Method for separating and recovering plastic base material
By crushing laminates into small fluffs and using a surfactant-containing desorption liquid, the method enhances the efficiency and quality of plastic substrate recovery, addressing the inefficiencies and quality issues in existing recycling methods.
Patent Information
- Application Number
- JP2023200774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-11-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for recycling multi-layered plastic packaging materials face challenges in efficiently separating and recovering plastic substrates due to the adherence of coating layers, which leads to poor quality and appearance of the recycled material, and the inefficiency of current desorption processes with large-sized fluffs.
A method involving the crushing of laminates into fluffs with an average size of 5 mm or less, followed by contact with a desorption liquid to detach the coating layer, and further pulverizing to 1 mm or less, using cooling means and a surfactant-containing desorption liquid to enhance detachment and prevent redeposition.
This approach significantly improves the throughput and efficiency of the desorption process, reduces redeposition of coating layers, and results in high-quality recycled plastic substrates suitable for molding, maintaining the appearance and physical properties of the recovered material.
Smart Images

Figure 2024153543000001 
Figure 2024153543000002 
Figure 2024153543000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for separating and recovering a plastic substrate from a laminate comprising at least a plastic substrate layer and a coating layer. [Background technology]
[0002] In recent years, packaging made from plastic film, plastic bottles, and other plastic products have been discarded and dumped as garbage in the ocean, causing environmental pollution. These plastic products break down in seawater and become submicron-sized fragments (microplastics), which float in the seawater. When these microplastics are ingested by marine organisms such as fish, they become concentrated in the organisms' bodies, and there are concerns that they may affect the health of seabirds and humans who consume these marine organisms as food.
[0003] The plastic products include food packaging packages having a multi-layer structure using plastic films, and various plastic substrates such as polyester substrates, nylon substrates (NY), polypropylene substrates (PP), and polyethylene substrates (PE) are used as film substrates in such food packaging packages. These film substrates are printed with printing ink, bonded to other film substrates or heat-melting resin substrates via adhesives, and then cut and heat-sealed to form packages. However, such food packaging packages having a multi-layer structure contain multiple incompatible materials, and therefore have the problem that they cannot be recycled as they are.
[0004] Regarding material recycling of such multi-layered packaging materials, for example, Patent Documents 1 and 2 disclose a technique for removing not only a surface-printed structure but also a printed layer from a multi-layered laminate by treating a laminate having a release layer containing a polyurethane resin having a predetermined acid value with an alkaline aqueous solution. Patent Document 3 discloses a technique for removing an adhesive layer from a multi-layered laminate by treating a laminate having a polyester polyol-based adhesive having a predetermined acid value with an alkaline aqueous solution. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-090627 A [Patent Document 2] Patent Publication No. 2021-098294 [Patent Document 3] JP 2020-084130 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the present invention, "fluff" refers to at least a sheet or the like that has been shredded, crushed, or the like to a size that allows a process to be carried out, and is a laminate comprising at least a plastic substrate and a coating layer in contact with the plastic substrate. In particular, it refers to fluff that is used for the purpose of contacting with a desorption liquid to remove the coating layer and recover a high-purity plastic substrate. The plastic substrate may be a single layer or multiple layers. When the plastic substrate is multiple layers, the recovered plastic substrate may be one in which some or all of the multiple layers have been separated, or may remain as multiple layers. The fluff used in the desorption steps described in Patent Documents 1 to 3 is large in size, so even if an attempt is made to increase the amount of fluff to be treated relative to the desorption liquid in order to improve the treatment efficiency, problems arise in that if the fluff is immersed in a certain amount or more, it cannot be immersed in the desorption liquid and overflows, and pressure is applied to the motor, making it impossible to stir. Since the coating layer is large, the detachment time is long, and there is also a problem that the detached coating layer reattaches to the substrate. Here, "reattachment" refers to the coating layer detached from the substrate or the coating layer detached from the substrate that is not in direct contact with the plastic substrate being finely dispersed by stirring and reattaching to the substrate, which causes discoloration of the substrate to be recovered and deterioration of the properties of the recycled material. In other words, the molding material (hereinafter also referred to as recycled material or recycled substrate) obtained by recycling the plastic substrate to which the detached coating layer reattaches as described above causes deterioration of the appearance and physical properties due to coloration.
[0007] Therefore, an object of the present invention is to provide a method for efficiently separating and recovering a laminate suitable for plastic recycling, which has excellent releasability of a coating layer and inhibits reattachment of the detached coating layer components, and further provides a method for producing a high-quality molded product obtained by hot molding the recovered plastic substrate. [Means for solving the problem]
[0008] That is, the present invention provides a method for crushing a laminate having at least a plastic substrate and a coating layer in contact with the plastic substrate, into fluffs having an average size of 5 mm or less; A method for separating and recovering a laminate, comprising a step of contacting the crushed fluff with a release liquid to release the coating layer from the plastic substrate, The present invention relates to a method for separating and recovering a laminate, wherein the content of the laminate is 10% by mass or more based on the total mass of the elution liquid.
[0009] The present invention also relates to a method for separating and recovering the above laminate, which further comprises, after the crushing step, a step of finely pulverizing the resulting material into fluff having an average size of 1 mm or less.
[0010] The present invention also relates to a method for separating and recovering the above laminate, characterized in that the pulverizing step is carried out under cooling means.
[0011] The present invention also relates to a method for separating and recovering the laminate, wherein the plastic substrate contains a polyolefin.
[0012] The present invention also relates to the method for separating and recovering the laminate, wherein the plastic substrate is a plastic film.
[0013] The present invention also relates to a method for separating and recovering the above laminate, wherein the eluent contains water and a surfactant.
[0014] The present invention also relates to a method for producing a molding material, which includes a step of melt-kneading the plastic base material recovered by the above-mentioned method for separating and recovering a laminate.
[0015] The present invention also relates to a method for producing a molded article, which comprises a step of hot-molding the molding material obtained by the above-mentioned production method. Effect of the Invention
[0016] The present invention provides a method for efficiently separating and recovering a laminate suitable for plastic recycling, which has excellent releasability of a coating layer and is furthermore inhibited from reattaching components of the detached coating layer, and further provides a method for producing a high-quality molded article obtained by hot molding the recovered plastic substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The following describes in detail the embodiments of the present invention. However, the following description of the embodiments or requirements is merely an example of the embodiments of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention.
[0018] The present invention provides a method for separating and recovering a laminate, comprising a step of crushing a laminate comprising at least a plastic substrate and a coating layer in contact with the plastic substrate into fluff having an average size of 5 mm or less (hereinafter also referred to as a crushing step), and a step of contacting the crushed fluff with a detachment liquid to detach the coating layer from the plastic substrate (hereinafter also referred to as a detachment step), characterized in that the content of the laminate is 10 mass% or more relative to the total mass of the detachment liquid.
[0019] The laminate used in the present invention has a process of crushing the fluff into fluff with an average size of 5 mm or less before the detachment process, which allows the amount of the laminate to be increased during the detachment process. In addition, the detachment property is improved and the detachment process time can be shortened, so that the coating layer after detachment can be prevented from reattaching to the substrate. Furthermore, since the fluff size is small, the fluff recovered after detachment can be uniformly supplied and dispersed in an extruder or the like when melt-kneading, which allows the quality of the recycled material to be improved and stable production to be achieved.
[0020] <Separation and recovery method> The method for separating and recovering a laminate of the present invention includes a step of crushing a plastic substrate and a laminate having a coating layer in contact with the plastic substrate into fluff having an average size of 5 mm or less, and a step of contacting the crushed fluff with a release liquid to release the coating layer, the content of the laminate being 10% by mass or more relative to the total mass of the release liquid. The present invention may further include a step of finely pulverizing the fluff into fluff having an average size of 1 mm or less (hereinafter also referred to as a crushing step or a pulverizing step) after the crushing step.
[0021] <Step of Crushing the Laminated Body, Crushing Step>
[0022] The separation and recovery method of the present invention includes a method of crushing the laminate into fluffs having an average size of 5 mm or less. As a crushing method, a known crushing device can be used, for example, a cutter mill (rotary cutter), a jaw crusher, an impact crusher, a stamp mill, a ring mill, a roller mill, a jet mill, or a hammer mill. As a crushing device using a cutter mill, for example, MF45-700WRS manufactured by Tanaka, PF-2000 type manufactured by Nippon Seam, etc. can be mentioned.
[0023] An example of the crushing step in the present invention is shown below. The laminate is fed into the crushing device through a laminate inlet, and is crushed to a predetermined size or less in the crushing section using water fed from a water inlet as necessary. The crushing section may have a known structure. The crushing section preferably uses a rotary cutter that crushes the laminate using shear force.
[0024] In the crushing step, in order to wash off dirt such as the contents adhering to the laminate, the water may contain a detergent or a component of the release liquid. When the water used in the crushing step contains a detergent or a component of the release liquid, separation in the release step can be promoted.
[0025] As the crushing progresses and the size of the fluff falls below a certain size, it passes through a screen installed at the bottom of the crushing section due to its own weight together with the water. A screen is a device that acts as a filter to allow particles below a certain size to pass through, and is sometimes called a filter or grid. The shape of the screen can be circular, diamond, fan-shaped, etc., and can be selected appropriately depending on the hardness and thickness of the fluff.
[0026] The long side of the fluff can be adjusted by the size of the screen used. For example, if the screen is circular, the average fluff size can be controlled to about 15 mm by using a screen with a diameter of 15 mm. However, it is also possible to adjust the size of the fluff by adjusting the amount of laminate fed into the crusher and the residence time of the laminate in the crushing section.
[0027] The mass of water used in the crushing step is preferably 10 to 100 times, more preferably 15 to 80 times, and further preferably 20 to 60 times, based on the mass of the laminate. Within the above range, the amount of water for cooling the laminate is sufficient, and water constantly flows in and out of the crushed parts, suppressing local temperature rises in the crushed parts due to shearing, thereby suppressing fusion and softening of the resin substrate of the laminate. Furthermore, by keeping the amount of water within the above range, not only the fluff but also unwanted components such as tiny ink particles and adhesive particles generated during crushing can easily pass through the screen described above, preventing the laminate from remaining in the crushing section and the screen from clogging with unwanted components. This prevents the laminate from remaining excessively in the crushing section, and suppresses fusion of the resin base material and the generation of fine fragments due to excessive crushing. The mass of water used in the crushing step refers to the mass of water fed into the crushing device per minute, and the mass of the laminate refers to the mass of the laminate fed into the crushing device per minute. After the crushing step, known steps such as washing with water, draining, dehydration, drying, etc. may be added as appropriate.
[0028] The separation and recovery method of the present invention may have a first sorting step of sorting at least a specific plastic substrate before the crushing step so as to obtain a molding material with high purity. The sorting method used in the first sorting may be the method described in the second sorting step below, or may be, for example, a method of determining the type of plastic substrate using a sensor or the like and sorting the specific substrate from the other substrates using wind pressure or the like. In addition, before the crushing step, a rough crushing step may be performed in which the laminate is crushed into pieces of a size that can be easily fed into a crushing device. Examples of the device used in the rough crushing step include a hydraulic cutter.
[0029] In the present invention, the average size of the fluff after crushing the laminate is 5 mm or less. More preferably, it is 3 mm or less, and even more preferably, it is 1 mm or less. When it is 5 mm or less, the detachment property is good. In addition, since the fluff is uniformly incorporated during melt kneading, the properties of the recycled material are stable.
