Metal layer integrated type polypropylene film

The metal layer-integrated polypropylene film addresses processing issues and enhances insulation resistance, ensuring reliable capacitors for vehicles by optimizing cumulative DC voltage, dielectric breakdown, and mechanical properties.

JP2024153836AInactive Publication Date: 2024-10-29OJI HLDG CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024124587
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Thin polypropylene films used in capacitors for vehicles face issues with processing suitability, such as wrinkles and winding misalignment during element winding, and require improved insulation resistance stability under high temperature and high voltage loads to ensure long-term reliability.

Method used

A metal layer-integrated polypropylene film is developed with specific properties, including a cumulative DC voltage of 350 to 425 V/μm, dielectric breakdown point density of 1000 pieces/m², and controlled heat shrinkage and tensile modulus, enhancing processability and insulation resistance.

Benefits of technology

The film achieves improved processability, capacitance stability, and insulation resistance under high temperature and high voltage loads, reducing the risk of thermal runaway and short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153836000004
    Figure 2024153836000004
  • Figure 2024153836000005
    Figure 2024153836000005
  • Figure 2024153836000006
    Figure 2024153836000006
Patent Text Reader

Abstract

To provide a metal layer integrated type polypropylene film having a processing suitability at a certain level as well as capable of obtaining a capacitor having an electrostatic capacitance stability at a certain level, and furthermore, capable of obtaining a capacitor excellent in an insulation resistance stability in a high-temperature high-voltage load.SOLUTION: A metal layer integrated type polypropylene film includes a polypropylene film and a metal layer laminated on one or both sides of the polypropylene film. The metal layer integrated type polypropylene film has a cumulative dielectric breakdown point number density of 1000 pcs / m2 or less, after a cumulative direct current voltage application test at 20°C and 350 to 425 V / μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal layer-integrated polypropylene film and the like. [Background technology]

[0002] Polypropylene films have excellent electrical properties such as high voltage resistance and low dielectric loss, and also have high moisture resistance. Therefore, they are widely used in electronic devices and electrical devices. Specifically, they are used as films for high-voltage capacitors, various switching power supplies, filter capacitors (e.g., converters, inverters, etc.), smoothing capacitors, etc.

[0003] In particular, in recent years, polypropylene films have begun to be widely used as capacitors for inverter power devices that control drive motors for electric vehicles, hybrid vehicles, etc. Inverter power device capacitors used in automobiles, etc., are required to be small, lightweight, high capacity, and highly reliable over a long period of time. 2 The biaxially oriented polypropylene film for capacitors, in which the number of particles per square meter and the 10-point average roughness satisfy a predetermined relationship, is disclosed. Patent Document 1 describes that the biaxially oriented polypropylene film for capacitors having the above-mentioned configuration has the following effects: it has excellent processability even though it is a thin film, and exhibits high voltage resistance under a wide range of ambient temperature conditions from low temperature (-40°C) to high temperature (150°C). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 146367 Summary of the Invention [Problem to be solved by the invention]

[0005] In particular, there is a growing need for thinner films for in-vehicle (e.g., xEV) capacitors due to the demand for miniaturization and high efficiency. However, thin polypropylene films have low processability, and for example, they are prone to wrinkles and misalignment during element winding processing when manufacturing capacitors.

[0006] In addition, the inventors have noticed that, in light of the increasing need for long-term reliability, not only capacitance stability over long-term use but also insulation resistance stability under high-temperature and high-voltage load is particularly important. Here, capacitance / insulation resistance stability refers to the small change from the initial capacitance / insulation resistance value when the capacitor is used. If the insulation resistance is significantly reduced under high-temperature and high-voltage load, leakage current increases rapidly, causing thermal runaway, which may ultimately cause a short circuit or fire.

[0007] Furthermore, in the course of research, the present inventors have noticed that the physical properties of the metal layer-integrated polypropylene film used for producing a capacitor are important in its state.

[0008] Therefore, the present invention aims to provide a metal layer-integrated polypropylene film that can not only provide a capacitor having a certain level of processability and a certain level of capacitance stability, but also can provide a capacitor with excellent insulation resistance stability under high temperature and high voltage load. [Means for solving the problem]

[0009] In consideration of the above problems, the present inventors have intensively conducted research and have discovered a metal layer-integrated polypropylene film having a polypropylene film and a metal layer laminated on one or both sides of the polypropylene film, the metal layer-integrated polypropylene film having a cumulative dielectric breakdown point density of 1000 / m after a cumulative DC voltage application test at 20° C. and 350 to 425 V / μm. 2It has been found that the above-mentioned problems can be solved by the metal layer-integrated polypropylene film described below. Based on this finding, the present inventors have conducted further research and have completed the present invention. That is, the present invention includes the following aspects.

[0010] Item 1. A metal layer-integrated polypropylene film having a polypropylene film and a metal layer laminated on one or both sides of the polypropylene film, the film having a cumulative dielectric breakdown density of 1000 / m2 after a cumulative DC voltage application test at 20°C and 350 to 425 V / μm. 2 The following is a metal layer-integrated polypropylene film.

[0011] Item 2. The metal layer-integrated polypropylene film according to Item 1, wherein the polypropylene film has a thickness of 1.0 to 3.0 μm.

[0012] Item 3. The metal layer-integrated polypropylene film according to Item 1 or 2, wherein the polypropylene film has a heat shrinkage rate of 0 to 8% in a first direction and a heat shrinkage rate of -2 to 2% in a second direction perpendicular to the first direction when treated at 120°C for 15 minutes.

[0013] Item 4. The metal layer-integrated polypropylene film according to any one of Items 1 to 3, wherein the polypropylene film has a heat shrinkage rate of 0 to 10% in a first direction and a heat shrinkage rate of -1 to 5% in a second direction perpendicular to the first direction when treated at 140°C for 15 minutes.

[0014] Item 5. The metal layer-integrated polypropylene film according to any one of Items 1 to 4, wherein the polypropylene film has a tensile modulus of elasticity in a first direction of 1.5 GPa or more and a tensile modulus of elasticity in a second direction perpendicular to the first direction of 3 GPa or more.

[0015] Item 6. The metal layer-integrated polypropylene film according to any one of Items 1 to 5, wherein the polypropylene film is a biaxially stretched film.

[0016] Item 7. The metal layer-integrated polypropylene film according to any one of Items 1 to 6, wherein the polypropylene film is a single-layer film.

[0017] Item 8. The metal layer-integrated polypropylene film according to any one of Items 1 to 7, which is for a capacitor.

[0018] Item 9. A capacitor comprising the metal layer-integrated polypropylene film according to any one of items 1 to 8.

[0019] Item 10. The capacitor according to item 9, comprising a roll of the metal layer-integrated polypropylene film according to any one of items 1 to 8. Effect of the Invention

[0020] According to the present invention, it is possible to provide a metal layer-integrated polypropylene film which not only makes it possible to obtain a capacitor having a certain level of processability and a certain level of capacitance stability, but also makes it possible to obtain a capacitor having excellent insulation resistance stability under high temperature and high voltage load. [Brief description of the drawings]

[0021] [Figure 1] 1 is a schematic perspective view for explaining a metal layer-integrated polypropylene film produced as an example and a comparative example. 1: metal layer-integrated polypropylene film, 2: biaxially stretched polypropylene film, 3: metal vapor deposition electrode, 3a: metal vapor deposition layer, 3b: electrode lead-out portion, 4: insulating margin [Diagram 2]Schematic diagram for explaining a method for manufacturing a metal layer-integrated polypropylene film according to an embodiment and a comparative example. 1: metal layer-integrated polypropylene film, 1R: metal layer-integrated polypropylene film roll, 2: biaxially stretched polypropylene film, 2a: vapor deposition surface, 2b: cooling roll contact surface, 2R: biaxially stretched polypropylene film roll, 101: dielectric film supply section, 102: insulating margin forming section, 103: special vapor deposition pattern margin forming section, 103d: printing roll, 104: vapor deposition section, 104a: metal vapor generating section, 104b: metal vapor generating section (for generating electrode extraction section), 104c: cooling roll, 105: static electricity removing section, 105a: DC magnetron discharge electrode, 105b: DC magnetron discharge electrode, 105c: DC magnetron discharge electrode, 105d: DC magnetron discharge electrode, 106: metal layer-integrated film winding section [Diagram 3] Schematic diagram of a measuring device for cumulative dielectric breakdown point density. 1: metal layer integrated polypropylene film, 1a: metal vapor deposition surface, 201: brass plate, 202: conductive rubber, 203: aluminum foil, 204: insulating polypropylene film (5 μm), 204a: window, 205: cylindrical brass electrode, 206: resistive element (10 kΩ), 207: DC power source, 301: cumulative dielectric breakdown point density test device DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] In this specification, the expressions "contain" and "comprise" include the concepts of "contain", "include", "consist essentially of" and "consist only of".

[0023] In this specification, based on the ranges consisting of the upper and / or lower limits described for each parameter, ranges in which the upper and / or lower limits are arbitrarily interchanged between multiple ranges are also exemplified.

[0024] In this specification, "X or more" (X is a negative value) refers to a range consisting of X to 0 and values ​​greater than 0. Additionally, "X or less" (X is a negative value) refers to a range consisting of X and negative values ​​whose absolute value is greater than X.

[0025] 1. Polypropylene film with metal layer In one aspect, the present invention provides a metal layer-integrated polypropylene film having a polypropylene film and a metal layer laminated on one or both sides of the polypropylene film, the metal layer-integrated polypropylene film having a cumulative dielectric breakdown point density of 1000 points / m after a cumulative DC voltage application test at 20° C. and 350 to 425 V / μm. 2 The present invention relates to a metal layer-integrated polypropylene film (sometimes referred to as the "metal layer-integrated polypropylene film of the present invention" in this specification). The polypropylene film (polypropylene film not laminated with a metal layer) possessed by the metal layer-integrated polypropylene film of the present invention is sometimes referred to as the "polypropylene film of the present invention" in this specification. These will be described below.

[0026] The metal layer-integrated polypropylene film of the present invention has a cumulative dielectric breakdown point density after a cumulative DC voltage application test at 20° C. and 350 to 425 V / μm (cumulative dielectric breakdown point density at 20° C. at 425 V / μm) of 1000 pieces / m 2 The cumulative dielectric breakdown density is 1000 / m 2 By making the density of the cumulative dielectric breakdown points equal to or less than 900 / m, it is possible to obtain a capacitor that exhibits a certain level of processability and capacitance stability, and furthermore, a capacitor that exhibits excellent insulation resistance stability under high temperature and high voltage load. 2 Less than or equal to 800 pieces / m 2 Less than 700 / m, more preferably 2 Less than 600 pieces / m 2 The following are particularly preferred: Approximately 500 pieces / m 2 Less than or equal to 400 pieces / m 2 Less than 300 pieces / m 2 Less than 200 pieces / m 2 Less than 100 pieces / m 2In this particularly preferred embodiment, the cumulative dielectric breakdown density is preferably 50 / m 2 Less than or equal to 20 pieces / m 2 Less than 10 pieces / m, more preferably 2 Less than 5 pieces / m 2 Less than 0 pieces / m 2 It is.

[0027] The cumulative dielectric breakdown density is measured as follows, with the metal layer-integrated polypropylene film set in the measuring device as shown in FIG. 3. After applying a DC voltage of 350 V / μm for 1 minute in an environment of 20°C, the number of dielectric breakdown points in the window area (100 mm×10 mm) of the insulating polypropylene film is visually counted. After counting, a DC voltage of 375 V / μm is applied for 1 minute, and the cumulative dielectric breakdown points in the window area of ​​the insulating polypropylene film are visually counted. Next, the DC voltage is increased by 25 V / μm at a time, and this operation is repeated up to 425 V / μm, to cumulatively apply the DC voltage. The test is performed on five metal layer-integrated polypropylene films, and the average value of the cumulative dielectric breakdown points at 20°C at 425 V / μm is calculated based on the area of ​​the window of the insulating polypropylene film (100 mm×10 mm=1,000 mm). 2 =0.001m 2 ) and calculate the cumulative dielectric breakdown density (unit: pieces / m2) at 425V / μm and 20℃. 2 ) is required.

