Low-dielectric resin composition and cured product thereof

A low dielectric resin composition with a siloxane compound and reduced ionic content addresses the high dielectric issues of epoxy-modified silicone resins, enabling effective high-frequency transmission by reducing dielectric constant and loss tangent.

JP2024153747AActive Publication Date: 2024-10-29SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024119291
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-26
Filing Date
2024-07-25
Publication Date
2024-10-29
Estimated Expiration
2041-04-14

AI Technical Summary

Technical Problem

Epoxy-modified silicone resins exhibit high dielectric constants and loss tangents, making them unsuitable for high-frequency applications due to significant transmission loss, and low-molecular-weight oligosiloxanes result in uncured resin compositions.

Method used

A siloxane compound with an ionic substance content less than 0.001% by mass, specifically designed to reduce the dielectric constant and loss tangent, is incorporated into a resin composition, using a hydrosilylation reaction with a platinum catalyst to form a low dielectric resin.

Benefits of technology

The resulting resin composition achieves a dielectric constant of 4.0ε or less and a dielectric loss tangent of 0.002 tan δ or less, suitable for high-frequency applications in the information and communication field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153747000001
    Figure 2024153747000001
  • Figure 2024153747000002
    Figure 2024153747000002
  • Figure 2024153747000003
    Figure 2024153747000003
Patent Text Reader

Abstract

To provide a low-dielectric resin composition including a dielectric property-lowering agent composed of an epoxy-modified silicone resin with a low relative dielectric constant and low dielectric loss tangent.SOLUTION: A low-dielectric resin composition includes: a dielectric property-lowering agent composed of a siloxane compound represented by general formula (1), with the content of an ionic substance being less than 0.001 mass%, where the ionic substance is at least one selected from fluoride ions, chloride ions, bromide ions and iodide ions; and a resin. In the formula (1), each group is as defined in the specifications, and a, b, c, d, and e are each an integer ranging from 0 to 1, fulfilling the conditions 1≤a+b+c≤3 and 1≤a+b+c+d+e≤5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a low dielectric resin composition and a cured product thereof. [Background technology]

[0002] Thermosetting resins such as urethane resins, epoxy resins, silicone resins, urea resins, phenolic resins, unsaturated polyester resins, and melamine resins form crosslinked structures by heating alone or in the presence of a curing agent, to give infusible and insoluble resin compositions with three-dimensional network structures. These resin compositions have excellent properties such as interface properties, mechanical properties, insulation properties, adhesive properties, adhesion, weather resistance, impact resistance, corrosion resistance, water resistance, heat resistance, abrasion resistance, and chemical resistance, and are used in a wide range of fields and applications such as laminating agents, adhesives, sealants, insulating films, paints, medical materials, building materials, molding materials, automotive materials, fiber materials, and electronic materials.

[0003] Among the above-mentioned thermosetting resins, the epoxy-modified silicone resin has an epoxy group and a siloxane structure, and therefore, when used, it is possible to improve a number of properties of the resin composition, such as the interfacial properties, insulating properties, adhesive properties, and heat resistance. Known examples of such epoxy-modified silicone resins include bis[(3,4-epoxycyclohexyl)ethyl]polydimethylsiloxane and tetrakis[(3,4-epoxycyclohexyl)ethyl]tetramethylcyclotetrasiloxane (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-9086 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, in the field of information and communications, there has been a dramatic demand for ultra-high-speed communication speeds due to the increase in the amount of information, simultaneous connection of a large number of devices due to the diversification of information, and ultra-low latency for remote operation, and technology is needed to process large volumes of electrical signals at high speed. In response to this demand, technology is being introduced that increases the amount of electrical signals transmitted per unit time in transmission paths by using higher frequency bands than the current frequencies.

[0006] On the other hand, in high frequency bands, there is a problem of transmission loss, where the strength of the electrical signal is easily attenuated and delayed. Transmission loss is affected by conductor loss in the conductor parts of the electronic material that forms the transmission path, and dielectric loss in the resin parts, but in high frequency bands, the effect of dielectric loss becomes dominant. Dielectric loss is the loss that changes to heat when an electrical signal flows through a resin part, and is expressed by the formula D=kf√εr·tanδ (D: dielectric loss, k: proportionality constant, f: frequency, εr: relative dielectric constant, tanδ: dielectric loss tangent), and is proportional to the relative dielectric constant and dielectric loss tangent of the resin. Therefore, in the above-mentioned information and communication field, there is a need for technology to control the relative dielectric constant and dielectric loss tangent of resins used in high frequency bands.

[0007] However, the epoxy-modified silicone resin described in Patent Document 1 has a high relative dielectric constant and dielectric loss tangent due to the high polarity of the epoxy group, making it difficult to apply it to high frequency bands. That is, when the siloxane structure of the epoxy-modified silicone resin is a low molecular weight oligosiloxane, the resin composition using this has a high ratio of epoxy groups in the molecule, and has a high relative dielectric constant and dielectric loss tangent, resulting in large transmission loss.When the siloxane structure is a high molecular weight polydimethylsiloxane, the resin composition is in a high viscosity oil state, which causes problems such as not curing. Therefore, there has been a demand for the development of an epoxy-modified silicone resin having a low relative dielectric constant and dielectric tangent, and further for the development of a low dielectric resin composition cured using the same.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a low dielectric resin composition containing a dielectric reducing agent made of an epoxy-modified silicone resin having a low relative dielectric constant and dielectric tangent, and a cured product thereof. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted extensive research to achieve the above object, and as a result have found that a siloxane compound represented by the following general formula (1) is an epoxy-modified silicone resin having a low dielectric constant and dielectric dissipation factor, and that when the content of an ionic substance in the siloxane compound is less than 0.001 mass%, the dielectric constant and dielectric dissipation factor of a resin composition cured using the siloxane compound decrease, thereby completing the invention.

