Rubber composition
A rubber composition with a specific aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin addresses the balance of wet grip, rolling resistance, and abrasion resistance, enhancing tire performance and durability.
Patent Information
- Application Number
- JP2023068257
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing rubber compositions for tires lack an optimal balance of wet grip, rolling resistance, abrasion resistance, and ice grip, particularly when incorporating aliphatic-aromatic-dicyclopentadiene copolymer resins, and there is a need for improved durability and load-bearing capabilities due to increased vehicle weights.
A rubber composition containing a specific aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin, characterized by specific hydrogen ratios, molecular weights, bromine numbers, softening points, and Gardner hue, blended with diene rubber, particularly natural rubber, to enhance compatibility and performance.
The composition achieves an excellent balance of wet grip, rolling resistance, abrasion resistance, and ice grip, with improved durability and processability, suitable for tire applications.
Smart Images

Figure 2024154451000001 
Figure 2024154451000002 
Figure 2024154451000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel rubber composition which has an excellent balance of wet grip properties, rolling resistance and abrasion resistance, and further has an excellent ice grip property, and which is particularly suitable for use in tires. [Background technology]
[0002] In recent years, with the advancement of high performance and high functionality of automobiles, the demand for tire performance is increasing. For example, tires with improved wet grip, rolling resistance, and abrasion resistance, which are in a contradictory relationship, are required. In addition, electric vehicles and plug-in hybrid vehicles equipped with a driving battery are subject to increased loads on tires as the vehicle weight increases, and tires with improved durability are required. To improve rolling resistance, a technique of compounding silica into rubber and a technique of using terminal-modified rubber in which a functional group that has high affinity with silica or can be chemically bonded to the terminal is introduced to increase the dispersibility of silica are used.
[0003] For the purpose of improving the mechanical properties of tires and imparting good adhesion to unvulcanized rubber compositions, it has been proposed to compound an aliphatic / aromatic copolymer resin (see, for example, Patent Document 1) or an aliphatic / alicyclic copolymer resin (see, for example, Patent Document 2) with rubber.
[0004] Furthermore, in order to achieve high braking performance on both dry and wet road surfaces, it has been proposed to blend a thermoplastic resin such as a C5 resin, a C5 / C9 resin, or a C9 resin with a rubber component containing 70% by mass or more of natural rubber (see, for example, Patent Document 3). Also proposed are a rubber composition containing an aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin (see, for example, Patent Document 4), and a new C5-dicyclopentadiene copolymer resin and a rubber composition containing it (see, for example, Patent Document 5). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5309529 [Patent Document 2] Patent No. 5375101 [Patent Document 3] Patent No. 6346325 [Patent Document 4] JP 2020-203962 A [Patent Document 5] Patent Publication No. 2022-55449 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the methods proposed in Patent Documents 1 and 2, the blending of carbon black as a main filler was proposed, and wet grip properties, rolling resistance, abrasion resistance, and the balance thereof were not considered, and there was room for improvement in the performance of the tire composition in particular. In addition, in the rubber composition proposed in Patent Document 3, no consideration was given to aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin and C5-dicyclopentadiene copolymer resin, and no proposal was made regarding their effects. Furthermore, the proposals in Patent Documents 4 and 5 provide rubber compositions containing aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin and novel C5-dicyclopentadiene copolymer resin, and although some effect was observed in the balance of wet grip properties, rolling resistance, and abrasion resistance, there was room for improvement in particular in abrasion resistance.
[0007] Therefore, an object of the present invention is to provide a novel rubber composition which contains a specific aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin and has an excellent balance of wet grip properties, rolling resistance and abrasion resistance, and is particularly excellent in abrasion resistance and ice grip properties. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems and have found that a rubber composition containing a specific aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin in a specific diene rubber exhibits excellent rubber properties, thereby completing the present invention.
