A one-component epoxy resin composition with glycidyl ether of diphenolic bis-carbamate addresses mechanical and thermal issues, providing stable and environmentally friendly epoxy resins with enhanced properties and processability.

JP2024153927AInactive Publication Date: 2024-10-29CHANDA CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024133393
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-06-05
Filing Date
2024-08-08
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing epoxy resins have poor mechanical properties, chemical inertness, and heat resistance, and conventional two-part compositions require separate handling, complicating the packaging and usage process.

Method used

Development of a one-component epoxy resin composition containing a glycidyl ether of diphenolic bis-carbamate with a curing agent, which provides good thermal stability and mechanical properties, and includes a curing reaction at elevated temperatures using additives to form a crosslinked network structure.

Benefits of technology

The composition offers improved thermal stability, mechanical properties, and storage stability without phase separation, while also being environmentally friendly by utilizing recycled polymers and avoiding carbon dioxide emissions during production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153927000001_ABST
    Figure 2024153927000001_ABST
Patent Text Reader

Abstract

To provide an epoxy resin having improved mechanical characteristics.SOLUTION: An epoxy resin has a structure represented by formula (1). In the formula (1), R is derived from aliphatic diamine, aromatic diamine, siloxane diamine or polyether diamine, EP is a structure derived from a polyglycidyl ether derivative of bisphenol A, a polyglycidyl ether derivative of polyether or a polyglycidyl ether derivative of a phenol resin, m is an integer of 1 to 5, and X is an integer of 1 to 25.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an epoxy resin, a composition for its preparation and a method for its preparation. In particular, the epoxy resin is a glycidyl ether of diphenolic bis-carbamate containing a dicarbamate group. The composition for its preparation is a one-part epoxy resin composition. The epoxy resin is prepared by curing the one-part epoxy resin composition. [Background technology]

[0002] Epoxy resins are widely used in various fields such as metal coating, electronic components, paint industry and adhesive industry. In general, uncured epoxy resins have poor mechanical properties, chemical inertness and heat resistance. The curing reaction between the conventional amine-based curing agent and the epoxy resin occurs even at room temperature. In order to avoid the epoxy resin and the amine-based curing agent from immediately occurring at room temperature, it is necessary to add the epoxy resin and the amine-based curing agent separately. This is a conventional two-liquid type epoxy resin composition. From the viewpoint of optimizing the processability of the epoxy resin composition and avoiding complicated packaging and use processes, one-liquid type epoxy resin compositions are an area in which research and development is urgently needed.

[0003] Therefore, in the current epoxy resin-related field, the development of epoxy resins capable of improving mechanical properties and one-liquid epoxy resin compositions having excellent thermal stability, as well as application examples thereof, are important issues that need to be solved, researched, and developed. Summary of the Invention

[0004] In view of the above circumstances and in accordance with the needs of the industry, the first object of the present invention is to provide an epoxy resin having a structure represented by formula (1). Specifically, the epoxy resin is a glycidyl ether of diphenolic bis-carbamate containing dicarbamate groups, and has good thermal stability and mechanical properties. Preferably, the epoxy resin has a strain% of more than 250%.

[0005] [ka]

[0006] R is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, Ep has a structure represented by formula (2), and (A) n is one or a combination selected from the following structural formula (3), structural formula (4), structural formula (5), structural formula (6), structural formula (7), and structural formula (8). [ka] JPEG2024153927000004.jpg12452

[0007] R1 includes a cyclic hydrocarbon group having 1 to 5 carbon atoms, a polyphenol group having 6 to 10 carbon atoms, a linear hydrocarbon group having 1 to 20 carbon atoms, a halohydrocarbon group having 1 to 20 carbon atoms, an imino group, an amide group, a phosphonate group, a phosphine group, a silane group, an ether group, a thioether group, a sulfonyl group, a selenide group, a ketone group, an aldehyde group, a carboxylic acid group, or an ester group.

[0008] R2 includes a hydrogen atom, a halogen, an alkyl group, an alkenyl group, an alkynyl group, a hydrocarbon group, a hydroxyl group, an amine group, a nitro group, or an alkoxy group having 1 to 5 carbon atoms.