[0010] That is, the present invention provides 1. A low dielectric resin composition comprising a resin and a dielectric reducing agent which is made of a siloxane compound represented by the following general formula (1), the content of an ionic substance being less than 0.001 mass %, the ionic substance being one or more selected from the group consisting of fluoride ions, chloride ions, bromide ions and iodide ions; [ka] [In the formula, R 1 are each independently represented by the following general formula (2): [ka] (In the formula, R 4 each independently represents an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms. represents a group represented by R 2 are each independently represented by the following general formula (3) or (4): [ka] (In the formula, R 5 represents a substituted or unsubstituted linear, branched or cyclic alkylene group having 1 to 10 carbon atoms. represents a group represented by R 3 each independently represents a hydrogen atom, an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, or a group represented by the following general formula (5): [ka] (In the formula, R 1 , R 4 and R 5 has the same meaning as above, and f represents an integer of 0 to 10. represents a group represented by a, b, c, d, and e are each independently an integer ranging from 0 to 1, and satisfying 1≦a+b+c≦3 and 1≦a+b+c+d+e≦5. 2. The low dielectric resin composition according to claim 1, further comprising a curing agent. 3. The low dielectric resin composition according to 1 or 2, wherein the dielectric constant of the dielectric constant reducing agent is 4.0 ε or less at a frequency of 1 MHz. 4. The low dielectric resin composition according to 1 or 2, wherein the dielectric tangent of the dielectric reducing agent is 0.002 tan δ or less at a frequency of 1 MHz. 5. The low dielectric resin composition according to 1 or 2, wherein the resin is a thermosetting resin or a thermoplastic resin. 6. The low dielectric resin composition according to 5, wherein the thermosetting resin is a urethane resin, an epoxy resin, a silicone resin, a urea resin, a phenol resin, an unsaturated polyester resin or a melamine resin. 7. The low dielectric resin composition according to 5, wherein the thermoplastic resin is an acrylic resin, a polyamide resin, a polyimide resin, a polyurethane resin, a polyester resin, a polyvinyl chloride resin, a polycarbonate resin, a polyvinyl acetate resin or a polystyrene resin. 8. Cured product of the low dielectric resin composition of 1 or 2 to provide. Effect of the Invention

[0011] The dielectric constant reducing agent used in the present invention is made of a specific siloxane compound and has a low content of ionic substances, and has a low relative dielectric constant and dielectric dissipation factor, and can reduce the relative dielectric constant and dielectric dissipation factor of a resin composition cured using this agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be specifically described below. [1] Low dielectric constant agents The dielectric lowing agent of the present invention comprises a siloxane compound represented by the following general formula (1) and has an ionic substance content of less than 0.001% by mass.

[0013] [ka]

[0014] In the general formula (1), R 1 each independently represents a group represented by the following general formula (2).

[0015] [ka]

[0016] In the general formula (2), R 4 each independently represents an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, and more preferably 1 to 6 carbon atoms. The monovalent hydrocarbon group may be linear, branched or cyclic, and specific examples thereof include linear alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl and n-decyl groups; branched alkyl groups such as isopropyl, sec-butyl, tert-butyl, sec-pentyl, tert-pentyl, sec-hexyl, tert-hexyl, sec-heptyl, tert-heptyl, sec-octyl, tert-octyl, sec-nonyl, tert-nonyl, sec-decyl and tert-decyl groups; cyclic alkyl groups such as cyclopentyl and cyclohexyl groups; alkenyl groups such as vinyl, allyl, butenyl and methallyl groups; aryl groups such as phenyl, tolyl and xylyl groups; and aralkyl groups such as benzyl and phenethyl groups. Among these, R 4As the group, an unsubstituted linear, branched or cyclic alkyl group having 1 to 6 carbon atoms; an alkenyl group; an aryl group; or an aralkyl group is preferable, and from the viewpoint of easy availability of the precursor raw material in particular, an unsubstituted linear or branched alkyl group having 1 to 3 carbon atoms; an alkenyl group is more preferable, and a methyl group, an ethyl group, an n-propyl group, or an isopropyl group is even more preferable.

[0017] In the general formula (1), R 2 each independently represents a group represented by the following general formula (3) or (4).

[0018] [ka]

[0019] In the general formula (3) and the general formula (4), R 5 represents a substituted or unsubstituted alkylene group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, and more preferably 1 to 6 carbon atoms. The alkylene group may be linear, branched, or cyclic, and specific examples thereof include linear alkylene groups such as methylene, ethylene, trimethylene, tetramethylene, pentamethylene, hexamethylene, heptamethylene, and octamethylene; branched alkylene groups such as isopropylene, sec-butylene, tert-butylene, sec-pentylene, tert-pentylene, sec-hexylene, tert-hexylene, sec-heptylene, tert-heptylene, sec-octylene, and tert-octylene; and cyclic alkylene groups such as cyclopropylene, cyclopentylene, and cyclohexylene.