[0030] <Fine grinding process, crushing process> The separation and recovery method of the present invention may include a step of finely pulverizing the material into fluff having an average size of 1 mm or less. As a pulverizing method, a known pulverizing device may be used, for example, a screw mill, stamp mill, disk mill, pin mill, screen mill, cutter mill, which utilize impact and shear, or a ball mill, which utilizes impact, friction, and shear. In addition, a mortar-type extruder is an apparatus that can pulverize the material in a solid state by setting the temperature of the melt kneader below the melting temperature of the resin, and these pulverizing methods may be repeated or two or more types may be used in combination.
[0031] The pulverization step is preferably carried out under cooling means using a cryogen as necessary. The temperature of the cryogen used for cooling is preferably 0°C or lower, more preferably -20°C or lower, and even more preferably -60°C or lower. By keeping the temperature of the cryogen used for cooling at 0°C or lower, it is expected that the melting of the plastic due to shear heat generated during pulverization will be prevented, and the separation and detachment properties of the laminate will be improved. The lower the temperature, the shorter the time required for granulation. Furthermore, by pulverizing at or below the brittle temperature of the plastic, pulverization is possible without changing the properties of the plastic. The cryogens used for cooling include cooling water, liquid nitrogen, dry ice, and the like.
[0032] In the crushing step, the size of the fluff can be adjusted by the type of crushing blade, the rotation speed, the blade gap, the cooling temperature, and the like. The average size of the fluff obtained after pulverization is preferably 1 mm or less. More preferably, it is 1 μm to 1 mm, even more preferably, it is 10 μm to 800 μm, and even more preferably, it is 100 μm to 600 μm. When it is 1 mm or less, the time for the released liquid to penetrate from the end face of the fluff to the center is shortened, and separation and recovery can be performed efficiently, so that the release property is further improved. In addition, the fluff is more uniformly incorporated during melt kneading, so that the properties of the recycled material are stabilized and improved.
[0033] <Step of removing the coating layer, removal step> The separation and recovery method of the present invention includes a step of contacting a plastic substrate and a laminate having a coating layer in contact with the plastic substrate with a release liquid to release the coating layer. Hereinafter, the coating layer released from the substrate by the release liquid is also referred to as a release layer (including a coating layer not in direct contact with the plastic substrate).
[0034] In the present invention, "detachment" refers to the detachment of at least a part of the detachment layer by dissolving or swelling in the detachment liquid and peeling off, thereby detaching the substrate from the laminate, and includes both cases: (1) the detachment layer dissolves and detaches from the substrate, and (2) even if the detachment layer does not dissolve, it peels off due to neutralization, swelling, etc., and detaches from the substrate.
[0035] Since the present invention aims to make the plastic substrate after detachment into a molding material that is a high-quality recycled substrate or regenerated substrate, an embodiment in which as much of the detachment layer and the like is removed from the plastic substrate is preferred. Specifically, it is preferred that at least 50% by mass or more of the detachment layer is detached out of 100% by mass. More preferably, it is preferred that 60% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more is detached. This does not necessarily mean that the coating layer peels off from the interface with the substrate.
[0036] <Removal solution> The release liquid may be any liquid capable of swelling and dissolving the coating layer, and may be appropriately selected in consideration of the ease of release of the coating layer described below. Examples of such release liquid include water, a basic aqueous solution, and an acidic aqueous solution. From the viewpoint of the environment and maintaining the properties of the recycled material using the recovered plastic substrate, an aqueous solution is preferable. The release liquid preferably contains water in an amount of 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. These release liquids may be heated. The temperature of the release liquid when the laminate is immersed is preferably in the range of 25 to 120° C., more preferably 30 to 100° C., and particularly preferably 50 to 80° C. A higher release temperature is preferable from the viewpoint of release properties, and a lower release temperature is preferable from the viewpoint of suppression of curling of the substrate and suppression of re-adhesion.
[0037] From the viewpoint of releasing a urethane adhesive layer that is usually used in packaging materials, the release liquid is more preferably a basic aqueous solution containing a basic compound.
[0038] The immersion time in the release liquid is preferably in the range of 1 minute to 24 hours, more preferably 1 minute to 6 hours, even more preferably 1 minute to 1 hour, and further preferably 1 minute to 10 minutes.
[0039] In order to improve the desorption efficiency, it is preferable to stir, vibrate, circulate, or the like the desorption liquid. The rotation speed of the stirring blade is preferably 80 to 5000 rpm, and more preferably 80 to 4000 rpm.
[0040] [Surfactants] The release liquid preferably contains water and a surfactant. The surfactant mainly plays a role in improving the release property of the coating layer. This is thought to be because the action of the surfactant makes it easier for the release liquid to penetrate into coating layers such as the primer layer, the printing layer, and the adhesive layer, and promotes the release property. In addition, when the amount of the laminate relative to the release liquid is increased in the separation and recovery, the laminate and the separated substrate tend to curl with the released ink particles and the like wrapped around them, and even if the laminate and the separated substrate are immersed in the release liquid, it is difficult to cleanly remove the ink particles and the like wrapped around the curl. However, when the release liquid contains a surfactant, the surfactant is adsorbed on the laminate and the separated substrate surface, suppressing curling. As a result, the release property is improved and reattachment can be suppressed. Furthermore, when the release liquid contains a surfactant, it is possible to release the coating layer in contact with the plastic substrate even if the release layer does not have release properties due to the action of the basic compound.
[0041] The HLB value is an index value relating to the affinity of a surfactant for water and oil, with the HLB value of a substance with no hydrophilic groups being 0 and the HLB value of a substance with only hydrophilic groups being 20. The concept of HLB was proposed by William Griffin of the Atlas Powder Company in 1949, and several methods for determining the HLB value by calculation have been proposed, but in the present invention, the HLB value can be calculated using the Griffin method from the following formula. Formula) HLB = 20 x [(molecular weight of hydrophilic group contained in surfactant) / (molecular weight of surfactant)] Examples of the hydrophilic group contained in the surfactant include a hydroxyl group and an ethyleneoxy group.
[0042] The HLB value of the surfactant used in the present invention is preferably 7 or more. With an HLB value of 7 or more, excellent releasability and anti-reattachment properties are exhibited. The HLB value of the surfactant is preferably 8 or more, more preferably 10 or more. The HLB value of the surfactant is preferably 20 or less, more preferably 19 or less, and even more preferably 17 or less. An HLB value of 20 or less is preferable because it has excellent defoaming properties.
[0043] The type of surfactant may be, for example, nonionic, anionic, cationic, or amphoteric, and the type and amount of the surfactant may be appropriately selected according to the required properties. From the viewpoint of releasing property and foaming property, the surfactant is preferably at least one selected from the group consisting of anionic surfactants and nonionic surfactants. Moreover, the surfactant preferably has a structure with an alkylene oxide (hereinafter, also referred to as AO) added thereto, since this improves the releasing property and the preventing property of reattachment.
[0044] (Nonionic surfactant) The nonionic surfactant is not particularly limited, but is preferably an alkylene oxide adduct in which an alkylene oxide is added. More preferably, it is a compound obtained by adding an alkylene oxide to an alcohol having active hydrogen, a compound obtained by adding an alkylene oxide to an amine, or a compound obtained by adding an alkylene oxide to a fatty acid. The above addition may be either random addition or block addition. In addition, the number of carbon atoms of the alkylene oxide is preferably 2 to 4. The nonionic surfactant is more preferably an alcohol-based nonionic surfactant in which an alkylene oxide having 2 to 4 carbon atoms is added to an alcohol.
[0045] [Alcohol-based nonionic surfactant] Examples of the alcohol-based nonionic surfactant include an alkylene oxide adduct of a primary or secondary alcohol having a total of 8 to 24 carbon atoms, or an alkylene oxide adduct of an alkylphenol having a total of 8 to 12 carbon atoms. The primary or secondary alcohols may be either saturated or unsaturated. Examples of the primary or secondary alcohol having a total of 8 to 24 carbon atoms include lauryl alcohol, stearyl alcohol, oleyl alcohol, dodecyl alcohol, arachidyl alcohol, behenyl alcohol, lignoceryl alcohol, and myristyl alcohol. Examples of the alkylene oxide added to the alcohol include ethylene oxide, propylene oxide, and butylene oxide, and it is preferable to use ethylene oxide as an essential component. The number of moles of the alkylene oxide added is preferably 1 to 100 moles, more preferably 2 to 50 moles, per mole of the alcohol or alkylphenol. The above range is preferable because it has excellent elimination properties.
[0046] [Fatty acid-based nonionic surfactant] The structure of the fatty acid-based nonionic surfactant is not particularly limited, and examples thereof include alkylene oxide adducts of higher fatty acids having a total of 10 to 24 carbon atoms, fats and oils consisting of esters of the above-mentioned saturated or unsaturated higher fatty acids having a total of 10 to 24 carbon atoms and glycerin, and further, alkylene oxide adducts of mixtures of the above-mentioned fats and oils and polyhydric alcohols having 2 to 10 carbon atoms. The above-mentioned higher fatty acids having a total of 10 to 24 carbon atoms may be either saturated or unsaturated. Examples of the higher fatty acid having a total carbon number of 10 to 24 include saturated higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, arachic acid, and behenic acid; and unsaturated higher fatty acids such as palmitoleic acid, oleic acid, elaidic acid, linoleic acid, linolenic acid, erucic acid, and ricinoleic acid. Examples of the dihydric to decahydric polyhydric alcohol include ethylene glycol, propylene glycol, glycerin, polyglycerin, sorbitol, sorbitan, and sucrose. The type and molar number of the alkylene oxide are the same as those described in the above section on [Alcohol-based nonionic surfactants].
[0047] [Amine-based nonionic surfactant] Examples of the amine-based nonionic surfactant include AO adducts of saturated or unsaturated primary or secondary amines having a total carbon number of 8 to 36. Examples of the amine include 2-ethylhexylamine, di-2-ethylhexylamine, laurylamine, dilaurylamine, tetradecylamine, ditetradecylamine, hexadecylamine, dihexadecylamine, stearylamine, distearylamine, oleylamine, dioleylamine, etc. The type and number of moles of AO added are the same as above.
[0048] (anionic surfactant) The anionic surfactant is preferably a non-soap surfactant, and examples thereof include sulfonic acid-based anionic surfactants, sulfate ester-based anionic surfactants, carboxylate-based anionic surfactants, and phosphate ester-based anionic surfactants.
[0049] [Sulfonic acid-based anionic surfactant] Examples of the sulfonic acid anionic surfactant include alkylsulfonic acid, alkylbenzenesulfonic acid, alkylnaphthalenesulfonic acid, alkyldiphenyletherdisulfonic acid, alkylmethyltaurine, sulfosuccinic acid diester, alkylene oxide adduct of sulfonic acid, and salts thereof.Specific examples include hexanesulfonic acid, octanesulfonic acid, decanesulfonic acid, dodecanesulfonic acid, toluenesulfonic acid, cumenesulfonic acid, octylbenzenesulfonic acid, dodecylbenzenesulfonic acid, dinitrobenzenesulfonic acid, and lauryldodecylphenyletherdisulfonic acid.
