Light shielding film, multilayer reflection prevention film, method for manufacturing the same, and optical member

By using non-oxide compounds like MgF2 and optical interference layers, the film's stability and optical performance are enhanced, addressing instability issues and maintaining accurate light-shielding and antireflection properties.

JP2024153959AInactive Publication Date: 2024-10-30KONICA MINOLTA INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021149619
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-09-14
Publication Date
2024-10-30
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing light-shielding films and multilayer antireflection films face challenges in maintaining chemical stability, optical properties, and ensuring accuracy in light-shielding and antireflection performance due to instability caused by oxygen interaction with chromium and silicon dioxide layers.

Method used

Incorporating layers made of compounds other than oxides, such as MgF2, AlF2, NdF3, LaF3, YF3, GdF3, YbF2, PbF2, Na3ALF6, Na5Al3F14, and CeF3, in contact with the chromium and silicon dioxide layers to prevent oxygen movement and stabilize the light-shielding film, along with the use of optical interference layers and spectral property adjustment layers to enhance performance.

Benefits of technology

The solution results in a light-shielding film and multilayer antireflection film with improved chemical stability, reduced deviation between designed and measured values, and enhanced light-shielding and antireflection properties, ensuring consistent optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153959000001_ABST
    Figure 2024153959000001_ABST
Patent Text Reader

Abstract

To provide a light shielding film and a multilayer reflection prevention film which are excellent in the light shielding property, the light reflection prevention property, and a chemical stability, a method for manufacturing the light shielding film and the multilayer reflection prevention film in which the gap between a design value and an actually measured value is small, and an optical member.SOLUTION: The light shielding film has a light shielding layer and layers in contact with the light shielding layer. The light shielding layer includes chromium and silicon dioxide. At least one of the layers in contact with the light shielding layer includes a compound other than oxide.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a light-shielding film, a multilayer antireflection film, their manufacturing methods, and an optical member. More specifically, the present invention relates to a light-shielding film and a multilayer antireflection film having excellent light-shielding and antireflection properties, their manufacturing methods, and an optical member. [Background technology]

[0002] 2. Description of the Related Art In recent years, in optical components such as mobile phone cameras and glass prisms, there has been a demand for anti-reflection and light-shielding measures to be taken on the inner wall surfaces of optical components in order to solve problems such as the occurrence of so-called ghosts and flares. For example, Patent Document 1 discloses an invention in which the inner wall surface of an optical member is coated with a black coating film made of a film-forming resin containing a plurality of fine particles of a plurality of different shapes.

[0003] This method aims to prevent ghosts and flare by reducing the spectral reflectance of optical components by applying an organic ink coating to them. However, it is difficult to ensure dimensional accuracy in the ink coating area, and because ink is an organic material, it is also difficult to ensure durability. In addition, there remains the problem that it is difficult to stabilize the optical properties while keeping the spectral reflectance low.

[0004] In contrast, in Patent Document 2, an inorganic material is used for the light-shielding film provided on the optical component, and the light-shielding film is made by combining multiple light-absorbing layers and a low refractive index layer having a refractive index of 1.7 or less, thereby not only blocking light incident on the light-shielding film but also reducing reflected light from its surfaces (the surface on the substrate side and the surface opposite the substrate). However, the present inventors have found through their investigations that the light-shielding film disclosed in Patent Document 2 also has room for improvement in terms of stability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-064737 A [Patent Document 2] JP 2013-148844 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a light-shielding film and a multilayer antireflection film that are excellent in light-shielding property, light antireflection property, and chemical stability, and a manufacturing method and an optical component thereof in which the deviation between the designed values ​​and the actually measured values ​​is small. [Means for solving the problem]

[0007] In order to solve the above-mentioned problems, the inventors investigated the causes of the above-mentioned problems and discovered that a light-shielding film containing chromium and silicon dioxide becomes unstable due to the influence of oxygen. They also discovered that the layer in contact with the light-shielding layer affects the stability and found a way to improve this stability, which led to the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.

[0008] 1. A light-shielding film having at least a light-shielding layer and a layer in contact with the light-shielding layer, wherein the light-shielding layer contains chromium and silicon dioxide, and at least one of the layers in contact with the light-shielding layer contains a compound other than an oxide.

[0009] 2. At least one of the layers in contact with the light-shielding layer is MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 and CeF 32. The light-shielding film according to claim 1, comprising any one of fluorides selected from the following:

[0010] 3. The light-shielding film according to item 1 or 2, wherein at least one of the layers in contact with the light-shielding layer contains a sulfide.

[0011] 4. The light-shielding film according to claim 3, wherein the sulfide is ZnS.

[0012] 5. The light-shielding film according to any one of items 1 to 4, wherein the average spectral transmittance in a wavelength range of 400 to 700 nm is 2% or less.

[0013] 6. A multilayer antireflection film having a light-shielding film, the multilayer antireflection film comprising the light-shielding film according to any one of items 1 to 5, and having at least an optical interference layer on at least one layer in contact with the light-shielding layer.

[0014] 7. The multilayer antireflection film according to item 6, further comprising a layer for adjusting spectral characteristics between the layer in contact with the light-shielding layer and the light interference layer.

[0015] 8. The multilayer antireflection film according to item 6 or 7, characterized in that the average spectral reflectance in the wavelength region of 400 to 700 nm is 2% or less.

[0016] 9. A method for producing a light-shielding film according to any one of items 1 to 5, comprising forming the light-shielding layer by depositing a mixture of chromium and silicon dioxide under an argon gas atmosphere.

[0017] 10. A method for producing a light-shielding film according to any one of items 1 to 5, comprising forming the light-shielding layer by depositing a mixture of chromium and silicon dioxide under a nitrogen gas atmosphere.

[0018] 11. A method for producing a multilayer antireflection film according to any one of items 6 to 8, comprising the steps of forming the light-shielding film and laminating at least an optical interference layer on the light-shielding film.

[0019] 12. An optical component comprising at least a light-shielding film on a substrate, the optical component comprising the light-shielding film according to any one of items 1 to 5 as the light-shielding film.

[0020] 13. The optical member according to item 12, further comprising a light interference layer formed on the light-shielding film.

[0021] 14. The optical member according to item 12 or 13, further comprising a light interference layer formed between the substrate and the light-shielding film. Effect of the Invention

[0022] The above-mentioned means of the present invention can provide a light-shielding film and a multilayer antireflection film excellent in light-shielding property, light antireflection property and chemical stability, as well as a manufacturing method and an optical member thereof with little deviation between the design values ​​and the actually measured values. Although the mechanism by which the effects of the present invention are expressed or the mechanism of action has not been clarified, it is speculated as follows.

