Polycarbonate-based resin composition excellent in appearance designability
A polycarbonate resin composition combining polycarbonate resin, rubber-reinforced styrene resin, and coffee extraction residue addresses the need for products with decorative designs, achieving high heat resistance and moldability while effectively utilizing coffee extraction residue's properties.
Patent Information
- Application Number
- JP2023068738
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
There is a lack of highly practical polycarbonate resin products with excellent appearance design and moldability for applications requiring decorative exterior designs, and existing attempts to incorporate coffee extraction residue into polyolefin resin have not fully utilized its unique properties.
A polycarbonate resin composition containing 8 to 96.5% polycarbonate resin, 3 to 80% rubber-reinforced styrene resin, and 0.5 to 12% coffee extraction residue, with optional additives like antioxidants, mold release agents, and impact modifiers, which maintains heat resistance and moldability while showcasing the coffee extraction residue's appearance.
The composition produces molded products and films with excellent appearance design, high heat resistance, and good productivity, suitable for interior goods and insert molded products.
Smart Images

Figure 2024154737000010 
Figure 2024154737000001 
Figure 2024154737000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycarbonate resin composition having excellent appearance design. [Background technology]
[0002] In recent years, canned coffee, coffee vending machines, instant coffee, etc. have been consumed in large quantities, and a large amount of coffee extraction residue is generated at the manufacturing plants of these products, major chain cafes, etc. Until now, the residue has often been disposed of by landfilling, incineration, etc., but with the increase in the amount generated and the growing interest in environmental issues, it is becoming difficult to dispose of it in such a way. Effective utilization of coffee extraction residue is an important issue for the future from the viewpoint of environmental issues as well.
[0003] Coffee extract residue has excellent heat retention, antiseptic and insect pest control properties, and has unique properties as a masking agent for bad odors. There have been attempts to utilize this unique property to develop a useful material that did not exist before. For example, Patent Document 1 discloses a food tray made of an olefin resin containing natural organic matter extract residue. However, the target is polyolefin resin, and in reality tea leaves are used. Even if polyolefin resin is used, the various properties are not sufficient.
[0004] On the other hand, polycarbonate resin is a thermoplastic resin with excellent impact resistance, heat resistance, paintability, etc., and is widely used in the fields of electricity, electronics, machinery, automobiles, daily necessities, etc. In addition, polymer alloy compositions in which polycarbonate resin is blended with ABS resin are applied to various fields due to their excellent moldability. Recently, there is a high demand for the development of products with various uses, such as interior materials with a designable appearance, but the reality is that there is no supply of highly practical products using polycarbonate resin. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-281917 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a polycarbonate resin composition which can be used to prepare molded articles and molded films having excellent appearance design. [Means for solving the problem]
[0007] As a result of intensive research to solve the above problems, the present inventors have found that a polycarbonate-based resin composition containing a polycarbonate resin (A), a rubber-reinforced styrene-based resin (B), and a coffee extraction residue (C) in specified blending amounts has excellent appearance design while maintaining various properties unique to polycarbonate-based resins, such as heat resistance, to the greatest extent possible, and has no problems with productivity, thereby completing the present invention.
[0008] That is, the present invention (1) relates to a polycarbonate resin composition having excellent appearance design, which contains 8 to 96.5% by weight of a polycarbonate resin (A), 3 to 80% by weight of a rubber-reinforced styrene-based resin (B), and 0.5 to 12% by weight of a coffee extraction residue (C).
[0009] The present invention (2) is the polycarbonate resin composition according to the present invention (1), further comprising 1% by weight or less of an antioxidant (D).
[0010] The present invention (3) is the polycarbonate resin composition according to the present invention (2), in which the antioxidant (D) is a phosphorus-based antioxidant.
[0011] The present invention (4) is the polycarbonate resin composition according to any one of the present inventions (1) to (3), further comprising one or more selected from the group consisting of colorants, release agents, softeners, antistatic agents and impact modifiers.
[0012] The present invention (5) relates to a molded article or a molded film made of the polycarbonate resin composition according to any one of the present inventions (1) to (4).
