Filter base material for mask, and mask with the same

JP2024154001APending Publication Date: 2024-10-30JAPAN VILENE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023067567
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Benefits of technology

【0011】 本願出願人は、繊維層Aと繊維層Bそして繊維層Cを備えており、前記繊維層A-前記繊維層B-前記繊維層Cの順に積層することで形成されている、マスク用フィルタ基材について検討を続けた。そして、検討の結果、当該マスク用フィルタ基材を備えてなるマスクにおいて、前記繊維層A-前記繊維層B-前記繊維層Cの順に通気度が低減しているときに、当該マスク用フィルタ基材の血液バリア性が向上して、血液バリア性に富むマスクを提供できることを見出した。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154001000001_ABST
    Figure 2024154001000001_ABST
Patent Text Reader

Abstract

To provide a filter base material for a mask capable of realizing a mask with an excellent blood barrier property, and a mask containing the filter base material for the mask that has an excellent blood barrier property.SOLUTION: A filter base material for a mask comprises a fiber layer A, a fiber layer B, and a fiber layer C, and is formed by laminating the fiber layer A, the fiber layer B and the fiber layer C in this order. The air-permeability decreases in the order of the fiber layer A, the fiber layer B and the fiber layer C from the outside in a mask containing the filter base material for the mask, which improves the blood barrier property of the filter base material for the mask, thereby providing a mask with an excellent blood barrier property.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a mask filter substrate and a mask including the mask filter substrate. [Background technology]

[0002] There has been a demand for masks with excellent dust collection effects. In order to provide masks that meet this demand, the configuration of the filter substrate of the mask (hereinafter, sometimes referred to as a mask filter substrate) has been studied.

[0003] For example, JP 2010-94503 A (Patent Document 1) discloses, as Examples 7 and 8, a mask equipped with a mask filter substrate formed by laminating a spunbond nonwoven fabric, a hydroentangled nonwoven fabric, and a corona-charged meltblown nonwoven fabric in this order from the outermost layer side (the side away from the face when a person wears the mask) to the innermost layer side (the side facing the face when a person wears the mask) in the mask configuration. It also discloses that the mask has an excellent dust collection effect.

[0004] It should be noted that the invention of Patent Document 1 is not an invention that considers the air permeability of the mask filter substrate or each of the fiber layers that constitute the mask filter substrate, and Patent Document 1 does not disclose or suggest the air permeability of each of the fiber layers. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication 2010-94503 Summary of the Invention [Problem to be solved by the invention]

[0006] Furthermore, in recent years, masks are required to have blood barrier properties in order to improve the infection prevention effect of the mask wearer. The blood barrier properties of a mask can be evaluated by whether or not artificial blood that imitates blood permeates the mask filter substrate that constitutes the mask.

[0007] In order to understand the blood barrier properties of masks according to the prior art, the applicant prepared, as an example, a mask having a configuration equivalent to that of the above-mentioned mask (a mask having a mask filter substrate formed by layering a spunbonded nonwoven fabric, a hydroentangled nonwoven fabric, and an electrically charged meltblown nonwoven fabric in this order from the outermost layer side to the innermost layer side when constructing the mask). Artificial blood was then applied to the outermost layer side of the prepared mask, and the blood barrier properties exhibited by the mask were evaluated. However, the evaluation results showed that the artificial blood attached to the outermost layer side of the mask easily permeated the mask filter substrate and seeped out to the innermost layer side of the mask.

[0008] Therefore, the masks according to the conventional technology have a problem in that they do not have sufficient blood barrier properties.

[0009] An object of the present invention is to provide a mask filter substrate that can realize a mask with excellent blood barrier properties, and a mask with excellent blood barrier properties that includes the mask filter substrate. [Means for solving the problem]

[0010] The present invention relates to "(Claim 1) A filter substrate for a mask, comprising a fiber layer A, a fiber layer B, and a fiber layer C, The fiber layer is formed by laminating the fiber layer A, the fiber layer B, and the fiber layer C in this order, The air permeability decreases in the order of the fiber layer A, the fiber layer B, and the fiber layer C. Filter substrate for masks. (Claim 2) A mask comprising the mask filter substrate according to claim 1. (Claim 3) The mask according to claim 2, having a fused portion on the outermost layer. It is. Effect of the Invention

[0011] The applicant of the present application has continued to study a mask filter substrate which includes a fiber layer A, a fiber layer B, and a fiber layer C, and is formed by laminating the fiber layer A, the fiber layer B, and the fiber layer C in this order. As a result of the study, the applicant has found that in a mask including the mask filter substrate, when the air permeability decreases in the order of the fiber layer A, the fiber layer B, and the fiber layer C, the blood barrier property of the mask filter substrate is improved, and a mask with excellent blood barrier property can be provided.

[0012] Although the reason why this composition improves the blood barrier property has not been completely clarified, it is believed to be due to the following effects.

[0013] The fiber layers A, B, and C that make up the mask filter substrate are stacked in such a way that their air permeability decreases in that order. This is thought to make it easier for blood adhering to the outermost layer of a mask equipped with a mask filter substrate having this layered structure to diffuse in a planar direction perpendicular to the thickness direction of the mask filter substrate. As a result, it is believed that by using the mask filter substrate of the present invention, blood adhering to the outermost layer of the mask will diffuse in the planar direction of the mask filter substrate, making it difficult for blood to pass through the mask filter substrate.

[0014] As described above, the mask filter substrate of the present invention can provide a mask with excellent blood barrier properties.

