Spatter detection method, and welded body manufacturing method
The method detects spatter in resistance spot welding by measuring volume changes in the molten part using electrode distance and stress, combined with machine learning, ensuring accurate spatter detection for improved welding quality.
Patent Information
- Application Number
- JP2023068665
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-19
AI Technical Summary
Existing spatter detection methods in resistance spot welding fail to accurately detect small spatter occurrences due to insignificant changes in electrode displacement, inter-electrode voltage, and inter-electrode resistance.
Detect spatter by monitoring the change in volume of the molten part during resistance spot welding using a pair of electrodes, calculating volume change based on the distance and internal stress between the electrodes, and employing a trained machine learning model to analyze the rate of volume change.
Accurately detects spatter occurrence with high precision, enabling the production of high-quality welded bodies by integrating spatter detection into the welding process.
Smart Images

Figure 2024154693000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a spatter detection method and a method for manufacturing a welded body. [Background technology]
[0002] In resistance spot welding, if spatter occurs, the nugget diameter becomes small and good weld quality cannot be obtained. Therefore, technology to detect the occurrence of spatter is being developed.
[0003] For example, Patent Document 1 discloses a resistance welding method for performing resistance welding by passing current through a pair of electrodes, and further discloses a method for detecting the occurrence of spatter. In the method for detecting the occurrence of spatter disclosed in Patent Document 1, the occurrence of spatter is detected by detecting a change in the amount of electrode displacement, interelectrode voltage, or interelectrode resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-105041 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the method of detecting the occurrence of sputtering disclosed in the above-mentioned Patent Document 1, even if sputtering occurs, if the sputtering size is small, it is not possible to detect any change in the electrode displacement amount, inter-electrode voltage, or inter-electrode resistance, and there is a risk that the occurrence of sputtering cannot be detected.
[0006] The present disclosure has been made in consideration of the above circumstances, and provides a spatter detection method that can detect the occurrence of spatter with high accuracy, and a method for manufacturing a welded body. [Means for solving the problem]
[0007] The sputter detection method according to the present disclosure includes: A spatter detection method for detecting the occurrence of spatter during resistance spot welding in which a workpiece made of a plurality of overlapping metal members is joined by sandwiching the workpiece between a pair of electrodes and passing a current therethrough, the method comprising: The occurrence of spatter is detected based on a change in volume of the molten portion of the material to be welded.
[0008] In the work spatter detection method according to the present disclosure, the occurrence of spatter is detected by a change in volume of the molten part of the workpiece melted by a pair of electrodes, so that the occurrence of spatter can be detected with high accuracy.
[0009] The spatter may be detected based on a rate of change in the volume of the molten portion. With this configuration, the occurrence of spatter can be detected from the rate of change in the volume of the molten portion, so that the occurrence of spatter can be detected with high accuracy.
[0010] Further, the pair of electrodes includes a first electrode and a second electrode that is movable relative to the first electrode in a direction in which the metal members are overlapped, A change in volume of the molten portion may be calculated based on a change in the distance between the first electrode and the second electrode and a change in internal stress of the molten portion. With this configuration, the change in volume of the molten portion can be calculated, so that the occurrence of spatters can be detected with high accuracy.
[0011] Here, the volume change of the molten part may be calculated by the following formula (1). E = S + a × F (1) where E is the volume change of the molten zone, S is the stroke of the second electrode, a is the strain conversion coefficient, and F is the applied pressure between the first and second electrodes. With this configuration, the volume change can be calculated by measuring the stroke of one electrode that moves relative to the other electrode and the pressure force between the pair of electrodes, thereby enabling high accuracy in detecting the occurrence of sputtering.
[0012] In the method for manufacturing a welded body according to the present disclosure, a step of performing resistance spot welding in which a workpiece formed by overlapping a plurality of metal members is sandwiched between a pair of electrodes and an electric current is passed through the workpiece to join the workpieces; Detecting a volume change of the molten portion of the workpiece; and detecting the occurrence of spatter during the resistance spot welding based on the volume change.