[0023] The light-shielding layer of the light-shielding film of the present invention contains chromium and silicon dioxide. The inclusion of chromium and silicon dioxide in the light-shielding layer is useful for improving the light-shielding properties and anti-reflection properties of the light-shielding film. However, the inventors' investigations revealed that when the light-shielding layer comes into contact with an oxide, oxygen is transferred between the light-shielding layer and the oxide, causing a change in the chemical properties of the mixture of chromium and silicon dioxide in the light-shielding layer, and causing changes in the optical properties, such as the refractive index and light absorption coefficient, of the light-shielding film having the light-shielding layer, resulting in a decrease in the light-shielding properties and anti-reflection properties. It has also become clear that the light blocking property and anti-reflection property are reduced, resulting in a discrepancy between the initial design values ​​of these optical properties and the values ​​actually measured after manufacture. In the present invention, by making the layer in contact with the light-shielding layer containing chromium and silicon dioxide a layer containing a compound other than an oxide, the movement of oxygen from outside the light-shielding layer is prevented, the components of the light-shielding layer do not change chemically and are optically stabilized, and a light-shielding film with excellent light-shielding properties and light reflectivity is formed. Therefore, a light-shielding film or the like with little deviation between the design value and the actual measured value can be manufactured. [Brief description of the drawings]

[0024] [Figure 1] A conceptual diagram showing the simplest configuration of the light-shielding film of the present invention. [Diagram 2] A conceptual diagram showing an example of the structure of a multilayer antireflection coating having a surface antireflection effect. [Diagram 3] A conceptual diagram showing an example of the structure of a multi-layer anti-reflection coating having a back surface anti-reflection effect. [Figure 4] (a) A conceptual diagram of an example showing the configuration of a multilayer antireflection coating that has antireflection effects on both the front and back surfaces. (b) A conceptual diagram of an example showing the configuration of a multilayer antireflection coating that has a front-surface antireflection effect and a multilayer antireflection coating that has a back-surface antireflection effect and has adjusted spectral characteristics. [Diagram 5] Conceptual diagram of the spectral reflectance of each optical component [Figure 6] Conceptual diagram of the spectral transmittance of each optical component [Figure 7] 1 is a flowchart showing an example of a manufacturing process of a light-shielding film. [Figure 8] A flowchart showing an example of a manufacturing process for a multilayer antireflection coating having a surface antireflection effect. [Figure 9] A flow chart showing an example of a manufacturing process for a multi-layer anti-reflection coating having a back surface anti-reflection effect. [Figure 10] A flow chart showing an example of a manufacturing process for a multi-layer anti-reflection coating having anti-reflection effects on both the front and back surfaces. [Figure 11] Schematic diagram showing an example of a vacuum deposition apparatus [Figure 12](a) Spectral reflectance of sample optical member A1 (b) Spectral reflectance of sample optical member A2 (c) Spectral reflectance of sample optical member A3 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The light-shielding film of the present invention is a light-shielding film having at least a light-shielding layer and a layer in contact with the light-shielding layer, characterized in that the light-shielding layer contains chromium and silicon dioxide, and at least one of the layers in contact with the light-shielding layer contains a compound other than an oxide. This feature is a technical feature common to or corresponding to each of the following embodiments (aspects).

[0026] In one embodiment of the present invention, at least one of the layers in contact with the light-shielding layer is made of MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 and CeF 3 From the viewpoint of stabilizing the chemical properties of the light-shielding film, it is preferable that the light-shielding film contains any one of the fluorides selected from the following.

[0027] From the viewpoint of stabilizing the chemical properties of the light-shielding film, it is preferable that at least one of the layers in contact with the light-shielding layer contains a sulfide.

[0028] It is more preferable that the sulfide is ZnS from the viewpoint of stabilizing the chemical properties of the light-shielding film.

[0029] From the viewpoint of light-shielding properties, it is preferable that the average spectral transmittance in the wavelength region of 400 to 700 nm is 2% or less.

[0030] From the viewpoint of light antireflection properties, it is preferable that the multilayer antireflection film having the light-shielding film of the present invention has at least a light interference layer on at least one layer in contact with the light-shielding layer.

[0031] From the viewpoint of light shielding and light antireflection properties, it is preferable that the multilayer antireflection film has a spectral characteristic adjusting layer between the layer in contact with the light shielding layer and the light interference layer.

[0032] From the viewpoint of light antireflection properties, it is preferable that the average spectral reflectance of the multilayer antireflection film in the wavelength region of 400 to 700 nm is 2% or less.

[0033] The light-shielding film is preferably produced by forming the light-shielding layer from a mixture of chromium and silicon dioxide in an argon gas atmosphere.

[0034] The light-shielding film is preferably produced by forming the light-shielding layer from a mixture of chromium and silicon dioxide in a nitrogen gas atmosphere.

[0035] The multilayer antireflection film can be suitably produced by the process for producing the multilayer antireflection film, which comprises a step of forming a light-shielding film and a step of laminating at least a light interference layer on the light-shielding film.

[0036] An optical member having at least a light-shielding film on a substrate preferably has the light-shielding film of the present invention as the light-shielding film.

[0037] From the viewpoint of antireflection properties, it is preferable that the optical member has a light interference layer formed on the light-shielding film.

[0038] From the viewpoint of antireflection properties, it is preferable that the optical member has a light interference layer formed between the base material and the light-shielding film.

[0039] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0040] 1. Light-shielding film The light-shielding film of the present invention is a light-shielding film having at least a light-shielding layer and a layer in contact with the light-shielding layer, characterized in that the light-shielding layer contains chromium and silicon dioxide, and at least one of the layers in contact with the light-shielding layer contains a compound other than an oxide.

[0041] FIG. 1 is a conceptual diagram showing the simplest configuration of the light-shielding film of the present invention. As shown in FIG. 1, the light-shielding film of the present invention has a light-shielding layer having excellent light-shielding properties and anti-reflection properties on a substrate, and in order to stabilize the chemical properties of the light-shielding layer, a layer in contact with the light-shielding layer is a layer containing a compound other than an oxide, thereby achieving the effects of the present invention.

[0042] (1.1) Base material The substrate according to the present invention is not particularly limited, but examples thereof include resins such as cycloolefin copolymers (COC), cycloolefin polymers (COP) and polyester resins.

[0043] (1.2) Light shielding layer The light-shielding layer constituting the light-shielding film of the present invention contains chromium and silicon dioxide. The film-forming material used in forming the light-shielding layer is not particularly limited as long as it contains chromium and silicon dioxide. For example, BlackA (Cr, SiO 2 )(Merck BlackA powder less than 0.3mm Patinal (Cr(45%)+SiO 2 (50-60%) mixture, hereafter referred to as "Black A".

[0044] (1.3) Layer in contact with the light-shielding layer The inclusion of chromium and silicon dioxide in the light-shielding layer is useful for improving the light-shielding properties and anti-reflection properties of the light-shielding film. However, when the light-shielding layer comes into contact with an oxide, oxygen is transferred between the light-shielding layer and the oxide, causing a change in the chemical properties of the mixture of chromium and silicon dioxide in the light-shielding layer, and causing changes in the optical properties, such as the refractive index and light absorption coefficient, of the light-shielding film having the light-shielding layer, resulting in a decrease in the light-shielding properties and anti-reflection properties. Therefore, by making at least one of the layers in contact with the light-shielding layer, i.e., the adjacent layers, a layer containing a compound other than an oxide, it is possible to suppress changes in the optical properties of the light-shielding layer due to the migration of oxygen.

[0045] At least one of the layers in contact with the light-shielding layer must be made of a film-forming material that is a compound other than an oxide, but the other layer may be made of an oxide as a film-forming material. Examples of film-forming materials that are compounds other than oxides include MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 , CeF 3 , ZnS, etc. At least one of the layers in contact with the light-shielding layer is made of MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 , CeF 3From the viewpoint of stabilizing the chemical properties of the light-shielding film, it is preferable that the light-shielding film contains any one of the fluorides selected from the following.

[0046] It is also preferable that at least one of the layers in contact with the light-shielding layer contains a sulfide from the viewpoint of stabilizing the chemical properties of the light-shielding film.

[0047] Moreover, it is more preferable that the sulfide is ZnS from the viewpoint of stabilizing the chemical properties of the light-shielding film.

[0048] (1.4) Average spectral transmittance From the viewpoint of light-shielding properties, it is preferable that the light-shielding film has an average spectral transmittance of 2% or less within a wavelength range of 400 to 700 nm. Here, "transmittance" refers to the ratio of transmitted radiant flux or luminous flux to incident radiant flux or luminous flux under given conditions (New Color Chemistry Handbook, 2nd Edition, edited by the Color Science Association of Japan, p. 222), and its unit is "1." However, in the present invention, the "spectral transmittance" refers to the transmittance (%) for light of a specific wavelength in the above definition of "transmittance". Moreover, the "average spectral transmittance" according to the present invention refers to the average value of the spectral transmittance at each wavelength measured within the spectral wavelength range of 400 to 700 nm.