[0020] In addition, a part or all of the hydrogen atoms of these alkylene groups may be substituted with other substituents, and specific examples of the substituents include alkoxy groups having 1 to 3 carbon atoms such as methoxy, ethoxy, and (iso)propoxy groups; halogen atoms such as fluorine, chlorine, and bromine; aromatic hydrocarbon groups such as phenyl groups; cyano groups, amino groups, ester groups, ether groups, carbonyl groups, acyl groups, and sulfide groups, and one or more of these may be used in combination. The substitution positions of these substituents are not particularly limited, and the number of substituents is also not limited. Furthermore, these alkylene groups may have one or more of ether groups, ester groups, carbonyl groups, sulfide groups, disulfide groups, etc. present in the molecular chain. Among these, R 5 As the alkyl group, an unsubstituted linear alkylene group having 1 to 8 carbon atoms is preferable, and from the viewpoint of easy availability of precursor materials, an unsubstituted linear alkylene group having 1 to 4 carbon atoms such as a methylene group or an ethylene group is more preferable.

[0021] In the general formula (1), R 3 each independently represents a hydrogen atom, an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, and more preferably 1 to 6 carbon atoms, or a group represented by the following general formula (5).

[0022] [ka]

[0023] In the general formula (5), R 1 , R 4 and R 5 The substituents include the same ones as those exemplified above. Furthermore, f is an integer of 0 to 10, but is preferably an integer of 0 to 3, and more preferably 0, particularly from the viewpoint of easy availability of precursor materials.

[0024] Among these, R 3As the group, an unsubstituted linear, branched or cyclic alkyl group having 1 to 6 carbon atoms; an alkenyl group; an aryl group; or an aralkyl group is preferable, and from the viewpoint of easy availability of the precursor raw material in particular, an unsubstituted linear or branched alkyl group having 1 to 3 carbon atoms; an alkenyl group is more preferable, and a methyl group, an ethyl group, an n-propyl group, or an isopropyl group is even more preferable.

[0025] In general formula (1), a, b, c, d, and e are each independently an integer of 0 to 1 that satisfies 1≦a+b+c≦3, 1≦a+b+c+d+e≦5. In particular, from the viewpoint of decreasing the relative dielectric constant and the dielectric loss tangent, the conditions of 1≦a+b+c≦1.1, 1≦a+b+c+d+e≦5 are more preferable.

[0026] In the general formula (1), R 1 and R 2 The combination of OR is favorable from the viewpoint of decreasing the relative dielectric constant and dielectric loss tangent. 1 The silicon atom to which is bonded is R 2 is preferably in the range of 2 to 59 mol, more preferably 3 to 59 mol, and even more preferably 4 to 59 mol, relative to 1 mol of the silicon atom to which it is bonded.

[0027] The dielectric lowing agent of the present invention is usually produced by subjecting a corresponding hydrosiloxane compound and an epoxy compound having an alkenyl group to a hydrosilylation reaction in the presence of a platinum catalyst.

[0028] The hydrosiloxane compound can be appropriately selected from known siloxane compounds having a hydrogen atom in the molecule. Specific examples thereof include hexamethyltrisiloxane, heptamethyltrisiloxane, (trimethylsiloxy)hexamethyltrisiloxane, octamethyltetrasiloxane, nonamethyltetrasiloxane, (trimethylsiloxy)octamethyltetrasiloxane, decamethylpentasiloxane, undecamethylpentasiloxane, (trimethylsiloxy)decamethylpentasiloxane, dodecamethylhexasiloxane, tridecamethylhexasiloxane, (trimethylsiloxy)dodecamethylhexasiloxane, tetradecamethylheptasiloxane, pentadecamethylheptasiloxane, (trimethylsiloxy)tetradecamethylheptasiloxane, hexadecamethyloctasiloxane, heptadecamethyloctasiloxane, (trimethyl Examples of suitable siloxy compounds include (hexadecamethyloctasiloxane), (octadecamethylnonasiloxane), (nonadecamethylnonasiloxane), (trimethylsiloxy)octadecamethylnonasiloxane, eicosamethyldecasiloxane, heneicosamethyldecasiloxane, (trimethylsiloxy)eicosamethyldecasiloxane, docosamethylundecasiloxane, tricosamethylundecasiloxane, (trimethylsiloxy)docosamethylundecasiloxane, tetracosamethyldodecasiloxane, pentacosamethyldodecasiloxane, (trimethylsiloxy)tetracosamethyldodecasiloxane, hexacosamethyltridecasiloxane, heptacosamethyltridecasiloxane, and (trimethylsiloxy)hexacosamethyltridecasiloxane. In particular, from the viewpoint of easy availability of precursor materials, hexamethyltrisiloxane, heptamethyltrisiloxane, and (trimethylsiloxy)hexamethyltrisiloxane are preferred.

[0029] The epoxy compound having an alkenyl group can be appropriately selected from known compounds having an alkenyl group and an epoxy group in the molecule. Specific examples thereof include epoxy compounds having a glycidyl ether structure, such as vinyl glycidyl ether, allyl glycidyl ether, 2-methylallyl glycidyl ether, butenyl glycidyl ether, hexenyl glycidyl ether, octenyl glycidyl ether, 2-ethylhexenyl glycidyl ether, and decenyl glycidyl ether; and epoxy compounds having a cycloalkene oxide structure, such as 1,2-epoxy-4-vinylcyclohexane, 1,2-epoxy-4-allylcyclohexane, 1,2-epoxy-4-(2-methylallyl)cyclohexane, 1,2-epoxy-4-butenylcyclohexane, 1,2-epoxy-4-hexenylcyclohexane, 1,2-epoxy-4-octenylcyclohexane, and 1,2-epoxy-4-decenylcyclohexane. In particular, from the viewpoint of easy availability of precursor raw materials, epoxy compounds having a glycidyl ether structure, such as allyl glycidyl ether and octenyl glycidyl ether, and epoxy compounds having a cycloalkene oxide structure, such as 1,2-epoxy-4-vinylcyclohexane and 1,2-epoxy-4-octenylcyclohexane, are preferred.

