Manufacturing control system of optical film, manufacturing control program of optical film, and manufacturing method of optical film

The optical film manufacturing management system addresses the issue of unstable quality in diverse optical film production by determining the processing order based on raw film characteristics, specifically the orientation of resin molecules, to enhance consistency and reduce losses.

JP2024154106APending Publication Date: 2024-10-30KONICA MINOLTA INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023067742
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2024-10-30

AI Technical Summary

Technical Problem

Existing methods for producing optical films in small quantities and varied types fail to account for the order of processing raw materials, leading to significant losses due to variations in processing conditions and equipment fluctuations, resulting in unstable quality.

Method used

An optical film manufacturing management system that determines the order of processing raw films based on the characteristics of their inner and outer sides, including the orientation of resin molecules, to adjust processing conditions and minimize differences, thereby reducing losses.

Benefits of technology

The system effectively reduces manufacturing losses by ensuring consistent quality and efficiency in producing optical films by aligning processing conditions with the characteristics of the raw films, stabilizing quality and minimizing adjustments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154106000001_ABST
    Figure 2024154106000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing control system of an optical film with reduced loss on manufacturing, a manufacturing control program of the optical film, and a manufacturing method of the optical film.SOLUTION: A manufacturing control system of an optical film of the present invention is a manufacturing control system of an optical film for determining, from a plurality of wound raw fabric films, the raw fabric film to be input in the next step, and determining a manufacturing order of an optical film, and is characterized by including: an information acquisition part relating to properties of the respective raw fabric films; an information extraction part relating to the properties of at least winding inner side and winding outer side of the respective raw fabric films; an information processing unit relating to the properties of at least the winding inner side and the winding outer side having been extracted; and an order determination unit of input of the raw fabric film in the next step based on the information relating to the properties of at least the winding inner side and the winding outer side having been processed.SELECTED DRAWING: Figure 17
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film production management system, an optical film production management program, and an optical film manufacturing method, and more particularly to providing an optical film production management system and the like that reduce losses during manufacturing. [Background technology]

[0002] In recent years, the variety of optical devices such as display devices has been diversified due to the expansion of their applications. Accordingly, the optical films provided in the optical devices have also become more diverse, and there is a demand for small-lot, high-mix production. One method for producing small-lot, high-mix optical films is to produce a desired optical film by preparing a raw film and appropriately processing the raw film.

[0003] However, when processing the raw film, even a slight change in the set values ​​of the processing conditions can cause a large difference in the properties of the optical film. If the properties of the optical film exceed the allowable range for the product, the product cannot be manufactured and a loss will occur. Therefore, the processing conditions must be precisely controlled. Even if the raw film is produced under the same conditions, the properties of the raw film may become uneven due to equipment troubles or environmental changes during production. In this case, in order to make the properties of the optical film obtained in the end uniform and within the allowable range, the processing conditions must be precisely controlled according to the properties of the raw film.

[0004] In conventional methods, even if raw materials are managed within an adjustable range and the efficiency of the processing process is improved, the load on the processing process caused by the processing order of the raw materials is not taken into consideration. In particular, when stretching is performed for film processing, the film may be stretched to several hundred meters. 3 Several thousand meters from 3It is necessary to control the temperature inside the stretching chamber, which can reach up to 1000 mm. Even if a local heating device is used, hunting occurs until the temperature stabilizes. In addition, feedback of control is not possible in time or is frequent. This leads to more fluctuations and unstable quality.

[0005] Since there are subtle differences in the thickness of the film, it is necessary to locally heat the relevant area. Even in this case, it was found that if the conditions were changed suddenly, a large amount of loss would occur until the product quality could be met due to the influence of the ambient temperature and the feedback of the temperature management control of the heating equipment.

[0006] To coat a polymerizable polymer on a substrate film and polymerize the polymerizable polymer while keeping it oriented, it is necessary to fine-tune the coating conditions depending on the orientation of the substrate film that serves as the base for the coating. Therefore, it is necessary to feed the substrate film within the adjustable range. Even when a liquid crystal layer is provided by applying an alignment layer onto a substrate film, a pattern alignment layer is formed to produce the alignment layer, so it is necessary to predict and correct the influence of the substrate film in advance.

[0007] For example, as shown in JP 2017-111267 A and WO 2020 / 110817 A, control of the contact angle in the substrate film is also important for controlling the orientation during the formation of the orientation layer. The contact angle is greatly affected by the orientation of the resin contained in the substrate film and unevenness in the surface shape of the substrate film.

[0008] The following techniques have been disclosed as techniques for improving film production efficiency. Patent Document 1 discloses a technique for controlling the order of processing steps in the production of a cellulose ester film, based on the properties such as the degree of substitution and viscosity of the raw cellulose ester.

[0009] In Patent Document 2, in a method of manufacturing products by processing materials, measures are classified according to the similarity of the processing path. Then, a technology is disclosed regarding a production management system that collectively produces products with high similarity.

[0010] However, these techniques are not applicable to the above-mentioned method for producing a wide variety of optical films in small quantities. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2009-172772 A [Patent Document 2] JP 2020-166548 A Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide an optical film production management system, an optical film production management program, and an optical film production method that reduce losses during production. [Means for solving the problem]

[0013] In order to solve the above-mentioned problems, the inventors have investigated the causes of the above-mentioned problems and have discovered that in an optical film production management system that determines the production order of optical films, losses during production can be reduced by having an information acquisition unit regarding the characteristics of each of the original films, an information extraction unit regarding the characteristics of the inside and outside of the roll of each of the original films, an information processing unit regarding the extracted characteristics of the inside and outside of the roll, and an order determination unit for determining the order of input of the original films in the next process based on the processed information regarding the characteristics of the inside and outside of the roll, and have arrived at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.

[0014] 1. A manufacturing management system for optical films, which determines a roll of film to be input in a next process from a plurality of rolls of film, and determines a manufacturing sequence of optical films, An information acquisition unit for acquiring information on characteristics of each of the raw films; An information extraction unit for extracting information on the characteristics of at least the inside or outside of the roll of each of the raw films; an information processing unit for processing the extracted characteristics of at least the inside or outside of the roll; and a sequence determination unit for determining the order of input of the raw film in the next process based on information regarding the characteristics of at least the processed inside or outside of the roll. A manufacturing management system for optical films.

[0015] 2. The information regarding the characteristics is information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction. 2. The production management system for an optical film according to claim 1,

[0016] 3. The next step includes a step of stretching the raw film. 2. The production management system for an optical film according to claim 1,

[0017] 4. The information processing unit has a function of sorting the raw film based on whether or not a difference in information regarding the orientation of the resin molecules at least on the inside or outside of the roll exceeds a threshold value. 3. The production management system for an optical film according to claim 2.

[0018] 5. The information processing unit has a function of calculating a similarity from information regarding the orientation of the resin molecules at least on the inside or outside of the roll. 3. The production management system for an optical film according to claim 2.

[0019] 6. The sequence determination unit has a function of adjusting the sequence of feeding the original film in the next process based on the standard deviation of the thickness at the position in the width direction of the original film. 3. The production management system for an optical film according to claim 1 or 2,

[0020] 7. The sequence determination unit adjusts the thickness of the raw film roll to satisfy the following formula (1), where σ1 is the standard deviation of the thickness of the raw film roll immediately before being loaded at the position in the width direction on the inside and σ2 is the standard deviation of the thickness of the raw film roll to be loaded at the position in the width direction on the outside. 7. The optical film production management system according to claim 6, Equation (1) |σ1-σ2| / σ1≦0.05

[0021] 8. The production management system for the optical film has a function of judging whether or not the stretching conditions or the stretching ratio need to be adjusted and the time required for the next process based on the acquired information on the orientation of the resin molecules, the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll, or the processed information on the orientation of the resin molecules at least on the inside or outside of the roll. 3. The production management system for an optical film according to claim 2.

[0022] 9. The manufacturing management system for the optical film has a function of determining the stretching speed, the stretching temperature, or the stretching ratio. 9. The optical film production management system according to item 8,

[0023] 10. A manufacturing management program for optical films, which determines a roll of film to be input in a next process from a plurality of rolls of film, and determines a manufacturing sequence of optical films, Obtaining information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction; Extracting information regarding the orientation of the resin molecules at least on the inside or outside of the roll of each of the raw films; Processing based on the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll; The order of inputting the raw film in the next process is determined based on the information on the orientation of the resin molecules at least on the inside or outside of the roll. A manufacturing management program for an optical film.

[0024] 11. Calculating the similarity from the extracted information regarding the orientation of the resin molecules at least on the inside or outside of the roll. 11. The optical film manufacturing management program according to claim 10.

[0025] 12. A method for producing an optical film, comprising determining a raw film to be fed to a next process from a plurality of wound raw films, and determining a production order of the optical films, Obtaining information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction; Extracting information regarding the orientation of the resin molecules at least on the inside or outside of the roll of each of the raw films; performing processing based on the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll; and determining the order of inputting the raw film in the next process based on information regarding the orientation of the resin molecules at least on the inside or outside of the roll that has been processed. A method for producing an optical film comprising the steps of:

[0026] 13. The next step includes a step of stretching the raw film. 13. The method for producing an optical film according to claim 12.

[0027] 14. The processing step includes a step of sorting the raw film based on whether or not a difference in information regarding the orientation of the resin molecules at least on the inside or outside of the roll exceeds a threshold value. 13. The method for producing an optical film according to claim 12.

[0028] 15. The processing step includes a step of calculating a similarity from information regarding the orientation of the resin molecules at least on the inside or outside of the roll. 13. The method for producing an optical film according to claim 12.

[0029] 16. The step of determining the order includes a step of adjusting the order in which the original film is fed in the next step based on a standard deviation of the thickness at a position in the width direction of the original film. 13. The method for producing an optical film according to claim 12.

[0030] 17. The step of determining the order includes a step of adjusting the thickness of the raw film rolls so as to satisfy the following formula (1), where σ1 is the standard deviation of the thickness of the raw film roll before being loaded at the position in the width direction on the inside of the roll, and σ2 is the standard deviation of the thickness of the raw film roll to be loaded at the position in the width direction on the outside of the roll. 17. The method for producing an optical film according to item 16, Equation (1) |σ1-σ2| / σ1≦0.05

[0031] 18. The method for producing the optical film includes a step of determining whether or not the stretching conditions or the stretching ratio should be adjusted and the time required for the next step based on the acquired information on the orientation of the resin molecules, the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll, or the processed information on the orientation of the resin molecules at least on the inside or outside of the roll. 13. The method for producing an optical film according to claim 12.

[0032] 19. The method for producing the optical film includes a step of determining a stretching speed, a stretching temperature, or the stretching ratio. 20. The method for producing an optical film according to item 18, Effect of the Invention

[0033] According to the above-mentioned means of the present invention, it is possible to provide an optical film production management system, an optical film production management program, and an optical film production method that reduce losses during production.

[0034] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.

[0035] In the method of manufacturing a desired optical film by subjecting a raw film to suitable processing, it is preferable to finely control the processing conditions according to the characteristics of the raw film. If the adjustment range of the processing conditions is small, it can be handled in a relatively short time. However, if the adjustment range is large, it cannot be handled in a short time, and in addition to the processing time of the raw film, it takes time to adjust the processing conditions. Furthermore, if the processing is performed in an insufficiently adjusted state, the characteristics of the optical film will exceed the allowable range for the product, and it will not be possible to commercialize it, resulting in a loss. Therefore, it is preferable to make the adjustment range of the processing conditions as small as possible.

[0036] In the case of continuous raw film, even if the properties of the raw film become uneven due to equipment troubles or environmental changes during production, the unevenness of the properties changes continuously. Therefore, the adjustment of processing conditions is also continuous, that is, the range of adjustment is small, and it can be dealt with in a relatively short time. However, in the manufacturing method in which the raw film is produced and then stored, and then processed as needed to make the final product, it is necessary to cut the raw film into an appropriate amount and store it.

[0037] Specifically, after the raw film is produced, it is wound up in a roll and stored. FIG. 14 is an explanatory diagram of a series of steps for processing a raw film wound into a roll. A continuous raw film is cut at points A, B, C, and D, and wound into a roll in the direction of the arrow. The raw film is wound into rolls 1, 2, and 3 in that order.

[0038] If the end of roll 1 formed by cutting at point A is A1 and the end of roll 1 formed by cutting at point B is B1, end A1 is located on the inside of the roll and end B1 is located on the outside of the roll. Similarly, in roll 2, end B2 is located on the inside and end C2 is located on the outside. In roll 3, end C3 is located on the inside and end D3 is located on the outside.

[0039] Next, the original film is pulled out from the rolls in the order of rolls 1, 2, and 3, and processed. At this time, the original film is processed from the outside to the inside of the roll, that is, from end B1 to end A1. Similarly, in roll 2, the film is processed from end C2 to end B2, and in roll 3, the film is processed from end D3 to end C3.

[0040] When the rolls 1, 2, and 3 are processed in succession, the end C2 is processed continuously with the end A1, and the end D3 is processed continuously with the end B2. However, the ends A1 and C2 are cut at points A and C, respectively, and are discontinuous portions of the original film. Therefore, differences are likely to occur in the properties of the original film at the ends A1 and C2, and the range of adjustment of the processing conditions to accommodate these differences becomes large, which is thought to reduce manufacturing efficiency.

[0041] In the present invention, information on the characteristics of the inner and outer ends of the raw film to be wound is accumulated. Then, the order of manufacturing (processing) the raw film rolls is determined based on the accumulated information so that there is no significant difference in the characteristics of the two ends that are processed consecutively. In other words, the raw film roll to be processed Nth is determined to have an outer end with characteristics relatively close to those of the inner end of the raw film roll to be processed N-1th. This makes it possible to reduce the adjustment range of the processing conditions, making it easier to process under sufficient adjustment, and is therefore believed to reduce losses during production. [Brief description of the drawings]

[0042] [Figure 1] Relationship between convex parts and film thickness profile in the width direction [Diagram 2] Flowchart showing the process of making raw film [Diagram 3] Schematic diagram of the device for producing raw film by the solution casting method [Figure 4] Schematic diagram showing arranging and adjusting the convex portion so as to move continuously in the longitudinal direction. (a) Schematic diagram showing continuously arranging and adjusting the convex portion in a straight line. (b) Schematic diagram showing continuously arranging and adjusting the convex portion in a straight line. (c) Schematic diagram showing arranging and adjusting along a curve. [Diagram 5] A plot of the position of the convex part and the relationship with the approximate line [Figure 6] Diagram showing the arrangement of infrared heaters: (a) Infrared heaters arranged in one row along the length of the film; (b) Infrared heaters arranged in two rows along the length of the film; (c) Infrared heaters arranged in five rows along the length of the film. [Figure 7] (a) A diagram showing the average inclination of the straight line formed by each heat source with the longitudinal direction. (b) A diagram showing the average inclination of the straight line formed by each heat source with the longitudinal direction. [Figure 8] Cross-sectional view of a tenter stretching apparatus viewed from above in a plane perpendicular to the film plane. [Figure 9] Schematic diagram of the nozzle and heater installation area when viewed from the front of the three zones in the tenter stretching device. [Figure 10] Side view of the three zones in a tenter stretching unit [Figure 11] Cross-sectional view of a tenter stretching apparatus viewed from above in a plane perpendicular to the film plane. [Figure 12] A schematic diagram showing the process of winding a raw film and the cross section of the raw film roll after winding. [Figure 13] Schematic diagram of the device for producing raw film by the melt casting method [Figure 14] An explanatory diagram of the series of steps involved in processing rolled raw film [Figure 15] A diagram showing the relationship between the position in the longitudinal direction and the degree of resin orientation for the original film before it is wound and cut. [Figure 16] A diagram showing the relationship between processing time and the degree of resin orientation when processing is performed on rolls of raw film in the order in which they were produced. [Figure 17] Flow diagram of the production management system for the optical film of the present invention. [Figure 18] FIG. 1 is an explanatory diagram of an example of measurement points of phase differences Ro and Rth. [Figure 19] An explanatory diagram of an example of thickness measurement points [Figure 20] Connection area diagram DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] The optical film manufacturing management system of the present invention is an optical film manufacturing management system that determines which original film to be input in the next process from a plurality of rolled original films and determines the manufacturing order of the optical films, and is characterized by having an information acquisition unit regarding the characteristics of each of the original films, an information extraction unit regarding the characteristics of at least the inside or outside of the roll of each of the original films, an information processing unit regarding the extracted characteristics of at least the inside or outside of the roll, and an order determination unit for the input of the original films in the next process based on the processed information regarding the characteristics of at least the inside or outside of the roll. This feature is a technical feature common to or corresponding to the following embodiments.

[0044] In an embodiment of the present invention, from the viewpoint of the effect when processing the raw film, it is preferable that the information regarding the characteristics is information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction.

[0045] In an embodiment of the present invention, from the viewpoint of continuously processing the raw film in the same processing step, it is preferable that the next step includes a step of stretching the input raw film.

[0046] In an embodiment of the present invention, from the viewpoint of reducing losses during manufacturing, it is preferable that the information processing unit has a function of sorting the raw film based on whether or not the difference in information regarding the orientation of the resin molecules at least on the inside or outside of the roll exceeds a threshold value.

[0047] In an embodiment of the present invention, from the viewpoint of reducing losses during production due to adjustment of conditions accompanying switching of raw webs in the stretching process, it is preferred that the information processing unit has a function of calculating the similarity from information regarding the orientation of the resin molecules at least on the inside side or the outside side of the roll.

[0048] In an embodiment of the present invention, from the viewpoint of reducing losses during production when making local adjustments, it is preferable that the order determination unit has a function of adjusting the order in which the raw film is fed in the next process based on the standard deviation of the thickness at a position in the width direction of the raw film.

[0049] In an embodiment of the present invention, from the viewpoint of reducing losses during production, it is preferable that the order determination unit adjusts the thickness so as to satisfy the above formula (1), where σ1 is the standard deviation of the thickness at the width direction position on the inside of the raw film roll immediately before being fed, and σ2 is the standard deviation of the thickness at the width direction position on the outside of the raw film roll to be fed.

[0050] In an embodiment of the present invention, from the viewpoint of reducing losses during production, it is preferable that the production management system for the optical film has a function of determining whether or not the stretching conditions or stretching ratio can be adjusted, and the required time for the next process, based on the acquired information on the orientation of the resin molecules, the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll, or the processed information on the orientation of the resin molecules at least on the inside or outside of the roll.

[0051] In an embodiment of the present invention, from the viewpoint of reducing losses during production, the production management system for the optical film preferably has a function of determining a stretching speed, a stretching temperature, or the stretching ratio.