[0049] Specifically, the spectral transmittance of the light-shielding film is measured using a Hitachi U-4100 spectrophotometer, and the average value of the spectral transmittance at 31 points at intervals of 10 nm in the wavelength region of 400 to 700 nm is determined. The average spectral transmittance is calculated according to the following formula (1).

[0050] Formula (1): Average spectral transmittance (%)=(T 400 +T 410 +····+T 690 +T 700 ) / 31 Here, for example, T 400 is the spectral transmittance (%) at a light wavelength of 400 nm, T 410indicates the spectral transmittance (%) at a light wavelength of 410 nm, etc.

[0051] (1.5) Refractive Index The "refractive index" is the ratio of the speed of light in a vacuum to the speed of light in a material, that is, (speed of light in vacuum) / (speed of light in material), and is an index used to describe how light travels through a material. Since the speed of light in a material varies with the wavelength of the light, the refractive index also varies with the wavelength of the light. The refractions described in this specification are those for the helium d-line (wavelength 587.56 nm) unless otherwise specified. The refractive index according to the present invention is a value measured at room temperature (25° C.). The refractive index of a substance is an important governing factor that affects the reflection, absorption, and transmission of light when light is incident on the substance. Therefore, the refractive index of the film-forming material of each layer constituting the light-shielding film or the multi-layer anti-reflection film is closely related to the anti-reflection properties.

[0052] The refractive index of the material used in the light-shielding film or anti-reflection film according to the present invention is preferably in the range of 1.33 to 2.5. Examples of the film-forming material having a refractive index within the above range include BlackA and MgF, which are used in the light-shielding layer and adjacent layers. 2 , Y.F. 3 , SiO 2 , AlF 2 , H 4 (LaTiO 3 ), NdF 3 , LaF 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F14, CeF 3 , ZnS, Al 2 O 3 , ZrTiO 4 etc.

[0053] 2.Multilayer anti-reflection coating The multilayer antireflection film of the present invention is a multilayer antireflection film comprising a light-shielding film, characterized in that the light-shielding film comprises the above-mentioned light-shielding film of the present invention and has at least an optical interference layer on at least one layer in contact with the light-shielding layer. The multilayer antireflection coating of the present invention preferably comprises one or more layers, and is preferably formed on a substrate. Specifically, it is preferable that the light-shielding film is composed of two or more layers, has at least a light interference layer, and has at least one low refractive index layer and at least one high refractive index layer, with the uppermost layer furthest from the substrate being the low refractive index layer.

[0054] In the present invention, the term "low refractive index layer" refers to a layer formed using a film-forming material having a refractive index of less than 1.6, and the term "high refractive index layer" refers to a layer formed using a film-forming material having a refractive index of 1.9 or more.

[0055] The number of layers is not particularly limited, but is preferably 30 layers or less from the viewpoint of obtaining an optical interference layer while maintaining high productivity. That is, the number of layers depends on the required optical performance, but by stacking about 2 to 26 layers, the reflectance over the entire visible light range can be reduced, and an upper limit of 30 layers or less is preferable in that it is possible to prevent the film from peeling off due to increased stress in the film.

[0056] The multilayer antireflection coating according to the present invention has various configurations, and FIG. 2 shows a conceptual diagram of one example of the configuration of a multilayer antireflection coating having a surface antireflection effect.

[0057] In the present invention, the "surface" refers to the "surface opposite the substrate side as viewed from the light-shielding film," and the "surface anti-reflection effect" refers to the "effect of preventing reflection of light incident from the surface opposite the substrate side as viewed from the light-shielding film."

[0058] In the configuration of the multilayer antireflection coating shown in FIG. 2, the optical interference layer is formed on the light-shielding film and serves to prevent reflection of light incident from the surface. The presence of this layer further improves the performance of the multilayer antireflection coating of the present invention.

[0059] (2.1) Optical interference layer The multilayer antireflection film of the present invention includes a light-shielding film, and preferably has at least a light interference layer on at least one layer in contact with the light-shielding layer from the viewpoint of light-antireflection properties. The "optical interference layer" according to the present invention refers to a layer having the function of reducing reflected light, i.e., the composite light of the reflected light from each layer, by utilizing the interference between reflected lights from the interfaces of each stacked layer (the action in which the reflected waves from each layer cancel each other out due to interference). The optical interference layer may have a variety of configurations, but is preferably configured by alternately laminating layers having different refractive indices, such as a low refractive index layer and a high refractive index layer.

[0060] The film forming material used for the optical interference layer according to the present invention may be an oxide, such as an oxide of Ti, Ta, Nb, Zr, Ce, La, Al, Si, or Hf, or an oxide compound of a combination of these. Also, deposition materials that are compounds other than oxides can be used, such as MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 , CeF 3 , ZnS, etc. The optical interference layer according to the present invention can have the function of reducing the reflectance over the entire visible light range by stacking a plurality of layers of different film-forming materials as described above.

[0061] The thickness of the optical interference layer according to the present invention (total thickness when multiple layers are laminated) is preferably within the range of 50 to 3000 nm. If the thickness is 50 nm or more, anti-reflection optical properties can be exhibited, and if the thickness is 3000 nm or less, surface deformation due to film stress of the multilayer film itself can be prevented. Preferably, it is within the range of 60 to 2000 nm.

[0062] (2.2) Spectral characteristic adjustment layer The multilayer antireflection film may have a spectral characteristic adjusting layer between the light interference layer and a layer in contact with the light shielding layer, from the viewpoint of light shielding and antireflection properties.

[0063] FIG. 3 is a conceptual diagram showing an example of the structure of a multilayer antireflection coating having a back surface antireflection effect, among various forms of the multilayer antireflection coating according to the present invention.

[0064] In the present invention, the "rear surface" refers to the "surface on the substrate side as viewed from the light-shielding film," and the "rear surface anti-reflection effect" refers to the "effect of preventing reflection of light incident from the substrate side as viewed from the light-shielding film."

[0065] In the configuration of the multilayer antireflection coating shown in FIG. 3, the spectral characteristic adjusting layer is formed between the light interference layer and the light-shielding film, and serves as an adjusting layer for maintaining the function of the light interference layer and preventing back surface reflection of the light-shielding film.

[0066] In order to further enhance the effect of the multilayer antireflection film according to the present invention, it is preferable that layers having an antireflection effect are formed on both sides of the light-shielding film. FIG. 4(a) shows a conceptual diagram of an example of an optical member having a multilayer antireflection coating on both sides of a substrate.

[0067] In the multilayer antireflection film of the present invention, the light-shielding property and the antireflection property are further improved by adopting a layer structure as shown in FIG. 4(a). However, from the viewpoint of the light-shielding property and the antireflection property, a spectral characteristic adjusting layer may be provided between the layer in contact with the light-shielding layer and the optical interference layer as shown in FIG. 4(b).

[0068] The configuration shown in Figure 4(b) provides a multilayer antireflection coating that simultaneously prevents the reflection of light incident from the surface and maintains and enhances the function of the optical interference layer, thereby further enhancing the effects of the invention.