[0013] The present invention (6) is the molded article or molded film according to the present invention (5) which is used for interior goods or insert moldings. Effect of the Invention
[0014] The polycarbonate-based resin composition of the present invention has excellent appearance design, and also has various properties inherent to polycarbonate-based resins, such as excellent deflection temperature under load and excellent productivity, so that molded articles or molded films having high appearance design can be produced. It can be used for interior goods, insert molded articles, etc., and has extremely high industrial utility value. [Brief description of the drawings]
[0015] [Figure 1] The left side is a photograph of a 0.5 mm-thick film for insert molding produced using the composition of Example 1. The right side is a photograph of a molded product obtained by insert molding using the film for insert molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The embodiments will be described in detail below. However, more detailed explanations than necessary may be omitted. For example, detailed explanations of already well-known matters or duplicate explanations of substantially the same configurations may be omitted. This is to avoid the following explanation becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. Note that the inventors provide the following explanations to enable those skilled in the art to fully understand the present invention, and do not intend to limit the subject matter described in the claims.
[0017] The polycarbonate-based resin composition of the present invention, which has excellent appearance designability, is characterized by containing 8 to 96.5% by weight of a polycarbonate resin (A), 3 to 80% by weight of a rubber-reinforced styrene-based resin (B), and 0.5 to 12% by weight of a coffee extraction residue (C). The appearance designability in the present invention means that when a molded product or molded film made from the composition is visually observed, the presence of the coffee extraction residue in the composition can be seen through the composition. Figure 1 shows a photograph of a molded film made from the polycarbonate-based resin composition of the present invention, which has excellent appearance designability. It can be seen that a wood grain pattern is formed by the coffee extraction residue being well dispersed in the transparent resin.
[0018] The polycarbonate resin (A) used in the present invention is a polymer obtained by the phosgene method in which various dihydroxydiaryl compounds are reacted with phosgene, or the ester exchange method in which a dihydroxydiaryl compound is reacted with a carbonate ester such as diphenyl carbonate. A representative example is a polycarbonate resin produced from 2,2-bis(4-hydroxyphenyl)propane (bisphenol A).
[0019] Examples of the dihydroxydiaryl compound include, in addition to bisphenol A, bis(hydroxyaryl)alkanes such as bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)octane, bis(4-hydroxyphenyl)phenylmethane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, and 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane; bis(hydroxyaryl)cycloalkanes such as 1,1-bis(4-hydroxyphenyl)cyclopentane and 1,1-bis(4-hydroxyphenyl)cyclohexane; dihydroxydiaryl ethers such as 4,4'-dihydroxydiphenyl ether and 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether; dihydroxydiaryl sulfides such as 4,4'-dihydroxydiphenyl sulfide; dihydroxydiaryl sulfoxides such as 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; and dihydroxydiaryl sulfones such as 4,4'-dihydroxydiphenyl sulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone.
[0020] These can be used alone or in combination of two or more, but those that are not substituted with halogens are preferred from the viewpoint of preventing the emission of gases containing the halogens into the environment during combustion. In addition to these, piperazine, dipiperidylhydroquinone, resorcinol, 4,4'-dihydroxydiphenyl, etc. may also be used in combination.
[0021] Furthermore, the above dihydroxydiaryl compounds may be used in combination with the following trivalent or higher phenol compounds: Trivalent or higher phenol compounds include phloroglucin, 4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptene, 2,4,6-dimethyl-2,4,6-tri-(4-hydroxyphenyl)-heptane, 1,3,5-tri-(4-hydroxyphenyl)-benzene, 1,1,1-tri-(4-hydroxyphenyl)-ethane, and 2,2-bis-[4,4-(4,4′-dihydroxydiphenyl)-cyclohexyl]-propane.
[0022] The viscosity average molecular weight of the polycarbonate resin (A) is not particularly limited, but is usually in the range of 10,000 to 100,000, more preferably 15,000 to 30,000, and even more preferably 17,000 to 26,000, from the viewpoints of moldability and strength. In addition, when producing such a polycarbonate resin, a molecular weight regulator, a catalyst, etc. can be used as necessary. The viscosity average molecular weight was measured by preparing a 0.5% by weight solution of the polycarbonate resin in methylene chloride as a solvent, measuring the specific viscosity (ηsp) at a temperature of 20°C using a Cannon-Fenske type viscometer, determining the limiting viscosity [η] by concentration conversion, and calculating it from the following Schnell formula. [η] = 1.23 × 10-4 M0.83
[0023] The amount of polycarbonate resin (A) is 8 to 96.5% by weight, preferably 20 to 80% by weight, more preferably 30 to 70% by weight, based on 100% by weight of the resin composition consisting of polycarbonate resin (A), rubber-reinforced styrene resin (B) and coffee extraction residue (C). If the amount of polycarbonate resin (A) is less than 8% by weight, the heat resistance decreases, and if it exceeds 96.5% by weight, the insert moldability and productivity are deteriorated, which is not preferable.
