Hybrid bonding insulation film formation material, method for manufacturing semiconductor device and semiconductor device
The hybrid bonding insulating film forming material with polyimide precursors and fillers addresses poor metal bonding issues by reducing thermal expansion and improving dispersibility, achieving reliable and precise bonding in semiconductor devices.
Patent Information
- Application Number
- JP2023068851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing hybrid bonding technologies face issues with poor metal-to-metal bonding due to insufficient heat resistance of organic materials like epoxy and cyclic olefin resins, leading to interface deterioration and gaps during high-temperature processes.
A hybrid bonding insulating film forming material comprising polyimide precursors, solvents, and fillers, with specific structural formulas and properties to reduce thermal expansion and improve bonding reliability, using polyimide resins with flexible skeletons and surface-treated fillers to enhance dispersibility.
The material effectively suppresses bonding defects between metals, ensuring high insulation reliability and precise bonding interfaces, even at lower annealing temperatures.
Smart Images

Figure 2024154789000018 
Figure 2024154789000019 
Figure 2024154789000020
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a hybrid bonding insulating film forming material, a method for manufacturing a semiconductor device, and a semiconductor device. [Background technology]
[0002] In recent years, three-dimensional mounting of semiconductor chips has been considered in order to improve the integration degree of LSIs (Large Scale Integrated Circuits). Non-Patent Document 1 discloses an example of three-dimensional mounting of semiconductor chips.
[0003] When three-dimensionally mounting semiconductor chips using C2W (Chip-to-Wafer) bonding, the use of hybrid bonding technology used in W2W (Wafer-to-Wafer) bonding is being considered to achieve fine bonding of wiring between devices.
[0004] In C2W hybrid bonding, there is a risk of misalignment due to the heat generated during bonding, which causes thermal expansion of the substrate, chip, etc. To address this issue, Patent Document 1 discloses an example of a technology that can lower the bonding temperature by using a cyclic olefin resin to form an insulating film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-204818 A [Non-patent literature]
[0006] [Non-Patent Document 1] FC Chen et al., “System on Integrated Chips(SoIC TM) for 3D Heterogeneous Integration”, 2019 IEEE 69th Electronic Components and Technology Conference (ECTC), p.594-599(2019) Summary of the Invention [Problem to be solved by the invention]
[0007] However, when organic materials such as epoxy resins and cyclic olefin resins such as benzocyclobutene are used as the material for the insulating film, the heat resistance of the organic materials is insufficient, and there is a risk that the organic materials will change when the insulating film is exposed to high temperatures during hybrid bonding, resulting in poor bonding at the interface between the substrate and the insulating film, for example.
[0008] The present inventors have been investigating the use of polyimide resin or polyimide precursor as a hybrid bonding material from the viewpoint of excellent heat resistance. However, when a metal such as copper is bonded to a metal and an insulating film is bonded to an insulating film in the same process by hybrid bonding, there is a problem that poor metal-metal bonding (for example, a gap at the bonding interface) is likely to occur.
[0009] The present disclosure has been made in consideration of the above, and aims to provide an insulating film forming material that can suppress poor bonding between metals during hybrid bonding, a method for manufacturing a semiconductor device using the insulating film forming material, and a semiconductor device including an insulating film formed from the insulating film forming material. [Means for solving the problem]
[0010] Specific means for achieving the above object are as follows. <1> (A) at least one of a polyimide precursor, which is at least one resin selected from the group consisting of polyamic acid, polyamic acid ester, polyamic acid salt, and polyamic acid amide, and a polyimide resin; (B) a solvent; (C) a filler; A hybrid bonding insulating film forming material comprising the above compound. <2> The polyimide resin includes a structure represented by the following formula (E) and a structure represented by the following formula (G). <1> 2. The hybrid bonding insulating film forming material according to claim 1 .
[0011] [ka]
[0012] [ka]
[0013] In formula (E), C is a divalent linking group containing an ether bond, and in formula (G), D is a divalent linking group having two or more atoms linked to the main chain. <3> In the formula (G), D contains an aromatic ring and an ether bond. <2> 2. The hybrid bonding insulating film forming material according to claim 1 . <4> The polyimide resin has a structural unit represented by the following general formula (1): <2> or <3> 2. The hybrid bonding insulating film forming material according to claim 1 .
[0014] [ka]
[0015] In the general formula (1), X represents a tetravalent organic group represented by the above formula (E), and Y represents a divalent organic group represented by the above formula (G). <5> The volume average particle size of the filler is 10 nm to 1 μm. <1> ~ <4> 10. A hybrid bonding insulating film forming material according to claim 9, wherein the first and second insulating films are formed of a fluororesin. <6> The filler is surface-treated. <1> ~ <5> 10. A hybrid bonding insulating film forming material according to claim 9, wherein the first and second insulating films are formed of a fluororesin. <7> The solvent includes an ester compound. <1> ~ <6> 10. A hybrid bonding insulating film forming material according to claim 9, wherein the first and second insulating films are formed of a fluororesin. <8> <1> ~ <7> 13. A method for manufacturing a semiconductor device, comprising the steps of: preparing at least one of a first organic insulating film and a second organic insulating film using the hybrid bonding insulating film forming material described in any one of claims 1 to 12; and bonding the first organic insulating film and the second organic insulating film together. <9> forming a first electrode on a first substrate body and then forming a first organic insulating film around the first electrode to prepare a first semiconductor substrate having the first organic insulating film and the first electrode provided on one surface of the first substrate body; forming a second electrode on a second substrate body and then forming a second organic insulating film around the second electrode to prepare a second semiconductor substrate having the second organic insulating film and the second electrode provided on one surface of the second substrate body; singulating the second semiconductor substrate to obtain a plurality of semiconductor chips; a step of bonding the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip to each other and joining the first electrode of the first semiconductor substrate to the second electrode of the semiconductor chip; Includes <8> A method for manufacturing the semiconductor device according to claim 1. <10> a first semiconductor substrate having a first substrate body, a first organic insulating film and a first electrode provided on one surface of the first substrate body; a semiconductor chip having a semiconductor chip substrate body and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body; the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other, and the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded to each other, At least one of the first organic insulating film and the second organic insulating film is <1> ~ <7> 13. A semiconductor device comprising an organic insulating film formed by curing the hybrid bonding insulating film forming material according to any one of claims 1 to 12. Effect of the Invention
[0016] According to the present disclosure, it is possible to provide an insulating film forming material capable of suppressing poor bonding between metals during hybrid bonding, a method for manufacturing a semiconductor device using the insulating film forming material, and a semiconductor device including an insulating film formed from the insulating film forming material. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a semiconductor device manufactured by a method for manufacturing a semiconductor device according to an embodiment of the present invention. [Diagram 2] 2A to 2C are diagrams sequentially showing a method for manufacturing the semiconductor device shown in FIG. [Diagram 3] FIG. 3 is a diagram showing in more detail the bonding method in the method for manufacturing the semiconductor device shown in FIG. [Figure 4] 4A to 4C are views showing a method for manufacturing the semiconductor device shown in FIG. 1, sequentially illustrating steps subsequent to the step shown in FIG. [Diagram 5] FIG. 5 is a diagram showing an example in which the method for manufacturing a semiconductor device according to an embodiment of the present invention is applied to Chip-to-Wafer (C2W). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the embodiments for carrying out the present disclosure will be described in detail. However, the present disclosure is not limited to the following embodiments. In the following embodiments, the components (including element steps, etc.) are not essential unless otherwise specified. The same applies to the numerical values and their ranges, and do not limit the present disclosure.