[0028] Details of Fig. 3 and the measurement method are as follows. Fig. 3 is a schematic diagram for explaining the cumulative dielectric breakdown point density measurement. First, a brass plate 201 (320 mm x 250 mm), a conductive rubber 202 (280 mm x 150 mm), and an aluminum foil 203 (280 mm x 150 mm) are laminated in this order on top of the aluminum foil 203, and further, an insulating polypropylene film 204 (300 mm x 210 mm, window 100 mm x 10 mm) having a rectangular (100 mm x 10 mm) cutout portion (hereinafter, this portion will be referred to as "window 204a") in the center is laminated on top of the aluminum foil 203 so as to cover the outer periphery of the aluminum foil 203.

[0029] The metal layer integrated polypropylene film 1 is superimposed on the insulating polypropylene film 204 laminated as described above so as not to protrude from the outer periphery of the insulating polypropylene film 204. At this time, the metal deposition surface 1a of the metal layer integrated polypropylene film 1 is placed on top, and the metal deposition layer 3a is superimposed so as to cover the window 204a of the insulating polypropylene film 204. However, when a special deposition pattern margin is formed on the metal layer integrated polypropylene film 1, it is preferable that the part overlapping the window 204a is a part of the metal deposition layer 3a without the special margin, that is, the so-called solid deposition part of the metal deposition layer 3a. The metal layer integrated polypropylene film 1 superimposed on the insulating polypropylene film 204 as described above has a cooling roll contact surface 2b that contacts the surface of the aluminum foil 203 through the window 204a of the insulating polypropylene film 204.

[0030] Furthermore, for the metal layer-integrated polypropylene film 1 superimposed on the insulating polypropylene film 204 as described above, a cylindrical brass electrode 205 (diameter 25 mm, height 65 mm) is placed on the metal deposition layer 3a away from the window 204a. At this time, the cylindrical brass electrode 205 is in contact with the metal deposition layer 3a.

[0031] The cylindrical brass electrode 205 is electrically connected to a DC power supply 207 via a resistive element (10 kΩ) 206 for preventing overcurrent. The brass plate 201 is also directly electrically connected to the DC power supply 207. As described above, the cumulative dielectric breakdown point density test device 301 is constructed.

[0032] By measuring the cumulative dielectric breakdown density of the metal layer-integrated polypropylene film 1 using the cumulative dielectric breakdown density test device 301, it is possible to predict the voltage resistance of a capacitor made from the metal layer-integrated polypropylene film without having to manufacture the capacitor. In the breakdown point density test device 301, when a high voltage is applied by the DC power supply 207, a dielectric breakdown occurs at the points of the metal layer-integrated polypropylene film 1 that are weak in terms of voltage resistance. When dielectric breakdown occurs, heat is generated instantaneously, causing the metal vapor deposition layer 3a to evaporate and the insulation to recover (self-healing). The points where self-healing occurs are visually recognized as milky white because the metal vapor deposition layer 3a is no longer present. After applying a predetermined voltage for a fixed period of time, the number of points where self-healing occurs (hereinafter referred to as the "number of dielectric breakdown points") is counted, and the voltage resistance of the metal layer-integrated polypropylene film can be evaluated.

[0033] The number of dielectric breakdown points depends on the voltage resistance of the metal layer-integrated polypropylene film 1 and the properties of the metal vapor deposition layer 3a. In other words, the number of dielectric breakdown points is also affected by whether the metal vapor deposition layer 3a is easily evaporated. The cumulative dielectric breakdown point density test device 301 uses the metal vapor deposition layer 3a as the upper conductor, so it is possible to see characteristics close to those of an actual capacitor.

[0034] In the cumulative dielectric breakdown density test, the voltage is increased stepwise at a constant interval from a predetermined starting voltage to an end voltage, and the voltage is applied for a certain period of time, and the number of dielectric breakdown points of the metal layer-integrated polypropylene film 1 is cumulatively counted each time (the cumulative counted number is hereinafter referred to as the "cumulative dielectric breakdown number"). After repeating the process up to the end voltage, the cumulative dielectric breakdown number of the metal layer-integrated polypropylene film 1 is counted based on the area of ​​the window 204a (100 mm x 10 mm = 1,000 mm 2 =0.001m 2 ) and divide it by the cumulative insulation breakdown density (unit: pieces / m 2 The cumulative dielectric breakdown density measurement is carried out by determining the cumulative dielectric breakdown density (c) of the metal layer-integrated polypropylene film. The window 204a allows voltage to be applied to a certain area and prevents creeping discharge, making it possible to measure the cumulative dielectric breakdown density of the metal layer-integrated polypropylene film with higher accuracy.

[0035] The polypropylene film of the present invention preferably has a heat shrinkage rate in a first direction of 0 to 8% (more preferably 0 to 6%, and even more preferably 0 to 4%) and a heat shrinkage rate in a second direction perpendicular to the first direction of 0 to 2% (more preferably -1 to 1%) when treated at 120°C for 15 minutes. In this specification, when the polypropylene film of the present invention is a biaxially oriented polypropylene film, the first direction is preferably the MD direction (Machine Direction) of the polypropylene film, and the second direction is preferably the TD direction (Transverse Direction) of the polypropylene film. When the thermal shrinkage rate in the first direction is 0% or more (i.e., when the thermal expansion rate is 0% or less) and the thermal shrinkage rate in the second direction is -2% or more (i.e., when the thermal expansion rate is 2% or less), and the thermal shrinkage rate in the first direction is 8% or less (i.e., when the thermal expansion rate is -8% or more), and the thermal shrinkage rate in the second direction is 2% or less (i.e., when the thermal expansion rate is -2% or more) under processing conditions at 120°C for 15 minutes, the thermal expansion and thermal contraction of the film on the cooling roll during metal vapor deposition processing can be further suppressed to suppress transport wrinkles, and the adhesion of the polypropylene film to the cooling roll can be further improved, thermal damage can be suppressed, and the voltage resistance of the metal layer-integrated polypropylene film can be further improved.

[0036] The heat shrinkage rate (120°C heat shrinkage rate) (unit: %) under the treatment condition of 120°C for 15 minutes is measured as follows. The sample used for the measurement is cut out from the roll, and the size of the sample is 130 mm in the first direction and 20 mm in the second direction when measuring the 120°C heat shrinkage rate in the first direction, and 20 mm in the first direction and 130 mm in the second direction when measuring the 120°C heat shrinkage rate in the second direction. Three samples are prepared for measuring the 120°C heat shrinkage rate in the first direction and three samples are prepared for measuring the 120°C heat shrinkage rate in the second direction. Next, for the three samples for measuring the 120°C heat shrinkage rate in the first direction, a marked line is marked at a position 15 mm from each end of the 130 mm in the first direction. At this time, the distance between the marked lines is 100 mm. For the three samples for measuring the 120°C heat shrinkage rate in the second direction, a marked line is marked at a position 15 mm from each end of the 130 mm in the second direction. At this time, the distance between the marked lines is 100 mm. Next, each sample with the marked lines is hung without load in a hot air circulating thermostatic chamber at 120°C so that the cut-out 130 mm length is vertical, and held for 15 minutes. After that, it is cooled to room temperature (23°C), and the distance between the marked lines is measured with a ruler and calculated using the following formula: Heat shrinkage rate (%) = (marked line spacing before heating - marked line spacing after heating) / marked line spacing before heating x 100 The heat shrinkage rate (%) is calculated for each sample using the above. The average of the heat shrinkage rates of the three samples for which the 120°C heat shrinkage rate in the first direction is measured is defined as the 120°C heat shrinkage rate (%) in the first direction. The average of the heat shrinkage rates of the three samples for which the 120°C heat shrinkage rate in the second direction is defined as the 120°C heat shrinkage rate (%) in the second direction. Note that measurement conditions other than those described here are in accordance with "25. Dimensional change" of JIS C 2151:2019.

[0037] The polypropylene film of the present invention preferably has a heat shrinkage rate of 0 to 10% (more preferably 0 to 8%, even more preferably 0 to 7%) in the first direction and a heat shrinkage rate of -1 to 5% (more preferably 0 to 4%) in the second direction perpendicular to the first direction under the treatment conditions of 140°C for 15 minutes. When the heat shrinkage rate in the first direction is 0% or more (i.e., when the thermal expansion coefficient is 0% or less), and when the heat shrinkage rate in the second direction is -1% or more (i.e., when the thermal expansion coefficient is 1% or less), and when the heat shrinkage rate in the first direction is 10% or less (i.e., when the thermal expansion coefficient is -10% or more), and when the heat shrinkage rate in the second direction is 5% or less (i.e., when the thermal expansion coefficient is -5% or more), the thermal expansion and thermal shrinkage of the film on the cooling roll during metal deposition processing can be further suppressed to suppress conveying wrinkles, and the adhesion of the polypropylene film to the cooling roll can be further improved, heat damage can be suppressed, and the voltage resistance of the metal layer-integrated polypropylene film can be further improved.

[0038] The heat shrinkage rate (140°C heat shrinkage rate) (unit: %) when treated at 140°C for 15 minutes is calculated by calculating the 140°C heat shrinkage rate (%) in the first direction and the 140°C heat shrinkage rate (%) in the second direction in the same manner as for the 120°C heat shrinkage rate, except that the 120°C hot air circulating thermostatic oven is changed to a 140°C hot air circulating thermostatic oven in the method for measuring the 120°C heat shrinkage rate.

[0039] The polypropylene film of the present invention preferably has a tensile modulus in a first direction of 1.5 GPa or more (more preferably 2.0 GPa or more) and a tensile modulus in a second direction perpendicular to the first direction of 3.0 GPa or more (more preferably 4.0 GPa or more). When the tensile modulus in the first direction is 1.5 GPa or more and the tensile modulus in the second direction is 3.0 GPa or more, wrinkles during transport during metal deposition processing are more suppressed, adhesion of the polypropylene film to the cooling roll can be more improved, heat damage can be suppressed, and the voltage resistance of the metal layer-integrated polypropylene film can be more improved. In one embodiment of the present invention, the tensile modulus of the polypropylene film of the present invention is not particularly limited in any direction, but can be substantially set to an upper limit of 6.0 GPa.

[0040] The tensile modulus (unit: GPa) is measured in accordance with JIS K-7127 (1999). The sample used for the measurement is cut out from a roll, and the size of the sample is 200 mm in the first direction and 15 mm in the second direction when measuring the tensile modulus in the first direction, and 15 mm in the first direction and 200 mm in the second direction when measuring the tensile modulus in the second direction. After cutting out the sample, a tensile test is performed using a tension and compression tester (manufactured by Minebea Co., Ltd.) under test conditions of a measurement temperature of 23°C, a chuck distance of 100 mm, and a tensile speed of 200 mm / min. Next, the tensile modulus in the first direction (GPa) and the tensile modulus in the second direction (GPa) are determined by automatic analysis using data processing software built into the tester.

[0041] The polypropylene film of the present invention has a thickness of preferably 9.5 μm or less, more preferably 6.0 μm or less, even more preferably 3.0 μm or less, even more preferably 2.9 μm or less, particularly preferably 2.8 μm or less, and even more preferably 2.5 μm or less. The thickness of the polypropylene film of the present invention is preferably 0.8 μm or more, and more preferably 1.0 μm or more. More preferably, the thickness is 1.4 μm or more, even more preferably, 1.5 μm or more, and particularly preferably, 1.8 μm or more. In particular, when the thickness is within the range of 1.0 to 6.0 μm, 1.0 to 3.0 μm, 1.0 to 2.9 μm, etc., the polypropylene film is very thin, but has excellent processability in the slit process, blocking suppression during the deposition process, and element winding processability, which is preferable. When the thickness is 9.5 μm or less, the capacitance can be increased, so that the film can be suitably used for a capacitor. From the viewpoint of production, the thickness can be 0.8 μm or more.

[0042] Film thickness is measured in accordance with JIS-C2330, except that it is measured at 100±10 kPa using a Citizen Seimitsu paper thickness measuring instrument MEI-11.

[0043] The haze value of the polypropylene film of the present invention is not particularly limited, but is, for example, 2.2 to 5.0%, preferably 2.3 to 4.5%, more preferably 2.5 to 4.5%, even more preferably 2.5 to 4.0%, and still more preferably 2.5 to 3.5%.

