Method of manufacturing solid-state battery, and anode active material layer

By treating silicon particles with hydrogen fluoride and applying controlled pressure to the negative electrode active material layer, the electrical resistance and strength issues in silicon-based solid-state batteries are addressed, ensuring crack resistance and low resistance.

JP2024155024AActive Publication Date: 2024-10-31TOYOTA JIDOSHA KK
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023069373
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

The oxidation of silicon negative electrode active material surfaces to form silicon oxide results in increased electrical resistance and reduced strength of the negative electrode active material layer in solid-state batteries, leading to potential cracking during charging.

Method used

Treat silicon particles with hydrogen fluoride to remove silicon oxide, disperse them with a binder and solid electrolyte in an organic solvent, apply the composite slurry to a base material, dry, and laminate with a solid electrolyte layer under controlled roll press pressure to form a negative electrode active material layer.

Benefits of technology

Reduces electrical resistance and enhances the strength of the negative electrode active material layer, preventing cracks during charging while maintaining low resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155024000001
    Figure 2024155024000001
  • Figure 2024155024000002
    Figure 2024155024000002
Patent Text Reader

Abstract

To provide a method of manufacturing a solid-state battery, the method enabling reduction of the electric resistance thereof by using silicon anode active material particles processed by hydrogen fluoride, and furthermore the method enabling improvement of strength of an anode active material layer having the silicon anode active material particles, to provide an anode active material layer for use in the manufacturing of such a solid-state battery, to provide a method of manufacturing a solid-state battery which has small electric resistance and in which cracking hardly occurs in an anode active material layer during charging, and to provide an anode active material layer for use in manufacturing of such a solid-state battery.SOLUTION: A method of manufacturing a solid-state battery includes: providing silicon particles which are provided by hydrogen fluoride; obtaining an anode mixture slurry by dispersing the silicon particles, a binder and a solid electrolyte in an organic solvent; obtaining an anode active material layer by applying the anode mixture slurry to a substrate and then drying the anode mixture slurry; and laminating and pressing the anode active material layer and the solid electrolyte layer. In the method of manufacturing the solid-state battery, a ratio of a mass of the binder in the anode active material layer with respect to a mass of the silicon particles is 0.6 mass% to 3.0 mass% and a roll press pressure in the press is 1.0 t / cm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a solid-state battery and a negative electrode active material layer. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as an active material for batteries, particularly lithium ion batteries.

[0003] For example, Patent Document 1 discloses an active material for use in an all-solid-state battery, which contains at least Si and has an infrared spectrum of 900 cm -1 More than 950cm -1 The maximum peak intensity below is I1, and the maximum peak intensity below 1000cm is I2. -1 More than 1100cm -1 The document discloses an active material in which, when the maximum peak intensity below is I2, the I1 and I2 satisfy 0.55≦I2 / I1≦1.0 and 0.01≦I1.

[0004] Patent Document 2 describes an all-solid-state battery in which a positive electrode layer, a solid electrolyte layer, and a negative electrode layer are laminated in this order, the negative electrode layer contains a negative electrode active material having a silicon clathrate II type crystal phase, the all-solid-state battery is applied with a confining pressure of 0 MPa or more and less than 5 MPa in the lamination direction, and the specific surface area of ​​the negative electrode active material is 8 m 2 / g or more 17m 2 / g or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-077326 [Patent Document 2] Patent Publication No. 2022-092725 Summary of the Invention [Problem to be solved by the invention]

[0006] When the surface of a silicon negative electrode active material is oxidized to form silicon oxide, the electrical resistance of the resulting negative electrode active material may become large when the silicon oxide is used in a negative electrode active material layer of a battery due to the low electrical conductivity of the silicon oxide. Therefore, the present inventors have investigated removing silicon oxide from the surface of silicon negative electrode active material particles by treating silicon particles with hydrogen fluoride.

[0007] However, the present inventors have found that when such silicon negative electrode active material particles treated with hydrogen fluoride are used in a negative electrode active material layer, the strength of the resulting negative electrode active material layer may be reduced.

