

[0025] The lower limit of the Cu content is 0.11 mass%, preferably 0.17 mass%, and more preferably 0.20 mass%. If the Cu content is less than 0.11 mass%, Cu, which increases the strength by solid solution or precipitation, is insufficient, and the strength of the alloy plate is reduced. In addition, the average value of the Cu content standard of the 3104 aluminum alloy is 0.15 mass%, and the average value of the Cu content standard of the 5182 aluminum alloy is 0.075 mass%. Therefore, by making the Cu content 0.11 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0026] The upper limit of the Cu content is 0.40 mass%, and preferably 0.25 mass%. If the Cu content exceeds 4.0 mass%, the amount of coarse precipitates increases, and the toughness of the alloy plate decreases. In addition, by making the Cu content 0.25 mass% or less, the strength can be increased without significantly impairing the toughness.

[0027] The lower limit of the Mn content is 0.70% by mass. If the Mn content is less than 0.70% by mass, the Mn that increases the strength by solid solution or precipitation is insufficient, and the average strength of the alloy plate is reduced. In addition, the average value of the Mn content standard of the 3104 aluminum alloy is 1.1% by mass, and the average value of the Mn content standard of the 5182 aluminum alloy is 0.35% by mass. Therefore, by setting the Mn content to 0.70% by mass or more, it is possible to mix more 3104 aluminum alloy scrap than the conventional 5182 aluminum alloy.

[0028] The upper limit of the Mn content is 1.20 mass%, preferably 0.98 mass%, and more preferably 0.92 mass%. If the Mn content exceeds 1.20 mass%, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases.

[0029] The lower limit of the Mg content is 1.1 mass%. If the Mg content is less than 1.1 mass%, the Mg that increases the strength by solid solution is insufficient, and the average strength of the alloy sheet decreases. Note that the strength of the alloy sheet is significantly increased by precipitating Mg during the processing of hot rolling and cold rolling after the solution treatment.

[0030] The upper limit of the Mg content is 3.7% by mass, preferably 3.3% by mass, more preferably 3.1% by mass, and even more preferably 2.9% by mass. If the Mg content exceeds 3.7% by mass, the solidus temperature of the Al matrix decreases and the dissolution temperature of Mg2Si increases, making it difficult to dissolve Mg2Si present in the ingot in the homogenization process. In addition, the solidus temperature of the Al matrix decreases, increasing the amount of coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds. This impairs strength and toughness.

[0031] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. The ingot structure of the alloy plate is refined by including Ti. On the other hand, if the Ti content is too high, it causes inclusions and reduces toughness. The alloy plate may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass%. Furthermore, the alloy plate may contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%.

[0032] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the above-mentioned ranges, with the balance being Al and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%.

[0033] <Calculation of phase diagrams using computer software> In the alloy plate of the present disclosure, in order to increase the toughness of the material, it is preferable to re-dissolve Mg2Si particles, which become the initiation points and propagation paths of cracks and affect the decrease in toughness, in a homogenization heat treatment process of the ingot.

[0034] In order to redissolve Mg2Si while avoiding local melting of the Al matrix, the solidus temperature must be higher than the solution temperature of Mg2Si. Furthermore, it is preferable that the temperature difference between the solidus temperature and the solution temperature of Mg2Si is 30°C or more. By having the solution temperature of Mg2Si lower than the solidus temperature, coarse crystals are not generated during casting, and performance degradation due to coarse crystals can be avoided.

[0035] Furthermore, in materials in which the crystallization temperature of Al6(Mn,Fe) is higher than the solidification start temperature of Al, Al6(Mn,Fe) is generated as coarse crystals during casting, which can lead to molding defects such as pinholes. Therefore, it is preferable that the solidification start temperature of Al is higher than the crystallization temperature of the primary crystal (i.e., Al6(Mn,Fe)), and it is even more preferable that the temperature difference obtained by subtracting the crystallization temperature of the primary crystal from the solidification start temperature of Al is 1°C or more.

[0036] When Al6(Mn,Fe) crystallizes, it tends to grow into giant crystals when the surrounding area is liquid Al. Such giant crystals can be the starting point for crack propagation in the alloy, leading to a decrease in toughness. If the solidification temperature of Al is higher than the crystallization temperature of Al6(Mn,Fe), the surrounding Al has already started to solidify when Al6(Mn,Fe) crystallizes, suppressing the generation of giant crystals and resulting in an aluminum alloy sheet for can ends with higher toughness.