[0019] In the present disclosure, "A or B" may include either A or B, or may include both. In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved. In the present disclosure, a numerical range indicated using "~" includes the numerical values before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In the present disclosure, each component may contain multiple types of corresponding substances. When multiple types of substances corresponding to each component are present in the composition, the content or amount of each component means the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the terms "layer" and "film" include cases where the layer or film is formed over the entire area when the area in which the layer or film is present is observed, as well as cases where the layer or film is formed over only a portion of the area. In the present disclosure, the term "insulating film" is a concept that also encompasses an insulating layer. In the present disclosure, when a functional group has a substituent, the number of carbon atoms in the functional group means the total number of carbon atoms including the number of carbon atoms in the substituent. When an embodiment of the present disclosure is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. In addition, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this.
[0020] <Hybrid bonding insulating film forming material> The hybrid bonding insulating film forming material of the present disclosure includes (A) at least one polyimide precursor, which is at least one resin selected from the group consisting of polyamic acid, polyamic acid ester, polyamic acid salt, and polyamic acid amide, and at least one polyimide resin (hereinafter also referred to as "component (A)"), (B) a solvent (hereinafter also referred to as "component (B)"), and (C) a filler (hereinafter also referred to as "component (C)").
[0021] The hybrid bonding insulating film forming material of the present disclosure can suppress poor bonding between metals during hybrid bonding, and the reason for this is presumed to be as follows. The hybrid bonding insulating film forming material contains components (A) and (B), and when formed into an insulating film, it is possible to reduce the difference in the thermal expansion coefficient between the insulating film and a metal such as copper, compared to a case where component (B) is not contained, which makes it possible to suppress poor bonding between metals caused by the difference in the thermal expansion coefficient between the insulating film and a metal such as copper.
[0022] The hybrid bonding insulating film forming material of the present disclosure has a thermal expansion coefficient of 50 ppm / K or less, more preferably 45 ppm / K or less, and even more preferably 40 ppm / K or less. This makes it possible to suitably suppress poor bonding between metals. The lower limit of the thermal expansion coefficient of the cured product is not particularly limited, and may be, for example, 20 ppm / K or more, or 25 ppm / K or more. The coefficient of thermal expansion indicates the rate at which the length of a cured material expands due to an increase in temperature per unit of temperature, and can be calculated by measuring the change in length of a cured material at temperatures between 50°C and 100°C using a thermomechanical analyzer or the like.
[0023] The hybrid bonding insulating film forming material of the present disclosure may be a material that is applied to techniques such as W2W (Wafer-to-Wafer) bonding, C2W (Chip-to-Wafer) bonding, etc. When insulating films are bonded together to perform hybrid bonding, it is sufficient that at least one of the insulating films is formed from the hybrid bonding insulating film forming material of the present disclosure, and it is preferable that both insulating films are formed from the hybrid bonding insulating film forming material of the present disclosure.
[0024] Furthermore, the insulating film obtained by curing the hybrid bonding insulating film forming material of the present disclosure has a lower elastic modulus and is softer than a molded product made of an inorganic material. Therefore, when insulating films are bonded together, even if a foreign substance or the like is present on the surface of one insulating film (hereinafter also referred to as the "first insulating film") or the surface of the other insulating film (hereinafter also referred to as the "second insulating film"), the insulating film at the bonding interface tends to easily deform and the foreign substance can be contained within the insulating film without generating a large void in the insulating film.
[0025] ((A) Polyimide precursor and polyimide resin) The hybrid bonding insulating film forming material of the present disclosure contains at least one of a polyimide precursor, which is at least one resin selected from the group consisting of polyamic acid, polyamic acid ester, polyamic acid salt, and polyamic acid amide (A) and a polyimide resin (A component). By containing at least one of a polyimide precursor and a polyimide resin, the insulating film formed tends to have excellent heat resistance.
[0026] In the present disclosure, the polyimide precursor refers to a compound corresponding to any one of polyamic acid; an ester compound (polyamic acid ester) in which the hydrogen atoms of at least a portion of the carboxy groups in a polyamic acid are substituted with monovalent organic groups; an amide compound (polyamic acid amide) in which the hydrogen atoms of at least a portion of the carboxy groups in a polyamic acid are substituted with monovalent organic groups; or a polyamic acid salt, which is a compound in which at least a portion of the carboxy groups in a polyamic acid form a salt structure with a basic compound having a pH of 7 or more. The polyamic acid ester, polyamic acid amide, etc. may have a polymerizable unsaturated bond.
[0027] From the viewpoint of low-temperature bonding property and insulation reliability during low-temperature curing of the hybrid bonding insulating film forming material, it is preferable that the main component of the component (A) is a polyimide resin. In this case, the content of the polyimide resin is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and further preferably 90% by mass to 100% by mass, based on the total amount of the component (A).
[0028] From the viewpoints of solubility in the component (B) and low-temperature bonding properties, the polyimide resin preferably contains a structure represented by the following formula (E) and a structure represented by the following formula (G).
[0029] [ka]
[0030] [ka]
[0031] In formula (E), C is a divalent linking group containing an ether bond, and in formula (G), D is a divalent linking group having two or more atoms linked to the main chain.
[0032] When component (A) contains the structure represented by formula (E) and the structure represented by formula (G), which are relatively flexible skeletons, the solubility in a solvent is improved. Furthermore, by using component (A) as a base polymer of an insulating material, the imidization rate in low-temperature curing is improved, and as a result, the insulating reliability of the insulating film is improved.
[0033] In the hybrid bonding insulating film forming material of the present disclosure, even when the (A) component containing the structure represented by formula (E) and the structure represented by formula (G), which are relatively flexible skeletons, is used, the thermal expansion coefficient of the cured product obtained by curing can be reduced. In order to reduce the thermal expansion coefficient of the cured product, it is usually assumed that the (A) component having a rigid skeleton is used. However, when the (A) component having a rigid skeleton is used, there is a problem that the glass transition temperature of the cured product increases, and a high-temperature process is required during hybrid bonding. In the present disclosure, by using the (A) component containing the structure represented by formula (E) and the structure represented by formula (G), which are relatively flexible skeletons, in combination with the (C) component, it is possible to achieve both a low thermal expansion coefficient and a low-temperature process.
[0034] From the viewpoint of achieving both a low thermal expansion coefficient and low-temperature processability, the proportion of component (A) including the structure represented by formula (E) and the structure represented by formula (G) in the entire component (A) is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass.
[0035] In addition, it is preferable that the component (A) does not have a carboxyl group in the molecule, which, unlike polyamic acids that have a carboxyl group in the molecule, results in excellent storage stability at room temperature and further improved insulation reliability.