[0069] (2.3) Average spectral reflectance From the viewpoint of light antireflection properties, it is preferable that the average spectral reflectance of the multilayer antireflection film in the wavelength region of 400 to 700 nm is 2% or less. Here, "reflectance" refers to the ratio of reflected radiant flux or luminous flux to incident radiant flux or luminous flux under given conditions (New Color Chemistry Handbook, 2nd Edition, edited by the Color Science Association of Japan, p. 222), and its unit is "1." However, in the present invention, the "spectral reflectance" refers to the reflectance (%) for light of a specific wavelength in the above definition of "reflectance". Moreover, the "average spectral reflectance" according to the present invention refers to the average value of the spectral reflectance at each wavelength measured within the spectral wavelength range of 400 to 700 nm.

[0070] In the multilayer antireflection coating of the present invention, light may be incident from either the front or rear surface, and therefore in the examples, the spectral reflectance was calculated as necessary for both the measured front surface spectral reflectance and rear surface spectral reflectance. Specifically, the spectral reflectance is measured using a microspectrophotometer USPM-RU III manufactured by Olympus Corporation, and the average value of the spectral reflectance at 31 points at intervals of 10 nm in the wavelength region of 400 to 700 nm is calculated. The average spectral reflectance is calculated according to the following formula (1).

[0071] Equation (1) Average spectral reflectance (%) = (R 400 +R 410 +···+R 690 +R 700 ) / 31

[0072] Here, for example, R 400 is the spectral reflectance value (%) at a light wavelength of 400 nm, R410 indicates the spectral reflectance (%) at a light wavelength of 410 nm, etc.

[0073] 3. Discrepancy between design values ​​and actual measurements In the present invention, as described above, the migration of oxygen from the outside to the light-shielding layer is prevented, thereby optically stabilizing the components of the light-shielding layer, thereby making it possible to reduce the deviation between the design values ​​of the ideal optical properties of the light-shielding film and the multilayer antireflection film and the actual measured values ​​when actually used after production.

[0074] (3.1) Deviation of Spectral Reflectance Values If the deviation between the preset design value and the actual measured value of the spectral reflectance is small, it is understood that the influence of oxygen is reduced and the film is chemically stable, and as a result, it is understood that the film has excellent anti-reflection properties.

[0075] Whether the deviation between the design value and the actual measured value was large was judged by whether the area in which the design value and the actual measured value differed by 1% or more in spectral reflectance when the design value and the actual measured value were graphed within the light wavelength range of 400 to 700 nm accounted for 50% or more of the line on the graph.

[0076] The design value of the spectral reflectance is calculated using the thin film calculation software TF-CALC (Software Spectra, Inc.), inputting the reflectance target (set to 0.5% from 400 to 700 nm) and optimizing the film structure and film thickness based on the needle method.

[0077] The actual measured value of the spectral reflectance is calculated by measuring the spectral reflectance with respect to light incident from the normal direction using a microspectrophotometer USPM-RU III manufactured by Olympus Corporation.

[0078] Figure 5 shows the spectral reflectance R required for a conventional light-shielding film when Black A is used as the film material. ref and the measured spectral reflectance D of the light-shielding film of the present invention. ref FIG.

[0079] That is, the measured spectral reflectance D of the light-shielding film of the present invention ref In the light wavelength range of 400 to 700 nm, the spectral reflectance value R required for the conventional light-shielding film is shown in FIG. ref falls below.

[0080] (3.2) Deviation of spectral transmittance values If the deviation of the spectral transmittance from the preset design value is small, the influence of oxygen is reduced and the film is chemically stable, and as a result, the film has excellent anti-reflection properties.

[0081] Whether the deviation between the design value and the actual measured value was large was judged by whether the area where the design value and the actual measured value differed by 1% or more in spectral transmittance when the design value and the actual measured value were graphed within the light wavelength range of 400 to 700 nm accounted for 50% or more of the line on the graph.

[0082] The design value of the spectral transmittance is calculated using the thin film calculation software TF-CALC (Software Spectra, Inc.), inputting the transmittance target (set to 0.5% from 400 to 700 nm) and optimizing the film structure and film thickness based on the needle method.

[0083] The actual measured value of the spectral transmittance is calculated by measuring using a spectrophotometer U4100 (manufactured by Hitachi High-Technologies Corporation).

[0084] Figure 6 shows the spectral transmittance R required for a conventional light-shielding film when Black A is used as the film-forming material. tra and the measured spectral transmittance D of the light-shielding film of the present invention. tra FIG.

[0085] That is, the measured spectral transmittance D of the light-shielding film of the present invention tra In the light wavelength range of 400 to 700 nm, the spectral transmittance R required for the conventional light-shielding film is shown in FIG. tra falls below.

[0086] 4.Optical components The optical member of the present invention is an optical member comprising at least a light-shielding film on a substrate, and is characterized in that the light-shielding film comprises the above-mentioned light-shielding film of the present invention.

[0087] From the viewpoint of antireflection properties, it is preferable that the optical member has a light interference layer formed on the light-shielding film. From the viewpoint of antireflection properties, it is preferable that the optical member has a light interference layer formed between the base material and the light-shielding film. The optical member of the present invention is preferably used as a light-shielding member for a mobile phone camera or a camera optical system. The optical member of the present invention may, for example, have the layer structure as shown in the above-mentioned FIGS. Substrates according to the present invention include, but are not limited to, resins such as cycloolefin copolymers (COC), cycloolefin polymers (COP) and polyester resins.

[0088] 5. Method for manufacturing light-shielding film and multi-layer anti-reflection film The method for producing a light-shielding film of the present invention is a method for producing the above-mentioned light-shielding film, and preferably, the light-shielding layer is formed by depositing a mixture of chromium and silicon dioxide in an argon gas or nitrogen gas atmosphere. Furthermore, the method for producing a multilayer antireflection film of the present invention is a method for producing the multilayer antireflection film of the present invention described above, and preferably includes a step of forming the light-shielding film, and a step of laminating at least a light interference layer on the light-shielding film.

[0089] (5.1) Method of forming each constituent layer in the manufacture of a light-shielding film and a multi-layer anti-reflection film The light-shielding film of the present invention is preferably produced by using argon gas or nitrogen gas as the inert gas, and forming the light-shielding layer by depositing a mixture of chromium and silicon dioxide in an argon gas or nitrogen gas atmosphere. The multilayer antireflection film can be suitably produced by the process for producing the multilayer antireflection film, which comprises a step of forming a light-shielding film and a step of laminating at least a light interference layer on the light-shielding film.

[0090] As a method for forming the above-mentioned light-shielding layer, the layer in contact with the light-shielding layer, the light interference layer, and the spectral characteristic adjusting layer on the substrate, various known methods can be used. However, it is preferable to form the layers by a chemical vapor deposition method such as a sputtering method (e.g., magnetron cathode sputtering, planar magnetron sputtering, two-pole AC planar magnetron sputtering, two-pole AC rotating magnetron sputtering, etc., including reactive sputtering methods), a deposition method (e.g., resistance heating deposition, electron beam deposition, ion beam deposition, plasma-assisted deposition, and vacuum deposition using an IAD method), a thermal CVD method, a catalytic chemical vapor deposition method (Cat-CVD), a capacitively coupled plasma CVD method (CCP-CVD), a photo-CVD method, a plasma CVD method (PE-CVD), an epitaxial growth method, or an atomic layer growth method.

[0091] The film-forming material used in the manufacture of the light-shielding film and the multilayer antireflection film of the present invention is as described above. Metal fluorides (e.g., MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 Al 3 F 14 and CeF 3 When using a method such as the IAD method, it is preferable not to use the IAD method, because the metal fluoride is decomposed by ion irradiation during film formation.