[0024] Examples of the rubber-reinforced styrene resin (B) used in the present invention include acrylonitrile-butadiene-styrene copolymer (ABS resin), high impact polystyrene resin (HIPS), methyl methacrylate-butadiene-styrene copolymer (MBS resin), etc. Examples of preferred rubber-reinforced styrene resins include those containing graft copolymers in which aromatic vinyl monomers and vinyl cyanide monomer components are graft-copolymerized in the presence of a rubber polymer, and preferably, ABS resins produced by bulk polymerization are used in terms of moldability.
[0025] The amount of the rubber-reinforced styrene resin (B) is 3 to 80% by weight, preferably 10 to 70% by weight, and more preferably 30 to 60% by weight, in 100% by weight of the resin composition consisting of the polycarbonate resin (A), the rubber-reinforced styrene resin (B) and the coffee extraction residue (C). If the amount of the rubber-reinforced styrene resin (B) is less than 3% by weight, the moldability may be insufficient, and if it exceeds 80% by weight, the heat resistance may decrease.
[0026] The amount of the rubber-reinforced styrene-based resin (B) is preferably 1 to 80 mass%, more preferably 30 to 60 mass%, in 100 mass% of the resin component consisting of the polycarbonate resin (A) and the rubber-reinforced styrene-based resin (B). If the amount of the rubber-reinforced styrene-based resin (B) is less than 1 mass%, the moldability may be insufficient, and if it exceeds 80 mass%, the heat resistance may decrease.
[0027] The coffee extraction residue (C) used in the present invention is a residue obtained after coffee beans are ground into powder using a mill or the like and extracted as coffee. The coffee extraction residue contains alkaloids such as caffeine, and therefore has high antiseptic and insecticidal properties. In addition, the coffee-specific odor and the combined action of these multiple components act as a deodorant and antibacterial agent against bad odors. In addition, the coffee extraction residue can be given a unique appearance design. For example, the coffee extraction residue can be obtained as Tully's coffee extraction residue. In addition, the coffee extraction residue contains a lot of moisture, and there is a risk of causing decomposition of the resin during granulation, so a previously dried coffee is used. There are no particular limitations on the drying method as long as it removes moisture from the coffee extraction residue, but a general hot air circulation type drying device is used, and the drying temperature is 140 to 170°C and the drying time is about 5 to 8 hours. More preferably, the drying temperature is 150 to 160°C and the drying time is 6 to 7 hours.
[0028] The moisture content of the coffee extraction residue (C) is preferably less than 30%, more preferably less than 10%, and even more preferably less than 5%. If it is 30% or more, the moldability may be insufficient. The moisture content can be measured by measuring the weight before and after drying.
[0029] The coffee extract residue (C) may be used in combination with optional ingredients that can be mixed and treated with a polymer binder, such as wood chips or powder, calcium carbonate, talc or ceramic powder, metal powders such as aluminum and copper (static charge removers), activated carbon, zeolite particles, and other functional materials.
[0030] The amount of the coffee extract residue (C) is 0.5 to 12% by weight, preferably 1 to 10% by weight, more preferably 1 to 5% by weight, based on 100% by weight of the resin composition consisting of the polycarbonate resin (A), the rubber-reinforced styrene-based resin (B) and the coffee extract residue (C). If the amount of the coffee extract residue (C) is less than 0.5% by weight, the appearance design becomes insufficient, and if it exceeds 12% by weight, the moldability becomes insufficient.
[0031] The amount of the coffee extraction residue (C) is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 150 parts by mass, and even more preferably 0.5 to 20 parts by mass, relative to 100 parts by mass of the resin component consisting of the polycarbonate resin (A) and the rubber-reinforced styrene-based resin (B). If it is less than 0.1 part by mass, the appearance design may be insufficient, and if it exceeds 100 parts by mass, the moldability may be insufficient.