[0052] The optical film manufacturing management program of the present invention is an optical film manufacturing management program that determines the original film to be input in the next process from a plurality of wound original films and determines the manufacturing order of optical films, and is characterized in that it acquires information regarding the orientation of resin molecules contained in each of the original films at least in the longitudinal direction, extracts information regarding the orientation of the resin molecules at least on the inside or outside of the roll for each of the original films, processes based on the extracted information regarding the orientation of the resin molecules at least on the inside or outside of the roll, and determines the order for input of the original films in the next process based on the processed information regarding the orientation of the resin molecules at least on the inside or outside of the roll.

[0053] As an embodiment of the present invention, from the viewpoint of reducing losses during production, it is preferable to calculate the similarity from extracted information on the orientation of the resin molecules at least on the inside or outside of the roll.

[0054] The optical film manufacturing method of the present invention is a method for manufacturing an optical film in which a raw film to be input in a next process is determined from a plurality of wound raw films and the order of manufacturing the optical films is determined, and is characterized by having the following steps: a step of acquiring information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction; a step of extracting information regarding the orientation of the resin molecules at least on the inside or outside of the roll of each of the raw films; a step of processing based on the extracted information regarding the orientation of the resin molecules at least on the inside or outside of the roll; and a step of determining the order of input of the raw films in the next process based on the processed information regarding the orientation of the resin molecules at least on the inside or outside of the roll.

[0055] In an embodiment of the present invention, from the viewpoint of continuously processing the raw film in the same processing step, it is preferable that the next step includes a step of stretching the input raw film.

[0056] In an embodiment of the present invention, from the viewpoint of reducing losses during production, it is preferable that the processing step includes a step of sorting the raw film based on whether or not a difference in information regarding the orientation of the resin molecules at least on the inside or outside of the roll exceeds a threshold value.

[0057] In an embodiment of the present invention, from the viewpoint of reducing losses during production due to adjustment of conditions accompanying switching of raw fabric in the stretching step, it is preferred that the processing step includes a step of calculating a similarity from information regarding the orientation of the resin molecules at least on the inside side or the outside side of the roll.

[0058] In an embodiment of the present invention, from the viewpoint of reducing losses during production when making local adjustments, it is preferable that the process of determining the order includes a process of adjusting the order in which the raw film is inserted in the next process based on the standard deviation of the thickness at a position in the width direction of the raw film.

[0059] In an embodiment of the present invention, from the viewpoint of reducing losses during production, it is preferable that the step of determining the order includes a step of adjusting the thickness so as to satisfy the above formula (1), where σ1 is the standard deviation of the thickness at the width direction position on the inside of the raw film web just before being inserted, and σ2 is the standard deviation of the thickness at the width direction position on the outside of the raw film web to be inserted.

[0060] As an embodiment of the present invention, from the viewpoint of reducing losses during production, it is preferable that the manufacturing method of the optical film includes a step of determining whether or not the stretching conditions or stretching ratio can be adjusted and the required time for the next step based on the acquired information on the orientation of the resin molecules, the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll, or the processed information on the orientation of the resin molecules at least on the inside or outside of the roll.

[0061] In an embodiment of the present invention, from the viewpoint of reducing loss during production, the method for producing the optical film preferably includes a step of determining a stretching speed, a stretching temperature, or the stretching ratio.

[0062] The present invention, its components, and modes and aspects for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0063] 1. Overview of the optical film manufacturing management system The optical film manufacturing management system of the present invention is an optical film manufacturing management system that determines which original film to be input in the next process from a plurality of rolled original films and determines the manufacturing order of the optical films, and is characterized by having an information acquisition unit regarding the characteristics of each of the original films, an information extraction unit regarding the characteristics of at least the inside or outside of the roll of each of the original films, an information processing unit regarding the extracted characteristics of at least the inside or outside of the roll, and an order determination unit for the input of the original films in the next process based on the processed information regarding the characteristics of at least the inside or outside of the roll.

[0064] Hereinafter, the "optical film manufacturing management system" may be simply referred to as the "system."

[0065] The "optical film manufacturing management system" of the present invention refers to a collection of devices or apparatuses having predetermined functions that are used as necessary means elements in each process of managing the manufacturing of optical films. These as a whole perform the function of managing the manufacturing of optical films. Each means element may be individually arranged in a different location away from each other. Also, they may be gathered together in a certain space as one device and arranged as a system device.

[0066] The system of the present invention may include a means for recording or storing various information as electronic data, and a means for wirelessly transmitting the electronic data. For example, it is preferable that the system has a wireless interface for transmitting and receiving data to and from the information processing means via wireless communication such as Bluetooth (registered trademark) or Wi-Fi (registered trademark).

[0067] In the present invention, the term "raw film" refers to a film before being processed in the next step, and the term "optical film" refers to a film obtained by processing the raw film, which has an optical function, and which is used as a member of an optical device.

[0068] In the present invention, the multiple rolls of raw film are processed in the next step to produce an optical film. Here, information on the characteristics of the inner and outer ends of the raw film being wound is collected. Then, based on the collected information, the order of manufacturing (processing) the rolls of raw film is determined. This makes it possible to reduce the range of adjustment of processing conditions and makes it easier to process under sufficient adjustments, thereby reducing losses during manufacturing.

[0069] Hereinafter, a case where "similarity" is used as an index representing the similarity of the characteristics of the original film will be described. However, the present invention is not limited to this, and the similarity of the characteristics of the original film may be represented by other indices. Other indices can also be treated in the same way as similarity.

[0070] In the present invention, the term "similarity" refers to the degree of difference, i.e., the degree of approximation, between statistical analysis values ​​(average values, standard deviation values, etc.) based on measured values ​​of characteristic values ​​(e.g., retardation value, refractive index, light transmittance, surface roughness, etc.) possessed by the films being compared.

[0071] Specifically, for example, the retardation values ​​are measured at multiple locations (n ​​locations) selected randomly or at regular intervals at least in the longitudinal or transverse direction of the original film to be compared. Next, the average value of the retardation values ​​for each original film and the degree of variation from the average value, i.e., the standard deviation value, are calculated. Then, the degree of difference (approximation) between the average value of the retardation values ​​for each original film thus obtained and the degree of difference (approximation) between the standard deviation values ​​are evaluated. Then, assuming that the N-1th original film and the Nth input candidate film are processed continuously, the similarity is evaluated for the connection part of the original film.

[0072] In the present invention, if the difference in the average values ​​between each raw film coincides within a range of -5% to +5% and the standard deviation is 0.5 or less, it is determined that the similarity is at a practically acceptable level. It is desirable that raw films with differences outside this range are excluded from the candidates without undergoing a similarity determination. It is also preferable to calculate the similarity for each original film and arrange the original films in ascending order of similarity value. The "similarity" will be described in detail later.

[0073] As described above, conventional techniques for improving film production efficiency have been achieved by controlling raw materials within an adjustable range and by improving the efficiency of processing steps. However, when processing raw film to produce a desired optical film, the burden on quality due to the processing order of the raw film has not been fully considered.

[0074] Fig. 15 is a diagram showing the relationship between the position in the longitudinal direction and the degree of resin orientation for an original film before it is wound and cut. The horizontal axis of the graph in Fig. 15 represents the position in the longitudinal direction. It is assumed that the original film is wound in the direction of the arrow on the horizontal axis and cut at the dotted line. The vertical axis of the graph in Fig. 15 represents the degree of resin orientation.

[0075] For example, in the case of roll No. 1 of the raw film, the end with a relatively low degree of resin orientation is the inside of the roll, and the end with a relatively high degree of resin orientation is the outside of the roll. Similarly, in the case of rolls No. 2 to 9, the end with a relatively low degree of resin orientation is the inside of the roll, and the end with a relatively high degree of resin orientation is the outside of the roll. Here, for example, it can be seen that the resin orientation degree on the outside of the roll No. 1 and the resin orientation degree on the inside of the roll No. 2 are very close values. In this way, nine rolls are produced by cutting the continuous raw film.

[0076] Fig. 16 is a graph showing the relationship between processing time and the degree of orientation of the resin when processing is performed in the order in which the rolls of raw film are produced. The horizontal axis of the graph in Fig. 16 represents time (processing time), and the vertical axis represents the degree of orientation of the resin.

[0077] For example, in roll No. 1, processing is performed from the outside to the inside of the roll. In other words, processing begins from the end with a relatively high degree of resin orientation, and processing ends at the end with a relatively low degree of resin orientation. Similarly, in rolls No. 2 to 9, processing begins from the end with a relatively high degree of resin orientation, and processing ends at the end with a relatively low degree of resin orientation.

[0078] For example, when moving from processing roll No. 2 to processing roll No. 3, a large difference in the degree of resin orientation occurs, as shown by the thick arrow in the graph. Therefore, if processing is performed on the rolls in the order in which the original film rolls were produced, significant adjustments to the processing conditions are required when changing rolls. And if the range of adjustment is large, production efficiency decreases.

[0079] For example, when stretching raw film, it takes several hundred meters 3 Several thousand meters from 3 It is necessary to control the temperature inside the stretching chamber, which extends over a large area. However, in a large stretching chamber, the heating temperature does not stabilize and may fluctuate (hunt) around the target temperature.

[0080] There is also a method of obtaining the status inside the stretching chamber in real time and controlling the temperature based on that. This is called "feedback control." It was found that feedback control in a large stretching chamber cannot keep up with the changes, and that frequent temperature control would increase temperature fluctuations. It was also found that increased temperature fluctuations would lead to unstable quality.

[0081] Furthermore, since the thickness of the raw film varies slightly within the roll of the raw film, it is preferable to locally heat the relevant area. Even with localized heating, if the temperature is changed suddenly and feedback control is attempted to be performed on the management of the ambient temperature and the temperature of the heating device, the control will not be able to keep up. As a result, it was found that the quality becomes unstable.

[0082] Another example is coating a raw film. In particular, when coating a raw film with a liquid crystal polymer, it is necessary to adjust the orientation of the liquid crystal polymer. However, since the orientation of the liquid crystal polymer is affected by the orientation of the resin molecules in the underlying raw film, it is necessary to control the coating conditions based on the orientation information of the raw film. For this coating process, feedback control is performed based on the orientation information of the raw film, and it was found that if the coating conditions are changed suddenly, the quality becomes unstable.

[0083] That is, in both the stretching process and the coating process, it is believed that the quality can be more stabilized by narrowing the range of adjustment of the processing conditions.

[0084] In the present invention, when the original film is produced, first, information on the characteristics of each original film is obtained. Next, information on the characteristics of the inside and outside of each original film is extracted. Then, it is preferable to process the extracted information on the characteristics of the inside and outside of the roll to obtain a similarity between the inside of the N-1th original film and the outside of the Nth candidate original film.

[0085] FIG. 17 is a flow diagram of a production management system for the optical film of the present invention. First, information on the characteristics of the original film is obtained and stored in a database. Next, information on the characteristics of the (N-1)th original film roll is retrieved from the database and set as a reference value. Then, information on the characteristics of the inside of the roll is extracted from the information on the characteristics of the (N-1)th original film roll.

[0086] On the other hand, raw film rolls whose characteristic information is close to the above-mentioned reference value are extracted from the storage pool and sorted into a selection candidate pool. Note that the "close" here may be any value that is relatively close to the reference value and can be set appropriately. Next, information about the characteristics of the outer side of the roll of each raw film roll in the selection candidate pool is extracted.

[0087] Then, a similarity is obtained from information regarding the characteristics of the inside of the extracted (N-1)th original film web and information regarding the characteristics of the outside of the web of each original film web in the selection candidate pool.

[0088] Select multiple original films with similar characteristics (similarity closer to 0). Among them, select the one with the closest orientation information to the (N-1)th original film as the (N)th. A series of steps are then repeated to determine the order in which the original film rolls are inserted. In addition, raw film that is not selected as a candidate is returned to the storage pool.

[0089] 2. Optical Film Manufacturing Management System Configuration The system of the present invention includes the following (1) to (4). (1) Information acquisition unit for the characteristics of each raw film (2) A section for extracting information on the characteristics of the inside and outside of each roll of film (3) An information processing unit for extracting the characteristics of the inside and outside of the roll (4) A unit for determining the sequence of feeding the raw film to the next process based on information regarding the characteristics of the inside and outside of the processed roll. In addition, it has the following functions (5) to (6) as necessary. (5) A function to determine whether or not the stretching conditions or stretching rate can be adjusted, and the time required for the next process. (6) A function for determining the stretching speed, stretching temperature, or stretching ratio

[0090] The following explains each in order. The details of each part and its function will be described later in the method for producing an optical film.

[0091] (1) Information acquisition department In the present invention, the "information acquisition section" refers to a section having a function of acquiring information about the characteristics of each raw film. In other words, this section acquires information about the characteristics from each raw film.

[0092] The "information on the characteristics of the raw film" includes not only information on the characteristics of the raw film itself, but also information that changes in response to the characteristics. Specifically, information on the orientation of the resin molecules contained in the raw film, the surface roughness, thickness, refractive index, light transmittance, etc. of the raw film are included. In other words, the information acquisition unit measures the physical properties of the raw film.

[0093] The measurement is preferably carried out during the preparation of the original film and before it is wound up. The measurement is preferably carried out continuously at intervals within a specific range in the longitudinal or transverse direction. The intervals do not have to be constant as long as they are within the specific range. For various measurements of the raw film, conventionally known methods can be used. Moreover, various measurements on the original film are carried out under the same conditions.

[0094] (1.1) Phase difference measurement The method for obtaining information on the orientation of the resin molecules is not particularly limited. One example is a method for measuring phase difference (retardation). Hereinafter, the information on the orientation of the resin molecules contained in the raw film is also simply referred to as "orientation information".

[0095] The retardation in the in-plane direction is called "in-plane retardation (Ro)", and the retardation in the thickness direction is called "thickness direction retardation (Rth)".

[0096] Ro and Rth are defined by the following formulas, respectively. Formula: Ro = (n x -n y )×d Formula: Rth=((n x +n y ) / 2-n z )×d During the ceremony, n x represents the refractive index in the in-plane slow axis direction of the original film (the direction in which the refractive index is maximum), n y represents the refractive index in a direction perpendicular to the in-plane slow axis of the original film, n z represents the refractive index in the thickness direction of the original film, d represents the thickness (nm) of the original film.

[0097] The in-plane slow axis of the original film can be confirmed, for example, by an automatic birefringence meter Axoscan "Axo Scan Mueller Matrix Polarimeter" (manufactured by Axometrics).

[0098] Ro and Rth can be measured, for example, by the following method. It is preferable to carry out the measurement during the period from preparation of the raw film to winding it up. 1) Condition the original film for 24 hours at 23°C and 55% RH. Measure the average refractive index of the original film with an Abbe refractometer. Measure the thickness d with a commercially available micrometer. 2) After humidity conditioning, the Ro and Rth of the film at a measurement wavelength of 550 nm are measured in an environment of 23° C. and 55% RH using an automatic birefringence meter Axo Scan “Axo Scan Mueller Matrix Polarimeter” (manufactured by Axometrics).

[0099] Alternatively, Ro and Rth may be measured using, for example, an in-line retardation / film thickness measuring device "RE-200L2T-Rth+film thickness" (manufactured by Otsuka Electronics Co., Ltd.).

[0100] The method for measuring the retardation in the production direction and the width direction of the raw film is not particularly limited, and any conventionally known method can be used.

[0101] (1.1.1) Measurement of phase difference in the longitudinal direction (production direction) In the present invention, the "production direction" refers to the longitudinal direction of the raw film. The phase difference is measured at any interval in the width direction over an area of ​​10 m or more from the edge of the original film in the production direction.

[0102] The measurement interval in the production direction is preferably within a range of 5 to 600 mm, more preferably within a range of 10 to 300 mm, in order to prevent overlooking a portion where the phase difference is locally changed. In addition, when multiple measurements are performed in the width direction, not just one arbitrary point, an average value in the width direction for each measurement is calculated. This may be used as a longitudinal phase difference for simplified processing. Details will be described later. The measurement intervals do not necessarily have to be constant.

[0103] As a measurement procedure, for example, the retardation is measured at an arbitrary interval in the width direction. Next, the sheet is moved in the production direction, and the retardation is measured again at an arbitrary interval in the width direction. This process is repeated.

[0104] It is preferable to measure the phase difference multiple times for each measurement point. For example, the phase difference is measured 100 times for each measurement point, and the arithmetic average value is calculated.

[0105] FIG. 18 is an explanatory diagram of an example of measurement points for the phase differences Ro and Rth. An example of a method for measuring the phase difference in the longitudinal direction will be described with reference to Fig. 18. However, the present invention is not limited to this. In FIG. 18, the number of measurement points is six for simplification in order to make it easier to understand, but in practice, it is preferable to have more measurement points than this.

[0106] The dotted lines L1 and L2 are straight lines parallel to the longitudinal direction. a , L b and L c is a straight line parallel to the width direction. a , L b The points on Lc and Ld are located at positions a, b, and c in the longitudinal direction, respectively. Measurement point P a2 , P a1 The phase difference is measured in the width direction in the order of a. Next, the position in the length direction is moved from a to b, and P b1 , P b2 The phase difference is measured in the width direction in the order of b. Furthermore, the position in the length direction is moved from b to c, and P c2 , P c1 The retardation is measured in the width direction in the order of 100. In this manner, six points are measured. The retardation is measured 100 times for each measurement point, and the arithmetic average value is calculated.

[0107] Measurement point P a1 , P b1 and P c1 are aligned on the dotted line L1. These three points are in the same position in the width direction and are continuous in the length direction. Similarly, the measurement point P a2 , P b2 and P c2 are lined up on the dotted line L2. These three points are in the same position in the width direction and are continuous in the longitudinal direction. a1 , P b1 and P c1 The interval is preferably within a range of 5 to 600 mm, and more preferably within a range of 10 to 300 mm. a2 , P b2 and P c2 The same is true for the intervals.

[0108] In this manner, the phase difference is measured at three different positions (a, b, and c) in the longitudinal direction. Moreover, by carrying out the measurement in this manner, the retardation in the longitudinal direction can be measured while the original film is being produced (manufactured).

[0109] (1.1.2) Measurement of phase difference in the width direction The retardation is measured at any interval in the width direction in an area of ​​10 m or more from the end of the raw film in the production direction. The measurement interval is preferably within a range of 5 to 600 mm in the width direction, and more preferably within a range of 10 to 300 mm. By keeping the measurement within the above range, it is possible to prevent overlooking a portion where the retardation changes locally. The measurement intervals do not necessarily have to be constant. Furthermore, the measurement points do not have to be at the same positions in the width direction. The measurement of the retardation in the longitudinal direction can also be used to measure the retardation in the width direction. By moving the measuring device, the number of measuring devices required can be reduced.

