Plating method to penetration hole and circuit board

The method addresses void formation in high aspect ratio through-holes by using electrolytic plating with a progressive current density increase and stirring, ensuring efficient and void-free filling of through-holes in circuit boards.

JP2024155302AActive Publication Date: 2024-10-31KANTO GAKUIN SCHOOL CORP

Patent Information

Application Number
JP2023069921
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
2043-04-21

AI Technical Summary

Technical Problem

Existing methods for filling high aspect ratio through-holes in circuit boards with conductive metal result in voids, leading to prolonged processing times and potential defects due to air expansion during heat processes.

Method used

A method involving electrolytic plating with a conductive metal layer A as a current-carrying layer, using a low current density initially and progressively increasing it while stirring the electrolytic solution with a strong jet stream to fill high aspect ratio through-holes without voids.

Benefits of technology

Enables the filling of high aspect ratio through-holes with conductive metal in a short time without voids, enhancing the reliability of circuit boards by preventing defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155302000001_ABST
    Figure 2024155302000001_ABST
Patent Text Reader

Abstract

To provide a plating method to a penetration hole, capable of filling a conductive metal to the penetration hole in a high aspect ratio of an insulation base material, and embedding a cavity part of the penetration hole without generating a void in a short time.SOLUTION: A plating method to a penetration hole, includes: step 1 of forming a conductive metal layer A covering at least circumference of the penetration hole and the penetration hole in a front surface of one surface A of an insulation base material; and step 2 of depositing a conductive metal layer B in a direction of a surface B of the insulation base material that is different from the surface A using the conductive metal layer A as a conductive layer by using an electrolytic plating method to embed the penetration hole. In the electrolytic plating method in step 2, an electrolytic plating liquid used for the electrolytic plating method starts a current density from a low current density while scattering with a strong jet flow so as to be circulated in the penetration hole, and uses a method for increasing the current density step by step in accordance with a deposition of the conductive metal layer B.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to a through-hole plating method for filling a through-hole in an insulating substrate with a metal to fill the hollow portion of the through-hole, and to a circuit board using an insulating substrate in which the hollow portion of the through-hole has been filled with a metal by the through-hole plating method. [Background technology]

[0002] In recent years, multi-layer boards that are stacked are used in electronic circuit boards to improve packaging density. In order to electrically connect the stacked insulating boards, a technique has been used in which through holes that penetrate the board from top to bottom are provided in each board, and a conductive metal such as copper is formed on the surface of the through hole using a technique such as conformal plating. Since this conformal plating is a technique for forming a conductive metal on the surface of the through hole, a gap is left in the through hole. If a gap is left in the through hole, during a thermal process such as solder reflow for connecting electronic components to the circuit board, the air in the gap of the through hole remaining after conformal plating expands, causing defects that lead to a decrease in product quality, such as cracks in the plating film and destruction of the circuit board. Therefore, a technique has been adopted in which a resin or the like is filled in the gap of the through hole after conformal plating to fill and eliminate the gap of the through hole.

[0003] However, in order to further improve the packaging density of electronic circuit boards, electronic components are becoming smaller and the wiring width and spacing of electronic circuit boards are becoming finer, and through holes are also becoming higher in aspect ratio, that is, the diameter of the through hole relative to the length of the through hole is becoming smaller, and it is becoming difficult to fill a through hole with resin with a high aspect ratio without leaving any voids.

[0004] Therefore, Patent Documents 1 and 2 disclose a method of forming a through via by depositing and stacking a conductive metal using an electrolytic plating method in which an electrode provided on one side of the through hole is used as a power supply layer to fill the through hole. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2017-126865 [Patent Document 2] JP 2006-210369 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, when depositing a conductive metal in a through hole with a high aspect ratio using the general electrolytic plating methods disclosed in Patent Documents 1 and 2, in order to deposit the conductive metal while suppressing the occurrence of voids (gaps that remain because the deposited conductive metal is not filled), it is necessary to perform electrolytic plating at a low current for a long period of time, which poses the problem of lengthening the process time.

[0007] The present invention has been made in view of the above circumstances, and aims to provide a method for plating through holes that can fill a through hole having a high aspect ratio in an insulating substrate with a conductive metal and fill the hollow portion of the through hole without generating voids in a short time. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, the present inventors have conducted extensive research and have come up with the following method for plating through holes.