[0009] That is, the present invention relates to a rubber composition comprising 5 to 40 parts by mass of an aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin, which is a copolymer resin of a C5 fraction, dicyclopentadienes, and a C9 fraction of petroleum, per 100 parts by mass of diene-based rubber, wherein the diene-based rubber contains more than 50% by mass of natural rubber, and the aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin satisfies all of the following properties (1) to (5): (1) As measured by proton NMR, (i) the ratio of aliphatic hydrogen derived from aliphatic components observed at 0.2 to 4.0 ppm is greater than 85% and not more than 89%, (ii) the ratio of dicyclopentadiene double bond hydrogen derived from double bonds of dicyclopentadiene components observed at 4.4 to 6.3 ppm is 7% or more and 10% or less, and (iii) the ratio of aromatic hydrogen derived from aromatic components observed at 6.3 to 7.6 ppm is 1% or more and not more than 8%. (2) The weight-average molecular weight, as measured by gel permeation chromatography using standard polystyrene as the standard substance in accordance with JIS K-0124 (2011), is 2,000 or more and 3,000 or less, and the weight-average molecular weight / number-average molecular weight ratio is 2.0 or more and 3.0 or less. (3) The bromine number measured in accordance with JIS K-2605 (1996) is 45 g-Br2 / 100 g or more and 60 g-Br2 / 100 g or less. (4) The softening point measured in accordance with JIS K-2207 (1996) (ring and ball method) is 85°C or higher and 115°C or lower. (5) As a 50% by mass solution in toluene, the Gardner hue, as measured in accordance with ASTM D-1544-63T, is 5 or greater and 10 or less.
[0010] The present invention will be described in detail below.
[0011] The rubber composition of the present invention has, per 100 parts by mass of diene rubber containing more than 50% by mass of natural rubber, (1) a ratio of aliphatic hydrogen derived from an aliphatic component observed at 0.2 to 4.0 ppm of more than 85% and not more than 89%, (ii) a ratio of dicyclopentadiene double bond hydrogen derived from a double bond of a dicyclopentadiene component observed at 4.4 to 6.3 ppm of 7% or more and not more than 10%, and (iii) a ratio of aromatic hydrogen derived from an aromatic component observed at 6.3 to 7.6 ppm of 1% or more and not more than 8%, as measured by proton NMR. The rubber composition comprises 5 parts by mass or more and 40 parts by mass or less of an aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin, which is a copolymer resin of a C5 fraction, dicyclopentadienes, and a C9 fraction of petroleum, and which satisfies the following: (1) a molecular weight (hereinafter sometimes referred to as Mw) of 2000 or more and 3000 or less, a weight average molecular weight / number average molecular weight (hereinafter sometimes referred to as Mw / Mn) of 2.0 or more and 3.0 or less, (2) a bromine number of 45 g-Br2 / 100 g or more and 60 g-Br2 / 100 g or less, (3) a softening point of 85°C or more and 115°C or less, and (4) a Gardner hue of 5 or more and 10 or less.
[0012] The diene rubber constituting the rubber composition of the present invention is one containing more than 50% by mass of natural rubber, and may contain other rubbers, such as diene rubbers, as long as they contain natural rubber (sometimes referred to as NR), e.g., RSS#3. The diene rubber is not limited as long as it is in the category of diene rubbers having carbon-carbon double bonds, and examples thereof include polyisoprene rubber (sometimes referred to as IR), polybutadiene rubber (sometimes referred to as BR), and styrene-butadiene copolymer rubber (sometimes referred to as SBR). These may be used alone or in combination. There is no particular limitation on the method of producing the diene rubber, and it may be an anionic polymer or an emulsion polymer. There is no particular limitation on the molecular weight or microstructure, and it may be terminally modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl, or the like, or may be epoxidized. It is preferable to use at least one of them in combination with SBR, since it enhances compatibility and provides an excellent balance including wear resistance.
[0013] The aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin constituting the rubber composition of the present invention is a petroleum resin obtained by copolymerizing a C5 fraction, which is an aliphatic fraction obtained by separation and refining of petroleum, a C9 fraction, which is an aromatic fraction, and a dicyclopentadiene (hereinafter, sometimes referred to as DCPD) fraction, and among them, (1) the aliphatic hydrogen ratio measured by proton NMR is more than 85% and not more than 89%, (ii) the dicyclopentadiene hydrogen ratio is more than 89%, and (iii) the dicyclopentadiene hydrogen ratio is more than 89%, and (iv) the dicyclopentadiene hydrogen ratio is more than 89%, and (v) the dicyclopentadiene hydrogen ratio is more than 89%, and (vi ... as measured by proton NMR. The aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin satisfies the following: (i) an ene double bond hydrogen ratio of 7% or more and 10% or less, (ii) an aromatic hydrogen ratio of 1% or more and 8% or less, (ii) an Mw of 2000 or more and 3000 or less, an Mw / Mn of 2.0 or more and 3.0 or less, (iii) a bromine number of 45 g-Br2 / 100 g or more and 60 g-Br2 / 100 g or less, (iv) a softening point of 85° C. or more and 115° C. or less, and (v) a Gardner hue of 5 or more and 10 or less. The aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin is a petroleum resin constituted of an aliphatic component derived from a C5 fraction, an aromatic component derived from a C9 fraction, and a DCPD component derived from a dicyclopentadiene fraction as copolymerization components.