[0050] [Sulfate ester-based anionic surfactants] Examples of the sulfate anionic surfactant include sulfate (alkyl ether sulfate), alkylene oxide adduct of sulfate, and salts thereof. Specific examples include lauryl sulfate, myristyl sulfate, and polyoxyethylene lauryl ether sulfate.
[0051] [Carboxylic acid type anionic surfactant] Examples of the carboxylic acid-based anionic surfactant include alkyl carboxylic acids, alkyl benzene carboxylic acids, alkylene oxide adducts of carboxylic acids, and salts thereof. Specific examples of the surfactant that can be used include lauric acid, myristic acid, palmitic acid, stearic acid, polyoxyethylene lauryl ether acetic acid, and polyoxyethylene tridecyl ether acetic acid.
[0052] [Phosphate-based anionic surfactant] Examples of the phosphate anionic surfactant include phosphate (alkyl ether phosphate), alkylene oxide adduct of phosphate, and salts thereof.Specific examples include octyl phosphate, lauryl phosphate, tridecyl phosphate, myristyl phosphate, cetyl phosphate, stearyl phosphate, polyoxyethylene octyl ether phosphate, polyoxyethylene lauryl ether phosphate, etc.
[0053] The anionic surfactant preferably has an alkyl group having 2 to 24 carbon atoms or an alkenyl group having 2 to 24 carbon atoms, and more preferably has an alkyl group having 8 to 18 carbon atoms. The alkyl group or the alkenyl group may be linear or branched. In addition, when the anionic surfactant is an alkylene oxide adduct, the alkylene oxide may be, for example, ethylene oxide, propylene oxide, or butylene oxide, with ethylene oxide being preferred. The number of moles of alkylene oxide added is preferably 1 to 12 moles, more preferably 1 to 8 moles, per mole of alcohol or alkylphenol. The above range is particularly preferred because of excellent releasability.
[0054] Examples of the salt constituting the anionic surfactant include metal salts such as sodium, potassium, magnesium, calcium, etc. These salts may be used alone or in combination of two or more. Among these, from the viewpoint of releasability and anti-reattachment properties, preferred anionic surfactants are sulfonate type and phosphate type, and more preferred are alkyl sulfonate, polyoxyalkylene alkyl ether sulfonate, polyoxyalkylene alkyl ether phosphate, etc.
[0055] (Cationic Surfactant) Examples of cationic surfactants include alkylamine salts and quaternary ammonium salts.Specific examples of usable surfactants include stearylamine acetate, trimethyl coconut ammonium chloride, trimethyl beef tallow ammonium chloride, dimethyldioleyl ammonium chloride, methyl oleyl diethanol chloride, tetramethyl ammonium chloride, lauryl pyridinium chloride, lauryl pyridinium bromide, lauryl pyridinium disulfate, cetyl pyridinium bromide, 4-alkyl mercaptopyridine, poly(vinylpyridine)-dodecyl bromide, and dodecyl benzyl triethyl ammonium chloride.
[0056] (Amphoteric surfactant) Examples of amphoteric surfactants include lauryl dimethylaminoacetate betaine, 2-alkyl Examples of suitable imidazoline derivatives include aryl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, coconut oil fatty acid amidopropyl dimethylaminoacetic acid betaine, polyoctyl polyaminoethyl glycine, and imidazoline derivatives.
[0057] These surfactants may be used alone or in combination of two or more. The content of the surfactant in the release liquid is preferably in the range of 0.001 to 10 mass%, more preferably in the range of 0.005 to 7 mass%, further preferably in the range of 0.03 to 5 mass%, and still more preferably in the range of 0.05 to 3 mass%, based on the mass of the release liquid. A content of 0.001 mass% or more is preferable because it suppresses curling of the substrate, provides excellent release properties, and also suppresses reattachment of the released coating layer components, and a content of 10 mass% or less is preferable from the viewpoint of defoaming properties.
[0058] [Antifoaming agent] In the present invention, it is also preferable that the release liquid further contains an antifoaming agent. By using the antifoaming agent in combination with the above-mentioned surfactant, good antifoaming properties can be exhibited without reducing the release property and the reattachment prevention property, and foaming caused by the surfactant can be suppressed. Examples of the antifoaming agent include silicone-based compounds and non-silicone-based compounds.
[0059] (Silicone compounds) Examples of the silicone-based compound include emulsion type, self-emulsifying type, oil type, oil compound type, and solvent type. The emulsion type is a silicone-based defoamer in which a silicone oil compound is emulsified with an activator to form an O / W type (oil in water type) emulsion. Examples of such antifoamers include "KM-89" and "KM-98" manufactured by Shin-Etsu Chemical Co., Ltd., "FC2913" and "SILFOAMSE47" manufactured by Asahi Kasei Wacker Silicone Co., Ltd., and "BYK-015" and "BYK-1640" manufactured by BYK Japan. The self-emulsifying type is a silicone-based defoamer that is 100% active ingredient and becomes an emulsion when diluted and mixed with water. Examples include "KS-540" and "X-50-1176" manufactured by Shin-Etsu Chemical Co., Ltd., and "SILFOAM SD670" and "SILFOAM SD850" manufactured by Wacker Asahi Kasei Silicones. Oil-type defoamers are 100% silicone oil defoamers that do not contain solvents or additives. Examples include "KM-89" and "KM-98" made by Shin-Etsu Chemical Co., Ltd., "AK350" and "AK12500" made by Asahi Kasei Wacker Silicone, and "BYK-1770" made by BYK Japan. Oil compound type is a silicone-based defoamer that combines silica particles with silicone oil. Examples include "KM-89" and "KM-98" manufactured by Shin-Etsu Chemical Co., Ltd., "SILFOAM SC370" and "PULPSIL22274VP" manufactured by Asahi Kasei Wacker Silicone, and "BYK-017" and "BYK-018" manufactured by BYK Japan. Solvent-type defoamers are silicone-based defoamers in which silicone oil is dissolved in a solvent. Examples include "KM-89" and "KM-98" manufactured by Shin-Etsu Chemical Co., Ltd., and "BYK-019" and "BYK-025" manufactured by BYK Japan.
[0060] (Non-silicone compounds) Examples of the non-silicone compounds include fatty acid ester compounds, urea resin compounds, paraffin compounds, polyoxyalkylene glycol compounds, acrylic ester copolymers, ester polymers, ether polymers, amide polymers, emulsion types of mineral oils, polysiloxane adducts, fluorine compounds, vinyl polymers, acetylene alcohol, acrylic polymers, special vinyl polymers, ethylene glycol, and higher alcohols (such as octyl alcohol and cyclohexanol).
[0061] The defoaming agent may be used alone or in combination of two or more. The content of the defoaming agent in the release liquid is preferably in the range of 0.0001 to 5 mass%, more preferably in the range of 0.001 to 4.5 mass%, further preferably in the range of 0.01 to 4 mass%, still more preferably in the range of 0.02 to 3.5 mass%, and particularly preferably in the range of 0.03 to 3 mass%, based on the mass of the release liquid. When it is 0.0001 mass% or more, the defoaming property is excellent, and when it is 5 mass% or less, the release property and the anti-reattachment property are excellent.
[0062] The above-mentioned defoaming agent is preferably at least one selected from the group consisting of emulsion-type silicone compounds, self-emulsifying silicone compounds, and non-silicone compounds, from the viewpoints that it has good alkali resistance and is unlikely to deteriorate releasability or anti-reattachment properties when combined with the above-mentioned surfactant.
[0063] [Basic compounds] As described above, the release liquid used in the present invention is preferably a basic aqueous solution containing a basic compound from the viewpoint of releasing a urethane adhesive layer that is usually used in packaging materials. The basic compound is not particularly limited, and for example, sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH)2), ammonia, barium hydroxide (Ba(OH)2), and sodium carbonate (Na2CO3) are preferably used. More preferably, it is at least one selected from the group consisting of sodium hydroxide and potassium hydroxide. The content of the basic compound in the basic aqueous solution is preferably in the range of 0.1 to 20 mass%, more preferably 0.3 to 15 mass%, and further preferably 0.5 to 10 mass%, based on the mass of the basic aqueous solution. Within the above range, the basic aqueous solution can retain sufficient basicity to remove the detachment layer described below by dissolving or swelling, and recover the plastic substrate.
[0064] The release liquid penetrates the end portion of the laminate, contacts the release layer, and dissolves or swells, separating the plastic substrate from the release layer. Therefore, in order to efficiently proceed with the release step, it is preferable that the laminate is crushed and the release layer is exposed on the cross section when it is immersed in the release liquid. In such a case, the substrate layer can be released in a shorter time.
[0065] [Fluff content before desorption (also called processing amount)] The content of the laminate when the laminate is separated in the release liquid is 10% by mass or more, preferably 10% by mass or more and 100% by mass or less, more preferably 15% by mass or more and 70% by mass or less, and even more preferably 20% by mass or more and 50% by mass or less, based on the total mass of the release liquid. 10% by mass or more is preferable from the viewpoint of processing efficiency. 100% by mass or less is preferable from the viewpoint of release property, anti-reattachment property, and stirring efficiency.
[0066] <Laminate> The laminate used in the present invention comprises a plastic substrate and a coating layer. The coating layer is, for example, at least one coating layer selected from the group consisting of a primer layer, a print layer, and an adhesive layer. By removing the plastic substrate with the release liquid, it becomes possible to recover and recycle the plastic substrate. In the present invention, in order to improve the releasing property when contacted with the release liquid, it is preferable to provide a primer layer having high affinity with the release liquid in contact with the plastic substrate layer.
[0067] <Print layer> In the present invention, the printed layer may be provided in contact with the plastic substrate, or in the case where the laminate has a primer layer, the printed layer may be provided in contact with the primer layer. The printed layer is a layer that forms an arbitrary printed pattern for the purpose of decoration, imparting aesthetic appeal, displaying contents, expiration date, manufacturer or seller, etc. The printed layer is a layer that includes a solid printed layer. The printed layer may be formed of a single layer or multiple layers. When the printed layer contains a water-soluble resin or a compound having an acidic group, which will be described later, the printed layer is endowed with a releasability function. The printing ink used to form the printed layer can be produced by dissolving and / or dispersing at least a colorant, a dispersant, and a binder resin in a solvent, and may contain other components as necessary.
[0068] [Coloring agent] The printing layer may be colored or colorless, and contains a known colorant used in printing inks and paints. Such colorants are not particularly limited, and may include inorganic pigments, organic pigments, dyes, metal powders that impart metallic luster, near-infrared absorbing materials, and ultraviolet absorbing materials. Examples of inorganic pigments include color pigments such as titanium oxide, red iron oxide, Prussian blue, ultramarine blue, carbon black, and graphite; and extender pigments such as calcium carbonate, kaolin, clay, barium sulfate, aluminum hydroxide, and talc. As the organic pigment, a soluble azo pigment, an insoluble azo pigment, an azo lake pigment, a condensed azo pigment, a copper phthalocyanine pigment, a condensed polycyclic pigment, etc. are suitably used. However, the pigment is not limited to these, and any pigment listed by its generic name in the Color Index can be used as appropriate. Among them, when the release solution is a basic aqueous solution, a pigment that is not eluted in the basic aqueous solution and has alkali resistance is preferred. Preventing the elution of the pigment makes it easy to reuse the basic aqueous solution. The alkali resistance of a pigment is generally estimated based on the skeleton or structure of the pigment. Examples of alkali-resistant pigments include inorganic pigments, CI Pigment Blue 15, and CI Pigment Yellow 83. When the pigment is titanium oxide, the content of titanium oxide in the printed layer is preferably 20 to 80% by mass, more preferably 30 to 75% by mass. When the pigment is an inorganic pigment other than titanium oxide, an extender pigment, or an organic pigment, the content of each of these pigments in the printed layer is preferably 0.5 to 60% by mass, more preferably 10 to 50% by mass.