[0044] The haze value is measured as follows: Using a haze meter ("NDH-5000" manufactured by Nippon Denshoku Industries Co., Ltd.), the measurement is performed in accordance with JIS K 7136:2000. The size of the sample is 50 mm x 100 mm.

[0045] The polypropylene film of the present invention may be a biaxially stretched film, a uniaxially stretched film, or a non-stretched film, and is preferably a biaxially stretched film.

[0046] The layer structure of the polypropylene film of the present invention is not particularly limited. The film of the present invention may be a single layer consisting of one layer, or may be a plurality of layers having the same or different compositions. The polypropylene film of the present invention is preferably a film consisting of one or more film-like molded layers, and more preferably a monolayer film (a film consisting of one film-like molded layer). The polypropylene film of the present invention contains a polypropylene resin as a main component. In this specification, "containing a polypropylene resin as a main component" means that the polypropylene resin is contained in an amount of 50% by mass or more with respect to the entire polypropylene film (when the entire polypropylene film is taken as 100% by mass). The content of the polypropylene resin with respect to the entire polypropylene film is preferably 75% by mass or more, and more preferably 90% by mass or more. The upper limit of the content of the polypropylene resin with respect to the entire polypropylene film is, for example, 100% by mass, 98% by mass, etc.

[0047] The polypropylene resin is not particularly limited, and one type may be used alone, or two or more types may be used in combination. Among them, the polypropylene resin is preferably a polypropylene resin that forms β-type spherulites when made into a cast sheet.

[0048] A linear polypropylene resin is preferred, and a linear homopolypropylene resin is more preferred.

[0049] The total ash content of the polypropylene resin is preferably as low as possible for electrical properties. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and even more preferably 30 ppm or less, based on the polypropylene resin. The lower limit of the total ash content is, for example, 2 ppm or 5 ppm. The lower the total ash content, the less impurities such as polymerization catalyst residues are present.

[0050] In the polypropylene film of the present embodiment, the polypropylene resin is, for example, The composition may contain only the first polypropylene resin, or may contain the second polypropylene resin described below together with the first polypropylene resin.

[0051] The polypropylene resin may contain a first polypropylene resin. When the polypropylene resin contains the first polypropylene resin, the content of the first polypropylene resin is preferably 50% by weight or more, more preferably 55% by weight or more, and even more preferably 60% by weight or more, based on 100% by weight of the polypropylene resin. The upper limit of the content of the first polypropylene resin may be, for example, 100% by weight or less, 99% by weight or less, 98% by weight or less, or 95% by weight or less, based on 100% by weight of the polypropylene resin, and is preferably 90% by weight or less, more preferably 85% by weight or less, and even more preferably 80% by weight or less, based on 100% by weight of the polypropylene resin. Thus, the polypropylene film of this embodiment may contain the first polypropylene resin as a main component. For example, isotactic polypropylene may be used as the first polypropylene resin.

[0052] The weight average molecular weight Mw of the first polypropylene resin is preferably 250,000 or more and less than 400,000, more preferably 260,000 or more and less than 370,000, and even more preferably 270,000 or more and less than 350,000. When Mw is 250,000 or more and less than 400,000, the resin fluidity becomes moderate, the thickness of the cast raw sheet is easily controlled, and it is easy to produce a thin stretched film with good thickness uniformity. Also, when Mw is 250,000 or more and less than 350,000, the resin fluidity becomes more moderate, the thickness of the cast raw sheet is easily controlled, and it is easier to produce a thin stretched film with good thickness uniformity.

[0053] The number average molecular weight Mn of the first polypropylene resin is preferably 30,000 or more and 52,000 or less, more preferably 32,000 or more and 50,000 or less, and further preferably 34,000 or more and 48,000 or less.

[0054] The first polypropylene resin has a z-average molecular weight Mz of preferably 600,000 or more and 1,650,000 or less, and more preferably 700,000 or more and 1,600,000 or less.

[0055] The molecular weight distribution (Mw / Mn) of the first polypropylene resin is preferably 5.0 or more, more preferably 5.5 or more. The Mw / Mn of the first polypropylene resin is preferably 11.0 or less, more preferably 10.0 or less. When the Mw / Mn of the first polypropylene resin is 5.0 or more and 11.0 or less, it is preferable because it is possible to obtain an appropriate resin fluidity during biaxial stretching, and it is easy to obtain an extremely thin biaxially stretched propylene film without thickness unevenness. The molecular weight distribution Mw / Mn is the ratio of the weight average molecular weight Mw to the number average molecular weight Mn.

[0056] The molecular weight distribution (Mz / Mn) of the first polypropylene resin is preferably from 10 to 60, more preferably from 12 to 50, and even more preferably from 15 to 45. The molecular weight distribution Mz / Mn is the ratio of the z-average molecular weight Mz to the number-average molecular weight Mn.

[0057] In this specification, the weight average molecular weight (Mw), number average molecular weight (Mn), z-average molecular weight (Mz), and molecular weight distribution (Mw / Mn and Mz / Mn) of the polypropylene resin are values ​​measured using a gel permeation chromatograph (GPC) device. More specifically, they are values ​​measured using a high-temperature GPC measuring device with built-in differential refractometer (RI) HLC-8121GPC-HT (product name) manufactured by Tosoh Corporation. As the GPC column, three TSKgel GMHHR-H(20)HT columns manufactured by Tosoh Corporation are connected and used. The column temperature is set to 140°C, and trichlorobenzene is passed as an eluent at a flow rate of 1.0 ml / 10 min to obtain the measured values ​​of Mw and Mn. A standard polystyrene column manufactured by Tosoh Corporation is used. A calibration curve for the molecular weight M is prepared using a polystyrene microscope, and the measured values ​​are converted into polystyrene values ​​to obtain Mw, Mn, and Mz.

[0058] The melt flow rate (MFR) of the first polypropylene resin at 230°C is preferably 8.0 g / 10 min or less, more preferably 7.0 g / 10 min or less, and even more preferably 6.0 g / 10 min or less. The melt flow rate at 230°C is preferably 3.5 g / 10 min or more. The melt flow rate at 230°C is measured in accordance with JIS K 7210-1999 under a load of 2.16 kg at 230°C. The unit of the melt flow rate, g / 10 min, is also called dg / min.

[0059] The heptane insoluble content of the first polypropylene resin is preferably 97.0% or more. The heptane insoluble content is preferably 98.5% or less. The higher the heptane insoluble content, the higher the stereoregularity of the resin. When the heptane insoluble content (HI) is 97.0% or more and 98.5% or less, the moderately high stereoregularity leads to a moderate improvement in the crystallinity of the polypropylene resin in the polypropylene film, and the voltage resistance at high temperatures is improved. Furthermore, the solidification (crystallization) speed during cast raw sheet molding becomes moderate, and the resin has moderate extensibility. The heptane insoluble content (HI) is measured by the method described in the Examples.

[0060] The total ash content of the first polypropylene resin is preferably as low as possible for electrical properties. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and even more preferably 30 ppm or less, based on the first polypropylene resin. The lower limit of the total ash content is, for example, 2 ppm or 5 ppm.

[0061] The polypropylene resin may further include a second polypropylene resin. The polypropylene film of the present embodiment preferably includes a second polypropylene resin in addition to the first polypropylene resin, and more preferably includes the first polypropylene resin and the second polypropylene resin as resins constituting the polypropylene film.

[0062] When the polypropylene resin contains a second polypropylene resin, the content of the second polypropylene resin is preferably 50% by weight or less, more preferably 49% by weight or less, even more preferably 45% by weight or less, and particularly preferably 40% by weight or less, relative to 100% by weight of the polypropylene resin. When the polypropylene resin contains a second polypropylene resin, the content of the second polypropylene resin may be, for example, 1% by weight or more, 2% by weight or more, or 5% by weight or more, relative to 100% by weight of the polypropylene resin, and is preferably 10% by weight or more, more preferably 15% by weight or more, and even more preferably 20% by weight or more, relative to 100% by weight of the polypropylene resin. As the second polypropylene resin, for example, isotactic polypropylene may be mentioned.

[0063] The Mw of the second polypropylene resin is preferably 300,000 or more, more preferably 350,000 or more. The Mw of the second polypropylene resin is preferably 450,000 or less, more preferably 400,000 or less.

[0064] The Mn of the second polypropylene resin is preferably 40,000 or more and 54,000 or less, more preferably 42,000 or more and 50,000 or less, and further preferably 44,000 or more and 48,000 or less.

[0065] The Mz of the second polypropylene resin is preferably more than 1,550,000 and not more than 2,000,000, and more preferably 1,580,000 or more and 1,700,000 or less.

[0066] In the second polypropylene resin, the ratio of Mw to Mn (Mw / Mn) is preferably is preferably 5.5 or more, more preferably 7.0 or more, and particularly preferably 7.5 or more. The upper limit of Mw / Mn in the second polypropylene resin is, for example, 11.0, 10.0, 9.0, or 8.5.

[0067] In the second polypropylene resin, the ratio of Mz to Mn (Mz / Mn) is preferably 30 or more and 40 or less, and more preferably 33 or more and 37 or less.

[0068] The melt flow rate of the second polypropylene resin at 230° C. is preferably less than 4.0 g / 10 min, more preferably 3.9 g / 10 min or less, and even more preferably 3.8 g / 10 min or less. The melt flow rate at 230° C. is preferably 1.0 g / 10 min or more, more preferably 1.5 g / 10 min or more, and even more preferably 2.0 g / 10 min or more.

[0069] The heptane insoluble content of the second polypropylene resin is preferably 97.5% or more, more preferably 98.0% or more, even more preferably more than 98.5%, particularly preferably 98.6% or more. The heptane insoluble content is preferably 99.5% or less, more preferably 99.0% or less.

[0070] The total ash content of the second polypropylene resin is preferably as low as possible for electrical properties. The total ash content is preferably 50 ppm or less, more preferably 40 ppm or less, and even more preferably 30 ppm or less, based on the second polypropylene resin. The lower limit of the total ash content is, for example, 2 ppm or 5 ppm.

[0071] The total amount of the first polypropylene resin and the second polypropylene resin, when the entire polypropylene resin is taken as 100% by weight, can be, for example, 90% by weight or more, or can be 95% by weight or more, or can be 100% by weight.

[0072] The polypropylene resin can be produced by a generally known polymerization method. There is no particular limitation as long as the polypropylene resin usable in the polypropylene film of the present embodiment can be produced. Examples of such polymerization methods include gas phase polymerization, bulk polymerization, and slurry polymerization.

[0073] The polymerization may be a single-stage polymerization using one polymerization reactor, or a multi-stage polymerization using at least two polymerization reactors. Furthermore, hydrogen or a comonomer may be added to the reactor as a molecular weight modifier.

[0074] The catalyst used in the polymerization can be a generally known Ziegler-Natta catalyst, and is not particularly limited as long as the polypropylene resin can be obtained. The catalyst may contain a cocatalyst component or a donor. The molecular weight, molecular weight distribution, etc. can be controlled by adjusting the catalyst and polymerization conditions.

[0075] The molecular weight, molecular weight distribution, etc. of the polypropylene resin can be determined, for example, by (i) the polymerization method and polymerization (ii) the conditions of the reactor during polymerization, such as temperature and pressure, (iii) the use of additives, and their types The amount of the solvent used can be adjusted by appropriately selecting (i) the type and amount of the solvent, and (ii) the type and amount of the catalyst used.

[0076] Specifically, the molecular weight, molecular weight distribution, etc. of the polypropylene resin can be adjusted, for example, by a multi-stage polymerization reaction. Examples of the multi-stage polymerization reaction include the following methods.

[0077] First, in the first polymerization step, propylene and a catalyst are supplied to a first polymerization reactor. Together with these components, hydrogen as a molecular weight regulator is mixed in an amount necessary to reach the required molecular weight of the polymer. The reaction temperature is, for example, about 70 to 100°C in the case of slurry polymerization, and the residence time is about 20 to 100 minutes. A plurality of reactors can be used, for example, in series. In this case, the polymerization product of the first step is continuously sent to the next reactor together with additional propylene, catalyst, and molecular weight regulator, and then a second polymerization is carried out in which the molecular weight is adjusted to a lower or higher molecular weight than in the first polymerization step. By adjusting the yield (production amount) of the first and second reactors, it is possible to adjust the composition (configuration) of the high molecular weight component and the low molecular weight component.