[0014] Examples of components constituting the aliphatic component include aliphatic compounds having 4 carbon atoms, such as butene, butadiene, and isobutene; linear aliphatic compounds having 5 carbon atoms, such as 2-methyl-1-butene, 3-methyl-1-butene, 2-methyl-2-butene, isoprene, and piperylene; cyclic aliphatic compounds having 5 carbon atoms, such as cyclopentadiene; 1-hexene, 2-hexene, 3-hexene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 2-methyl-2-pentene, 3-methyl-2-pentene, 4-methyl-2-pentene, 2-ethyl-1-butene, 2-ethyl-2-but ... chain aliphatic compounds having 6 carbon atoms, such as 1-heptene, 2-heptene, 3-heptene, 2-methyl-3-hexene, 4-methyl-2-hexene, 3,4-dimethyl-2-pentene, etc.; chain aliphatic compounds having 6 carbon atoms, such as 1-heptene, 2-heptene, 3-heptene, 2-methyl-3-hexene, 4-methyl-2-hexene, 3,4-dimethyl-2-pentene, etc.; mixtures of these, and further components based on mixtures called C5 fractions, are particularly preferred, as they are easily available and have excellent performance as a tackifier.
[0015] Examples of components that make up the aromatic component include aromatic compounds having 8 carbon atoms, such as styrene; aromatic compounds having 9 carbon atoms, such as α-methylstyrene, β-methylstyrene, vinyltoluene, and indene; aromatic compounds having 10 carbon atoms, such as 1-methylindene, 2-methylindene, and 3-methylindene; aromatic compounds having 11 carbon atoms, such as 2,3-dimethylindene and 2,5-dimethylindene; mixtures of these, and components based on mixtures known as C9 fractions. Components based on aromatic compounds having 8 to 10 carbon atoms are preferred because they are particularly easy to obtain and have excellent performance as a tackifier.
[0016] Examples of components constituting the DCPD class components include cyclic aliphatic compounds having 10 carbon atoms, such as dicyclopentadiene; cyclic aliphatic compounds having 11 carbon atoms, such as methyldicyclopentadiene; cyclic aliphatic compounds having 12 carbon atoms, such as dimethyldicyclopentadiene; mixtures of these compounds, and further components based on mixtures called dicyclopentadiene fractions. In particular, components based on dicyclopentadiene compounds having 10 to 12 carbon atoms are easily available and have excellent performance as a tackifier.
[0017] The aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin is (1) an aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin having (i) an aliphatic hydrogen ratio of more than 85% and not more than 89%, (ii) a DCPD type double bond hydrogen ratio of 7% or more and not more than 10%, and (iii) an aromatic hydrogen ratio of 1% or more and not more than 8%, and each hydrogenation ratio can be measured under the following conditions (A) to (C) based on the area percentage of the spectrum measured and observed by proton NMR using chloroform-d as a solvent.
[0018] (A) It is determined from the area ratio of hydrogen derived from aliphatic components observed in the range of 0.2 to 4.0 ppm.
[0019] (a) It is determined from the area ratio of hydrogen derived from the double bonds of DCPD components observed at 4.4 to 6.3 ppm.
[0020] (c) Calculate from the area ratio of hydrogen derived from aromatic components observed at 6.3 to 7.6 ppm.
[0021] An aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin that satisfies all of the above (i) to (iii) has excellent compatibility with diene rubbers.
[0022] The aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin has (2) an Mw / Mn of 2.0 or more and 3.0 or less, measured by GPC in accordance with JIS K-0124 (1994) using standard polystyrene as the standard substance. If the Mw / Mn is less than 2.0 or more than 3.0, the resin will have poor mixability (compatibility) when used in a rubber composition, and poor performance when used in a tire. In addition, the resin will have excellent processability when used in a rubber composition, and is therefore an aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin with an Mw of 2000 or more and 3000 or less.