[0110] (1.1.3) Measurement of thickness in the cross direction The thickness is measured at any interval in the width direction in a region of 10 m or more from the end of the raw film in the production direction. The measurement interval is preferably within a range of 5 to 600 mm in the longitudinal direction and the width direction, and more preferably within a range of 10 to 300 mm. By keeping the measurement within the above range, it is possible to prevent overlooking a portion where the retardation changes locally.

[0111] FIG. 19 is an explanatory diagram of an example of thickness measurement points. All the measurement points indicated by black circles are aligned on a dotted line parallel to the width direction. The thickness can be measured by a conventional method.

[0112] (2) Information extraction section In the present invention, the "information extraction unit" refers to a part having a function of extracting information about the characteristics of at least the inside or outside of each raw film. In other words, this part extracts information about the characteristics of the inside or outside of the raw film from the information about the characteristics of each raw film obtained by the information acquisition unit. For one raw film, the extraction of information about the characteristics may be performed only on the inside side of the roll, only on the outside side of the roll, or on both the inside and outside sides of the roll.

[0113] In the present invention, of both longitudinal ends of an original film wound into a roll, the end located on the inside of the roll is referred to as the "inner side of the roll," and the end located on the outside of the roll is referred to as the "outer side of the roll." The "ends" refer to areas within, for example, 1000 m from both ends in the longitudinal direction.

[0114] (3) Information Processing Section In the present invention, the "information processing section" refers to a section having a function of processing the extracted information on the characteristics of the inside and outside of the roll. In other words, this section processes the information on the characteristics of the inside and outside of the roll obtained by the information extraction section.

[0115] The type of information obtained by processing is not particularly limited. However, as described above, it is preferable that the outer end of the raw film roll to be processed Nth has characteristics relatively similar to the inner end of the raw film roll to be processed N-1th. The following describes the processing performed on the extracted information in order to use it to determine whether or not the information has similar characteristics.

[0116] In the method to be described, the in-plane retardation Ro is measured as the characteristic, although in the present invention the characteristic here is not limited to the in-plane retardation Ro. In this method, the retardation in the longitudinal direction (production direction) is processed, and the retardation in the width direction is processed. Then, the similarity is calculated. In the present invention, the "similarity" refers to a value calculated by the method described below.

[0117] The information extraction unit extracts information about the Ro of the inside and outside of each roll of raw film. More specifically, the information about the Ro of the inside and outside of the roll acquired by the information acquisition unit is extracted. Then, the information is processed in the following manner.

[0118] (3.1) Processing of phase difference in the longitudinal direction (production direction) For the retardation Ro in the longitudinal direction (production direction) measured above, an individual value or an average value is extracted for each measurement count at the measurement position in the width direction set for the target raw film. The retardation values ​​may be calculated individually in the width direction and all values ​​may be displayed. Alternatively, for simplified processing, an average value for each measurement may be used.

[0119] The following description will be given with reference to FIG. 18, which is a simplified conceptual diagram for ease of understanding. In the present invention, the term "set measurement position in the width direction" refers to a measurement position in the width direction that is appropriately set. In Fig. 18, this refers to the position 1 in the width direction and the position 2 in the width direction. The "number of measurements" refers to the number of measurements at different measurement positions in the width direction relative to the measurement position in the longitudinal direction. At the position a in the longitudinal direction, P a1 and P a2 Since the measurement was performed twice, the number of measurements was two. a1 and P a2 Similarly, individual values ​​can be extracted for positions b and c in the longitudinal direction.

[0120] From the viewpoint of simplified processing, an average value for each measurement may be used. In other words, measurement point P a1 and P a2 Since multiple measurements (2 times) were taken in the width direction, from the viewpoint of simplified processing, a1 and P a2Alternatively, the arithmetic average value of the phase difference at the position a in the longitudinal direction may be calculated. The calculated value is the phase difference value at the position a in the longitudinal direction. Similarly, the average values ​​can be extracted for the positions b and c in the longitudinal direction. In addition, it is preferable that the number of actual measurement points is more than the six points shown in Fig. 18. For example, if the number of measurements at the position a in the longitudinal direction is n, the individual values ​​are P a1 ~P an The average phase difference value is P a1 ~P an The arithmetic mean value of each of the phase difference values ​​is calculated.

[0121] For the extracted Ro, calculate the standard deviation in the production direction. Standard deviation is a widely used index that indicates the degree of variation in measured values. A small standard deviation means that the distribution of measured values ​​is relatively concentrated around the average value. Conversely, a large standard deviation means that the distribution of measured values ​​is relatively far from the average value. In other words, the degree of variation in Ro at the end of each raw film can be determined.

[0122] The standard deviation can be calculated using the following formula (2).

[0123]

number

[0124] During the ceremony, σ represents the standard deviation, X1~X n represents n measurements, m represents the average value of n measured values. The average value is not particularly limited, but is preferably an arithmetic average value.

[0125] It is preferable to select the standard deviation threshold value appropriately depending on the situation. From the viewpoint of manufacturing efficiency, the threshold value of the standard deviation is preferably 0.5 or less, and more preferably 0.4 or less. It is preferable to sort the raw film based on whether the threshold value is exceeded. Raw films below the threshold are selected as raw films to be input. Raw films may also be sorted in ascending order of standard deviation. Raw films above the threshold are returned to a storage pool for storing raw films.

[0126] Furthermore, Ro here may be, for example, the arithmetic mean value of measurements taken multiple times at each measurement point.

[0127] When the standard deviation σ of Ro at the end portion is equal to or greater than a certain value, it can be seen that the variation in Ro at the end portion is relatively large. It can also be inferred that the variation in Ro is large for the portions other than the end portion. Since such a raw film requires a large range of adjustment of the processing conditions, it takes time to adjust the processing conditions, and it is considered that the production speed until the optical film is manufactured is slow. By processing such a raw film when there is ample time, the production efficiency can be improved.

[0128] (3.2) Processing of phase difference in the width direction The retardation Ro in the width direction measured above is extracted for each individual measurement point set in the width direction. For the extracted Ro, calculate the standard deviation for each measurement in the same manner as above. This processing is applied to raw film that is below the above threshold and is a candidate for input.

[0129] This will be explained using FIG. At the position a in the longitudinal direction, the individual measurement points set in the width direction are P a1 and P a2 The phase difference values ​​at these points are extracted. The standard deviation of the extracted phase difference values ​​is calculated in the same manner as above. Similarly, the standard deviation of the phase difference values ​​at positions b and c in the longitudinal direction is calculated.

[0130] It is preferable to set a threshold for the standard deviations resulting from this processing, and any standard deviations exceeding the threshold are returned to a storage pool.

[0131] (3.3) Calculation of similarity The degree of difference in the average value of the phase difference value for each original film obtained by the above processing and the degree of difference (approximation) in the standard deviation value are selected within a threshold range. For each selected candidate, the standard deviation is calculated when an arbitrary length on the inside of the N-1th original roll is connected to an arbitrary length on the outside of the roll of the candidate. The standard deviation is used as the similarity. The closer the similarity is to 0, the more similar it is, and the greater the similarity is, the worse it is considered to be.

[0132] The length or number of times to be used when calculating the standard deviation by consecutively measuring the N-1th and Nth samples may be determined arbitrarily based on the characteristics of the original film and the processing conditions. In particular, in the case of optical films, it is preferable to perform the calculation by consecutively measuring 10 m or more in the production direction, and more preferably to perform the calculation by consecutively measuring 100 m or more. The standard deviation of consecutive phase difference values ​​is calculated and regarded as the "similarity." The similarity between the (N-1)th original film roll and the inside and outside of each of the original film rolls that are candidates for input is calculated. It is also preferable to arrange the original films in ascending order of similarity value.

[0133] An example of a procedure for calculating the similarity will be described. By the above-mentioned processing of retardation in the longitudinal direction (production direction), the average value and standard deviation value of retardation value in the longitudinal direction (production direction) on the outer side of the raw film are calculated. As described above, raw films with standard deviation values ​​below the threshold value are considered to be input candidates.

[0134] Next, the degree of difference (difference) between the average value of the retardation value in the longitudinal direction (production direction) on the inside of the N-1th original film roll and the outside of the Nth original film roll candidate is calculated. Those with a difference below a threshold are narrowed down as original films to be input candidates. The threshold is not particularly limited, but is preferably 5 nm or less, more preferably 2 nm or less.

[0135] Furthermore, the degree of difference (difference) between the standard deviation value of the retardation value in the longitudinal direction (production direction) on the inside of the (N-1)th original film roll and the outside of the (N)th original film roll candidate is calculated. Those with a difference below a threshold value are narrowed down as original films to be input candidates. The threshold value is not particularly limited, but is preferably 1 or less, and more preferably 0.3 or less.

[0136] Then, consider the connection area that can be created by connecting any area on the inside of the N-1th original film roll to any area on the outside of the Nth input candidate original film roll via the ends of each original film roll. In other words, consider the area where the original films switch when the N-1th original film roll and the Nth input candidate original film roll are processed continuously. Calculate the standard deviation value in the longitudinal direction (production direction) for the entire connection area. Then, the standard deviation value is regarded as the "similarity."

[0137] Fig. 20 is an explanatory diagram of a connection region. Note that Fig. 20 is a simplified conceptual diagram for ease of understanding. The left side is an arbitrary area on the inside of the N-1th original film roll, and the right side is an arbitrary area on the outside of the Nth original film roll candidate. Assume that they are connected via their respective ends. In an arbitrary area on the inside of the N-1th original film roll, the measurement point of the longitudinal retardation value is P 11 , P 12 and P 13 In an arbitrary area on the outer side of the raw film of the Nth input candidate, the measurement point of the retardation value in the longitudinal direction is P 21 , P 22 and P 23The standard deviation in the longitudinal direction is calculated for all of these measurement points.

[0138] In addition, the number of actual measurement points is preferably more than the six points shown in Fig. 20. For example, in an arbitrary region on the inside of the (N-1)th original film, the number of measurement points for the retardation value in the longitudinal direction is n (P 11 ~P 1n ) In addition, in an arbitrary region on the outer side of the raw film of the Nth input candidate, the number of measurement points of the longitudinal retardation value is n (P 21 ~P 2n ) In this case, P 11 ~P 1n and P 21 ~P 2n The standard deviation is calculated for all data.

[0139] The "length used when connecting the N-1th and Nth to calculate the standard deviation", i.e., the length in the longitudinal direction in the connection region, may be set as needed. Also, the "number of times used when connecting the N-1th and Nth to calculate the standard deviation", i.e., the number of measurement points for phase difference, may be set as needed.

[0140] (3.4) Calculation of thickness deviation The order in which the raw films are fed is preferably determined taking into consideration the standard deviation of the thickness in addition to the similarity. The information extracting unit extracts information about the thickness of the inside and outside of each raw film web, and calculates the standard deviation in the same manner as above.

[0141] (4) Order determining part In the present invention, the "order determination unit" refers to a unit having a function of determining the order of feeding original film in the next process based on information on the characteristics of at least the inside or outside of the roll that has been processed. In other words, this unit determines the order of feeding original film in the next process based on information on the characteristics of the inside and outside of the roll that has been processed by the information processing unit.

[0142] The following describes a case where the information obtained by the information processing section is the similarity. The same applies to a case where the information obtained by the information processing section is information other than the similarity.

[0143] From the similarity information, select multiple original films that have a low similarity and are closer to 0 (high similarity) in combination with the N-1th original film that has been previously introduced. Then, from among them, select the one with the orientation information closest to the inside of the N-1th original film as the Nth. When calculating the similarity, "the orientation information is closest" means that the average values ​​of the retardation in the longitudinal direction are close (the difference is small). In addition, it is preferable that the standard deviation of the retardation in the longitudinal direction and the standard deviation of the retardation in the width direction both show close values.

[0144] Also, instead of determining the (N-1)th to (N)th, it is also possible to determine, for example, up to (N+10)th at once. In this case, it is preferable to combine the orders up to the N+10th order, starting from the difference between the similarity score of the N-1th order and the Nth order, so that the sum of the similarity scores of the N+9th order and the N+10th order is the smallest.

[0145] In addition to the similarity, it is preferable that the outer end of the raw film roll to be processed Nth is similar in thickness to the inner end of the raw film roll to be processed N-1th. By continuously processing raw film rolls with relatively small differences in thickness, the range of adjustment of processing conditions can be reduced.

[0146] Specifically, it is preferable to determine the order of feeding the raw film based on the standard deviation of thickness at each position in the width direction of the raw film, which is calculated by the information processing unit.

[0147] When the standard deviation of thickness at a width direction position on the inside of the roll of the previous (N-1th) original film roll to be loaded is σ1, and the standard deviation of thickness at a width direction position on the outside of the roll of the original film roll to be loaded (Nth) is σ2, it is preferable to satisfy the following formula (1). Equation (1) |σ1-σ2| / σ1≦0.05

[0148] (5) A function to determine whether or not the stretching conditions or stretching rate can be adjusted, and the time required for the next process. In the system of the present invention, when the next process includes a process of stretching the input raw film, it is preferable that the system further has a function of determining whether the stretching conditions or stretching ratio can be adjusted and the time required for the next process, based on the information obtained in parts (1) to (4) above.

[0149] The information obtained in the above (1) to (4) specifically refers to the acquired information regarding the orientation, the extracted information regarding the orientation at least on the inside or outside of the roll, and the processed information regarding the orientation at least on the inside or outside of the roll.

[0150] By having such a function, it is possible to select appropriate processing conditions in the next process, and it becomes easier to process in a state where the adjustments are sufficient, so that losses during production can be further reduced. Also, when the adjustment range of the processing conditions is large, the adjustment can be performed sufficiently by ensuring the adjustment time. Therefore, by judging the time required for the next process, losses during production can be further reduced.

[0151] (6) A function for determining the stretching speed, stretching temperature, or stretching ratio In the system of the present invention, it is preferable that the function (5) further includes a function of determining the stretching speed, the stretching temperature, or the stretching ratio. That is, when it is judged that the stretching conditions or the stretching ratio can be adjusted, it is preferable to further have a function of determining the stretching conditions such as the stretching speed and the stretching temperature or the stretching ratio.

[0152] 3. Optical film manufacturing management program The optical film manufacturing management program of the present invention is an optical film manufacturing management program that determines the original film to be input in the next process from a plurality of wound original films and determines the manufacturing order of optical films, and is characterized in that it acquires information regarding the orientation of resin molecules contained in each of the original films in at least the longitudinal direction, extracts information regarding the orientation on the inside and outside of the roll of each of the original films, processes based on the extracted information regarding the orientation on the inside and outside of the roll, and determines the order for input of the original films in the next process based on the processed information regarding the orientation on the inside and outside of the roll. It is also preferable to calculate the similarity from the extracted information on the orientation on the inside and outside of the roll.

[0153] For example, all or any part of the processing functions performed by each part and function in the optical film production management system may be realized by a program interpreted and executed by a CPU (Central Processing Unit). The program is recorded on a non-transitory, computer-readable recording medium including programmed instructions for causing an information processing device to execute the system.

[0154] That is, a computer program that works with an OS (Operating System) to give instructions to a CPU and perform various processes is recorded in a ROM, HDD, etc. This computer program is executed by being loaded into a RAM, and works with the CPU to form a control unit.

[0155] The computer program may also be stored in an application program server connected via any network, and may be downloaded in whole or in part as required.

[0156] The program may be stored in a non-transitory computer-readable recording medium. It may also be configured as a program product. Here, the "recording medium" includes any "portable physical medium" such as a memory card, a USB memory, an SD card, a flexible disk, a magneto-optical disk, a ROM, an EPROM, an EEPROM (registered trademark), a CD-ROM, an MO, a DVD, and a Blu-ray (registered trademark) Disc.

[0157] In the present invention, a "program" refers to a data processing method written in any language or description method. It may be in any format, such as source code or binary code. Note that a "program" is not necessarily limited to a single configuration, but also includes a distributed configuration consisting of multiple modules or libraries, and a program that achieves its function by working together with a separate program, such as an OS (Operating System). Note that the specific configuration for reading a recording medium, the reading procedure, the installation procedure after reading, etc., may be any well-known configuration or procedure.

[0158] The various databases are storage means such as memory devices such as RAM and ROM, fixed disk devices such as hard disks, flexible disks, and optical disks. They store various programs, tables, databases, and web page files used for various processes and providing websites.

[0159] 4. Optical film manufacturing method The optical film manufacturing method of the present invention is a method for manufacturing an optical film in which a raw film to be input in a next process is determined from a plurality of wound raw films and the order of manufacturing the optical films is determined, and is characterized by having the following steps: a step of acquiring information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction; a step of extracting information regarding the orientation on the inside and outside of the roll of each of the raw films; a step of processing based on the extracted information regarding the orientation on the inside and outside of the roll; and a step of determining the order of input of the raw films in the next process based on the processed information regarding the orientation on the inside and outside of the roll.

[0160] Each step is as described above. The structure of the raw film, the method of production, and the subsequent stretching process will be described below.

[0161] (1) Composition of the original film The configuration of the raw film is not particularly limited, and a conventionally known one can be used. An example of the raw film will be described below, but the present invention is not limited thereto.

[0162] (1.1) Thermoplastic resin There are no limitations on the thermoplastic resin material used for the raw film of the present invention, so long as it can be handled in a roll form after film formation.

[0163] For example, thermoplastic resins include cellulose ester resins such as triacetyl cellulose (TAC), cellulose acetate propionate (CAP), and diacetyl cellulose (DAC); cyclic olefin resins such as cycloolefin resin (COP); polypropylene resins such as polypropylene (PP); acrylic resins such as polymethyl methacrylate (PMMA); and polyester resins such as polyethylene terephthalate (PET).

[0164] In the case of a raw film having a low modulus of elasticity, for example, a raw film having a modulus of elasticity of less than 3.0 GPa, it is difficult to relieve stress at multiple locations of the raw film when forming a roll. Therefore, the raw film is difficult to expand and contract in the width direction or length direction. In addition, in the case of a roll-shaped raw film, the surface cannot absorb the stress, and the winding slippage is likely to occur. In addition, when a raw film having a low modulus of elasticity has a height difference in the width direction or length direction, the difference between the expansion and contraction at the high points and the low points of the raw film becomes large.

[0165] Therefore, the maximum height difference (PV) of the longitudinal average film thickness is preferably within a range of 0.02 to 0.40 μm. From this viewpoint, the thermoplastic resin is preferably a cycloolefin resin (COP) or polymethyl methacrylate (acrylic resin (PMMA)).

[0166] Among these, cycloolefin resins (COP) are preferred, since the stretchability and crystallinity can be easily controlled by using cycloolefin resins (COP). The raw film may be subjected to a surface modification treatment after production.