[0009] Z and n each independently represent an integer of 1 to 5; m represents an integer of 0 to 5; and X represents an integer of 1 to 25.

[0010] A second object of the present invention is to provide a one-component epoxy resin composition. This one-component epoxy resin composition is a reaction recipe for producing the epoxy resin described in the first object, and contains a curing agent having a structure represented by formula (9) and an epoxy compound. The weight ratio of the curing agent having a structure represented by formula (9) to the epoxy compound is 0.5 to 20. R1 is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine or a polyether diamine, and m is an integer selected from 0 to 5.

[0011] [ka]

[0012] Specifically, the one-part epoxy resin composition further comprises an additive, which comprises a modifier, an accelerator, an activator, a catalyst, or a combination thereof, and the function of the additive is to catalyze the curing reaction or to ensure that the resulting epoxy resin has a crosslinked network structure after curing.

[0013] The contents of the one-component epoxy resin composition of the present invention, for example, the curing agent and the epoxy compound, have good compatibility, so that reduction such as phase separation or precipitation of the contents does not occur, and the composition has excellent storage stability.

[0014] A third object of the present invention is to provide a method for preparing an epoxy resin containing carbamate groups, comprising the steps of:

[0015] Step 1: Provide a curing agent having a structure represented by formula (9) and an epoxy compound. The weight ratio of the curing agent to the epoxy compound is 0.5-20. R1 is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, and m is an integer selected from 1-5.

[0016] [ka]

[0017] Step 2: The hardener and the epoxy compound are reacted in a solvent to form an epoxy resin prepolymer.

[0018] Step 3: A curing reaction is performed to form the epoxy resin containing the carbamate groups from the epoxy resin prepolymer.

[0019] In the method for producing the carbamate group-containing epoxy resin, the curing agent can be made from waste polymers (e.g., waste polycarbonate), which can solve the problem of environmental pollution caused by waste polymers and achieve the goal of a circular economy. In addition, since no carbon dioxide is emitted during the production process, the carbon cycle of carbon dioxide can be effectively extended.

[0020] Specifically, the reaction temperature of the curing reaction is 150 to 350°C.

[0021] From the above, the technology of the present invention has at least the following technical features and advantages compared to the conventional technology. (1) To provide an epoxy resin having good thermal stability and mechanical properties. (2) To provide a one-liquid type epoxy resin composition (formulation) having good compatibility with contents and storage stability. (3) To provide an environmentally friendly method for producing an epoxy resin containing a carbamate group. [Brief description of the drawings]

[0022] [Figure 1] 1H-NMR spectrum of an epoxy resin produced using one-component epoxy resin composition E1DP1. [Diagram 2] 1 is a Fourier transform infrared spectrum of an epoxy resin produced using one-component epoxy resin composition E1DP1. [Diagram 3] 1 is a Fourier transform infrared spectrum of an epoxy resin produced using one-component epoxy resin composition E1DP2. [Figure 4] 1 is a Fourier transform infrared spectrum of an epoxy resin produced using one-component epoxy resin composition E1DP3. [Diagram 5] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E1BPA. [Figure 6] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E1DP1. [Figure 7] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E1DP2. [Figure 8] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E1DP3. [Figure 9] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E2DP1. [Figure 10] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E2DP2. [Figure 11] 1 is a differential scanning calorimeter curve of a one-component epoxy resin composition E2DP3. [Figure 12] 1 is a differential scanning calorimeter curve of an epoxy resin produced using one-component epoxy resin composition E2DP3. [Figure 13] 1 is a differential scanning calorimeter curve of an epoxy resin produced using one-component epoxy resin composition E1DP2. [Figure 14] 1 is a differential scanning calorimeter curve of an epoxy resin produced using one-component epoxy resin composition E2DP2. [Figure 15] 1 is a curve of tensile strength and elongation of epoxy resins produced using one-component epoxy resin compositions E2S430, E1DP3, and E2DP3, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] A first embodiment of the present invention provides an epoxy resin comprising a structure represented by formula (1). Specifically, the epoxy resin is a glycidyl ether of diphenolic bis-carbamate containing a dicarbamate group, and has good thermal stability and mechanical properties.