[0069] [Dispersant] The printing layer contains a pigment derivative and / or a resin-type dispersant as a dispersant for the colorant, which improves the releasability. Furthermore, the dispersion stability and stability over time of the ink are improved. These may be used alone, but it is preferable to use them in combination, as this further improves the dispersion stability and stability over time.
[0070] (Pigment derivatives) Pigment derivatives are compounds in which a substituent has been introduced into the pigment skeleton. In printing ink, the pigment skeleton of the pigment derivative is adsorbed onto the pigment surface in the printing ink, and the substituent portion of the pigment derivative is oriented toward the solvent in the printing ink, thereby dispersing the pigment in the printing ink. As the pigment derivative, for example, a pigment having a functional group such as a carboxyl group, a sulfonic acid group, a carbonyl group, a sulfonyl group, etc. added to the skeleton of a phthalocyanine-based, azo-based, anthraquinone-based, quinacridone-based, etc. pigment, and a salt thereof can be preferably used. These can be used alone or in combination.
[0071] Commercially available pigment derivatives that can be preferably used include Solsperse 5000, Solsperse 12000 (manufactured by Lubrizol Japan), BYK-SYNERGIST 2100, BYK-SYNERGIST 2105 (manufactured by Big Chemie Japan), Efka 6745, Efka 6750 (manufactured by BASF), etc. These can be used alone or in combination.
[0072] The pigment derivative preferably exhibits the same or a similar color as the pigment in the ink. For example, when added to black ink or cyan ink, a phthalocyanine pigment derivative can be preferably used as the pigment derivative.
[0073] The total amount of the pigment derivatives is preferably 0.01 to 10% by mass, more preferably 0.05 to 6% by mass, and even more preferably 0.1 to 4% by mass, based on the total amount of the colorant. If the amount is 0.01% by mass or more, the dispersion stability of the printing ink is good, and the releasability is also improved. Furthermore, if the amount is 0.01 to 10% by mass, this contributes to improving the releasability and suppressing reattachment, and allows the material to be regenerated into a high-quality recycled molding material.
[0074] (Resin-type dispersant) The resin-type dispersant has a portion having an affinity for the pigment composition and has the property of being adsorbed to the pigment composition, and a portion having compatibility with the pigment composition carrier, and functions to adsorb to the pigment composition and stabilize the dispersion of the pigment composition in the pigment composition carrier. Specific examples of the resin-type dispersant include polycarboxylates such as polyurethane and polyacrylate, unsaturated polyamides, polycarboxylic acids, polycarboxylate (partial) amine salts, polycarboxylate ammonium salts, polycarboxylate alkylamine salts, polysiloxanes, long-chain polyaminoamide phosphates, hydroxyl group-containing polycarboxylates, and modified products thereof, oil-based dispersants such as amides formed by the reaction of poly(lower alkylene imines) with polyesters having free carboxyl groups and salts thereof, water-soluble resins and water-soluble polymer compounds such as (meth)acrylic acid-styrene copolymers, (meth)acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, polyvinyl alcohol, and polyvinylpyrrolidone, polyesters, modified polyacrylates, ethylene oxide / propylene oxide adducts, and phosphates. These can be used alone or in combination of two or more, but are not necessarily limited to these.
[0075] The total amount of the resin-type dispersant is preferably 0.01 to 30% by mass, more preferably 0.05 to 20% by mass, and even more preferably 0.1 to 10% by mass, based on the total amount of the colorant. If it is 0.01% by mass or more, the dispersion stability of the printing ink is improved, and the releasability is also improved. If it is 30% by mass or less, the water resistance of the printed layer is improved.
[0076] [Binder resin] As the binder resin of the printing layer, for example, a fibrous material such as nitrocellulose, cellulose acetate propionate, chlorinated polypropylene, vinyl chloride-vinyl acetate copolymer, polyester, acrylic, urethane resin and acrylic urethane, polyamide, polybutyral, cyclized rubber, chlorinated rubber, or a binder using them in combination can be used. When the printing layer contains a water-soluble resin or a compound having an acidic group, which will be described later, the printing layer is provided with a releasability function. These resins may be used alone or in combination of two or more.
[0077] [Primer layer] The laminate used in the present invention may have a primer layer. When the laminate has a primer layer, the primer layer is disposed in contact with the plastic substrate and is formed from a primer composition having a water-soluble resin or a compound having an acidic group. Even if a non-removable printed layer or adhesive layer is present, the primer layer plays a role in removing the plastic substrate by dissolving or peeling with a release liquid.
[0078] (Water-soluble resin) The water-soluble resin may be any resin that can swell or dissolve in water and be removed from the plastic substrate. The water may be heated to a temperature of about 25 to 100° C. This allows the primer layer to be removed by water (including warm water). Such resins can be selected from known resins as long as they do not impair water solubility, and examples thereof include water-soluble polyester resins, water-soluble polyamide resins, water-soluble polyimide resins, water-soluble acrylic resins, water-soluble polyurethane resins, water-soluble polyallylamine resins, water-soluble phenolic resins, water-soluble epoxy resins, water-soluble phenoxy resins, water-soluble urea resins, water-soluble melamine resins, polyvinyl alcohol resins, and modified products of these resins. These can be used alone or in combination of two or more. Among them, polyvinyl alcohol (PVA) resins are preferably used from the viewpoints of availability and release properties. When the water-soluble resin has film-forming properties, the water-soluble resin may be used as the binder resin constituting the primer layer.
[0079] As the polyvinyl alcohol resin, in addition to unmodified polyvinyl alcohol, modified polyvinyl alcohol obtained by copolymerizing various monomers during the production of vinyl ester resin and saponifying the copolymer, or various post-modified polyvinyl alcohols obtained by introducing various functional groups into unmodified polyvinyl alcohol by post-modification may be used. Also, modified polyvinyl alcohols further modified may be used. These modifications may be performed within a range that does not impair the water solubility of the polyvinyl alcohol resin. These resins may be used alone or in combination of two or more.
[0080] Preferred examples of polyvinyl alcohol resins include resins containing structural units having a primary hydroxyl group in the side chain, and ethylene-modified polyvinyl alcohol resins. Among them, polyvinyl alcohol resins containing structural units having a primary hydroxyl group in the side chain are preferred, because they have excellent melt moldability and water solubility. The number of primary hydroxyl groups in these structural units is usually 1 to 5, preferably 1 to 2, and more preferably 1. In addition to the primary hydroxyl groups, it is also preferred that the structural units have secondary hydroxyl groups.
[0081] The saponification degree of the polyvinyl alcohol resin used in the present invention (measured according to JIS K 6726) is usually 60 to 100 mol%. The preferred range of the saponification degree varies depending on the modified species. For example, in the case of an unmodified polyvinyl alcohol resin, it is usually 60 to 99.9 mol%, preferably 70 to 99.0 mol%, more preferably 75 to 98.5%. The saponification degree of the modified polyvinyl alcohol resin containing a side chain 1,2-diol structural unit is usually 60 to 99.9 mol%, preferably 65 to 99.8 mol%, more preferably 70 to 99.5 mol%. If the saponification degree is too low, the water solubility tends to decrease. The saponification degree of the ethylene-modified polyvinyl alcohol resin modified with a small amount of ethylene is usually 60 mol% or more, preferably 70 to 99.5 mol%, particularly preferably 75 to 99.0 mol%. The saponification degree within the above range is preferable because it provides excellent water solubility and good releasability, and is also preferable because it provides excellent coatability when forming a primer layer.
[0082] The average degree of polymerization of the polyvinyl alcohol resin (measured in accordance with JIS K 6726) is usually 100-3,000, preferably 150-2,000, more preferably 180-1,000, and particularly preferably 200-800.
[0083] (Compounds having an acidic group) The compound having an acidic group may be a resin having an acidic group or a low molecular weight compound having an acidic group, which allows the primer layer to be removed by the above-mentioned basic aqueous solution.
[0084] Examples of the resin having an acidic group include a cellulose resin, a urethane resin, a polyamide resin, a vinyl chloride / vinyl acetate copolymer, a ketone resin, a polyester resin, and a (meth)acrylic resin. Examples of the acidic group include a carboxy group, a phosphoric acid group, a sulfo group, a sulfino group, and the like, or an ester or salt thereof. Furthermore, as the resin having an acidic group, a rosin-modified resin having an acid value, such as maleic rosin or fumaric rosin, can be used. In addition, examples of resins having an acidic group that can be used include radical copolymers such as styrene-(meth)acrylic resins, styrene-maleic acid (anhydride) resins, and terpene-maleic acid (anhydride) resins, which are copolymerized with polymerizable monomers having an acidic group, such as polymerizable monomers having a carboxy group, such as itaconic acid, maleic acid, fumaric acid, and cinnamic acid; polymerizable monomers which are acid anhydrides, such as itaconic acid anhydride and maleic acid anhydride; polymerizable monomers having a sulfonic acid group, such as sulfonated styrene; and polymerizable monomers having a sulfonamide group, such as vinylbenzenesulfonamide; and acid-modified polyolefin resins. These may be used alone or in combination of two or more.
[0085] The low molecular weight compound having an acidic group refers to a compound that does not have a molecular weight distribution and has a molecular weight of 1,000 or less. Examples of such compounds include saturated fatty acids such as lauric acid, myristic acid, palmitic acid, margaric acid, and stearic acid; unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, arachidonic acid, eicosapentaenoic acid, docosahexaenoic acid, and sorbic acid; hydroxy acids such as lactic acid, malic acid, and citric acid; aromatic carboxylic acids such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, salicylic acid, gallic acid, mellitic acid, and cinnamic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, fumaric acid, and maleic acid; tricarboxylic acids such as aconitic acid; oxocarboxylic acids such as pyruvic acid and oxaloacetic acid; carboxylic acid derivatives such as amino acids and nitrocarboxylic acids; and acid anhydrides such as trimellitic anhydride and pyromellitic anhydride. The low molecular weight compound having an acidic group can be used in combination with the above-mentioned resin having an acidic group or a known binder resin constituting a known primer layer to form a primer layer.
[0086] From the viewpoint of recoating suitability, the primer layer preferably contains a compound having an acidic group. Also, from the viewpoint of printability, the primer layer preferably contains a urethane resin having an acidic group, an acrylic resin having an acidic group, or a rosin-modified resin. The primer layer may contain one of these resins alone or two or more of them in combination.
[0087] [Urethane resin having acidic groups] The urethane resin having an acidic group is not particularly limited, and examples thereof include a urethane resin obtained by reacting a polyol having an acidic group with a polyisocyanate, a resin obtained by acid-modifying hydroxyl groups in a urethane resin obtained by reacting a polyol with a polyisocyanate, and a resin obtained by acid-modifying amino groups in a urethane urea resin obtained by reacting a polyamine with an isocyanate group in a urethane resin obtained by reacting a polyol with a polyisocyanate. In addition, as the urethane resin having an acidic group, a resin obtained by reacting a polyol containing a hydroxy acid with a polyisocyanate may be used. By using a hydroxy acid as the polyol, it is possible to impart an acid value derived from a carboxy group to the urethane resin, and it is possible to improve the releasability. In addition, when the urethane resin having an acidic group has an isocyanate group, a polyamine may be reacted with a part of the isocyanate group to introduce a urea bond, thereby forming a urethane urea.