[0167] The thickness of the raw film is preferably within the range of 5 to 80 μm, more preferably within the range of 10 to 65 μm, and further preferably within the range of 10 to 45 μm. When the thickness is 5 μm or more, the raw film has high rigidity and can easily maintain its roll shape. By keeping the thickness at 80 μm or less, the mass of the original film does not increase too much, making it easy to produce a long roll.

[0168] (1.1.1) Cycloolefin resin The cycloolefin resin is preferably a polymer of a cycloolefin monomer, or a copolymer of a cycloolefin monomer and another copolymerizable monomer.

[0169] The cycloolefin monomer is preferably a cycloolefin monomer having a norbornene skeleton, and more preferably a cycloolefin monomer having a structure represented by the following general formula (A-1) or (A-2).

[0170] [ka]

[0171] In general formula (A-1), R 1 ~R 4 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 30 carbon atoms, or a polar group, and p represents an integer of 0 to 2. 1 ~R 4 Not all of these represent hydrogen atoms at the same time, and R 1 and R 2 does not simultaneously represent a hydrogen atom, and R 3 and R 4 does not simultaneously represent a hydrogen atom.

[0172] In general formula (A-1), R 1 ~R 4 The hydrocarbon group having 1 to 30 carbon atoms represented by the following formula is, for example, preferably a hydrocarbon group having 1 to 10 carbon atoms, and more preferably a hydrocarbon group having 1 to 5 carbon atoms. The hydrocarbon group having 1 to 30 carbon atoms may further have a linking group containing, for example, a halogen atom, an oxygen atom, a nitrogen atom, a sulfur atom or a silicon atom. Examples of such linking groups include divalent polar groups such as a carbonyl group, an imino group, an ether bond, a silyl ether bond, and a thioether bond. Examples of the hydrocarbon group having 1 to 30 carbon atoms include a methyl group, an ethyl group, a propyl group, and a butyl group.

[0173] In general formula (A-1), R 1 ~R 4Examples of the polar group represented by the formula (I) include a carboxy group, a hydroxy group, an alkoxy group, an alkoxycarbonyl group, an aryloxycarbonyl group, an amino group, an amido group, and a cyano group. Among these, a carboxy group, a hydroxy group, an alkoxycarbonyl group, or an aryloxycarbonyl group is preferable, and from the viewpoint of solubility during solution casting, an alkoxycarbonyl group or an aryloxycarbonyl group is more preferable.

[0174] In formula (A-1), p is preferably 1 or 2 from the viewpoint of increasing the heat resistance of the film. When p is 1 or 2, the resulting polymer becomes bulky and the glass transition temperature is likely to be improved.

[0175] [ka]

[0176] In general formula (A-2), R 5 R represents a hydrogen atom, a hydrocarbon group having 1 to 5 carbon atoms, or an alkylsilyl group having an alkyl group having 1 to 5 carbon atoms. 6 represents a carboxy group, a hydroxy group, an alkoxycarbonyl group, an aryloxycarbonyl group, an amino group, an amido group, a cyano group, or a halogen atom. The halogen atom represents a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom. p represents an integer of 0 to 2.

[0177] R in general formula (A-2) 5 is preferably a hydrocarbon group having 1 to 5 carbon atoms, and more preferably a hydrocarbon group having 1 to 3 carbon atoms.

[0178] R in general formula (A-2) 6 is preferably a carboxy group, a hydroxy group, an alkoxycarbonyl group or an aryloxycarbonyl group, and from the viewpoint of solubility during solution casting, is more preferably an alkoxycarbonyl group or an aryloxycarbonyl group.

[0179] In formula (A-2), p is preferably 1 or 2 from the viewpoint of improving the heat resistance of the raw film. When p is 1 or 2, the resulting polymer becomes bulky and the glass transition temperature is likely to be improved.

[0180] A cycloolefin monomer having a structure represented by the general formula (A-2) is preferred from the viewpoint of improving the solubility in an organic solvent. In general, by breaking the symmetry of an organic compound, the crystallinity decreases and the solubility in organic solvents increases. R in general formula (A-2) 5 and R 6 is substituted only on one ring carbon atom with respect to the axis of symmetry of the molecule, so the symmetry of the molecule is low. In other words, the cycloolefin monomer having the structure represented by the general formula (A-2) has high solubility and is suitable for producing the raw film by the solution casting method.

[0181] The content of the cycloolefin monomer having the structure represented by general formula (A-2) is preferably 70 mol% or more, more preferably 80 mol% or more, and even more preferably 100 mol% based on the total amount of all cycloolefin monomers constituting the cycloolefin resin. By containing at least a certain amount of a cycloolefin monomer having a structure represented by general formula (A-2), the orientation of the resin is improved, and the phase difference (retardation) value tends to increase.

[0182] Specific examples of the cycloolefin monomer having a structure represented by general formula (A-1) are shown below as exemplary compounds 1 to 14. Specific examples of the cycloolefin monomer having a structure represented by general formula (A-2) are shown below as exemplary compounds 15 to 34.

[0183] [ka]

[0184] Examples of the copolymerizable monomer copolymerizable with the cycloolefin monomer include a copolymerizable monomer capable of ring-opening copolymerization with the cycloolefin monomer, and a copolymerizable monomer capable of addition copolymerization with the cycloolefin monomer.

[0185] Examples of copolymerizable monomers capable of ring-opening copolymerization include cycloolefins such as cyclobutene, cyclopentene, cycloheptene, cyclooctene, and dicyclopentadiene.

[0186] Examples of copolymerizable monomers capable of addition copolymerization include unsaturated double bond-containing compounds, vinyl-based cyclic hydrocarbon monomers, and (meth)acrylates.

[0187] The unsaturated double bond-containing compound may be an olefin-based compound having 2 to 12 carbon atoms, such as ethylene, propylene, butene, etc. The number of carbon atoms is more preferably within the range of 2 to 8.

[0188] Examples of the vinyl cyclic hydrocarbon monomer include vinylcyclopentene monomers such as 4-vinylcyclopentene and 2-methyl-4-isopropenylcyclopentene.

[0189] Examples of (meth)acrylates include alkyl (meth)acrylates having 1 to 20 carbon atoms, such as methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate.

[0190] The content of the cycloolefin monomer is preferably within a range of 20 to 80 mol %, and more preferably within a range of 30 to 70 mol %, based on the total of all monomers constituting the copolymer.

[0191] As described above, the cycloolefin resin is a polymer obtained by polymerizing or copolymerizing a cycloolefin monomer having a norbornene skeleton, preferably a cycloolefin monomer having a structure represented by the general formula (A-1) or (A-2). Examples of the cycloolefin resin include the following polymers (1) to (7).

[0192] (1) Ring-opening polymer of cycloolefin monomer (2) Ring-opening copolymers of cycloolefin monomers and copolymerizable monomers capable of ring-opening copolymerization with the cycloolefin monomers. (3) Hydrogenated product of the ring-opening (co)polymer of (1) or (2) above (4) A (co)polymer obtained by cyclizing the ring-opening (co)polymer of (1) or (2) above by the Friedel-Crafts reaction and then adding hydrogen thereto. (5) Saturated copolymers of cycloolefin monomers and compounds containing unsaturated double bonds (6) Addition copolymers of cycloolefin monomers with vinyl cyclic hydrocarbon monomers and their hydrogenated products (7) Alternating copolymer of cycloolefin monomer and (meth)acrylate

[0193] The above polymers (1) to (7) can all be obtained by known methods, for example, the methods described in JP-A-2008-107534 and JP-A-2005-227606.

[0194] As the catalyst and solvent used in the above ring-opening copolymerization (2), for example, those described in paragraphs 0019 to 0024 of JP-A No. 2008-107534 can be used. As the catalyst for the hydrogenated products (3) and (6) above, for example, those described in paragraphs 0025 to 0028 of JP-A No. 2008-107534 can be used. As the acidic compound used in the above Friedel-Crafts reaction (4), for example, those described in paragraph 0029 of JP-A-2008-107534 can be used. As the catalyst used in the above addition polymerizations (5) to (7), for example, those described in paragraphs 0058 to 0063 of JP-A No. 2005-227606 can be used. The alternating copolymerization reaction of (7) above can be carried out by, for example, the method described in paragraphs 0071 and 0072 of JP-A No. 2005-227606.

[0195] Among them, the above polymers (1) to (3) and (5) are preferred, and the above polymers (3) and (5) are more preferred.

[0196] That is, the cycloolefin monomer preferably contains at least one of a structural unit represented by the following general formula (B-1) and a structural unit represented by the following general formula (B-2). It is more preferable that the cycloolefin monomer contains only a structural unit represented by the general formula (B-2), or contains both a structural unit represented by the general formula (B-1) and a structural unit represented by the general formula (B-2). This can increase the glass transition temperature and light transmittance of the resulting cycloolefin resin.

[0197] The structural unit represented by the general formula (B-1) is a structural unit derived from the cycloolefin monomer represented by the general formula (A-1) above. The structural unit represented by the general formula (B-2) is a structural unit derived from the cycloolefin monomer represented by the general formula (A-2) above.

[0198] [ka]

[0199] In the general formula (B-1), X represents -CH=CH- or -CH2CH2-. 1 ~R 4 and p are each R in general formula (A-1). 1 ~R 4 and p.

[0200] [ka]

[0201] In the general formula (B-2), X represents -CH=CH- or -CH2CH2-. 5 ~R6 and p are each R in general formula (A-2). 5 ~R 6 and p.

[0202] The cycloolefin resin according to the present invention may be a commercially available product. Examples of commercially available cycloolefin resins include "Arton (registered trademark) G7810", "Arton (registered trademark) F", "Arton (registered trademark) R4500, R4900, R5000", and "Arton (registered trademark) RX" (all manufactured by JSR Corporation).

[0203] The intrinsic viscosity [η]inh of cycloolefin resin is 0.2 to 5 cm when measured at 30°C. 3 / g, and 0.3 to 3 cm 3 More preferably, the range is 0.4 to 1.5 cm / g. 3 It is more preferable that the molecular weight is in the range of / g.

[0204] The number average molecular weight (Mn) of the cycloolefin resin is preferably within the range of 8,000 to 100,000, more preferably within the range of 10,000 to 80,000, and further preferably within the range of 12,000 to 50,000.

[0205] The weight average molecular weight (Mw) of the cycloolefin resin is preferably within a range of 20,000 to 300,000, more preferably within a range of 30,000 to 250,000, and further preferably within a range of 40,000 to 200,000.

[0206] The number average molecular weight and weight average molecular weight of the cycloolefin resin can be measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0207] (Gel Permeation Chromatography) Solvent: Methylene chloride Columns: Three columns, Shodex K806, K805, and K803G (Showa Denko K.K.), were connected together and used. Column temperature: 25℃ Sample concentration: 0.1% by mass Detector: RI Model 504 (GL Sciences) Pump: L6000 (Hitachi, Ltd.) Flow rate: 1.0ml / min Calibration curve: A calibration curve was used using 13 samples of standard polystyrene STK standard polystyrene (manufactured by Tosoh Corporation) in the range of Mw=500 to 2,800,000. It is preferable to use the 13 samples at approximately equal intervals.

[0208] When the intrinsic viscosity [η]inh, number average molecular weight and weight average molecular weight are within the above ranges, the cycloolefin resin has good heat resistance, water resistance, chemical resistance, mechanical properties and moldability as a raw film.

[0209] The glass transition temperature (Tg) of the cycloolefin resin is preferably 110°C or higher, more preferably within the range of 110 to 350°C, even more preferably within the range of 120 to 250°C, and particularly preferably within the range of 120 to 220°C.

[0210] By having a glass transition temperature (Tg) of 110°C or higher, deformation under high temperature conditions is easily suppressed. On the other hand, when the glass transition temperature (Tg) is 350° C. or lower, molding is easy and deterioration of the resin due to heat during molding can be suppressed.

[0211] The content of the cycloolefin resin is preferably 70% by mass or more, and more preferably 80% by mass or more, based on the total mass of the raw film.

[0212] (1.1.2) Acrylic resins Acrylic resins are polymers of acrylic acid esters or methacrylic acid esters, and also include copolymers with other monomers. Therefore, the acrylic resin according to the present invention also includes methacrylic resin.

[0213] The acrylic resin is not particularly limited. The content of methyl methacrylate units is preferably within a range of 50 to 99% by mass based on the total mass of the acrylic resin. In addition, the content of other monomer units copolymerizable with methyl methacrylate is preferably within a range of 1 to 50% by mass.

[0214] Examples of other monomer units include alkyl methacrylates in which the alkyl group has 2 to 18 carbon atoms; alkyl acrylates in which the alkyl group has 1 to 18 carbon atoms; hydroxyalkyl acrylates such as isobornyl methacrylate and 2-hydroxyethyl acrylate; α,β-unsaturated acids such as acrylic acid and methacrylic acid; acrylamides such as acryloylmorpholine and N-hydroxyphenylmethacrylamide; unsaturated group-containing dicarboxylic acids such as N-vinylpyrrolidone, maleic acid, fumaric acid, and itaconic acid; aromatic vinyl compounds such as styrene and α-methylstyrene; α,β-unsaturated nitriles such as acrylonitrile and methacrylonitrile; maleic anhydride; maleimide; N-substituted maleimide; glutarimide; and glutaric anhydride.

[0215] Among the above, copolymerizable monomers forming monomer units other than glutarimide and glutaric anhydride include monomers corresponding to the above monomer units.

[0216] That is, alkyl methacrylates in which the alkyl group has 2 to 18 carbon atoms; alkyl acrylates in which the alkyl group has 1 to 18 carbon atoms; hydroxyalkyl acrylates such as isobornyl methacrylate and 2-hydroxyethyl acrylate; α,β-unsaturated acids such as acrylic acid and methacrylic acid; acrylamides such as acryloylmorpholine and N-hydroxyphenylmethacrylamide; unsaturated group-containing dicarboxylic acids such as N-vinylpyrrolidone, maleic acid, fumaric acid, and itaconic acid; aromatic vinyl compounds such as styrene and α-methylstyrene; α,β-unsaturated nitriles such as acrylonitrile and methacrylonitrile; maleic anhydride; maleimide; and N-substituted maleimides.

[0217] The glutarimide unit can be formed, for example, by reacting an intermediate polymer having a (meth)acrylic acid ester unit with a primary amine (imidizing agent) to effect imidization (see JP-A-2011-26563).

[0218] The glutaric anhydride units can be formed, for example, by heating an intermediate polymer having a (meth)acrylic acid ester unit (see Japanese Patent No. 4961164).

[0219] Among these, from the viewpoint of mechanical strength, the monomer unit is preferably isobornyl methacrylate, acryloylmorpholine, N-hydroxyphenylmethacrylamide, N-vinylpyrrolidone, styrene, hydroxyethyl methacrylate, maleic anhydride, maleimide, N-substituted maleimide, glutaric anhydride, or glutarimide.

[0220] The weight average molecular weight (Mw) of the acrylic resin is preferably within a range of 50,000 to 1,000,000, more preferably within a range of 100,000 to 1,000,000, and even more preferably within a range of 200,000 to 800,000. By having a weight average molecular weight (Mw) of 50,000 or more, the raw film has excellent heat resistance and mechanical strength. In addition, by having a weight average molecular weight of 1,000,000 or less, the raw film has excellent peelability from the metal support and drying ability of organic solvents during production.

[0221] The method for synthesizing the acrylic resin is not particularly limited, and any of the known methods such as suspension polymerization, emulsion polymerization, bulk polymerization, and solution polymerization may be used.

[0222] As the polymerization initiator, known peroxide-based and azo-based initiators can be used, and redox-based initiators may also be used.

[0223] The polymerization temperature is preferably within the range of 30 to 100°C in suspension or emulsion polymerization, and preferably within the range of 80 to 160°C in bulk or solution polymerization.

[0224] From the viewpoint of controlling the reduced viscosity of the obtained copolymer, an alkyl mercaptan or the like may be used as a chain transfer agent.

[0225] From the viewpoint of the mechanical strength of the raw film, the glass transition temperature (Tg) of the acrylic resin is preferably within the range of 80 to 120°C.

[0226] As the acrylic resin, commercially available products can be used. Examples of such materials include "Delpet (registered trademark) 60N, 80N, 980N, SR8200" (all manufactured by Asahi Kasei Chemicals Corporation), "Dianale (registered trademark) BR52, BR80, BR83, BR85, BR88, EMB-143, EMB-159, EMB-160, EMB-161, EMB-218, EMB-229, EMB-270, EMB-273" (all manufactured by Mitsubishi Rayon Co., Ltd.), and "KT75, TX400S and IPX012" (all manufactured by Denki Kagaku Kogyo Co., Ltd.). These may be contained alone or in combination of two or more.

[0227] The acrylic resin preferably contains an additive. As an example of the additive, it is preferable to contain acrylic particles (rubber elastomer particles) described in International Publication No. 2010 / 001668 from the viewpoint of improving the mechanical strength of the raw film and adjusting the dimensional change rate. The rubber elastomer particles are a multi-layered acrylic granular composite.

[0228] Examples of commercially available rubber elastomer particles include "Metablen (registered trademark) W-341" (manufactured by Mitsubishi Rayon Co., Ltd.), "Kane Ace (registered trademark)" (manufactured by Kaneka Corporation), "Paraloid (registered trademark)" (manufactured by Kureha Corporation), "Acryloid" (manufactured by Rohm and Haas Co., Ltd.), "Staphyloid (registered trademark)" (manufactured by Aica Corporation), "Chemisnow (registered trademark) MR-2G, MS-300X" (all manufactured by Soken Chemical & Engineering Co., Ltd.), and "Parapet (registered trademark) SA" (manufactured by Kuraray Co., Ltd.). These may be contained alone or in combination of two or more.

[0229] The volume average particle diameter of the rubber elastomer particles is preferably 0.35 μm or less, more preferably in the range of 0.01 to 0.35 μm, and even more preferably in the range of 0.05 to 0.30 μm. By being within the above range, the raw film is easily stretched under heating, and the transparency of the raw film is not easily impaired.

[0230] From the viewpoint of flexibility, the bending modulus of the raw film measured in accordance with JIS K7171 is preferably 10.5 GPa or less, more preferably 1.3 GPa or less, and even more preferably 1.2 GPa or less. The bending modulus varies depending on the type and amount of the acrylic resin and rubber elastomer particles in the raw film. For example, the greater the content of the rubber elastomer particles, the smaller the bending modulus generally becomes.

[0231] Furthermore, in general, the flexural modulus of elasticity is smaller when a copolymer of alkyl methacrylate and alkyl acrylate is used as the acrylic resin than when a homopolymer of alkyl methacrylate is used.