[0032] The polycarbonate resin composition of the present invention preferably contains an antioxidant. Examples of the antioxidant include phosphorus-based antioxidants and / or phenol-based antioxidants, and it is preferable to contain a phosphorus-based antioxidant. As the phosphorus-based antioxidant, a phosphite ester compound having the following phosphite ester structure is preferable, and examples thereof include compounds represented by the following general formulas (1), (2), (3) and (4).
[0033] [ka]
[0034] General formula (1): [ka] (In the formula, R 1 represents an alkyl group having 1 to 20 carbon atoms, and a represents an integer of 0 to 3.
[0035] In the general formula (1), R 1 is an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms.
[0036] Examples of the compound represented by the general formula (1) include triphenyl phosphite, tricresyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, trisnonylphenyl phosphite, etc. Among these, tris(2,4-di-t-butylphenyl)phosphite is particularly suitable, and is commercially available as, for example, Irgafos 168 manufactured by BASF ("Irgafos" is a registered trademark of BASF Societas Europea).
[0037] General formula (2): [ka] (In the formula, R 2 , R 3 , R 5 and R 6 R each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group. 4 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms; X represents a single bond, a sulfur atom, or a group represented by the formula: -CHR 7 - (where R 7 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. A represents an alkylene group having 1 to 8 carbon atoms or a group represented by the formula: *-COR 8 - (where R 8 represents a single bond or an alkylene group having 1 to 8 carbon atoms, and * represents a bond on the oxygen side. Either Y or Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms.
[0038] In the general formula (2), R 2 , R 3 , R 5 and R 6each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, an alkylcycloalkyl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, or a phenyl group.
[0039] Here, examples of the alkyl group having 1 to 8 carbon atoms include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, t-butyl, t-pentyl, i-octyl, t-octyl, and 2-ethylhexyl groups. Examples of the cycloalkyl group having 5 to 8 carbon atoms include cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl groups. Examples of the alkylcycloalkyl group having 6 to 12 carbon atoms include 1-methylcyclopentyl, 1-methylcyclohexyl, and 1-methyl-4-i-propylcyclohexyl groups. Examples of the aralkyl group having 7 to 12 carbon atoms include benzyl, α-methylbenzyl, and α,α-dimethylbenzyl groups.
[0040] R 2 , R 3 and R 5 are each independently preferably an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 5 to 8 carbon atoms, or an alkylcycloalkyl group having 6 to 12 carbon atoms. 2 and R 5 are each independently preferably a t-alkyl group such as a t-butyl group, a t-pentyl group, or a t-octyl group, a cyclohexyl group, or a 1-methylcyclohexyl group. 3 As the alkyl group, an alkyl group having 1 to 5 carbon atoms such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, or a t-pentyl group is preferable, and a methyl group, a t-butyl group, or a t-pentyl group is more preferable.
[0041] R 6is preferably a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms, and more preferably a hydrogen atom, or an alkyl group having 1 to 5 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, or a t-pentyl group.
[0042] In the general formula (2), R 4 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Examples of the alkyl group having 1 to 8 carbon atoms include the above-mentioned R 2 , R 3 , R 5 and R 6 In particular, R 4 is preferably a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and more preferably a hydrogen atom or a methyl group.
[0043] In the general formula (2), X is a single bond, a sulfur atom or a group represented by the formula: -CHR 7 -, where the formula is -CHR 7 -R in 7 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a cycloalkyl group having 5 to 8 carbon atoms. Examples of the alkyl group having 1 to 8 carbon atoms and the cycloalkyl group having 5 to 8 carbon atoms include the above-mentioned R 2 , R 3 , R 5 and R 6 Examples of X include the alkyl and cycloalkyl groups exemplified in the description of 1. In particular, X is preferably a single bond, a methylene group, or a methylene group substituted with a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a t-butyl group, or the like, and more preferably a single bond.