[0078] The molecular weight, molecular weight distribution, etc. of the polypropylene resin can also be adjusted by peroxidation decomposition, for example, a method of peroxidation treatment using a decomposing agent such as hydrogen peroxide or an organic peroxide.

[0079] When peroxide is added to a degradable polymer such as polypropylene, a hydrogen abstraction reaction occurs from the polymer, and some of the resulting polymer radicals recombine and undergo crosslinking reactions, but most of the radicals undergo secondary decomposition (β-cleavage) and split into two polymers with smaller molecular weights. In other words, the higher the molecular weight component, the higher the probability of decomposition. This increases the amount of low molecular weight components, making it possible to adjust the molecular weight distribution.

[0080] When adjusting the content of low molecular weight components by blending (resin mixing), it is preferable to dry mix or melt mix at least two or more resins with different molecular weights. In general, a two-type polypropylene mixture system in which a main resin is mixed with an additive resin having a higher or lower average molecular weight in an amount of about 1 to 40 mass % is preferably used because it is easy to adjust the amount of low molecular weight components.

[0081] In addition, in the case of this mixing adjustment, the melt flow rate (MFR) may be used as a guide for the average molecular weight. In this case, it is preferable to set the difference in MFR between the main resin and the added resin to about 1 to 30 g / 10 min from the viewpoint of convenience in adjustment.

[0082] As the polypropylene resin, commercially available products can also be used.

[0083] The polypropylene film of the present invention may contain other resins other than polypropylene resin (hereinafter also referred to as "other resins"). The "other resins" are generally resins other than polypropylene resin, which is considered to be the main component resin, and are not particularly limited as long as the desired polypropylene film can be obtained. Examples of other resins include other polyolefins other than polypropylene, such as polyethylene, poly(1-butene), polyisobutene, poly(1-pentene), and poly(1-methylpentene), copolymers of α-olefins such as ethylene-propylene copolymers, propylene-butene copolymers, and ethylene-butene copolymers, random copolymers of vinyl monomers-diene monomers such as styrene-butadiene random copolymers, and random copolymers of vinyl monomers-diene monomers-vinyl monomers such as styrene-butadiene-styrene block copolymers. The polypropylene film of the present invention may contain an amount that does not adversely affect the desired polypropylene film. The polypropylene film of the present invention may contain preferably 10 parts by mass or less of other resins, more preferably 5 parts by mass or less, based on 100 parts by mass of polypropylene resin. The polypropylene film of the present invention may contain another resin in an amount of preferably 0.1 part by mass or more, more preferably 1 part by mass or more, based on 100 parts by mass of the polypropylene resin.

[0084] The polypropylene film of the present invention may further contain at least one additive in addition to the resin component. The "additive" is an additive generally used in polypropylene. There are no particular limitations as long as the desired polypropylene film can be obtained by the additives. Examples of additives include nucleating agents (α-crystal nucleating agents, β-crystal nucleating agents), antioxidants, necessary stabilizers such as chlorine absorbers and ultraviolet absorbers, lubricants, plasticizers, flame retardants, antistatic agents, inorganic fillers, organic fillers, etc. Examples of the inorganic fillers include barium titanate, strontium titanate, and aluminum oxide. When the additives are used, they can be included in an amount that does not adversely affect the desired polypropylene film.

[0085] The "nucleating agent" is not particularly limited as long as it is commonly used in polypropylene and can provide the desired polypropylene film.

[0086] Examples of the nucleating agent include an α-crystal nucleating agent that preferentially nucleates α-crystals and a β-crystal nucleating agent that preferentially nucleates β-crystals.

[0087] Among the α-crystal nucleating agents, organic nucleating agents include dispersion-type nucleating agents and dissolution-type nucleating agents. Dispersion-type nucleating agents include phosphate metal salt-based nucleating agents, carboxylate metal salt-based nucleating agents, and rosin metal salt-based nucleating agents. Dissolution-type nucleating agents include sorbitol-based nucleating agents, nonitol-based nucleating agents, xylitol-based nucleating agents, and amide-based nucleating agents.

[0088] Examples of the β-crystal nucleating agent include amide-based nucleating agents, di- or polycarboxylate-based metal salt-based nucleating agents, quinacridone-based nucleating agents, aromatic sulfonic acid-based nucleating agents, phthalocyanine-based nucleating agents, and tetraoxaspiro compound-based nucleating agents.

[0089] The nucleating agent can be dry-blended or melt-blended with the polypropylene raw material and pelletized, or can be used by feeding it into an extruder together with polypropylene pellets. The surface roughness of the film can be adjusted to a desired roughness by using the nucleating agent. A representative example of a commercially available nucleating agent is, for example, N-Jester NU-100 manufactured by New Japan Chemical Co., Ltd., which is a β-crystal nucleating agent. When the polypropylene film of the present invention contains a β-crystal nucleating agent, the content thereof is preferably 1 to 1000 ppm by mass, more preferably 50 to 600 ppm by mass, based on the mass of the resin component (mass when the resin component is taken as the whole).

[0090] The term "antioxidant" is generally used for polypropylene and is not particularly limited as long as it can obtain the desired polypropylene film. Antioxidants are generally used for two purposes. One purpose is to suppress thermal and oxidative degradation in an extruder, and the other purpose is to contribute to suppressing degradation during long-term use as a capacitor film and improving capacitor performance. An antioxidant that suppresses thermal and oxidative degradation in an extruder is also called a "primary agent," and an antioxidant that contributes to improving capacitor performance is also called a "secondary agent."

[0091] Two types of antioxidants may be used for these two purposes, or one type of antioxidant may be used for the two purposes.

[0092] An example of the primary agent is 2,6-di-tertiary-butyl-para-cresol (general name: BHT). The primary agent can usually be added for the purpose of suppressing thermal and oxidative degradation in an extruder during the preparation of a polypropylene resin composition, which will be described later in the method for producing a polypropylene film. The antioxidant added to the polypropylene resin composition for this purpose is mostly consumed in the molding process in the extruder, and almost none remains in the film after film formation. Therefore, when the polypropylene film of the present invention contains a primary agent, the content thereof is usually less than 100 ppm by mass relative to the mass of the resin component (mass when the resin component is taken as the whole).

[0093] The secondary agent may be a hindered phenol-based antioxidant having a carbonyl group.

[0094] The "hindered phenol-based antioxidant having a carbonyl group" is generally understood to be a hindered phenol-based antioxidant having a carbonyl group, and is not particularly limited as long as the desired polypropylene film can be obtained.

[0095] Examples of the hindered phenol-based antioxidant having a carbonyl group include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] (trade name: Irganox 245), 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: Irganox 259), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: Irganox 1010), 2,2-thio-diethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name: Irganox 1010), and the like. Examples of suitable polyolefins include N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (trade name: Irganox 1035), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (trade name: Irganox 1076), and N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamamide) (trade name: Irganox 1098). Of these, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] is particularly preferred, as it has a high molecular weight, is highly compatible with polypropylene, and has low volatility and excellent heat resistance.

[0096] The polypropylene film of the present invention may contain one or more types of hindered phenol-based antioxidants (secondary agents) having a carbonyl group for the purpose of suppressing deterioration that progresses over time during long-term use. When the polypropylene film of the present invention contains one or more types of hindered phenol-based antioxidants having a carbonyl group, the content thereof is preferably 2000 mass ppm or more and 6000 mass ppm or less, more preferably 3000 mass ppm or more and 6000 mass ppm or less, based on the mass of the resin component (mass when the resin component is taken as the whole). From the viewpoint of appropriate effect expression, it is preferable that the content of the hindered phenol-based antioxidant having a carbonyl group in the film is 2000 mass ppm or more and 6000 mass ppm or less.

[0097] A polypropylene film containing an optimal specific range of a hindered phenol-based antioxidant having a carbonyl group, which has good compatibility with polypropylene at the molecular level, is preferred because it improves long-term durability.

[0098] The term "chlorine absorbent" is generally used for polypropylene and is not particularly limited as long as it can obtain the desired polypropylene film. Examples of chlorine absorbents include metal soaps such as calcium stearate. When such a chlorine absorbent is used, it can be contained in an amount that does not adversely affect the desired polypropylene film.

[0099] Fig. 1 is a schematic perspective view for explaining one embodiment of the metal layer-integrated polypropylene film of the present invention. As shown in Fig. 1, the metal layer-integrated polypropylene film 1 is composed of a biaxially oriented polypropylene film 2 and a metal layer laminated on the biaxially oriented polypropylene film 2 so as to leave an insulating margin 4 (insulating groove: the length in the width direction is not particularly limited as long as the area of ​​the metal vapor deposition electrode 3 is not too small to significantly impair the capacitance when used as a capacitor) that continues in the longitudinal direction of the film at one end in the width direction of the film. The biaxially oriented polypropylene film has a metal vapor deposition electrode 3. The metal vapor deposition electrode 3 has a metal vapor deposition layer 3a laminated on the biaxially oriented polypropylene film 2 so as to be in direct contact with the biaxially oriented polypropylene film 2, and an electrode lead-out portion 3b formed on part of the upper surface of the metal vapor deposition layer 3a. The metal vapor deposition layer 3a functions as an electrode when the metal layer-integrated polypropylene film is used as a capacitor. The electrode lead-out portion 3b is a portion known as a heavy edge.

[0100] The metal used for the metal vapor deposition layer 3a and the electrode extraction portion 3b may be, for example, a single metal such as zinc, lead, silver, chromium, aluminum, copper, or nickel, or a mixture or alloy of two or more of these metals. However, taking into consideration the environment, economy, and capacitor performance, zinc and aluminum are preferred.

[0101] The layer structure of the metal layer is not particularly limited. The metal layer may be a single layer or may be a multi-layer structure having the same or different compositions.

[0102] The thickness of the metal vapor deposition layer 3a and the electrode lead-out portion 3b is controlled by the film resistance (resistance per unit area, unit: Ω / sq). Since the resistance is inversely proportional to the thickness, the lower the film resistance, the thicker the film. When the metal layer-integrated polypropylene film 1 is used as a capacitor, insulation may occur at locations of the metal layer-integrated polypropylene film 1 that are weak in terms of withstanding voltage. When insulation breakdown occurs, heat is generated instantaneously, causing the metal vapor deposition layer 3a to evaporate and the insulation to be restored (self-healing). When the metal vapor deposition layer 3a evaporates (self-healing occurs), the function of the capacitor is restored, allowing it to be used continuously.

[0103] The ease of evaporation of the metal vapor deposition layer 3a (ease of self-healing to occur) varies depending on the film resistance (film thickness). The film resistance of the metal vapor deposition layer 3a is preferably 1 Ω / sq or more, and more preferably 5 Ω / sq or more. If the film resistance is lower than 1 Ω / sq, evaporation of the metal vapor deposition layer 3a is unlikely to occur (self-healing is unlikely to occur), which is undesirable because it increases the risk of fire due to heat generation caused by leakage current flow due to insulation breakdown.

[0104] The film resistance of the metal deposition layer 3a is preferably 30 Ω / sq or less, more preferably 27 Ω / sq or less. If the film resistance exceeds 30 Ω / sq, the metal deposition layer 3a is likely to evaporate (self-healing is likely to occur), and the capacitance of the capacitor is likely to decrease significantly, which is not preferable.

[0105] The film resistance of the electrode extraction portion 3b (heavy edge) is preferably 1 Ω / sq or more and 7 Ω / sq or less, and more preferably 2 Ω / sq or more and 6 Ω / sq or less.

[0106] 2. Polypropylene film manufacturing method The polypropylene film of the present invention is preferably biaxially stretched as described above. When the polypropylene film of the present invention is a biaxially stretched polypropylene film, the biaxially stretched polypropylene film can be produced by a commonly known method for producing a biaxially stretched polypropylene film. For example, the polypropylene film can be produced by producing a cast sheet from a polypropylene resin composition obtained by mixing the first polypropylene resin and the second polypropylene resin, or the first polypropylene resin together with other resins, additives, etc. as necessary, and then biaxially stretching the cast sheet.

