Platinum-phosphite complex-containing hydrosilylation catalyst, method for producing the platinum-phosphite complex-containing hydrosilylation catalyst, and curable organopolysiloxane composition containing the catalyst
A platinum-phosphite complex hydrosilylation catalyst, formed with a silane compound, addresses storage stability issues by remaining liquid at room temperature, enhancing workability and stability in curable organopolysiloxane compositions.
Patent Information
- Application Number
- JP2023069709
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Existing hydrosilylation catalysts containing platinum-phosphite complexes face issues with storage stability at room temperature and require organic solvents, leading to changes in physical properties and increased costs due to refrigeration or freezing requirements.
A platinum-phosphite complex hydrosilylation catalyst is developed, formed by associating a platinum-phosphite complex with a silane compound, which remains liquid at 23°C without organic solvents, ensuring stable physical properties and easy dispersion in curable organopolysiloxane compositions.
The catalyst maintains stability at room temperature, allowing for uniform dispersion and improved workability, resulting in a curable organopolysiloxane composition with stable properties even at elevated temperatures, reducing storage and handling costs.
Smart Images

Figure 2024155216000001 
Figure 2024155216000002 
Figure 2024155216000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a platinum-phosphite complex-containing hydrosilylation catalyst, a curable organopolysiloxane composition using the catalyst, and a method for producing the platinum-phosphite complex-containing hydrosilylation catalyst. [Background technology]
[0002] The addition reaction curable organopolysiloxane composition contains an organohydrogenpolysiloxane having hydrogen atoms bonded to silicon atoms (i.e., hydrosilyl groups), an organopolysiloxane having alkenyl groups such as vinyl groups bonded to silicon atoms, and a platinum-based catalyst.
[0003] In the case of so-called one-liquid organopolysiloxane compositions in which these three components are combined into one composition, when exposed to high temperature conditions, problems arise such as changes in properties such as thickening and gelation, and changes in the physical properties of the organopolysiloxane cured product obtained after curing. To avoid these problems, a method has been adopted in which the components are divided into two or more components and mixed just before use to make a mixed organopolysiloxane composition, or the one-liquid organopolysiloxane composition is transported refrigerated or frozen.
[0004] In the former case, there is a concern that the physical properties of the organopolysiloxane cured product obtained may change due to blending or mixing, so highly advanced blending and mixing techniques are required. In the latter case, refrigeration or freezing conditions are required from storage to use, which increases the transportation and storage costs significantly and is commercially disadvantageous. Against this background, there has been an increasing demand in recent years for one-component organopolysiloxane compositions whose properties and performance do not change even when stored for long periods at room temperature (25°C).
[0005] Patent Documents 1 and 2 propose a method of improving storage stability by using a certain specific phosphite compound. Although these methods dramatically improve storage stability, they have problems such as the fact that a sufficiently cured organopolysiloxane cured product cannot be obtained unless it is exposed to a high temperature of about 150°C, that the phosphite compound is easily hydrolyzed and has poor storage stability in air, and that the catalyst recrystallizes when the coordination number of the phosphite compound is large. Therefore, there is a demand for a platinum-phosphite complex-containing hydrosilylation catalyst that is liquid at 23°C without containing organic solvents, and if such a catalyst can be obtained, a curable organopolysiloxane composition that is free of organic solvents and has stable properties and physical properties can be obtained, so there has been an increasing demand for a platinum-phosphite complex-containing hydrosilylation catalyst that is liquid at 23°C without containing organic solvents. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2021 / 014970 [Patent Document 2] Patent Publication No. 2021-042323 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made to solve these problems, and has as its object to obtain a platinum-phosphite complex-containing hydrosilylation catalyst that is liquid at 23°C even without containing an organic solvent, thereby improving the stability of the properties of the catalyst itself, and to obtain a curable silicone composition that does not contain an organic solvent by using this catalyst in a curable organopolysiloxane composition. Another object of the present invention is to provide an organopolysiloxane composition that has stable properties and physical properties even when exposed to temperatures above room temperature for long periods of time. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention is the result of extensive research and provides a hydrosilylation catalyst containing a platinum-phosphite complex formed by association of a platinum-phosphite complex with a silane compound and / or a partial hydrolysate thereof.
[0009] That is, the present invention provides a platinum-phosphite complex-containing hydrosilylation catalyst which is an association of the following component (A) and component (B), which contains no organic solvent and is liquid at 23°C: (A) a platinum-phosphite complex composed of platinum and a phosphite compound represented by the following general formula (1): [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. and (B) A silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof: [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 is)
[0010] The component (B) is R 2 is preferably an alkoxysilane derivative in which the group is a vinyl group.
[0011] The platinum-phosphite complex-containing hydrosilylation catalyst obtained by associating a complex of a phosphite compound and platinum represented by the above formula (1) with a silane compound represented by the above formula (2) and / or a partial hydrolyzate thereof can be maintained in a liquid state at room temperature. This has the advantages of providing good workability when the catalyst is blended into a curable organopolysiloxane composition, as well as facilitating uniform dispersion.
[0012] The present invention can provide a curable organopolysiloxane composition that contains the above-mentioned platinum-phosphite complex-containing hydrosilylation catalyst and does not contain organic solvents.
[0013] Such a curable organopolysiloxane composition has stable properties and physical characteristics even when exposed to temperatures above room temperature for an extended period of time, and an article having a cured product of the composition can be provided.
[0014] The present invention also provides a method for producing the above platinum-phosphite complex-containing hydrosilylation catalyst composition. That is, the present invention provides a method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, which comprises the following steps (a) to (d): (a) preparing a solution of a phosphite compound represented by the following general formula (1) in a hydrocarbon solvent having a boiling point of 80° C. or less; [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. (b) adding to the solution a platinum compound not containing an organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof to the solution obtained by the above (a) to (b) and dispersing the silane compound and / or a partial hydrolysate thereof to prepare a solution containing an association product of at least a part of the platinum-phosphite ester complex and the silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof; [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) (d) removing the hydrocarbon solvent from the solution obtained in (c).