[0092] When using vacuum deposition as the deposition condition for each layer, the degree of vacuum in the chamber is usually 1×10 -4 ~1×10 -1 Pa, preferably 1×10 -3 ~3×10 -2Pa range, the deposition rate is within the range of 1 to 10 Å / sec, specifically, for example, a BES-1300DN manufactured by Shincron is used, the heating temperature is 340°C, and the initial vacuum is 1.33×10 -3 It is preferable to form each layer at a film formation rate suited to Pa and each film formation material.

[0093] Examples of the form of the light-shielding film and the multilayer antireflection film formed on the substrate include the forms shown in Figs. 1 to 4, and the layers of the light-shielding film and the multilayer antireflection film are formed in order from the substrate side in accordance with the above-mentioned "(5.1) Method of forming each constituent layer in the production of the light-shielding film and the multilayer antireflection film".

[0094] When forming each layer of the light-shielding film and the multilayer antireflection film, an appropriate film-forming material is loaded into the evaporation source of the evaporation device used. When forming the light-shielding layer, a film-forming material containing chromium and silicon dioxide is loaded into the evaporation source of the evaporation device used, and when forming a layer in contact with the light-shielding layer, a film-forming material containing a compound other than an oxide is loaded into the evaporation source of the evaporation device used.

[0095] (5.2) Manufacturing process flow FIG. 7 is a flowchart showing an example of the manufacturing process flow for a light-shielding film, FIG. 8 is a flowchart showing an example of the manufacturing process flow for a multilayer antireflection film having a front-side antireflection effect, FIG. 9 is a flowchart showing an example of the manufacturing process flow for a multilayer antireflection film having a back-side antireflection effect, and FIG. 10 is a flowchart showing an example of the manufacturing process flow for a multilayer antireflection film having both a front-side and back-side antireflection effect.

[0096] That is, FIG. 7 shows the flow of the manufacturing process for producing the light-shielding film of FIG. 1, FIG. 8 shows the flow of the manufacturing process for producing the multilayer antireflection film of FIG. 2, and FIG. 9 shows the flow of the manufacturing process for producing the multilayer antireflection film of FIG. 3. In FIG. 10, the steps from D1, in which an optical interference layer for front-surface antireflection is formed, to D2, in which a spectral characteristic adjustment layer for back-surface antireflection is formed, are not a single process. Between D1 and D2, there is a process in which the multilayer antireflection film being formed is temporarily removed from the film-forming apparatus, and an optical element is set on a mask jig for forming a light-shielding film in the atmosphere. From D3 onwards, the optical element is returned to the film-forming apparatus, and film formation is started again.

[0097] (5.3) Vapor deposition equipment FIG. 11 is a schematic diagram showing an example of a vacuum deposition apparatus. The vacuum deposition apparatus 1 includes a dome 3 in a chamber 2 , along which a substrate 4 is placed. The deposition source 5 is equipped with an electron gun for evaporating the deposition material or a resistance heating device, and the deposition material 6 is scattered from the deposition source 5 toward the substrate 4 and condenses and solidifies on the substrate 4 . When the IAD method is used, an ion beam 8 is irradiated from an IAD ion source 7 toward the substrate, and the high kinetic energy of the ions is used during film formation to form a dense film and increase the adhesion of the film. Here, an example of the substrate 4 is glass.

[0098] A plurality of deposition sources 5 may be disposed at the bottom of the chamber 2 . Although one vapor deposition source is shown as the vapor deposition source 5 here, the number of vapor deposition sources 5 may be multiple. A deposition material (evaporation material) from an evaporation source 5 is generated by an electron gun to generate an evaporation substance 6, which is then scattered and attached to a substrate 4 (e.g., a glass plate) placed in a chamber 2, thereby forming a layer made of the film formation material on the substrate 4.

[0099] The chamber 2 is also provided with a vacuum exhaust system (not shown), which draws a vacuum inside the chamber 2 . The vacuum level in the chamber is usually 1×10 -4 ~1×10 -1 Pa, preferably 1×10 -3 ~3×10 -2 The range is Pa.

[0100] The dome 3 holds at least one holder (not shown) that holds the substrate 4, and is also called an evaporation umbrella. The dome 3 has an arc-shaped cross section and a rotationally symmetric shape that rotates about an axis that passes through the center of a chord connecting both ends of the arc and is perpendicular to the chord. When the dome 3 rotates around the axis at, for example, a constant speed, the substrate 4 held by the dome 3 via the holder revolves around the axis at a constant speed.

[0101] This dome 3 is capable of holding a plurality of holders arranged in the direction of the radius of rotation (orbital radius) and the direction of rotation (orbital direction). This makes it possible to simultaneously form films on a plurality of substrates 4 held by a plurality of holders, thereby improving the efficiency of device manufacturing.

[0102] The IAD ion source 7 is a device that introduces argon gas or oxygen gas into its body, ionizes the gas, and irradiates the substrate 4 with the ionized gas molecules (ion beam 8). As the ion source, a Kaufman type (filament), hollow cathode type, RF type, bucket type, duoplasmatron type, etc. can be used. By irradiating the substrate 4 with the above-mentioned gas molecules from the IAD ion source 7, for example, molecules of film-forming material evaporated from multiple evaporation sources can be pressed against the substrate 4, and a film with high adhesion and density can be formed on the substrate 4. The IAD ion source 7 is disposed at the bottom of the chamber 2 so as to face the substrate 4, but may be disposed at a position shifted from the facing axis.

[0103] The ion beam used in the IAD method tends to be used at a lower degree of vacuum and at a lower acceleration voltage than the ion beam used in the ion beam sputtering method. For example, an ion beam with an acceleration voltage of 100 to 2000 V and a current density of 1 to 120 μA / cm 2 An ion beam of 1000 nm can be used. The ion beam used in the film forming process may be an oxygen ion beam, an argon ion beam, or an ion beam of a mixed gas of oxygen and argon. For example, it is preferable that the amount of oxygen gas introduced is within the range of 30 to 60 sccm, and the amount of argon gas introduced is within the range of 0 to 10 sccm.

[0104] The monitor system (not shown) is a system for monitoring the wavelength characteristics of the layer formed on the substrate 4 by monitoring the layer that evaporates from each deposition source 5 and adheres to itself during vacuum film formation. This monitor system makes it possible to grasp the optical characteristics (eg, spectral transmittance, spectral reflectance, optical layer thickness, etc.) of the layer formed on the substrate 4. The monitoring system may also include a quartz layer thickness monitor to monitor the physical layer thickness of the layers deposited on the substrate 4 . This monitor system also functions as a control unit that controls the ON / OFF switching of the multiple evaporation sources 5 and the ON / OFF switching of the IAD ion source 7 according to the results of monitoring the layer. EXAMPLES

[0105] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.

[0106] (Outline of optical component formation, deposition materials and deposition conditions) Using a deposition apparatus BES-1300DN (manufactured by Shincron Co., Ltd.) and a glass substrate H-ZF52GT (nd=1.8467, manufactured by Chengdu Guangming Co., Ltd.), various optical components were formed by forming each layer in order from the substrate side on one side of the substrate.

[0107] (Layer thickness measurement) The thickness of each of the above layers was measured by the following method.

[0108] (1) A layer to be measured is formed in advance on a substrate to a thickness of 1 / 4λ (λ=550 nm), and the spectral reflectance is measured.