[0024] [ka]

[0025] In one embodiment, R is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, m is an integer from 0 to 5, and X is an integer from 1 to 25.

[0026] In one embodiment, Ep has a structure represented by formula (2): n is one or a combination selected from the following structural formula (3), structural formula (4), structural formula (5), structural formula (6), structural formula (7), and structural formula (8).

[0027] [ka] JPEG2024153927000009.jpg3551

[0028] In one embodiment, R1 comprises a cyclic hydrocarbon group having 1 to 5 carbon atoms, a polyphenol group having 6 to 10 carbon atoms, a linear hydrocarbon group having 1 to 20 carbon atoms, a halohydrocarbon group having 1 to 20 carbon atoms, an imino group, an amide group, a phosphonate group, a phosphine group, a silane group, an ether group, a thioether group, a sulfonyl group, a selenide group, a ketone group, an aldehyde group, a carboxylic acid group, or an ester group.

[0029] In one embodiment, R2 comprises a hydrogen atom, a halogen, an alkyl group, an alkenyl group, an alkynyl group, a hydrocarbon group, a hydroxyl group, an amine group, a nitro group, or an alkoxy group having 1 to 5 carbon atoms.

[0030] In one embodiment, Z and n are each independently an integer from 1 to 5; m is an integer from 0 to 5; and X is an integer from 1 to 25.

[0031] In one embodiment, the aliphatic diamine includes a linear aliphatic diamine having 2 to 40 carbon atoms or a branched aliphatic diamine having 2 to 40 carbon atoms. Preferably, the linear aliphatic diamine having 2 to 40 carbon atoms is 1,4-butanediamine, 1,5-pentanediamine or 1,6-hexanediamine.

[0032] In one embodiment, the aromatic diamine comprises o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether, or a combination thereof.

[0033] In one embodiment, the molecular weight of the siloxane diamine is 150 to 10,000 Da.

[0034] The structure of the siloxane group contained in the siloxane diamine is represented by the formula (10).

[0035] [ka]

[0036] In one embodiment, the weight average molecular weight of the polyether diamine is 100 to 5,000 Da. Preferably, the polyether diamine is JEFFAMINE polyether diamine.

[0037] The second embodiment of the present invention provides a one-liquid type epoxy resin composition. This one-liquid type epoxy resin composition is a reaction recipe for producing the epoxy resin described in the first embodiment, and contains a curing agent having a structure represented by formula (9) and an epoxy compound. The weight ratio of the curing agent having a structure represented by formula (9) to the epoxy compound is 0.5-20.

[0038] [ka]

[0039] In one embodiment, R1 is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, and m is an integer from 0 to 5.

[0040] The one-part epoxy resin composition further comprises an additive, which may include a modifier, an accelerator, an activator, a catalyst, or a combination thereof, and the function of the additive is to catalyze the curing reaction or to ensure that the resulting epoxy resin has a crosslinked network structure after curing.

[0041] The additive includes a phosphorus-based catalyst or a nitrogen-based catalyst.

[0042] In one embodiment, the phosphorus-based catalyst includes a quaternary phosphonium halide catalyst (methyl or ethyl triphenylphosphonium iodide or bromide), an organophosphorus catalyst (triphenylphosphine or tributylphosphine), a quaternary phosphonium carboxylic acid salt (ethyl triphenylphosphonium acetate), a phosphate ester (formylmethylene triphenylphosphorane) or a quaternary phosphonium halide precursor (formylmethyltriphenylphosphonium chloride).

[0043] In one embodiment, the nitrogen-based catalyst comprises a tertiary amine, preferably trimethylamine, triethylamine, triethanolamine, triisopropanolamine, benzyldimethylamine, dimethylamino-methylphenol or a derivative thereof.

[0044] In one embodiment, the additive includes a quaternary phosphonium halide catalyst, an organophosphorus catalyst, a quaternary phosphonium carboxylate, a phosphate ester, a tertiary amine, a stannous carboxylate, an organolithium salt, an imidazole, or a benzimidazole.