[0036] The polyimide resin preferably has a structural unit represented by the following general formula (1): This tends to provide a semiconductor device having an insulating film with high reliability.
[0037] [ka]
[0038] In the general formula (1), X represents a tetravalent organic group represented by the above formula (E), and Y represents a divalent organic group represented by the above formula (G). The component (A) may have a plurality of structural units represented by the above general formula (1), and X and Y in the plurality of structural units may be the same or different. The component (A) may or may not contain a structural unit in which X is a tetravalent organic group having a structure other than that of formula (E). The component (A) may or may not contain a structural unit in which Y is a divalent organic group having a structure other than that of formula (G).
[0039] In general formula (1), the tetravalent organic group represented by X preferably has 12 to 40 carbon atoms, more preferably 12 to 35 carbon atoms, and even more preferably 12 to 30 carbon atoms. In X, each benzene ring in formula (E) may have a substituent or may be unsubstituted. Examples of the substituent on the aromatic ring include an alkyl group, a fluorine atom, a halogenated alkyl group, a hydroxyl group, and an amino group. In formula (E), two adjacent benzene rings may be linked at two positions by at least one of a single bond and a linking group via a divalent linking group containing an ether bond (C in formula (E)), thereby forming a 5- or 6-membered ring containing the linking group between the two benzene rings.
[0040] Examples of the structure represented by formula (E) include a structure containing an ether bond (-O-) and a phenylene group, a structure which is an ether bond (-O-), and a structure containing an ether bond and an alkylene group.
[0041] Examples of the structure represented by formula (E) include groups represented by the following formulae (I) to (O).
[0042] [ka]
[0043] Examples of the structure containing an ether bond (-O-) and a phenylene group include the groups represented by the above formulae (J) to (O). An example of the structure which is an ether bond (-O-) is the group represented by the above formula (I).
[0044] Examples of the structure containing an ether bond and an alkylene group include groups represented by the following formulae (P) to (R).
[0045] [ka]
[0046] In general formula (1), the divalent organic group represented by Y preferably has 4 to 25 carbon atoms, more preferably 6 to 20 carbon atoms, and further preferably 12 to 18 carbon atoms. The divalent organic group represented by Y has a structure represented by formula (G). The structure represented by formula (G) is a structure in which two aromatic rings are bonded to a main chain via a divalent linking group (D in formula (G)) in which two or more atoms are linked. The proportion of m-bonds contained in formula (G) may be greater than 0%, may be 50% to 100%, or may be 100%. The proportion of m-bonds means the proportion of the number of aromatic rings substituted at the m-position (meta position) to the total number of aromatic rings contained in formula (G), and preferably means the proportion of the number of aromatic rings which constitute the main chain and are substituted at the m-position (meta position) to the total number of aromatic rings which constitute the main chain in formula (G).
[0047] From the viewpoints of the heat resistance of the polyimide resin and the solubility of the polyimide resin in a solvent, D in formula (G) preferably contains an aromatic ring and an ether bond, and is more preferably a group represented by the following formula (G1).
[0048] [ka]
[0049] The content of the structural unit represented by general formula (1) in component (A) is preferably 60 mol% or more, more preferably 70 mol% or more, and even more preferably 80 mol% or more, based on the total structural units. The upper limit of the content is not particularly limited, and may be 100 mol%.
[0050] The component (A) may be synthesized using a tetracarboxylic dianhydride and a diamine compound. In this case, in the general formula (1), X corresponds to a residue derived from the tetracarboxylic dianhydride, and Y corresponds to a residue derived from the diamine compound. The component (A) may be synthesized using a tetracarboxylic acid instead of the tetracarboxylic dianhydride.
[0051] There are no particular limitations on the molecular weight of the component (A), and for example, the weight average molecular weight is preferably 10,000 to 200,000, and more preferably 10,000 to 100,000. The weight average molecular weight can be measured, for example, by gel permeation chromatography, and can be calculated using a standard polystyrene calibration curve.
[0052] Component (A) may have a nonvolatile crosslinking group at the end of the main chain. The nonvolatile crosslinking group is a functional group capable of crosslinking reaction that is located at the end of the main chain of component (A) and does not volatilize due to heating, drying, etc. The nonvolatile crosslinking group may be a functional group containing an unsaturated double bond.
[0053] Examples of compounds used to form a nonvolatile crosslinking group at the main chain end of component (A) (hereinafter also referred to as a nonvolatile crosslinking group forming compound) include maleic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, itaconic anhydride, methacrylic anhydride, 2-isocyanatoethyl methacrylate, 2-isocyanatoethyl acrylate, 4-ethynylphthalic anhydride, 4-vinylphthalic anhydride, di-t-butyl dicarbonate, etc. These compounds react with amino groups derived from diamine compounds to obtain compounds having a nonvolatile crosslinking group at the main chain end. The non-volatile crosslinking group-forming compounds may be used alone or in combination of two or more.
[0054] The hybrid bonding insulating film forming material of the present disclosure may contain a resin component other than component (A). From the viewpoint of heat resistance, examples of the resin component other than component (A) include novolac resin, acrylic resin, polyether nitrile resin, polyether sulfone resin, epoxy resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polyvinyl chloride resin, etc. The resin components other than the component (A) may be used alone or in combination of two or more.
[0055] In the hybrid bonding insulating film forming material of the present disclosure, the content of component (A) relative to the total amount of resin components is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass.
[0056] The hybrid bonding insulating film forming material of the present disclosure may or may not contain a resin component such as a cyclic olefin resin such as benzocyclobutene, an epoxy resin, etc. From the viewpoint of obtaining an insulating film with superior heat resistance and mechanical properties, and from the viewpoint of suitably suppressing poor bonding between an insulating film and an electrode and poor bonding between insulating films when performing hybrid bonding, the content of the cyclic olefin resin and the content of the epoxy resin are each independently preferably 30% by mass or less, more preferably 0% by mass to 10% by mass, and even more preferably 0% by mass to 5% by mass, based on the total amount of the hybrid bonding insulating film forming material of the present disclosure.
[0057] ((B) Solvent) The hybrid insulating film forming material of the present disclosure may contain a (B) solvent (component (B)). The (B) component preferably contains at least one compound selected from the group consisting of compounds represented by the following formulas (3) to (10). The component (B) may be used alone or in combination of two or more types.
[0058] [ka]
[0059] [ka]
[0060] In formulas (3) to (10), R 1 , R 2 , R 8 , R 10 , R 11 , R 13 and R 14 are each independently an alkyl group having 1 to 4 carbon atoms; R 3 ~R 7 , R 9 and R 12 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. s is an integer of 0 to 8, t is an integer of 0 to 4, r is an integer of 0 to 4, u is an integer of 0 to 3, v is an integer of 0 to 3, w is an integer of 0 to 4, and x is an integer of 0 to 5.