[0023] Furthermore, the aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin satisfies all of the following properties: (3) a bromine number of 45 g-Br2 / 100 g or more and 60 g-Br2 / 100 g or less, as measured in accordance with JIS K-2605 (1996); (4) a softening point of 85° C. or more and 115° C. or less, as measured in accordance with JIS K-2207 (1996) (ring and ball method); and (5) a Gardner hue of 5 or more and 10 or less, as measured in accordance with ASTM D-1544-63T, as a 50% by mass toluene solution.
[0024] The aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin satisfies all of the characteristics (1) to (5), and therefore has excellent compatibility with diene rubbers, and further with diene rubbers containing more than 50 mass% of natural rubber, and makes it possible to provide a rubber composition that has an excellent balance of wet grip properties, rolling resistance, abrasion resistance, and ice grip properties.
[0025] The method for producing the aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin is not particularly limited, and any method may be used. For example, the resin may be produced by using a mixture containing a fraction having a boiling point range of 20° C. to 110° C. (C5 fraction; aliphatic components), a fraction having a boiling point range of 140° C. to 280° C. (C9 fraction; aromatic components), and a dicyclopentadiene fraction obtained by thermal decomposition of petroleum as a raw material oil, adding a catalyst to the mixture, and polymerizing by heating. The catalyst used for polymerization is not particularly limited, and examples thereof include aluminum trichloride, aluminum tribromide, boron trifluoride, and complexes thereof. Among these, alcohol and phenol complexes of boron trifluoride such as methanol, propanol, butanol, isobutanol, isopentanol, and phenol are selected because of their excellent catalytic activity. Among these, butanol complexes, isobutanol complexes, and isopentanol complexes are more preferable, and boron trifluoride butanol complexes are particularly preferable. The complex may be used as it is, or may be prepared in-suit from boron trifluoride, alcohols, and phenols immediately before use. Examples of the solvent during polymerization include saturated hydrocarbons in the C5 fraction and the C9 fraction. The feedstock oil is preferably a mixture of 35% by mass to 45% by mass of an aliphatic component, 5% by mass to 15% by mass of an aromatic component, and 45% by mass to 55% by mass of a DCPD component, since this produces an aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin that is particularly excellent in softening point and color.
[0026] The polymerization temperature during production is not particularly limited, and is preferably 20°C to 80°C, particularly 30°C to 60°C, since it provides high polymerization activity and excellent productivity. The amount of catalyst and polymerization time can be appropriately selected depending on the temperature and the water concentration in the raw oil, and typically, for example, the catalyst is 0.1% by mass to 2.0% by mass relative to the raw oil, and the polymerization time is 0.1 hours to 10 hours. The reaction pressure is also not particularly limited, and is preferably atmospheric pressure or higher and 1 MPa or lower. The atmosphere is also not particularly limited, and a nitrogen atmosphere is particularly preferred.
[0027] The rubber composition of the present invention contains 5 to 40 parts by mass, preferably 8 to 30 parts by mass, of the aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin per 100 parts by mass of the diene rubber. If the aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin is less than 5 parts by mass, the resulting composition will have poor wet grip properties and abrasion resistance. On the other hand, if the aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin is more than 40 parts by mass, the resulting composition will have poor rolling resistance and ice grip properties.
[0028] In addition, the rubber composition of the present invention preferably contains 5 to 200 parts by mass of silica per 100 parts by mass of diene rubber, particularly preferably 10 to 150 parts by mass, and more preferably 20 to 120 parts by mass. The silica is not particularly limited, and those used in commercially available rubber compositions can be used, among which wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), colloidal silica, etc. can be used, and wet silica is particularly preferred. In particular, a rubber composition containing an aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin can reduce viscosity, so that even if the rubber composition contains 70 parts by mass or more of silica at a high content, it is excellent in processability and can provide a tire with an excellent balance of wet grip, rolling resistance, and abrasion resistance.
[0029] When silica is used, it is preferable to use a silane coupling agent in combination. By using a silane coupling agent in combination, the bond between the rubber component and silica is strengthened via the silane coupling agent, and the balance of wet grip performance, rolling resistance, and abrasion resistance can be highly improved. Examples of the silane coupling agent include sulfide-based, mercapto-based, vinyl-based, amino-based, glycidoxy-based, nitro-based, and chloro-based silane coupling agents. These silane coupling agents can be used alone or in combination.
[0030] In the rubber composition of the present invention, in addition to the silica, for example, carbon black can be used in combination as a reinforcing filler, and the carbon black may have a grade such as FEF, SRF, HAF, ISAF, SAF, etc. The content of the carbon black is preferably 10 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the diene rubber, since this provides excellent rolling resistance.