[0030] The above-mentioned epoxy compound having an alkenyl group is usually produced by a method of reacting an epihalohydrin compound with an alcohol compound (epihalohydrin method), a method of oxidizing an olefin compound using a peracid compound (peracid compound oxidation method), or the like.

[0031] In the epihalohydrin process, an organic halogen compound is used as a raw material, so the epoxy compound produced contains ionic substances derived from the raw material, whereas in the peroxy acid oxidation process, an organic halogen compound is not used as a raw material, so the epoxy compound produced does not substantially contain ionic substances. As described above, the dielectric lowing agent of the present invention has an ionic substance content of less than 0.001 mass %. Therefore, from the viewpoint of reducing the ionic substance content, the epoxy compound having an alkenyl group is preferably one produced by a peroxy acid compound oxidation method. In addition, by reacting a hydrosiloxane compound with an epoxy compound having an alkenyl group produced by the peroxy acid oxidation method, the content of ionic substances contained in the dielectric lowing agent can be reduced.

[0032] In the method for producing a low dielectric agent of the present invention, the compounding ratio of the hydrosiloxane compound to the epoxy compound having an alkenyl group is not particularly limited, but from the viewpoints of reactivity and productivity, the amount of the hydrosiloxane compound is preferably in the range of 1 to 20 moles, more preferably 1 to 10 moles, and even more preferably 1 to 5 moles, per mole of the epoxy compound having an alkenyl group.

[0033] The platinum catalyst can be appropriately selected from known platinum (Pt) and complex compounds having platinum as the central metal. Specific examples include alcohol solutions of chloroplatinic acid such as chloroplatinic acid, a 2-ethylhexanol solution of chloroplatinic acid (IV) acid, a toluene or xylene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, dichlorobisacetonitrile platinum, dichlorobisbenzonitrile platinum, dichlorocyclooctadiene platinum, etc. Also usable are catalysts in which platinum black or the like is supported on a carrier such as alumina, silica, or carbon. In particular, from the viewpoint of high reactivity, an alcohol solution of chloroplatinic acid such as a 2-ethylhexanol solution of chloroplatinic (IV) acid, and a toluene or xylene solution of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex are preferred.

[0034] The amount of platinum catalyst used is not particularly limited as long as it is an amount that exerts a catalytic effect in the hydrosilylation reaction. From the viewpoints of reactivity and productivity, however, the amount of platinum metal used is preferably in the range of 0.0000001 to 1 mol, more preferably 0.000001 to 0.1 mol, and even more preferably 0.00001 to 0.01 mol per 1 mol of the epoxy compound having an alkenyl group.

[0035] The reaction temperature for the hydrosilylation reaction is not particularly limited, but from the viewpoints of reactivity and productivity, it is preferably in the range of 50 to 200°C, more preferably 50 to 150°C, and even more preferably 50 to 100°C. The reaction time is not particularly limited, but is preferably in the range of 1 to 30 hours, more preferably 1 to 20 hours, and even more preferably 1 to 10 hours.

[0036] The hydrosilylation reaction proceeds in the absence of a solvent, but can also be carried out in the presence of a solvent. Examples of the solvent include hydrocarbon solvents such as pentane, hexane, cyclohexane, heptane, isooctane, benzene, toluene, and xylene; ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; ester solvents such as ethyl acetate and butyl acetate; aprotic polar solvents such as acetonitrile and N,N-dimethylformamide; and chlorinated hydrocarbon solvents such as dichloromethane and chloroform. These solvents may be used alone or in combination of two or more.

[0037] The reaction liquid obtained in the above hydrosilylation reaction contains the platinum catalyst used in the reaction. The platinum catalyst contained in the reaction solution will turn black, significantly worsening the appearance of the reaction solution, and will also cause the generation of ionic substances derived from the ligands of the platinum catalyst, etc. Furthermore, if unreacted hydrosiloxane compounds remain, there is a risk of dehydrogenation. For the above reasons, it is preferable to remove the platinum catalyst contained in the reaction mixture after the hydrosilylation reaction. There are no particular limitations on the method for removing the platinum catalyst contained in the reaction solution, and treatment means such as distillation, column chromatography, washing with water, extraction, filtration, and adsorption with activated carbon or diatomaceous earth can be used.

[0038] The dielectric lowing agent of the present invention contains ionic substances derived from the above-mentioned raw materials. Specific examples of ionic substances include fluoride ions, chloride ions, bromide ions, and iodide ions. In the dielectric lowing agent of the present invention, the content of the ionic substance is less than 0.001 mass % from the viewpoint of decreasing the relative dielectric constant and the dielectric loss tangent, but is preferably in the range of 0.000001 mass % or more and less than 0.001 mass %, more preferably 0.00001 mass % or more and less than 0.001 mass %, and even more preferably 0.0001 mass % or more and less than 0.001 mass %.

[0039] The method for measuring the content of the ionic substance is not particularly limited, and analytical means such as ion chromatography, high performance liquid chromatography, potentiometric titration, and fluorescence spectrometry can be used.

[0040] [2] Low dielectric resin composition The low dielectric resin composition of the present invention contains the above-mentioned dielectric lowing agent and a resin. Specific examples of the resin include thermosetting resins such as urethane resin, epoxy resin, silicone resin, urea resin, phenol resin, unsaturated polyester resin, and melamine resin, and thermoplastic resins such as acrylic resin, polyamide resin, polyimide resin, polyurethane resin, polyester resin, polyvinyl chloride resin, polycarbonate resin, polyvinyl acetate resin, and polystyrene resin. Among these, from the viewpoint of reactivity with the dielectric reducing agent, thermosetting resins are preferred, and epoxy resin and silicone resin are more preferred.