[0015] Furthermore, when a mask equipped with the mask filter substrate according to the present invention has a fused portion on the outermost layer, the mask has improved shape stability in the thickness direction, and therefore is less likely to be unintentionally crushed in the thickness direction when blood adheres to the outermost layer of the mask. As a result, it is believed that when blood adheres to the outermost layer of the mask, the mask is unintentionally crushed in its thickness direction (the thickness direction of the mask filter substrate), which inhibits blood from passing through the mask. From the above, the mask according to the present invention has excellent blood barrier properties. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view of a mask equipped with a mask filter substrate according to the present invention, in which ear hooks provided on the mask are not shown. [Diagram 2] FIG. 1 is a schematic plan view of a mask provided with a mask filter substrate according to the present invention, viewed from the outermost layer side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In the present invention, various configurations, such as the following configurations, can be appropriately selected. Note that, unless otherwise specified, the various measurements described in the present invention are performed under normal pressure, at a temperature of 20°C, and at a humidity of 65 RH%. Furthermore, unless otherwise specified, the various measurement results described in the present invention are measured to a value one digit smaller than the desired value, and the desired value is calculated by rounding off the value. As a specific example, when the desired value is to the first decimal place, the value is measured to the second decimal place, and the obtained value to the first decimal place is rounded off to calculate the value to the first decimal place, and this value is the desired value. Furthermore, each upper limit value and each lower limit value exemplified in the present invention can be combined arbitrarily.

[0018] The configuration of the mask filter substrate according to the present invention will be described with reference to FIG. 1, which is a schematic cross-sectional view of a mask equipped with the mask filter substrate according to the present invention.

[0019] The mask filter substrate (10) according to the present invention includes a fiber layer A (A), a fiber layer B (B), and a fiber layer C (C). The mask filter substrate (10) is formed by laminating the fiber layer A (A), the fiber layer B (B), and the fiber layer C (C) in this order. The mask filter substrate (10) included in the mask (20) shown in FIG. 1 illustrates an embodiment in which the mask filter substrate (10) is formed by laminating the fiber layer A (A), the fiber layer B (B), and the fiber layer C (C) in this order from the outermost layer side to the innermost layer side when the mask (20) is constructed. The outermost layer side of the mask filter substrate (10) when the mask is constructed is the side away from the face when a person wears the mask, and is the side of the mask filter substrate (10) marked with O on the paper. In addition, the innermost layer side of the mask filter substrate (10) when forming a mask is the side that faces the face when a person wears the mask, and is the side of the mask filter substrate (10) marked with I on the paper.

[0020] In Fig. 1, the innermost layer side (fiber layer C (C) side) of the mask filter substrate (10) is superimposed on the main surface of the cup-shaped breathable reinforcement material (11) protruding in one direction, so that the innermost layer side (fiber layer C (C) side) of the mask filter substrate (10) faces the main surface of the cup-shaped breathable reinforcement material (11) protruding in one direction, thereby forming a cup-shaped mask body (12). Then, ear hook members (not shown in Fig. 1) are provided on both the left and right ends of the mask body (12), thereby forming a mask (20) according to one embodiment of the present invention.

[0021] The fiber layer A, fiber layer B, and fiber layer C (hereinafter, sometimes collectively referred to as each fiber layer) according to the present invention are layers derived from, for example, a fiber web or nonwoven fabric, or a fiber aggregate having a sheet shape derived from a woven fabric, knitted fabric, etc. It is preferable that each fiber layer is a fiber layer derived from a fiber web or nonwoven fabric so as to provide a mask filter substrate capable of realizing a mask with excellent blood barrier properties, and a mask with excellent blood barrier properties including the mask filter substrate.

[0022] The fibers constituting each fiber layer may be, for example, a polyolefin resin (e.g., polyethylene, polypropylene, polymethylpentene, polyolefin resin having a structure in which a part of a hydrocarbon is substituted with a cyano group or a halogen such as fluorine or chlorine, etc.), a styrene resin, a polyvinyl alcohol resin, a polyether resin (e.g., polyether ether ketone, polyacetal, modified polyphenylene ether, aromatic polyether ketone, etc.), a polyester resin (e.g., polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polycarbonate, polyarylate, wholly aromatic polyester resin, etc.), a polyimide resin, It can be constructed using known resins such as amide-imide resin, polyamide resin (e.g., aromatic polyamide resin, aromatic polyetheramide resin, nylon resin, etc.), resin having a nitrile group (e.g., polyacrylonitrile, etc.), urethane resin, epoxy resin, polysulfone resin (e.g., polysulfone, polyethersulfone, etc.), fluorine resin (e.g., polytetrafluoroethylene, polyvinylidene fluoride, etc.), cellulose resin, polybenzimidazole resin, acrylic resin (e.g., polyacrylonitrile resin copolymerized with vinyl acetate, acrylic acid ester, or methacrylic acid ester, modacrylic resin copolymerized with acrylonitrile and vinyl chloride or vinylidene chloride, etc.). In particular, each fiber layer is preferably hydrophobic, so that blood can easily diffuse in the plane direction perpendicular to the thickness direction of the mask filter substrate, and each fiber layer is preferably composed of a polyolefin resin. In addition, a fiber layer whose constituent fibers are polyolefin-based resin fibers is more hydrophobic than a fiber layer whose constituent fibers are polyethylene terephthalate fibers.

[0023] These resins may be either linear or branched polymers, and may be block or random copolymers. Furthermore, the resins may have any three-dimensional structure or may have crystallinity, without any particular limitations.