[0013] In the method for manufacturing a welded body according to the present disclosure, a welded body can be manufactured while detecting the occurrence of spatters based on a change in volume of the molten portion of the material to be welded that is melted by a pair of electrodes. Effect of the Invention
[0014] The present disclosure provides a spatter detection method that can detect the occurrence of spatter with high accuracy, and a method for manufacturing a welded body. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram of resistance spot welding. [Diagram 2] 1 is a cross-sectional view of a workpiece and a pair of electrodes during resistance spot welding. FIG. [Diagram 3] 6 is a diagram showing a change in the stroke of a second electrode and a change in the applied pressure between a first electrode and a second electrode in resistance spot welding. FIG. [Figure 4] FIG. 4 is a diagram showing the volume change of a molten zone W1 during resistance spot welding. [Diagram 5] FIG. 13 is a diagram showing the maximum value of the rate of change in the volume of the molten part in each of resistance spot welding performed multiple times. [Figure 6] 2 is a flowchart illustrating a method for producing a welded body according to the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described below through embodiments of the invention, but the invention according to the claims is not limited to the following embodiments. In addition, not all of the configurations described in the embodiments are necessarily essential as means for solving the problems. For clarity of explanation, the following description and drawings are omitted and simplified as appropriate. In each drawing, the same elements are given the same reference numerals, and repeated explanations are omitted as necessary. Naturally, the right-handed xyz Cartesian coordinate system shown in the drawings is for the convenience of explaining the positional relationship of the components. Usually, the positive direction of the z axis is vertically upward, and the xy plane is a horizontal plane.
[0017] (Embodiment 1) <Overview of resistance spot welding> First, an overview of resistance spot welding will be described with reference to Fig. 1. Fig. 1 is a schematic diagram of resistance spot welding.
[0018] As shown in Fig. 1, the workpiece M is formed by stacking metal members M1 and M2 on top of each other in the z-axis direction. The metal members M1 and M2 are typically plate-shaped members as shown in Fig. 1, but are not limited thereto, and may be cylindrical members, for example, flange members. In the example shown in Fig. 1, the workpiece M is formed by stacking two plate-shaped metal members M1 and M2, but may be formed of a plurality of metal members.
[0019] As shown in Fig. 1, the pair of electrodes includes a first electrode 11 and a second electrode 12. In the example shown in Fig. 1, the first electrode 11 is fixed in position, and the second electrode 12 has a structure that is movable relative to the first electrode 11 in the direction in which the metal members M1 and M2 are stacked (the z-axis direction).
[0020] However, without being limited thereto, the second electrode 12 may be configured to move relatively to the first electrode in the overlapping direction of the metal members M1 and M2 (z-axis direction). More specifically, the first electrode 11 moves in the overlapping direction of the metal members M1 and M2 (z-axis direction) while in contact with the metal member M2. In response to the movement of the first electrode 11, the second electrode 12 may be configured to move relatively to the first electrode 11 so that the distance between the first electrode 11 and the second electrode 12 becomes a predetermined distance.
[0021] In resistance spot welding, metal members M1 and M2 are joined by sandwiching workpiece M between a pair of electrodes, a first electrode and a second electrode, and passing current through the workpiece M. The first electrode and the second electrode press the metal members M1 and M2 in the z-axis direction to prevent them from shifting in response to a change in volume of the molten part of the workpiece M, as described below.
[0022] <Melted part> Next, a fusion zone in resistance spot welding will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view of a workpiece and a pair of electrodes during resistance spot welding.
[0023] First, the generation of the molten zone W1 will be described. In resistance spot welding, a workpiece M is sandwiched between a pair of electrodes, a first electrode and a second electrode, and an electric current is passed through the workpiece M, thereby generating a molten zone W1 between a metal member M1 and a metal member M2, as shown in Fig. 2.