[0015] By carrying out the above steps (a) to (d), a platinum-phosphite complex-containing hydrosilylation catalyst can be produced stably.
[0016] In the step (c), the molar number of alkenyl groups in the silane compound represented by general formula (2) and / or its partial hydrolysate to be added is preferably within the range of 0.01 to 500 times the molar number of one platinum atom in the platinum compound. If the ratio is 0.01 times or more, the catalyst can maintain its liquid properties at 23° C., and no problems such as poor dispersibility or reduced blending workability will occur in the curable organopolysiloxane composition containing the catalyst due to precipitation of crystals. If the ratio is 500 times or less, the amount of the silane compound represented by general formula (2) and / or its partial hydrolyzate added is not too large, the molecular weight of the siloxane compound itself becomes appropriate, there is no problem with the effect on the viscosity of the obtained platinum-phosphite complex-containing hydrosilylation catalyst, the property stability of the obtained platinum-phosphite complex-containing hydrosilylation catalyst is good, and the workability when blending the catalyst is also good. Effect of the Invention
[0017] The platinum-phosphite complex-containing hydrosilylation catalyst of the present invention is liquid at 23°C even without organic solvent, so the catalyst itself has excellent stability in properties. In addition, when the catalyst is blended into a curable silicone composition, it can be easily dispersed uniformly, and a curable organopolysiloxane composition that does not contain organic solvent can be obtained. The obtained curable organopolysiloxane composition that does not contain organic solvent provides an organopolysiloxane composition that has stable properties and physical properties even when exposed to temperatures above room temperature for a long period of time. Furthermore, since it does not contain organic solvent, etc., a very safe organopolysiloxane cured product can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present inventors have searched for a catalyst useful as a resin curing catalyst, in particular as a curing catalyst for organopolysiloxane compositions, and have found that an association product of platinum and a platinum-phosphite ester complex represented by the following general formula (1) and a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof is useful, and have completed the present invention, including a method for producing the same.
[0019] That is, the present invention provides: (A) Platinum and the following general formula (1) [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. and a platinum-phosphite complex composed of a phosphite compound represented by the formula: (B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof: A platinum-phosphite complex-containing hydrosilylation catalyst comprising: [ka] (In the formula, R 2represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) The hydrosilylation catalyst is The platinum-phosphite complex-containing hydrosilylation catalyst is an association of component (A) and component (B), contains no organic solvent, and is liquid at 23°C.
[0020] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: The present invention relates to a method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, the method comprising the steps of: (a) preparing a solution of a phosphite compound represented by the following general formula (1) in a hydrocarbon solvent having a boiling point of 80° C. or less; [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. (b) adding to the solution a platinum compound not containing an organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof to the solution obtained in the above steps (a) and (b) and dispersing the silane compound and / or a partial hydrolysate thereof to prepare a solution containing an association product of at least a part of the platinum-phosphite ester complex and the silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof; [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) (d) removing the hydrocarbon solvent from the solution obtained in (c).
[0021] [Phosphite ester compounds] The phosphite compound used in the present invention and represented by the following general formula (1) forms a complex with platinum, and is an essential component for dramatically improving the storage stability of the properties and physical properties of the curable organopolysiloxane composition that contains a platinum-phosphite complex-containing hydrosilylation catalyst obtained using this compound. [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.
[0022] In the above general formula (1), R 1 are independently a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms, preferably 1 to 2 carbon atoms, more preferably 1 carbon atom, i.e., a methyl group. Specific examples of the phosphite ester compound include tris(2,4-dimethylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris(2,4-bis(3-ethylpentan-3-yl)phenyl)phosphite, tris(2,4-bis(4-propylheptan-4-yl)phenyl)phosphite, etc. 1 and phosphite compounds having the same carbon number, such as tris(4-(tert-butyl)-2-methylphenyl)phosphite, tris(4-(tert-butyl)-2-ethylphenyl)phosphite, tris(2-(tert-butyl)-4-(3-ethylpentan-3-yl)phenyl)phosphite, and tris(2-(tert-butyl)-4-(3-methylhexan-3-yl)phenyl)phosphite. 1Among these, it is particularly preferable to use tris(2,4-di-tert-butylphenyl)phosphite, which is easily available and has a high storage stability effect.
[0023] The amount of the phosphite compound used in the present invention is optimally more than 0.6 molecules and 3.0 molecules or less per platinum molecule, and more preferably, it is particularly good to add an amount in the range of 0.8 to 2.5 molecules per platinum molecule. Here, when the amount is more than 0.6 molecules per platinum molecule, the storage stability of the curable organopolysiloxane composition containing the catalyst is good, and there is no risk of the organopolysiloxane composition gelling. On the other hand, when the amount is 3.0 molecules or less per platinum molecule, even if the catalyst is associated with a silane compound and / or its partial hydrolyzate, which will be described later, there is no risk of crystallization at room temperature, so the liquid state of the platinum-phosphite complex-containing hydrosilylation catalyst can be sufficiently maintained. Furthermore, the catalyst has good dispersibility in the curable organopolysiloxane composition containing the catalyst, and there is no problem such as a decrease in blending workability.
[0024] [Silane compounds and / or their partial hydrolysates] The compound represented by the following general formula (2) is used in the present invention. [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 is) The silane compound represented by the formula (I) and / or its partial hydrolysate is an essential component for preventing crystallization at room temperature by associating with the above-mentioned complex of platinum and a phosphite compound.