[0061] In formula (3), s is preferably 0. In formula (4), R 2 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. t is preferably 0, 1 or 2, and more preferably 1. In formula (5), R 3 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group, an ethyl group, a propyl group, or a butyl group. 4 and R 5 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. In formula (6), R 6 ~R 8The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. r is preferably 0 or 1, and more preferably 0. In formula (7), R 9 and R 10 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. u is preferably 0 or 1, and more preferably 0. In formula (8), R 11 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. u is preferably 0 or 1, and more preferably 0. In formula (9), R 12 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. 13 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. w is preferably 0 or 1, and more preferably 0. In formula (10), R 14 The alkyl group having 1 to 4 carbon atoms is preferably a methyl group or an ethyl group. x is preferably 0 or 1, and more preferably 0.
[0062] Specific examples of the component (B) include the following compounds.
[0063] [ka] [ka]
[0064] From the viewpoint of improving the dispersibility of the filler, the component (B) preferably contains a compound containing an ester bond (ester compound), and more preferably contains a cyclic ester compound. As the cyclic ester compound, a compound containing an ester bond in a cyclic structure such as γ-butyrolactone, δ-valerolactone, ε-caprolactone, ethylene carbonate, propylene carbonate, etc. is preferable, and among them, γ-butyrolactone is preferable.
[0065] In the hybrid insulating film forming material of the present disclosure, from the viewpoint of reducing toxicity such as reproductive toxicity, the content of N-methyl-2-pyrrolidone (NMP) may be 1 mass % or less based on the total amount of the hybrid insulating film forming material, and may be 3 mass % or less based on the total amount of the component (A).
[0066] In the hybrid bonding insulating film forming material of the present disclosure, the content of the component (B) is preferably 1 part by mass to 10,000 parts by mass, and more preferably 50 parts by mass to 10,000 parts by mass, per 100 parts by mass of the component (A).
[0067] From the viewpoint of improving filler dispersibility, the proportion of the ester compound in the component (B) may be from 20% by mass to 100% by mass, or may be from 50% by mass to 100% by mass. When a filler dispersed in a dispersion solvent is used as component (C) described below, the dispersion solvent is classified as component (B) in the hybrid bonding insulating film forming material.
[0068] ((C) Filler) The hybrid insulating film-forming material of the present disclosure may contain a filler (C) (component (C)). The component (C) may be an organic filler, an inorganic filler, or an inorganic-organic composite filler. The component (B) may be used alone or in combination of two or more types.
[0069] Examples of organic fillers include polyethylene fibers, polypropylene fibers, polyester fibers, polyamide fibers, fluorine fibers, ebonite powder, thermosetting resin hollow spheres, epoxy resin fillers, silicon-based fillers, saran hollow spheres, shellac, wood powder, cork powder, polyvinyl alcohol fibers, cellulose powder, and wood pulp. Among these, epoxy resin fillers, silicon-based fillers, thermosetting resin hollow particles, fluorine fibers, and the like are particularly preferred because of their excellent heat resistance and mechanical properties.
[0070] Examples of inorganic fillers include silica, alumina, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, zirconium silicate, calcium oxide, magnesium oxide, titanium oxide, silicon nitride, aluminum nitride, boron nitride, calcium titanate, barium titanate, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, and mica. Among these, silica and alumina are particularly preferred, and silica is more preferred.
[0071] When component (C) is particulate, its volume average particle size is not particularly limited. For example, the volume average particle size is preferably 10 nm to 1 μm, more preferably 10 nm to 500 nm, and from the viewpoint of resin fluidity and filler dispersibility, further preferably 20 nm to 300 nm. The volume average particle size of component (C) refers to the value measured as the volume average particle size (D50) using a laser diffraction scattering particle size distribution measuring device.
[0072] The volume average particle diameter of the component (C) in the hybrid bonding insulating film forming material or its cured product can be measured by a known method. As an example, the component (C) (preferably an inorganic filler) is extracted from the hybrid bonding insulating film forming material or the cured product using an organic solvent, nitric acid, aqua regia, etc., and thoroughly dispersed using an ultrasonic disperser or the like to prepare a dispersion. Using this dispersion, the volume average particle diameter of the component (C) (preferably an inorganic filler) can be measured from the volume-based particle size distribution measured using a laser diffraction scattering method particle size distribution measuring device. Alternatively, the volume average particle diameter of the component (C) can be measured from the volume-based particle size distribution obtained by embedding the cured product in a transparent epoxy resin or the like and polishing the cross section obtained by observing the cross section with a scanning electron microscope. Furthermore, the volume average particle diameter of the component (C) can be measured by continuously observing the two-dimensional cross section of the cured product using an FIB device (focused ion beam SEM) or the like and performing three-dimensional structural analysis.
[0073] The (C) component is preferably surface-treated. This tends to improve the dispersibility of the (C) component in the hybrid bonding insulating film forming material of the present disclosure. The improved dispersibility suppresses aggregation of the (C) component, which can suppress the variation in the thermal expansion coefficient in the insulating film when the insulating film is formed, and as a result, tends to suppress poor bonding between insulating films. Furthermore, it tends to reduce foreign matter on the insulating film caused by aggregation of the (C) component.
[0074] The hybrid bonding insulating film forming material of the present disclosure preferably contains a surface-treated inorganic filler, and more preferably contains at least one of surface-treated silica and surface-treated alumina.
[0075] The surface treatment may be a hydrophobization treatment from the viewpoint of improving the dispersibility of the (C) component. A commercially available filler may be used as the (C) component that has been surface-treated. Alternatively, the (C) component that has not been surface-treated may be surface-treated using various surface treatment agents such as the coupling agent described below.
[0076] In the hybrid bonding insulating film forming material of the present disclosure, the content of the (C) component may be 5 parts by mass to 200 parts by mass, 10 parts by mass to 150 parts by mass, or 10 parts by mass to 100 parts by mass, relative to 100 parts by mass of the (A) component.
[0077] From the viewpoint of suppressing aggregation, the component (C) may be a filler dispersed in a dispersion solvent. The dispersion solvent is not particularly limited, and examples thereof include known solvents such as cyclohexanone and dimethylacetamide.
[0078] The hybrid bonding insulating film forming material of the present disclosure may contain at least one of a polymerizable monomer, a photopolymerization initiator, a thermal polymerization initiator, a polymerization inhibitor, an antioxidant, a coupling agent, a surfactant, a leveling agent, a rust inhibitor, a nitrogen-containing compound, or a dicarboxylic acid, as necessary.
[0079] The coupling agent is not particularly limited, and examples thereof include 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinopropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N-(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-trimethyl ... silane coupling agents such as benzene-1,4-bis(N-[3-triethoxysilyl]propylamido)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamido)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride, N-phenylaminopropyltrimethoxysilane, N,N'-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-ureidopropyltriethoxysilane; aluminum-based adhesion aids such as aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), ethylacetoacetate aluminum diisopropylate; and the like. These coupling agents may be used in the surface treatment of the above-mentioned component (C). The coupling agents may be used alone or in combination of two or more.
[0080] The method for preparing the hybrid bonding insulating film forming material of the present disclosure is not particularly limited, and it is sufficient to mix the above-mentioned components.