[0024] In resistance spot welding, the molten zone W1 thermally expands due to heat generated by passing current between the first electrode and the second electrode. This causes the volume of the molten zone W1 to expand. Furthermore, when the resistance spot welding is completed, the molten zone W1 is cooled by the surrounding air and thermally contracts. This causes the volume of the molten zone W1 to contract. In this way, in resistance spot welding, the volume of the molten zone W1 generated between the metal members M1 and M2 changes.
[0025] Next, the volume change of the fusion zone W1 will be described in detail with reference to Fig. 2. In the following, the description will be made on the assumption that the first electrode 11 is fixed in position and the second electrode 12 is movable in the direction in which the metal members M1 and M2 are stacked (z-axis direction) relative to the first electrode 11. In addition, the volume change of the fusion zone W1 will be described using as an example a case in which the fusion zone W1 thermally expands.
[0026] As shown in Fig. 2, in resistance spot welding, the fusion zone W1 thermally expands, generating internal stress IF1. This internal stress IF1 in the fusion zone W1 causes the workpiece M to expand in the positive direction of the z-axis. In addition, in resistance spot welding, the workpiece M is sandwiched between the first electrode 11 and the second electrode 12, and a pressurized force F between the first electrode 11 and the second electrode acts on the workpiece M. In other words, the pressurized force F is a force that acts on the workpiece M to offset the internal stress IF1 in the fusion zone W1. The magnitude of the pressurized force F per unit area is referred to as the pressurized stress.
[0027] Here, when the compression stress is equal to the internal stress F1 of the fusion zone W1, the second electrode 12 is located at the stroke reference position S0 shown in Figures 1 and 2. The stroke reference position S0 is the position where the second electrode 12 is in contact with the metal member M1 immediately before the start of resistance spot welding.
[0028] On the other hand, when the internal stress F1 of the molten part W1 is larger than the compression stress, the second electrode 12 moves in the positive direction of the z-axis, and is therefore located at the stroke position S1 shown in Figures 1 and 2. Therefore, the stroke S of the second electrode 12 is the stroke position S1 minus the stroke reference position S0.
[0029] In other words, the amount by which the workpiece M expands in accordance with the thermal expansion of the fusion zone W1 and pushes the second electrode 12 up in the positive direction of the z-axis is the stroke S of the second electrode 12. In other words, the stroke S of the second electrode 12 indicates the change in the distance between the first electrode 11 and the second electrode 12.
[0030] In this way, the change in the distance between the first electrode 11 and the second electrode 12 can be calculated by measuring the stroke S of the second electrode 12. Also, the change in the internal stress of the molten zone W1 can be calculated by measuring the applied pressure F.
[0031] In resistance spot welding, when the fusion zone W1 thermally expands, the distance between the first electrode 11 and the second electrode 12 and the internal stress of the fusion zone W1 change. Therefore, the volume change of the fusion zone W1 can be calculated based on the change in the distance between the first electrode 11 and the second electrode 12 and the change in the internal stress of the fusion zone W1.
[0032] In the example shown in Figure 2, the volume change of the molten portion W1 is explained using the case where the molten portion W1 thermally expands as an example. However, in the case where the molten portion W1 thermally contracts, the volume change of the molten portion W1 can be calculated similarly based on the change in the distance between the first electrode 11 and the second electrode 12 and the change in the internal stress of the molten portion W1.
[0033] Next, an example of calculating the volume change of the fusion zone W1 will be described with reference to Figs. 3 and 4. Fig. 3 is a diagram showing the change in the stroke of the second electrode and the change in the pressing force between the first and second electrodes in resistance spot welding. In Fig. 3, the upper part shows the change in the pressing force between the first and second electrodes, and the lower part shows the change in the stroke of the second electrode. The horizontal axis indicates time and is common to the upper and lower parts. Fig. 4 is a diagram showing the volume change of the fusion zone W1 in resistance spot welding.