[0025] In the above general formula (2), R 2is an alkenyl group having 2 to 10 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 8 carbon atoms, and among these, particularly preferably a vinyl group. 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a 3-propenyl group, and an isopropenyl group. The group having 1 or 2 carbon atoms is preferable, and the group having 1 carbon atom, i.e., a methyl group, is more preferable. Specific examples of the siloxane compound include vinyl group-containing alkoxysilanes such as vinyltrimethoxysilane, vinyldimethoxymethylsilane, vinyltriethoxysilane, vinyldiethoxymethylsilane, allyltrimethoxysilane, allyldimethoxymethylsilane, 7-octenyltrimethoxysilane, and 7-octenyldimethoxymethylsilane, and / or partial hydrolysates thereof. In the above general formula (2), X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 Specific examples include a methyl group, an ethyl group, a propyl group, a methoxy group, an ethoxy group, a propoxy group, and an isopropoxy group.
[0026] The amount of the silane compound and / or its partial hydrolysate used in the present invention to be added is optimally within the range of 0.05 mol % or more and 100 mol % or less per platinum molecule, and more preferably within the range of 0.05 mol % or more and 90 mol % or less per platinum molecule. Here, when the amount is 0.05 mol% or more per platinum molecule, the resulting platinum-phosphite complex-containing hydrosilylation catalyst does not crystallize at room temperature, can maintain the liquid state of the platinum-phosphite complex-containing hydrosilylation catalyst, and has good dispersibility in the curable organopolysiloxane composition containing the catalyst, and does not cause problems such as a decrease in blending workability. Also, when the amount is 100 mol% or less per platinum molecule, the platinum-phosphite complex-containing hydrosilylation catalyst itself is stable, and the effective platinum amount of the platinum-phosphite complex-containing hydrosilylation catalyst itself does not decrease, so that when a curable organopolysiloxane composition containing the catalyst is obtained, the blending amount is appropriate, and the addition amount of the silane compound and / or its partial hydrolyzate is also appropriate, resulting in good mechanical properties and curability.
[0027] One of the features of the platinum-phosphite complex-containing hydrosilylation catalyst of the present invention is that it does not contain a hydrocarbon organic solvent. Here, "hydrocarbon organic solvent" refers to an aliphatic hydrocarbon solvent or an aromatic hydrocarbon solvent. Aliphatic hydrocarbon solvents include not only hydrocarbon solvents with a boiling point of 80°C or less used in step (a) of the catalyst production method described below, but also aliphatic hydrocarbon solvents with a boiling point of more than 80°C. Specific examples include n-pentane, n-hexane, 2-methylbutane, 2,2-dimethylbutane, 2,3-dimethylbutane, 2-methylpentane, 3-methylpentane, n-heptane, and n-octane. Aromatic hydrocarbons include benzene, toluene, xylene, ethylbenzene, and isopropylbenzene.
[0028] [Use of platinum-phosphite complex-containing hydrosilylation catalysts] The platinum-phosphite complex-containing hydrosilylation catalyst described above can be used for various resin curing catalysts and purification catalysts, but when used as a curing catalyst for organopolysiloxane compositions that are converted into resins (or gels) through hydrosilylation reactions, it can demonstrate its characteristics. The reason is that when heated, it has almost the same curability as conventional platinum compound-based hydrosilylation catalysts, and when stored at room temperature, the phosphite compound forms a complex with platinum, suppressing catalytic activity and causing the hydrosilylation reaction to proceed very slowly. Therefore, the curable organopolysiloxane composition using this catalyst has stable properties and physical properties even when exposed to temperatures above room temperature for a long period of time. Furthermore, by associating the complex of the phosphite compound and platinum with the silane compound represented by the general formula (2) and / or its partial hydrolysate, the resulting platinum-phosphite complex-containing hydrosilylation catalyst can be kept in a liquid state at room temperature. This has the advantage that when this catalyst is blended into a curable organopolysiloxane composition, workability is improved and uniform dispersion is facilitated.
[0029] The amount of platinum-phosphite complex-containing hydrosilylation catalyst in the curable organopolysiloxane composition is 0.001 to 10.0 parts by mass, preferably 0.010 to 5.0 parts by mass, and more preferably 0.050 to 3.0 parts by mass, per 100 parts by mass of the polymer containing an alkenyl group. When the amount of platinum-phosphite complex-containing hydrosilylation catalyst is 0.001 part by mass or more, the strength of the resulting silicone rubber composition is sufficient and there is no curing failure. On the other hand, when the amount of platinum-phosphite complex-containing hydrosilylation catalyst is 10.0 parts by mass or less, the resulting silicone rubber composition does not become discolored or the time until curing is not shortened, and it is also advantageous in terms of cost. The activity of the catalyst, i.e., the adjustment of the curability, can be controlled by increasing or decreasing the concentration of the platinum-phosphite complex-containing hydrosilylation catalyst added.
[0030] [Method for producing a platinum-phosphite complex-containing hydrosilylation catalyst] [Process (a)] Step (a) is a step of preparing a solution in which a phosphite compound represented by general formula (1) is dissolved in a hydrocarbon solvent having a boiling point of 80° C. or lower. [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms.
[0031] When the phosphite compound is liquid at room temperature, a complex can be easily formed by blending it with a platinum compound that does not contain an organic solvent selected from the group consisting of complexes of platinum chloride, chloroplatinic acid or chloroplatinate salts with vinyl group-containing siloxanes in the step (b) described below. However, since many of the phosphite compounds are solid at room temperature, by dissolving the phosphite compound in a hydrocarbon solvent in the step (a) above, it is possible to rapidly form a complex by blending it with a platinum compound that does not contain an organic solvent selected from the group consisting of complexes of platinum chloride, chloroplatinic acid or chloroplatinate salts with vinyl group-containing siloxanes.