[0041] Specific examples of urethane resins include moisture-curing urethane resins made from aromatic isocyanates such as diphenylmethane diisocyanate and toluene diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate and isophorone diisocyanate; polyol-curing urethane resins made from polyol and aromatic isocyanate or aliphatic isocyanate; and blocked urethane resins made from polyol and blocked isocyanate. These urethane resins may be used alone or in combination of two or more. Among these, particularly from the viewpoint of availability, moisture-curing urethane resin and polyol-curing urethane resin are preferred, with moisture-curing urethane resin being more preferred.

[0042] Specific examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, novolac type epoxy resins, cyclic aliphatic type epoxy resins, long-chain aliphatic type epoxy resins, heterocyclic type epoxy resins, glycidyl ester type epoxy resins, and glycidyl amine type epoxy resins. These epoxy resins may be used alone or in combination of two or more. Among these, particularly from the viewpoint of availability, bisphenol A type epoxy resins, novolac type epoxy resins, and cyclic aliphatic type epoxy resins are preferred, and bisphenol A type epoxy resins are more preferred.

[0043] Specific examples of silicone resins include amino-modified silicone, epoxy-modified silicone, carboxy-modified silicone, carbinol-modified silicone, methacryl-modified silicone, mercapto-modified silicone, and phenol-modified silicone, and these silicone resins may be used alone or in combination of two or more. Among these, amino-modified silicone, epoxy-modified silicone, and methacryl-modified silicone are preferred, particularly from the viewpoint of availability, and epoxy-modified silicone is more preferred.

[0044] Specific examples of the phenolic resin include novolac-type phenolic resin, resol-type phenolic resin, rosin-modified phenolic resin, etc., and these phenolic resins may be used alone or in combination of two or more. Among these, from the viewpoint of availability, novolac-type phenolic resin and resol-type phenolic resin are preferred, and resol-type phenolic resin is more preferred.

[0045] Specific examples of the unsaturated polyester resin include unsaturated acid type unsaturated polyester resin, aromatic saturated acid type unsaturated polyester resin, and aliphatic saturated acid type unsaturated polyester resin. These unsaturated polyester resins may be used alone or in combination of two or more. Among these, from the viewpoint of easy availability, unsaturated acid type unsaturated polyester resins and aromatic saturated acid type unsaturated polyester resins are preferred, and unsaturated acid type unsaturated polyester resins are more preferred.

[0046] The amount of the dielectric lowing agent added to the resin is preferably in the range of 0.1 to 100 mass %, more preferably 0.2 to 80 mass %, and even more preferably 0.5 to 50 mass %, relative to the resin, from the viewpoint of sufficiently lowering the relative dielectric constant and the dielectric loss tangent.

[0047] The relative dielectric constant of the dielectric lowing agent is preferably 4.0ε or less, more preferably 3.8ε or less, even more preferably 3.6ε or less at a frequency of 1 MHz, and is preferably 4.4ε or less, more preferably 4.2ε or less, even more preferably 4.0ε or less at a frequency of 1 GHz.

[0048] The dielectric tangent of the dielectric lowing agent is preferably 0.002 tan δ or less, more preferably 0.001 tan δ or less, even more preferably 0.0005 tan δ at a frequency of 1 MHz, and is preferably 0.2 tan δ or less, more preferably 0.1 tan δ or less, even more preferably 0.05 tan δ or less at a frequency of 1 GHz.

[0049] The method for measuring the relative dielectric constant and the dielectric loss tangent is not particularly limited, and analytical means such as the coaxial probe method, the transmission line method, the free space method, the cavity resonator method, the parallel plate capacitor method, the inductance measurement method, etc. can be used.

[0050] The low dielectric resin composition of the present invention can be cured by adding a known curing agent. Specific examples of the curing agent include aliphatic amine-based curing agents, aromatic amine-based curing agents, modified amine-based curing agents, isocyanate-based curing agents, blocked isocyanate-based curing agents, imidazole-based curing agents, acid anhydride-based curing agents, phenol-based curing agents, polyaminoamide-based curing agents, polymercaptan-based curing agents, cationic curing agents, and anionic curing agents. These curing agents may be used alone or in combination of two or more. Among these, particularly from the viewpoint of availability, aliphatic amine-based curing agents, aromatic amine-based curing agents, imidazole-based curing agents, acid anhydride-based curing agents, phenol-based curing agents, and polyaminoamide-based curing agents are preferred, and aliphatic amine-based curing agents, aromatic amine-based curing agents, imidazole-based curing agents, and acid anhydride-based curing agents are more preferred.

[0051] The amount of the curing agent added to the resin composition is preferably 0.2 to 2 mol, more preferably 0.5 to 1.5 mol, and even more preferably 0.8 to 1.2 mol, per mol of epoxy groups in the resin composition, from the viewpoint of sufficient curing.