[0034] The upper part of Fig. 3 shows an example of measuring the stroke S of the second electrode 12 with respect to time in order to calculate the change in the distance between the first electrode 11 and the second electrode 12. As shown in the upper part of Fig. 3, from 0 ms to about 180 ms, the fusion zone W1 is in the generation stage or the start of thermal expansion, so the stroke S of the second electrode 12 is almost constant with time. From 180 ms to 400 ms, the fusion zone W1 thermally expands, so the stroke S of the second electrode 12 increases with time. After 400 ms, resistance spot welding is completed and the fusion zone W1 thermally contracts, so the stroke S of the second electrode is almost constant with time.
[0035] The lower part of Fig. 3 shows an example of measuring the applied pressure F between the first electrode 11 and the second electrode 12 with respect to time in order to calculate the change in internal stress of the fusion zone W1. As shown in the lower part of Fig. 3, from 0 ms to about 180 ms, the fusion zone W1 is in the generation stage or in the stage of starting thermal expansion, so the applied pressure F between the first electrode 11 and the second electrode 12 is almost constant with time. From 180 ms to 400 ms, the fusion zone W1 thermally expands, so the applied pressure F between the first electrode 11 and the second electrode 12 increases with time. After 400 ms, resistance spot welding is completed and the fusion zone W1 thermally contracts, so the applied pressure F between the first electrode 11 and the second electrode 12 decreases with time.
[0036] Here, the volume change of the fusion zone W1 is calculated by the following formula (1).
[0037]
number
[0038] Here, E is the volume change of the fusion zone W1, S is the stroke of the second electrode, a is the strain conversion coefficient, and F is the pressure between the first electrode 11 and the second electrode 12.
[0039] The change in volume of the fusion zone W1 can be calculated by using the stroke S of the second electrode shown in Fig. 3, the applied pressure F between the first electrode 11 and the second electrode 12, and formula (1). Fig. 4 shows the change in volume of the fusion zone W1 with respect to time calculated using the results of Fig. 3 and formula (1).
[0040] Here, in formula (1), the volume change of the molten part W1 is calculated by focusing on the change in the z-axis direction shown in Figure 2. Normally, the volume change of the molten part W1 needs to be calculated by also calculating the changes in the x and y directions during thermal expansion or contraction, but because the volume of the molten part W1 changes isotropically, the volume change of the molten part W1 can be calculated simply by focusing on the change in one direction, the z-axis direction.
[0041] <Detection of spatter occurrence> In the sputter detection method according to the first embodiment, the occurrence of sputters is detected based on the volume change of the molten part W1. A more specific description will be given with reference to Fig. 4. Fig. 4 shows curves EC1 and EC2. Curve EC1 is the volume change E of the molten part W1 with respect to time calculated using the results of Fig. 3 and formula (1), and is a curve in the case where no sputters are occurring. Curve EC2 is a curve showing the volume change of the molten part W1 with respect to time in the case where sputters are occurring.
[0042] In curve EC1 shown in Fig. 4, the molten zone W1 is generated and thermally expands from 0 ms to 400 ms, so the volume change of the molten zone W1 increases. After 400 ms, resistance spot welding is completed and the molten zone W1 thermally contracts, so the volume change E of the molten zone W1 decreases.
[0043] In contrast, in the curve EC2 shown in Fig. 4, the molten portion W1 is generated and thermally expands from 0 ms to approximately 300 ms, but the amount of the molten portion W1 is small due to the occurrence of sputtering, so the volume change of the molten portion W1 is smaller than that of the curve EC1. Also, after approximately 300 ms, the molten portion W1 thermally contracts, but the amount of the molten portion W1 is small due to the occurrence of sputtering, so the volume change E of the molten portion W1 decreases rapidly in a shorter time than that of the curve EC1.