[0032] The hydrocarbon solvent having a boiling point of 80° C. or less may be linear or branched. Specific examples of the hydrocarbon solvent having a boiling point of 80° C. or less include n-pentane (boiling point: 36° C.), n-hexane (boiling point: 68° C.), 2-methylbutane (boiling point: 30° C.), 2,2-dimethylbutane (boiling point: 50° C.), 2,3-dimethylbutane (boiling point: 58° C.), 2-methylpentane (boiling point: 62° C.), and 3-methylpentane (boiling point: 63° C.). Among them, n-hexane (boiling point: 68° C.) is particularly suitable because it is relatively easy to handle for industrial use and easy to remove in the subsequent removal process. From the viewpoint of vacuum distillation of the hydrocarbon solvent, it is preferable that the boiling point of the hydrocarbon solvent used is 80° C. or less. In this case, a stable platinum-phosphite complex-containing hydrosilylation catalyst can be obtained by setting the vacuum distillation temperature at 40° C. or lower. In the case of a hydrocarbon solvent having a boiling point of 80° C. or higher, the used hydrocarbon solvent cannot be completely removed unless the vacuum distillation temperature is set at 40° C. or higher, and therefore the hydrocarbon solvent may remain in the platinum-phosphite complex-containing hydrosilylation catalyst or the platinum-phosphite complex-containing hydrosilylation catalyst may decompose due to the temperature in the solvent removal step, resulting in precipitation of crystals.
[0033] In addition, the amount of the hydrocarbon solvent having a boiling point of 80°C or less is not particularly limited. In addition, the temperature at which the phosphite compound represented by general formula (1) is dissolved in the hydrocarbon solvent is 40°C or less, more preferably in the range of 0 to 35°C. If the phosphite compound is dissolved at 40°C or less, the phosphite compound represented by general formula (1) is unlikely to hydrolyze with the moisture contained in the hydrocarbon solvent, so that the phosphite compound represented by (1) does not change to a phosphate compound, and the stability of the resulting platinum-phosphite complex-containing hydrosilylation catalyst is good. In addition, the dissolution time is not particularly limited. It is preferable to select a container for dissolving that can block oxygen.
[0034] difficult [Step (b)] Step (b) is a step of adding to the solution a platinum compound containing no organic solvent, which is selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, and dispersing the compound to prepare a solution containing a platinum-phosphite complex.
[0035] [Organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane] The platinum compound containing no organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, used in the present invention is usually a curing catalyst that promotes the hydrosilylation addition reaction of SiH groups in an organohydrogenpolysiloxane to an alkenyl group-containing polymer contained in a curable organopolysiloxane composition. [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. By forming a complex with the silane compound represented by general formula (2) and / or a partial hydrolyzate thereof, the storage stability of the properties and physical properties of the curable organopolysiloxane composition obtained using the complex can be significantly improved. [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 is) By associating this with a platinum-phosphite complex, a hydrosilylation catalyst can be obtained that is liquid at room temperature without containing an organic solvent, and this makes it possible to improve the uniform dispersion of the catalyst and the stability and uniformity of the properties of the catalyst itself when obtaining a curable organopolysiloxane composition using this catalyst.
[0036] Specific examples of platinum compounds that do not contain organic solvents and are selected from the group consisting of platinum chloride, chloroplatinic acid or chloroplatinate and vinyl group-containing siloxane complexes include platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt complex), platinum-1,3-diallyl-1,1,3,3-tetramethyldisiloxane complex, platinum-1,3-divinyl-1,3-dimethyl-1,3-diphenyldisiloxane complex, platinum-1,1,3,3-tetraphenyldisiloxane complex, and platinum-1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane complex. It is essential that the compound contains at least one hydrosilylation catalyst selected from these groups, and it is also essential that the compound does not contain organic solvents. Of the above-mentioned organic solvent-free hydrosilylation catalysts, it is particularly preferable to use a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt complex).
[0037] The organic solvent-free platinum compound selected from the group consisting of platinum chloride, chloroplatinic acid or chloroplatinate salts and vinyl group-containing siloxanes shown here must be free of basic organic solvents such as aromatic hydrocarbon organic solvents such as toluene and xylene, and alcohol organic solvents such as ethanol, n-butanol, and 2-ethylhexyl alcohol (excluding low molecular weight vinyl group-containing siloxanes such as tetramethyldivinylsiloxane, trimethyltrivinylcyclotrisiloxane, and tetramethyltetravinylcyclotetrasiloxane).
[0038] The platinum compound not containing an organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, is usually used in the form of a solution in a siloxane that forms a ligand of a platinum-siloxane complex. The solution is usually prepared so that the platinum atom content is about 0.001 to 0.010 moles. This is to increase the stability of the platinum-siloxane complex. The mass percentage of platinum contained is 0.2 to 2.0%. Examples of compounds that can form a platinum-siloxane complex are tetramethyldivinylsiloxane, trimethyltrivinylcyclotrisiloxane, and tetramethyltetravinylcyclotetrasiloxane, as shown below. [ka]
[0039] A preferred platinum compound is platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt complex), which is believed to have the following structure: [ka] The time required for this step is preferably 30 minutes or more at a temperature of 40° C. or less. As in step (a), it is preferable to select a container capable of blocking oxygen for this step (b).
[0040] [Process (c)] Step (c) is a step of adding a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof to the solution obtained in the above steps (a) and (b) and dispersing it to prepare a solution containing an association product of at least a part of the platinum-phosphite ester complex and the silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof. [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 is)
[0041] This step is preferably carried out at a temperature of 40°C or less for 60 minutes or more. As in step (a), it is preferable to select a container capable of blocking oxygen for this step. The silane compound represented by general formula (2) and / or its partial hydrolyzate used here is selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate salt with a vinyl group-containing siloxane, and is formed by mixing R in general formula (2) with one platinum atom in a platinum compound not containing an organic solvent. 2 It is preferable to add the silane compound in an amount such that the unit is within the range of 0.01 to 500 times. 2 When the unit is 0.01 times or more, the amount of the silane compound represented by general formula (2) and / or its partial hydrolyzate associated with one platinum atom is sufficient, and the liquid properties can be reliably maintained at 23°C, and there is no problem such as deterioration of dispersibility or reduced blending workability in the curable organopolysiloxane composition containing the catalyst due to precipitation of crystals. 2 When the unit represented by the unit is 500 times or less, the amount of the silane compound represented by general formula (2) and / or its partial hydrolyzate added is appropriate, and the molecular weight of the siloxane compound itself becomes large, and there is no significant effect on the viscosity of the resulting platinum-phosphite complex-containing hydrosilylation catalyst, no deterioration in the property stability of the resulting platinum-phosphite complex-containing hydrosilylation catalyst, no decrease in workability when compounding the catalyst, or other problems.