[0107] In one embodiment of the present invention, as described below, it is preferable to set the heat melting temperature in the production of the cast sheet to a relatively high temperature, to set the cooling drum temperature in the production of the cast sheet to a relatively high temperature, to set the longitudinal stretching temperature to a relatively high temperature, and to appropriately adjust other stretching conditions. It is preferable to set the heating and melting temperature at a relatively high temperature, and to set the cooling drum temperature or the longitudinal stretching temperature at a relatively high temperature in the production of a cast sheet.

[0108] 2-1. Preparation of polypropylene resin composition The method for preparing the polypropylene resin composition is not particularly limited, and examples thereof include a method in which the first polypropylene resin and the second polypropylene resin, or polymer powder or pellets of the first polypropylene resin, are dry-blended using a mixer or the like, together with other resins, additives, etc., as necessary; and a method in which the first polypropylene resin and the second polypropylene resin, or polymer powder or pellets of the first polypropylene resin, together with other resins, additives, etc., as necessary, are supplied to a kneader and melt-kneaded to obtain a melt blend resin composition.

[0109] The mixer and kneader are not particularly limited. The kneader may be of a single screw type, a twin screw type, or a multi-screw type having more than one screw. In the case of a twin or more screw type, the kneader may be of either a co-rotating or counter-rotating type.

[0110] In the case of blending by melt kneading, the kneading temperature is not particularly limited as long as good kneading can be obtained, but is preferably in the range of 170 to 320°C, more preferably in the range of 200°C to 300°C, and further preferably in the range of 230°C to 270°C. In order to suppress deterioration during kneading and mixing of the resin, an inert gas such as nitrogen may be purged into the kneader. The melt-kneaded resin can be pelletized to an appropriate size using a commonly known granulator to obtain pellets of the melt blend resin composition.

[0111] When preparing the polypropylene resin composition, a primary agent as an antioxidant explained in the above section on additives can be added for the purpose of suppressing thermal and oxidative degradation in the extruder.

[0112] When the polypropylene resin composition contains a primary agent, the content thereof is preferably 1000 mass ppm to 5000 mass ppm relative to the mass of the resin component (mass of the resin component as a whole). Most of the antioxidant for this purpose is consumed in the molding process in the extruder, and almost none remains in the film after film formation.

[0113] The hindered phenol-based antioxidant having a carbonyl group, which has been described above in the section on additives, can be added to the polypropylene resin composition as a secondary agent.

[0114] When the polypropylene resin composition contains a hindered phenol-based antioxidant having a carbonyl group, the content thereof is preferably 100 ppm by mass to 10,000 ppm by mass, more preferably 3,000 ppm by mass to 7,000 ppm by mass, based on the mass of the resin component (mass when the resin components are taken as the whole). In the extruder, the hindered phenol-based antioxidant having a carbonyl group is also consumed to a not small extent.

[0115] When the polypropylene resin composition does not contain a primary agent, a larger amount of the hindered phenol-based antioxidant having a carbonyl group can be used. This is because the consumption of the hindered phenol-based antioxidant having a carbonyl group increases in the extruder. When the polypropylene resin composition does not contain a primary agent and contains the hindered phenol-based antioxidant having a carbonyl group, the content is 4000 mass ppm to 8000 mass ppm or less with respect to the mass of the resin component (mass when the resin component is taken as the whole).

[0116] 2-2. Making the cast sheet The cast sheet is made of a dry blend resin composition and / or a melt blend resin composition. The pellets of the resin composition are fed to an extruder, heated and melted, passed through a filter, and then heated and melted at a relatively high temperature, preferably 255°C to 320°C, more preferably 260°C to 300°C, and even more preferably 265°C to 280°C, melt-extruded from a T-die, and cooled and solidified by at least one metal drum maintained at a relatively high temperature, preferably 96°C to 120°C, more preferably 96°C to 110°C, and even more preferably 96°C to 100°C (casting temperature). In this case, it is preferable to press the melt-extruded resin composition against the metal drum with an air knife. The surface in contact with the metal drum is the first surface, and the opposite surface (the surface on the air knife side) is the second surface.

[0117] The thickness of the cast sheet is not particularly limited as long as the desired polypropylene film can be obtained, but is preferably 0.05 mm to 2 mm, more preferably 0.1 mm to 1 mm.

[0118] During the process of producing a cast sheet (especially in the extruder), polypropylene undergoes thermal degradation (oxidative degradation) and shear degradation to a certain extent. The degree of progression of such degradation, i.e., changes in molecular weight distribution and stereoregularity, can be suppressed by purging the extruder with nitrogen (to suppress oxidation), the screw shape in the extruder (shear force), the internal shape of the T-die during casting (shear force), the amount of antioxidant added (to suppress oxidation), and the winding speed during casting (extension force).

[0119] 2-3. Stretching process The biaxially stretched polypropylene film can be produced by subjecting the cast sheet to a stretching treatment. As a stretching method, a sequential biaxial stretching method is preferred. In the sequential biaxial stretching method, the cast sheet is first kept at a relatively high temperature, preferably 142 to 180°C, more preferably 143 to 160°C, and even more preferably 144 to 150°C, and is stretched in the machine direction by preferably 3 to 7 times, more preferably 4 to 6 times, between rolls with a speed difference, and immediately cooled to room temperature. Subsequently, the stretched film is introduced into a tenter and transversely stretched by 3 to 11 times (preferably 8 to 11 times) in the width direction at a temperature of preferably 150 to 160°C, more preferably 150 to 159°C, even more preferably 150 to 158°C, and even more preferably 150 to 157°C, and then relaxed and heat-set, and wound into a roll.

[0120] The longitudinal stretching speed is preferably 100 to 100,000% / sec, more preferably 1,000 to 80,000% / sec, even more preferably 60,000 to 70,000% / sec, and even more preferably 65,000 to 70,000% / sec. The transverse stretching speed is preferably 10 to 800% / sec, more preferably 100 to 600% / sec, even more preferably 300 to 400% / sec, and even more preferably 300 to 350% / sec.

[0121] The film wound into a roll is subjected to an aging treatment in an atmosphere of about 20 to 45°C, and then, while being rewound (unwound), it is slit (cut) to the desired product width using a slitter or the like, and each piece is then wound again.

[0122] Such a stretching process results in a film with excellent mechanical strength and rigidity.

[0123] The polypropylene film is preferably subjected to an online or offline corona discharge treatment after the stretching and heat setting processes. By performing the corona discharge treatment, the adhesive properties in the subsequent processes such as the metal deposition processing process can be improved. The corona discharge treatment can be performed by using a known method. It is preferable to perform the treatment using air, carbon dioxide gas, nitrogen gas, or a mixture thereof as the atmospheric gas.

[0124] 3. Manufacturing method of metal layer integrated polypropylene film The metal layer-integrated polypropylene film of the present invention can be obtained, for example, by a method including a step of laminating a metal layer on one or both sides of the polypropylene film of the present invention. Examples of the method for laminating a metal layer on one or both sides of the polypropylene film of the present invention include a vacuum deposition method and a sputtering method. From the viewpoints of productivity and economy, the vacuum deposition method is preferred. Examples of the vacuum deposition method include a crucible method and a wire method in general, but are not particularly limited, and an optimal method can be appropriately selected.

[0125] In the vacuum deposition method, the thickness of the metal layer is controlled by the film resistance. As a deposition condition in the vacuum deposition method, the film resistance of the metal deposition layer 3a is preferably 1 Ω / □Ω / sq or more, more preferably 5 Ω / □Ω / sq or more. In addition, the film resistance of the metal deposition layer 3a is preferably 30 Ω / □Ω / sq or less, more preferably 27 Ω / □Ω / sq or less.

[0126] The film resistance of the electrode extraction portion 3b (heavy edge) is preferably 1 Ω / □Ω / sq or more and 7 Ω / □Ω / sq or less, and more preferably 2 Ω / □Ω / sq or more and 6 Ω / □Ω / sq or less.

[0127] The margin pattern when laminating the metal layer by vapor deposition is not particularly limited, but from the viewpoint of improving the characteristics such as safety of the capacitor, it is preferable to apply a pattern including a so-called special margin, such as a fishnet pattern or a T-margin pattern, on one side of the film. This is effective in terms of increasing safety and preventing destruction and short circuits of the capacitor.

[0128] As a method for forming the margin, a generally known method such as a tape method or an oil method can be used without any limitation.

[0129] After laminating a metal layer on one or both sides of the polypropylene film of the present invention, a post-heat treatment may be further performed. Examples of the post-heat treatment conditions include application of silicone oil heated to 120 to 130°C.

[0130] A preferred method for producing the metal layer-integrated polypropylene film of the present invention will be described below with reference to Fig. 2. By controlling the deposition conditions (mainly the voltage speed ratio and discharge amount per unit width of the cooling roll) as described later, the cumulative density of dielectric breakdown points can be suppressed.

[0131] Fig. 2 is a schematic diagram for explaining a method for producing a metal layer-integrated polypropylene film. The metal layer-integrated polypropylene film is preferably produced by a production apparatus described below. As shown in Fig. 2, the production apparatus for a metal layer-integrated polypropylene film includes a dielectric film supply section 101, an insulating margin forming section 102, a special deposition pattern margin forming section 103, a metal deposition section 104, a DC magnetron discharge electrode 105, and a metal layer-integrated film winding section 106.

[0132] The dielectric film supply unit 101 supports a biaxially oriented polypropylene film roll 2R around which the biaxially oriented polypropylene film 2 is wound, and supplies the biaxially oriented polypropylene film 2. The biaxially oriented polypropylene film 2 supplied from the biaxially oriented polypropylene film roll 2R is transported to an insulating margin forming unit 102.

[0133] The insulating margin forming section 102 applies oil in a pattern corresponding to the pattern of the insulating margin 4 to the metallized surface 2a of the biaxially oriented polypropylene film 2 to form an oil mask. The oil mask is intended to prevent metal particles from adhering to the portion of the metal layer-integrated polypropylene film 1 that will become the insulating margin during the vapor deposition process. The insulating margin forming unit 102 vaporizes oil stored in an oil tank and applies the oil directly to the metal vapor deposition surface 2a of the polypropylene film 2 from a nozzle (slit) provided in the tank, forming an oil mask.

[0134] The special vapor deposition pattern margin forming unit 103 applies oil to the metal vapor deposition surface 2a of the biaxially oriented polypropylene film 2 in a pattern that roughly corresponds to the electrode pattern of the metal vapor deposition layer 3a, forming an oil mask. The oil mask is intended to prevent metal particles from adhering to the vertical and horizontal margins of the metal layer-integrated polypropylene film 1 during the vapor deposition process. The special vapor deposition pattern margin forming unit 103 is equipped with an oil tank 103. The oil tank 103a has an anilox roll 103b, a transfer roll 103c, a printing roll 103d, and a backup roll 103e. The oil tank 103a stores oil. The oil is vaporized and sprayed out from the nozzle. The anilox roll 103b and the transfer roll 103c rotate with the oil sprayed from the nozzle of the oil tank 103a attached to their outer circumferential surfaces. The backup roll 103e is attached to the printing roll 103 via a polypropylene film 2. d and abuts against the cooling roll contact surface 2b of the biaxially oriented polypropylene film 2.

[0135] The biaxially oriented polypropylene film 2 that has passed through the insulating margin forming section 102 and the special vapor deposition pattern margin forming section 103 is transported to the vapor deposition section 104 .

[0136] The deposition unit 104 includes metal vapor generation units 104a and 104b. The biaxially oriented polypropylene film 2 is opposed to the electrode 104b and a cooling roll 104c is provided. The metal vapor generating unit 104a generates metal vapor by supplying the metal vapor onto a heated boat by passing an electric current through a metal wire, which is the material of the metal vapor deposition layer 3a, and vaporizes the metal vapor onto the metal vapor deposition surface 2a of the biaxially oriented polypropylene film 2. The metal vapor generating unit 104b heats and evaporates the metal, which is the material of the electrode extraction unit 3b, to generate metal vapor, which is vaporized by the metal vapor generating unit 104a on the metal vapor deposition layer 3a previously formed on the metal vapor deposition surface 2a of the biaxially oriented polypropylene film 2. As a result, the metal vapor deposition layer at the electrode extraction unit 3b becomes thicker than the metal vapor deposition layer at the other parts, forming a heavy edge structure. The metal vapor generated by the metal vapor generating units 104a and 104b adheres to the parts other than the oil mask formed on the metal vapor deposition surface 2a of the biaxially oriented polypropylene film 2 to form the metal vapor deposition electrode 3.