[0052] Furthermore, a known curing accelerator may be added to the low dielectric resin composition of the present invention in order to accelerate the curing reaction between the resin composition and the curing agent. Specific examples of the curing accelerator include organic phosphorus compounds such as triphenylphosphine and tributylphosphine; quaternary phosphonium salts such as ethyltriphenylphosphonium bromide and tetrabutylphosphonium O,O-diethylphosphorodithioate; quaternary ammonium salts such as 1,8-diazabicyclo[5.4.0]undec-7-ene, a salt of 1,8-diazabicyclo[5.4.0]undec-7-ene with octylic acid, zinc octylate, and tetrabutylammonium bromide; imidazoles such as 2-methylimidazole and 2-ethyl-4-methylimidazole; amines such as 2,4,6-tris(dimethylaminomethyl)phenol and benzyldimethylamine; and inorganic fillers such as fused silica, crystalline silica, alumina, boron nitride, aluminum nitride, silicon nitride, magnesia, magnesium silicate, and aluminum. These curing accelerators may be used alone or in combination of two or more. Among these, from the viewpoint of easy availability, organic phosphorus compounds, quaternary ammonium salts, imidazoles, and amines are particularly preferred, with quaternary ammonium salts, imidazoles, and amines being more preferred.

[0053] The amount of the curing accelerator added to the resin composition is preferably in the range of 0.001 to 1 mass %, more preferably 0.001 to 0.5 mass %, and even more preferably 0.001 to 0.1 mass %, based on the curing agent in the resin composition, from the viewpoint of sufficient curing acceleration.

[0054] The method for curing the low dielectric resin composition of the present invention is not particularly limited as long as the resin composition is cured, and examples thereof include a method of heating a mixture of a low dielectric agent and a resin to cure it, a method of adding a curing agent and, if necessary, a curing accelerator to a mixture of a low dielectric agent and a resin to cure it, and a method of adding a mixture of a low dielectric agent and a resin to a curing agent to cure it. Examples of methods for obtaining a cured product of the resin composition include casting, injection, potting, dipping, drip coating, transfer molding, compression molding, and forming a laminate from a resin sheet or the like.

[0055] The conditions for curing the low dielectric resin composition of the present invention are not particularly limited as long as the conditions are such that the resin composition can be cured. From the viewpoint of productivity, the curing temperature is preferably in the range of 20 to 200°C, more preferably 50 to 150°C, and even more preferably 80 to 120°C. From the viewpoint of productivity, the curing time is preferably in the range of 1 to 10 hours, more preferably 1 to 5 hours, and even more preferably 1 to 3 hours, and may be appropriately set in relation to the above curing temperature.

[0056] The dielectric lowing agent of the present invention may be used as it is, but may also be used after diluting in a solvent. Specific examples of solvents include hydrocarbon solvents such as pentane, hexane, cyclohexane, heptane, isooctane, benzene, toluene, and xylene; ketone solvents such as acetone and methyl isobutyl ketone; alcohol solvents such as methyl alcohol and ethyl alcohol; ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; ester solvents such as ethyl acetate and butyl acetate; aprotic polar solvents such as acetonitrile and N,N-dimethylformamide; and chlorinated hydrocarbon solvents such as dichloromethane and chloroform. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of compatibility with the dielectric low agent, particularly preferred are hydrocarbon solvents, ketone solvents, alcohol solvents, ether solvents, and ester solvents, and more preferred are hydrocarbon solvents, ketone solvents, and alcohol solvents.

[0057] When the dielectric lowing agent of the present invention is used by diluting it in a solvent, the concentration of the siloxane compound is not particularly limited, but from the viewpoints of reactivity and productivity, the siloxane compound is preferably diluted in the above-mentioned solvent so that the concentration is in the range of 0.001 to 50 mass %, more preferably 0.1 to 50 mass %, and even more preferably 0.1 to 10 mass %.

[0058] [3] Use as a dielectric reduction method and dielectric reduction agent Since the dielectric constant and dielectric loss tangent of the present invention are epoxy-modified silicone resins having low dielectric constants and dielectric loss tangents, the dielectric constant and dielectric loss tangent of a resin composition cured using the dielectric constant lowing agent can be reduced. The low dielectric resin composition obtained by using the dielectric reducing agent of the present invention is suitable as an electronic material for use in the high frequency band in the field of information and communication. Examples of such electronic materials include optical thin films, adhesives, laminates, insulating films, anti-reflection films, sealing materials, printed wiring boards, etc. EXAMPLES

[0059] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The purity of the fraction obtained by the distillation described below is a value measured under the gas chromatography measurement conditions described below, the content of ionic substances is measured under the titration conditions described below, and the values ​​of the relative dielectric constant and dielectric loss tangent are values ​​measured by dielectric constant measurement under the conditions described below. [Gas chromatography measurement conditions] Gas chromatograph: GC-2014 (Shimadzu Corporation) Packed column: Silicone SE-30 (GL Sciences, Inc.) Detector:TCD Detector temperature: 300℃ Inlet temperature: 300℃ Heating program: 70℃ (0 min) → 10℃ / min → 300℃ (10 min) Carrier gas: Helium (50ml / min) Injection volume: 1μl [Titration conditions] Titrator: Automatic titrator COM-2000 (Hiranuma Sangyo Co., Ltd.) Titration reagent: 0.025N silver nitrate aqueous solution Titration solvent: Acetone / methanol mixed solution Method: Potentiometric titration Sample size: 2g [Conditions for measuring the dielectric constant of low-dielectric materials (parallel plate capacitor method)] LCR meter: HP4284A (Keysight Technologies, Inc.) Liquid test fixture: HP16452A (Keysight Technologies, Inc.) Measurement atmosphere: Room temperature 24℃ in air Frequency: 1MHz Standard material: Air [Conditions for measuring the dielectric constant of low-dielectric materials (coaxial probe method)] Impedance analyzer: E4991B (Keysight Technologies, Inc.) Dielectric probe kit: N1501A-101 (Keysight Technologies, Inc.) Measurement atmosphere: Room temperature 24℃ in air Frequency: 1GHz Standard materials: air, 1-butanol [Conditions for measuring the dielectric constant of resin compositions (parallel plate capacitor method)] LCR meter: E4980A (Keysight Technologies, Inc.) Dielectric test fixture: 16451B (Keysight Technologies, Inc.) Measurement atmosphere: Room temperature 25℃ in air Frequency: 1KHz, 1MHz Standard material: Air