[0042] [Step (d)] Step (d) is a step of removing the hydrocarbon solvent from the solution obtained in steps (a) to (c). This step is an essential step for removing the hydrocarbon solvent from the solution obtained in steps (a) to (c) to obtain a platinum-phosphite complex-containing hydrosilylation catalyst that does not contain an organic solvent. The solvent removal method used here is preferably a reduced pressure distillation method in which the solvent is distilled off under reduced pressure using a vacuum pump or the like. This is because a stable platinum-phosphite complex-containing hydrosilylation catalyst can be obtained by setting the reduced pressure distillation temperature to 40°C or less. The degree of reduced pressure varies depending on the boiling point of the hydrocarbon solvent used, but the hydrocarbon solvent used can be completely removed by setting the pressure to 50 hPa or less. The method for confirming whether the hydrocarbon solvent used has been completely removed can be confirmed by the weight ratio of the total weight of the phosphite compound, platinum compound, and silane compound used to the platinum-phosphite complex-containing hydrosilylation catalyst obtained after the completion of step (d). When the weight of the resulting platinum-phosphite complex-containing hydrosilylation catalyst is more than the combined weight of the phosphite compound, platinum compound, and silane compound used, the hydrocarbon solvent will remain, and can be completely removed by adding additional time to the present process to remove the hydrocarbon solvent. EXAMPLES
[0043] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited thereto. In the examples, "parts" means "parts by mass" and "%" means "% by mass".
[0044] [Example 1] 0.6622 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25g transparent glass container, 9.3378 parts of n-hexane was added, and the container was sealed and dissolved at room temperature for about 1 hour. After visually confirming that the crystals of tris(2,4-di-tert-butylphenyl)phosphite had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was added, the container was sealed, and the container was stirred for 30 minutes to make the mixture uniform. Then, 0.06 parts of vinyltrimethoxysilane was added, the container was sealed, and the container was stirred for 60 minutes to make the mixture uniform. Then, the solution was transferred to a 100ml eggplant-shaped flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / about 35hPa). In a 100 ml eggplant-shaped flask, 10.31 g of a colorless, transparent liquid was obtained (yield: 96.2%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 1". (The amount of the phosphite compound is 2.0 molecules per platinum molecule in the platinum compound, and the amount of the silane compound is 0.79 molecules per platinum molecule in the platinum compound.)
[0045] [Example 2] 0.3311 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25g transparent glass container, 9.6689 parts of n-hexane was added, and the container was sealed and dissolved at room temperature for about 1 hour. After visually confirming that the crystals of tris(2,4-di-tert-butylphenyl)phosphite had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was added, the container was sealed, and the container was stirred for 30 minutes to make the mixture uniform. Then, 0.06 parts of vinyltrimethoxysilane was added, the container was sealed, and the container was stirred for 60 minutes to make the mixture uniform. Then, the solution was transferred to a 100ml eggplant-shaped flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / about 32hPa). In a 100 ml eggplant-shaped flask, 10.25 g of a colorless, transparent liquid was obtained (yield: 98.7%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated as "Catalyst 2." (The amount of the phosphite compound is 1.0 molecule per platinum molecule in the platinum compound, and the amount of the silane compound is 0.79 molecule per platinum molecule in the platinum compound.)
[0046] [Example 3] 0.3311 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25g transparent glass container, 9.6689 parts of n-hexane was added, and the container was sealed and dissolved at room temperature for about 1 hour. After visually confirming that the crystals of tris(2,4-di-tert-butylphenyl)phosphite had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was added, the container was sealed, and the container was stirred for 30 minutes to make the mixture uniform. Then, 1.00 parts of vinyltrimethoxysilane was added, the container was sealed, and the container was stirred for 60 minutes to make the mixture uniform. Then, the solution was transferred to a 100ml eggplant-shaped flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / about 34hPa). In a 100 ml eggplant-shaped flask, 11.12 g of a colorless, transparent liquid was obtained (yield: 98.1%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated as “Catalyst 3.” (The amount of the phosphite compound is 1.0 molecule per platinum molecule in the platinum compound, and the amount of the silane compound is 13.16 molecules per platinum molecule in the platinum compound.)
[0047] [Example 4] 0.6622 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25g transparent glass container, 9.3378 parts of n-hexane was added, and the container was sealed and dissolved at room temperature for about 1 hour. After visually confirming that the crystals of tris(2,4-di-tert-butylphenyl)phosphite had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was added, the container was sealed, and the container was stirred for 30 minutes to make the mixture uniform. Then, 0.06 parts of 7-octenyltrimethoxysilane (product name: KBM-1083 [manufactured by Shin-Etsu Chemical Co., Ltd.]) was added, the container was sealed, and the container was stirred for 60 minutes to make the mixture uniform. Then, the solution was transferred to a 100ml eggplant-shaped flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 30°C x 2 hours / about 35hPa). In a 100 ml eggplant-shaped flask, 10.31 g of a colorless, transparent liquid was obtained (yield: 96.2%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated as "Catalyst 4." (The amount of the phosphite compound is 2.0 molecules per platinum molecule in the platinum compound, and the amount of the silane compound is 0.50 molecules per platinum molecule in the platinum compound.)