[0031] The rubber composition of the present invention may further contain additives that are usually compounded in resin compositions or rubber compositions. For example, compounding agents such as crosslinking agents including sulfur, vulcanization accelerators, vulcanization accelerator assistants, stearic acid, zinc oxide, plasticizers, oils, and antioxidants may be added. Commercially available products can be suitably used as these compounding agents.
[0032] The rubber composition of the present invention may contain additives that are usually blended into resin compositions and rubber compositions, such as a phenol-based antioxidant, a phosphorus-based antioxidant, a sulfur-based antioxidant, a lactone-based antioxidant, an ultraviolet absorber, a pigment, calcium carbonate, glass beads, etc., as long as the blended additives do not deviate from the object of the present invention.
[0033] Furthermore, the rubber composition of the present invention includes its form and shape, and may be a crosslinked product (vulcanizate) that contains a crosslinking agent, a vulcanization accelerator, a vulcanization acceleration assistant, etc. and has been crosslinked (vulcanized).
[0034] The rubber composition of the present invention can be prepared by blending diene rubber, aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin, and various compounding agents appropriately selected as necessary, and mixing them using a mixing method such as a Banbury mixer, a pressure kneader, an open roll, etc. Furthermore, the obtained unvulcanized rubber composition can be produced as a vulcanized rubber composition by crosslinking using, for example, a calendar, a roll, an extruder, a press, etc.
[0035] According to the present invention, a rubber composition having excellent wet grip properties, abrasion resistance, and processability can be provided, and the rubber composition can be applied to various rubber applications such as rolls, mats, tubes, grips, handles, etc. Among these, the present invention can provide an excellent tire constituent material, particularly a tread, a tire having the same, and further a studless tire and an all-season tire. Effect of the Invention
[0036] INDUSTRIAL APPLICABILITY The present invention can provide a rubber composition having an excellent balance between wet grip properties, rolling resistance and abrasion resistance, and further having excellent ice grip properties, and a tire using the same, which is extremely useful industrially. EXAMPLES
[0037] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The analytical and test methods used in the examples and comparative examples are as follows.
[0038] The analytical method for aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin is shown below.
[0039] ~Proton NMR (Nuclear Magnetic Resonance Spectrum) Measurement~ The copolymerized petroleum resin was dissolved in chloroform-d (manufactured by Wako Pure Chemical Industries, Ltd.) and measured by a conventional NMR measurement method. For the spectrum obtained, the hydrogen ratio was calculated from the area ratio based on the following calculation formula. Area ratio (%) = (each peak area) / (total of all peak areas) x 100 The peaks are assigned as follows: Aliphatic hydrogen peak: 0.2 to 4.0 ppm. DCPD double bond hydrogen peak: 4.4 to 6.3 ppm. Aromatic hydrogen peak: 6.3 to 7.6 ppm.
[0040] ~Measurement of weight average molecular weight (Mw) and number average molecular weight (Mw)~ Polystyrene was used as the standard substance and measurements were performed by gel permeation chromatography in accordance with JIS K-0124 (2011).
[0041] ~Bromine number~ The measurement was performed according to a method conforming to JIS K-2605 (1996).
[0042] ~Softening point~ The measurement was performed according to JIS K-2207 (1996) (Ball and Ring Method).
[0043] ~Hue~ The measurement was performed in accordance with ASTM D-1544-63T as a 50% by mass toluene solution.
[0044] The evaluation methods and evaluation criteria for the physical properties of the rubber composition are shown below.
[0045] ~Wet grip~ Using a viscoelasticity measuring device (manufactured by Rheometrics), tan δ was measured at a temperature of 0° C., a strain of 5%, and a frequency of 15 Hz, and the value at 0° C. was evaluated as wet grip performance.
[0046] When tan δ at 0° C. was 0.27 or more, the wet grip performance was determined to be good.
[0047] ~Ice grip~ Using a viscoelasticity measuring device (manufactured by Rheometrics), the storage modulus (hereinafter sometimes referred to as E') was measured at a temperature of -20°C, a strain of 5%, and a frequency of 15 Hz, and the value at -20°C was evaluated as ice grip property.
[0048] When E' at -20°C was 55 MPa or less, the ice grip property was judged to be good.