[0137] A voltage is applied to the cooling roll 104C, and the application of the voltage causes the cooling roll contact surface 2b of the biaxially oriented polypropylene film 2 to come into close contact with the cooling roll 104C, cooling the biaxially oriented polypropylene film 2. The degree of contact of the cooling roll contact surface 2b with the cooling roll 104C is proportional to the voltage (V) applied to the cooling roll 104C, and is inversely proportional to the width (m) of the cooling roll and the deposition rate (m / min). For this reason, the voltage speed ratio per unit width of the cooling roll (unit: V·min / m 2 The higher the voltage speed ratio per unit width of the cooling roll, the closer the contact surface 2b of the biaxially oriented polypropylene film 2 to the cooling roll 104C, the higher the cooling efficiency, and the more it is possible to prevent damage to the evaporated metal due to heat. The voltage speed ratio per unit width of the cooling roll is 0.20 V·min / m 2 More than 0.45V min / m2 The voltage speed ratio per unit width of the cooling roll is preferably 0.20 V min / m or less. 2 If it is smaller than this, the cooling roll contact surface 2b of the biaxially oriented polypropylene film 2 will not be in sufficient contact with the cooling roll 104C, resulting in poor cooling efficiency, and the biaxially oriented polypropylene film 2 or the metal layer integrated polypropylene film 1 will be thermally damaged. As a result, the voltage resistance of the metal layer integrated polypropylene film 1 will decrease, and when it is used as a capacitor, its life will be shortened due to insulation breakdown and heat generation. In addition, if the voltage speed ratio per unit width of the cooling roll is 0.45 V·min / m 2 If it is larger, the cooling roll contact surface 2 of the biaxially oriented polypropylene film 2 Since b is sufficiently in close contact with the cooling roll 104C, the cooling efficiency is improved, and the thermal damage of the biaxially oriented polypropylene film 2 or the metal layer integrated polypropylene film 1 is reduced, but discharge is likely to occur between the biaxially oriented polypropylene film 2 and the roll 104C, or between the metal layer integrated polypropylene film 1 and the roll 104C. If discharge occurs, the biaxially oriented polypropylene film 2 or the metal layer integrated polypropylene film 1 is electrically damaged, resulting in damage. Even if discharge does not occur, the metal layer integrated polypropylene film 1 is easily charged, and when the metal layer integrated polypropylene film 1 is wound into a roll by the metal layer integrated film winding section 106, electrical damage occurs due to the discharge of static electricity in the metal layer integrated polypropylene film 1, resulting in damage to the metal layer integrated polypropylene film 1. If the biaxially oriented polypropylene film 2 or the metal layer integrated polypropylene film 1 is electrically damaged and damaged, the voltage resistance is reduced, and when it is made into a capacitor, it is likely to cause a reduction in life due to insulation breakdown or heat generation. Furthermore, when the metal layer-integrated polypropylene film 1 becomes electrostatically charged, its slipperiness deteriorates, making it more likely to wrinkle during winding at the metal layer-integrated film winding section 106 or during the element winding process for producing a capacitor. Furthermore, during the press processing process after element winding for producing a capacitor, buckling is more likely to occur due to the deterioration of slipperiness caused by electrostatic charging. Wrinkles and buckling are undesirable as they damage the metal layer-integrated polypropylene film 1 and can cause insulation breakdown or heat generation in the capacitor, shortening its lifespan. The voltage speed ratio per unit width of the cooling roll is 0.24 V·min / m 2 More than 0.41V min / m 2 The following is even more preferred:

[0138] From the viewpoint of preventing thermal damage to the biaxially oriented polypropylene film 2 or the metal layer-integrated polypropylene film 1, the temperature of the cooling roll 104C is preferably −18° C. or lower, and more preferably −19° C. or lower.

[0139] The metal layer-integrated polypropylene film 1, which is formed by forming the metal vapor deposition electrode 3 on the biaxially oriented polypropylene film 2 in the vapor deposition unit 104, passes through the static electricity removing unit 105. The static electricity removing unit 105 is equipped with DC magnetron discharge electrodes 105a, 105b, 105c, and 105d, and argon gas ions are generated by supplying power to the DC magnetron discharge electrode units 105a, 105b, 105c, and 105d while argon gas is being supplied. When the metal layer-integrated polypropylene film 1 passes through the static electricity removing unit 105 while argon gas ions are being generated, the static electricity of the metal layer-integrated polypropylene film 1 is neutralized by the argon gas ions, and the metal layer-integrated polypropylene film roll 1R is prevented from being charged. The degree of neutralization of static electricity provided by argon gas ions to metal layer integrated polypropylene film 1 can be expressed as the discharge amount, which is proportional to the total power (W) of DC magnetron discharge electrode portions 105a, 105b, 105c, and 105d, and inversely proportional to the width (m) of the DC magnetron discharge electrode portions and the deposition rate (m / min). Here, the width of each of DC magnetron discharge electrode portions 105a, 105b, 105c, and 105d is the same, and the width (m) of the DC magnetron discharge electrode portion is the width per portion, not the total width of DC magnetron discharge electrode portions 105a, 105b, 105c, and 105d. The discharge amount is 1.5 W·min / m 2 Above, 3.7W min / m 2 A discharge rate of 3.7 W min / m is preferable. 2 If it is larger than 1.5 W·min / m, the discharge of the DC magnetron discharge electrodes 105a, 105b, 105c, and 105d will be too strong, causing electrical damage to the metal layer-integrated polypropylene film 1, and even if no discharge occurs, the metal layer-integrated polypropylene film 1 will be charged by ions of the argon gas. 2If the value is smaller than this, the neutralization of the static electricity in the metal layer-integrated polypropylene film 1 is insufficient, and the film becomes charged. If the metal layer-integrated polypropylene film 1 is electrically damaged and damaged, its voltage resistance decreases, and when it is made into a capacitor, it is likely to suffer from insulation breakdown or heat generation, resulting in a shortened lifespan. Furthermore, if the metal layer-integrated polypropylene film 1 becomes charged, electrical damage will occur due to the discharge of static electricity from the metal layer-integrated polypropylene film 1 when it is wound into a roll by the metal layer-integrated film winding section 106, This causes damage to the metal layer-integrated polypropylene film 1. When the metal layer-integrated polypropylene film 1 is damaged, its voltage resistance decreases, and when it is made into a capacitor, it is likely to cause a shortened lifespan due to insulation breakdown or heat generation. In addition, when the metal layer-integrated polypropylene film 1 becomes charged, its slipperiness deteriorates, so that it is likely to wrinkle during winding at the metal layer-integrated film winding section 106 or during the element winding process in the capacitor production. In addition, during the press processing process after winding the element in the capacitor production, buckling is likely to occur due to the deterioration of slipperiness caused by charging. Wrinkles and buckling are undesirable as they damage the metal layer-integrated polypropylene film 1 and cause a shortened lifespan due to insulation breakdown or heat generation in the capacitor. The discharge amount is 1.9 W·min / m 2 Above, 3.3W min / m 2 The following is more preferred:

[0140] The metal layer-integrated polypropylene film 1 that has passed through the static electricity removing unit 105 is transported to the metal layer-integrated film winding unit 106 and wound up to become a metal layer-integrated polypropylene film roll 1R.

[0141] Using the above-mentioned production apparatus, a metal vapor deposition electrode 3 is formed on the metal vapor deposition surface 2a of the polypropylene film 2, and a metal layer-integrated polypropylene film 1 can be obtained.

[0142] 4. Capacitor In one aspect, the present invention relates to a capacitor (sometimes referred to as "the capacitor of the present invention" in this specification) including the metal layer-integrated polypropylene film of the present invention. This will be described below.

[0143] The capacitor of the present invention not only has a constant level of capacitance stability over long-term use, but also has excellent insulation resistance stability under high temperature and high voltage load.

[0144] For example, the capacitance change rate of the capacitor of the present invention, measured by a high-temperature short-time pressure test described in the Examples, is preferably −5% or more, more preferably −2% or more. The upper limit of the capacitance change rate is not particularly limited, and is, for example, 2%, 1%, 0.5%, 0.2%, or 0%.

[0145] For example, the capacitance change rate of the capacitor of the present invention, measured by a 105°C life test described in the Examples, is preferably -25% or more, more preferably -20% or more, and even more preferably -15% or more. The upper limit of the capacitance change rate is not particularly limited, and is, for example, 2%, 1%, 0.5%, 0.2%, or 0%.

[0146] For example, the insulation resistance value of the capacitor of the present invention, measured by the 105°C life test described in the Examples, is preferably 20 MΩ or more, more preferably 300 MΩ or more, even more preferably 500 MΩ or more, even more preferably 800 MΩ or more, and particularly preferably 1000 MΩ or more. There is no particular upper limit to the insulation resistance value, and it is, for example, 20000 MΩ, 15000 MΩ, or 13000 MΩ.

[0147] For example, the capacitance change rate of the capacitor of the present invention, measured by a 115°C life test described in the Examples, is preferably -30% or more, more preferably -25% or more, and even more preferably -20% or more. The upper limit of the capacitance change rate is not particularly limited, and is, for example, 2%, 1%, 0.5%, 0.2%, or 0%.

[0148] For example, the insulation resistance value of the capacitor of the present invention, measured by the 115°C life test described in the Examples, is preferably 20 MΩ or more, more preferably 100 MΩ or more, even more preferably 150 MΩ or more, even more preferably 200 MΩ or more, and particularly preferably 250 MΩ or more. There is no particular upper limit to the insulation resistance value, and it can be, for example, 20,000 MΩ, 15 000MΩ, or 13000MΩ.

[0149] For example, the insulation resistance of the capacitor of the present invention is measured by the high voltage application test described in the Examples. The insulation resistance is preferably 20 MΩ or more, more preferably 3000 MΩ or more, even more preferably 5000 MΩ or more, even more preferably 8000 MΩ or more, and particularly preferably 10000 MΩ or more. The upper limit of the insulation resistance is not particularly limited, and is, for example, 20000 MΩ, 15000 MΩ, or 13000 MΩ.

[0150] In one embodiment of the present invention, in the process of producing a capacitor, for example, a film winding process is performed. For example, two pairs of metal layer-integrated polypropylene films of the present invention are overlapped and wound so that the metal layers of the metal layer-integrated polypropylene film of the present invention and the polypropylene film of the present invention are alternately laminated, and further, the insulating margin parts are on opposite sides. In this case, it is preferable to laminate the two pairs of metal layer-integrated polypropylene films of the present invention with a shift of 1 to 2 mm so that the electrode extraction parts are outward from the insulating margin parts of the other pair. The winding machine used is not particularly limited, and for example, an automatic winding machine 3KAW-N2 type manufactured by Kaito Seisakusho Co., Ltd. can be used.

[0151] When manufacturing a flat capacitor, after winding, the resulting wound product is usually pressed. Pressing promotes tightening of the capacitor and element formation. From the viewpoint of controlling and stabilizing the interlayer gap, the optimum pressure to be applied varies depending on the thickness of the film of the present invention, but is generally a load of 1 to 20 kgf / cm. 2 It is.

[0152] Next, metal is sprayed onto both end faces of the winding to provide metallikon electrodes, thereby completing a capacitor.

[0153] The capacitor is further subjected to a predetermined heat treatment. That is, the present invention includes a step of subjecting the capacitor to a heat treatment (hereinafter, sometimes referred to as "thermal aging"). The heat treatment temperature is not particularly limited, but is, for example, 80 to 190°C. The method of subjecting the capacitor to heat treatment is not particularly limited, but may be appropriately selected from known methods including, for example, a method using a thermostatic bath under atmospheric pressure or a vacuum atmosphere, a method using high-frequency induction heating, and the like. The time for which the heat treatment is performed is not particularly limited, but, for example, when a thermostatic bath is used under a vacuum atmosphere, it is preferably 1 hour or more from the viewpoint of obtaining mechanical and thermal stability, and more preferably 3 hours or more, but more preferably 20 hours or less from the viewpoint of preventing molding defects such as heat wrinkles and molding.