[0024] The constituent fibers may be composed of one type of resin or multiple types of resins. Fibers composed of multiple types of resins may be in the form of what are generally called composite fibers, such as core-sheath type, sea-island type, side-by-side type, orange type, bimetal type, etc. Furthermore, the constituent fibers may be fibers spun by mixing multiple resin components.

[0025] The constituent fibers may include irregular cross-section fibers other than the roughly circular and elliptical fibers. The irregular cross-section fibers may have a fiber cross section of a hollow shape, a polygonal shape such as a triangular shape, an alphabetic shape such as a Y-shape, an irregular shape, a multi-lobed shape, a symbolic shape such as an asterisk shape, or a shape in which a plurality of these shapes are combined.

[0026] The constituent fibers may be formed by kneading a pigment into the fibers, or may be colored dyed fibers (for example, light orange dyed fibers).

[0027] The constituent fibers can be obtained by known methods such as melt spinning, dry spinning, wet spinning, direct spinning (melt blowing, spunbonding, electrostatic spinning, etc.), a method of extracting fibers having a small fiber diameter by removing one or more resin components from composite fibers, and a method of beating fibers to obtain split fibers.

[0028] Each fiber layer can be formed using a fiber web prepared by, for example, a dry method in which the above-mentioned fibers are fed into a carding device or an air-laying device to entangle the fibers; a wet method in which the fibers are dispersed in a solvent and laid into a sheet to entangle the fibers; or a direct spinning method (melt-blowing method, spunbonding method, electrostatic spinning method, or a method in which a spinning solution and a gas flow are discharged in parallel to spin the fibers (e.g., the method disclosed in JP 2009-287138 A) to spin the fibers and collect the fibers, or the like.

[0029] Alternatively, the fibers constituting the prepared fiber web may be entangled and / or integrated to prepare a nonwoven fabric, and the nonwoven fabric may be used to form the nonwoven fabric. Examples of methods for entangling and / or integrating the fibers constituting the fiber web include a method of entangling the fibers with a needle or a water flow, and a method of subjecting the fiber web to a heat treatment, etc., so that the binder or, if the constituting fibers contain heat-fusible fibers, the constituting fibers are bonded and integrated with the heat-fusible fibers.

[0030] The heat treatment method can be appropriately selected, and examples of the method that can be used include heating or heating and pressurizing with a roll, heating by subjecting the material to a heater such as an oven dryer, a far-infrared heater, a dry heat dryer, or a hot air dryer, and heating the resin contained therein by irradiating the material with infrared rays without pressure.

[0031] In addition, as the binder, the various resins mentioned above as the resins capable of preparing the fibers constituting each fiber layer can be used. The weight of the binder is 1 to 200 g / m 2 and 5 to 100 g / m 2 and 10 to 50 g / m 2 It can be.

[0032] Each fiber layer may or may not contain an oil (e.g., a hydrophilic oil). However, in order to provide a mask filter substrate having improved blood barrier properties by including a highly hydrophobic fiber layer B, it is preferable that the fiber layer B does not contain a hydrophilic oil or contains a small amount of hydrophilic oil.

[0033] When each fiber layer contains a heat-fusible fiber as a constituent fiber, the fibers are heat-fused together to impart dimensional stability to the mask equipped with the mask filter substrate. As a result, when blood adheres to the outermost layer side of the mask, the thickness of the mask (the thickness of the mask filter substrate) is unintentionally crushed, which is preferable because blood can be prevented from penetrating the mask. Such heat-fusible fibers may be fully fused heat-fusible fibers, or may be partially fused heat-fusible fibers such as the above-mentioned composite fibers. For example, a low-melting polyolefin resin such as polyethylene or a polyester resin such as low-melting polyethylene terephthalate can be used as a component that exhibits heat fusibility in the heat-fusible fiber.

[0034] The average fiber diameter of the fibers constituting each fiber layer is not particularly limited, but can be 0.1 μm or more, 1 μm or more, 3 μm or more, or 5 μm or more so as to provide a mask filter substrate capable of providing a mask with improved dimensional stability, and can be 100 μm or less, 50 μm or less, or 30 μm or less so as to provide a mask filter substrate with excellent filtration performance.

[0035] The fiber length of the fibers constituting each fiber layer is not particularly limited, but fibers having a specific cut length (hereinafter, sometimes referred to as short fibers) and fibers having no specific cut length (hereinafter, sometimes referred to as continuous fibers) can be used. For example, as short fibers, fibers cut to have a fiber length of 5 mm or more can be used, fibers cut to have a fiber length of 20 mm or more can be used, fibers cut to have a fiber length of 50 mm or more can be used, and fibers cut to have a fiber length of 60 mm or more can be used. The upper limit of the fiber length can also be appropriately adjusted, but it can be 160 mm or less, 110 mm or less, or 80 mm or less. The "fiber length" refers to a value measured in accordance with JIS L1015 (2010), 8.4.1c) direct method (C method).

[0036] In particular, it is preferable that fiber layer B is a fiber layer composed of short fibers, and fiber layer A and fiber layer C are fiber layers composed of continuous fibers. By adopting such fiber layers, it tends to be easier to provide a mask filter substrate with improved blood barrier properties. Although the reason for this is not completely clear, it is thought to be due to the following effects.

[0037] When the fiber layer B is a fiber layer composed of short fibers (for example, a fiber layer derived from a nonwoven fabric such as a hydroentangled nonwoven fabric or a needle-punched nonwoven fabric), the fiber layer B is likely to be a fiber layer in which the fibers are oriented in the thickness direction by being manufactured through an opening process and an entanglement process (hydroentanglement treatment, needle-punch treatment), etc. As a result, a fiber layer B that is difficult to be crushed in the thickness direction can be realized.