[0049] ~Rolling resistance~ Using a viscoelasticity measuring device (manufactured by Rheometrics), tan δ was measured at a temperature of 60° C., a strain of 5%, and a frequency of 15 Hz, and the value at 60° C. was evaluated as the rolling resistance.
[0050] When tan δ at 60° C. was 0.14 or less, the rolling resistance was determined to be good.
[0051] ~Abrasion resistance~ Vulcanized rubber test pieces were prepared, and the amount of wear was measured at 23° C. using a Lambourn abrasion tester in accordance with JIS K-6264.
[0052] Wear at 23℃ is 24mm 3 / min or less, the abrasion resistance was determined to be good.
[0053] Manufacturing Example 1 A raw oil containing 40% by mass of aliphatic components, 12% by mass of aromatic components, and 48% by mass of DCPD components obtained by cracking naphtha was prepared and charged into a 2-liter glass autoclave. Next, after adjusting the temperature to 40°C under a nitrogen atmosphere, 1.4 parts by mass of boron trifluoride butanol complex was added as a Friedel-Crafts catalyst per 100 parts by mass of the raw oil and polymerized for 2 hours. Then, the catalyst was deactivated and removed with an aqueous caustic soda solution, the oil phase was recovered, and the unreacted raw oil was removed from the oil phase by distillation to obtain an aliphatic-aromatic-dicyclopentadiene copolymerized petroleum resin A (sometimes referred to as resin A). The evaluation results are shown in Table 1.
[0054] Manufacturing Examples 2 to 7 Aliphatic-aromatic-dicyclopentadiene copolymer petroleum resins (referred to as resins B, C, D, E, F, G, and H) were obtained in the same manner as in Production Example 1, except that the feedstock oil was changed to a feedstock oil consisting of 40% by mass of aliphatic components, 12% by mass of aromatic components, and 48% by mass of DCPD-type components obtained by cracking naphtha, and the blending ratios of the aliphatic components, aromatic components, and DCPD-type components were set as shown in Table 1. The evaluation results are shown in Table 1.
[0055] [Table 1]
[0056] Example 1 In a Banbury mixer (volume 1.7 liters), 55 parts by mass of natural rubber (RSS#3) and 45 parts by mass of solution polymerized terminal modified styrene-butadiene copolymer rubber (modified S-SBR) (manufactured by JSR Corporation, (trade name) HPR-350) were mixed and masticated for 30 seconds to obtain a total of 100 parts by mass of rubber components. Then, 2 parts by mass of stearic acid (manufactured by New Japan Chemical Co., Ltd.), 70 parts by mass of silica (manufactured by Tosoh Silica, (trade name) Nipsil AQ), 5.6 parts by mass of a silane coupling agent (manufactured by Shin-Etsu Silicone, (trade name) KBE46), and 20 parts by mass of the resin A obtained in Production Example 1 were added to the total of 100 parts by mass of rubber components, and the total kneading time was 5 minutes, after which the mixture was taken out. The ram pressure and rotation speed were adjusted so that the compound temperature at the time of taking out was 140°C to 150°C. The obtained compound was cooled to room temperature, and then 1 part by mass of an antioxidant (manufactured by Ouchi Shinko, product name: 810NA), 3 parts by mass of zinc oxide (manufactured by Inoue Lime Industry), 1.2 parts by mass of a vulcanization accelerator (1) (manufactured by Ouchi Shinko, product name: Noccela CZ), 1.5 parts by mass of a vulcanization accelerator (2) (manufactured by Ouchi Shinko, product name: Noccela D), and 1.5 parts by mass of sulfur (manufactured by Tsurumi Chemical Industry) as a vulcanizing agent were added and kneaded for about 1 minute (the temperature at the time of removal was 110°C or less), and then sheeted using an 8-inch roll to obtain an unvulcanized rubber composition.
[0057] The rubber composition was then vulcanized using a steam heating press at a temperature of 150°C for 30 minutes to obtain a vulcanized rubber composition. The properties of the vulcanized rubber composition obtained (wet grip, ice grip, rolling resistance, and abrasion resistance) were measured. The results are shown in Table 2.
[0058] Examples 2 to 4 Unvulcanized rubber compositions and vulcanized rubber compositions were prepared and evaluated in the same manner as in Example 1, except that Resins B, C, and D were used instead of Resin A. The results are shown in Table 2.