[0088] Polyol Polyol is a general term for compounds having at least two hydroxyl groups in one molecule. The number average molecular weight of the polyol is preferably 500 to 10,000, more preferably 1,000 to 5,000. The number average molecular weight is calculated from the hydroxyl value of the polyol, and the hydroxyl value refers to a value measured according to JIS K 0070. When the number average molecular weight of the polyol is 500 or more, the flexibility of the primer layer is excellent and the adhesion to the plastic substrate is improved. When the number average molecular weight is 10,000 or less, the adhesion to the plastic substrate is improved. It has excellent blocking resistance.
[0089] The polyol is not particularly limited, and more preferably, at least one polyol selected from the group consisting of polyester polyol, polyether polyol, and polycarbonate polyol is used. The polyol may further include other dimer diol, hydrogenated dimer diol, castor oil modified polyol, etc. That is, the urethane resin preferably contains a structural unit derived from at least one polyol selected from the group consisting of polyester polyol, polyether polyol, and polycarbonate polyol. Since the ester bond site of the polyester polyol is hydrolyzed by alkali to improve the releasability, the urethane resin more preferably contains a structural unit derived from a polyester polyol. The content of the structural units derived from polyol is preferably 10 to 75% by mass, more preferably 15 to 70% by mass, and even more preferably 20 to 65% by mass, based on the total amount of the urethane resin. The content of the structural units derived from polyester polyol is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 60% by mass or more, and particularly preferably 80% by mass or more, based on the total amount of the structural units derived from polyol.
[0090] Hydroxy acids The polyol may contain a hydroxy acid. The hydroxy acid refers to a compound having both a hydroxyl group, which is an active hydrogen group, and an acidic functional group in one molecule. The acidic functional group refers to a functional group that can be neutralized with potassium hydroxide when measuring the acid value, and specifically includes a carboxy group and a sulfonic acid group, and is preferably a carboxy group. As such a hydroxy acid, for example, dimethylolalkanoic acid such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, and 2,2-dimethylolvaleric acid is preferably used.
[0091] <Polyisocyanate> The polyisocyanate is not particularly limited and can be selected from conventionally known polyisocyanates. It preferably contains a diisocyanate or triisocyanate, and more preferably contains an aromatic, aliphatic or alicyclic diisocyanate. These may be used alone or in combination of two or more kinds.
[0092] Polyamines The polyamine for forming the urethane urea is not particularly limited, and is preferably a diamine compound. A diamine having a hydroxyl group may be used because it can introduce a hydroxyl group into the urethane resin.
[0093] The acid value of the urethane resin having an acidic group is preferably 15 mgKOH / g or more. It is more preferably 15 to 70 mgKOH / g, and further preferably 20 to 50 mgKOH / g. When it is 15 mgKOH / g or more, the desorption property by the desorption liquid becomes good, and therefore it is preferable. The hydroxyl value of the urethane resin is preferably 1 to 35 mgKOH / g, more preferably 10 to 30 mgKOH / g. A hydroxyl value of 1 mgKOH / g or more is preferable because the release property by the release solution is good, and a hydroxyl value of 35 mgKOH / g or less is preferable because the release property by the release solution is good.
[0094] The weight average molecular weight of the urethane resin having an acidic group is preferably 10,000 to 100,000, more preferably 15,000 to 70,000, and further preferably 15,000 to 50,000. The molecular weight distribution (Mw / Mn) of the urethane resin is preferably 6 or less. Mw represents the weight average molecular weight, and Mn represents the number average molecular weight. When the molecular weight distribution is 6 or less, the releasing property, drying property of the primer composition, and retort resistance are excellent. In addition, when the molecular weight distribution is The smaller the molecular weight distribution, i.e., the sharper the molecular weight distribution, the more uniform the dissolution and peeling action by the release liquid occurs, and the more improved the release properties of the plastic substrate. The molecular weight distribution is more preferably 5 or less, and even more preferably 4 or less. The molecular weight distribution is also preferably 1.5 or more, and more preferably 1.2 or more. In the present invention, Mw, Mn and molecular weight distribution (Mw / Mn) are values calculated as polystyrene by gel permeation chromatography (GPC).
[0095] The urethane resin having an acidic group may have an amine value. When the urethane resin has an amine value, the amine value is preferably 0.1 to 20 mgKOH / g, and more preferably 1 to 10 mgKOH / g. When the amine value is within the above range, the adhesion to the substrate is excellent.
[0096] The number of urethane bonds in the polyurethane resin having an acidic group is preferably 1 to 3 mmol / g, more preferably 1.5 to 2 mmol / g. The number of urea bonds is preferably 0 to 3 mmol / g, more preferably 0.2 to 1 mmol / g. The total number of urethane bonds and urea bonds is preferably 1 to 6 mmol / g, more preferably 1.7 to 3 mmol / g. By setting the number of urethane bonds and the number of urea bonds within the corresponding ranges, releasability and adhesion to substrates are improved.
[0097] [Acrylic resin having acidic group] Examples of acrylic resins having an acidic group include polymers obtained by polymerizing a monomer containing a (meth)acrylic monomer having an acidic group, such as (meth)acrylic acid or maleic acid; and resins obtained by polymerizing a monomer containing a (meth)acrylic monomer having a hydroxyl group or a glycidyl group, and then modifying the functional group to introduce a carboxyl group (e.g., maleic anhydride modified resin). The acid value of the acrylic resin having an acidic group is preferably 50 mgKOH / g or more, and more preferably 100 mgKOH / g or more.
[0098] [Rosin-modified resin] Rosin-modified resins are resins prepared using rosin as one of the raw materials. Rosin contains a mixture of resin acids such as abietic acid, palustric acid, isopimaric acid, and levopimaric acid, and these resin acids contain hydrophilic and chemically active carboxyl groups, some of which have conjugated double bonds. For this reason, various rosin-modified resins are prepared by combining polyhydric alcohols and polybasic acids and polycondensing them, adding resol, which is a condensate of phenol, to the benzene ring contained in the rosin skeleton, or by carrying out a Diels-Alder reaction with maleic anhydride or maleic acid, which is a dienophile, to add maleic acid or maleic anhydride skeletons. Various types of such rosin-modified resins are commercially available, and it is also possible to obtain and use them.
[0099] Examples of rosin-modified resins include maleated rosin, fumarated rosin, rosin-modified maleic acid resin, rosin-modified fumaric acid resin, rosin-modified phenolic resin, rosin-modified alkyd resin, and rosin-modified polyester resin. In the present invention, any rosin-modified resin may be used, but among these, those containing a moiety derived from at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride in its structure are preferably used. The resin "containing a moiety derived from at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride in its structure" is prepared using at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride as part of the raw material, and examples thereof include rosin-modified maleic acid resins and rosin-modified fumaric acid resins obtained by condensation polymerization of maleic acid or fumaric acid as part of the polybasic acid, and maleic acid, maleic anhydride, fumaric acid, and fumaric anhydride as dienophiles. This refers to maleated rosin, fumarated rosin, and resins obtained by polymerizing other chemical species using the functional groups contained in these resins, which have a structure obtained by adding water-fumaric acid through a Diels-Alder reaction.
[0100] The acid value of the rosin-modified resin is preferably from 10 to 400 mgKOH / g, and more preferably from 100 to 300 mgKOH / g.
[0101] (Other ingredients) The primer layer may contain a resin other than the water-soluble resin or the compound having an acidic group. Examples of such resins include cellulose resins, polyamide resins, vinyl chloride resins such as vinyl chloride-vinyl acetate copolymer resins or vinyl chloride-acrylic copolymer resins, ethylene-vinyl acetate copolymer resins, vinyl acetate resins, acrylic resins, styrene resins, dammar resins, styrene-acrylic copolymer resins, polyester resins, alkyd resins, terpene resins, phenol-modified terpene resins, ketone resins, cyclized rubbers, chlorinated rubbers, butyral, polyacetal resins, petroleum resins, and modified resins thereof. These resins may be used alone or in combination of two or more. Among them, the primer layer preferably contains at least one resin selected from the group consisting of cellulose resin, vinyl chloride resin, rosin resin, and acrylic resin, and more preferably contains vinyl chloride resin or acrylic resin. The mass ratio of the urethane resin having an acidic group to the other resins (urethane resin having an acidic group:other resins) is preferably 95:5 to 50:50. When the mass ratio is within the above range, the printed layer is peeled off in a thin film state when peeled off together with the primer layer in a basic aqueous solution, which is preferable because recovery is easy.
[0102] The primer layer may contain a body pigment. Examples of the body pigment include silica, barium sulfate, kaolin, clay, calcium carbonate, magnesium carbonate, zinc oxide, zirconium oxide, and other metal oxides. Among these, silica is preferred, and hydrophilic silica is more preferred. The average particle size of the extender pigment is preferably 0.5 to 10 μm, more preferably 1 to 8 μm. The content of the extender pigment in the primer layer is preferably 0.5 to 10 mass %, more preferably 1 to 5 mass %. When the average particle size and the content of the extender pigment are within the above ranges, the wettability of the printing layer is improved, and the image quality is improved.
[0103] The primer layer may be a layer in which the above-mentioned urethane resin having an acidic group is crosslinked with a curing agent. By introducing a crosslinked structure into the primer layer, the penetration and bleeding of the printing layer formed on the primer layer is suppressed, and excellent image quality can be achieved. The curing agent may be, for example, a polyisocyanate. The polyisocyanate is not particularly limited and may be selected from conventionally known polyisocyanates, for example, an aliphatic polyisocyanate or an aromatic aliphatic polyisocyanate. These may be used alone or in combination of two or more kinds.
[0104] The primer layer may further contain known additives, such as dispersants, wetting agents, adhesion promoters, leveling agents, defoamers, antistatic agents, viscosity modifiers, metal chelates, trapping agents, antiblocking agents, wax components other than those mentioned above, and silane coupling agents.
[0105] The thickness of the primer layer is preferably in the range of 0.5 to 3.0 μm, more preferably 0.6 to 2.0 μm, and further preferably 0.8 to 1.5 μm, and can be formed by using a known method.
[0106] [Adhesive Layer] The laminate of the present invention may have an adhesive layer. When the laminate has an adhesive layer, the adhesive layer is preferably disposed in contact with the plastic substrate, contains a compound having an acidic group, and plays a role in releasing the plastic substrate by dissolution, peeling, or the like using a release liquid. When the adhesive layer contains a resin having an acidic group or a low molecular weight compound having an acidic group, the adhesive layer can be released using the above-mentioned basic aqueous solution. For the compound having an acidic group, the resin having an acidic group, and the low molecular weight compound having an acidic group, the description of (Compound having an acidic group) in the above section [Primer layer] can be applied. The method for forming the adhesive layer is not limited, and the adhesive layer can be formed by using a known method.