[0045] In one embodiment, the aliphatic diamine includes a linear aliphatic diamine having 2 to 40 carbon atoms or a branched aliphatic diamine having 2 to 40 carbon atoms. Preferably, the linear aliphatic diamine having 2 to 40 carbon atoms is 1,4-butanediamine, 1,5-pentanediamine or 1,6-hexanediamine.

[0046] In one embodiment, the aromatic diamine comprises o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether, or a combination thereof.

[0047] In one embodiment, the molecular weight of the siloxane diamine is 150 to 10,000 Da.

[0048] The structure of the siloxane group contained in the siloxane diamine is represented by the formula (10).

[0049] [ka]

[0050] In one embodiment, the weight average molecular weight of the polyether diamine is 100 to 5,000 Da. Preferably, the polyether diamine is JEFFAMINE polyether diamine.

[0051] In one embodiment, the epoxy compound has a structure represented by formula (2): (A) n is one or a combination selected from the following structural formula (3), structural formula (4), structural formula (5), structural formula (6), structural formula (7), and structural formula (8).

[0052] [ka] JPEG2024153927000014.jpg4551

[0053] In one embodiment, R1 comprises a cyclic hydrocarbon group having 1 to 5 carbon atoms, a polyphenol group having 6 to 10 carbon atoms, a linear hydrocarbon group having 1 to 20 carbon atoms, a halohydrocarbon group having 1 to 20 carbon atoms, an imino group, an amide group, a phosphonate group, a phosphine group, a silane group, an ether group, a thioether group, a sulfonyl group, a selenide group, a ketone group, an aldehyde group, a carboxylic acid group, or an ester group.

[0054] In one embodiment, R2 comprises a hydrogen atom, a halogen, an alkyl group, an alkenyl group, an alkynyl group, a hydrocarbon group, a hydroxyl group, an amine group, a nitro group, or an alkoxy group having 1 to 5 carbon atoms.

[0055] In one embodiment, Z and n are each independently an integer from 1-5.

[0056] Preferably, the epoxy compound includes a polyglycidyl ether derivative of bisphenol A, a polyglycidyl ether derivative of polyether, or a polyglycidyl ether derivative of a phenol resin. Specifically, the polyglycidyl ether derivative of bisphenol A is bisphenol A diglycidyl ether (trade name DER332), and the polyglycidyl ether derivative of polyether is diglycidyl ether of poly(propylene glycol) (trade name DER736).

[0057] In one embodiment, the curing reaction temperature of the one-component epoxy resin composition is higher than 150°C, 160°C, 170°C, 180°C, 190°C or 200°C.

[0058] A third embodiment of the present invention provides a method for preparing an epoxy resin containing carbamate groups, the method comprising the steps of:

[0059] Step 1: Provide a curing agent having a structure represented by formula (9) and an epoxy compound. The weight ratio of the curing agent to the epoxy compound is 0.5-20. R1 is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, and m is an integer selected from 1-5.

[0060] [ka]

[0061] Step 2: The hardener and the epoxy compound are reacted in a solvent to form an epoxy resin prepolymer.

[0062] Step 3: A curing reaction is performed to form an epoxy resin containing the carbamate groups from the epoxy resin prepolymer.

[0063] In the method for producing the carbamate group-containing epoxy resin, the curing agent can be made from waste polymers (e.g., waste polycarbonate), which can solve the problem of environmental pollution caused by waste polymers and achieve the goal of a circular economy. In addition, since no carbon dioxide is emitted during the production process, the carbon cycle of carbon dioxide can be effectively extended.

[0064] Preferably, the process may use a modifier, an activator, a catalyst or a combination thereof as an additive, the function of which is to catalyze the curing reaction or to ensure that the resulting epoxy resin has a crosslinked network structure after curing.

[0065] In one embodiment, the aliphatic diamine includes a linear aliphatic diamine having 2 to 40 carbon atoms or a branched aliphatic diamine having 2 to 40 carbon atoms. Preferably, the linear aliphatic diamine having 2 to 40 carbon atoms is 1,4-butanediamine, 1,5-pentanediamine or 1,6-hexanediamine.