[0037] The solubilization temperature of Mg2Si here refers to the highest temperature at which Mg2Si can exist in the equilibrium diagram, and is the lowest temperature at which the liquid phase can exist. The solidification start temperature of Al refers to the highest temperature at which solid Al can exist in the equilibrium diagram, and the crystallization temperature of the primary crystal is the highest temperature at which Al6(Mn,Fe) can exist.

[0038] The solution temperature of Mg2Si, the solidus temperature of the aluminum alloy, the solidification start temperature of Al, and the crystallization temperature of the primary crystal can be obtained from the equilibrium phase diagram of the aluminum alloy calculated using thermodynamic calculation software.

[0039] The solution temperature of Mg2Si, the solidus temperature of an aluminum alloy, the solidification start temperature of Al, and the crystallization temperature of the primary crystal are uniquely determined by the composition of the aluminum alloy. One method for determining these boundary temperatures from the alloy composition is to calculate the thermodynamic quantities required for each calculation using the CALPHAD method.

[0040] Such thermodynamic calculations for multi-component alloys can be performed using commercially available system software (e.g., "JMatPro" developed by Sente Software) that combines the thermodynamic database, interface, and phase diagram creation functions required for the calculations.

[0041] <Method of manufacturing aluminum alloy sheet> The aluminum alloy plate of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy plate of the present disclosure is subjected to semi-continuous casting (i.e., DC casting) according to a conventional method to produce an ingot.

[0042] Next, the four faces of the ingot, excluding the front and rear ends, are chamfered. After that, the ingot is placed in a soaking furnace and subjected to homogenization treatment. The temperature in the homogenization treatment is preferably, for example, 470°C or higher and 620°C or lower. The time for the homogenization treatment is preferably, for example, 1 hour or higher and 20 hours or lower.

[0043] When the homogenization temperature is 400°C or higher, segregation of the ingot structure is easily eliminated. Furthermore, when the homogenization temperature is 450°C or higher, Mg2Si particles are redissolved, and the strength and toughness of the alloy plate can be improved. Furthermore, when the homogenization temperature is 490°C or higher, preferably 550°C or higher, and more preferably the solution temperature of Mg2Si or higher, the redissolution of Mg2Si particles is promoted, and the strength and toughness of the alloy plate can be further improved. On the other hand, when the homogenization temperature is 620°C or lower, and more preferably the solidus temperature or lower, local melting of the aluminum alloy is difficult to occur.

[0044] When the homogenization treatment time is 1 hour or more, the temperature of the entire ingot becomes uniform, segregation of the ingot structure is easily eliminated, and Mg2Si particles are easily redissolved. The longer the homogenization treatment time, the more the Mg2Si particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.

[0045] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot rolled coil.

[0046] If the total reduction rate of the finish rolling is high, the recrystallized structure will be formed after coiling, and the concentration of isotropic cube orientation can be increased. If the coiling temperature of the finish rolling is high, the recrystallized structure will be formed after coiling, and the concentration of cube orientation can be increased. Increasing the concentration of cube orientation in aluminum alloy plate improves toughness.

[0047] Following hot rolling, the plate material is cold rolled. In cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. Cold rolling may be either single rolling or tandem rolling. In single cold rolling, rolling is preferably performed in multiple passes, such as two or more passes.

[0048] By setting the finishing temperature of cold rolling in the intermediate passes other than the final pass at 120°C or higher, Si, Cu, Mg, etc. are finely precipitated and age hardened, so that the strength of the alloy sheet can be increased. Furthermore, by setting the finishing temperature at 130°C or higher, the strength of the alloy sheet can be further increased.

[0049] The cold rolling reduction (i.e., the total reduction) is preferably 80% or more. When the cold rolling reduction is 80% or more, the strength of the alloy sheet can be increased. On the other hand, the cold rolling reduction is preferably 92% or less. By setting the cold rolling reduction to 92% or less, the anisotropy of the crystal grain structure is reduced, and the toughness against tensile stress and bending stress in the direction perpendicular to the rolling direction is improved.

[0050] The cold rolling reduction ratio R (%) is calculated by the following formula (1) using the plate thickness t0 (mm) of the hot rolled plate after hot finish rolling and the plate thickness t1 (mm) of the product after cold rolling. R = (t0-t1) / t0 × 100 (1)

[0051] The product plate thickness can be appropriately selected so as to obtain a desired pressure resistance. Although the pressure resistance improves as the plate thickness increases, the aluminum alloy plate of the present disclosure can suppress an increase in plate thickness required to maintain a high pressure resistance.