[0232] (1.1.3) Cellulose ester resin In the present invention, the term "cellulose ester" refers to a cellulose acylate resin in which some or all of the hydrogen atoms of the hydroxyl groups (-OH) at the 2-, 3-, and 6-positions in the β-1,4-bonded glucose units that constitute cellulose are substituted with acyl groups.

[0233] The cellulose ester used is not particularly limited, and is preferably, for example, an ester of a linear or branched carboxylic acid having a carbon number in the range of 2 to 22. The carboxylic acid constituting the ester may be an aliphatic carboxylic acid or an aromatic carboxylic acid having a ring.

[0234] Examples of cellulose esters include cellulose esters in which a hydrogen atom in a hydroxyl group of cellulose is substituted with an acyl group having a carbon number of 2 to 22, such as an acetyl group, a propionyl group, a butyryl group, an isobutyryl group, a valeryl group, a pivaloyl group, a hexanoyl group, an octanoyl group, a lauroyl group, or a stearoyl group.

[0235] The carboxylic acid (acyl group) constituting the ester may have a substituent. The carboxylic acid constituting the ester is preferably a lower fatty acid having 6 or less carbon atoms, more preferably a lower fatty acid having 3 or less carbon atoms. The acyl group in the cellulose ester may be a single type or a combination of multiple acyl groups.

[0236] Specific examples of cellulose esters include cellulose acetates such as diacetyl cellulose (DAC) and triacetyl cellulose (TAC), as well as mixed fatty acid esters of cellulose in which a propionate group or a butyrate group is bonded in addition to an acetyl group, such as cellulose acetate propionate (CAP), cellulose acetate butyrate, and cellulose acetate propionate butyrate. These may be contained alone or in combination of two or more.

[0237] (Type and Degree of Substitution of Acyl Group) By adjusting the type and substitution degree of the acyl group of the cellulose ester, the humidity change in retardation of the raw film can be controlled within a desired range, and the thickness uniformity of the raw film can be improved.

[0238] The smaller the substitution degree of the acyl group of the cellulose ester, the better the retardation expression, and therefore the thinner the raw film can be. On the other hand, by substituting a certain amount of acyl groups, the durability of the raw film can be improved. In addition, the Rt humidity fluctuation, which is the retardation (retardation) in the thickness direction, occurs when water molecules coordinate to the carbonyl group of cellulose. Therefore, the Rt humidity fluctuation can be adjusted by adjusting the substitution degree of the acyl group.

[0239] The total degree of substitution of the acyl group of the cellulose ester is preferably within the range of 2.1 to 2.5. By being within the above range, it is possible to suppress the Rt fluctuation due to environmental fluctuation, particularly humidity, and to improve the uniformity of the film thickness. From the viewpoint of improving the flowability and stretchability during the preparation of the raw film and further improving the uniformity of the film thickness, the total degree of substitution is more preferably within the range of 2.2 to 2.45.

[0240] Specifically, the cellulose ester satisfies both of the following formulae (a) and (b): In the following formulae (a) and (b), X is the degree of substitution of an acetyl group, and Y is the degree of substitution of a propionyl group or a butyryl group, or the degree of substitution of a mixture thereof.

[0241] Formula (a) 2.1≦X+Y≦2.5 Formula (b) 0≦Y≦1.5

[0242] The cellulose ester is preferably cellulose acetate (Y=0) or cellulose acetate propionate (CAP) (Y: propionyl group, Y>0). From the viewpoint of reducing the variation in the film thickness, cellulose acetate with Y=0 is even more preferable.

[0243] From the viewpoints of retardation expression, Rt humidity fluctuation, and film thickness variation, cellulose diacetate (DAC) satisfying 2.1≦X≦2.5 is preferable, and cellulose diacetate (DAC) satisfying 2.15≦X≦2.45 is more preferable.

[0244] Furthermore, when Y>0, the cellulose acetate propionate (CAP) preferably satisfies 0.95≦X≦2.25, 0.1≦Y≦1.2, and 2.15≦X+Y≦2.45.

[0245] By using the above cellulose acetate or cellulose acetate propionate, it is possible to obtain a raw film having excellent retardation, mechanical strength, and resistance to environmental changes.

[0246] The degree of substitution of acyl groups indicates the average number of acyl groups per glucose unit. That is, it indicates how many of the hydrogen atoms of the hydroxyl groups at the 2nd, 3rd, and 6th positions of one glucose unit are substituted with acyl groups. Therefore, the maximum value of the degree of substitution is 3.0, which means that all of the hydrogen atoms of the hydroxyl groups at the 2nd, 3rd, and 6th positions are substituted with acyl groups. The acyl groups may be substituted evenly or distributed at the 2nd, 3rd, and 6th positions of the glucose unit. The degree of substitution is determined by the method specified in ASTM-D817-96.

[0247] From the viewpoint of optical properties, cellulose acetates having different degrees of substitution may be mixed. In this case, the mixing ratio of the different cellulose acetates is not particularly limited.

[0248] The number average molecular weight (Mn) of cellulose ester is 2×10 4 ~3×10 5 It is preferable that the range is 2×10 4 ~1.2×10 5 More preferably, it is within the range of 4×10 4 ~8×10 4 It is more preferable that the thickness is within the above range. By keeping the thickness within the above range, the mechanical strength of the raw film can be improved.

[0249] The number average molecular weight (Mn) of the cellulose ester can be calculated by measurement using gel permeation chromatography (GPC) under the above-mentioned measurement conditions.

[0250] The weight average molecular weight (Mw) of the cellulose ester is 2×10 4 ~1×10 6 It is preferable that the range is 2×10 4 ~1.2×10 5 More preferably, it is within the range of 4×10 4 ~8×10 4 It is more preferable that the thickness is within the above range. By keeping the thickness within the above range, the mechanical strength of the raw film can be improved.

[0251] The raw cellulose of the cellulose ester is not particularly limited, and examples thereof include cotton linters, wood pulp, kenaf, etc. Furthermore, the cellulose esters obtained from these can be mixed in any desired ratio.

[0252] Cellulose esters such as cellulose acetate and cellulose acetate propionate can be synthesized by known methods.

[0253] In general, the raw material cellulose is mixed with a specific organic acid (acetic acid, propionic acid, etc.), an acid anhydride (acetic anhydride, propionic anhydride, etc.), and a catalyst (sulfuric acid, etc.). The cellulose is then esterified, and the reaction is continued until a cellulose triester is produced.

[0254] In the triester, the three hydroxy groups of the glucose unit are replaced with the acyl group of an organic acid.

[0255] By using two kinds of organic acids at the same time, mixed ester type cellulose esters, such as cellulose acetate propionate and cellulose acetate butyrate, can be synthesized.

[0256] Next, the cellulose triester is hydrolyzed to synthesize a cellulose ester having a desired degree of acyl substitution. Then, the cellulose ester is obtained through processes such as filtration, precipitation, washing with water, dehydration, and drying. Specifically, the synthesis can be performed by referring to the method described in JP-A-10-45804.

[0257] (1.2) Other additives The raw film may contain the following additives in addition to the above-mentioned thermoplastic resin.

[0258] (1.2.1) Plasticizers By including a plasticizer, processability can be imparted to the raw film. The plasticizer may be contained alone or in combination of two or more kinds.

[0259] Among them, it is preferable to contain at least one plasticizer selected from the group consisting of sugar esters, polyesters, and styrene-based compounds, which allows both control of moisture permeability and compatibility with cellulose esters.

[0260] From the viewpoint of achieving both moist heat resistance and compatibility with cellulose ester, the number average molecular weight of the plasticizer is preferably 15,000 or less, and more preferably 10,000 or less.

[0261] When the compound having a number average molecular weight of 10,000 or less is a polymer, the weight average molecular weight (Mw) is preferably 10,000 or less. The weight average molecular weight (Mw) is more preferably within the range of 100 to 10,000, and further preferably within the range of 400 to 8,000.

[0262] In particular, the content of the compound having a molecular weight of 1500 or less is preferably within a range of 6 to 40 mass % relative to the total mass of the thermoplastic resin, and more preferably within a range of 10 to 20 mass %. By being within the above range, it is possible to achieve both control of moisture permeability and compatibility with the thermoplastic resin.

[0263] <Sugar ester> From the viewpoint of preventing hydrolysis, the plasticizer is preferably a sugar ester compound. Specifically, the sugar ester compound has at least one type of pyranose structure or furanose structure in the range of 1 to 12. All or a part of the OH groups in the structure are esterified.

[0264] <polyester> The plasticizer is preferably a polyester. The polyester is not particularly limited. For example, a polymer (polyester polyol) obtained by condensation reaction of dicarboxylic acid or its ester-forming derivative with glycol, the terminal of which is a hydroxyl group, can be mentioned. In addition, a polymer (terminal-capped polyester) in which the terminal hydroxyl group of the polyester polyol is capped with a monocarboxylic acid can be mentioned. The term "ester-forming derivative" refers to an ester of a dicarboxylic acid, a dicarboxylic acid chloride, or an anhydride of a dicarboxylic acid.

[0265] <Styrene-based compounds> From the viewpoint of water resistance, the plasticizer is preferably a styrene-based compound.

[0266] The styrene-based compound may be a homopolymer of a styrene-based monomer, or a copolymer of a styrene-based monomer and another copolymerizable monomer. From the viewpoint of ensuring that the molecular structure has a certain level of bulkiness or more, the content of the structural units derived from the styrene-based monomer is preferably within a range of 30 to 100 mol %, and more preferably within a range of 50 to 100 mol %, based on the entire styrene-based compound.

[0267] Examples of styrene monomers include styrene; alkyl-substituted styrenes such as α-methylstyrene, β-methylstyrene, and p-methylstyrene; halogen-substituted styrenes such as 4-chlorostyrene and 4-bromostyrene; hydroxystyrenes such as p-hydroxystyrene, α-methyl-p-hydroxystyrene, 2-methyl-4-hydroxystyrene, and 3,4-dihydroxystyrene; vinylbenzyl alcohols; alkoxy-substituted styrenes such as p-methoxystyrene, p-tert-butoxystyrene, and m-tert-butoxystyrene; 3-vinylbenzoic acid, 4-vinylbenzoic acid, and the like. Examples of such vinyl benzoates include vinyl benzoates such as benzoic acid; 4-vinylbenzyl acetate; 4-acetoxystyrene; amidostyrenes such as 2-butylamidostyrene, 4-methylamidostyrene, and p-sulfonamidostyrene; aminostyrenes such as 3-aminostyrene, 4-aminostyrene, 2-isopropenylaniline, and vinylbenzyldimethylamine; nitrostyrenes such as 3-nitrostyrene and 4-nitrostyrene; cyanostyrenes such as 3-cyanostyrene and 4-cyanostyrene; vinylphenylacetonitrile; arylstyrenes such as phenylstyrene; and indenes. These may be contained alone or in combination of two or more.

[0268] (1.2.2) Optional components The raw film may further contain other optional components such as an antioxidant, a colorant, an ultraviolet absorbing agent, a matting agent, acrylic particles, a hydrogen bonding solvent, and an ionic surfactant. The content of these is preferably within a range of 0.01 to 20% by mass relative to the total mass of the thermoplastic resin.

[0269] (Antioxidants) The antioxidant may be any of those conventionally known. Among these, lactone-based, sulfur-based, phenol-based, double bond-based, hindered amine-based and phosphorus-based compounds are preferred. These may be contained alone or in combination of two or more. For example, lactone-based, phosphorus-based, phenol-based and double bond-based compounds may be used in combination.

[0270] The content of the antioxidant is preferably within a range of 0.05 to 20% by mass, and more preferably within a range of 0.1 to 1% by mass, based on the total mass of the thermoplastic resin.

[0271] (Coloring agent) By including a colorant, the color can be adjusted. The term "colorant" refers to dyes and pigments. The colorant may be any of a variety of dyes and pigments, with anthraquinone dyes, azo dyes, phthalocyanine pigments, and the like being preferred.

[0272] (UV absorber) By including an ultraviolet absorbing agent, an ultraviolet absorbing function can be imparted to the raw film.

[0273] The ultraviolet absorbing agent is not particularly limited, and examples thereof include ultraviolet absorbing agents based on benzotriazole, 2-hydroxybenzophenone, and salicylic acid phenyl ester. Examples include triazoles such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, and 2-(3,5-di-t-butyl-2-hydroxyphenyl)benzotriazole; and benzophenones such as 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 2,2'-dihydroxy-4-methoxybenzophenone. These may be contained alone or in combination of two or more.

[0274] The content of the ultraviolet absorber is preferably adjusted appropriately depending on the type of ultraviolet absorber, the conditions of use, etc. For example, it is preferably within a range of 0.05 to 10 mass %, and more preferably within a range of 0.1 to 5 mass %, relative to the total mass of the thermoplastic resin.

[0275] (fine particles) By including the fine particles, slipperiness can be imparted to the raw film. In particular, the lubricity of the surface of the raw film is improved, and the lubricity during winding is improved, thereby making it possible to suppress the occurrence of scratches and blocking.

[0276] The fine particles may be either inorganic or organic as long as they do not impair the transparency of the raw film and have heat resistance when melted, but inorganic fine particles are more preferred. These may be contained alone or in combination of two or more.

[0277] By using particles of different particle sizes and shapes, for example, needle-like and spherical particles, it is possible to achieve both high transparency and lubricity.

[0278] Among these, the fine particles are preferably silicon dioxide, which has a refractive index close to that of the above-mentioned cycloolefin resins, acrylic resins, cellulose esters, etc., and is excellent in transparency (haze).

[0279] Specific examples of silicon dioxide include "Aerosil (registered trademark) 200V", "Aerosil (registered trademark) R972V", "Aerosil (registered trademark) R972, R974, R812, 200, 300, R202, OX50, TT600, NAX50" (all manufactured by Nippon Aerosil Co., Ltd.), "Seahoster (registered trademark) KEP-10", "Seahoster (registered trademark) KEP-30", "Seahoster (registered trademark) KEP-50" (all manufactured by Nippon Shokubai Co., Ltd.), "Silohovic (registered trademark) 100" (manufactured by Fuji Silysia Co., Ltd.), "Nipseal (registered trademark) E220A" (manufactured by Nippon Silica Kogyo Co., Ltd.), "Admafine (registered trademark) SO" (manufactured by Admatechs Co., Ltd.), and the like.

[0280] The shape of the particles is not particularly limited and may be amorphous, acicular, flat, spherical, etc. Among them, spherical particles provide excellent transparency of the raw film.

[0281] If the particle size is close to the wavelength of visible light, the light will be scattered and transparency will be poor, so the particle size is preferably smaller than the wavelength of visible light, and more preferably 1 / 2 or less of the wavelength of visible light.

[0282] From the viewpoint of lubricity, the particle size is preferably within the range of 80 to 180 nm. The term "particle size" refers to the size of the aggregate when the particle is an aggregate of primary particles, and refers to the diameter of a circle equivalent to the projected area of ​​a particle when the particle is not spherical.

[0283] The content of the fine particles is preferably within a range of 0.05 to 10% by mass, and more preferably within a range of 0.1 to 5% by mass, based on the total mass of the thermoplastic resin.

[0284] (2) How to make the original film The method for producing the raw film is not particularly limited, and any conventionally known method can be used. The method for producing the raw film preferably includes a raw film forming step (S1), a trimming step (S2), and a winding step (S3). The film may be formed by a solution casting method or a melt casting method. Each method will be described below.

[0285] (2.1) Solution casting method 3 is a schematic diagram of an apparatus for producing a film by a solution casting film-forming method.

[0286] (2.1.1) Raw film formation process (S1) (2.1.1.1) Preparation of dope In the film forming step (S1), first, at least a resin and a solvent are stirred in a stirring tank 1a of a stirring device 1 to prepare a dope to be cast onto a support 3 (endless belt).

[0287] Hereinafter, as one embodiment of the present invention, a case where a dope containing a cycloolefin resin (COP) as a thermoplastic resin is prepared will be described, although the present invention is not limited thereto.

[0288] In a dissolving vessel, COP and possibly other compounds are dissolved in a solvent mainly consisting of a good solvent for COP while stirring to prepare a dope. Alternatively, a COP solution and possibly other compound solutions are mixed to prepare a dope, which is a main solution.

[0289] (Resin concentration) The concentration of COP in the dope is preferably high because the load on drying after casting on the support can be reduced. Also, by not making the concentration of COP too high, the load on filtration can be suppressed and the accuracy of filtration can be maintained. The concentration of COP is preferably within the range of 10 to 35% by mass, and more preferably within the range of 15 to 30% by mass.

[0290] (solvent) As the above-mentioned solvent, a mixed solvent of a good solvent and a poor solvent is used. The solvent used in the dope may be one kind or two or more kinds. It is preferable to use a mixture of a good solvent and a poor solvent for COP from the viewpoint of production efficiency, and it is preferable to use a large amount of the good solvent from the viewpoint of solubility of COP.

[0291] The mixing ratio of the good solvent to the poor solvent is preferably within a range of 70 to 98 mass % of the good solvent, and more preferably within a range of 2 to 30 mass % of the poor solvent. In the present invention, the terms "good solvent" and "poor solvent" refer to a solvent that dissolves COP alone, and a poor solvent that swells or does not dissolve COP alone. Therefore, the good solvent and the poor solvent vary depending on the average degree of substitution of COP.

[0292] The good solvent used in the present invention is not particularly limited, and examples thereof include organic halogen compounds such as methylene chloride, dioxolanes, acetone, methyl acetate, methyl acetoacetate, etc. Among these, methylene chloride or methyl acetate is preferred.

[0293] The poor solvent used in the present invention is not particularly limited, and examples thereof include methanol, ethanol, n-butanol, cyclohexane, and cyclohexanone. The content of water in the dope is preferably within the range of 0.01 to 2% by mass.

[0294] The solvent used to dissolve the COP is removed from the film by drying in the film formation process and then recovered and reused.

[0295] The recovered solvent may contain trace amounts of additives added to the COP, such as plasticizers, ultraviolet absorbers, etc. However, even if these are contained, the recovered solvent can be preferably reused, and if necessary, it can be purified and reused.

[0296] The COP can be dissolved in the dope by a general method. Specifically, the method is preferably carried out at normal pressure, at or below the boiling point of the main solvent, or under pressure at or above the boiling point of the main solvent. By combining heating and pressure, it is possible to heat to or above the boiling point at normal pressure.

[0297] A method of dissolving the mixture by stirring while heating at a temperature equal to or higher than the boiling point of the solvent at normal pressure and within a range in which the solvent does not boil under pressure is also preferred. This method can prevent the formation of lumpy undissolved matter called gels or lumps.