[0060] [1] Synthesis of low dielectric constant agents [Example 1-1] Synthesis of 1,1,1,3,5,5,5-heptamethyl-3-[2-(3,4-epoxy)-cyclohexylethyl]trisiloxane A flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer was charged with 124.2 g (1.000 mol) of 1,2-epoxy-4-vinylcyclohexane and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.000010 mol as platinum atoms) and heated to 50° C. After the internal temperature stabilized, 222.5 g (1.000 mol) of 1,1,1,3,5,5,5-heptamethyltrisiloxane was added dropwise over 10 hours, and the mixture was stirred at that temperature for 2 hours. After cooling to room temperature, the resulting reaction mixture was distilled to obtain 338.7 g of a colorless, transparent fraction with a boiling point of 116-117°C / 0.2 kPa. Analysis of the resulting fraction by gas chromatography confirmed that the purity of 1,1,1,3,5,5,5-heptamethyl-3-[2-(3,4-epoxy)-cyclohexylethyl]trisiloxane was 99.9% (0.977 mol, yield 97.7%).

[0061] [Example 1-2] Synthesis of a mixture of 1,1,1,3,5,5,5-heptamethyl-3-(3-glycidyloxypropyl)trisiloxane and 1,1,1,3,5,5,5-heptamethyl-3-[1-methyl-2-(glycidyloxy)ethyl]trisiloxane A flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer was charged with 114.1 g (1.000 mol) of allyl glycidyl ether and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.000010 mol as platinum atoms) and heated to 50° C. After the internal temperature stabilized, 222.5 g (1.000 mol) of 1,1,1,3,5,5,5-heptamethyltrisiloxane was added dropwise over 10 hours, and the mixture was stirred at that temperature for 2 hours. After cooling to room temperature, the resulting reaction mixture was distilled to obtain 252.5 g of a colorless, transparent fraction having a boiling point of 105-110°C / 0.4 kPa. Analysis of the resulting fraction by gas chromatography confirmed that the purity of the mixture of 1,1,1,3,5,5,5-heptamethyl-3-[3-(glycidyloxy)propyl]trisiloxane and 1,1,1,3,5,5,5-heptamethyl-3-[1-methyl-2-(glycidyloxy)ethyl]trisiloxane was 99.9% (0.750 mol, yield 75.0%).

[0062] [Example 1-3] Synthesis of 1,1,1,5,5,5-hexamethyl-3-[2-(3,4-epoxy)-cyclohexylethyl]-3-(trimethylsiloxy)trisiloxane A flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer was charged with 124.2 g (1.000 mol) of 1,2-epoxy-4-vinylcyclohexane and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.000010 mol as platinum atoms) and heated to 50° C. After the internal temperature stabilized, 296.7 g (1.000 mol) of 1,1,1,5,5,5-hexamethyl-3-(trimethylsiloxy)trisiloxane was added dropwise over 10 hours, and the mixture was stirred at that temperature for 2 hours. After cooling to room temperature, 2.0 g of activated carbon was added to the resulting reaction mixture and stirred at that temperature for 2 hours. After stirring, the activated carbon was removed by filtration, and the mixture was concentrated under reduced pressure at 100°C / 0.1 kPa to obtain 391.4 g of a colorless, transparent solution. The resulting solution was analyzed by gas chromatography to confirm that the purity of 1,1,1,5,5,5-hexamethyl-3-[2-(3,4-epoxy)-cyclohexylethyl]-3-(trimethylsiloxy)trisiloxane was 99.9% (0.930 mol, yield 93.0%).

[0063] [Example 1-4] Synthesis of a mixture of 1,1,1,5,5,5-hexamethyl-3-(3-glycidyloxypropyl)-3-(trimethylsiloxy)trisiloxane and 1,1,1,5,5,5-hexamethyl-3-[1-methyl-2-(glycidyloxy)ethyl]-3-(trimethylsiloxy)trisiloxane A flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer was charged with 114.1 g (1.000 mol) of allyl glycidyl ether and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.000010 mol as platinum atoms) and heated to 50° C. After the internal temperature stabilized, 296.7 g (1.000 mol) of 1,1,1,5,5,5-hexamethyl-3-(trimethylsiloxy)trisiloxane was added dropwise over 10 hours, and the mixture was stirred at that temperature for 2 hours. After cooling to room temperature, 2.0 g of activated carbon was added to the resulting reaction mixture, and the mixture was stirred at that temperature for 2 hours. After stirring, the activated carbon was removed by filtration, and the mixture was concentrated under reduced pressure at 100°C / 0.1 kPa to obtain 299.9 g of a colorless, transparent solution. The resulting solution was analyzed by gas chromatography to confirm that the mixture was a mixture of 1,1,1,5,5,5-hexamethyl-3-(3-glycidyloxypropyl)-3-(trimethylsiloxy)trisiloxane and 1,1,1,5,5,5-hexamethyl-3-[1-methyl-2-(glycidyloxy)ethyl]-3-(trimethylsiloxy)trisiloxane with a purity of 99.9% (0.730 mol, yield 73.0%).