[0154] By carrying out the heat treatment, the effect of heat aging can be obtained. Specifically, the gap between the films constituting the capacitor based on the metal layer-integrated polypropylene film of the present invention is reduced, corona discharge is suppressed during the use of the capacitor, and the internal structure of the metal layer-integrated polypropylene film of the present invention is changed and crystallization is promoted. As a result, it is considered that the voltage resistance is further improved.

[0155] Lead wires are usually welded to the metallikon electrodes of the capacitor that has been heat aged. Although not particularly limited, it is preferable to encapsulate the capacitor in a case and pot it with epoxy resin to impart weather resistance, particularly to prevent deterioration due to humidity.

[0156] The capacitor of the present invention using the polypropylene film of the present invention can be suitably used in high temperature environments, and can be a small-sized capacitor with a high capacity (for example, a capacitance of 5 μF or more, preferably 10 μF or more, more preferably 20 μF or more, even more preferably 30 μF or more, and particularly preferably 40 μF or more. There is no particular upper limit to the capacitance, and it can be, for example, 100 μF, 80 μF, 70 μF, or 60 μF). Therefore, The capacitor of the present invention can be used as a high-voltage capacitor, a filter capacitor and a smoothing capacitor for various switching power supplies, converters, inverters, etc., which are used in electronic devices, electric devices, etc. In addition, the capacitor of the present invention can also be suitably used as an inverter capacitor, a converter capacitor, etc., which control the drive motor of electric vehicles and hybrid vehicles, for which demand has been increasing in recent years. EXAMPLES

[0157] The present invention will be described in detail below using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. In addition, unless otherwise specified, parts and % indicate "parts by mass" and "% by mass", respectively.

[0158] (1) Preparation of polypropylene resin The polypropylene resins used to produce the biaxially oriented polypropylene films of the Examples and Comparative Examples are shown in Table 1.

[0159] Resin A shown in Table 1 is a product manufactured by Prime Polymer Co., Ltd. Resin B is S802M manufactured by Daehan Petrochemical Co., Ltd. Both Resins A and B are linear homopolypropylene resins.

[0160] Table 1 shows the number average molecular weight (Mn), weight average molecular weight (Mw), z-average molecular weight (Mz), molecular weight distribution (Mw / Mn), molecular weight distribution (Mz / Mn), melt flow rate (MFR), and heptane insolubles (HI) of the linear homopolypropylene resin. These values ​​are in the form of raw material resin pellets. The measurement method is as follows.

[0161] (1-1) Measurement of number average molecular weight (Mn), weight average molecular weight (Mw), z-average molecular weight (Mz), molecular weight distribution (Mw / Mn), and molecular weight distribution (Mz / Mn) of linear polypropylene resin Using GPC (gel permeation chromatography) under the following conditions, the number average molecular weight (Mn), weight average molecular weight (Mw), z-average molecular weight (Mz), molecular weight distribution (Mw / Mn), and molecular weight distribution (Mz / Mn) of each resin were measured.

[0162] Specifically, a high-temperature GPC device with a built-in differential refractometer (RI), HLC-8121GPC-HT model manufactured by Tosoh Corporation, was used. Three GMHHR-H(20)HT columns were connected and used. Measurements were performed at a column temperature of 140°C, with trichlorobenzene as the eluent flowing at a flow rate of 1.0 ml / min. A calibration curve for the molecular weight M was created using standard polystyrene from Tosoh Corporation, and the measured values ​​were converted to the molecular weight of polypropylene using the Q-factor to obtain the number average molecular weight (Mn), weight average molecular weight (Mw), and z-average molecular weight (Mz). The values ​​of Mw and Mn were used to obtain the molecular weight distribution (Mw / Mn). The values ​​of Mz and Mn were also used to obtain the molecular weight distribution (Mz / Mn).

[0163] (1-2) Measurement of Melt Flow Rate (MFR) The melt flow rate (MFR) of each resin in the form of raw resin pellets was measured in accordance with JIS K 7210 condition M using a melt indexer manufactured by Toyo Seiki Co., Ltd. Specifically, a sample weighing 4 g was inserted into a cylinder with a test temperature of 230°C and preheated for 3.5 minutes under a load of 2.16 kg. The weight of the sample extruded from the bottom hole in 30 seconds was then measured to determine the MFR (g / 10 min). The above measurement was repeated three times, and the average value was taken as the measured MFR value. The results are shown in Table 1.

[0164] (1-3) Measurement of heptane insolubles (HI) For each resin, a measurement sample of about 3 g was prepared by pressing to 10 mm x 35 mm x 0.3 mm. Next, about 150 mL of heptane was added and Soxhlet extraction was performed for 8 hours. The heptane insoluble matter was calculated from the sample mass before and after extraction. The results are shown in Table 1.

[0165] (1-4) Physical properties of polypropylene resin

[0166] [Table 1]

[0167] (2) Preparation of biaxially oriented polypropylene film Resin A and resin B were dry blended. The mixing ratio was (resin A):(resin B) = 75:25 by mass ratio. After that, the dry blended resin was used and melted at a resin temperature of 270 ° C, extruded using a T-die, and then wrapped around a metal drum whose surface temperature was kept at 98 ° C to solidify. As a result, a cast sheet with a thickness of 115 μm was produced. At this time, the cast sheet was produced while pressing the melt-extruded resin composition against the metal drum with an air knife. The obtained unstretched cast sheet was kept at a temperature of 146 ° C, passed between rolls with a speed difference, stretched 5 times in the flow direction at a stretching speed of 67300% / sec, and immediately cooled to room temperature. Subsequently, the stretched film was introduced into a tenter, stretched 10 times in the width direction at a temperature of 155 ° C and a stretching speed of 335% / sec, and then relaxed and heat-set. Next, the film surface (the side contacting the metal drum) was subjected to a 25 W · min / m 2 After the film was subjected to a corona discharge treatment in the atmosphere at a treatment speed of 100 rpm, it was taken up and subjected to an aging treatment in an atmosphere at about 30° C. As a result, a biaxially oriented polypropylene film having a thickness of 2.3 μm was obtained.

[0168] (3) Measurement of physical properties of biaxially oriented polypropylene film (3-1) Thickness measurement of biaxially oriented polypropylene film The thickness (unit: μm) of the biaxially stretched polypropylene film prepared in (2) above was measured. Specifically, the thickness was measured in accordance with JIS-C2330, except that the thickness was measured at 100±10 kPa using a paper thickness measuring instrument MEI-11 manufactured by Citizen Seimitsu Co., Ltd. As a result, the thickness of the biaxially stretched polypropylene film was 2.3 μm.

[0169] (3-2) Measurement of heat shrinkage rate at 120℃ for biaxially oriented polypropylene film The heat shrinkage (120°C heat shrinkage) (unit: %) of the biaxially stretched polypropylene film prepared in (2) above was measured under the treatment condition of 120°C for 15 minutes. Specifically, a sample was cut out from a roll, and the size of the sample for measuring the 120°C heat shrinkage in the MD direction was 130 mm in the MD direction and 20 mm in the TD direction, and the size of the sample for measuring the 120°C heat shrinkage in the TD direction was 20 mm in the MD direction and 130 mm in the TD direction. Three samples were prepared for measuring the 120°C heat shrinkage in the MD direction and three samples were prepared for measuring the 120°C heat shrinkage in the TD direction. Next, for the three samples for measuring the 120°C heat shrinkage in the MD direction, a marked line was marked at a position 15 mm from each end of the 130 mm in the MD direction. At this time, the distance between the marked lines was 100 mm. For the three samples for measuring the 120°C heat shrinkage in the TD direction, a marked line was marked at a position 15 mm from each end of the 130 mm in the TD direction. At this time, the distance between the marked lines was 100 mm. Next, each sample with the marked lines was hung without load in a hot air circulating thermostatic chamber at 120°C so that the direction in which the 130 mm sample was cut out was vertical, and held for 15 minutes. After that, the sample was cooled to room temperature (23°C), the distance between the marked lines was measured with a ruler, and the heat shrinkage rate (%) of each sample was calculated using the following formula: Heat shrinkage rate (%) = (marked line distance before heating - marked line distance after heating) / marked line distance before heating x 100.

[0170] The average of the heat shrinkage rates of three samples for which the 120°C heat shrinkage rate in the MD direction was measured was taken as the 120°C heat shrinkage rate in the MD direction (%). Also, the average of the heat shrinkage rates of three samples for which the 120°C heat shrinkage rate in the TD direction was measured was taken as the 120°C heat shrinkage rate in the TD direction (%).

[0171] Measurement conditions other than those described here were in accordance with "25. Dimensional change" of JIS C 2151:2019.

[0172] As a result, the heat shrinkage rate at 120°C in the MD direction of the biaxially oriented polypropylene film was 3.7%, and the heat shrinkage rate at 120°C in the TD direction was 0.4%.

[0173] (3-3) Measurement of heat shrinkage rate of biaxially oriented polypropylene film at 140℃ The heat shrinkage (140°C heat shrinkage) (unit: %) of the biaxially oriented polypropylene film prepared in (2) above was measured under the treatment conditions of 140°C for 15 minutes. The 140°C heat shrinkage (%) in the MD direction and the 140°C heat shrinkage (%) in the TD direction were calculated in the same manner as for the 120°C heat shrinkage, except that the 120°C hot air circulation type thermostatic oven was changed to a 140°C hot air circulation type thermostatic oven.

[0174] As a result, the heat shrinkage rate at 140°C in the MD direction of the biaxially oriented polypropylene film was 6.1%, and the heat shrinkage rate at 140°C in the TD direction was 3.1%.

[0175] (3-4) Measurement of tensile modulus of biaxially oriented polypropylene film The tensile modulus (unit: GPa) of the biaxially stretched polypropylene film prepared in (2) above was measured in accordance with JIS K-7127 (1999). Specifically, a sample was cut out from a roll, and the size of the sample for measuring the tensile modulus in the MD direction was 200 mm in the MD direction and 15 mm in the TD direction, and the size of the sample for measuring the tensile modulus in the TD direction was 15 mm in the MD direction and 200 mm in the TD direction. Next, a tensile test was performed using a tension and compression tester (manufactured by Minebea Co., Ltd.) under test conditions (measurement temperature 23°C, chuck distance 100 mm, tensile speed 200 mm / min). Next, the tensile modulus in the MD direction (GPa) and the tensile modulus in the TD direction (GPa) were each determined by automatic analysis using data processing software built into the tester.

[0176] As a result, the tensile modulus of the biaxially oriented polypropylene film in the MD direction was 2.76 GPa, and the tensile modulus in the TD direction was 4.56 GPa.

[0177] (3-5) Haze measurement of biaxially oriented polypropylene film The haze (unit: %) of the biaxially stretched polypropylene film prepared in (2) above was measured in accordance with JIS K 7136:2000 using a haze meter ("NDH-5000" manufactured by Nippon Denshoku Industries Co., Ltd.). A sample was cut out from a roll, and the size of the sample was 50 mm in the MD direction and 100 mm in the TD direction. As a result, the haze of the biaxially stretched polypropylene film was 3.1%.

[0178] (4) Preparation of film rolls after cutting The biaxially oriented polypropylene film prepared in (2) above was unwound from the roll and cut in the width direction using a slitter. When winding the cut polypropylene film, a fiber-reinforced plastic core with an outer diameter of 176 mm was used, and a winding device equipped with a contact pressure roll was used to wind the polypropylene film while applying surface pressure. The cutting conditions were a speed of 300 m / min, unwinding force of 40 N / m, winding tension of 50 N / m, and winding surface pressure of 400 N / m. A rubber contact pressure roll with an outer diameter of 152 mm and a surface hardness of 40° was used, and a biaxially oriented polypropylene roll (film roll after cutting) with a width of 620 mm and a length of 75,000 m was finished. The film was visually observed during winding to confirm that no wrinkles were occurring. In addition, the end surface of the resulting cut film roll was observed, and it was confirmed that no misalignment of 2 mm or more had occurred.

[0179] (5) Preparation of metal layer integrated polypropylene film <Example 1> Using a deposition device (ULVAC, product name: roll-type vacuum deposition device EWE-060), the cooling roll temperature was -22°C, and the voltage speed ratio per unit width of the cooling roll was 0.32 V·min / m. 2 , discharge amount 2.5W min / m 2Under the above conditions, a special deposition pattern margin and an insulating margin were formed on the cut film roll prepared in (4) above to provide film capacitor safety, and aluminum deposition was performed so that the surface resistivity of the metal film was 20Ω / sq, to ​​obtain a polypropylene film integrated with a metal layer. A schematic diagram of the polypropylene film integrated with a metal layer is shown in Figure 1. A schematic diagram of the manufacturing equipment is shown in Figure 2.