[0109] (2) Each layer is formed on the layer formed in (1) above under the film formation conditions shown in Table I below, the spectral reflectance is measured, and the refractive index and layer thickness of the layer are calculated from the change in the spectral reflectance. The film forming materials used in the examples are as follows:

[0110] (Film forming materials) (1)BlackA powder less than 0.3mm Patinal (Merck, Cr[45%]+SiO 2 [50-60%] mixture, hereafter referred to as "Black A" (2)Magnesium fluoride granules about 1-2.5mm(MgF 2 ) Patinal (Merck, hereafter referred to as "MgF 2 " is written as ".) (3) Substance H4 granules about 0.1-2 mm Patinal (Merck, LaTiO 3 [99%], hereafter the product name will be referred to as "H4".) (4) YF 3 (Merck) (5)Silicon dioxide granules about 1-4mm(SiO 2 ) Patinal (Merck, hereafter referred to as "SiO 2 " is written as ".) (6) AlF 2 (Merck) (7) NdF 3 (Merck) (8) LaF 3 (Merck) (9) GdF 3 (Merck) (10)YbF 3 (Merck) (11)PbF 2 (Merck) (12)Na 3 AlF 6 (Merck) (13)Na 5 Al 3 F 14 (Merck) (14) CeF 3 (Merck) (15) ZnS (Merck) (16) Al 2 O 3 (Merck) (17)ZrTiO 4 (Merck)

[0111] First, Table I shows the film formation conditions when each layer was formed using each film formation material. In Table I, for example, AlF is used as the deposition material when forming each layer. 2 When using the conditions shown in Table I (AlF 2 )> to form each layer, and YbF 3 When using YbF 3 )> to form each layer. Hereinafter, in the description of the examples, "the XXth layer counted from the substrate" will be expressed as "the XXth layer". For example, "the third layer counting from the base material" should be written as "the third layer."

[0112] [Table 1]

[0113] (Confirmation of the deviation between the design value and the actual measured value of the spectral reflectance and spectral transmittance of the light-shielding film) Before preparing the optical members in the examples, sample optical members A1, A2, and A3 were prepared according to the following procedure in order to confirm the effect on the design values ​​and actual measured values ​​of the spectral reflectance and the spectral transmittance when the layer in contact with the light-shielding layer contains an oxide and when it contains a substance other than an oxide during the formation of the light-shielding film. The sample optical member was produced according to the layer structure shown in FIG.

[0114] (1) Preparation of optical components for each sample According to the film-forming conditions shown in Table I above, the following various optical members were produced. [Preparation of sample optical member A1] Under the conditions (Black A) shown in Table I above, a light-shielding layer containing chromium and silicon dioxide and having a thickness of 1,500 nm was formed on a substrate. Next, the conditions shown in Table I (MgF 2 )>, a layer containing a compound other than an oxide and having a thickness of 114 nm (a layer in contact with the light-shielding layer) was formed on the light-shielding layer to prepare a sample optical member A1.

[0115] [Preparation of sample optical member A2] Under the conditions (Black A) shown in Table I above, a light-shielding layer containing chromium and silicon dioxide and having a thickness of 1,500 nm was formed on a substrate. Next, the conditions (SiO 2 )>, a layer containing an oxide and having a thickness of 188 nm (a layer in contact with the light-shielding layer) was formed on the light-shielding layer, thereby preparing a sample optical member A2.

[0116] [Preparation of sample optical member A3] Under the conditions (Black A) shown in Table I above, a light-shielding layer containing chromium and silicon dioxide and having a thickness of 1,500 nm was formed on a substrate. Next, under the <Condition (H4)> shown in Table I above, a layer containing an oxide (a layer in contact with the light-shielding layer) having a thickness of 114 nm was formed on the light-shielding layer to prepare a sample optical member A3.

[0117] (2) Deviation between design value and actual measurement value For the sample optical members A1 to A3 obtained as described above, design values ​​and actual measured values ​​of the spectral reflectance and the spectral transmittance in the light wavelength range of 400 to 700 nm were calculated. FIG. 12 shows a graph of the spectral reflectances of the sample optical members A1 to A3.

[0118] As for the spectral transmittance, since almost no deviation was observed between the design value and the measured value for each optical member, a graph is omitted.

[0119] As can be seen from Figure 12, with regard to spectral reflectance, the deviation between the design value and the actual measured value is smaller for sample optical member A1 than for sample optical members A2 and A3. This shows that an optical member containing a compound other than an oxide in a layer in contact with the light-shielding layer is less affected by oxygen and is more chemically stable than an optical member containing an oxide in a layer in contact with the light-shielding layer, and as a result, has excellent anti-reflection effect.

[0120] A. Preparation of optical components with light-shielding films [Preparation of Optical Component No. 1] (A.1) Formation of light-shielding film (A.1.1) Formation of light-shielding layer (first layer) Under the conditions (Black A) shown in Table I above, a light-shielding layer having a thickness of 1500 nm was formed on the substrate.

[0121] (A.1.2) Formation of the layer in contact with the light-shielding layer (second layer) The conditions shown in Table I (MgF 2 )>, a layer having a thickness of 81.2 nm (a layer in contact with the light-shielding layer) was formed on the light-shielding layer (first layer).

[0122] (A.2) Fabrication of optical components By the above steps, an optical member No. 1 was produced, which was provided with a light-shielding film formed with the layer structure shown in Table II.

[0123] [Preparation of Optical Members No. 2 and 3] Optical members Nos. 2 and 3 were produced by changing the film forming materials and layer thicknesses of the first and second layers as shown in Table II and applying the conditions in Table I in accordance with each film forming material.

[0124] [Table 2]

[0125] B. Preparation of optical components with multi-layer anti-reflection coatings having surface anti-reflection effects As described above, in the present invention, the "surface" refers to the "surface opposite the substrate side as viewed from the light-shielding film," and the "surface anti-reflection effect" refers to the "effect of preventing reflection of light incident from the surface opposite the substrate side as viewed from the light-shielding film."

[0126] [Preparation of Optical Component No. 4] (B.1) Formation of light-shielding film (B.1.1) Formation of light-shielding layer (first layer) Under the conditions (Black A) shown in Table I above, a light-shielding layer having a thickness of 1500 nm was formed on the substrate.

[0127] (B.1.2) Formation of the layer (second layer) in contact with the light-shielding layer The conditions shown in Table I (MgF 2 )>, a layer having a thickness of 8.0 nm (a layer in contact with the light-shielding layer) was formed on the light-shielding layer (first layer).

[0128] (B.2) Formation of multi-layer anti-reflection coating (B.2.1) Formation of optical interference layers (layers 3 to 8) Condition (H4) or Condition (MgF 2 )> was applied in the layer order of Table III, and each layer was formed on the layer (second layer) adjacent to the light-shielding layer, thereby forming a light interference layer.

[0129] (B.3) Fabrication of optical components By the above steps, an optical member No. 4 was prepared, which was provided with a multi-layer antireflection coating having a surface antireflection effect and having the layer structure shown in Table III.

[0130] [Preparation of Optical Component No. 5] In the formation of the light-shielding layer (first layer) in [Preparation of Optical Member No. 4] (B.1.1), the <Conditions (Black A)> shown in Table I were changed to <Conditions (Black A:Ar)>, and argon (Ar) gas was introduced as an inert gas when forming the light-shielding layer. Except for this, the film-forming materials and layer thicknesses of the first to eighth layers (light-shielding layer, layer in contact with the light-shielding layer, and optical interference layer) were changed as shown in Table III, and the conditions in Table I were applied according to each film-forming material to prepare Optical Member No. 5. As described above, by introducing argon (Ar) gas as an inert gas during the formation of the light-shielding layer, oxidation of the light-shielding film BlackA is suppressed, and the refractive index and light absorption coefficient of the light-shielding layer are increased. Because the absorption coefficient of the light-shielding film is increased, the same transmittance can be ensured even if the light-shielding layer is thin, and it is possible to obtain results equivalent to those of optical member No. 4. In the above fabrication method, argon (Ar) gas was introduced as an inert gas, but nitrogen (N 2 ) gas can also be used to obtain the same effect.