[0038] Therefore, by using fiber layer B made of short fibers, it is possible to provide a mask filter substrate that is resistant to unintentional crushing in the thickness direction.

[0039] When fiber layer A and fiber layer C are fiber layers composed of continuous fibers (for example, when fiber layer A is a fiber layer derived from a spunbonded nonwoven fabric and fiber layer C is a fiber layer derived from a meltblown nonwoven fabric), fiber layer A and fiber layer C are produced through a process in which spun fibers are collected in a collector and accumulated, and thus tend to be fiber layers in which the fibers are oriented in a plane direction perpendicular to the thickness direction. As a result, fiber layer A and fiber layer C having main surfaces composed of fibers oriented in the plane direction can be realized.

[0040] Therefore, by having fiber layer A and fiber layer C be fiber layers composed of continuous fibers, blood adhering to the outermost layer side of the mask can easily diffuse in a planar direction perpendicular to the thickness direction of the mask filter substrate, and a mask filter substrate can be provided that is less susceptible to penetration in the thickness direction of the mask filter substrate.

[0041] In addition, when the fiber layer C is a fiber layer with a high fiber density, a mask filter substrate capable of providing a mask with excellent dust collection effect can be realized.

[0042] In particular, the property of fiber layer B of being difficult to crush in the thickness direction, and the properties of fiber layer A and fiber layer C of blood diffusing easily in the planar direction and difficult to penetrate in the thickness direction, are likely to be most effectively exhibited in a mask filter substrate in which fiber layer A, which is a fiber layer made of continuous fibers, is laminated on one main surface of fiber layer B, which is a fiber layer made of short fibers, and fiber layer C, which is a fiber layer made of continuous fibers, is laminated on the other main surface of fiber layer B.

[0043] By having the above-mentioned configuration of the mask filter substrate of the present invention, it is further possible to realize a mask filter substrate capable of realizing a mask with excellent blood barrier properties, and a mask with excellent blood barrier properties comprising the mask filter substrate, which is preferable.

[0044] The configurations of each fiber layer, such as thickness and basis weight, are not particularly limited and may be adjusted as appropriate.

[0045] The thickness of each fiber layer may be 0.05 to 5 mm, 0.1 to 3 mm, or 0.15 to 1 mm. In the present invention, the thickness of each fiber layer refers to the length between the opposing front and back surfaces of each fiber layer when a load of 2 KPa is applied to the main surface of each fiber layer.

[0046] The basis weight of each fiber layer is, for example, 10 to 300 g / m 2 and can be 15 to 200 g / m 2 and 20 to 100 g / m 2 In the present invention, the basis weight is the weight per square meter on the surface (principal surface) having the widest area of ​​the object to be measured. 2 This refers to the mass per unit.

[0047] Each fiber layer may be electrically charged. The type of charging can be appropriately selected, but may be a method using corona charging (corona charging treatment), a method of charging the constituent fibers by contacting them with a polar liquid and applying an external force (liquid charging treatment), or a method of charging constituent fibers of different resin types by rubbing them together (friction charging treatment). In particular, if the fiber layer C, which mainly exhibits filter performance, is electrically charged, it is preferable to realize a mask filter substrate that can provide a mask with excellent dust collection effect. In this case, if the fiber layer C is charged by liquid charging treatment, it is preferable to provide a mask with excellent dust collection effect and a mask filter substrate with improved blood barrier properties.

[0048] The mask filter substrate according to the present invention includes a fiber layer A, a fiber layer B, and a fiber layer C. The mask filter substrate is formed by laminating the fiber layer A, the fiber layer B, and the fiber layer C in this order. The mask filter substrate included in the mask shown in FIG. 1 is formed by laminating the fiber layer A, the fiber layer B, and the fiber layer C in this order from the outermost layer side to the innermost layer side when the mask is constructed. The mask filter substrate is characterized in that the air permeability decreases in the order of the fiber layer A, the fiber layer B, and the fiber layer C.

[0049] The air permeability of each fiber layer can be appropriately adjusted as long as the above-mentioned configuration is satisfied. For example, the air permeability of the fiber layer A is 200 to 500 cm 3 / cm 2 sec., 300~400cm 3 / cm 2 The air permeability of the fiber layer B can be 50 to 300 cm 3 / cm 2 sec., 100~250cm 3 / cm 2 The air permeability of the fiber layer C can be 10 to 100 cm 3 / cm 2 sec., 20~50cm 3 / cm 2 · sec. can be.

[0050] In addition, test pieces (square shape, 150 mm on each side) are prepared using each fiber layer taken from the mask filter substrate, and these are subjected to 6.8.1 (Fragile method) specified in JIS L1913:2010 "General nonwoven fabric test method," whereby the air permeability of each fiber layer can be measured and determined.

[0051] If it is not possible to prepare a square test piece with sides of 150 mm, the air permeability of each fiber layer can be determined as follows.

[0052] Prepare two square flat plates with sides of 150 mm each, each having a circular opening (e.g., a circular opening with a diameter of 50 mm) in the center large enough to be covered by a test piece. Next, stack the flat plates with a test piece (smaller than a square shape with sides of 150 mm) sandwiched between them, so that the opening is covered by the test piece. The flat plates with the test piece sandwiched therebetween thus prepared are used as the test piece in 6.8.1 (Fragile method) to measure the air permeability of each fiber layer. The air permeability of each fiber layer can be calculated by converting the air permeability measured in the open area of ​​the laminated flat plates into the air permeability that would be measured in the area through which air passes through a square test piece with sides of 150 mm when measuring air permeability using the Frazier type testing machine used in 6.8.1 (Fragile type method).