[0298] A method in which the COP is mixed with a poor solvent to wet or swell it, and then a good solvent is further added to dissolve it is also preferably used.

[0299] Pressurization may be performed by injecting an inert gas such as nitrogen gas or by increasing the vapor pressure of the solvent by heating. Heating is preferably performed from the outside, and for example, a jacket type is preferred because it is easy to control the temperature.

[0300] From the viewpoint of solubility of COP, a higher heating temperature is preferable, but by not setting the heating temperature too high, the pressure does not become too high and productivity can be maintained.

[0301] The heating temperature is preferably within the range of 30 to 120°C, more preferably within the range of 60 to 110°C, and further preferably within the range of 70 to 105°C. The pressure is adjusted so that the solvent does not boil at the set temperature.

[0302] Alternatively, a cooling dissolution method can be preferably used, in which COP can be dissolved in a solvent such as methyl acetate.

[0303] (Filtration) Next, the dope in which the COP is being dissolved or after it has been dissolved is preferably filtered using a suitable filter material such as filter paper.

[0304] The filter preferably has a small absolute filtration accuracy from the viewpoint of removing insoluble matters, etc. Also, by not making the absolute filtration accuracy too small, clogging of the filter can be suppressed. For this reason, the absolute filtration accuracy of the filter material is preferably 0.008 mm or less, more preferably within the range of 0.001 to 0.008 mm, and even more preferably within the range of 0.003 to 0.006 mm.

[0305] The material of the filter is not particularly limited, and a general filter can be used. For example, a filter made of a plastic such as polypropylene or Teflon (registered trademark), or a filter made of a metal such as stainless steel is preferable because it prevents fibers from falling off.

[0306] It is preferable to remove or reduce impurities, particularly bright spot foreign matter, contained in the raw COP by filtration.

[0307] "Bright spot foreign matter" refers to a point (foreign matter) that appears as light leaking from the opposite side when two polarizing plates are placed in a crossed Nicol state, a film or the like is placed between them, and light is applied from one polarizing plate side and observed from the other polarizing plate side. The diameter of the bright spot foreign matter is 0.01 mm or more. The number of bright spots is 200 / cm. 2 It is preferable that the number of particles is less than 100 / cm. 2 More preferably, it is 50 pieces / m or less. 2 More preferably, it is 0 to 10 particles / cm or less. 2 It is particularly preferred that: It is also preferable to have fewer bright spots of 0.01 mm or less.

[0308] The dope can be filtered by a general method. Among them, the method of filtering the dope while heating it at a temperature above the boiling point of the solvent at normal pressure and within a range where the solvent does not boil under pressure is preferred. This method can reduce the difference in filtration pressure before and after filtration, i.e., the increase in differential pressure.

[0309] The heating temperature is preferably within the range of 30 to 120°C, more preferably within the range of 45 to 70°C, and even more preferably within the range of 45 to 55°C.

[0310] A smaller filtration pressure is preferred. Specifically, the filtration pressure is preferably 1.6 MPa or less, more preferably 1.2 MPa or less, and even more preferably 1.0 MPa or less.

[0311] (2.1.1.2) Dope casting The dope cast on the support 3 is fed to the casting die 2 through a conduit via a pressure type metering gear pump or the like. The dope is cast from the casting die 2 to a casting position on the support 3. The support 3 is an endless belt made of stainless steel that is rotated and moves infinitely.

[0312] At this time, the inclination of the casting die 2, i.e., the direction of the dope discharged from the casting die 2 to the support 3, is an angle with respect to the normal line of the surface of the support 3 (the surface onto which the dope is cast), and is preferably set appropriately to be within a range of 0 to 90°. Then, the casting film 5 is heated on the support 3 until the casting film 5 can be peeled off from the support 3 by the peeling roller 4, and the solvent is evaporated. The casting film 5 after being solidified and becoming peelable is called "original film".

[0313] (Solvent evaporation method) The evaporation is preferably carried out in an atmosphere within a range of 5 to 75°C. Examples of methods for evaporating the solvent include a method of applying hot air to the upper surface of the casting film, a method of transferring heat from the back surface of the support 3 using a liquid, a method of transferring heat from the front and back using radiation heat, etc. Among them, the method of transferring heat from the front and back using radiation heat is preferred because of its high drying efficiency. These methods may also be combined.

[0314] (Casting width) From the viewpoint of productivity, the casting width is preferably 1.3 m or more, and more preferably within the range of 1.3 to 4.0 m. By setting the casting width to 4.0 m or less, it is possible to prevent stripes from appearing in the raw film forming process, and it is possible to increase stability in the subsequent transport process. From the viewpoint of transportability and productivity, the casting width is more preferably within the range of 1.3 to 3.0 m.

[0315] (Support) The support 3 for casting the dope preferably has a mirror-finished surface. The support 3 is held by a pair of rollers 3a and 3b and a number of rollers positioned between them.

[0316] One or both of the rollers 3a and 3b are provided with a drive device that applies tension to the support 3, so that the support 3 is used in a tensioned state. As the support 3, a stainless steel belt or a cast drum with a plated surface is preferably used.

[0317] The surface temperature of the support 3 during casting of the dope is preferably in the range of -50°C or more and the boiling point of the solvent or less. A higher temperature is preferable because the drying speed of the casting film can be increased. The temperature of the support is preferably in the range of 0 to 55°C, more preferably in the range of 22 to 50°C.

[0318] The method for controlling the temperature of the support 3 is not particularly limited, and examples thereof include a method of blowing hot or cold air or a method of bringing hot water into contact with the back side of the support. The method using hot water is preferable because heat is efficiently transferred, and therefore the time required for the temperature of the support to become constant is short. When using hot air, air at a temperature higher than the desired temperature may be used.

[0319] <Means for controlling film thickness in the raw film forming process> In the method for producing the raw film, it is preferable to control the film thickness. The maximum height difference (PV) of the longitudinal average film thickness at each width position of the film thickness value is preferably within the range of 0.02 to 0.40 μm. The longitudinal average film thickness at each width position of the film thickness value can be measured in a diagonal direction relative to the width direction of the original film by the following steps 1 to 3.

[0320] Step 1: Measure the film thickness at any position on the edge of the film. After that, for each measurement, measure the film thickness at a position 10 mm in the width direction and 30 mm in the length direction from the arbitrary position. Record the width position, length position, and film thickness value, and repeat the process to the other edge of the film. Step 2: After the end of step 1, measurements similar to those in step 1 are carried out until the total distance of the movement positions in the longitudinal direction reaches 1000 m. Step 3: From the multiple thickness data obtained in steps 1 and 2, the thickness values ​​at the same widthwise position are averaged to obtain the longitudinal average thickness value at each widthwise position. From these, the height difference (PV) between the maximum and minimum values ​​is calculated.

[0321] In the process of forming the raw film, the maximum difference in height (PV) of the longitudinal average film thickness can be adjusted, for example, by the following three film thickness control means. In addition, the maximum difference in height (PV) of the longitudinal average film thickness can also be adjusted in the convex portion adjustment process described later. These methods may be combined to control the film thickness.

[0322] (Film thickness control means 1: pump pulsation pitch control) The film thickness is controlled by controlling the pitch of the pump pulsation. It is known that a high-precision gear pump is used to transport the dope in the piping leading to the casting die (to extrude the resin in the case of melting). The gear ratio of the gear pump controls the pump rotation speed, thereby controlling the pitch of the pump pulsation. The pulsation during the transport has a large effect on the longitudinal film thickness and the average maximum height difference (PV) of the longitudinal average film thickness.

[0323] Here, a supplementary explanation will be given regarding the liquid delivery capacity of the pump. In casting the dope, if the length of the piping from the pump to the casting die is not too short, the pulsation does not become large due to the influence of the rotation speed of the pump. If the length of the piping is not too long, the pressure loss can be suppressed, and the liquid delivery capacity of the pump can be prevented from decreasing below the lower limit. If the rotation speed of the pump is not too slow, the liquid delivery capacity can be prevented from decreasing. If the rotation speed is not too fast, the pressure loss can be suppressed, and the liquid delivery capacity can be prevented from decreasing.

[0324] From the above viewpoints, the length of the pipe from the pump to the casting die is preferably within the range of 50 to 100 m. In addition, the gear ratio of the gear pump used for sending the dope (extrusion of the resin in the case of melting) is adjusted. This allows the rotation speed of the pump to be adjusted within the range of 10 to 50 rpm.

[0325] (Film thickness control means 2: Film thickness control by heat bolt) The initial film thickness is controlled by the heat bolt of the casting die. In casting a dope, in both the solution casting film-forming method and the melt casting film-forming method, a method for improving the uniformity of the film thickness includes controlling the slit gap at the lip portion of the casting die.

[0326] For example, when a highly viscous dope (including melt) is extruded, the slit gap varies in the width direction. To prevent this, a plurality of heat bolts are installed in the width direction to control the slit gap. However, there is a physical limit to the number of heat bolts that can be installed.

[0327] In order to suppress the pressure fluctuation in the width direction, which causes the slit gap to vary in the width direction, there is a method of changing the internal structure of the casting die in the width direction. However, this requires changing the casting die for each production type, which is time-consuming and costly. The casting die is provided with a mechanism for adjusting a slit for discharging the dope (extruding the resin in the case of melting) in the width direction.

[0328] Here, a method for controlling the initial thickness of the cast film by adjusting the width direction of the slit through which the dope is discharged using the heat bolt of the casting die will be described. In casting the dope, if the gap in the width direction of the slit through which the dope is discharged by the heat bolt of the casting die is not too small, the film thickness can be easily controlled and the time can be shortened. If the gap in the width direction of the slit through which the dope is discharged is not too large, the initial discharged film thickness of the casting film can be made uniform.

[0329] The thickness deviation immediately after extrusion is preferably within a range of 1.0 to 5.0% with respect to the entire cast film, and it is preferable to control the initial extrusion thickness of the cast film.

[0330] The part of the casting die slit where the dope comes out is called the "lip". The shape of the slit at the lip can be adjusted, and it is preferable that the casting die is one that can easily make the film thickness uniform. Examples of the casting die include a coat hanger die and a T-die, and any of them is preferably used. In the present invention, the term "cast film" refers to the dope film cast from the lip portion.

[0331] In order to increase the film-forming speed of the raw film, two or more of the above-mentioned casting dies may be provided on the support, and the amount of the dope may be divided and layered. Also, a raw film having a laminated structure may be formed by a co-casting method in which a plurality of dopes are simultaneously cast.

[0332] The slit can be narrowed by manually turning and pushing the heat bolt, making the film thinner. Conversely, the slit can be opened to make the film thicker. Generally, the film is pushed in by applying a voltage to the heat bolt. Usually, a combination of manual pushing and voltage pushing is used. Pushing and pulling can also be used.

[0333] Due to the mechanism of the casting die, the pitch of the bolts may not be narrowed. In this case, the pressure load on the lip of the casting die is large when the dope (including the melt) has high viscosity, and the load drops suddenly after the dope is discharged, causing the film thickness to increase (balance effect). This may cause the film thickness to vary across the width. Therefore, it is necessary to design the internal structure of the casting die so that the load on the lip of the casting die is not too high.

[0334] (Film thickness control means 3: Film thickness control by hot air) Hot air is blown onto the cast film, and the heat is used to flatten the protrusions, thereby controlling the film thickness. The air may be blown on the surface of the opposite side of the casting film to the belt while the dope is being cast, or the hot air may be blown on the surface of the opposite side of the casting film immediately after the casting film is peeled off from the belt.

[0335] The inside of the casting film contains the solvent and is soft, so the protrusions can be flattened. Specifically, the film thickness is controlled by measuring the nonuniformity of the casting film in the width direction online and adjusting the temperature, speed, and amount of the drying air to adjust the amount of the residual solvent.

[0336] The temperature, velocity, and amount of the drying air, and the amount of residual solvent will now be explained in more detail. The film thickness can be controlled by setting the temperature, speed and volume of the drying air to a certain value or higher. Also, the film thickness can be prevented from becoming locally uncontrollable by setting the temperature, speed and volume of the drying air to a certain value or lower.

[0337] By making the residual solvent amount equal to or more than a certain value, the casting film can be made soft and can be flattened. Also, by making the residual solvent amount equal to or more than a certain value, the film thickness is less likely to vary during flattening. In other words, by adjusting the residual solvent amount, flattening 3 can be performed with a thin film formed on the surface.

[0338] From the above viewpoints, the temperature of the drying air is preferably within the range of 10 to 80° C., and the air speed is preferably within the range of 5 to 40 m / sec. The amount of residual solvent is preferably within a range of 150 to 550% by mass.

[0339] If the above operation is performed when the surface layer of the casting film on the opposite side of the belt is not yet formed into a film, streaks are likely to occur. In addition, it is preferable that the inside of the casting film contains a solvent and is soft. On the belt during casting of the dope, the non-uniformity of the film thickness deviation in the width direction of the casting film is measured online. It is preferable to adjust the temperature when blowing hot air to control the film thickness so as to reduce the non-uniformity.

[0340] (2.1.1.3) Peeling off the original film On the support 3, the solvent is evaporated until the casting film 5 has a film strength that allows peeling, and the film is dried and solidified or cooled and solidified. Then, before the original film makes one revolution around the support 3, the original film is peeled off from the support 3 by a peeling roller 4 while maintaining self-supporting property. The casting film 5 after being solidified and becoming peelable is called "original film".

[0341] From the viewpoints of surface quality, moisture permeability and peelability, it is preferable to peel the original film from the support within a range of 30 to 600 seconds. The position where the film is peeled from the support is called the "peeling point", and the roller that assists the peeling is called the "peeling roller".

[0342] The temperature at the peeling position on the support is preferably within the range of -50 to 40°C, more preferably within the range of 10 to 40°C, and further preferably within the range of 15 to 30°C.

[0343] (Residual solvent amount when film is peeled off) The amount of solvent remaining in the original film on the support 3 at the time of peeling is appropriately adjusted depending on the strength of the drying conditions, the length of the support 3, and the like.

[0344] Although it depends on the thickness of the original film, by making the amount of residual solvent at the peeling point below a certain amount, the original film is not too soft and is easy to peel off. In addition, the flatness of the original film is improved, and the occurrence of horizontal buckling, creases, and vertical streaks due to peeling tension can be suppressed. By making the amount of residual solvent above a certain amount, it is possible to suppress the peeling of part of the original film. From the viewpoint of flatness of the raw film, the amount of residual solvent is preferably within a range of 10 to 50% by mass.

[0345] As a method for increasing the film-forming speed, there is a gel casting method, which allows peeling even when the residual solvent amount is large. By peeling while the residual solvent amount is as large as possible, the film-forming speed can be increased. Specifically, a method of adding a poor solvent for cycloolefin resin (COP) to the dope, and gelling the casting film after casting the dope can be mentioned. In addition, a method of gelling the casting film by cooling the support and peeling it off in a state containing a large amount of residual solvent can be mentioned. In addition, a metal salt can be added to the dope. As described above, the cast film is gelled on the support to strengthen the film, thereby facilitating peeling and increasing the film production rate.

[0346] The residual solvent amount is defined by the following formula. Residual solvent amount [mass%] = {(MN) / N} x 100 Here, M is the mass of a sample taken from the cast film or the raw film at any time during or after the production, and N is the mass of the sample with mass M after heating at 115°C for 1 hour.

[0347] (peel tension) The peel tension when peeling the support and the film is preferably 300 N / m or less, more preferably in the range of 196 to 245 N / m. If wrinkles are likely to occur during peeling, peeling is preferably performed with a tension of 190 N / m or less.

[0348] (2.1.1.4) Shrinkage within the plane of the original film The original film after peeling from the support is stretched by applying tension in the machine direction (hereinafter also referred to as "MD") to shrink it. In this case, the original film shrinks in the transverse direction (hereinafter also referred to as "TD") perpendicular to the MD within the plane of the original film.

[0349] The above operation promotes entanglement between polymer molecules (matrix molecules) in the thickness direction of the original film. For example, when an optical film is bonded to another film via an adhesive, the adhesive is likely to penetrate into the film via the entangled parts (crosslinked parts) between the matrix molecules. As a result, the optical film can be firmly fixed to the other film via the adhesive. In other words, the adhesion between the optical film and the other film can be improved.

[0350] Other methods for shrinking the raw film include, for example, a method of treating the raw film at a high temperature without holding the width of the raw film to increase the density of the raw film, and a method of rapidly reducing the amount of residual solvent in the raw film.

[0351] (Film shrinkage rate) In the present invention, the shrinkage rate is defined by the following formula.

[0352] Shrinkage rate [%] = film width after shrinkage [mm] / film width at start of shrinkage [mm] x 100

[0353] The shrinkage rate of the raw film is preferably within a range of 1 to 40%, and more preferably within a range of 5 to 20%. By keeping it within the above range, entanglement between matrix molecules is promoted. Also, a decrease in the production efficiency of the film can be suppressed.

[0354] (Method of measuring and calculating shrinkage rate) In the present invention, the width of the raw film was measured using "LS-9000" (manufactured by Keyence Corporation). The shrinkage rate of the original film was calculated by measuring the width of the original film every second for 5 minutes (300 seconds) using the above measuring device, taking the average value of each measurement, and substituting it into the above formula. However, the method is not limited to the above, and for example, the width of the original film may be read using a ruler, and used as the width of the original film, and then substituted into the above formula.

[0355] (2.1.1.5) Drying of Raw Film The raw film is heated on the support by the drying device 6 to evaporate the solvent, thereby further drying the raw film. The support may be at the same temperature all over, or the temperature may vary depending on the position.

[0356] Methods for drying raw film include a roller drying method in which the raw film is dried by passing it alternately between multiple rollers arranged above and below, and a tenter method in which the raw film is dried while being transported.

[0357] The tenter stretching apparatus is preferably an apparatus capable of independently controlling the left and right gripping lengths of the raw film by the left and right gripping means. The "grip length" refers to the distance from the gripping start to the gripping end.

[0358] In drying device 6 in FIG. 3, the film is transported by a plurality of transport rollers arranged in a staggered pattern when viewed from the side, and the film is dried during this transport. The drying method in the drying device 6 is not particularly limited, and for example, the raw film is dried using hot air, infrared rays, a heated roller, microwaves, etc. From the viewpoint of simplicity, a method of drying the film with hot air is preferred. These drying methods may also be combined. The above operations may be performed as necessary.

[0359] If the film is thin, it dries quickly, but rapid drying can easily damage the flatness of the finished raw film, so it is preferable to allow a certain amount of drying time.