[0008] Therefore, the present disclosure aims to provide a method for manufacturing a solid-state battery that can reduce electrical resistance by using silicon negative electrode active material particles treated with hydrogen fluoride, while improving the strength of a negative electrode active material layer having such silicon negative electrode active material particles, and a negative electrode active material layer used in the manufacture of such a solid-state battery.The present disclosure also aims to provide a method for manufacturing a solid-state battery that has low electrical resistance and is less likely to crack during charging, and a negative electrode active material layer used in the manufacture of such a solid-state battery. [Means for solving the problem]

[0009] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> Providing silicon particles treated with hydrogen fluoride; dispersing the silicon particles, the binder, and the solid electrolyte in an organic solvent to obtain a negative electrode mixture slurry; The negative electrode mixture slurry is applied to a substrate and then dried to obtain a negative electrode active material layer; and laminating and pressing the negative electrode active material layer and the solid electrolyte layer; Contains The ratio of the mass of the binder to the mass of the silicon particles in the negative electrode active material layer is 0.6% by mass to 3.0% by mass, and The roll press pressure in the press is 1.0 t / cm or more; How solid-state batteries are manufactured. <Aspect 2> 2. The method according to aspect 1, wherein the roll press pressure is 1.2 t / cm to 2.5 t / cm. <Aspect 3> 3. The method according to claim 1 or 2, wherein the proportion is 1.0% by mass to 2.0% by mass. <Aspect 4> Weight per unit area is 5.0mg / cm 2 ~10.0mg / cm 2 The method according to any one of aspects 1 to 3, wherein the negative electrode mixture slurry is applied to the substrate so as to obtain a negative electrode mixture slurry having a thickness of 100 nm to 150 nm. <Aspect 5> A porous silicon clathrate, a binder, and a solid electrolyte, The ratio of the mass of the binder to the mass of the porous silicon clathrate is 0.6% by mass to 3.0% by mass. Negative electrode active material layer. Aspect 6 The negative electrode active material layer according to aspect 5, wherein the proportion is 1.0% by mass to 2.0% by mass. Aspect 7 The negative electrode active material layer according to aspect 5 or 6 is included, and Resistance is 150 Ω cm 2 Below is the solid state battery. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a method for manufacturing a solid-state battery that can reduce electrical resistance by using silicon negative electrode active material particles treated with hydrogen fluoride, while improving the strength of a negative electrode active material layer having such silicon negative electrode active material particles, and a negative electrode active material layer used in the manufacture of such a solid-state battery. Also, according to the present disclosure, it is possible to provide a method for manufacturing a solid-state battery that has low resistance and is less likely to crack during charging, and a negative electrode active material layer used in the manufacture of such a solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0012] <<Method for manufacturing solid-state batteries>> The method of the present disclosure for manufacturing a solid-state battery includes providing silicon particles treated with hydrogen fluoride, dispersing the silicon particles, a binder, and a solid electrolyte in an organic solvent to obtain an anode composite slurry, applying the anode composite slurry to a substrate and then drying to obtain an anode active material layer, and laminating and pressing the anode active material layer and the solid electrolyte layer. In addition, the method of the present disclosure for manufacturing a solid-state battery includes a method in which the ratio of the mass of the binder to the mass of the silicon particles in the anode active material layer is 0.6% by mass to 3.0% by mass, and the roll press pressure in the press is 1.0 t / cm or more.

[0013] According to the method disclosed herein, the strength of the anode active material layer having the silicon anode active material particles treated with hydrogen fluoride can be improved while reducing the electrical resistance by using the silicon anode active material particles. Without being limited by theory, it is believed that this is because the silicon anode active material particles treated with hydrogen fluoride, i.e., the silicon anode active material particles from which oxygen on the surface is at least partially removed, are combined with an appropriate amount of binder and an appropriate pressing pressure (roll pressing pressure), and while taking advantage of the low resistance of the silicon anode active material particles treated with hydrogen fluoride, the anode active material layer having the silicon anode active material particles can be provided with an appropriate strength.

[0014] In the present disclosure, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. Also, the solid-state battery of the present disclosure may be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.

[0015] <Providing silicon particles treated with hydrogen fluoride> The disclosed method for producing a solid-state battery includes providing silicon particles that have been treated with hydrogen fluoride. Such treatment with hydrogen fluoride, particularly with an aqueous hydrogen fluoride solution, can remove silicon oxide from the surface of the silicon anode active material particles.