[0044] In the general formula (2), A is an alkylene group having 1 to 8 carbon atoms or a group represented by the formula: 8Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a 2,2-dimethyl-1,3-propylene group, and the like, with a propylene group being preferred. 8 -R in 8 R represents a single bond or an alkylene group having 1 to 8 carbon atoms. 8 Examples of the alkylene group having 1 to 8 carbon atoms represented by the formula (I) include the alkylene groups exemplified in the description of A above. 8 is preferably a single bond or an ethylene group. 8 The * in - is a bond on the oxygen side, indicating that the carbonyl group is bonded to the oxygen atom of the phosphite group.
[0045] In the general formula (2), one of Y and Z represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an aralkyloxy group having 7 to 12 carbon atoms, and the other represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. Examples of the alkoxy group having 1 to 8 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a t-butoxy group, and a pentyloxy group. Examples of the aralkyloxy group having 7 to 12 carbon atoms include a benzyloxy group, an α-methylbenzyloxy group, and an α,α-dimethylbenzyloxy group. Examples of the alkyl group having 1 to 8 carbon atoms include the alkyl groups exemplified in the description of R2, R3, R5, and R6 above.
[0046] Examples of the compound represented by the general formula (2) include 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosphepine, Examples thereof include 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin, and 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxy]-4,8-di-t-butyl-2,10-dimethyl-12H-dibenzo[d,g][1,3,2]dioxaphosphocin. Among these, when the polycarbonate resin composition is used in a field where optical properties are particularly required, 2,4,8,10-tetra-t-butyl-6-[3-(3-methyl-4-hydroxy-5-t-butylphenyl)propoxy]dibenzo[d,f][1,3,2]dioxaphosphepine is suitable, and is commercially available, for example, as Sumilizer GP manufactured by Sumitomo Chemical Co., Ltd. ("Sumilizer" is a registered trademark).
[0047] General formula (3): [ka] (In the formula, R 9 and R 10 each independently represents an alkyl group having 1 to 20 carbon atoms or an aryl group which may be substituted with an alkyl group, and b and c each independently represent an integer of 0 to 3.
[0048] Examples of the compound represented by the general formula (3) include bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, phenyl bisphenol A pentaerythritol diphosphite, etc. Bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite is commercially available as Adeka STAB PEP-36 ("Adeka STAB" is a registered trademark) manufactured by ADEKA CORPORATION.
[0049] General formula (4): [ka]
[0050] (In the formula, R 11 ~R 18 R each independently represents an alkyl group or an alkenyl group having 1 to 3 carbon atoms. 11 and R 12 , R 13 and R 14 , R 15 and R 16 , R 17 and R 18 may be bonded to each other to form a ring. 19 ~R 22 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. each of d to g independently represents an integer of 0 to 5. X 1 ~X 4 Each of X independently represents a single bond or a carbon atom. 1 ~X 4 is a single bond, R 11 ~R 22 The functional group connected to the single bond is excluded from the general formula (4).
[0051] A specific example of the compound represented by the general formula (4) is bis(2,4-dicumylphenyl)pentaerythritol diphosphite, which is commercially available under the trade name "Doverphos (registered trademark) S-9228" manufactured by Dover Chemical Co., and under the trade name "ADEKA STAB PEP-45" (bis(2,4-dicumylphenyl)pentaerythritol diphosphite) manufactured by ADEKA Corporation.
[0052] Moreover, instead of or in addition to any of the compounds represented by the general formulas (1) to (4) above, a compound represented by the following general formula (5) may be used.
[0053] General formula (5): [ka] (In the formula, R 23 ~R 26 represents an alkyl group having 1 to 20 carbon atoms, or an aryl group which may be substituted with an alkyl group.
[0054] Specific examples of the compound represented by general formula (5) include, for example, [1,1'-biphenyl]-4,4-diylbis[bis(2,4-di-t-butylphenoxy)phosphine], and the like. For example, Irgafos P-EPQ (trade name) manufactured by BASF and Sandstab P-EPQ (trade name) manufactured by Clariant Japan Co., Ltd. are commercially available.
[0055] The amount of the antioxidant is preferably 1% by weight or less, more preferably 0.02 to 0.8% by weight, based on 100% by weight of the resin composition consisting of the polycarbonate resin (A), the rubber-reinforced styrene-based resin (B) and the coffee extraction residue (C). If the amount of the antioxidant exceeds 1% by weight, the impact strength may decrease. If the amount of the antioxidant is less than 0.02% by weight, the effect of improving the color may be insufficient.