[0044] Thus, the volume change E of the fusion zone W1 differs between when spatters are not occurring and when they are occurring. Therefore, in the spatter detection method according to embodiment 1, the occurrence of spatters can be detected based on the volume change E of the fusion zone W1 of the workpiece M melted by a pair of electrodes. In addition, since the volume change E of the fusion zone W1 occurs regardless of the size of the spatters, the spatter detection method according to embodiment 1 can accurately detect the occurrence of spatters.
[0045] 4, when focusing on the thermal contraction of the molten part W1 in the curves EC1 and EC2, the curve EC2 in the case where sputtering is occurring has a larger rate of contraction of the volume of the molten part W1 than the curve EC1 in the case where sputtering is not occurring. The occurrence of sputtering may be detected based on this rate of change.
[0046] A method for detecting the occurrence of spatters based on the rate of change in the volume of the molten zone W1 will be described in more detail with reference to Fig. 5. Fig. 5 is a diagram showing the maximum value of the rate of change in the volume of the molten zone W1 in resistance spot welding performed multiple times. In the example shown in Fig. 5, the horizontal axis indicates the number of resistance spot welding operations, and this is an example in which resistance spot welding was performed 120 times. The vertical axis indicates the maximum value of the rate of change in the volume of the molten zone W1 per 2 ms.
[0047] As shown in Fig. 5, when spattering occurs, the maximum value of the rate of change in the volume of the molten part per 2 ms is greater than the reference value SD1. When spattering does not occur, the maximum value of the rate of change in the volume of the molten part per 2 ms is smaller than the reference value SD1. In this way, the presence or absence of spattering can be determined based on whether the maximum value of the rate of change in the volume of the molten part per 2 ms is greater than the reference value SD1.
[0048] The reference value SD1 is, for example, a standard deviation of the maximum value of the rate of change of the volume of the molten part per 2 ms, and may be a predetermined value according to the material of the workpiece.
[0049] In FIG. 5, the rate of change in the shrinkage of the volume of the molten portion is calculated per 2 ms, but is not limited to this and may be calculated for a time longer or shorter than 2 ms.
[0050] In this way, the occurrence of spatters is detected based on the rate of change in the volume of the molten part W1. More specifically, the change in the volume of the molten part during resistance spot welding is calculated based on the change in the distance between the first electrode 11 and the second electrode 12 and the change in the internal stress of the molten part W1. Next, the maximum value of the rate of change in the volume of the molten part is calculated. Then, the occurrence of spatters is detected based on whether the maximum value of the rate of change in the volume of the molten part is greater than a reference value SD1. With this configuration, the occurrence of spatters can be detected with high accuracy.
[0051] Here, an example has been described in which the occurrence of spatter is detected based on whether or not the maximum value of the rate of change of the shrinkage of the volume of the molten part is greater than the reference value SD1. However, the present invention is not limited to this, and the occurrence of spatter may be detected using a trained model generated by learning the rate of change of the shrinkage of the volume of the molten part.
[0052] More specifically, a learning model according to a machine learning algorithm is made to learn the rate of change of the volume of the molten part when spattering occurs and the rate of change of the volume of the molten part when spattering does not occur. The machine learning algorithm is, for example, an SVM algorithm, a nearest neighbor method, a naive Bayes method, a decision tree, or a neural network. The trained model is generated by making the learning model learn the rate of change of the volume of the molten part.
[0053] The trained model takes the rate of change in the volumetric shrinkage of the molten part as input and the presence or absence of spatter generation as output. In this way, by using the trained model, it is possible to efficiently detect the occurrence of spatter generation.
[0054] In this way, the spatter detection method according to the first embodiment can detect the occurrence of spatter based on the volume change of the molten part W1 of the workpiece M melted by the pair of electrodes. Since the volume change of the molten part W1 occurs regardless of the size of the spatter, the spatter detection method according to the first embodiment can accurately detect the occurrence of spatter.
[0055] <Method of manufacturing welded body> Next, a method for producing a welded body according to the first embodiment will be described with reference to Fig. 6. Fig. 6 is a flow chart illustrating the method for producing a welded body according to the first embodiment.