[0016] The method for treating silicon particles with hydrogen fluoride is not particularly limited, but an example thereof is a method in which an aqueous hydrogen fluoride solution is added to water in which silicon particles are dispersed, and then mixed.

[0017] The silicon particles may be porous silicon clathrate.

[0018] The method for producing the porous silicon clathrate is not particularly limited, but an example thereof is a method in which silicon and metallic lithium are mixed to obtain a lithium silicon (LiSi) alloy, and the obtained LiSi alloy is reacted with ethanol.

[0019] <Negative electrode mixture slurry manufacturing process> The disclosed method of manufacturing a solid-state battery includes dispersing silicon particles, a binder, and a solid electrolyte in an organic solvent to obtain an anode mix slurry.

[0020] The dispersion method is not particularly limited, but may be, for example, a method in which a solution in which each raw material is dispersed is subjected to ultrasonic treatment.

[0021] For silicon particles, reference may be made to the above description in this disclosure.

[0022] The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), or styrene butadiene rubber (SBR), or a combination thereof, and is preferably SBR.

[0023] The material of the solid electrolyte is not particularly limited. For example, the solid electrolyte may be a sulfide solid electrolyte, an oxide solid electrolyte, a polymer electrolyte, or the like, and is preferably a sulfide solid electrolyte.

[0024] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl xetc.; or combinations thereof, but are not limited to these.

[0025] Examples of the organic solvent include non-polar solvents such as heptane, xylene, and toluene, and polar solvents such as ester solvents, tertiary amine solvents, ether solvents, thiol solvents, and ketone solvents. The organic solvent is preferably a polar solvent, more preferably a ketone solvent, and even more preferably diisobutyl ketone.

[0026] <Negative electrode active material layer manufacturing process> The disclosed method of manufacturing a solid-state battery includes applying an anode mix slurry to a substrate and then drying to obtain an anode active material layer.

[0027] The ratio of the mass of the binder to the mass of the silicon particles in the negative electrode active material layer is 0.6% by mass to 3.0% by mass. When the amount of the binder is within the above range, the resistance of the obtained solid state battery can be reduced.

[0028] This ratio is preferably 1.0 mass% to 2.0 mass%, more preferably 1.1 mass% to 1.8 mass%, and even more preferably 1.2 mass% to 1.6 mass%. By setting this ratio within the above range, the resistance of the obtained solid battery can be reduced, and the occurrence of cracks in the negative electrode active material layer can be suppressed.

[0029] The coating method is not particularly limited, but may be, for example, a blade coating method.

[0030] In the method of the present disclosure for producing a solid-state battery, the negative electrode mixture slurry is applied to a substrate at a basis weight of 5.0 mg / cm 2 ~10.0mg / cm 2 It is preferable to set the density to 5.5 mg / cm 2 ~9.0mg / cm 2 More preferably, it is 6.0 mg / cm 2 ~8.0mg / cm 2By setting the basis weight within the above range, the resistance of the obtained solid-state battery can be further reduced.

[0031] The drying method is not particularly limited, but an example thereof is a method in which the substrate is left standing on a heated hot plate.

[0032] The substrate is not particularly limited, but is preferably one that can be used as a negative electrode current collector layer.

[0033] <Pressing process> The disclosed method of manufacturing a solid-state battery includes stacking and pressing a negative electrode active material layer and a solid electrolyte layer.

[0034] The roll press pressure in the press is 1.0 t / cm or more. When the roll press pressure is 1.0 t / cm or more, it is possible to transfer the solid electrolyte layer to the negative electrode active material layer, and the resistance of the obtained solid battery can be reduced.

[0035] The roll press pressure is preferably from 1.2 t / cm to 2.5 t / cm, more preferably from 1.3 t / cm to 2.4 t / cm, and further preferably from 1.4 t / cm to 2.3 t / cm.

[0036] The pressing pressure in the present disclosure refers to the line pressure applied when pressing with a roll press machine.

[0037] The negative electrode active material layer used is that obtained in the above-described negative electrode active material layer production process in this disclosure.