[0081] <Semiconductor device> The semiconductor device of the present disclosure comprises a first substrate body, a first semiconductor substrate having a first organic insulating film and a first electrode provided on one surface of the first substrate body, a semiconductor chip substrate body, and a semiconductor chip having a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body, wherein the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded, the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded, and at least one of the first organic insulating film and the second organic insulating film is an insulating film formed by hardening the hybrid bonding insulating film forming material of the present disclosure. The semiconductor device of the present disclosure has excellent insulation reliability because at least one of the first organic insulating film and the second organic insulating film is an insulating film formed by curing the hybrid bonding insulating film forming material of the present disclosure. Moreover, the semiconductor device of the present disclosure can be manufactured, for example, by the manufacturing method of a semiconductor device described below.
[0082] <Method of Manufacturing Semiconductor Device> The method for manufacturing a semiconductor device according to the present disclosure includes preparing at least one of a first organic insulating film and a second organic insulating film using the hybrid bonding insulating film forming material according to the present disclosure, and bonding the first organic insulating film and the second organic insulating film together. More specifically, the semiconductor device can be manufactured through the following steps (1) to (5). Step (1) A first semiconductor substrate is prepared, the first semiconductor substrate having a first substrate body, and the first organic insulating film and a first electrode provided on one surface of the first substrate body. Step (2) A second semiconductor substrate is prepared, the second semiconductor substrate having a second substrate body, and the second organic insulating film and a plurality of second electrodes provided on one surface of the second substrate body. Step (3): The second semiconductor substrate is diced into individual semiconductor chips, each of which includes the second organic insulating film and at least one of the second electrodes. Step (4): The first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other. Step (5): The first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded to each other.
[0083] In the step (1), the first semiconductor substrate may be prepared by forming a first electrode on a first substrate body and then forming a first organic insulating film around the first electrode. In the step (1), the second semiconductor substrate may be prepared by forming a second electrode on the second substrate body and then forming a second organic insulating film around the second electrode.
[0084] Hereinafter, an embodiment of the semiconductor device of the present disclosure and an embodiment of the manufacturing method of the semiconductor device of the present disclosure will be described in detail with reference to the drawings. In the following description, the same or corresponding parts are given the same reference numerals, and duplicated descriptions will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0085] (An example of a semiconductor device) Fig. 1 is a cross-sectional view showing a schematic example of a semiconductor device according to the present disclosure. As shown in Fig. 1, the semiconductor device 1 is, for example, an example of a semiconductor package, and includes a first semiconductor chip 10 (a first semiconductor substrate), a second semiconductor chip 20 (a semiconductor chip), a pillar portion 30, a redistribution layer 40, a substrate 50, and a circuit substrate 60.
[0086] The first semiconductor chip 10 is a semiconductor chip such as an LSI (large-scale integrated circuit) chip or a CMOS (Complementary Metal Oxide Semiconductor) sensor, and has a three-dimensional mounting structure in which the second semiconductor chip 20 is mounted downward. The second semiconductor chip 20 is a semiconductor chip such as an LSI or memory, and is a chip component having a smaller area in a plan view than the first semiconductor chip 10. The second semiconductor chip 20 is bonded to the back surface of the first semiconductor chip 10 by chip-to-chip (C2C) bonding. The first semiconductor chip 10 and the second semiconductor chip 20 are finely bonded to each other by hybrid bonding, the details of which will be described later, with the respective terminal electrodes and the insulating films around them being firmly bonded to each other without misalignment.
[0087] The pillar portion 30 is a connection portion in which a plurality of pillars 31 formed of a metal such as copper (Cu) are sealed with a resin 32. The plurality of pillars 31 are conductive members extending from the upper surface of the pillar portion 30 to the lower surface. The plurality of pillars 31 may have a cylindrical shape with a diameter of, for example, 3 μm to 20 μm (for example, a diameter of 5 μm), and may be arranged so that the center-to-center distance between each pillar 31 is 15 μm or less. The plurality of pillars 31 flip-chip connect the lower terminal electrode of the first semiconductor chip 10 and the upper terminal electrode of the rewiring layer 40. By using the pillar portion 30, the semiconductor device 1 can form a connection electrode without using a technique called TMV (Through mold via), which is a technique of drilling holes in a mold and soldering the mold. The pillar portion 30 has a thickness approximately the same as that of the second semiconductor chip 20, for example, and is arranged on the side of the second semiconductor chip 20 in the horizontal direction. In addition, multiple solder balls may be arranged instead of the pillar portion 30, and the lower terminal electrode of the first semiconductor chip 10 and the upper terminal electrode of the redistribution layer 40 may be electrically connected by the solder balls.
[0088] The rewiring layer 40 is a wiring layer having a terminal pitch conversion function, which is a function of the package substrate, and is a layer in which a rewiring pattern is formed of polyimide, copper wiring, etc. on the insulating film on the lower side of the second semiconductor chip 20 and on the lower surface of the pillar portion 30. The rewiring layer 40 is formed in a state in which the first semiconductor chip 10 (first semiconductor substrate 100), the second semiconductor chip 20, etc. are turned upside down (see (d) of FIG. 4).
[0089] The rewiring layer 40 electrically connects the terminal electrodes on the underside of the second semiconductor chip 20 and the terminal electrodes of the first semiconductor chip 10 via the pillar parts 30 to the terminal electrodes of the substrate 50. The terminal pitch of the substrate 50 is wider than the terminal pitch of the pillars 31 and the terminal pitch of the second semiconductor chip 20. Various electronic components 51 may be mounted on the substrate 50. Furthermore, when there is a large difference between the terminal pitches of the rewiring layer 40 and the substrate 50, an inorganic interposer or the like may be used between the rewiring layer 40 and the substrate 50 to electrically connect the rewiring layer 40 and the substrate 50.
[0090] The circuit board 60 is a board on which the first semiconductor chip 10 and the second semiconductor chip 20 are mounted, and has a plurality of through electrodes therein electrically connected to a board 50 connected to the first semiconductor chip 10, the second semiconductor chip 20, and electronic components 51, etc. In the circuit board 60, the terminal electrodes of the first semiconductor chip 10 and the second semiconductor chip 20 are electrically connected to terminal electrodes 61 provided on the rear surface of the circuit board 60 by the plurality of through electrodes.
[0091] (An example of a manufacturing method for a semiconductor device) Next, an example of a method for manufacturing the semiconductor device 1 will be described with reference to Fig. 2 to Fig. 4. Fig. 2 is a diagram sequentially showing a method for manufacturing the semiconductor device shown in Fig. 1. Fig. 3 is a diagram showing in more detail a bonding method (hybrid bonding) in the method for manufacturing the semiconductor device shown in Fig. 2. Fig. 4 is a diagram sequentially showing steps subsequent to the steps shown in Fig. 2 in the method for manufacturing the semiconductor device shown in Fig. 1.