[0048] [Comparative Example 1] The same procedure as in Example 1 was carried out, except that 0.06 parts of 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane was used instead of vinyltrimethoxysilane. As a result, 10.33 g of a colorless, transparent liquid was obtained in a 100 ml eggplant-shaped flask (yield: 96.3%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 5." (The amount of the phosphite compound is 1.0 molecule per platinum molecule in the platinum compound, and the amount of the silane compound is 0 molecule per platinum molecule in the platinum compound. [The amount of the ligand, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, is 0.34 molecules per platinum molecule in the platinum compound.])
[0049] [Comparative Example 2] The same procedure as in Example 1 was carried out except that vinyltrimethoxysilane was omitted. As a result, 10.50 g of a colorless, transparent liquid was obtained in a 100 ml eggplant-shaped flask (yield: 98.5%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 6." (The amount of the phosphite compound is 1.0 molecule per platinum molecule in the platinum compound, and the amount of the silane compound is 0 molecule per platinum molecule in the platinum compound.)
[0050] [Comparative Example 3] 0.3311 parts of tris(2,4-di-tert-butylphenyl)phosphite was weighed into a 25g transparent glass container, 9.6689 parts of n-heptane (boiling point: 98°C) was added, and the container was sealed and dissolved at room temperature for about 1 hour. After visually confirming that the crystals of tris(2,4-di-tert-butylphenyl)phosphite had dissolved, 10.0 parts of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was added, the container was sealed, and the container was stirred for 30 minutes to make the mixture uniform. Then, 0.06 parts of vinyltrimethoxysilane was added, the container was sealed, and the container was stirred for 60 minutes to make the mixture uniform. Then, the solution was transferred to a 100ml eggplant-shaped flask, and n-hexane was distilled off under reduced pressure using a rotary evaporator (conditions: 50°C x 2 hours / about 35hPa). In a 100 ml eggplant flask, a colorless, transparent liquid with dispersed white crystals (yield: 10.95 g) was obtained, but a colorless, transparent liquid could not be obtained (yield: 105.4%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 7." (The amount of the phosphite compound is 1.0 molecule per platinum molecule in the platinum compound, and the amount of the silane compound is 0.79 molecule per platinum molecule in the platinum compound.)
[0051] [Comparative Example 4] The same procedure as in Example 1 was carried out without using n-hexane. As a result, a liquid with dispersed white crystals (yield: 10.33 g) was obtained in a 100 ml eggplant-shaped flask, and a colorless, transparent liquid could not be obtained (yield: 99.9%). This platinum-phosphite complex-containing hydrosilylation catalyst is designated "Catalyst 8."
[0052] The yields and yields of the platinum-phosphite complex-containing hydrosilylation catalysts obtained in the above Examples 1 to 4 and Comparative Examples 1 to 4 are shown in Table 1. In addition, the following tests were carried out on the appearance of the catalysts obtained in these Examples and Comparative Examples. The obtained platinum-phosphite complex-containing hydrosilylation catalyst was stored in a sealed container filled with nitrogen. After storing at 23°C for 7 days, the appearance was checked and the catalyst was judged as passing if no crystals were formed in the container, and failing if crystals were formed. The results are shown in Table 1.
[0053] [Table 1]
[0054] [evaluation] The platinum-phosphite complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 satisfy the requirements of the present invention. In all of the Examples, the amount of the phosphite compound was 1.0 or 2.0 molecules per platinum molecule of the platinum compound. However, the same procedure was performed by increasing the amount of the phosphite compound in increments of 0.1 molecules up to 3.0 molecules per platinum molecule of the platinum compound, and it was confirmed that a colorless, transparent liquid was obtained in all cases. The platinum-phosphite complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 showed suppressed crystal precipitation even after being left at 23°C for 7 days under sealed conditions, indicating that a platinum-phosphite complex-containing hydrosilylation catalyst with highly stable properties was obtained. In contrast, the platinum-phosphite complex-containing hydrosilylation catalysts of Comparative Examples 1 and 2 do not contain the silane compound represented by the general formula (2) and / or its partial hydrolyzate, and therefore crystals precipitate at 23°C for about 7 days. The platinum-phosphite complex-containing hydrosilylation catalyst of Comparative Example 3 uses n-heptane with a boiling point of 80°C or higher as a hydrocarbon solvent for dissolving the phosphite compound. Therefore, even if the temperature of the vacuum distillation is increased, the n-heptane used cannot be completely distilled off. In addition, as a result of increasing the heating temperature, the coordination of the phosphite compound in the platinum-phosphite complex-containing hydrosilylation catalyst is lost, causing crystals to precipitate, and it is not possible to obtain a liquid platinum-phosphite complex-containing hydrosilylation catalyst. In the platinum-phosphite complex-containing hydrosilylation catalyst of Comparative Example 4, the phosphite compound is not dissolved in a hydrocarbon solvent, but is coordinated to the platinum compound. As a result, it is found that the phosphite compound is not dissolved, and a liquid in which crystals are dispersed is obtained. The above results confirm the effectiveness of the catalyst production method of the present invention for obtaining a stable liquid platinum-phosphite complex-containing hydrosilylation catalyst.
[0055] [Examples of Curable Organopolysiloxane Compositions Utilizing Hydrosilylation Catalysts Containing Platinum-Phosphite Complexes] Examples and comparative examples relating to a curable organopolysiloxane composition utilizing the platinum-phosphite complex-containing hydrosilylation catalyst obtained in the present invention will be specifically described below. Note that the following are examples and comparative examples of a one-component millable silicone rubber composition, but the present invention is not limited thereto.
[0056] The evaluation of this example was carried out as follows.