[0038] The mass ratio of the silicon particles to the solid electrolyte in the negative electrode active material layer (mass of silicon particles:mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0039] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.

[0040] The solid electrolyte layer includes at least a solid electrolyte. In addition to the solid electrolyte, the solid electrolyte layer may include a binder or the like as necessary. For the solid electrolyte and the binder, the above description regarding the negative electrode mixture slurry manufacturing process of the present disclosure can be referred to.

[0041] The thickness of the solid electrolyte layer is, for example, 0.1 to 1000 μm. The thickness of the solid electrolyte layer is preferably 0.1 to 300 μm, and particularly preferably 0.1 to 100 μm.

[0042] The method of the present disclosure for producing a solid-state battery may further include a step of laminating an anode current collector layer, an anode active material layer, a solid electrolyte layer, a cathode active material layer, and a cathode current collector layer in this order.

[0043] (Negative electrode current collector layer) The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, the material may be stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, a resin current collector, or the like, but is not limited to these.

[0044] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0045] (Negative electrode active material layer) For the negative electrode active material layer, the above description in this disclosure can be referred to.

[0046] (solid electrolyte layer) For the solid electrolyte layer, reference may be made to the above description in this disclosure.

[0047] (Cathode active material layer) The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.

[0048] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y M y The material may be, but is not limited to, a Li-Mn spinel substituted with a different element having a composition represented by O4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn).

[0049] For the solid electrolyte, the conductive assistant, and the binder, reference can be made to the above description regarding the negative electrode mixture slurry production process of the present disclosure.

[0050] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0051] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0052] (Positive electrode current collector layer) The material and shape of the positive electrode current collector layer are not particularly limited, and the above description of the negative electrode active material layer of the present disclosure can be referred to. In particular, the material of the positive electrode current collector layer is preferably aluminum. The shape is preferably a foil.

[0053] The solid-state battery obtained by the method of the present disclosure includes the negative electrode active material layer of the present disclosure and has a resistance of 150 Ω cm 2 The following is the result. EXAMPLES

[0054] <<Creating a solid-state battery>> The solid-state batteries of each example were fabricated as follows.

[0055] <Production of hydrogen fluoride-treated silicon particles> Si powder was prepared as a silicon (Si) source. This Si source and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0 and mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere to obtain silicon particles. The obtained silicon particles had a porous structure.

[0056] The obtained silicon particles were added to ion-exchanged water, and while stirring at room temperature, a 46 wt% aqueous hydrogen fluoride solution was added dropwise over 10 minutes, and the mixture was stirred at room temperature for 30 minutes. After stirring, the suspension was poured into a 1 L centrifuge bottle, and the solid and liquid were separated using a centrifuge (9000 rpm), and the supernatant was removed by decantation. Methanol was added to the settled solid, and the mixture was stirred, then centrifuged again, and the supernatant was decanted. This operation was repeated three times. The obtained solid was dried in a vacuum at 100°C for 12 hours to obtain hydrogen fluoride-treated silicon particles.

[0057] <Formation of negative electrode active material layer> Example 1 7.0 g of hydrogen fluoride-treated silicon particles, 5.9 g of sulfide solid electrolyte, 0.91 g of vapor-grown carbon fiber (VGCF-H) as a conductive additive, 1.95 g of a 5 wt % diisobutyl ketone (DIBK) solution of styrene butadiene rubber (SBR) as a binder, and 26.4 g of DIBK were placed in a glass container and ultrasonically treated for 50 minutes using an ultrasonic homogenizer with an amplitude of 40 μm / frequency of 20 kHz / horn diameter of 13 mm to obtain a negative electrode composite slurry.

[0058] The obtained negative electrode mixture slurry was mixed with a 1.8 mg / cm 2 or 7.1 mg / cm 2The coating was applied to a nickel foil with a blade of 8 cm wide x 30 cm long so that the coating was 8 cm wide x 30 cm long, and then dried on a hot plate at 50°C for 30 minutes, and then dried on a hot plate at 150°C for 30 minutes. After drying, the coated foil was cut to a length of 8 cm. In this way, a negative electrode active material layer was formed on the nickel foil as a negative electrode current collector layer. In Example 1, the ratio of the mass of the binder to the mass of the silicon particles in the negative electrode active material layer was 0.6 mass%.