[0131] [Preparation of optical components No. 6 to 25] The film-forming materials and layer thicknesses of the first to eighth layers (light-shielding layer, layer in contact with the light-shielding layer, and light interference layer) were changed as shown in Tables III to VI, and optical members Nos. 6 to 25 were produced by applying the conditions in Table I according to each film-forming material.

[0132] [Table 3]

[0133] [Table 4]

[0134] [Table 5]

[0135] [Table 6]

[0136] C. Fabrication of optical components equipped with a multi-layer anti-reflection coating having a back surface anti-reflection effect As described above, in the present invention, the "rear surface" refers to the "surface on the substrate side as viewed from the light-shielding film," and the "rear surface anti-reflection effect" refers to the "effect of preventing reflection of light incident from the substrate side as viewed from the light-shielding film."

[0137] [Preparation of Optical Component No. 26] (C.1) Formation of multi-layer anti-reflection coating (C.1.1) Formation of optical interference layers (1st to 8th layers) Condition (H4) or Condition (MgF 2 )> were applied in the layer order of Table VII to form optical interference layers (1st layer to 8th layer).

[0138] (C.2) Fabrication of optical components By the above steps, optical member No. 26 was prepared, which was provided with a multilayer antireflection coating having a back surface antireflection effect and having the layer structure shown in Table VII.

[0139] [Preparation of Optical Component No. 27] (C.3) Formation of multi-layer anti-reflection coating (C.3.1) Formation of optical interference layers (1st to 7th layers) Condition (H4) or Condition (MgF 2 )> were applied in the layer order of Table VII to form a light interference layer (first layer to seventh layer).

[0140] (C.4) Formation of light-shielding film (C.4.1) Formation of layer in contact with light-shielding layer (layer 8) The conditions shown in Table I (MgF 2 )>, a layer having a thickness of 94.1 nm (a layer in contact with the light-shielding layer) was formed on the seventh layer.

[0141] (C.4.2) Formation of light-shielding layer Under the conditions (Black A) shown in Table I above, a light-shielding layer having a thickness of 1500 nm was formed on the layer (layer 8) in contact with the light-shielding layer.

[0142] (C.5) Fabrication of optical components By the above steps, optical member No. 27 was prepared, which was provided with a multilayer antireflection coating having a back surface antireflection effect and having the layer structure shown in Table VII.

[0143] [Preparation of Optical Component No. 28] (C.6) Formation of multi-layer anti-reflection coating (C.6.1) Formation of optical interference layers (1st to 8th layers) Condition (H4) or Condition (MgF 2 )> were applied in the layer order of Table VII to form optical interference layers (1st layer to 8th layer).

[0144] (C.6.2) Formation of spectral characteristic adjustment layers (9th to 17th layers) Condition (H4) or Condition (MgF 2 )> was applied in the layer order of Table VII to form spectral characteristic adjustment layers (9th to 17th layers) on the light interference layers (1st to 8th layers).

[0145] (C.7) Formation of light-shielding film (C.7.1) Formation of layer (18th layer) adjacent to the light-shielding layer The conditions shown in Table I (MgF 2 )>, a layer having a thickness of 8.0 nm (layer in contact with the light-shielding layer) was formed on the spectral characteristic adjustment layers (9th to 17th layers).

[0146] (C.7.2) Formation of light-shielding layer (19th layer) Under the conditions (Black A) shown in Table I above, a light-shielding layer having a thickness of 1500 nm was formed on the layer (layer 18) in contact with the light-shielding layer.

[0147] (C.8) Fabrication of optical components By the above steps, optical member No. 28 was prepared, which was provided with a multilayer antireflection coating having a back surface antireflection effect and having the layer structure shown in Table VII.

[0148] [Preparation of Optical Component No. 29] (C.9) Formation of multi-layer anti-reflection coating (C.9.1) Formation of optical interference layers (1st to 8th layers) Condition (H4) or Condition (MgF 2 )> were applied in the layer order of Table VII to form optical interference layers (1st layer to 8th layer).

[0149] (C.9.2) Formation of spectral characteristic adjustment layers (9th to 16th layers) Condition (H4) or Condition (MgF 2 )> were applied in the layer order of Table VII to form spectral characteristic adjustment layers (9th to 16th layers) on the 8th layer.

[0150] (C.10) Formation of light-shielding film (C.10.1) Formation of layer (17th layer) adjacent to the light-shielding layer The conditions shown in Table I (MgF 2 )>, a layer having a thickness of 40.7 nm (layer in contact with the light-shielding layer) was formed on the spectral characteristic adjustment layers (9th to 16th layers).

[0151] (C.10.2) Formation of light-shielding layer (18th layer) Under the conditions (Black A) shown in Table I above, a light-shielding layer having a thickness of 1500 nm was formed on the layer (layer 17) in contact with the light-shielding layer.

[0152] (C.11) Fabrication of optical components By the above steps, optical member No. 29 was prepared, which was provided with a multilayer antireflection coating having a back surface antireflection effect and having the layer structure shown in Table VII.

[0153] [Table 7]

[0154] D. Multi-layer anti-reflection coating with anti-reflection effect on both the front and back sides [Preparation of Optical Component No. 30] (D.1) Formation of a layer having a back surface antireflection effect in a multi-layer antireflection coating (D.1.1) Formation of optical interference layers (1st to 8th layers) Condition (H4) or Condition (MgF 2 )> were applied in the layer order of Table VIII to form a light interference layer (1st layer to 8th layer). Thereafter, the optical member in the process of being manufactured was temporarily removed from the film-forming apparatus, and set on a mask jig for forming a light-shielding film under atmospheric conditions.

[0155] (D.1.2) Formation of Spectral Characteristics Adjustment Layers (Layers 9 to 17) Condition (H4) or Condition (MgF 2 )> was applied in the layer order of Table VIII to form spectral characteristic adjustment layers (9th to 17th layers) on the light interference layers (1st to 8th layers).

[0156] (D.1.3) Formation of the spectral characteristic adjustment layer and the layer (18th layer) that contacts the light-shielding layer formed in a single process In the process of forming the adjustment layer, the conditions shown in Table I above (MgF 2 )>, a layer having a thickness of 8.0 nm (layer in contact with the light-shielding layer) was formed on the spectral characteristic adjustment layers (9th to 17th layers).

[0157] (D.2) Formation of light-shielding film (D.2.1) Formation of layer in contact with light-shielding layer (layer 18) Since the layer (18th layer) in contact with the light-shielding layer was formed by the above steps, the formation of the light-shielding layer was started as the next step.

[0158] (D.2.2) Formation of light-shielding layer (19th layer) The optical element with the above-mentioned layers formed thereon was returned to the film-forming apparatus, and a light-shielding layer having a thickness of 1,500 nm was formed on the layer in contact with the light-shielding layer (layer 18) under the <Conditions (Black A)> shown in Table I above.

[0159] (D.2.3) Formation of layer in contact with light-shielding layer (layer 20) The conditions shown in Table I (MgF2 )> to form a layer having a thickness of 8.0 nm (a layer in contact with the light-shielding layer) on the light-shielding layer (19th layer).

[0160] (D.3) Formation of a layer having a surface antireflection effect in a multilayer antireflection coating (D.3.1) Formation of optical interference layers (Layers 21 to 26) Condition (H4) or Condition (MgF 2 )> was applied in the layer order of Table VIII, and each layer was formed on the layer (20th layer) adjacent to the light-shielding layer, thereby forming a light interference layer.

[0161] (D.4) Fabrication of optical components By the above steps, optical member No. 30 was prepared, which was provided with a multilayer antireflection coating having antireflection effects on both the front and back surfaces and having the layer structure shown in Table VIII.