[0107] From the viewpoint of releasability, the adhesive layer may be a cured product of an adhesive containing a polyester polyol having an acidic group and at least one polyisocyanate selected from the group consisting of an aliphatic polyisocyanate and an araliphatic polyisocyanate. The cured product corresponds to a resin having an acidic group. The adhesive layer may also be a cured product of an adhesive containing a polyester polyol, at least one polyisocyanate selected from the group consisting of aliphatic polyisocyanates and araliphatic polyisocyanates, and a low molecular weight compound having an acidic group.
[0108] (Polyester polyol) The polyester polyol may have an acidic group and may be appropriately selected from known polyester polyols. By including such a polyester polyol, when a basic aqueous solution is used as the release liquid, the release property is improved by having an ester bond with high affinity with a basic compound, which is preferable. The polyester polyol may be used alone or in combination of two or more kinds.
[0109] The polyester polyol is not particularly limited, but polyester polyols obtained by reacting a carboxyl group component with a hydroxyl group component; or polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone) are preferably used. Examples of the carboxyl group component include dibasic acids such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, phthalic anhydride, adipic acid, azelaic acid, sebacic acid, succinic acid, glutaric acid, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, maleic anhydride, and itaconic anhydride, or dialkyl esters thereof, or mixtures thereof. Examples of the hydroxyl group component include diols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, butylene glycol, neopentyl glycol, trimethylolpropane, glycerin, 1,6-hexanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, 1,9-nonanediol, polyoxyethylene glycol, polyoxypropylene glycol, polytetramethylene ether glycol, polyether polyol, polycarbonate polyol, polyolefin polyol, acrylic polyol, polyurethane polyol, and mixtures thereof. The above carboxyl group components and hydroxyl group components may be used in combination of two or more kinds.
[0110] The polyester polyol may be a polyester urethane polyol obtained by reacting a hydroxyl group in a polyol with a polyisocyanate. The polyester polyol has a urethane bond, and thus exhibits excellent heat resistance and adhesiveness. Examples of the polyisocyanate include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, hexafluoroisocyanate, and 1,2-diisocyanate. Examples include methylene diisocyanate and hydrogenated diphenylmethane diisocyanate.
[0111] The polyester polyol may be an acid anhydride-modified product obtained by reacting an acid anhydride with a hydroxyl group in the polyol, thereby introducing a carboxyl group, which is an acidic group, into the polyester polyol. Examples of the acid anhydride include pyromellitic anhydride, mellitic anhydride, trimellitic anhydride, and trimellitic ester anhydride. Examples of the trimellitic ester anhydride include ethylene glycol bisanhydrotrimellitate and propylene glycol bisanhydrotrimellitate.
[0112] The acid value of the polyester polyol is preferably 5.0 mgKOH / g or more, more preferably 10.0 mgKOH / g or more. The acid value of the polyester polyol is preferably 100 mgKOH / g or less, more preferably 80 mgKOH / g or less. When the acid value of the polyester polyol is in the above range, when the polyester polyol is contacted with a release liquid that is a basic aqueous solution, the basic aqueous solution penetrates and decomposes the polyester polyol, thereby exhibiting better release properties. When the adhesive contains a plurality of polyester polyols, the acid value of the entire polyester polyols can be determined from the acid value of each polyester polyol and its mass ratio.
[0113] The number average molecular weight (Mn) of the polyester polyol is preferably 3,000 to 25,000, more preferably 5,000 to 20,000, and particularly preferably 7,000 to 15,000. When the number average molecular weight of the polyester polyol is 3,000 or more, not only the coatability but also sufficient retort resistance can be exhibited, and when it is 20,000 or less, not only the coatability but also the release property is improved, so this is preferable.
[0114] In order to satisfy various physical properties required for the packaging material, the polyester polyol component may contain a combination of multiple polyester polyol components, for example, a polyester polyol having a number average molecular weight of 5,000 to 20,000, and further, in order to improve adhesion to the substrate, a polyester polyol having a number average molecular weight of less than 3,000 may be contained. The content of the polyester polyol having a number average molecular weight of less than 3,000 is preferably 0 to 30 mass %, more preferably 0 to 20 mass %, based on the total mass of the polyester polyol. When it is 30 mass % or less, retort resistance can be maintained.
[0115] (Other polyols) The adhesive constituting the adhesive layer may contain a polyol other than the polyester polyol. The polyol that may be contained other than the polyester polyol is not particularly limited, and examples thereof include polycarbonate polyol, polycaprolactone polyol, polyether polyol, polyolefin polyol, acrylic polyol, silicone polyol, castor oil-based polyol, and fluorine-based polyol.
[0116] (Polyisocyanate) The polyisocyanate to be combined with the above-mentioned polyester polyol to form the adhesive layer is preferably at least one selected from the group consisting of known aliphatic polyisocyanates and araliphatic polyisocyanates.
[0117] Examples of the aliphatic polyisocyanate include acyclic aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, 1,2-propylene diisocyanate, and 1,2-butylene diisocyanate; alicyclic diisocyanates such as 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, and 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (hereinafter, isophorone diisocyanate); and the above diisocyanates. and polyisocyanates such as allophanate type, nurate type, biuret type, and adduct type derivatives derived from the above, or complexes thereof. The derivative is preferably a nurate type or an adduct type, more preferably an adduct type. As the aliphatic polyisocyanate, a polyisocyanate derived from hexamethylene diisocyanate (hereinafter also referred to as HDI) is preferred, which can easily ensure a balance between releasability and laminate properties.
[0118] Examples of the araliphatic polyisocyanate include araliphatic diisocyanates such as 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or a mixture thereof; and polyisocyanates such as allophanate type, nurate type, biuret type, and adduct type derivatives derived from the above araliphatic diisocyanates, or complexes thereof.
[0119] (Other polyisocyanates) The adhesive may contain polyisocyanates other than the aliphatic polyisocyanates and aromatic aliphatic polyisocyanates, as long as the effects of the present invention are not impaired. Examples of such polyisocyanates include aromatic diisocyanates such as toluene diisocyanate and diphenylmethane diisocyanate; and polyisocyanates such as derivatives of the above diisocyanates or complexes thereof.
[0120] The polyol and polyisocyanate may be mixed so that the molar ratio (NCO / OH) of the isocyanate groups of the polyisocyanate to the hydroxyl groups of the polyol is 0.3 to 10.0, preferably 0.3 to 7.0, and more preferably 0.5 to 5.0.
[0121] (Other ingredients) The adhesive layer may contain, in addition to a silane coupling agent, a phosphorus oxygen acid or a derivative thereof, a leveling agent, an antifoaming agent, and a reaction accelerator, inorganic fillers (e.g., silica, alumina, mica, talc, aluminum flakes, glass flakes), layered inorganic compounds, stabilizers (e.g., antioxidants, heat stabilizers, UV absorbers, hydrolysis inhibitors), rust inhibitors, thickeners, plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, catalysts for adjusting the curing reaction, and the like.
[0122] <Plastic substrate layer> Examples of the plastic substrate include polyolefin resin, polyester resin, polyamide resin, polystyrene resin, vinyl chloride resin, vinyl acetate resin, ABS resin, acrylic resin, acetal resin, polycarbonate resin, polyvinyl alcohol resin, and cellulose-based plastics.
[0123] From the viewpoint of reuse as a recycled substrate, the plastic substrate is preferably a polyolefin substrate containing a polyolefin resin. Examples of substrates containing such polyolefin resin include plastic substrates such as polyethylene (PE) and biaxially oriented polypropylene (OPP), as well as sealant substrates such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), high-density polyethylene (HDPE), acid-modified polyethylene, non-oriented polypropylene (CPP), acid-modified polypropylene, and copolymer polypropylene. The plastic substrate may be a gas barrier substrate that has been subjected to a gas barrier treatment.
[0124] The thickness of the plastic substrate layer is not particularly limited and may be appropriately selected depending on the application. The thickness is preferably 5 to 200 μm, and more preferably 10 to 150 μm. The thinner the thickness, the more likely the substrate is to curl, and the more difficult it is to remove. Examples of gas barrier substrates include aluminum foil, a metal vapor deposition layer such as aluminum, and a plastic substrate having a metal oxide vapor deposition layer such as silica or alumina. The thickness of the aluminum foil is often in the range of 3 to 50 μm from an economical point of view. Furthermore, the aluminum foil, the aluminum vapor deposition layer, and the alumina vapor deposition layer are dissolved and desorbed in a basic aqueous solution, and therefore have desorption properties, allowing the plastic substrate to be easily separated.
[0125] Examples of the laminate structure used in the present invention are given below, but are not limited to these. In the following structures, the "plastic substrate" does not need to be a single layer, and may be a laminate in which multiple substrates are laminated. In addition, the layer in contact with the plastic substrate to be separated and recovered need only be removable. For example, a laminate that is "plastic substrate / multiple printed layers" can be said to be a "plastic substrate / printed layer" or a "plastic substrate / primer layer / printed layer" if the printed layer in contact with the plastic substrate is removable. Plastic substrate / printing layer Plastic substrate / Primer layer / Printing layer ·Plastic substrate / printing layer / adhesive layer / plastic substrate ·Plastic substrate / Primer layer / Printing layer / Adhesive layer / Plastic substrate · Substrate layer / printed layer / adhesive layer / plastic substrate ·Plastic substrate / Primer layer / Printed layer / Adhesive layer / Vapor deposition layer / Plastic substrate
[0126] <Process for separating and recovering plastic base materials> After the detachment step, the separated plastic substrate is collected. The collection method can be a known method that utilizes the difference in physical properties between the plastic substrate after detachment and the coating layer pieces after detachment. For example, a floating / sinking method that utilizes specific gravity or a centrifugal separation method can be applied.
[0127] Before recovering the plastic substrate, a process of removing components other than the resin substrate layer, such as ink and adhesive, which have been removed from the laminate, may be provided. The components such as the ink and adhesive are finely divided by the shear force during the removal process, so that the plastic substrate can be recovered while removing fine pieces of the ink and adhesive components attached to the plastic substrate by adjusting the size of the filter using the difference in size with the fluff. There is also a method of separation using the specific gravity difference between the plastic substrate and the fine pieces of the ink and adhesive components. The release liquid obtained after recovering the plastic substrate and removing components other than the plastic substrate layer, such as ink and adhesive, may be reused in the release step.
[0128] After the detachment step, a step of selecting the resin type of the plastic substrate (second selection step) may be included. Examples of the selection step include a gravity selection method using a liquid, a wind selection method, and a near-infrared selection method. From the viewpoint of productivity, the gravity selection method using a liquid is preferred. In the gravity separation method using a liquid, for example, when water is used as the density liquid, it is possible to separate resin substrates having a lower density than water, such as polyethylene and polypropylene, from resin substrates having a higher density than water, such as polyester, nylon and cellophane. The density liquid may be appropriately adjusted by blending an organic solvent, an aqueous solution of a metal salt compound, or the like, either alone or in combination. Such density separation may be performed multiple times. The recovered plastic substrates are reused after being subjected to processes such as dehydration and drying, if necessary.