[0057] [About the workability of making one-component millable silicone rubber compositions] In the preparation of the one-component millable silicone rubber compositions prepared in the following Examples and Comparative Examples, those in which the platinum-phosphite complex-containing hydrosilylation catalyst was liquid and no problems occurred when it was added were judged as passing. Conversely, those in which the platinum-phosphite complex-containing hydrosilylation catalyst crystallized during the catalyst blending process and problems occurred in the workability when it was added were judged as failing.
[0058] [Storage stability of one-component millable silicone rubber composition] The storage stability of the one-component millable silicone rubber compositions prepared in the following Examples and Comparative Examples was compared using a rheometer (ALPHA TECHNOLOGIES Rubber Process Analyzer RPA2000) to compare the initial curing properties of the obtained one-component millable silicone rubber compositions with the curing properties after 6 months of storage at 23°C. At this time, those that could be evaluated after 6 months at 23°C were judged to pass. Here, the curing data of the one-component millable silicone rubber compositions are shown as values measured at 150°C. In Table 2, T50* and T50** are calculated assuming that 100% hardening occurs when the torque stabilizes on the time-torque curve at 150°C, and T50 is the time T from when the torque starts to increase to 50%.
[0059] [Composition Example 1] 100 parts by mass of organopolysiloxane raw rubber having an average degree of polymerization of 6,000 and consisting of 99.85 mol % dimethylsiloxane units, 0.125 mol % methylvinylsiloxane units, and 0.025 mol % dimethylvinylsiloxy units, and a BET specific surface area of 200 m 2 55 parts by mass of fumed silica (Aerosil 200, Nippon Aerosil Co., Ltd.) having a molecular weight of 100 / g, 12 parts by mass of dimethyldimethoxysilane, 0.2 parts by mass of vinyltrimethoxysilane, 12 parts by mass of dimethylpolysiloxane having silanol groups at both ends, an average degree of polymerization of 4, and a viscosity of 15 mPa s at 25°C, and 0.15 parts by mass of 3% potassium siliconate were added, and the mixture was heated under mixing in a kneader at 170°C for 2 hours to prepare base compound (1). The base compound (1) is mixed with 100 parts by mass of organopolysiloxane raw rubber to form a rubber composition having a structure of M2D H 20 D 18 (H content: 0.00726 mol / g) (where M: (CH3)3SiO 1 / 2 -, D H :(CH3)HSiO 2 / 2 -,D:(CH3)2SiO 2 / 2 1.7 parts by mass of an organohydrogensiloxane in which H is an integer of 0 to 5, and 0.05 parts by mass of the “catalyst 1” prepared in Example 1 were added using a two-roll mill and mixed uniformly to produce a raw rubber-like one-component silicone rubber composition 1.
[0060] Composition Example 2 A one-component silicone rubber composition 2 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of “Catalyst 2” was used in place of “Catalyst 1”.
[0061] Composition Example 3 A one-component silicone rubber composition 3 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of “Catalyst 3” was used in place of “Catalyst 1”.
[0062] Composition Example 4 A one-component silicone rubber composition 4 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of “Catalyst 4” was used in place of “Catalyst 1”.
[0063] [Comparative Composition Example 1] One-component silicone rubber composition 5 was produced in the same manner as in composition example 1, except that 0.05 parts by mass of “catalyst 5” was used in place of “catalyst 1”.
[0064] [Comparative Composition Example 2] A one-component silicone rubber composition 6 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of “Catalyst 6” was used in place of “Catalyst 1”.
[0065] [Comparative Composition Example 3] One-component silicone rubber composition 7 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of “Catalyst 7” was used in place of “Catalyst 1”.
[0066] [Comparative Composition Example 4] A one-component silicone rubber composition 8 was produced in the same manner as in Composition Example 1, except that 0.05 parts by mass of “Catalyst 8” was used in place of “Catalyst 1”.
[0067] [Comparative Composition Example 5] One-component silicone rubber composition 9 was produced in the same manner as in composition example 1, except that 0.05 parts by mass of a platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex having 1% Pt atoms was used instead of “catalyst 1”.
[0068] [test] The results obtained in the above Composition Examples 1 to 4 and Comparative Composition Examples 1 to 5 are shown in Table 2.
[0069] [Table 2]
[0070] [Composition Evaluation] The platinum-phosphite complex-containing hydrosilylation catalysts obtained in Examples 1 to 4 satisfy the requirements of the present invention, and it can be seen that the curable organopolysiloxane compositions in Examples 1 to 4 using these catalysts also have good storage stability at 23°C. In contrast, the platinum-phosphite complex-containing hydrosilylation catalysts of Comparative Examples 1 to 4 failed the judgment of the pass / fail of the catalyst itself because crystals were precipitated at 23°C, and furthermore, they failed in the workability because it was necessary to add the required amount while removing the crystalline components when adding the catalyst. However, the curable organopolysiloxane compositions using these catalysts show good storage stability. Therefore, if the catalyst is liquid at 23°C, the workability when adding the catalyst is also improved. In addition, the platinum-phosphite complex-containing hydrosilylation catalyst of Comparative Example 4 does not use a hydrocarbon solvent to obtain the desired platinum-phosphite complex-containing hydrosilylation catalyst. Therefore, the complex formation between the phosphite compound and platinum was poor, and the curable silicone composition prepared using it had a reduced storage stability. Comparative Example 5 is an example of a curable organopolysiloxane composition that does not form a complex between platinum and a phosphite ester or associate with a siloxane compound, and does not contain an organic solvent, and is selected from the group consisting of complexes of chloroplatinic acid or chloroplatinic acid salts and vinyl group-containing siloxanes. The curable organopolysiloxane composition prepared using this catalyst had a reduced storage stability. From the above results, it can be seen that the curable organopolysiloxane composition using the platinum-phosphite complex-containing hydrosilylation catalyst obtained in the present invention exhibits very excellent performance in terms of improved workability and storage stability.