[0056] First, resistance spot welding is performed to join the workpieces M, which are made of a plurality of overlapping metal members, by sandwiching the workpieces M between a pair of electrodes and passing current through the workpieces M (step ST1). More specifically, as shown in Fig. 2, the workpieces M M are sandwiched between a pair of electrodes, a first electrode 11 and a second electrode 12, and current is passed through the workpieces M M to generate a molten zone W1 between the metal members M1 and M2, thereby joining the workpieces M M.
[0057] Next, a change in volume of the fusion zone W1 of the workpiece M is detected (step ST2). More specifically, as shown in Fig. 2 and Fig. 3, the stroke S of the second electrode 12 is measured to calculate the change in the distance between the first electrode 11 and the second electrode 12. Also, the applied pressure F between the first electrode 11 and the second electrode 12 is measured to calculate the change in internal stress IF1 of the fusion zone W1. Then, as shown in Fig. 4, the change in volume of the fusion zone W1 is calculated based on the change in the distance between the first electrode 11 and the second electrode 12 and the change in internal stress IF1 of the fusion zone W1.
[0058] Next, the occurrence of spatter during resistance spot welding is detected based on the volume change of the fusion zone W1 (step ST3). More specifically, when spatter is occurring, the rate of change in the volume of the fusion zone W1 shrinks is greater than when spatter is not occurring. The occurrence of spatter is detected based on this rate of change.
[0059] In this way, in the manufacturing method of a welded body according to the first embodiment, the occurrence of spatters can be detected based on the volume change of the molten zone W1 of the material to be welded M melted by the pair of electrodes, and a welded body can be manufactured. Since the volume change of the molten zone W1 occurs regardless of the size of the spatters, the manufacturing method of a welded body according to the first embodiment can accurately detect the occurrence of spatters.
[0060] The present disclosure is not limited to the above-described embodiment, and may be modified as appropriate without departing from the spirit and scope of the present disclosure. [Explanation of symbols]
[0061] 11 1st electrode 12 2nd electrode E Volume change of the molten part EC1, EC2 curve F Pressure IF1 internal stress M1, M2 metal parts M Welding material S Stroke S0 Stroke reference position S1 Stroke Position SD1 standard value W1 Welded part
Claims
1. A spatter detection method for detecting the occurrence of spatter during resistance spot welding in which a workpiece made of a plurality of overlapping metal members is joined by sandwiching the workpiece between a pair of electrodes and passing a current therethrough, the method comprising: Detecting the occurrence of spatter based on a change in volume of the molten portion of the workpiece. Spatter detection method.
2. The spatter is detected based on a rate of change in volume of the molten portion. The sputter detection method according to claim 1 .
3. the pair of electrodes includes a first electrode and a second electrode movable relative to the first electrode in a direction in which the metal members are overlapped, calculating a volume change of the molten portion based on a change in the distance between the first electrode and the second electrode and a change in internal stress of the molten portion; The sputter detection method according to claim 1 or 2.
4. The volume change of the molten part is calculated by the formula (1), The sputter detection method according to claim 3. E=S+a×F...(1) where E is the volume change of the molten part, S is the stroke of the second electrode, a is the strain conversion coefficient, and F is the pressure between the first electrode and the second electrode.
5. A method for manufacturing a welded body, comprising the steps of: A step of performing resistance spot welding in which a workpiece formed by overlapping a plurality of metal members is sandwiched between a pair of electrodes and a current is passed through the workpiece to join the workpieces; Detecting a volume change of the molten portion of the workpiece; detecting occurrence of spatter during the resistance spot welding based on the volume change; A method for manufacturing a welded body comprising the steps of:
Citation Information
Patent Citations
Method and device for controlling motor-driven servo type resistance welding equipment
JP2001300738A
Resistance spot welding method and resistance spot welding device
JP2019155389A
Method and system for on-line detection of spatter in resistance spot welding based on intrinsic process signals
JP2023500999A
Resistance welding method
JP2008105041A