[0129] <Recycling resin substrates> [Process for melting and kneading the recovered plastic base material] The plastic base material is recovered by the above-mentioned separation and recovery method. The resin substrate thus obtained can be melt-kneaded to produce a molding material. The melt-kneading process refers to adding various additives as necessary, mixing with a Henschel mixer, tumbler, disperser, etc., and then mixing and dispersing using a batch type kneader such as a kneader, roll mill, super mixer, Henschel mixer, Shugi mixer, vertical granulator, high-speed mixer, Farmatrix, ball mill, steel mill, sand mill, vibration mill, attritor, Banbury mixer, twin-screw extruder, single-screw extruder, rotor-type twin-screw kneader, etc. This results in a recycled resin, which is a resin composition. The shape of the recycled resin is not particularly limited, and may be pellet-shaped, powder-shaped, granular, or bead-shaped. The melt-kneading process is preferably performed using a twin-screw extruder. Recovered plastic substrates may also be used to produce masterbatches.
[0130] The molding material may further contain a master batch or a plastic other than recycled plastic. The master batch is not particularly limited as long as it is compatible with the recycled resin, and generally, a mixture of a thermoplastic resin such as a polyethylene resin or a polypropylene resin and a colorant can be used. The thermoplastic resin contained in the master batch may be used alone or in combination of two or more kinds. The master batch may contain, within the scope not impairing the effects of the present invention, a metallic soap of an alkali metal, an alkaline earth metal, or zinc, hydrotalcite, a nonionic surfactant, a cationic surfactant, an anionic surfactant, an amphoteric surfactant, an antistatic agent, a flame retardant such as a halogen-based, phosphorus-based, or metal oxide, a lubricant such as ethylene bis alkyl amide, an antioxidant, an ultraviolet absorber, or a filler.
[0131] [Thermal molding process] The molding material obtained as described above can be heated and molded to obtain a molded article. The heating and molding method is not particularly limited, and examples thereof include injection molding, extrusion molding, blow molding, and compression molding. Molding materials produced using plastic base materials recovered by the separation and recovery method of the present invention have excellent releasability because the cross sections of the fluff are not blocked, and therefore have reduced amounts of adhering components and are of high quality. They can be used in a variety of fields, including home appliances, stationery, automobile parts, toys, sporting goods, medical materials, and building and construction materials. EXAMPLES
[0132] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts and % represent parts by mass and % by mass unless otherwise noted.
[0133] <Molecular weight and molecular weight distribution> The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) were measured by GPC (gel permeation chromatography) and calculated as molecular weights using polystyrene as a standard substance. The measurement conditions are shown below. GPC equipment: Showa Denko Shodex GPC-104 Columns: The following columns were used in series connection: Showa Denko Shodex LF-404 x 2 Showa Denko Shodex LF-G Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 0.3mL / min
[0134] <Acid value> The acid value was measured according to the method described in JIS K 0070 (1992).
[0135] <Production of primer composition and resin for printing ink> [Synthesis Example 1-1] (Polyurethane Resin P1) In a reactor equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer, while introducing nitrogen gas, 152.2 parts of PPA (a polyester polyol composed of a polycondensation product of propylene glycol and adipic acid and having a number average molecular weight of 2,000), 15.2 parts of PPG (a polyether polyol composed of polypropylene glycol and having a number average molecular weight of 2,000), 13.6 parts of BD (1,4-butanediol), 99.8 parts of IPDI (isophorone diisocyanate), and 200 parts of NPAC (normal propyl acetate) were charged and reacted at 90°C for 5 hours to obtain a urethane prepolymer solution having an isocyanate group at the end. Next, a mixture of 19.2 parts of AEA (2-(2-aminoethylamino)ethanol) and 350 parts of IPA (isopropyl alcohol) was added dropwise at room temperature over 60 minutes, and then reacted at 70°C for 3 hours to obtain a polyurethane resin solution. NPAC was added to the resulting polyurethane resin solution to adjust the solid content, thereby obtaining a solution of polyurethane resin P1 having a solid content concentration of 30%, a weight average molecular weight of 27,000, Mw / Mn=3.1 and an acid value of 0.0 mgKOH / g.
[0136] [Synthesis Example 1-2] (Polyurethane Resin P2) In a reactor equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer, 135.7 parts of PPA, 13.6 parts of PPG, 28.3 parts of DMPA (2,2-dimethylolpropanoic acid), 105.7 parts of IPDI, and 200 parts of NPAC were charged while introducing nitrogen gas, and the mixture was reacted at 90°C for 5 hours to obtain a urethane prepolymer solution having an isocyanate group at its end. Next, a mixture of 16.7 parts of AEA and 350 parts of IPA was added dropwise at room temperature over 60 minutes, and then the mixture was reacted at 70° C. for 3 hours to obtain a polyurethane resin solution. NPAC was added to the resulting polyurethane resin solution to adjust the solid content, thereby obtaining a solution of polyurethane resin P2 having a solid content concentration of 30%, a weight average molecular weight of 30,000, Mw / Mn=3.0 and an acid value of 39.3 mgKOH / g.
[0137] <Production of primer layer-forming composition> [Production Example 1-1] (Primer composition S1) 87 parts of polyurethane resin P2 solution, 5 parts of ethyl acetate (EA), 5 parts of IPA, and 3 parts of silica particles (P-73 manufactured by Mizusawa Chemical Industries, Ltd.: hydrophilic silica particles having an average particle size of 3.8 μm) were mixed and stirred using a disper to obtain primer composition S1.
[0138] <Printing ink manufacturing> [Production Example 2-1] (Printing ink R1) 10 parts of indigo pigment PB15 (CI Pigment Blue 15), 0.2 parts of BYK-SYNERGIST2100 (pigment derivative, manufactured by BYK Japan), 0.5 parts of DISPER BYK-142 (resin type dispersant, manufactured by BYK Japan), 24.3 parts of polyurethane resin P1 solution, 5 parts of PVC solution (vinyl chloride-vinyl acetate copolymer resin solution (Nissin Chemical Solvine TAO, solid content 30%, EA solution)), 10 parts of EA, and 10 parts of IPA were mixed and stirred, and dispersed for 20 minutes using a sand mill as a bead mill. Then, 20 parts of polyurethane resin P1 solution, 10 parts of EA, and 10 parts of IPA were mixed and stirred to obtain printing ink R1.
[0139] [Production Example 2-2] (Printing ink R2) 10 parts of indigo pigment PB15, 0.2 parts of BYK-SYNERGIST 2100, 0.5 parts of DISPER BYK-142, polyurethane 24.3 parts of polyurethane resin P2 solution, 5 parts of PVC solution, 10 parts of EA, and 10 parts of IPA were mixed and stirred, and dispersed for 20 minutes using a sand mill as a bead mill. Then, 20 parts of polyurethane resin P2 solution, 10 parts of EA, and 10 parts of IPA were mixed and stirred to obtain printing ink R2.
[0140] <Production of polyols used in adhesives> [Synthesis Example 2-1] (Polyester polyol B1) In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank and a nitrogen gas inlet tube, 124 parts of ethylene glycol, 212 parts of neopentyl glycol, 368 parts of 1,6-hexanediol, 645 parts of isophthalic acid, 36 parts of adipic acid and 265 parts of sebacic acid were charged, and the mixture was heated to 250°C while stirring under a nitrogen stream to carry out an esterification reaction. After a predetermined amount of water was distilled and the reaction was continued until the acid value was 5 or less, the pressure was gradually reduced and a deglycolization reaction was carried out at 1 mmHg or less for 5 hours to obtain a polyester polyol. Then, 35 parts of isophorone diisocyanate was gradually added, and the reaction was carried out at 150°C for about 2 hours to obtain a polyester polyurethane polyol. 12.0 parts of ethylene glycol bis-anhydrotrimellitate were added to 100 parts of this polyester polyurethane polyol and reacted at 180°C for approximately 2 hours. The mixture was then diluted with EA until the solids concentration reached 50%, yielding a solution of partially acid-modified polyester polyol B1 with a number average molecular weight of 9,000 and an acid value of 30.3 mgKOH / g.
[0141] [Synthesis Example 2-2] (Polyester polyol B2) A reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank and a nitrogen gas inlet tube was charged with 58 parts of ethylene glycol, 412 parts of diethylene glycol, 343 parts of neopentyl glycol, 517 parts of isophthalic acid and 393 parts of adipic acid, and the mixture was heated to 250 ° C. while stirring under a nitrogen stream to carry out an esterification reaction. After a predetermined amount of water was distilled and the reaction was continued until the acid value was 5 or less, the pressure was gradually reduced and a deglycolization reaction was carried out at 1 mmHg or less for 5 hours to obtain a polyester polyol. 4.0 parts of trimellitic anhydride were added to 100 parts of this polyester polyol, and the reaction was carried out at 180 ° C. for about 2 hours, and then diluted with EA until the solid content concentration was 50%, to obtain a solution of partially acid-modified polyester polyol B2 with a number average molecular weight of 2,000 and an acid value of 23.5 mg KOH / g.
[0142] [Synthesis Example 2-3] (Polyester polyol B3) A reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank and a nitrogen gas inlet tube was charged with 188 parts of ethylene glycol, 316 parts of neopentyl glycol, 179 parts of 1,6-hexanediol, 315 parts of terephthalic acid, 315 parts of isophthalic acid, 64 parts of adipic acid and 323 parts of sebacic acid, and the mixture was heated to 250°C while stirring under a nitrogen stream to carry out an esterification reaction. After a predetermined amount of water was distilled and the reaction was continued until the acid value was 5 or less, the pressure was gradually reduced and a deglycolization reaction was carried out at 1 mmHg or less for 5 hours to obtain a polyester polyol. Then, 8.5 parts of isophorone diisocyanate was gradually added, and the reaction was carried out at 150°C for about 2 hours, and then diluted with EA until the solid content concentration was 50%, to obtain a solution of partially acid-modified polyester polyol B3 with a number average molecular weight of 7,500 and an acid value of 0 mgKOH / g.
[0143] <Adjustment of polyisocyanate> [Preparation Example 1] (Polyisocyanate C1) Coronate 2785 (biuret type polyisocyanate derived from hexamethylene diisocyanate, manufactured by Tosoh Corporation) was diluted with EA to adjust the solid concentration to 50% and NCO% to 9.6%, to obtain a solution of polyisocyanate C1.
[0144] <Adhesive manufacturing> [Manufacturing Example 3-1] (Adhesive D1) 90 parts of polyester polyol B1 solution, 10 parts of polyester polyol B2 solution , 8 parts of polyisocyanate C1 solution was mixed, and EA was added to prepare an adhesive solution with a solids concentration of 30%.
[0145] [Manufacturing Example 3-2] (Adhesive D2) 100 parts of the polyester polyol B3 solution and 8 parts of the polyisocyanate C1 solution were mixed, and EA was added thereto to prepare an adhesive solution with a solids concentration of 30%.
[0146] <Manufacture of Laminate> The manufacturing method of the laminate is described below. The primer composition and the printing ink were each diluted with a mixed solvent of EA / IPA (mass ratio 70 / 30) to a viscosity of 15 seconds (25°C, Zahn cup #3 (manufactured by Rigo Co., Ltd.) before use. The thickness of the primer layer and the printing layer were each adjusted to about 1.5 μm.
[0147] [Manufacturing Example 4-1] (Laminate L1) The diluted primer composition S1 and printing ink R1 were printed in that order onto OPP (corona-treated stretched polypropylene film, thickness 20 μm) using a gravure printing machine equipped with a gravure plate with a plate depth of 30 μm, and dried at 50°C to obtain a laminate L1 having a structure of base layer (OPP) / primer layer (S1) / printing layer (R1).