[0056] The amount of the antioxidant is preferably 1 part by weight or less, more preferably 0.02 to 0.8 parts by weight, based on 100 parts by weight of the resin component consisting of the polycarbonate resin (A) and the rubber-reinforced styrene-based resin (B). If the amount of the antioxidant exceeds 1 part by weight, the impact strength may decrease. If the amount of the antioxidant is less than 0.02 parts by weight, the effect of improving the color may be insufficient.
[0057] Moreover, the resin composition according to the present invention may contain a phenol-based antioxidant in place of or in addition to the phosphorus-based antioxidant.
[0058] An example of the phenol-based antioxidant is a compound represented by the following general formula (6).
[0059] General formula (6): [ka] (In the general formula (6), R 23 represents an alkyl group having 1 to 20 carbon atoms, or an aryl group which may be substituted with an alkyl group.
[0060] Other phenolic antioxidants include α-tocopherol, butylated hydroxytoluene, sinapyl alcohol, vitamin E, 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenylacrylate, 2,6-di-tert-butyl-4-(N,N-dimethylaminomethyl)phenol, 3,5-di-tert-butyl-4-hydroxybenzylphosphonate diethyl ester, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methyl 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-dimethylenebis(6-α-methyl-benzyl-p-cresol) 2,2'-ethylidenebis(4,6-di-tert-butylphenol), 2,2'-butylidenebis(4-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6-tert-butylphenol), triethyl 1,6-Hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[2-tert-butyl-4-methyl 6-(3-tert-butyl-5-methyl-2-hydroxybenzyl)phenyl]terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1,-dimethylethyl}-2,4,8 ,10-Tetraoxaspiro[5,5]undecane, 4,4'-thiobis(6-tert-butyl-m-cresol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol), bis(3,5-di-tert-butyl-4-hydroxybenzyl)sulfide, 4,4'-di-thiobis(2,6-di-tert-butylphenol), 4,4'-tri-thiobis(2,6-di-tert-butylphenol), 2,2-thiodiethylenebis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3',5'-di-tert-butylanilino)-1,3,5-triazine, N,N'-hexamethylenebis-(3,5-di-tert-butyl-4-hydroxyhydrocinnamide), N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl- Examples include 4-hydroxybenzyl)benzene, tris(3,5-di-tert-butyl-4-hydroxyphenyl)isocyanurate, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 1,3,5-tris-2[3(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl isocyanurate, and tetrakis[methylene-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate]methane. All of these are easily available. The above phenol-based antioxidants can be used alone or in combination of two or more.
[0061] Among these, n-octadecyl-3-(3',5'-di-tert-butyl-4-hydroxyphenyl)propionate, which is a compound represented by the above general formula (6), is suitable, and is commercially available, for example, under the trade name "ADEKA STAB AO-50" manufactured by ADEKA Corporation.
[0062] The amount of the phenol-based antioxidant is preferably 0.5 parts by weight or less based on 100 parts by weight of the resin component consisting of the polycarbonate resin (A) and the rubber-reinforced styrene-based resin (B).
[0063] The polycarbonate resin composition of the present invention may contain additives other than the above-mentioned components, such as a heat stabilizer, a colorant, a release agent, a softener, an antistatic agent, an impact modifier, an ultraviolet absorber, a pigment, a filler, a flow modifier, etc., within the scope of not impairing the effects. Among these, it is preferable to contain one or more selected from the group consisting of a colorant, a release agent, a softener, an antistatic agent, and an impact modifier, and it is more preferable to contain a release agent.
[0064] Examples of the releasing agent (E) include natural beeswax, fatty acid esters, glycerin fatty acid esters, polyol fatty acid esters, and the like.
[0065] As the fatty acid ester, a condensation compound of a normal aliphatic carboxylic acid and an alcohol can be used.
[0066] The aliphatic carboxylic acid includes saturated or unsaturated monocarboxylic acid, dicarboxylic acid, tricarboxylic acid, etc. The aliphatic carboxylic acid also includes alicyclic carboxylic acid. Among these, monocarboxylic acid and dicarboxylic acid having 6 to 36 carbon atoms are preferable, and saturated monocarboxylic acid having 6 to 36 carbon atoms is more preferable.