[0053] As a specific example, suppose that the open area of ​​the laminated flat plates is 1 / 10 of the area through which air passes through a square test piece with sides of 150 mm when measuring the air permeability using the Frazier type testing machine used in 6.8.1 (Fragile type method). And, if the air permeability measured and found through the open area of ​​the laminated flat plates is 100 cm 3 / cm 2 Assume that sec. In this case, the air permeability that would be measured when air passes through a square test piece with sides of 150 mm when measuring air permeability using the Frazier tester used in 6.8.1 (Fragile method) can be converted to 10 times the air permeability. From the conversion result, the air permeability of the test piece (smaller than a square shape with sides of 150 mm) is 1000 cm 3 / cm 2 It can be found that sec.

[0054] The mask according to the present invention can be configured as a mask body using only the mask filter substrate. However, in order to realize a mask with excellent rigidity, the mask may be provided with a breathable reinforcing material (such as a sheet-shaped fiber aggregate or porous film) separately provided on the innermost layer side of the mask filter substrate.

[0055] Furthermore, in order to realize a mask with excellent filtering performance, the mask may include a pre-filter layer (such as a sheet-shaped fiber aggregate or a porous film) provided separately on the outermost layer side of the mask filter substrate, or a back-up filter layer (for example, a tribo-electrically charged nonwoven fabric) provided separately on the innermost layer side.

[0056] The lamination method of each fiber layer, or the mask filter substrate and the breathable reinforcing material, prefilter, or backup filter can be adjusted as appropriate. In order to provide a mask that can easily diffuse blood in the surface direction of the mask filter substrate when blood adheres to the outermost layer of the mask, it is preferable that the main surfaces of each layer are simply laminated together without being bonded with fiber adhesive or binder. In this case, the contours of each layer and the fused parts on the main surfaces (14 in Figure 2) may be fused to each other.

[0057] The mask according to the present invention will be described with reference to FIG. 2, which is a schematic plan view of a mask provided with a mask filter substrate according to the present invention, viewed from the outermost layer side.

[0058] A mask (20) can be prepared by providing ear loop members (13) on both the left and right ends of a cup-shaped mask body (12) prepared using the mask filter substrate of the present invention.

[0059] In the mask (20) equipped with the mask filter substrate according to the present invention, in order to provide a mask (20) with better blood barrier properties, the mask (20) preferably has a fused portion (14) on the main surface exposed to the outermost layer. The mask (20) having the fused portion (14) improves shape stability in the thickness direction. As a result, when blood adheres to the outermost layer side of the mask (20), the mask is prevented from being unintentionally crushed in its thickness direction (the thickness direction of the mask filter substrate), and blood is prevented from penetrating the mask (20).

[0060] The shape and size of the fused portion (14) on the outermost layer of the mask (20) can be adjusted as appropriate, but it is preferable that the fused portion (14) is formed on the main surface exposed to the outermost layer of the mask (20) in the form of a straight line or curve passing through the apex portion (15) on the outermost layer side when a person wears the mask (20). Specifically, it is preferable that the fused portion (14) is provided on the main surface exposed to the outermost layer of the mask (20) so as to draw the longest straight line or curve passing through the ear loop members (13) provided on both the left and right ends of the main surface exposed to the outermost layer and the apex portion (15) on the outermost layer side.

[0061] The method for forming the fused portion (14) can be appropriately selected, but the fused portion (14) in a linear shape can be formed by melting the constituent members of the mask (20) by ultrasonic welding or heat sealing. EXAMPLES

[0062] The present invention will be specifically described below with reference to examples, but the scope of the present invention is not limited thereto.

[0063] (Prepare spunbond nonwoven fabric a) Spunbond nonwoven fabric a (weight: 20 g / m) made of polypropylene 2 , Thickness: 0.17mm, Breathability: 360cm 3 / cm 2 sec., average fiber diameter: 21 μm, constituent fibers: continuous fibers) were prepared.

[0064] (Preparation of hydroentangled nonwoven fabric a) Polypropylene fibers (average fiber diameter: 17.5 μm, fiber length: 51 mm) were opened by a carding machine to form a fiber web. Next, the fiber web was subjected to a hydroentanglement treatment (water pressure: 3 MPa, process conveying speed: 5 m / min) from one main surface side to the other main surface side, and then again to the same conditions, from the other main surface side to one main surface side of the web (water pressure: 3 MPa, process conveying speed: 5 m / min), to entangle the constituent fibers. Thereafter, the hydroentangled fiber web was placed in an oven dryer (heating temperature: 80°C) to remove water contained in the fiber web, resulting in a hydroentangled nonwoven fabric a (basis weight: 50 g / m 2 , Thickness: 0.48mm, Breathability: 210cm 3 / cm 2 sec., average fiber diameter: 17.5 μm, average fiber length: 51 mm, constituent fibers: short fibers) were prepared.