[0360] (Residual solvent amount when film is dried) When drying at high temperatures, it is necessary to take into consideration the amount of residual solvent. If the amount of residual solvent is not too high, breakdowns due to solvent foaming can be prevented. The amount of the residual solvent is preferably 30% by mass or less. Throughout, the drying temperature is preferably within a range of 30 to 250° C., and more preferably within a range of 35 to 200° C. It is preferable to increase the drying temperature in stages.

[0361] The amount of residual solvent in the original film on the support 3 when the original film is peeled off is appropriately adjusted depending on the strength of the drying conditions, the length of the support 3, etc. Since the shrinkage within the plane of the original film and the amount of residual solvent in the drying of the original film are significantly affected by the film thickness, resin, etc., it is preferable to appropriately adjust them.

[0362] (2.1.2) Trimming process (S2) In the trimming step (S2), a cutting unit 8 consisting of a slitter cuts (trims) both ends of the original film in the width direction. It is preferable not to oscillate the original film prior to the above trimming. In this specification, the term "oscillate" refers to moving the original film itself in the width direction.

[0363] The cut portions of the original film may be collected and reused as part of the raw material for producing the original film. It is also possible to subject the raw film to knurling after the trimming step, however, from the viewpoint of suppressing excessive air entrapment, it is preferable not to subject the raw film to knurling after the trimming step.

[0364] (2.1.3) Winding process (S3) In the winding step (S3), the raw film is wound by a winding device 13 to obtain a raw film roll. That is, in the winding step, the raw film is wound around a core while being transported, thereby producing a raw film roll. The initial tension when winding the film in the winding step is preferably within a range of 20 to 300 N / m.

[0365] (Residual solvent amount just before winding) Specifically, this is a step in which the raw film is wound up by a winding device 12 after the amount of residual solvent in the raw film becomes 2% by mass or less. Furthermore, by keeping the amount of residual solvent to 0.4% by mass or less, raw film with good dimensional stability can be obtained. In particular, it is preferable to wind up the raw film when the amount of residual solvent is within the range of 0.00 to 0.20% by mass.

[0366] (Winding method) The raw film may be wound up using a commonly used winder. There are several tension control methods, such as the constant torque method, constant tension method, taper tension method, and program tension control method with constant internal stress, and any of these may be used appropriately.

[0367] Before winding, the ends of the film are slit and cut to an appropriate width, and a surface modification treatment may be applied to both ends of the film to prevent sticking or scratches during winding.

[0368] (After winding) The raw film roll is preferably a long film, specifically, preferably in the range of 100 to 10,000 m. Usually, it is provided in a roll form.

[0369] <Details of film winding method> The raw film is preferably wound up by the following winding method. The winding method preferably includes a straight winding step of winding the original film around a core so that the side edges of the original film are aligned. After the straight winding step, the original film or the core is periodically vibrated in the width direction of the original film so that the side edges are periodically shifted within a certain range relative to the width direction of the original film. Then, the method preferably includes an oscillating winding step of winding the original film around the core.

[0370] It is preferable to switch from the straight winding process to the oscillating winding process when the winding length of the original film reaches a switching winding length that is predetermined within a range of 1 to 30% of the total winding length of the original film.

[0371] The winding device for the original film includes a winding unit for winding the original film around the core by rotating the core. The winding device also includes an oscillation unit for vibrating the original film or the core in the width direction of the original film in conjunction with the winding of the original film so as to achieve oscillatory winding. It is preferable that the winding device further includes a switching unit for switching the winding of the original film from straight winding to oscillatory winding when the winding length of the original film reaches a predetermined switching winding length. Hereinafter, details regarding the oscillator winding will be omitted.

[0372] FIG. 12 is a schematic diagram showing the process of winding a film and a cross section of the film roll according to the present invention after winding. In FIG. 11, the formed film 31 is wound around a roll 32 and a touch roll 33 , and taken up as a film roll 30 .

[0373] (2.2) Melt casting film method The raw film can also be formed by a melt casting film forming method. The "melt casting film-forming method" refers to a method in which a composition containing a thermoplastic resin and the above-mentioned additives is heated to a temperature at which the composition exhibits fluidity and then melted, and the melt containing the fluid thermoplastic resin is cast.

[0374] Examples of molding methods involving heating and melting include melt extrusion molding, press molding, inflation molding, injection molding, blow molding, and stretch molding. Among these, the melt extrusion method is preferred from the viewpoints of mechanical strength, surface accuracy, and the like.

[0375] The process flow of the melt casting film-forming method will be described below in the same manner as the process flow of the solution casting film-forming method described above with reference to FIG. FIG. 13 is a schematic diagram of an apparatus for producing a raw film by the melt casting film-forming method. The solution casting film-forming method will be described below with reference to FIG. 2 and FIG.

[0376] The method for producing a raw film by the melt casting film forming method includes a raw film forming step (S1), a trimming step (S2), and a winding step (S3).

[0377] (2.2.1) Raw film formation process (S1) (2.2.1.1) Melt extrusion of resin At least the resin is melt-extruded by the extruder 14 and molded onto a cast drum 16. The resin is preferably kneaded and pelletized in advance, and the pelletization may be performed by a known method.

[0378] For example, dry resin, plasticizer, and other additives are fed into an extruder with a feeder and mixed using a single-screw or twin-screw extruder. The mixture is extruded in the form of a strand from a casting die, cooled with water or air, and cut into pellets.

[0379] The additives may be mixed with the resin before being fed to the extruder, or the additives and the resin may be fed to the extruder by separate feeders. It is preferable to mix small amounts of additives such as particles and antioxidants with the resin in advance in order to mix them uniformly.

[0380] When the pellets are introduced from the supply hopper into the extruder, it is preferable to prevent oxidative decomposition and the like by drying, placing them under a vacuum or reduced pressure, or placing them under an inert gas atmosphere.

[0381] It is preferable that the extruder is operable to process at a temperature as low as possible while still being capable of pelletizing in order to suppress shearing force and prevent deterioration of the resin (reduction in molecular weight, coloration, gel formation, etc.).

[0382] For example, in the case of a twin-screw extruder, it is preferable to use deep-groove type screws and rotate them in the same direction. From the viewpoint of uniformity of kneading, it is preferable to use intermeshing type screws. It is preferable to filter the pellets with a leaf disk type filter or the like when melted to remove foreign matter.

[0383] The pellets thus obtained are used to produce a raw film. Of course, it is also possible to feed the raw resin material (powder, etc.) directly to an extruder using a feeder without pelletizing, and to produce a raw film directly.

[0384] (2.2.1.2) Casting and molding of molten resin "Resin" as used herein includes pellets. The molten resin is passed through a pressure type metering gear pump or the like and cast into a film form from a casting die 15 through a conduit. The molten resin is cast from the casting die 15 onto a casting position on a rotating stainless steel endless casting drum 16 that moves infinitely. The cast molten resin is then molded on the casting drum 16 to form a raw film.

[0385] The inclination of the casting die 15, i.e., the direction in which the molten resin is discharged from the casting die 15 to the support 16, may be appropriately set within a range of 0 to 90° with respect to the normal to the surface of the cast drum 16 (the surface on which the molten resin is cast).

[0386] The touch roller 16a and the cooling drum 17 that assists the cast drum 16 may be used alone or in combination as appropriate to form the raw film.

[0387] The thickness control means and other matters in the raw film forming process are the same as those in the raw film manufacturing process by the solution casting film forming method. The description of the residual solvent amount, shrinkage rate, drying method, etc. is omitted because they are redundant.

[0388] (2.2.2) Trimming process (S2) In the trimming step (S2), a cutting unit 20 consisting of a slitter cuts (trims) both ends of the original film in the width direction. The portion cut from the original film may be collected and reused as part of the raw material for producing the original film. It is also possible to subject the raw film to knurling after the trimming step, however, from the viewpoint of suppressing excessive air entrapment, it is preferable not to subject the raw film to knurling after the trimming step.

[0389] (2.2.3) Winding process (S3) Finally, in the winding step (S3), the original film is wound by the winding device 23 to obtain an original film roll. That is, in the winding step, the original film is wound around a core while being transported, thereby producing a film roll. The raw film may be wound up using a commonly used winder. For example, tension control methods such as a constant torque method, a constant tension method, a taper tension method, and a program tension control method with constant internal stress may be used.

[0390] (3) Method of stretching in the next process In the present invention, the next step, that is, the method of processing the raw film, is not particularly limited. As an example of the processing, stretching processing will be described. First, the meanings of major terms used in the present invention will be explained below.

[0391] <Definition of terms related to convex parts> In the present invention, the term "protruding portion" refers to a portion in which the height of the peaks and valleys of the uneven shape of the film thickness measured and observed by film thickness measurement is higher than the average film thickness, that is, is thicker. The term "film" used herein refers to raw film or optical film. The details are as follows:

[0392] The condition of the convex parts is measured and evaluated by measuring the film thickness at an arbitrary position on the edge of the film. After that, the film thickness is measured at a position moved 10 mm in the width direction and 30 mm in the length direction from the arbitrary position for each measurement. This is repeated up to the other edge of the film, and noise is removed by Gaussian filter processing. A film thickness profile in the width direction is obtained, and the condition of the convex parts is measured and evaluated based on the profile.

[0393] In the present invention, the term "film edge" refers to a region within a range of 15 to 30 mm inward from the end of the film (roll) in the width direction. The term "film roll" refers to a film wound in a roll shape.

[0394] (Number of protrusions) The average thickness is determined by averaging the measured values ​​of each thickness in the width direction. As shown in Figure 1, a part where the thickness profile in the width direction is thicker than the average thickness and continues for 50 mm or more in the width direction is defined as a convex part. The number of such parts is defined as the number of convex parts. By not making the number of protrusions too large, each peak is not sharp, and deformation of the film is unlikely to occur. Also, by not making the number of protrusions too small, excessive stress concentration on the protrusions during film winding is prevented, and twisting and the like is unlikely to occur. The number of protrusions is preferably within a range of 1 to 10 per meter in the width direction.

[0395] (Position and height of protrusion) In addition, for each convex portion determined by the above method, the position where the maximum value is reached is defined as the position of the convex portion, and the value obtained by subtracting the average film thickness in the width direction from the maximum value of the convex portion is defined as the height h of each convex portion. By not making the height of the protrusions too high, it is possible to prevent the formation of chains at the base of the film after the film roll is left for a long time, and by not making the height of the protrusions too low, the film thickness dispersion effect is achieved.

[0396] The height of the convex portions is preferably within a range of 0.05 to 0.50 μm. The positions of the protrusions are adjusted so that they move continuously in the longitudinal direction of the film surface, which prevents the protrusions from overlapping with each other when the film is wound up, thereby enhancing the effectiveness of the aforementioned function of adjusting the number and height of the protrusions.

[0397] The film thickness can be measured, for example, by using an in-line retardation / film thickness measuring device "RE-200L2T-Rth+film thickness" (manufactured by Otsuka Electronics Co., Ltd.).

[0398] (3.1) Convexity adjustment process (3.1.1) Overview of the convex portion adjustment process The step of preparing the convex portions in the width direction of the film surface is a step of adjusting the number, height and position of the convex portions. By locally heating the film, the number of convex portions is preferably adjusted to within a range of 1 to 10 per meter in the width direction. In addition, the height of the convex portions is preferably adjusted to within a range of 0.05 to 0.50 μm. Furthermore, it is preferable to adjust the positions of the convex portions so that they move continuously in the longitudinal direction of the film surface.

[0399] As a means for adjusting the convex portions, it is preferable to locally heat the raw film. Examples of localized heating means include infrared (IR) heaters and hot air. The heat treatment method is not particularly limited, and other methods may be used for heat treatment. The advantage of the hot air method is that it has sufficient film thickness adjustment capability regardless of the material.

[0400] On the other hand, although it is somewhat difficult to control the continuous movement of the peaks and valleys, it is possible to move the convex portions continuously by appropriately controlling the temperature, air volume, nozzle pressure, etc. From the viewpoints of film thickness controllability and stability, it is preferable to perform localized heating using infrared heaters arranged in the width direction and length direction of the original film.

[0401] In the convex portion adjustment step, the raw film is stretched in a stretching device while being locally heated. For example, the in-line retardation / film thickness measuring device "RE-200L2T-Rth+film thickness" (manufactured by Otsuka Electronics Co., Ltd.) is used to measure the film thickness profile in the width direction of the target raw film. Then, the set temperature of each infrared heater is calculated on a computer from the difference with the target film thickness profile. The set temperature of each heat source is output via the programmable controller "PLC KV-8000" (manufactured by Keyence Corporation) to adjust the convex parts. This process is repeated automatically to automate film thickness adjustment.

[0402] (3.1.2) Stretching of raw film The raw film may be stretched only in the MD direction or only in the TD direction within the plane of the raw film. It may also be stretched in both the MD and TD directions, or may be stretched in an oblique direction. The stretching direction is not limited.

[0403] From the viewpoint of obtaining a wide film, it is preferable to stretch the film at least in the width direction. The stretching method may be a method of stretching in the conveying direction by setting a difference in peripheral speed of rollers. The conveying direction here is the longitudinal direction of the film, the film-forming direction, the casting direction, or the MD direction. Another example is a tenter method in which both side edges of the raw film are fixed with clips or the like and stretched in the width direction. The width direction here is the direction perpendicular to the film plane or the TD direction. By using these methods, the performance, productivity, flatness, dimensional stability, etc. of the optical film can be improved.

[0404] In the case of a tenter system, if the clip portion is driven by a linear drive system, the film can be stretched smoothly and the risk of breakage can be reduced.

[0405] (Stretching ratio) From the viewpoint of ensuring a high retardation and a wide width, it is preferable to stretch the raw film at a high ratio in the stretching process. However, if the stretching ratio is too high, crazes are likely to occur in the optical film due to stretching stress. In addition, entanglement between matrix molecules that maintain the strength of the optical film is likely to be dissociated, making the optical film vulnerable.

[0406] The stretching ratio of the raw film is preferably within the range of 1.1 to 5.0, and more preferably within the range of 1.3 to 3.0. When stretching is performed multiple times, the highest stretching ratio, which has the highest risk of dissociating the matrix molecules, is preferably performed in the final stretch.

[0407] (Residual Solvent Amount When Film Stretched) The amount of residual solvent in the raw film during stretching is preferably 20% by mass or less, and more preferably 15% by mass or less.

[0408] (3.1.3) Definitions of terms used in the convex portion adjustment process (Definition of terms related to convex parts) The definitions of terms relating to the convex portions have been described above and will not be repeated here.

[0409] (Continuity of the protrusion in the longitudinal direction: Adjustment of the position of the protrusion in the longitudinal direction) In the convex portion adjustment process, the positions of the convex portions are adjusted so as to move continuously in the longitudinal direction of the optical film surface. The positions of the convex portions are determined by the definition described below. When the positions of the convex portions are connected to each other, they form a substantially straight line as shown in Figures 4(a) and 4(b), for example. Alternatively, they form a curved line having a curvature that changes at a substantially constant rate of change as shown in Figure 4(c). In addition, in order to facilitate understanding of the present invention, the widths of the widthwise and longitudinal directions of Figs. 4(a), 4(b) and 4(c) are shown at different scales for convenience.

[0410] In other words, "moving continuously in the longitudinal direction of the film surface" means that when the positions of the protrusions are connected, a substantially straight line or a curved locus having a curvature that changes at a substantially constant rate of change is described. The substantially straight line or the curved line having a curvature that changes at a substantially constant rate of change may have periodicity. In addition, although Fig. 4(a), Fig. 4(b) and Fig. 4(c) show a series of periodic convex portions, the present invention is not limited to those having periodicity.

[0411] "Approximately a straight line" refers to a line that can be seen as substantially a straight line when the center points of each protrusion are plotted with the width direction of the film as the horizontal axis (x-axis) and the length direction of the film as the vertical axis (y-axis) as shown in Figure 5. Note that "substantially seen as a straight line" means that the plot of the center points of each protrusion is a straight line, excluding points that deviate from a straight line in the strict sense due to variations in the control conditions of the protrusion adjustment process and the properties of the film. When the approximate straight line is an approximation straight line obtained by the least squares method, it is preferable that the absolute value of the correlation coefficient of the linear expression expressing the approximate straight line is 0.8 or more. Moreover, the term "substantially constant rate of change" refers to a rate of change within the range of the average value ±10%.

[0412] (Inclination θ' of the approximately straight line relative to the longitudinal direction of the film surface) It is preferable to adjust the positions of the protrusions so that they are aligned in a substantially straight line in the longitudinal direction of the film surface by locally heating the film. It is preferable to prevent the film thickness profile from changing suddenly in the longitudinal direction of the film by controlling the positions of the protrusions. In other words, it is preferable to maintain the continuity of the protrusions. Moreover, it is preferable that the absolute value of the inclination of the approximately straight line is within a range of 0.01 to 0.6°.

[0413] The inclination θ′ of the approximately straight line with respect to the longitudinal direction of the film surface is determined as follows.

[0414] For example, the film thickness profile is measured using an in-line retardation / film thickness measurement device "RE-200L2T-Rth+film thickness" (manufactured by Otsuka Electronics Co., Ltd.) This and the position of the convex part calculated from the average film thickness are plotted as shown in Figure 5, with the width direction of the film as the horizontal axis (x-axis) and the length direction of the film as the vertical axis (y-axis).

[0415] When the position of a convex part at an arbitrary position on the edge of the film is P0(x0,y0), the coordinates of each of the other convex parts are P1(x1,y1), P2(x2,y2), . . . , P n (x n ,yn ) where n is an integer equal to or greater than 1.

[0416] FIG. 5 shows the resulting plot of the positions of the convex portions and the relationship with the approximate straight line. From the locus of the plotted convexity, the position of the convexity at any position on the edge of the film is set as P0(x0,y0)=P0(0,0). The slope of the approximation line obtained by the least squares method is set as a. Then, a straight line of the linear function y=ax (x and y are variables) is drawn, and the angle θ[°] corresponding to the slope a is found. The correlation coefficient R is 0.9 or more. In this case, the inclination θ′ [°] of the approximately straight line with respect to the longitudinal direction of the film surface is θ′ [°] = (90 - θ) [°].

[0417] (Heat source part E A and E B The average slope θ of the line connecting the E ') In the width direction of the film, the heat source parts of the infrared heaters are preferably arranged at intervals of 10 to 100 mm. The heat source parts are preferably arranged in the longitudinal direction of the film at positions different from the width direction. A and E B It is preferable that the average gradient θE′ of the line connecting the lines is within a range of 2 to 45° with respect to the longitudinal direction. By making the interval between the heat sources of the infrared heaters smaller, the profile can be adjusted more finely.