[0067] Specific examples of the aliphatic carboxylic acid include palmitic acid, stearic acid, valeric acid, caproic acid, capric acid, lauric acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetratriacontanoic acid, montanic acid, glutaric acid, adipic acid, and azelaic acid.
[0068] The alcohol includes saturated or unsaturated monohydric alcohols and polyhydric alcohols, and these alcohols may have a substituent such as a fluorine atom, a chlorine atom, a bromine atom, an aryl group, etc. Among these, saturated alcohols having 30 or less carbon atoms are preferred, and aliphatic saturated monohydric alcohols and aliphatic saturated polyhydric alcohols having 30 or less carbon atoms are more preferred. The aliphatic alcohols also include alicyclic alcohols.
[0069] Specific examples of the alcohol include octanol, decanol, dodecanol, tetradecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol.
[0070] Specific examples of fatty acid esters include behenyl behenate, octyldodecyl behenate, stearyl stearate, glycerin monopalmitate, glycerin monostearate, glycerin monooleate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, etc., which can be used alone or in combination of two or more. Among these, pentaerythritol stearate is preferred, and for example, Roxiol VPG861 from Emery Oleo is commercially available.
[0071] The amount of the release agent (E) is preferably 0.01 to 1.0 parts by weight, more preferably 0.05 to 0.5 parts by weight, based on 100 parts by weight of the resin components consisting of the polycarbonate resin (A) and the rubber-reinforced styrene-based resin (B). If the amount is less than 0.01 part by weight, the release effect is insufficient, and if the amount is more than 1.0 part by weight, the physical properties may decrease, the thermal stability may become insufficient during retention during molding processing, and discoloration may occur.
[0072] The polycarbonate resin composition of the present invention can be used to produce molded articles or molded films with excellent appearance design by injection molding or extrusion molding. The uses of the molded articles or molded films are not particularly limited, but include interior goods, pets, indoor and insert molded products, etc. In addition, the pellets before injection molding or extrusion molding can be used for the above-mentioned uses.
[0073] The polycarbonate-based resin composition of the present invention can also be used as a resin film for insert molding. The resin film for insert molding is a resin film that is inserted into a mold when insert molding a thermoplastic resin such as a polycarbonate resin. Since polycarbonate resin is usually injection molded at a molding temperature of 280°C or higher, a high degree of heat resistance is required even for the film inserted into the mold, so the polycarbonate-based resin composition of the present invention, which has high heat resistance, can be preferably used. The thickness of the resin film is preferably 0.05 to 2.0 mm, more preferably 0.1 to 1.5 mm, and even more preferably 0.2 to 0.8 mm.
[0074] The method of blending the various blending components used in the present invention is not particularly limited, and they can be mixed in any mixer, such as a tumbler, ribbon blender, high-speed mixer, etc., and melt-kneaded easily in a normal single-screw or twin-screw extruder. There is also no particular limitation on the order of blending these components.
[0075] Since the coffee extraction residue used contains a large amount of moisture, if the moisture content exceeds 30%, the moisture content is reduced in advance using a mixer-type dryer, hot air circulation dryer, box dryer, etc., before melt-kneading. The moisture content is preferably 10% or less, and more preferably 5% or less. If the moisture content exceeds 30%, molding processability decreases and granulation becomes impossible. EXAMPLES
[0076] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" and "%" are based on weight.
[0077] The following raw materials were used: 1. Polycarbonate resin (A): Polycarbonate resin synthesized from bisphenol A and phosgene (SD Polycarbonate 200-20 manufactured by Sumika Polycarbonate Co., Ltd., hereafter abbreviated as PC) 2. Rubber-reinforced styrene resin (B): Bulk polymerization ABS resin (Santac AT-05 manufactured by Nippon A&L Co., Ltd., hereafter abbreviated as ABS) 3. Coffee Extraction Residue (C): (Tully's Coffee Extraction Residue, hereafter abbreviated as "Coffee Extraction Residue") 4. Phosphorus-based antioxidants (D): Tris(2,4-di-t-butylphenyl)phosphite represented by the following formula:
[0078] [ka] (BASF Irgafos 168 (trade name), hereafter abbreviated as AO) 5. Other Ingredients Release agent (E): Glycerin Monostearate (Rikemal S-100A (product name) manufactured by Riken Vitamin Co., Ltd., hereafter abbreviated as MR)
[0079] Examples 1 to 7 and Comparative Examples 1 to 4 The various ingredients were mixed in a tumbler with the ingredients and ratios shown in Table 1, and melt-kneaded at a cylinder temperature of 210 to 260°C using a 37 mm diameter twin-screw extruder (TEM37SS manufactured by Shibaura Machine Co., Ltd.) to obtain various pellets. Evaluation was performed using the methods shown below. The evaluation results are shown in Table 1.