[0066] In one embodiment, the aromatic diamine comprises o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether, or a combination thereof.

[0067] In one embodiment, the molecular weight of the siloxane diamine is from 150 to 10,000 Da.

[0068] The structure of the siloxane group of the siloxane diamine is represented by formula (10).

[0069] [ka]

[0070] In one embodiment, the weight average molecular weight of the polyether diamine is 100 to 5,000 Da. Preferably, the polyether diamine is a JEFFAMINE polyether diamine.

[0071] In one embodiment, the epoxy compound has a structure represented by formula (2): (A) n is one or a combination selected from the following structural formula (3), structural formula (4), structural formula (5), structural formula (6), structural formula (7), and structural formula (8).

[0072] [ka]

[0073] In one embodiment, R1 comprises a cyclic hydrocarbon group having 1 to 5 carbon atoms, a polyphenol group having 6 to 10 carbon atoms, a linear hydrocarbon group having 1 to 20 carbon atoms, a halohydrocarbon group having 1 to 20 carbon atoms, an imino group, an amide group, a phosphonate group, a phosphine group, a silane group, an ether group, a thioether group, a sulfonyl group, a selenide group, a ketone group, an aldehyde group, a carboxylic acid group, or an ester group.

[0074] In one embodiment, R2 comprises a hydrogen atom, a halogen, an alkyl group, an alkenyl group, an alkynyl group, a hydrocarbon group, a hydroxyl group, an amine group, a nitro group, or an alkoxy group having 1 to 5 carbon atoms.

[0075] In one embodiment, Z and n are each independently an integer from 1-5.

[0076] Preferably, the epoxy compound includes a polyglycidyl ether derivative of bisphenol A, a polyglycidyl ether derivative of polyether, or a polyglycidyl ether derivative of a phenol resin. Specifically, the polyglycidyl ether derivative of bisphenol A is bisphenol A diglycidyl ether (trade name DER332), and the polyglycidyl ether derivative of polyether is diglycidyl ether of poly(propylene glycol) (trade name DER736).

[0077] Specifically, the reaction temperature of the curing reaction is 150 to 350°C.

[0078] Experimental examples of the present invention are given below.

[0079] Experimental Example 1: General method for producing the curing agent of the present invention A mixture is provided that includes a solvent, a polycarbonate, and a diamine compound. The diamine compound may be a diamine compound having a siloxane group or a polysiloxane group. The mixture may further include diphenyl carbonate. The solvent includes isopropyl ether, anisole, ethyl phenyl ether, propyl phenyl ether, butyl phenyl ether, o-methyl anisole, m-methyl anisole, p-methyl anisole, benzyl ethyl ether, diphenyl ether, dibenzyl ether, tetrahydrofuran, dihydropyran, tetrahydropyran, 2-methyltetrahydropyran, benzene, toluene, xylene, ethyl benzene, diethyl benzene, or cyclohexyl benzene. Then, the mixture is mixed and reacted at 50 to 200°C to obtain a crude product, and the curing agent is obtained after removing the solvent by vacuum distillation. Usually, the weight yield of this manufacturing method is higher than 95%. That is, 1.9 to 2 g of a curing agent is obtained by reacting 1 g of polycarbonate with 1 g of diamine compound. A specific curing agent reaction composition is shown in Table 1.

[0080] [Table 1]

[0081] The structures of the curing agents DP1, DP2 and DP3 shown in Table 1 above were analyzed by 1H-NMR spectrum, and as a result, all of them have a characteristic peak at a chemical shift of about 7.61 ppm, indicating that the structure has a urethane group.

[0082] Experimental Example 2: General method for producing the epoxy resin of the present invention First, a curing agent is added to an epoxy compound or epoxy resin, a catalyst, and a solvent to form a mixture, and the mixture is heated to 50-80°C to form an epoxy resin prepolymer. After standing overnight, the epoxy resin prepolymer is placed in an oven to carry out a curing reaction, and after the curing reaction is completed, the epoxy resin is obtained. Specifically, the curing reaction includes at least four heating steps. The first step is maintained at 60°C for 3 hours, the second step is maintained at 80°C for 3 hours, the third step is maintained at 150°C for 3 hours, and the fourth step is maintained at 180°C for 3 hours.