[0418] The infrared heaters on the film are regularly arranged in one or more rows in the longitudinal direction of the film, for example, as shown in Figures 6(a), (b) and (c). Note that in Figure 6(a), one row is arranged in the longitudinal direction of the film, in Figure 6(b), two rows are arranged in the longitudinal direction of the film, and in Figure 6(c), five rows are arranged in the longitudinal direction of the film.

[0419] In Fig. 6, P1, P2, and P3 represent the pitch of the heat source of each infrared heater. Here, each heat source of the infrared heater is located at the center of each infrared heater, as shown in Fig. 6(a), (b), and (c). The shape of the infrared heater is not limited, and examples of the shape of the heat source of the infrared heater include a dot shape, a line shape, a surface shape, and the like. Further, the "heat source part of the infrared heater" refers to the center part of the heat source part of the infrared heater, regardless of whether the shape of the infrared heater is point-like, linear, planar, or the like.

[0420] The infrared heater is preferably disposed at a position 30 to 120 mm away from the film surface. The heating width is preferably within a range of 100 to 250 mm. The heat source parts of the infrared heater are preferably installed at intervals within a pitch of 10 to 100 mm. The temperature of each heat source part of the infrared heater is preferably within a range of 100 to 1000 W and 180 to 350° C.

[0421] The positional relationship of each heat source will be specifically described below. Each heat source E A and E B The average slope of the line connecting E When calculating the heat source E A and E B The positional relationship between and is the closest positional relationship, with the coordinate positions in the width direction and the longitudinal direction being different (see FIG. 6).

[0422] Specifically, for example, the positional relationships shown in FIG. 7(a) and FIG. 7(b) can be mentioned. In addition, each heat source E A and E B The average slope θ of the line connecting the E ' is derived as follows:

[0423] The following description will be given with reference to FIG. As shown in Figure 7(a), when the x-axis is taken in the width direction of the film and the y-axis is taken in the length direction, the heat source part EA The coordinates of the heat source E are (x1, y1). B Let the coordinates be (x2,y2). The angle θ obtained when |x2-x1| is the base of a triangle and |y2-y1| is the height of the triangle E [°]For values ​​of (0°≦θ≦90°), 90-θ E This calculates the average slope of the line θ E ' is derived.

[0424] <Film thickness control means in the convex portion adjustment process> (Film thickness control means 4) The film thickness control means can be implemented, for example, by changing the temperature inside the tenter stretching apparatus or the timing of heat treatment. Heat treatment can be implemented using an infrared (IR) heater or other methods. The film thickness control means 4 can also be implemented outside the tenter stretching apparatus by changing the environmental temperature or the timing of heat treatment in a furnace of another process.

[0425] (Tenter stretching device) [Furnace temperature] The "furnace temperature" refers to the temperature measured at a position 100 mm above the center of the film in the tenter stretching apparatus just before the film passes through the stretching zone described below. Each temperature value is measured every minute for one hour, and the average value is calculated. If the temperature difference between the furnace temperature and the heat treatment temperature is not too small or too large, the formation of the convex portions is easy.

[0426] From the above viewpoints, the temperature difference between the furnace temperature and the heat treatment temperature is preferably within a range of 100 to 200° C. The furnace temperature is preferably within a range of 120 to 220° C., and more preferably within a range of 120 to 180° C. Here, when a temperature gradient is applied in the longitudinal direction in a plurality of sections, the section to be heat-treated is the subject of the discussion.

[0427] [Residual Solvent Amount Just Before the Film Passes Through the Stretching Zone] The amount of residual solvent in the film immediately before it passes through the stretching zone is preferably 20% by mass or less, and more preferably 15% by mass or less.

[0428] [Internal structure of tenter stretching device 1] A tenter stretching device holds both ends of the film in the width direction with clips. The clips run together with the film, widening the gap between them to stretch the film. It is usually divided into multiple zones: a preheating zone, a stretching zone, and a heat setting zone. The timing of heat treatment in the above three zones can be changed as needed.

[0429] For example, an infrared (IR) heater is used for the heat treatment. The number of infrared (IR) heaters is appropriately set in each zone as required. However, heaters other than infrared (IR) heaters may be used for the heat treatment.

[0430] Hereinafter, an apparatus used as the tenter stretching apparatus 7 will be described with reference to FIG. FIG. 8 is a plan view that typically illustrates the internal configuration of a tenter stretching apparatus, and is a cross-sectional view of the tenter stretching apparatus, viewed from above, in a plane perpendicular to the film surface. FIG. 8 shows a state in which the cover has been removed, and the cover is indicated by a two-dot chain line.

[0431] The tenter stretching device 40 is equipped with a number of clips 42 that grip both ends of the film in the width direction, and the clips 42 are attached to an endless chain 48 at regular intervals. The endless chains 48 are arranged on both sides of the film, and each chain is stretched between a driving sprocket 50 on the inlet side and a driven sprocket 52 on the outlet side. The driving sprocket 50 is connected to a motor (not shown), and the driving sprocket 50 rotates when this motor is driven. As a result, the endless chain 48 travels between the driving sprocket 50 and the driven sprocket 52, and the clips 42 attached to the endless chain 48 travel in a circular motion.

[0432] Between the driving sprocket 50 and the driven sprocket 52, rails 54 are provided for guiding the endless chain 48 or the clips 42. The rails 54 are arranged on both sides of the film, and the distance between the rails 54 is configured to be wider on the downstream side than on the upstream side in the film transport direction. As a result, the distance between the clips 42 is widened as the clips 42 travel around, so that the film gripped by the clips 42 can be transversely stretched in the width direction.

[0433] An opening member 56 is attached to each of the driving sprocket 50 and the driven sprocket 52. The opening member 56 is a device that displaces a flapper (not shown) of the clip 42, which will be described later, from a gripping position to an open position. The opening member 56 automatically performs the film gripping and releasing operations.

[0434] [Internal configuration 2 of tenter stretching device] A preheating zone, a (transverse) stretching zone, and a heat setting zone are provided inside the tenter stretching apparatus 40, as shown in Fig. 8. Each zone is separated by a windshield curtain (not shown).

[0435] In each zone, hot air is supplied to the film from above, below, or both. The hot air is blown uniformly across the width of the film while being controlled to a predetermined temperature for each zone. This allows the inside of each zone to be controlled to the desired temperature. Each zone will be described below.

[0436] The preheating zone is a zone in which the film is preheated, and the film is heated without widening the gap between the clips 42 .

[0437] The film preheated in the preheating zone is transferred to the transverse stretching zone, where the film is transversely stretched in the width direction by increasing the distance between clips 42. The stretching ratio is preferably within the range of 1.0 to 2.5 times, more preferably within the range of 1.05 to 2.3 times, and even more preferably within the range of 1.1 to 2 times.

[0438] The film stretched transversely in the transverse stretching zone moves to the heat setting zone.

[0439] In this embodiment, the inside of the tenter 40 is divided into a preheating zone, a (transverse) stretching zone, and a heat setting zone, but the types and arrangements of the zones are not limited thereto. For example, a cooling zone for cooling the film may be provided after the transverse stretching zone. Also, a heat relaxation zone may be provided within the heat setting zone.

[0440] In this embodiment, only transverse stretching is performed by the tenter 40, but longitudinal stretching may also be performed at the same time. In this case, the interval between the clips 42 in the conveying direction, i.e., the pitch, may be changed when the clips 42 move. As a mechanism for changing the pitch of the clips 42, for example, a pantograph mechanism or a linear guide mechanism may be used.

[0441] [Internal structure of tenter stretching device 3] Fig. 9 is a schematic diagram of the nozzles and heaters installed in the three zones in the tenter stretching apparatus when viewed from the front. As an example of an infrared (IR) heater installed in each zone, Fig. 10 shows a side view of the three zones in the tenter stretching apparatus when an infrared (IR) heater is installed in the preheating zone.

[0442] As shown in Figure 9, the infrared (IR) heater is placed only above the nozzle so that the film does not come into contact with the infrared (IR) heater when the film breaks. Also, the closer the infrared (IR) heater is to the film, the more the radiant energy from the infrared (IR) heater can be concentrated in a narrower area. Therefore, it is preferable to place the infrared (IR) heater as close as possible to the film without interfering with the width adjustment operation by the clip.

[0443] In Figure 9, the distance H from the film to the infrared (IR) heater A The heating width of the infrared (IR) heater is preferably within a range of 100 to 250 mm. The "heating width" refers to the width heated by an infrared (IR) heater until the heating intensity becomes 0.2, assuming that the heating intensity directly below the infrared (IR) heater is 1. The infrared (IR) heaters are preferably installed at intervals (pitch) within a range of 10 to 100 mm. In addition, heating is preferably performed at 100 to 1000 W within a range of 150 to 400°C.

[0444] For example, the film thickness profile in the width direction of the film is measured at each position. Then, the set temperature of each infrared (IR) heater is calculated on a computer from the difference between the target film thickness profile and the current film thickness profile. The set temperature is output to each infrared (IR) heater via a programmable controller "PLC KV-8000" (manufactured by Keyence Corporation). The convex parts are adjusted by automatically repeating these operations.

[0445] 9, heat treatment from the center nozzle is mainly shown. In this embodiment, heat treatment from the end nozzle can also be used in combination.

[0446] As shown in Figure 10, in a stretching device, an infrared (IR) heater coming out of the nozzle gap can transmit radiant energy to the film efficiently.

[0447] Figure 11 is a cross-sectional view of the tenter stretching apparatus as viewed from above on a plane perpendicular to the film plane, from a different perspective than that of Figure 8. As shown in Figure 11, infrared (IR) heaters may be arranged in a row so that the entire width of the film can be heated even before stretching. The heaters may be arranged in a staggered manner in the longitudinal direction.

[0448] (Relationship between the amount of heat A at the center of an infrared heater and the average amount of heat B at the ends of the infrared heater) In the convex portion adjusting step (S2), it is preferable that localized heating is performed using an infrared (IR) heater, and it is preferable that the heat amount A of the center of the infrared (IR) heater and the average heat amount B of the infrared (IR) heater end 75 mm away from the center satisfy the following formula (3). Equation (3) 0.2<(B / A)<0.6 If the heat generated by the infrared ray irradiation has good convergence properties, the film thickness profile can be adjusted more precisely.

[0449] The "center of the infrared (IR) heater" refers to each heat source in the above-mentioned Figure 6. The "end of the infrared (IR) heater" refers to a position 75 mm away from the center in the width direction.

[0450] The heat quantity A at the center of the infrared (IR) heater and the average heat quantity B at the ends of the infrared heater can be calculated by, for example, measuring the temperature distribution with a thermoviewer "VIM-640G2ULC" (manufactured by Vision Sensing Co., Ltd.) and taking the average value. If the heat treatment is performed by another method, it is preferable to calculate by a method corresponding to that method.

[0451] The principle and calculation method are explained in detail below. The film is heated by the infrared (IR) heater. The temperature fluctuation range of the heated part is integrated in the longitudinal direction, and the center of the width is the heat amount A, and the average value at a position 75 mm in the width direction is the average heat amount of the infrared heater ends B. From the above values, calculate the heat amount ratio (B / A) of the heat amount A of the center of the infrared (IR) heater and the average heat amount B of the infrared (IR) heater ends.

[0452] If the heat ratio (B / A) is too small, the value of the heat ratio (B / A) can be controlled by increasing the number of infrared (IR) heaters installed across the width.

[0453] [Infrared (IR) heater] The details of infrared (IR) heaters are explained below. Unlike general infrared (IR) heaters, the infrared (IR) heater is preferably designed so that the irradiation range of the infrared rays can be pinpointed and narrowed by using a mirror that reflects the infrared rays.

[0454] Examples of mirrors that reflect infrared rays include cold mirrors (manufactured by Sigma Koki Co., Ltd.) and infrared aluminum enhanced reflection mirrors (manufactured by Novo Optics).

[0455] The infrared radiation irradiation range of one currently available general infrared (IR) heater, for example, "MCHNNS3 (irradiation energy 400 W)" (manufactured by Misumi Corporation), is 500 mm in the width direction.

[0456] (4) Other processing in the next process In the present invention, the "next step" is not limited to stretching. For example, a liquid crystal polymer may be applied to an original film to produce a laminated film having a liquid crystal layer. The layer to be laminated is not limited to a liquid crystal layer, and any layer may be formed. [Explanation of symbols]

[0457] 1, 1a Stirring device (stirring tank) 2 Casting die 3 Support (endless belt, drum) 3a, 3b rollers 4 Peeling roller 5 Casting membrane 6 Drying equipment 7 Stretching device (stenter stretching device, diagonal stretching device) 8 Cut section 10 Cut section 11 Drying equipment 12 Cut section 13 Winding device 14 Extruder 15 Casting die 16 Cast drum, support 16a Touch Roller 17 Cooling drum 19 Stretching device (tenter stretching device) 20 Cut section 23 Winding device 30 film rolls 31 Film 32 Roller 33 Touch Roller 40 Stretching device (tenter stretching device) 42 clips 46 Cover 48 Endless Chain 50 Driving sprocket 52 Driven sprocket 54 Rail 56 Opening member 80 Temperature distribution sensor 101 Nozzle fixing part 102 Nozzle 103 Casting membrane 104 End nozzle 105 Center nozzle 106 Clip Cover A Part of the end of a film roll B Part of the uneven shape of the knurling process C Width direction adhesion part D Longitudinal adhesion area F Film H A , H B width Q Infrared (IR) Heater h Convex height E A , E B , heat source part θ': Inclination of the approximate straight line with respect to the longitudinal direction of the film surface θ E ′ Heat source E A and E B The length of the straight line connecting

Claims

1. A manufacturing management system for optical films, which determines a raw film to be input in a next process from a plurality of wound raw films, and determines a manufacturing sequence of the optical films, An information acquisition unit for acquiring information on characteristics of each of the raw films; An information extraction unit for extracting information on the characteristics of at least the inside or outside of the roll of each of the raw films; an information processing unit for processing the extracted characteristics of at least the inside or outside of the roll; and a sequence determination unit for determining the order of input of the raw film in the next process based on information regarding the characteristics of at least the processed inside or outside of the roll. A manufacturing management system for optical films.

2. The information on the characteristics is information on the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction. The optical film manufacturing management system according to claim 1 .

3. The next step includes a step of stretching the raw film that has been introduced. The optical film manufacturing management system according to claim 1 .

4. The information processing unit has a function of sorting the raw film based on whether or not a difference in information regarding the orientation of the resin molecules at least on the inside or outside of the roll exceeds a threshold value. The optical film production management system according to claim 2 .

5. The information processing unit has a function of calculating a similarity from information regarding the orientation of the resin molecules at least on the inside or outside of the roll. The optical film production management system according to claim 2 .

6. The order determination unit has a function of adjusting the order in which the original film is fed in the next process based on a standard deviation of the thickness at a position in the width direction of the original film.

3. The optical film production management system according to claim 1 or 2.

7. The order determination unit determines a standard deviation of the thickness at a position in the width direction on the inside of the raw film roll immediately before being loaded as σ 1 The standard deviation of the thickness at the position in the width direction on the outer side of the raw film to be fed is σ 2 Then, adjust so as to satisfy the following formula (1): The optical film production management system according to claim 6 . Formula (1) |s 1 -s 2 | / s 1 ≦0.05

8. The optical film manufacturing management system has a function of judging whether or not the stretching conditions or the stretching ratio need to be adjusted and the time required for the next process based on the acquired information on the orientation of the resin molecules, the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll, or the processed information on the orientation of the resin molecules at least on the inside or outside of the roll. The optical film production management system according to claim 2 .

9. The manufacturing management system for the optical film has a function of determining a stretching speed, a stretching temperature, or the stretching ratio. The optical film production management system according to claim 8 .

10. A manufacturing management program for optical films, which determines a web of film to be input in a next process from a plurality of webs of film that have been wound up, and determines a manufacturing sequence of the optical films, Obtaining information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction; Extracting information regarding the orientation of the resin molecules at least on the inside or outside of the roll of each of the raw films; Processing based on the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll; The order of inputting the raw film in the next process is determined based on the information on the orientation of the resin molecules at least on the inside or outside of the roll. A manufacturing management program for an optical film.

11. A similarity is calculated from the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll.

11. The optical film manufacturing management program according to claim 10.

12. A method for producing an optical film, comprising the steps of: determining a web of film to be fed to a next process from a plurality of webs of film that have been wound up; and determining a production order of the optical films, Obtaining information regarding the orientation of resin molecules contained in each of the raw films at least in the longitudinal direction; Extracting information regarding the orientation of the resin molecules at least on the inside or outside of the roll of each of the raw films; performing processing based on the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll; and determining the order of inputting the raw film in the next process based on information regarding the orientation of the resin molecules at least on the inside or outside of the roll that has been processed. A method for producing an optical film comprising the steps of:

13. The next step includes a step of stretching the raw film that has been introduced. The method for producing an optical film according to claim 12 .

14. The processing step includes a step of sorting the raw film based on whether or not a difference in information regarding the orientation of the resin molecules at least on the inside or outside of the roll exceeds a threshold value. The method for producing an optical film according to claim 12 .

15. The processing step includes a step of calculating a similarity from information regarding the orientation of the resin molecules at least on the inside or outside of the roll. The method for producing an optical film according to claim 12 .

16. The step of determining the order includes a step of adjusting the order of feeding the original film in the next step based on a standard deviation of the thickness at a position in the width direction of the original film. The method for producing an optical film according to claim 12 .

17. The step of determining the order is carried out by determining a standard deviation of the thickness of the raw film at a position in the width direction on the inside of the raw film immediately before being loaded, σ 1 The standard deviation of the thickness at the position in the width direction on the outer side of the raw film to be fed is σ 2 The method includes a step of adjusting the content of the polycyclic aromatic compound so as to satisfy the following formula (1): The method for producing an optical film according to claim 16 . Formula (1) |s 1 -s 2 | / s 1 ≦0.05

18. The method for producing the optical film includes a step of determining whether or not the stretching conditions or the stretching ratio can be adjusted and the time required for the next step based on the acquired information on the orientation of the resin molecules, the extracted information on the orientation of the resin molecules at least on the inside or outside of the roll, or the processed information on the orientation of the resin molecules at least on the inside or outside of the roll. The method for producing an optical film according to claim 12 .

19. The method for producing the optical film includes a step of determining a stretching speed, a stretching temperature, or the stretching ratio. The method for producing an optical film according to claim 18 .

Citation Information

Patent Citations

  • Scheduling device and automatic programming device for punch presses

    JP2005215720A

  • Optical film for display and its manufacturing method

    JP2007045029A

  • Manufacturing process of optical film, optical film, liquid crystal display device, image display device

    JP2009051202A

  • Production system of cellulose ester film

    JP2009172772A

  • Production management system and production management method

    JP2020166548A