[0092] The semiconductor device 1 can be manufactured, for example, through the following steps (a) to (n). (a) A step of preparing a first semiconductor substrate 100 corresponding to a first semiconductor chip 10. (b) A step of preparing a second semiconductor substrate 200 corresponding to the second semiconductor chip 20. (c) A process of polishing the surface 101a of the first semiconductor substrate 100 using a polishing method such as a CMP method or polishing using a surface planer so that each surface 103a of the terminal electrodes 103 is at the same position or protrudes from the surface 102a of the insulating film 102 (see (a) of Figure 3). (d) A process of polishing the surface 201a of the second semiconductor substrate 200 using a polishing method such as a CMP method or polishing using a surface planer so that each surface 203a of the terminal electrodes 203 is at the same position or protrudes from the surface 202a of the insulating film 202 (see (a) of Figure 3). (e) As shown in FIG. 2(b), a step of dicing the second semiconductor substrate 200 to obtain a plurality of semiconductor chips 205. (f) A step of aligning the terminal electrodes 203 of each of the multiple semiconductor chips 205 with the terminal electrodes 103 of the first semiconductor substrate 100 as shown in (c) of FIG. (g) A step of bonding the insulating film 102 of the first semiconductor substrate 100 and each insulating film 202b of the multiple semiconductor chips 205 to each other (see FIG. 2(d) and FIG. 3(b)). At this time, heat H, pressure, or both may be applied. (h) A step of bonding the terminal electrodes 103 of the first semiconductor substrate 100 to the terminal electrodes 203 of each of the plurality of semiconductor chips 205 (see FIG. 3(c)). (i) A step of forming a plurality of pillars 300 (corresponding to pillars 31) between a plurality of semiconductor chips 205 on the connection surface of the first semiconductor substrate 100 (see FIG. 4(a)). (j) A step of molding a resin 301 onto the connection surface of the first semiconductor substrate 100 so as to cover the semiconductor chip 205 and the pillars 300 to obtain a semi-finished product M1 (see FIG. 4(b)). (k) A process of obtaining a semi-finished product M2 by grinding and thinning the resin 301 side of the semi-finished product M1 molded in the process (j) (see FIG. 4(c)). (l) A step of forming a wiring layer 400 corresponding to the rewiring layer 40 on the semi-finished product M2 thinned in the step (k) (see FIG. 4(d)). (m) A step of cutting the semi-finished product M3 on which the wiring layer 400 has been formed in the step (l) along the cutting lines A so as to obtain individual semiconductor devices 1 (see FIG. 4(d)). (n) A step of inverting the semiconductor device 1a separated in step (m) and placing it on the substrate 50 and the circuit board 60 (see FIG. 1).
[0093] For example, in the manufacturing method of a semiconductor device of the present disclosure, step (1) corresponds to the above-mentioned steps (a) and (c), step (2) corresponds to the above-mentioned steps (b) and (d), step (3) corresponds to step (e), step (4) corresponds to step (g), and step (5) corresponds to step (h). Furthermore, the hybrid bonding insulating film forming material of the present disclosure may be an insulating film forming material for use in producing at least one of the first organic insulating film and the second organic insulating film in the manufacturing method of a semiconductor device.
[0094] Step (a) is a step of preparing a first semiconductor substrate 100, which is a silicon substrate on which an integrated circuit composed of semiconductor elements and wiring connecting them is formed, corresponding to a plurality of first semiconductor chips 10. In step (a), as shown in FIG. 2(a), a plurality of terminal electrodes 103 (first electrodes) made of copper, aluminum, etc. are provided at predetermined intervals on one surface 101a of a first substrate body 101 made of silicon, etc., and an insulating film 102 (first insulating film) which is a hardened product obtained by hardening the hybrid bonding insulating film forming material of the present disclosure is provided. When the insulating film forming material is a photosensitive material such as a negative photosensitive insulating film forming material or a positive photosensitive insulating film forming material, the insulating film 102 may be provided on the one surface 101a of the first substrate body 101 before providing the plurality of terminal electrodes 103, or the insulating film 102 may be provided on the one surface 101a of the first substrate body 101 before providing the plurality of terminal electrodes 103. When the insulating film forming material is a non-photosensitive material, the insulating film 102 may be provided after the terminal electrodes 103 are provided on the first surface 101a of the first substrate body 101.
[0095] Step (b) is a step of preparing a second semiconductor substrate 200, which is a silicon substrate on which an integrated circuit having semiconductor elements and wiring connecting them is formed, corresponding to a plurality of second semiconductor chips 20. In step (b), as shown in FIG. 2(a), a plurality of terminal electrodes 203 (a plurality of second electrodes) made of copper, aluminum, or the like are continuously provided on one surface 201a of a second substrate body 201 made of silicon or the like, and an insulating film 202 (a second insulating film) which is a cured product obtained by curing the hybrid bonding insulating film forming material of the present disclosure is provided. When the insulating film forming material is a photosensitive material such as a negative-type photosensitive insulating film forming material or a positive-type photosensitive insulating film forming material, the insulating film 202 may be provided on the one surface 201a of the second substrate body 201 before the plurality of terminal electrodes 203 are provided, or the insulating film 202 may be provided on the one surface 201a of the second substrate body 201 before the plurality of terminal electrodes 203 are provided. When the insulating film forming material is a non-photosensitive material, the insulating film 202 may be provided after the multiple terminal electrodes 203 are provided on the one surface 201a of the second substrate main body 201.
[0096] The insulating films 102 and 202 used in steps (a) and (b) are not limited to a configuration in which both are cured products obtained by curing the hybrid bonding insulating film forming material of the present disclosure, and at least one of the insulating films 102 and 202 may be a cured product obtained by curing the hybrid bonding insulating film forming material of the present disclosure.
[0097] In addition, although FIG. 1 shows an example of C2C bonding, the Chip-to-Wafer (C The present invention may be applied to bonding in a C2W process. In the C2W process, a semiconductor wafer 410 (first semiconductor substrate) is prepared, which has a substrate body 411 (first substrate body), an insulating film 412 (first insulating film) provided on one surface of the substrate body 411, and a plurality of terminal electrodes 413 (first electrodes). Furthermore, a semiconductor substrate (second semiconductor substrate) is prepared, which has a substrate body 421 (second substrate body), an insulating film 422 (second insulating film) provided on one surface of the substrate body 421, and a plurality of terminal electrodes 423 (second electrodes). Then, one surface of the semiconductor wafer 410 and one surface of the second semiconductor substrate before being singulated into the semiconductor chips 420 are polished by a polishing method such as a CMP method or polishing using a surface planer, as in the above steps (c) and (d). Thereafter, a singulation process similar to that in step (e) is performed on the second semiconductor substrate, and a plurality of semiconductor chips 420 are obtained.
[0098] 5(a), the terminal electrodes 423 of the semiconductor chip 420 are aligned with the terminal electrodes 413 of the semiconductor wafer 410 (step (f)). Then, the insulating film 412 of the semiconductor wafer 410 and the insulating film 422 of the semiconductor chip 420 are attached to each other (step (g)), and the terminal electrodes 413 of the semiconductor wafer 410 and the terminal electrodes 423 of the semiconductor chip 420 are bonded to each other (step (h)), to obtain a semi-finished product shown in FIG. 5(b). As a result, the insulating film 412 and the insulating film 422 are bonded to each other to form an insulating bonded portion S3, and the semiconductor chip 420 is attached to the semiconductor wafer 410 mechanically and with high accuracy. Also, the terminal electrodes 413 and the corresponding terminal electrodes 423 are bonded to each other to form an electrode bonded portion S4, and the terminal electrodes 413 and 423 are bonded to each other mechanically and electrically.