[0065] (Preparation of charged melt-blown nonwoven fabric a) Volume resistivity is 10 16 A commercially available hindered amine light stabilizer (CHIMASSORB 944FDL, BASF Japan Ltd.) was mixed with commercially available polypropylene (Prime Polypro, Prime Polymer Co., Ltd.) with a viscosity of about Ω·cm to prepare a resin for spinning. The resin for spinning prepared in this way was spun into fibers by melt-blowing, and the spun fibers were deposited and collected on a flat collector to prepare a melt-blown nonwoven fabric composed of polypropylene containing the hindered amine light stabilizer. The obtained melt-blown nonwoven fabric was transferred to a bath containing pure water (equivalent to secondary distilled water that has been distilled and ion exchanged) with an electrical conductivity of 3.2 (μS / cm) and a temperature kept in the range of 20±5°C as a polar liquid, and while supporting the pure water, ultrasound with a frequency of 20 kHz was applied. Next, the melt-blown nonwoven fabric to which the ultrasonic waves had been applied was dried by being fed to a conveyor-type dryer with a heating temperature adjusted to 105°C, to obtain an electrically charged melt-blown nonwoven fabric a (basis weight: 45 g / m 2 , Thickness: 0.60mm, Breathability: 32cm 3 / cm 2 sec., main fiber diameter distribution: 1-10 μm, average fiber diameter: 4.0 μm, constituent fibers: continuous fibers) were prepared.

[0066] (Example 1, Comparative Examples 1-2) The spunbonded nonwoven fabric a, the hydroentangled nonwoven fabric a, and the charged meltblown nonwoven fabric a prepared as above were simply stacked in the stacking order (stacking order of fiber layer A-fiber layer B-fiber layer C) shown in Table 1 to prepare a laminate. Each of the laminates prepared in this manner was used as a filter substrate for a mask (each of which had a basis weight of 115 g / m 2 , thickness: 1.25 mm).

[0067] In the tables below, "SB" means spunbonded nonwoven fabric, "HE" means hydroentangled nonwoven fabric, and "MB" means liquid-charged meltblown nonwoven fabric.

[0068] [Table 1]

[0069] (Breathable reinforcement material) 30% polyethylene / polypropylene composite fiber (fineness 20 dtex, fiber length 102 mm), 65% polyethylene / polypropylene composite fiber (fineness 6.6 dtex, fiber length 102 mm), 5% polyethylene-polyethylene vinyl acetate copolymer / polypropylene composite fiber (fineness 3.3 dtex, fiber length 64 mm) were mixed and carded to produce a fiber size of 85 g / m 2 A fiber web of 1000 g was prepared. The fiber web thus prepared was molded and punched into a cup shape protruding in one direction, and then used as a breathable reinforcement material (breathability: 150 cm 3 / cm 2 ·sec., constituent fibers: short fibers).

[0070] (Ear hook component) A mask string (cross section: rectangular shape with width 3 mm and thickness 1.5 mm) made of polyester fiber and polyurethane fiber with a length of 17 cm was prepared. A plastic plate capable of holding the mask string was also prepared. The mask string was held by the plastic plate to form an ear hook member.

[0071] (How to prepare the mask) The mask filter substrate was simply superimposed on the main surface of the breathable reinforcement protruding in one direction, with the fiber layer C of the mask filter substrate facing the main surface.Then, the entire outer circumference of both the mask filter substrate and the breathable reinforcement was fused together and integrated using an ultrasonic welding device to prepare a cup-shaped mask body.The mask filter substrate provided in the prepared mask was formed by laminating the fiber layer A-fiber layer B-fiber layer C in this order from the outermost layer side to the innermost layer side. Next, an ultrasonic welding device was applied to the main surface exposed to the outermost layer of the mask, in such a way that a curve passing through both the left and right ends of the mask body and the apex of the outermost layer in the shortest possible direction was drawn on the main surface exposed to the outermost layer when a person is wearing the mask. Through this process, a linear fused portion was formed in the portion of the outermost layer of the mask body where the ultrasonic welding device was applied. Thereafter, a plastic plate holding a mask string was fixed to both left and right ends of the mask body in the outermost layer of the mask body to prepare a mask.

[0072] The masks equipped with the mask filter substrates prepared in Example 1 and Comparative Examples 1 and 2 as described above were subjected to the following measurements, and the blood barrier properties exhibited by the masks were evaluated.

[0073] (Method for evaluating blood barrier properties) The blood barrier properties of the masks were evaluated using the test pressure of 16.0 kPa (120 mmHg) in accordance with the test method of JIS T 9001 "Performance requirements and test methods for medical and general masks." In conducting the evaluation test, the artificial blood was applied to the apex of the outermost layer on the exposed main surface of the mask (the main surface on which the fiber layer A is exposed).

[0074] After the artificial blood was applied to the apex of the outermost layer of the mask in this manner, the mask filter substrate was quickly removed from the mask. The main surface of the innermost layer side of the removed mask filter substrate (the main surface of the innermost layer side of the fiber layer C) when the mask was constructed was visually observed to confirm whether the artificial blood had permeated the mask filter substrate. In the same manner, a total of 32 masks were checked to see whether the artificial blood had permeated the mask filter substrate. Note that the fewer the number of masks in which the artificial blood had permeated the mask filter substrate, the more likely it was that the mask filter substrate would be capable of realizing a mask with excellent blood barrier properties.

[0075] The results of the evaluation method for the blood barrier properties of the masks are summarized in Table 2. Specifically, when the permeation of artificial blood into the mask filter substrate (the seepage of artificial blood to the main surface of the innermost layer side of fiber layer C) was not observed in any of the measurement results for a total of 32 masks, the blood barrier property column in Table 2 was marked with "○." In addition, when artificial blood permeation into the mask filter substrate was observed in 1 to 3 masks out of the measurement results for a total of 32 masks, the blood barrier property column in Table 2 was marked with "△". If artificial blood was found to penetrate the mask filter substrate in four or more of the 32 masks measured, an "X" was entered in the blood barrier property column in Table 2.