[0059] <Formation of solid electrolyte layer> 40g of sulfide solid electrolyte, 8g of 5wt% heptane solution of SBR, 25g of heptane, and 8g of dibutyl ether were placed in a plastic container. Magnetic media was then added and the mixture was dispersed for 1 hour at 2500 rpm in a magnetic barrel mixer. The magnetic media was then removed to obtain a solid electrolyte slurry.

[0060] The obtained solid electrolyte slurry was mixed with a 5.5 mg / cm 2 The coating was applied to a stainless steel foil with a width of 8 cm and a length of 30 cm, and then dried on a hot plate at 50°C for 30 minutes, and then dried on a hot plate at 150°C for 30 minutes. After drying, the foil was cut to a length of 8 cm. This formed a solid electrolyte layer on the stainless steel foil.

[0061] <Formation of Positive Electrode Active Material Layer> 80 g of nickel-cobalt-manganese oxide (NCM) active material, 9.5 g of sulfide solid electrolyte, 2.0 g of conductive additive (VGCF-H), 9.6 g of a 5 wt% SBR solution in DIBK, and 32 g of DIBK were placed in the dispersion vessel of a thin-film swirling high-speed mixer and dispersed at a peripheral speed of 25 m / s for 20 minutes to obtain a positive electrode composite slurry.

[0062] The obtained positive electrode mixture slurry was applied to a substrate having a basis weight of 4.5 mg / cm2 or 17.9 mg / cm2. 2The coating was applied to a stainless steel foil with a width of 8 cm and a length of 30 cm so that the positive electrode active material layer was formed on the stainless steel foil, and then dried on a hot plate at 50° C. for 30 minutes, and then dried on a hot plate at 150° C. for 30 minutes. After drying, the coated foil was cut to a length of 8 cm. This formed a positive electrode active material layer on the stainless steel foil.

[0063] <Transfer of solid electrolyte layer> The solid electrolyte layer was superimposed on the negative electrode active material layer, and pressed using a roll press machine so that the roll press pressure was a linear pressure of 0.25 t / cm, 0.4 t / cm, 1.5 t / cm, or 2.2 t / cm, to transfer the solid electrolyte layer to the negative electrode active material layer.

[0064] <Transfer of Positive Electrode Active Material Layer> The stainless steel foil on this solid electrolyte layer was peeled off, and the positive electrode active material layer was superimposed on the solid electrolyte layer. Pressing was performed using a roll press machine so that the roll press pressure was a linear pressure of 0.25 t / cm, 0.4 t / cm, 1.5 t / cm, or 2.2 t / cm, and the positive electrode active material layer was transferred to the solid electrolyte layer.

[0065] 〈Densification〉 The stainless steel foil on the positive electrode active material layer was peeled off, and the sample in which the negative electrode current collector layer, the negative electrode active material layer, the solid electrolyte layer, and the positive electrode active material layer were laminated in this order was pressed at a linear pressure of 4.0 t / cm using a roll press.

[0066] Sealing Unnecessary portions were cut off so that the battery dimensions were 7 cm square, aluminum foil was attached onto the positive electrode active material layer, the tab was ultrasonically welded, and the battery was sealed in an aluminum pouch.

[0067] (Example 2 and Comparative Example 1) The negative electrode active material layers of Example 2 and Comparative Example 1 were formed in the same manner as in Example 1, except that in forming the negative electrode active material layer, the ratio of the mass of the binder to the mass of the silicon particles was changed as shown in Table 1.

[0068] "evaluation" <Transcribing possible or not> The negative electrode active material layer and the solid electrolyte layer were laminated and pressed to evaluate whether they could be transferred. The results are shown in Table 1. <resistance> The resistance of the solid-state batteries of the examples and comparative examples was measured by a general method. The results are shown in Table 1. In the tables shown in this disclosure, "Si" means silicon particles.

[0069] [Table 1]

[0070] As shown in Table 1, in all the examples, the solid electrolyte layer could be transferred to the negative electrode active material layer. Furthermore, in Examples 1 and 2 in which the ratio of the mass of the binder to the mass of the silicon particles was within the range of the present disclosure, the resistance was smaller than that of Comparative Example 1.