[0071] The present specification includes the following aspects. [1]: (A) Platinum and the following general formula (1) [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. and a platinum-phosphite complex composed of a phosphite compound represented by the formula: (B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof: A platinum-phosphite complex-containing hydrosilylation catalyst comprising: [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) The hydrosilylation catalyst is an association of the component (A) and the component (B), does not contain an organic solvent, and is liquid at 23°C. [2]: The component (B) is R 2 The platinum-phosphite complex-containing hydrosilylation catalyst according to [1], wherein the alkoxysilane derivative is a vinyl group. [3]: A curable organopolysiloxane composition, characterized by containing the platinum-phosphite complex-containing hydrosilylation catalyst according to [1] or [2]. [4]: The curable organopolysiloxane composition according to [3], which is characterized in that it does not contain an organic solvent. [5]: An article comprising a cured product of the curable organopolysiloxane composition according to [3] or [4]. [6]: A method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, comprising the following steps (a) to (d): (a) preparing a solution of a phosphite compound represented by the following general formula (1) in a hydrocarbon solvent having a boiling point of 80° C. or less; [ka] (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. (b) adding to the solution a platinum compound not containing an organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid or a complex of a chloroplatinate with a vinyl group-containing siloxane, and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof to the solution obtained in the above steps (a) and (b) and dispersing the silane compound and / or a partial hydrolysate thereof to prepare a solution containing an association product of at least a part of the platinum-phosphite ester complex and the silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof; [ka] (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) (d) removing the hydrocarbon solvent from the solution obtained in (c). [7]: A method for producing a platinum-phosphite complex-containing hydrosilylation catalyst according to [6], characterized in that in step (c), the silane compound and / or partial hydrolysate thereof is added such that the number of moles of alkenyl groups in the silane compound and / or partial hydrolysate thereof is within a range of 0.01 to 500 times that of one platinum atom in the platinum compound.
[0072] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Industrial Applicability]
[0073] The platinum-phosphite complex-containing hydrosilylation catalyst of the present invention can maintain liquid properties at 23°C without using organic solvents, even in the case of platinum-phosphite complex-containing hydrosilylation catalysts that would previously have generated crystals. Therefore, the stability of the properties of the hydrosilylation catalyst itself can be improved, the workability can be improved when producing a curable organopolysiloxane composition using this catalyst, and a curable organopolysiloxane composition that is highly safe and does not contain a hydrocarbon organic solvent can be obtained. Therefore, the platinum-phosphite complex-containing hydrosilylation catalyst has very little adverse effect on the human body. In addition, the obtained curable organopolysiloxane composition that does not contain a hydrocarbon organic solvent can become an organopolysiloxane composition that has stable properties and physical properties even when exposed to temperatures above room temperature for a long period of time, and is therefore expected to be used in a wide range of fields, such as electrical equipment, automobiles, construction, medicine, and food.
Claims
1. (A) Platinum and the following general formula (1) 【Chemical 1】 (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. and a platinum-phosphite ester complex composed of a phosphite ester compound represented by the formula: (B) a silane compound represented by the following general formula (2) and / or a partial hydrolyzate thereof: A platinum-phosphite complex-containing hydrosilylation catalyst comprising: 【Chemistry 2】 (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) The hydrosilylation catalyst is an association of the component (A) and the component (B), does not contain an organic solvent, and is liquid at 23°C.
2. The component (B) is 2 2. The platinum-phosphite complex-containing hydrosilylation catalyst according to claim 1, wherein the alkoxysilane derivative is a vinyl group.
3. A curable organopolysiloxane composition comprising the platinum-phosphite complex-containing hydrosilylation catalyst according to claim 1 or 2.
4. 4. The curable organopolysiloxane composition according to claim 3, which does not contain an organic solvent.
5. An article comprising a cured product of the curable organopolysiloxane composition of claim 3.
6. A method for producing a platinum-phosphite complex-containing hydrosilylation catalyst, comprising the following steps (a) to (d): (a) preparing a solution of a phosphite ester compound represented by the following general formula (1) in a hydrocarbon solvent having a boiling point of 80°C or less; 【Chemistry 3】 (In the formula, R 1 is a hydrogen atom or a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. (b) adding to the solution a platinum compound containing no organic solvent, selected from the group consisting of platinum chloride, chloroplatinic acid, or a complex of a chloroplatinate with a vinyl group-containing siloxane, and dispersing the compound to prepare a solution containing a platinum-phosphite complex; (c) adding a silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof to the solution obtained in the above steps (a) and (b) and dispersing the silane compound and / or a partial hydrolysate thereof to prepare a solution containing an association product of at least a portion of the platinum-phosphite ester complex and the silane compound represented by the following general formula (2) and / or a partial hydrolysate thereof; 【Chemistry 4】 (In the formula, R 2 represents an alkenyl group having 2 to 10 carbon atoms, and R 3 is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms. X is a monovalent aliphatic hydrocarbon group having 1 to 3 carbon atoms or OR 3 It is.) (d) A step of removing the hydrocarbon solvent from the solution obtained in the step (c).
7. 7. The method for producing a platinum-phosphite complex-containing hydrosilylation catalyst according to claim 6, wherein in step (c), the silane compound and / or the partial hydrolyzate thereof is added so that the number of moles of alkenyl groups in the silane compound and / or the partial hydrolyzate thereof is within a range of 0.01 to 500 times that of one platinum atom in the platinum compound.
Citation Information
Patent Citations
High-temperature-resistance, anti-aging and high-transparent organic silica gel
CN108587454A
Organosilicon composition for ultraviolet LED packaging and preparation method thereof
CN109749701A
Platinum-phosphite ester complex-containing hydrosilylation catalyst, method for preparing same, method for inhibiting crystallization of platinum-phosphite ester complex-containing hydrosilylation catalyst, and curable organopolysiloxane composition and article
WO2023013443A1
Curable silicone gel composition and silicone gel cured product
JP2021042323A
One-pack type curable silicone gel composition and cured silicone gel
WO2021014970A1
Cited By