[0059] Examples 5 to 6 Except for using Resin C in the amount shown in Table 2 instead of 20 parts by mass of Resin A, unvulcanized rubber compositions and vulcanized rubber compositions were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0060] [Table 2]
[0061] The rubber compositions obtained in Examples 1 to 6 had an excellent balance of wet grip properties, rolling resistance and abrasion resistance, and further had excellent ice grip properties.
[0062] Comparative Example 1 An unvulcanized rubber composition and a vulcanized rubber composition were obtained in the same manner as in Example 1, except that Resin A was not used. The evaluation results are shown in Table 3.
[0063] Comparative Examples 2 to 5 Unvulcanized rubber compositions and vulcanized rubber compositions were prepared and evaluated in the same manner as in Example 1, except that Resins E, F, G, and H were used instead of Resin A. The results are shown in Table 3.
[0064] Comparative Example 6 An unvulcanized rubber composition and a vulcanized rubber composition were prepared and evaluated in the same manner as in Example 1, except that a petroleum resin (product name: T-REZ RD104, manufactured by ENEOS Corporation; sometimes referred to as Resin I) was used instead of Resin A. The results are shown in Table 3.
[0065] Comparative Example 7 An unvulcanized rubber composition and a vulcanized rubber composition were prepared and evaluated in the same manner as in Example 1, except that a petroleum resin (product name: T-REZ RA100, manufactured by ENEOS Corporation; sometimes referred to as Resin J) was used instead of Resin A. The results are shown in Table 3.
[0066] Comparative Examples 8 to 9 Except for using the amount shown in Table 3 instead of 20 parts by mass of Resin A, unvulcanized rubber compositions and vulcanized rubber compositions were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 3.
[0067] Comparative Example 10 Except for changing the mass ratio to natural rubber / modified S-SBR=45 / 55, an unvulcanized rubber composition and a vulcanized rubber composition were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 3.
[0068] [Table 3] [Industrial Applicability]
[0069] According to the present invention, by blending an aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin having a specific double bond amount with a specific diene rubber, it is possible to provide a rubber composition which has an excellent balance of wet grip properties, rolling resistance and abrasion resistance, and further has excellent ice grip properties. The rubber composition can be used as tire tread rubber to provide tires and all-season tires, and the industrial value of the rubber composition is extremely high.
Claims
1. A rubber composition comprising 100 parts by mass of diene rubber, and 5 to 40 parts by mass of an aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin, which is a copolymer resin of a C5 fraction, a dicyclopentadiene, and a C9 fraction of petroleum, wherein the diene rubber contains more than 50% by mass of natural rubber, and the aliphatic-aromatic-dicyclopentadiene copolymer petroleum resin satisfies all of the following properties (1) to (5): (1) As measured by proton NMR, (i) the ratio of aliphatic hydrogen derived from aliphatic components observed at 0.2 to 4.0 ppm is more than 85% and not more than 89%, (ii) the ratio of dicyclopentadiene double bond hydrogen derived from double bonds of dicyclopentadiene components observed at 4.4 to 6.3 ppm is 7% or more and 10% or less, and (iii) the ratio of aromatic hydrogen derived from aromatic components observed at 6.3 to 7.6 ppm is 1% or more and not more than 8%. (2) The weight average molecular weight measured by gel permeation chromatography in accordance with JIS K-0124 (2011) using standard polystyrene as the standard substance is 2000 to 3000, and the weight average molecular weight / number average molecular weight is 2.0 to 3.
0. (3) The bromine number measured in accordance with JIS K-2605 (1996) is 45 g-Br2 / 100 g or more and 60 g-Br2 / 100 g or less. (4) The softening point measured in accordance with JIS K-2207 (1996) (ring and ball method) is 85° C. or higher and 115° C. or lower. (5) The Gardner hue of a 50% by mass solution in toluene, as measured in accordance with ASTM D-1544-63T, is 5 or greater and 10 or less.
2. 2. The rubber composition according to claim 1, wherein the diene rubber further comprises a styrene-butadiene rubber in addition to a natural rubber.
3. 3. The rubber composition according to claim 1, which is a vulcanized rubber composition for use in a tire.
4. A tire having a tread made of the rubber composition according to claim 3.
Citation Information
Patent Citations
Yellow two equivalent coupler
JP1978009529A
Hovel device for stable
JP1978075101A
Abnormality display device for ventilating fan
JP1988046325A
Rubber composition
JP2020203962A
C5-dicyclopentadiene copolymer resin
JP2022055449A