[0076] [Table 2]

[0077] From the above results, it was found that by using a mask filter substrate satisfying the configuration of the present invention, a mask with excellent blood barrier properties can be provided.

[0078] Example 2 As the fiber layer B, a hydroentangled nonwoven fabric b prepared as follows was used. Otherwise, a mask filter substrate (basis weight: 115 g / m2) was prepared in the same manner as in Example 1. 2 , thickness: 1.17 mm was prepared. (Preparation of hydroentangled nonwoven fabric b) Polyethylene terephthalate fibers to which an alkyl phosphate-based hydrophilic oil agent had been applied were opened by a carding machine to form a fiber web. Next, the fiber web was subjected to a hydroentanglement treatment (water pressure: 3 MPa, process conveying speed: 5 m / min) from one main surface side to the other main surface side, and then again to the same conditions, from the other main surface side to one main surface side of the web (water pressure: 3 MPa, process conveying speed: 5 m / min), to entangle the constituent fibers. Thereafter, the hydroentangled fiber web was placed in an oven dryer (heating temperature: 80°C) to remove water contained in the fiber web, resulting in hydroentangled nonwoven fabric b (basis weight: 50 g / m 2 , Thickness: 0.40mm, Air permeability: 180cm 3 / cm 2sec., average fiber diameter: 12 μm, average fiber length: 51 mm, constituent fibers: short fibers, containing alkyl phosphate-based hydrophilic oil agent) was prepared.

[0079] Comparative Example 3 A spunbond nonwoven fabric b prepared as follows was used as the fiber layer A, and an electrically charged meltblown nonwoven fabric b prepared as follows was used as the fiber layer C. In the same manner as in Example 1, a mask filter substrate (basis weight: 87 g / m) was prepared. 2 , thickness: 0.91 mm) was prepared. (Prepare spunbond nonwoven fabric b) Spunbond nonwoven fabric b (weight: 17 g / m) made of polypropylene fibers 2 , Thickness: 0.15mm, Breathability: 100cm 3 / cm 2 sec., constituent fibers: continuous fibers) were prepared. (Preparation of charged melt-blown nonwoven fabric b) Volume resistivity is 10 16 A commercially available hindered amine light stabilizer (CHIMASSORB 944FDL, BASF Japan Ltd.) was mixed with commercially available polypropylene (Prime Polypro, Prime Polymer Co., Ltd.) with a viscosity of about Ω·cm to prepare a resin for spinning. The resin for spinning prepared in this way was spun into fibers by melt-blowing, and the spun fibers were deposited and collected on a flat collector to prepare a melt-blown nonwoven fabric composed of polypropylene containing the hindered amine light stabilizer. The obtained melt-blown nonwoven fabric was transferred to a bath containing pure water (equivalent to secondary distilled water that has been distilled and ion exchanged) with an electrical conductivity of 3.2 (μS / cm) and a temperature kept in the range of 20±5°C as a polar liquid, and while supporting the pure water, ultrasound with a frequency of 20 kHz was applied. Next, the melt-blown nonwoven fabric to which the ultrasonic waves had been applied was dried by being fed to a conveyor-type dryer with a heating temperature adjusted to 105°C, to obtain an electrically charged melt-blown nonwoven fabric b (basis weight: 20 g / m 2 , Thickness: 0.28mm, Breathability: 45cm3 / cm 2 sec., main fiber diameter distribution: 1-8 μm, average fiber diameter: 3.5 μm, constituent fibers: continuous fibers) were prepared.

[0080] Comparative Example 4 A spunbond nonwoven fabric c prepared as follows was used as the fiber layer A, and a hydroentangled nonwoven fabric c prepared as follows was used as the fiber layer B. Other than that, a mask filter substrate (basis weight: 120 g / m2) was prepared in the same manner as in Example 1. 2 , thickness: 1.54 mm was prepared. (Prepare spunbond nonwoven fabric c) Spunbond nonwoven fabric c (weight: 25 g / m) made of polypropylene fibers 2 , Thickness: 0.29mm, Breathability: 290cm 3 / cm 2 sec., average fiber diameter: 21 μm, constituent fibers: continuous fibers) were prepared. (Preparation of hydroentangled nonwoven fabric c) A fiber web was formed by opening 36% by mass of core-sheath type composite fibers (core: polypropylene, sheath: polyethylene, average fiber diameter: 21 μm, fiber length: 51 mm) and 64% by mass of polypropylene fibers (average fiber diameter: 17 μm, fiber length: 51 mm) using a carding machine. Next, the fiber web was subjected to a hydroentanglement treatment (water pressure: 3 MPa, process conveying speed: 5 m / min) from one main surface side to the other main surface side, and then again to the same conditions, from the other main surface side to one main surface side of the web (water pressure: 3 MPa, process conveying speed: 5 m / min), to entangle the constituent fibers. Thereafter, the hydroentangled fiber web was subjected to an oven dryer (heating temperature: 80°C) to remove water contained in the fiber web, and a hydroentangled nonwoven fabric c (basis weight: 50 g / m 2 , Thickness: 0.65mm, Breathability: 305cm 3 / cm 2 sec., average fiber diameter: 18 μm, average fiber length: 51 mm, constituent fibers: short fibers) were prepared.