[0099] In step (h), as shown in FIG. 2(d), after the bonding in step (g) is completed, heat H, pressure, or both are applied to bond the terminal electrode 103 of the first semiconductor substrate 100 to each of the terminal electrodes 203 of the semiconductor chips 205 as hybrid bonding (see FIG. 3(c)). When the terminal electrodes 103 and 203 are made of copper, the annealing temperature in step (g) is preferably 150° C. or higher and 400° C. or lower, and more preferably 200° C. or higher and 300° C. or lower. In particular, by using the hybrid bonding insulating film forming material of the present disclosure, it is possible to set the annealing temperature low. By such bonding process, the terminal electrode 103 and the corresponding terminal electrode 203 are bonded to form an electrode bonding portion S2, and the terminal electrode 103 and the terminal electrode 203 are mechanically and electrically firmly bonded to each other. The electrode bonding in step (h) may be performed after the bonding in step (g) or may be performed simultaneously with the bonding in step (g).
[0100] 5(c) and 5(d), a plurality of semiconductor chips 420 are bonded to a semiconductor wafer 410, which is a semiconductor wafer, in a similar manner to obtain a semiconductor device 401. Note that the plurality of semiconductor chips 420 may be bonded to the semiconductor wafer 410 one by one by hybrid bonding, or may be bonded to the semiconductor wafer 410 collectively by hybrid bonding.
[0101] In the manufacturing method of such a semiconductor device 401, at least one of the insulating film 412 of the semiconductor wafer 410 and the insulating film 422 of the semiconductor chip 420 is an insulating film that is a cured product obtained by curing the hybrid bonding insulating film forming material of the present disclosure, as in the manufacturing method of the above-mentioned semiconductor device 1. Therefore, a semiconductor device provided with an insulating film having excellent insulating reliability can be obtained.
[0102] (Modification) In the semiconductor device and the method for manufacturing the semiconductor device according to the present disclosure, a configuration in which the first electrode and the second electrode are joined has been described, but the present invention is not limited to this configuration. For example, in the semiconductor device of the present disclosure, the first electrode and the second electrode may be through electrodes that penetrate the first semiconductor substrate and the second semiconductor substrate. The method for manufacturing a semiconductor device according to the present disclosure may be, for example, a method for manufacturing a semiconductor device by using the hybrid bonding insulating film forming material according to the present disclosure in preparing at least one of a first organic insulating film and a second organic insulating film, and by carrying out the following steps (1)' to (5)'. Step (1)' A first semiconductor substrate is prepared, the first semiconductor substrate having a first substrate body and the first organic insulating film provided on one surface of the first substrate body. Step (2)' A second semiconductor substrate is prepared, the second semiconductor substrate having a second substrate body and the second organic insulating film provided on one surface of the second substrate body. Step (3)' The second semiconductor substrate is divided into individual pieces to obtain a plurality of semiconductor chips each having the second organic insulating film. Step (4)' The first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other. Step (5)' A through hole is provided in a part of the bonded first semiconductor substrate and second semiconductor substrate, and a through electrode is provided in the through hole. In the above (5)', the method for providing the through holes and the method for providing the through electrodes are not particularly limited. For example, the through holes may be provided by etching or the like, and the through electrodes may be provided by electrolytic plating, electroless plating, sputtering or the like. EXAMPLES
[0103] The present disclosure will be described in more detail below with reference to examples and comparative examples. Note that the present disclosure is not limited to the following examples.
[0104] (Synthesis Example 1 (Synthesis of A1)) 50g of 3,3',4,4'-biphenylethertetracarboxylic dianhydride (ODPA) and 46g of 1,3-bis(3-aminophenoxy)benzene were dissolved in 640g of 3-methoxy-N,N-dimethylpropionamide. The resulting solution was stirred at 30°C for 2 hours to obtain polyamic acid. Then, 52g of pyridine and 34g of acetic anhydride were added to the resulting polyamic acid solution and heated at 45°C for 5h. This reaction solution was dropped into distilled water, and the precipitate was collected by filtration and dried under reduced pressure to obtain polyimide resin A1. The weight average molecular weight of A1 was determined by gel permeation chromatography (GPC) in terms of standard polystyrene. The weight average molecular weight of A1 was 27000. Specifically, a solution in which 0.5 mg of A1 was dissolved in 1 mL of a solvent [tetrahydrofuran (THF) / dimethylformamide (DMF) = 1 / 1 (volume ratio)] was used, and the measurement was performed under the following conditions. (Measurement conditions) Measuring device: Shimadzu Corporation SPD-M20A Pump: Shimadzu Corporation LC-20AD Column oven: Shimadzu Corporation: CTO-20A Measurement conditions: Column Gelpack GL-S300MDT-5 x 2 Eluent: THF / DMF=1 / 1 (volume ratio) LiBr(0.03mol / L), H3PO4(0.06mol / L) Flow rate: 1.0 mL / min, detector: UV 270 nm, column temperature: 40°C Standard polystyrene: Calibration curves created using Tosoh TSKgel standard Polystyrene Types F-1, F-4, F-20, F-80, and A-2500
[0105] [Examples 1 to 8, Comparative Examples 1 to 5] (Preparation of insulating film forming material) The insulating film-forming materials of Examples 1 to 10 and Comparative Example 1 were prepared as follows, using the components and amounts shown in Table 1. The units of the amount of each component in Table 1 are parts by mass. In addition, "-" in Table 1 means that the corresponding component is not blended. In each Example and Comparative Example, a mixture of each component was kneaded overnight at room temperature in a general solvent-resistant container, and then pressure filtered using a filter with 3 μm pores. The following evaluations were performed using the obtained insulating film-forming materials. For C1 to C5 of component (C), fillers dispersed in a solvent were used. The numerical value in parentheses for component (C) in Table 1 indicates the solid content of the filler per 100 parts by mass of component (A).