[0071] On the other hand, some cracks occurred in the negative electrode active material layer in Example 1. Therefore, in the following example, a manufacturing method for a solid-state battery having low resistance and no cracks occurring in the negative electrode active material layer was further investigated.

[0072] (Examples 3 and 4, and Comparative Examples 2 to 5) The negative electrode active material layers of Examples 3 and 4 and Comparative Examples 2 to 5 were formed in the same manner as in Example 1, except that in forming the negative electrode active material layer, the ratio of the mass of the binder to the mass of the silicon particles, the negative electrode basis weight, and the pressing pressure were changed as shown in Table 2.

[0073] For these examples, the transferability and resistance were evaluated in the same manner as above. In addition, the presence or absence of cracks in the negative electrode active material layer was visually determined. The results are shown in Table 2.

[0074] [Table 2]

[0075] As shown in Table 2, in Comparative Examples 2 to 4 in which the ratio of the binder mass to the silicon particle mass was 1.4 mass% or less and the pressing pressure was less than 1.0 t / cm, which is outside the range of the present disclosure, it was not possible to transfer the solid electrolyte layer to the negative electrode active material layer.

[0076] In contrast, in Examples 2 to 4, in which the ratio was set to 1.4 mass% within the range of the present disclosure and the pressing pressure was set to 1.5 t / cm or 2.2 t / cm within the range of the present disclosure, the solid electrolyte layer could be transferred to the negative electrode active material layer. Furthermore, in Examples 2 to 4, the resistance was small and no cracks occurred in the negative electrode active material layer.

[0077] Furthermore, the basis weight is 7.1mg / cm 2 As shown, in Examples 3 and 4 in which the negative electrode composite slurry was applied to the nickel foil, the resistance was particularly small.

[0078] On the other hand, when the ratio of the mass of the binder to the mass of the silicon particles was made larger than 3.0 mass%, which is outside the range of the present disclosure, the solid electrolyte layer could be transferred to the negative electrode active material layer, but the resistance was large and cracks occurred in the negative electrode active material layer in Comparative Example 5. Moreover, in Comparative Example 1, no cracks occurred in the negative electrode active material layer, but the resistance was the largest.

Claims

1. Providing silicon particles treated with hydrogen fluoride; dispersing the silicon particles, the binder, and the solid electrolyte in an organic solvent to obtain a negative electrode mixture slurry; The negative electrode mixture slurry is applied to a substrate and then dried to obtain a negative electrode active material layer; and laminating and pressing the negative electrode active material layer and the solid electrolyte layer; Contains The ratio of the mass of the binder to the mass of the silicon particles in the negative electrode active material layer is 0.6 mass% to 3.0 mass%; and The roll press pressure in the press is 1.0 t / cm or more. How solid-state batteries are manufactured.

2. The method according to claim 1, wherein the roll press pressure is from 1.2 t / cm to 2.5 t / cm.

3. The method according to claim 1, wherein the proportion is from 1.0% to 2.0% by weight.

4. Weight per unit area is 5.0 mg / cm 2 ~10.0mg / cm 2 The method of claim 1 , wherein the negative electrode mixture slurry is applied to the substrate so that:

5. A porous silicon clathrate, a binder, and a solid electrolyte; The ratio of the mass of the binder to the mass of the porous silicon clathrate is 0.6% by mass to 3.0% by mass; Negative electrode active material layer.

6. The negative electrode active material layer according to claim 5 , wherein the ratio is 1.0% by mass to 2.0% by mass.

7. The negative electrode active material layer according to claim 5 or 6 is included, and Resistance is 150 Ω cm 2 Below is the solid state battery.

Citation Information

Patent Citations

  • Negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    JP2013229163A

  • Secondary battery, electronic equipment, electric motor-driven tool, electric vehicle and electric power storage system

    JP2018037414A

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158004A

  • Manufacturing method negative electrode active material, and manufacturing method of lithium-ion battery

    JP2024155061A

  • Current collector for lithium-ion secondary cell, manufacturing method thereof and nonaqueous electrolyte secondary cell

    WO2016072090A1