[0162] [Table 8]

[0163] <Spectral reflectance and spectral transmittance> (1) Spectral reflectance <Design value> The design values ​​of the spectral reflectance of the obtained optical member samples No. 1 to No. 29 were calculated using thin film calculation software TF-CALC (Software Spectra, Inc.). For thin film design, the reflectance target (set to 0.5% from 400 to 700 nm) was input, and the film structure and film thickness were optimized based on the needle method. In this case, the spectral reflectance values ​​at 10 nm intervals from 400 to 700 nm were extracted and graphed, and the performance of each optical member was evaluated by evaluating the deviation between the design value and the actual measured value of each optical member. At the same time, the design value of the average spectral reflectance was calculated according to the above-mentioned calculation method.

[0164] <Actual measurements> The spectral reflectance for light incident from the normal direction was measured using an Olympus USPM-RU III microspectrometer. In this case, the spectral reflectance values ​​at 10 nm intervals from 400 to 700 nm were extracted and graphed, and the performance of each optical member was evaluated by evaluating the deviation between the design value and the actual measured value of each optical member. At the same time, the actual average spectral reflectance was calculated according to the above-mentioned calculation method.

[0165] <Evaluation method> The deviation between the design value and the measured value of each of the optical members was evaluated according to the following criteria. In the following criteria, "the deviation between the design value and the actual measurement value is large" means that, when the design value and the actual measurement value are graphed within a light wavelength range of 400 to 700 nm, the area where the two values ​​differ from each other by 1% or more in terms of spectral reflectance accounts for 50% or more of the line on the graph, as in the case of optical members A2 and A3 in FIG. 10, while a case where this is not the case, as in the case of optical member A1, is defined as "the deviation between the design value and the actual measurement value is small."

[0166] (Evaluation Criteria) ◯: When the design value and the actual measured value of the spectral reflectance are graphed, the difference between the two values ​​is small and at a level that is not problematic for practical use. ×: When the design value and the actual measured value of the spectral reflectance are graphed, the difference between the two values ​​is large, to a level that causes problems in practical use.

[0167] (2) Spectral transmittance <Design value> The design values ​​of the spectral reflectance of the obtained optical member samples No. 1 to No. 29 were calculated using thin film calculation software TF-CALC (Software Spectra, Inc.). In this case, the spectral transmittance values ​​at 10 nm intervals from 400 to 700 nm were extracted and graphed, and the performance of each optical member was evaluated by evaluating the deviation between the design value and the actual measured value of each optical member. At the same time, the design value of the average spectral transmittance was calculated according to the above-mentioned calculation method. The design values ​​of the spectral transmittance of each optical member were graphed.

[0168] <Actual measurements> The spectral transmittance was measured using a spectrophotometer U4100 (manufactured by Hitachi High-Technologies Corporation). In this case, the spectral transmittance values ​​at 10 nm intervals from 400 to 700 nm were extracted and graphed, and the performance of each optical member was evaluated by evaluating the deviation between the design value and the actual measured value of each optical member. At the same time, the design value of the average spectral transmittance was calculated according to the above-mentioned calculation method.

[0169] <Evaluation method> The deviation between the design value and the measured value of each of the optical members was evaluated according to the following criteria. In the following criteria, "the deviation between the design value and the actual measurement value is large" means that when the design value and the actual measurement value are graphed within the light wavelength range of 400 to 700 nm, the area where the two values ​​differ by 1% or more in spectral transmittance accounts for 50% or more of the line on the graph, and if this is not the case, it is defined as "the deviation between the design value and the actual measurement value is small."

[0170] (Evaluation Criteria) ◯: When the design value and the actual measured value of the spectral transmittance are graphed, the difference between the two values ​​is small and at a level that does not cause any practical problems. ×: When the design value and the actual measured value of the spectral transmittance are graphed, the difference between the two values ​​is large, to a level that is problematic in practical use.

[0171] (3) Evaluation of each optical component Each of the optical members produced in the examples and comparative examples was evaluated according to the above evaluation criteria. The evaluation results are shown in Tables II to VIII.

[0172] (4) Summary From the above, it was found that in each of the optical components of the Examples, unlike each of the optical components of the Comparative Examples, the deviation range from the preset design values ​​in terms of spectral reflectance and spectral transmittance is small, and light-shielding films and multilayer anti-reflection films having excellent light-shielding properties, light anti-reflection properties, and chemical stability can be obtained. [Explanation of symbols]

[0173] 1 Vacuum deposition equipment 2 Chambers 3. Dome 4. Board 5 Vapor deposition source 6 Deposited substance 7 IAD ion source 8. Ion Beam L(1) Light shielding layer L(2) Layer adjacent to the light-shielding layer L R Optical interference layer L a Spectroscopic properties of the layers R ref Spectral reflectance values ​​required for conventional light-shielding films D ref Actual measured spectral reflectance R tra Spectral transmittance values ​​required for conventional light-shielding films D tra Actual measured spectral transmittance

Claims

1. A light-shielding film having at least a light-shielding layer and a layer in contact with the light-shielding layer, the light-shielding layer contains chromium and silicon dioxide; At least one of the layers in contact with the light-shielding layer contains a compound other than an oxide. A light-shielding film characterized by:

2. At least one of the layers in contact with the light-shielding layer is made of MgF 2 , AlF 2 , NdF 3 , LaF 3 , Y.F. 3 , GdF 3 , YbF 3 , PbF 2 , Na 3 AlF 6 , Na 5 A 3 F 14 and CeF 3 Contains any one of the fluorides selected from The light-shielding film according to claim 1 .

3. At least one of the layers in contact with the light-shielding layer contains a sulfide.

3. The light-shielding film according to claim 1 or 2.

4. The sulfide is ZnS. The light-shielding film according to claim 3 .

5. The average spectral transmittance in the wavelength range of 400 to 700 nm is 2% or less. The light-shielding film according to any one of claims 1 to 4.

6. A multi-layer anti-reflection film having a light-shielding film, The light-shielding film according to any one of claims 1 to 5 is provided as the light-shielding film, and at least one light interference layer is provided on a layer in contact with the light-shielding layer. A multilayer anti-reflection coating comprising:

7. A layer for adjusting spectral characteristics is provided between the layer in contact with the light-shielding layer and the light interference layer.

7. The multilayer anti-reflection coating according to claim 6.

8. The average spectral reflectance in the wavelength range of 400 to 700 nm is 2% or less.

8. The multilayer antireflection coating according to claim 6 or 7.

9. A method for producing the light-shielding film according to any one of claims 1 to 5, comprising the steps of: The light-shielding layer is formed by depositing a mixture of chromium and silicon dioxide in an argon gas atmosphere. A method for producing a light-shielding film comprising the steps of:

10. A method for producing the light-shielding film according to any one of claims 1 to 5, comprising the steps of: The light-shielding layer is formed by depositing a mixture of chromium and silicon dioxide in a nitrogen gas atmosphere. A method for producing a light-shielding film comprising the steps of:

11. A method for producing the multilayer antireflection film according to any one of claims 6 to 8, comprising the steps of: The method includes the steps of forming the light-shielding film and laminating at least a light interference layer on the light-shielding film.

2. A method for producing a multilayer anti-reflection coating comprising the steps of:

12. An optical member having at least a light-shielding film on a substrate, The light-shielding film according to any one of claims 1 to 5 is provided as the light-shielding film. An optical member characterized by:

13. An optical interference layer is formed on the light-shielding film. The optical member according to claim 12 .

14. A light interference layer is formed between the substrate and the light-shielding film.

14. The optical member according to claim 12 or 13.

Citation Information

Patent Citations

  • Optical system component

    JP2011064737A

  • Light absorber and imaging apparatus using the same

    JP2013148844A