[0052] In addition, as long as the effects of the aluminum alloy sheet of the present disclosure are exhibited, in the above-mentioned method for producing an aluminum alloy sheet, annealing may be performed, for example, before or after cold rolling or between passes.

[0053] After the coils have been cold-rolled to the product thickness, they are pre-coated in a painting line, etc. The surface of the cold-rolled coils is degreased, cleaned, and chemically treated, and then painted, after which the coils are painted and baked.

[0054] Chemical solutions such as chromate-based and zirconium-based are used in chemical conversion treatment. Epoxy-based and polyester-based paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the material recovery is suppressed, and the higher the strength of the alloy plate can be maintained.

[0055] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained. (1a) The solidus temperature of the aluminum alloy can be made higher than the solution temperature of Mg2Si crystallization. Therefore, by subjecting the aluminum alloy ingot to a soaking treatment within this temperature range, it is expected that the formation of Mg2Si crystallization, which causes cracks and unexpected openings during molding, can be suppressed.

[0056] As a result, it is possible to obtain both high strength and high toughness in an aluminum alloy sheet while blending scrap raw materials derived from can materials. In other words, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, thereby reducing the usage rate of new ingots and reducing CO2 emissions. Furthermore, it is possible to obtain an aluminum alloy sheet for can ends that has high formability and can be used for positive pressure can ends that require high pressure resistance.

[0057] 2. Other embodiments Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take various forms.

[0058] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments of a member constituted by this aluminum alloy sheet, a manufacturing method of this aluminum alloy sheet, and the like.

[0059] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. In addition, a part of the configuration of the above embodiments may be omitted. In addition, at least a part of the configuration of the above embodiments may be added to or substituted for the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified from the wording of the claims are embodiments of the present disclosure.

[0060] 3. Working Examples The following describes the tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.

[0061] <Calculation of equilibrium phase diagram> As examples and comparative examples, the equilibrium diagrams of aluminum alloys S1-S14 shown in Table 1 were calculated using "JMatPro" by the calculation method described in the embodiment. The results are shown in Table 1.

[0062] [Table 1]

[0063] <Evaluation of aluminum alloy sheets> (Various temperatures) The solidus temperatures of S2-S9 and S11-S14 are higher than the Mg2Si solid solution temperature, so these alloys can be soaked at temperatures at which Mg2Si can be dissolved.

[0064] In S1, the amount of Si is relatively large, so the Mg2Si dissolution temperature is higher than the solidus temperature. As a result, when the temperature rises, Al melts locally before Mg2Si dissolves, making it difficult to soak S1 to dissolve Mg2Si.

[0065] On the other hand, in S2, the amount of Si is less than that in S1, so there is a temperature range where the liquid phase does not appear even at the temperature where Mg2Si dissolves. In addition, in S3, the amount of Si is even less than that in S2, so the temperature difference between the solidus temperature and the Mg2Si dissolution temperature is large, at 30°C or more. As a result, in S3, there is a temperature range where soaking is possible even taking into account manufacturing variations.

[0066] In S4, the Fe content is relatively high, so the crystallization temperature of Al6(Mn,Fe) is higher than the solidification temperature of Al. Therefore, when S4 is cooled, Al6(Mn,Fe) crystallizes in the Al liquid phase, and this may become a large crystal.

[0067] On the other hand, in S5, the amount of Fe is less than that in F4, so the Al solidification start temperature is higher than the crystallization temperature of Al6(Mn,Fe). Therefore, in S5, the generation of giant crystals is suppressed. In addition, in S6, the amount of Fe is even less than that in F5, so the difference between the Al solidification start temperature and the crystallization temperature of Al6(Mn,Fe) is large. Therefore, in S6, the decrease in strength and toughness due to giant crystals is less likely to occur.

[0068] In S7, since the Mn content is relatively large, the crystallization temperature of Al6(Mn,Fe) is higher than the solidification temperature of Al. Therefore, in S7, Al6(Mn,Fe) may crystallize in the Al liquid phase and become large crystals when cooled.

[0069] On the other hand, in S8, the Mn content is less than that in S7, so the Al solidification start temperature is higher than the crystallization temperature of Al6(Mn,Fe). Therefore, in S8, the generation of giant crystals is suppressed. In addition, in S9, the Mn content is even less than that in S8, so the difference between the Al solidification start temperature and the crystallization temperature of Al6(Mn,Fe) is large. Therefore, in S9, the decrease in strength and toughness due to giant crystals is less likely to occur.