[0148] [Manufacturing Example 4-2] (Laminate L2) The diluted printing ink R2 was printed onto the OPP using a gravure printing machine equipped with a gravure plate with a plate depth of 30 μm, and dried at 50° C. to obtain a laminate L2 having a structure of base layer (OPP) / printed layer (R2).
[0149] [Manufacturing Example 4-3] (Laminate L3) The diluted printing ink R1 was printed onto anti-fog OPP (anti-fog treated stretched polypropylene film, thickness 20 μm) using a gravure printing machine equipped with a gravure plate with a plate depth of 30 μm, and dried at 50°C to obtain a laminate L3 having a structure of base layer (anti-fog OPP) / printing layer (R1).
[0150] [Manufacturing Example 4-4] (Laminate L4) The diluted primer composition S1 and printing ink R1 were printed in that order onto the OPP using a gravure printing machine equipped with a gravure plate with a plate depth of 30 μm, and then dried at 50° C. to obtain a laminate having a structure of OPP / S1 / R1. Next, adhesive D1 was applied and dried using a dry laminator onto the printed layer of the obtained laminate so that the film thickness after drying would be approximately 3 μm, and then it was laminated with CPP (unstretched polypropylene film, thickness 30 μm) to obtain a laminate L4 having a structure of base layer (OPP) / primer layer (S1) / printed layer (R1) / adhesive layer (D1) / base layer (CPP).
[0151] [Manufacturing Example 4-5] (Laminate L5) Adhesive D1 was applied to the OPP using a dry laminator so that the film thickness after drying would be approximately 3 μm, and then dried. The OPP was then bonded to the CPP to obtain a laminate L5 having a structure of base layer (OPP) / adhesive layer (D1) / base layer (CPP).
[0152] [Manufacturing example 4-6] (laminate L6) Diluted printing ink R1 was printed on NY (stretched nylon film, thickness 15 μm) using a gravure printing machine equipped with a gravure plate with a plate depth of 30 μm, and dried at 50°C to obtain a laminate having a configuration of NY / R1. Next, adhesive D1 was applied to the printed layer of the obtained laminate using a dry laminator, and dried so that the film thickness after drying would be approximately 3 μm, and then the laminate was laminated with LLDPE (unstretched linear low density polyethylene film, thickness 130 μm). A laminate L6 having a structure of substrate layer (NY) / printed layer (R1) / adhesive layer (D1) / substrate layer (LLDPE) was obtained.
[0153] [Manufacturing Example 4-7] (Laminate L7) The diluted primer composition S1 and printing ink R1 were printed in that order onto the OPP using a gravure printing machine equipped with a gravure plate with a plate depth of 30 μm, and then dried at 50° C. to obtain a laminate having a structure of OPP / S1 / R1. Next, adhesive D2 was applied and dried using a dry laminator onto the printed layer of the obtained laminate so that the film thickness after drying would be approximately 3 μm, and then it was bonded to VMCPP (aluminum-vapor-deposited unoriented polypropylene film, thickness 25 μm) to obtain a laminate L7 having a structure of base layer (OPP) / primer layer (S1) / printed layer (R1) / adhesive layer (D2) / base layer (VMCPP).
[0154] [Table 1]
[0155] The abbreviations in Table 1 are as follows: OPP: Corona-treated oriented polypropylene film, thickness 20 μm CPP: Non-oriented polypropylene film, thickness 50 μm Anti-fog OPP: Anti-fog treated oriented polypropylene film, thickness 20μm NY: oriented nylon film, thickness 15 μm LLDPE: Unstretched linear low density polyethylene film, thickness 130 μm VMCPP: Aluminum-coated non-oriented polypropylene film, thickness 25 μm
[0156] <Crushing the laminate and creating fluff> [Production Example 5-1] (Fluff F1) The laminate L1 was crushed using a wet crushing device (a cutter mill equipped with a circular screen with a diameter of 3 mm) [crusher A] manufactured by Nippon Seam while flowing in water at 20°C, to obtain fluff F1 with an average size of 3 mm.
[0157] [Manufacturing Examples 5-2 to 9, 19] (Fluff F2 to 9, 19) Except for changing the laminate to one shown in Table 2, the laminate was crushed using the same equipment and method as in Production Example 5-1 to obtain fluffs F2 to 9 and 19. For F2 and F3, the screen size and the introduction speed of the laminate were adjusted so that the fluff sizes were as shown in Table 2.
[0158] [Manufacturing Example 5-10] (Fluff F10) The fluff F1 crushed in Production Example 5-1 was crushed using a fine grinding device (a disc mill equipped with a cooling mechanism) [Crushing device B] manufactured by Nippon Coke & Co., Ltd., while cooling the grinding blades with cooling water at -10°C, to obtain fluff F10 with an average size of 0.5 mm.
[0159] [Manufacturing Examples 5-11~18] (Fluff F11~18) Fluff was crushed using the same equipment and method as in Production Example 5-10 to obtain fluffs F11 to 18, except that the fluff used for crushing was changed to the fluff shown in Table 2. For F11 and F12, the rotation speed and gap of the rotary blade were adjusted so that the size of the fluff after crushing became the value shown in Table 2.
[0160] [Manufacturing Example 5-20] (Fluff F20) The fluff F1 crushed in Production Example 5-1 was crushed under a liquid nitrogen atmosphere (-196°C) using a fine crushing device (freezing crushing cryomill) manufactured by Retsch [Crushing Device C] to obtain fluff F20 having an average size of 0.4 mm.
[0161] [Manufacturing Examples 5-21~28] (Fluff F21~28) Fluff was pulverized using the same equipment and method as in Production Example 5-20, except that the fluff used for pulverization was changed to the fluff shown in Table 2, to obtain fluffs F21 to 28. For F21 and F22, the shaking number and pulverization time were adjusted so that the size of the pulverized fluff became the value shown in Table 2.
[0162] [Table 2]
[0163] <Production of the desorption solution> [Production Example 6-1] (Elution Solution A1) 2 parts of sodium hydroxide, 0.4 parts of polyoxyethylene lauryl ether (HLB; 13.6), 0.004 parts of BYK-1650 (manufactured by BYK Japan, silicone-based emulsion type defoamer, solid content concentration 27.5%), and 97.6 parts of water were mixed and stirred with a disperser to obtain a release liquid A1.
[0164] <Separation and recovery of laminates and production of recycled film> [Example 1] 200g of the release solution A1 and 40g of the fluff F1 were placed in a 500mL stainless steel beaker and stirred for 10 minutes at 70°C and 2000 rpm to separate the laminate and remove the printed layer. After that, the mixture was left to stand for 30 minutes, and the fluff floating to the top was collected and washed. The collected fluff was then extruded at 200°C using a single-screw extruder and pelletized to obtain pellets of the recycled resin. The recycled resin was extruded at 200°C using a T-die film molding machine to produce a recycled film with a thickness of 30 μm. The following evaluations were performed on the obtained recycled film.
[0165] [Examples 2 to 31, Comparative Examples 1 to 3] The laminate was separated and recovered, and a recycled film was produced and evaluated in the same manner as in Example 1, except that the type of fluff and the amount of fluff blended at the time of removal were changed to those shown in Table 3. In Comparative Example 3, the removal step was not performed, and the fluff was pelletized to produce a recycled film. In Examples 6, 7, 9, 15, 16, 18-20, 26, 27, and 29-31, Substrate 1 and Substrate 2 were detached, but they were not distinguished and were collected together for the recycled film evaluation. In Examples 8, 17, and 28, the nylon film of Substrate 1 did not float to the top layer and was not collected, and only the polyethylene film of Substrate 2 was collected and the recycled film evaluation was performed.
[0166] <Evaluation of recycled film> (transmittance) Regarding the coloration of the recycled film, the total light transmittance was measured using a haze meter (SH7000, manufactured by Nippon Denshi Kogyo Co., Ltd.) and evaluated according to the following criteria. A (Excellent): Total light transmittance is 80% or more. B (Good): Total light transmittance is 60% or more but less than 80%. C (Acceptable): Total light transmittance is 40% or more but less than 60%. D (unacceptable): Total light transmittance is less than 40%
[0167] (Tensile strength) Test pieces 15 mm wide and 150 mm long were taken from the recycled film in both the machine direction (MD) and the transverse direction (TD). In accordance with JIS K 7127, they were stretched at a chuck distance of 50 mm and a tensile speed of 200 mm / min. The strength (stress) at the maximum elongation was measured in both the MD and TD, and the larger value was evaluated according to the following criteria. A (Excellent): Tensile strength is 35 MPa or more. B (Good): Tensile strength is 25 MPa or more and less than 35 MPa. C (Acceptable): Tensile strength is 15 MPa or more but less than 25 MPa. D (Not acceptable): Tensile strength is less than 15MPa Examples 8 and 17 were evaluated according to the following criteria. A (Excellent): Tensile strength is 12 MPa or more. B (Good): Tensile strength is 7 MPa or more and less than 12 MPa. C (Acceptable): Tensile strength is 2MPa or more but less than 7MPa. D (Not acceptable): Tensile strength is less than 2MPa
[0168] [Table 3]
[0169] The above evaluation results show that with the separation and recovery method of the present invention, since the fluff size is small, the coating layer can be easily detached from a large amount of laminates in a short period of time, resulting in a high-quality plastic substrate with little re-adhesion of the coating layer, and furthermore, since the fluff is uniformly incorporated during melt-kneading, a high-quality molding material with little discoloration can be obtained.
Claims
1. A step of crushing a laminate comprising at least a plastic substrate and a coating layer in contact with the plastic substrate into fluffs having an average size of 5 mm or less; A method for separating and recovering a laminate, comprising a step of contacting the crushed fluff with a release liquid to release the coating layer from the plastic substrate, A method for separating and recovering a laminate, wherein the content of the laminate is 10 mass% or more based on the total mass of the elution liquid.
2. 2. The method for separating and recovering a laminate according to claim 1, further comprising a step of pulverizing the material into fluff having an average size of 1 mm or less after the crushing step.
3. 3. The method for separating and recovering a laminate according to claim 2, wherein the pulverizing step is carried out under cooling means.
4. 4. The method for separating and recovering a laminate according to claim 3, wherein the pulverizing step is carried out under cooling means using a cryogen at 0° C. or lower.
5. The method for separating and recovering a laminate according to claim 1 , wherein the plastic substrate comprises a polyolefin.
6. The method for separating and recovering a laminate according to claim 1 , wherein the plastic substrate is a plastic film.
7. The method for separating and recovering a laminate according to claim 1 , wherein the elution liquid contains water and a surfactant.
8. A method for producing a molding material, comprising a step of melt-kneading the plastic substrate recovered by the method for separating and recovering a laminate according to any one of claims 1 to 7.
9. A method for producing a molded article, further comprising a step of hot-molding the molding material obtained by the method according to claim 8.
Citation Information
Patent Citations
Laminate adhesive having detachment property from composite film, laminate, and recycling method of sheet-like substrate
JP2020084130A
Organic solvent-based printing ink, printed material, and laminate
JP2020090627A
Packaging material, and recycled base material production method
JP2021098294A
Cited By
Method for cleaning printed materials and method for producing recycled materials
JP2026177937A
Method for cleaning printed materials and method for producing recycled materials
JP2026179591A
Method for cleaning printed matter and method for producing recycled materials
JP7816614B1