[0083] The curing agent used in this Experimental Example 2 was prepared in Experimental Example 1. The composition of the Experimental Example is shown in Table 2. DER332 is bisphenol A diglycidyl ether. DER736 is diglycidyl ether of poly(propylene glycol).

[0084] [Table 2]

[0085] The epoxy resin of the present invention was structurally analyzed by 1H-NMR spectrum and Fourier transform infrared spectrum. In representative examples, the Fourier transform infrared spectra of the epoxy resins produced from the one-liquid epoxy resin compositions E1DP1, E1DP2 and E1DP3 in Table 2 are shown in Figures 2, 3 and 4, respectively. The positions of the characteristic peaks and the functional groups are shown in Table 3.

[0086] [Table 3]

[0087] Differential Scanning Calorimetry (DSC) of the One-Component Epoxy Resin Composition of the Present Invention

[0088] The differential scanning calorimetric curves of the one-component epoxy resin compositions E1BPA, E1DP1, E1DP2, E1DP3, E2DP1, E2DP2 and E2DP3 are shown in Figures 5, 6, 7, 8, 9, 10 and 11, respectively. The reaction temperatures of representative one-component epoxy resin compositions are shown in Table 4. As is clear from the results of differential scanning calorimetric analysis, the reaction temperatures of E1DP1 and E2DP1 are 160 to 280°C, those of E1DP2, E2DP2 and E2DP3 are 170 to 290°C, and that of E1DP3 is 240 to 310°C. Thus, the reaction temperature of the one-component epoxy resin composition of the present invention is higher than 150°C, 160°C, 170°C, 180°C, 190°C or 200°C.

[0089] [Table 4]

[0090] Characterization of the epoxy resin of the present invention The characteristic analysis of the epoxy resin produced by the one-liquid epoxy resin composition of the present invention is shown in Table 5. The glass transition temperature (Tg) is measured by DSC analysis. The Tg of the produced epoxy resin is -10 to 120°C. As shown in FIG. 12, the epoxy resin produced by E2DP3 is a low glass transition temperature type epoxy resin. As shown in FIG. 13, the epoxy resin produced by E1DP2 is a low glass transition temperature type epoxy resin. As shown in FIG. 14, the epoxy resin produced by E2DP2 is a high glass transition temperature type epoxy resin. Therefore, the one-liquid epoxy resin composition of the present invention can produce various glass transition temperature types of epoxy resins at different reaction temperatures by designing the composition components, and can be applied to different fields.

[0091] [Table 5]

[0092] Tensile Test of the Epoxy Resin of the Present Invention The epoxy resins produced with E1DP3, E2DP3 and E2S430 are subjected to tensile strength and elongation tests using a universal tensile tester (manufacturer and model: MTS Landmark 370.02 Test System). The test conditions are as follows: the sample size is prepared according to ASTM D638, and the tensile speed of the test sample is 100 mm / min. The results are shown in FIG. 15. As is clear, the epoxy resins produced with the one-component epoxy resin compositions E1DP3 and E2DP3 of the present invention have elongations of more than 150% and show good toughness. In contrast, the epoxy resin produced with the epoxy resin composition E2S430, which does not use the curing agent of the present invention, breaks during the tensile test. Therefore, it is possible to produce epoxy resins with toughness, high elongation and high tensile strength by using the curing agent containing a silane group of the present invention.

[0093] The present invention has been described above with specific experimental examples, but these examples are not intended to limit the scope of the present invention. Various modifications or changes may be made by those skilled in the art without departing from the spirit of the present invention. Furthermore, the abstract and title of the invention are intended to aid in searching patent documents, and are not intended to limit the scope of the present invention.