[0070] In S10, the Mg content is relatively high, so the Mg2Si solution temperature is higher than the solidus temperature. Therefore, in S10, when the temperature rises, Al melts locally before Mg2Si dissolves, making it difficult to perform the soaking homogenization process to dissolve Mg2Si. Also, in S10, the crystallization temperature of Al6(Mn,Fe) is higher than the solidification start temperature of Al. Therefore, in S10, Al6(Mn,Fe) crystallizes in the Al liquid phase when cooled, forming giant crystals, which cause a decrease in strength and toughness.

[0071] On the other hand, in S11, the amount of Mg is less than that in S10, so there is a temperature range where the liquid phase does not appear even at the temperature where Mg2Si is in solid solution. In addition, in S12, the amount of Mg is even less than that in S11, so the solidification start temperature of Al is higher than the crystallization temperature of Al6(Mn,Fe). Therefore, the formation of giant crystals is suppressed in S12.

[0072] In S13, the amount of Mg is even less than in S12, so the temperature difference between the solidus temperature and the Mg2Si solid solution temperature is large, at 30° C. or more. As a result, in S13, there exists a temperature range in which it is possible to perform isothermal heating, even taking into account manufacturing variations.

[0073] In addition, since the Mg content in S14 is smaller than that in S13, the difference between the Al solidification start temperature and the crystallization temperature of Al6(Mn,Fe) becomes larger, and therefore, in S14, the decrease in strength and toughness due to the large crystallized particles is less likely to occur.

[0074] (scrap mixture ratio) Table 2 shows the average values ​​of the component specifications for 3104 aluminum alloy and 5182 aluminum alloy, and the corresponding blend ratios. The first line of Table 2 shows the average values ​​of the component specifications for 3104 aluminum alloy, and the second line shows the average values ​​of the component specifications for 5182 aluminum alloy.

[0075] For example, when the blend ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.

[0076] Therefore, when the ratio of each component of the aluminum alloy plate is equal to or greater than the above values ​​of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of the 3104 aluminum alloy plate is 50% by mass or more. As the blending ratio of the 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy plates of S1-S14 can be blended with 50% by mass or more of the 3104 aluminum alloy scrap.

[0077] [Table 2]

Claims

1. The silicon (Si) content is 0.20% by mass or more and 0.47% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.70 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.70 mass% or more and 1.20 mass% or less, The magnesium (Mg) content is 1.1% by mass or more and 3.7% by mass or less, The balance is aluminum (Al) and unavoidable impurities, Solidus temperature is Mg 2 Aluminum alloy sheet for can lids, with a temperature higher than the solid solution temperature of Si.

2. The aluminum alloy sheet for can ends according to claim 1, The silicon (Si) content is 0.20% by mass or more and 0.47% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.59 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.70% by mass or more and 0.98% by mass or less, The magnesium (Mg) content is 1.1% by mass or more and 3.3% by mass or less, An aluminum alloy sheet for can ends, in which the solidification start temperature of Al is higher than the crystallization temperature of the primary crystal.

3. The aluminum alloy sheet for can ends according to claim 2, The silicon (Si) content is 0.20% by mass or more and 0.39% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.59 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.70% by mass or more and 0.98% by mass or less, The magnesium (Mg) content is 1.1% by mass or more and 3.1% by mass or less, Solidus temperature to Mg 2 An aluminum alloy sheet for can ends, having a temperature difference of 30°C or more minus the solid solution temperature of Si.

4. The aluminum alloy sheet for can lids according to claim 3, The silicon (Si) content is 0.20% by mass or more and 0.39% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.51 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.70 mass% or more and 0.92 mass% or less, The magnesium (Mg) content is 1.1% by mass or more and 2.9% by mass or less, An aluminum alloy sheet for can ends, in which the temperature difference obtained by subtracting the crystallization temperature of primary crystals from the solidification start temperature of Al is 1°C or more.

Citation Information

Patent Citations

  • 3104 Aluminum alloy can lid material and production method thereof

    CN105568085A

  • Aluminum alloy plate as well as production method and applications thereof

    CN107058823A

  • Aluminum two piece can body and its manufacture

    JP1992221036A

  • Cover material for stay-on-tab type aluminum can and its production

    JP1992235248A

  • Production of hard aluminum alloy sheet for forming

    JP1992276046A