[0081] Using each mask filter substrate prepared as described above, masks were prepared in the same manner as in Example 1. Then, the masks equipped with the mask filter substrates prepared in Example 2 and Comparative Examples 3 and 4 were subjected to the above-mentioned (method for evaluating blood barrier properties). Thereby, the blood barrier properties exhibited by the masks were evaluated.

[0082] The configuration of the mask prepared using the prepared mask filter substrate and the evaluation of the blood barrier properties exhibited by the mask are summarized in Table 3. The evaluation results of Example 1 are also shown for reference.

[0083] [Table 3]

[0084] From the above results, it was found that a mask with excellent blood barrier properties can be provided by using a mask filter substrate that satisfies the configuration of the present invention.

[0085] The fiber layers A to C used in Comparative Examples 3 and 4 were all nonwoven fabric-derived fiber layers prepared using the same manufacturing method as the fiber layers A to C used in Examples 1 and 2, and differed mainly only in air permeability. Nevertheless, the blood barrier properties of the masks equipped with the mask filter substrates prepared in Comparative Examples 3 and 4 were inferior to the blood barrier properties of the masks equipped with the mask filter substrates prepared in Examples 1 and 2. Therefore, the effect of the mask filter substrate of the present invention, that is, the ability to provide a mask with excellent blood barrier properties, is not exhibited by differences in the manufacturing methods of the fiber layers A to C, but by the configuration in which the fiber layers are stacked in the order of fiber layer A-fiber layer B-fiber layer C with decreasing air permeability (in particular, the fiber layers are stacked in the order of fiber layer A-fiber layer B-fiber layer C with decreasing air permeability from the outermost layer side to the innermost layer side when constructing the mask).

[0086] It was also found that the mask filter substrate prepared in Example 1 provided a mask with better blood barrier properties than a mask equipped with the mask filter substrate prepared in Example 2. This was believed to be because the fiber layer B constituting the mask filter substrate of Example 1 had a more hydrophobic structure than the fiber layer B constituting the mask filter substrate of Example 2.

[0087] Example 3 40% by mass of polypropylene fibers (fiber diameter: 18 μm, fiber length: 51 mm) and 60% by mass of acrylic resin fibers (fiber diameter: 15 μm, fiber length: 51 mm) were mixed and opened by a carding machine to form a fiber web (average fiber diameter: 16 μm, average fiber length: 51 mm). Then, the fiber web was simply superimposed on the spunbond nonwoven fabric c to prepare a laminated fiber web. Next, cross barb needles having a needle count of 40 were inserted from the main surface of the prepared laminated fiber web on the spunbond nonwoven fabric c side to the other main surface at a needle depth of 16 mm and a needle density of 34 needles / cm. 2 The needle punching process was carried out under the following conditions. The needle punching process caused the constituent polypropylene fibers and acrylic resin fibers to be rubbed together, generating a triboelectrically charged nonwoven fabric (basis weight: 120 g / m 2 , Thickness: 1.60mm, Breathability: 130cm 3 / cm 2 -sec.) has been adjusted. The tribo-electrically charged nonwoven fabric prepared as described above was then simply laid over the main surface of the fiber layer C side of the mask filter substrate prepared in Example 1, as a backup filter. At this time, the two were laid over each other so that the main surface of the fiber layer C side faced the main surface of the tribo-electrically charged nonwoven fabric that had been subjected to needle punching. In this way, a laminate of the mask filter substrate and the backup filter (basis weight: 235 g / m 2 , thickness: 2.85 mm) was prepared.

[0088] Using the laminate prepared as described above, the mask filter substrate was simply superimposed on the main surface of the breathable reinforcing material protruding in one direction, with the tribo-electrically charged nonwoven fabric of the laminate facing said main surface. After that, an ultrasonic welding device was used to fuse and integrate the entire outer peripheries of both the mask filter substrate and the breathable reinforcing material, thereby preparing a cup-shaped mask main body.

[0089] Using the mask body prepared as described above, a mask was prepared in the same manner as in Example 1. Then, the mask equipped with the prepared mask filter substrate was subjected to the above-mentioned (method for evaluating blood barrier properties). Thereby, the blood barrier properties exhibited by the mask were evaluated.

[0090] The configuration of the mask prepared using the prepared mask filter substrate and the evaluation of the blood barrier properties exhibited by the mask are summarized in Table 4. The evaluation results of Example 1 are also shown for reference.

[0091] [Table 4]

[0092] From the above results, it was found that a mask with excellent blood barrier properties can be provided by using a mask filter substrate that satisfies the configuration of the present invention. [Industrial Applicability]

[0093] The mask filter substrate of the present invention can provide a mask with excellent blood barrier properties. [Explanation of symbols]

[0094] 10: Mask filter substrate A: Fiber layer A B: Fiber layer B C: Fiber layer C O: Outermost layer side of the mask filter substrate when constructing the mask I: The innermost layer of the mask filter substrate when constructing the mask 11: Cup-shaped breathable reinforcement material protruding in one direction 12: Cup-shaped mask body 13: Ear hook component 14: Fusion part 15: Vertex part 20: Mask

Claims

1. A mask filter substrate comprising a fiber layer A, a fiber layer B, and a fiber layer C, The fiber layer A, the fiber layer B, and the fiber layer C are laminated in this order, The air permeability decreases in the order of the fiber layer A, the fiber layer B, and the fiber layer C. Filter substrate for masks.

2. A mask comprising the mask filter substrate according to claim 1.

3. The mask of claim 2 having a fused portion on the outermost layer.

Citation Information

Patent Citations

  • Shaped mask and method for manufacturing the same

    JP2010094503A