[0064] [2] Performance evaluation of low dielectric constant agents The 1,1,1,3,5,5,5-heptamethyl-3-[2-(3,4-epoxy)-cyclohexylethyl]trisiloxane obtained in Example 1-1 was titrated by potentiometric titration, and the content of ionic substances was confirmed to be 0.00005 mass%. The mixture of 1,1,1,3,5,5,5-heptamethyl-3-(3-glycidyloxypropyl)trisiloxane and 1,1,1,3,5,5,5-heptamethyl-3-[1-methyl-2-(glycidyloxy)ethyl]trisiloxane obtained in Example 1-2 was titrated using potentiometric titration, and the content of ionic substances was confirmed to be 0.00008 mass%. The 1,1,1,5,5,5-hexamethyl-3-[2-(3,4-epoxy)-cyclohexylethyl]-3-(trimethylsiloxy)trisiloxane obtained in Example 1-3 was titrated by potentiometric titration, and the content of ionic substances was confirmed to be 0.00005 mass%. The mixture of 1,1,1,5,5,5-hexamethyl-3-(3-glycidyloxypropyl)-3-(trimethylsiloxy)trisiloxane and 1,1,1,5,5,5-hexamethyl-3-[1-methyl-2-(glycidyloxy)ethyl]-3-(trimethylsiloxy)trisiloxane obtained in Example 1-4 was titrated using potentiometric titration, and the content of ionic substances was confirmed to be 0.00008 mass%. The siloxane compound obtained in Example 1-1 was subjected to dielectric constant measurement by the parallel plate capacitor method and the coaxial probe method to measure the relative dielectric constant and the dielectric loss tangent. The results are shown in Table 1.

[0065] [Table 1]

[0066] The siloxane compound obtained in Example 1-1 had 2 moles of trialkylsilyl groups per mole of silicon atoms bonded to epoxy groups, and it was confirmed that the epoxy-modified silicone resin had a low relative dielectric constant and dielectric tangent due to the effect of the excess trialkylsilyl groups.

[0067] [3] Preparation of resin composition [Example 2-1] To 100 parts by mass of bisphenol A type epoxy resin JER828 (manufactured by Mitsubishi Chemical Corporation, epoxy equivalent weight approximately 190 g / mol), 5 parts by mass of the siloxane compound obtained in Example 1-1 and 10 parts by mass of a curing agent triethylenetetramine were added at room temperature, and the mixture was heated at 100° C. for 2 hours. After cooling to room temperature, a cured resin composition was prepared.

[0068] [Example 2-2] A cured resin composition was prepared in the same manner as in Example 2-1, except that the amount of the siloxane compound was changed to 10 parts by mass.

[0069] [Comparative Example 2-1] A cured resin composition was prepared in the same manner as in Example 2-1, except that no siloxane compound was used.

[0070] [4] Performance evaluation of resin compositions The resin compositions prepared in Examples 2-1 to 2-2 and Comparative Example 2-1 were subjected to dielectric constant measurement by a parallel plate capacitor method to measure the relative dielectric constant and the dielectric loss tangent. The results are shown in Table 2.

[0071] [Table 2]

[0072] As shown in Table 2, it was confirmed that the resin compositions of Examples 2-1 and 2-2, which were cured using the siloxane compound obtained in Example 1-1, had low relative dielectric constants and low dielectric loss tangents.

Claims

1. A low dielectric resin composition comprising a resin and a low dielectric agent comprising a siloxane compound represented by the following general formula (1), the content of an ionic substance being less than 0.001 mass %, the ionic substance being one or more selected from the group consisting of fluoride ions, chloride ions, bromide ions and iodide ions: 【Chemistry 1】 [In the formula, R 1 each independently represents the following general formula (2): 【Chemistry 2】 (In the formula, R 4 each independently represents an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms. represents a group represented by R 2 each independently represents the following general formula (3) or (4): 【Chemistry 3】 (In the formula, R 5 represents a substituted or unsubstituted linear, branched or cyclic alkylene group having 1 to 10 carbon atoms. represents a group represented by R 3 each independently represents a hydrogen atom, an unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, or a group represented by the following general formula (5): 【Chemistry 4】 (In the formula, R 1 , R 4 and R 5 has the same meaning as above, and f represents an integer of 0 to 10. represents a group represented by a, b, c, d, and e each independently represent an integer of 0 to 1, and satisfy 1≦a+b+c≦3 and 1≦a+b+c+d+e≦5.]

2. The low dielectric resin composition according to claim 1, further comprising a curing agent.

3. 3. The low dielectric resin composition according to claim 1, wherein the dielectric constant of the dielectric constant reducing agent is 4.0 ε or less at a frequency of 1 MHz.

4. 3. The low dielectric resin composition according to claim 1, wherein the dielectric loss tangent of the dielectric reducing agent is 0.002 tan δ or less at a frequency of 1 MHz.

5. 3. The low dielectric resin composition according to claim 1, wherein the resin is a thermosetting resin or a thermoplastic resin.

6. 6. The low dielectric resin composition according to claim 5, wherein the thermosetting resin is a urethane resin, an epoxy resin, a silicone resin, a urea resin, a phenol resin, an unsaturated polyester resin or a melamine resin.

7. 6. The low dielectric resin composition according to claim 5, wherein the thermoplastic resin is an acrylic resin, a polyamide resin, a polyimide resin, a polyurethane resin, a polyester resin, a polyvinyl chloride resin, a polycarbonate resin, a polyvinyl acetate resin or a polystyrene resin.

8. A cured product obtained by curing the low dielectric resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Reactive siloxane

    JP1997316085A

  • Triallyl isocyanurate having high quality level, and its production

    JP1999255753A

  • Additive for epoxy resin and epoxy resin composition

    JP2007023061A

  • Anisotropic film

    JP2020084168A

  • Resin composition for sealing, electronic component device, and method for producing electronic component device