[0180] <Example 2> The voltage speed ratio per unit width of the cooling roll is 0.21V·min / m. 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except that the above-mentioned conditions were met.

[0181] <Example 3> The voltage speed ratio per unit width of the cooling roll is 0.44V·min / m. 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0182] <Example 4> Discharge rate 1.6W·min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0183] <Example 5> Discharge rate 3.6W·min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0184] <Example 6> The voltage speed ratio per unit width of the cooling roll is 0.21V·min / m. 2 , discharge rate 3.6W min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0185] <Comparative Example 1> The voltage speed ratio per unit width of the cooling roll is 0.18V·min / m. 2A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0186] <Comparative Example 2> The voltage speed ratio per unit width of the cooling roll is 0.47V·min / m. 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0187] <Comparative Example 3> Discharge rate 1.3W·min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0188] <Comparative Example 4> Discharge rate 3.9W·min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0189] <Comparative Example 5> The voltage speed ratio per unit width of the cooling roll is 0.18V·min / m. 2 , discharge rate 3.9W min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0190] <Comparative Example 6> The voltage speed ratio per unit width of the cooling roll is 0.47V·min / m. 2 , discharge rate 3.9W min / m 2 A metal layer-integrated polypropylene film was obtained in the same manner as in Example 1, except for the above.

[0191] (6) Measurement of physical properties of metal layer integrated polypropylene film For the metal layer-integrated polypropylene films obtained in Examples 1 to 6 and Comparative Examples 1 to 6, the cumulative breakdown point density after a cumulative DC voltage application test of 350 to 425 V / μm at 20°C (425 V / μm cumulative breakdown point density at 20°C) was measured in the following procedure, with the configuration shown in FIG. 3. After applying a DC voltage of 350 V / μm for 1 minute in an environment of 20°C, the number of breakdown points in the window region (100 mm x 10 mm) of the insulating polypropylene film was counted visually. After counting, a DC voltage of 375 V / μm was applied for 1 minute, and the cumulative breakdown points in the window region of the insulating polypropylene film were counted visually. Next, the DC voltage was increased by 25 V / μm at a time, and this operation was repeated up to 425 V / μm, and the DC voltage was applied cumulatively. The test was carried out on five sheets of metal-layered polypropylene film, and the average cumulative number of dielectric breakdown points at 20°C at 425V / μm was calculated based on the window area of ​​the insulating polypropylene film (100mm x 10mm = 1,000mm 2 =0.001m 2 ) and calculate the cumulative dielectric breakdown density (unit: pieces / m 2 The results are shown in Tables 2 and 3.

[0192] (7) Evaluation (7-1) Press processing yield evaluation The metal layer-integrated polypropylene films prepared in the examples and comparative examples were slit into small rolls with a width of 30 mm. Next, of the small rolls of the metal layer-integrated polypropylene films with a width of 30 mm, one small roll with an insulating margin (2 mm in width) on the left side as viewed from the unwinding side and one small roll with an insulating margin (2 mm in width) on the right side as viewed from the unwinding side were used, and two sheets were combined so that the electrode extraction part of each small roll of the metal layer-integrated polypropylene film protruded beyond the insulating margin of the other small roll of the metal layer-integrated polypropylene film, and wound 1350 turns using an automatic winding machine 3KAW-N2 manufactured by Kaito Seisakusho at a winding speed of 4 m / sec, a winding tension of 180 g, and a contact roller contact pressure of 260 g.

[0193] The wound element is subjected to a load of 5.9kgf / cm2 The mixture was then pressed and flattened.

[0194] The side of the elements flattened by the press treatment was observed while the press load was applied to check for buckling of the metal layer-integrated polypropylene film. Any elements that showed buckling were deemed to have failed. The proportion of the number of flattened elements that passed the above criteria was calculated as the press treatment yield rate α for all flattened elements, and the following criteria were applied to evaluate the results. The results are shown in Tables 2 and 3.

[0195] A: α = 100% B: 100%>α≧80% C: 80%>α.

[0196] (7-2) Capacitor performance evaluation The elements flattened by the press process in (7-1) above were subjected to a press load. First, zinc metal was sprayed on the element end surface. The spraying conditions were a feed rate of 20 mm / s, a spraying voltage of 21 V, and a spraying pressure of 0.4 MPa. The spraying was performed to a thickness of 0.6 mm to 0.7 mm to form an electrode extraction part, and the electrode was heat-treated in a vacuum thermostatic chamber at 120°C for 15 hours in a vacuum atmosphere to be thermally cured. In this way, a flat film capacitor was obtained. Then, lead wires were soldered to the element end surface of the flat film capacitor, and the flat film capacitor was sealed with epoxy resin. The epoxy resin was cured by heating at 90°C for 2.5 hours and then at 120°C for another 2.5 hours. The capacitance of the completed capacitors was 50 μF (±3 μF). The obtained capacitors were used in the following six tests.

[0197] (7-2-1) High temperature short-time voltage test of capacitors (rate of change in capacitance) The initial capacitance (C0) of the obtained capacitor before the test was measured using an LCR HiTester 3522-50 manufactured by Hioki E.E. Corporation. Next, a DC voltage of 325 V / μm was applied to the capacitor for 10 seconds in a thermostatic chamber at 105° C. The capacitance was measured in the same manner, and the capacitance change rate (ΔC) before and after the test was calculated using the following formula: ΔC = [(capacitance after voltage application)-C0] / C0×100(%) The calculation was made as follows.

[0198] Next, a DC voltage of 350 V / μm was applied for 10 seconds in a thermostatic chamber at 105°C. The capacitance was measured in the same manner. Next, the DC voltage was increased by 25 V / μm increments in a thermostatic chamber at 105°C, and this operation was repeated up to 425 V / μm, cumulatively applying a DC voltage. The test was performed on two samples, and the average rate of change in capacitance at 425 V / μm was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0199] A: ΔC≧-2% B: -2%>ΔC≧-5% C: -5%>ΔC

[0200] (7-2-2) 105℃ life test of capacitor (rate of change in capacitance) The initial capacitance (C0) of the obtained capacitor before the test was measured using an LCR HiTester 3522-50 manufactured by Hioki E.E. Corporation. Next, a direct current voltage of 325 V / μm was continuously applied to the capacitor for 1,500 hours in a thermostatic chamber at 105° C. After 1,500 hours had elapsed, The capacitance (C1500H105C) of the capacitor was measured in the same manner, and the capacitance change rate (ΔC105C) before and after voltage load was calculated using the following formula: ΔC105C=(C1500H105C-C0) / C0. The test was performed on two samples, and the average capacitance change rate (ΔC105C) was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0201] A: ΔC105C≧-15% B:-15%>ΔC105C≧-25% C:-25%>ΔC105C

[0202] (7-2-3) Capacitor life test at 105℃ (insulation resistance value) The obtained capacitor was placed in a thermostatic chamber at 105°C and subjected to a DC voltage of 325 V / μm for 1, The load was continued for 500 hours. A shielding box SME-8350 was connected to a Hioki E.E. Corporation super insulation resistance meter DSM8104, and the capacitor after 1,500 hours was placed in the shielding box. A DC voltage of 500V was applied, and the insulation resistance value (IR105C) was read after 1 minute. The test was performed on two samples, and the average insulation resistance value (IR105C) was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0203] Measurement conditions other than those described here were in accordance with "4.2.4 Insulation Resistance" of JIS C 5101-16:2009.

[0204] A:IR105C≧500MΩ B: 500MΩ>IR105C≧20MΩ C:20MΩ>IR105C

[0205] (7-2-4) 115℃ life test of capacitor (rate of change in capacitance) The initial capacitance (C0) of the obtained capacitor before the test was measured using an LCR HiTester 3522-50 manufactured by Hioki E.E. Corporation. Next, a direct current voltage of 325 V / μm was continuously applied to the capacitor for 1,500 hours in a thermostatic chamber at 115° C. After 1,500 hours had elapsed, The capacitance (C1500H115C) of the capacitor was measured in the same manner, and the capacitance change rate (ΔC115C) before and after voltage load was calculated using the following formula: ΔC115C=(C1500H115C-C0) / C0. The test was performed on two samples, and the average capacitance change rate (ΔC115C) was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0206] A: ΔC115C≧-20% B:-20%>ΔC115C≧-30% C:-30%>ΔC115C

[0207] (7-2-5) Capacitor life test at 115℃ (insulation resistance value) The obtained capacitor was placed in a thermostatic chamber at 115°C and subjected to a DC voltage of 325 V / μm for 1, The load was continued for 500 hours. A shielding box SME-8350 was connected to a Hioki E.E. Corporation super insulation resistance meter DSM8104, and the capacitor after 1,500 hours was placed in the shielding box. A DC voltage of 500V was applied, and the insulation resistance value (IR115C) was read after 1 minute. The test was performed on two samples, and the average insulation resistance value (IR115C) was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0208] Measurement conditions other than those described here were in accordance with "4.2.4 Insulation Resistance" of JIS C 5101-16:2009.

[0209] A:IR115C≧150MΩ B: 150MΩ>IR115C≧20MΩ C:20MΩ>IR115C

[0210] (7-2-6) High voltage application test for capacitors (insulation resistance value) The obtained capacitor was placed in a thermostatic chamber at 105°C and a DC voltage of 1200V was continuously applied for 10 minutes. A shielding box SME-8350 was connected to a Hioki E.E. Corporation ultra insulation resistance meter DSM8104, and the capacitor after 10 minutes was placed in the shielding box. A DC voltage of 500V was applied, and the insulation resistance value (IR10) after 1 minute was read. The test was performed on two samples, and the average insulation resistance value (IR10) was evaluated according to the following criteria. The results are shown in Tables 2 and 3.

[0211] Measurement conditions other than those described here were in accordance with "4.2.4 Insulation Resistance" of JIS C 5101-16:2009.

[0212] A:IR10≧5000MΩ B: 5000MΩ>IR10≧20MΩ C:20MΩ>IR10

[0213] [Table 2]

[0214]

Table 3

Claims

1. A metal layer-integrated polypropylene film having a polypropylene film and a metal layer laminated on one or both sides of the polypropylene film, the film having a cumulative dielectric breakdown point density of 1000 / m after a cumulative DC voltage application test at 20°C and 350 to 425 V / μm. 2 The following is a metal layer-integrated polypropylene film.

2. The metal layer-integrated polypropylene film according to claim 1, wherein the polypropylene film has a thickness of 1.0 to 3.0 μm.

3. The metal layer-integrated polypropylene film according to claim 1 or 2, wherein the heat shrinkage rate of the polypropylene film in a first direction is 0 to 8% and the heat shrinkage rate of the polypropylene film in a second direction perpendicular to the first direction is -2 to 2% when treated at 120°C for 15 minutes.

4. The metal layer-integrated polypropylene film according to any one of claims 1 to 3, wherein the heat shrinkage rate of the polypropylene film in a first direction is 0 to 10% and the heat shrinkage rate of the polypropylene film in a second direction perpendicular to the first direction is -1 to 5% when treated at 140°C for 15 minutes.

5. The metal layer-integrated polypropylene film according to any one of claims 1 to 4, wherein the polypropylene film has a tensile modulus of elasticity in a first direction of 1.5 GPa or more and a tensile modulus of elasticity in a second direction perpendicular to the first direction of 3 GPa or more.

6. The metal layer-integrated polypropylene film according to any one of claims 1 to 5, wherein the polypropylene film is a biaxially oriented film.

7. The metal layer-integrated polypropylene film according to any one of claims 1 to 6, wherein the polypropylene film is a single layer film.

8. The metal layer-integrated polypropylene film according to any one of claims 1 to 7, which is for a capacitor.

9. A capacitor comprising the metal layer-integrated polypropylene film according to any one of claims 1 to 8.

10. The capacitor according to claim 9, comprising a roll of the metal layer-integrated polypropylene film according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Biaxially stretched polypropylene film for capacitors, metallized film, and film capacitor