[0106] The components in Table 1 are as follows: Component (A) A1: Polyimide resin A1 synthesized in Synthesis Example 1 above ·(B) Component B1: γ-butyrolactone B2: 3-Methoxy-N,N-dimethylpropionamide B3: Cyclohexanone ·(C) component C1: Silica particles (volume average particle size: 50 nm, surface treatment: phenylaminosilane, dispersion solvent: cyclohexanone, non-volatile content: 40% by mass) C2: Silica particles (volume average particle size: 180 nm, surface treatment: phenylaminosilane, dispersion solvent: cyclohexanone, non-volatile content: 50% by mass) C3: Silica particles (volume average particle size: 500 nm, surface treatment: phenylaminosilane, dispersion solvent: cyclohexanone, non-volatile content: 70% by mass) C4: Silica particles (volume average particle size: 22 nm, surface treatment: hydrophobic treatment, dispersion solvent: cyclohexanone, non-volatile content: 30% by mass) C5: Alumina particles (volume average particle size: 60 nm, surface treated, dispersion solvent: dimethylacetamide, non-volatile content: 20% by mass) C6: Silica particles (volume average particle size: 12 nm, powder without surface treatment, no dispersion solvent)
[0107] [Filler dispersion evaluation] The insulating film forming materials of Examples 1 to 10 and Comparative Example 1 were evaluated for filler dispersibility in the insulating film as follows. The insulating film forming material was spin-coated on a Si substrate, and heated and dried on a hot plate at 100°C for 120 seconds, and then heated and dried at 110°C for 120 seconds to form a resin film. The obtained resin film was cured in a vertical diffusion furnace μ-TF under a nitrogen atmosphere at 200°C for 2 hours to obtain a cured product. The cross section of the obtained cured film was observed by SEM, and the dispersibility was evaluated based on the following evaluation criteria. The results are shown in Table 1. -Evaluation criteria- A: The filler is uniformly dispersed in the film, and no aggregates are visible on the cross section of the cured film. B: The filler is uniformly dispersed in the film, but some aggregates are visible on the cross section of the cured film. C: The filler is unevenly dispersed in the film, and many aggregates are observed on the cross section of the cured film.
[0108] (Measurement of thermal expansion coefficient) Cured films were formed as follows using the insulating film forming materials of Examples 1 to 10 and Comparative Example 1, and then the thermal expansion coefficient was measured. The insulating film forming materials were spin-coated on a Si substrate, heated and dried on a hot plate at 100°C for 120 seconds, and then heated and dried at 110°C for 120 seconds, to form a resin film with a thickness of about 10 μm after curing.
[0109] The obtained resin film was cured in a vertical diffusion furnace μ-TF under a nitrogen atmosphere at a curing temperature of 200°C for 2 hours to obtain a cured product with a film thickness of 10 μm. The obtained cured product was molded into a width of 10 mm using a razor to obtain a patterned cured product with a width of 10 mm. Using a TMA tester (TMA2940 manufactured by DuPont), the linear thermal expansion coefficient of the patterned cured product in the surface direction was measured from 50°C to 100°C under the conditions of an initial sample length of 10 mm, a load of 10 g, and a heating rate of 5°C / min. The results are shown in Table 1 as thermal expansion coefficient (ppm / K).
[0110] [Table 1]
[0111] As shown in Table 1, the thermal expansion coefficients were low, at 50 ppm / K or less, in Examples 1 to 10. On the other hand, in Comparative Example 1, the thermal expansion coefficient was greater than 50 ppm / K. In Example 4, the results of filler dispersibility were inferior to those of Examples 1 to 3, 5 to 7, 9, and 10. The reason for this is presumably that the volume average particle size of the filler in Example 3 was larger than the volume average particle size of the filler in these examples. In Example 8, the results of filler dispersibility were inferior to those of Examples 1 to 3, 5 to 7, 9, and 10. The reason for this is presumably that the filler used in Example 8 was not surface-treated, and therefore the filler was prone to aggregation. [Explanation of symbols]
[0112] Reference Signs List 1, 1a, 401...semiconductor device, 10...first semiconductor chip, 20...second semiconductor chip, 30...pillar portion, 40...rewiring layer, 50...substrate, 60...circuit board, 61...terminal electrode, 100...first semiconductor substrate, 101...first substrate body, 101a...one surface, 102...insulating film (first insulating film), 103...terminal electrode (first electrode), 103a...surface, 200...second semiconductor substrate, 201...second substrate body, 201a...one surface, 202...insulating film (second insulating film), 203...terminal electrode (second electrode), 203a...surface, 205 ...semiconductor chip, 300...pillar, 301...resin, 410...semiconductor wafer (first semiconductor substrate), 411...substrate body (first substrate body), 412...insulating film (first insulating film), 413...terminal electrode (first electrode), 420...semiconductor chip (second semiconductor substrate), 421...substrate body (second substrate body), 422...insulating film (second insulating film), 423...terminal electrode (second electrode), A...cutting line, H...heat, M1 to M3...semi-finished product, S1...insulating joint portion, S2...electrode joint portion, S3...insulating joint portion, S4...electrode joint portion.
Claims
1. (A) at least one of a polyimide precursor, which is at least one resin selected from the group consisting of polyamic acid, polyamic acid ester, polyamic acid salt, and polyamic acid amide, and a polyimide resin; (B) a solvent; (C) a filler; and A hybrid bonding insulating film forming material comprising the above compound.
2. 2. The hybrid bonding insulating film forming material according to claim 1, comprising the polyimide resin, the polyimide resin comprising a structure represented by the following formula (E) and a structure represented by the following formula (G). [Formula 1] [chemical 2] In formula (E), C is a divalent linking group containing an ether bond, and in formula (G), D is a divalent linking group having two or more atoms linked to the main chain.
3. The hybrid bonding insulating film forming material according to claim 2 , wherein D in the formula (G) contains an aromatic ring and an ether bond.
4. 3. The hybrid bonding insulating film forming material according to claim 2, wherein the polyimide resin has a structural unit represented by the following general formula (1): [C3] In the general formula (1), X represents a tetravalent organic group represented by the formula (E) above, and Y represents a divalent organic group represented by the formula (G) above.
5. 2. The hybrid bonding insulating film forming material according to claim 1, wherein the volume average particle diameter of the filler is 10 nm to 1 μm.
6. 2. The hybrid bonding insulating film forming material according to claim 1, wherein the filler has been subjected to a surface treatment.
7. The hybrid bonding insulating film forming material according to claim 1 , wherein the solvent contains an ester compound.
8. A method for manufacturing a semiconductor device, comprising the steps of: preparing at least one of a first organic insulating film and a second organic insulating film using the hybrid bonding insulating film forming material according to any one of claims 1 to 7; and bonding the first organic insulating film and the second organic insulating film.
9. forming a first electrode on a first substrate body and then forming a first organic insulating film around the first electrode to prepare a first semiconductor substrate having the first organic insulating film and the first electrode provided on one surface of the first substrate body; forming a second electrode on a second substrate body and then forming a second organic insulating film around the second electrode to prepare a second semiconductor substrate having the second organic insulating film and the second electrode provided on one surface of the second substrate body; singulating the second semiconductor substrate to obtain a plurality of semiconductor chips; a step of bonding the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip to each other and joining the first electrode of the first semiconductor substrate to the second electrode of the semiconductor chip; The method for manufacturing a semiconductor device according to claim 8 , comprising:
10. a first semiconductor substrate having a first substrate body, a first organic insulating film and a first electrode provided on one surface of the first substrate body; a semiconductor chip having a semiconductor chip substrate body and a second organic insulating film and a second electrode provided on one surface of the semiconductor chip substrate body; the first organic insulating film of the first semiconductor substrate and the second organic insulating film of the semiconductor chip are bonded to each other, and the first electrode of the first semiconductor substrate and the second electrode of the semiconductor chip are bonded to each other, A semiconductor device, wherein at least one of the first organic insulating film and the second organic insulating film is an organic insulating film formed by curing the hybrid bonding insulating film forming material according to any one of claims 1 to 7.