[0080] <Heat resistance> The pellets obtained were dried at 70-120°C for 4 hours or more, and then test pieces with a thickness of 4 mm were produced using an injection molding machine (ROBOSHOT S2000i100A, manufactured by Fanuc Corporation) at a cylinder temperature of 240-260°C, a mold temperature of 50-80°C, and in accordance with the ISO test method. The deflection temperature under load was measured using the obtained test pieces in accordance with ISO 75. A deflection temperature under load of 80°C or higher was considered to have passed (○).
[0081] <Productivity> During the process from melt kneading in a twin-screw extruder to pelletization, the state of the strand emerging from the tip of the extruder was visually inspected and evaluated according to the following criteria. ◯: The strands are stable and pellets can be produced. △: Although strands were occasionally disturbed or broken, pellets could be produced. ×: Disorders and breakage of strands frequently occur, making it difficult to prepare pellets.
[0082] <Appearance Judgment (Design)> 〇: It is easy to see how the coffee extract residue has been added, and the design is excellent. △: It can be seen that coffee extract residue has been added, but the design is not sufficient. ×: No sign of coffee extraction residue being added, poor design. <Insert moldability judgment> The obtained pellets were dried at 70 to 120°C for 4 hours or more, and then a film having a thickness of 300 μm to 700 μm was molded using an extrusion molding machine (Tanabe Plastics Machinery Co., Ltd., VS40 mm extruder) at a cylinder temperature of 210°C to 230°C and a die temperature of 210°C. The molded film and polycarbonate resin pellets were insert molded using an injection molding machine (FANUC Corporation, ROBOSHOT S2000i100A) at a cylinder temperature of 280°C to 310°C. The state of the obtained insert molded product was visually confirmed and evaluated according to the following criteria. ◯: No whitening or sink marks occurred on the insert film, and the design was excellent. △: No whitening or sink marks occurred on the insert film, but the design was not sufficient. ×: Whitening, sink marks, etc. occurred on the insert film, and the design was poor. [Table 1]
[0083] As shown in Table 1, it was confirmed that the polycarbonate-based resin compositions of Examples 1 to 7 had excellent appearance design, excellent deflection temperature under load, and excellent productivity and insert moldability. On the other hand, the polycarbonate-based resin compositions of Comparative Examples 1 to 3 were inferior in any of appearance design, productivity, heat resistance, and insert moldability. Moreover, the polycarbonate-based resin composition of Comparative Example 4 was excellent in all of appearance design, productivity, and insert moldability, but had a low deflection temperature under load and was inferior in heat resistance. [Industrial Applicability]
[0084] The polycarbonate resin composition of the present invention makes it possible to prepare molded articles or molded films having excellent appearance design, and is therefore of extremely high industrial utility.
Claims
1. A polycarbonate-based resin composition having excellent appearance design, comprising 8 to 96.5% by weight of a polycarbonate resin (A), 3 to 80% by weight of a rubber-reinforced styrene-based resin (B), and 0.5 to 12% by weight of a coffee extraction residue (C).
2. 2. The polycarbonate resin composition according to claim 1, further comprising 1% by weight or less of an antioxidant (D).
3. 3. The polycarbonate resin composition according to claim 2, wherein the antioxidant (D) is a phosphorus-based antioxidant.
4. The polycarbonate-based resin composition having excellent appearance design according to any one of claims 1 to 3, further comprising at least one selected from the group consisting of a colorant, a release agent, a softener, an antistatic agent and an impact modifier.
5. A molded article or molded film comprising the polycarbonate-based resin composition according to any one of claims 1 to 3, which has excellent appearance design.
6. The molded article or molded film according to claim 5, which is used for interior decoration or insert molding.
Citation Information
Patent Citations
Composition, molded article and packaging material
JP2000281917A