Claims

1. An epoxy resin having a structure represented by formula (1). 【Chemistry 1】 (In formula (1), R is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine; Ep is a structure derived from a polyglycidyl ether derivative of bisphenol A, a polyglycidyl ether derivative of a polyether, or a polyglycidyl ether derivative of a phenol resin; m is an integer of 1 to 5; and X is an integer of 1 to 25.)

2. The epoxy resin according to claim 1, wherein the aliphatic diamine comprises a linear aliphatic diamine having 2 to 40 carbon atoms or a branched aliphatic diamine having 3 to 40 carbon atoms.

3. The epoxy resin according to claim 1, characterized in that the aromatic diamine comprises o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether or a combination thereof.

4. The epoxy resin according to claim 1, wherein the molecular weight of the siloxane diamine is 150 to 10,000 Da.

5. The epoxy resin according to claim 1, wherein the weight average molecular weight of the polyether diamine is 100 to 5,000 Da.

6. Epoxy resin composition of claim 1, characterized in that it comprises a curing agent represented by formula (9) and an epoxy compound, and the weight ratio of the curing agent represented by formula (9) to the epoxy compound is 0.5-20. 【Chemistry 4】 (In the formula, R1 is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, and m is an integer selected from 1 to 5.)

7. 7. The one-component epoxy resin composition according to claim 6, further comprising an additive, the additive comprising a quaternary phosphonium halide catalyst, an organic phosphorus catalyst, a quaternary phosphonium carboxylate, a phosphoric acid ester, a tertiary amine, a tin carboxylate, an organic lithium salt, imidazole or benzimidazole.

8. 7. The epoxy resin composition according to claim 6, wherein the aliphatic diamine comprises a linear aliphatic diamine having 2 to 40 carbon atoms or a branched aliphatic diamine having 3 to 40 carbon atoms.

9. 7. The epoxy resin composition according to claim 6, wherein the aromatic diamine comprises o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether, or a combination thereof.

10. The epoxy resin composition according to claim 6, wherein the molecular weight of the siloxane diamine is 150 to 10,000 Da.

11. The epoxy resin composition according to claim 6, wherein the polyether diamine has a weight average molecular weight of 100 to 5,000 Da.

12. 7. The epoxy resin composition according to claim 6, wherein the epoxy compound comprises a polyglycidyl ether derivative of bisphenol A, a polyglycidyl ether derivative of a polyether, or a polyglycidyl ether derivative of a phenol resin.

13. An epoxy resin containing a carbamate group, The carbamate group-containing epoxy resin is produced by a curing reaction between a curing agent having a structure represented by formula (9) and an epoxy compound, 【Chemistry 7】 The weight ratio of the curing agent to the epoxy compound is 0.5 to 20, wherein R1 is derived from an aliphatic diamine, an aromatic diamine, a siloxane diamine, or a polyether diamine, and m is an integer selected from 1 to 5.

14. The epoxy resin containing a carbamate group according to claim 13, wherein the aliphatic diamine comprises a linear aliphatic diamine having 2 to 40 carbon atoms or a branched aliphatic diamine having 3 to 40 carbon atoms.

15. 14. The epoxy resin containing carbamate groups according to claim 13, wherein the aromatic diamine comprises o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenyl ether, or a combination thereof.

16. The carbamate group-containing epoxy resin according to claim 13, wherein the molecular weight of the siloxane diamine is 150 to 10,000 Da.

17. The carbamate group-containing epoxy resin according to claim 13, wherein the polyether diamine has a weight average molecular weight of 100 to 5,000 Da.

18. 14. The carbamate group-containing epoxy resin according to claim 13, wherein the epoxy compound comprises a polyglycidyl ether derivative of bisphenol A, a polyglycidyl ether derivative of a polyether, or a polyglycidyl ether derivative of a phenolic resin.

Citation Information

Patent Citations

  • Self-curing epoxy resins

    GB1326669A

  • Polyurethane or polyurea containing phenol as terminal group and epoxide resin containing the same

    JP1989188512A

  • New polymer, its production, and epoxy resin composition

    JP1996301967A

  • Toughening agents and reinforced epoxy adhesives

    JP2014529654A