[0009] The plating method for through holes according to the present invention is a method for plating through holes provided in an insulating base material, which fills a hollow portion of the through hole with a metal, and the aspect ratio of the through hole is such that when the diameter of the through hole is 1, the thickness of the insulating base material is 10 or more. The plating method for through holes includes a step 1 of forming a conductive metal layer A on the surface of one side A of the insulating base material to cover at least the periphery of the through hole and the through hole, and a step 2 of depositing a conductive metal layer B in the direction of a side B of the insulating base material different from the side A using an electroplating method, with the conductive metal layer A as a current-carrying layer, to fill the through hole. The electroplating method in the step 2 employs a method in which a current density is started from a low current density while stirring an electrolytic plating solution used in the electrolytic plating method with a strong jet so as to circulate the electrolytic plating solution in the through hole, and the current density is increased stepwise as the deposition of the conductive metal layer B progresses.

[0010] The circuit board according to the present invention is characterized in that it uses an insulating base material in which the hollow portion of the through hole is filled with metal by the above-mentioned through hole plating method. Effect of the Invention

[0011] By adopting the through-hole plating method of the present invention, it is possible to fill a high aspect ratio through hole in an insulating substrate with a conductive metal, filling the hollow portion of the through hole without generating voids, in a short period of time. [Brief description of the drawings]

[0012] [Figure 1] 3A to 3C are schematic diagrams illustrating enlarged cross-sectional states of a through-hole portion provided in an insulating substrate at each process step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiment of the through-hole plating method and the circuit board according to the present invention will be described. Note that the following description merely shows one embodiment, and the following description should not be construed as being limited to the following description.

[0014] 1. Embodiments of the method for plating through holes The through-hole plating method according to the present invention is a through-hole plating method for filling a through-hole provided in an insulating base material with a metal to fill a hollow portion of the through-hole. In this case, the aspect ratio of the through-hole is such that the thickness of the insulating base material is 10 or more when the diameter of the through-hole is 1. The through-hole plating method includes a step 1 of forming a conductive metal layer A that covers at least the periphery of the through-hole and the through-hole on the surface of one side A of the insulating base material, and a step 2 of depositing a conductive metal layer B in the direction of a side B of the insulating base material different from the side A using an electrolytic plating method, with the conductive metal layer A as a current-carrying layer, to fill the through-hole.

[0015] The electrolytic plating method in step 2 uses a method in which the current density is started from a low current density while stirring the electrolytic plating solution used in the electrolytic plating method with a strong jet so that it circulates in the through hole, and the current density is increased stepwise as the deposition of the conductive metal layer B progresses. In this way, by starting the current density of the electrolytic plating method from a low current density, the conductive metal layer B is deposited without generating voids in the deep part of the through hole with a high aspect ratio. Then, by increasing the current density stepwise as the deposition of the conductive metal layer B progresses and the through hole gradually becomes shallower, the deposition of the conductive metal layer B can be accelerated and plating of the through hole can be completed in a short time. The stepwise increase in the current density is performed as the deposition of the conductive metal layer B progresses and the through hole gradually becomes shallower. That is, at the timing of the stepwise increase in the current density, the aspect ratio in the part where the deposition of the conductive metal layer B is performed is smaller than the point at which the electrolytic plating method was started. Therefore, even if the deposition of the conductive metal layer B is accelerated by increasing the current density, the generation of voids can be suppressed.

[0016] In this way, the through-hole plating method according to the present invention can fill a high aspect ratio through-hole in an insulating substrate with a conductive metal and fill the hollow portion of the through-hole without generating voids in a short time. This through-hole plating method will be described in detail below.

[0017] Fig. 1 shows enlarged schematic diagrams of the cross-sectional state of the through-hole portion provided in the insulating substrate at each step in the plating method for through-holes according to the present invention. Fig. 1 shows enlarged schematic diagrams of the cross-sectional state of the through-hole portion as the steps progress from No. 1 to No. 4. Note that Fig. 1 does not preclude states other than those shown in No. 1 to No. 4 from being included between No. 1 to No. 4.

[0018] The state of No. 1 in FIG. 1 shows a state in which a through hole 11 is provided in an insulating substrate 10. The lower side of the cross section of No. 1 is the surface A12, and the upper side of the cross section of No. 1 is the surface B13. The material of the insulating substrate 10 can be any material having insulating properties, such as a resin substrate such as glass epoxy or phenol resin, or a substrate such as glass or ceramic. In addition, a substrate in which the surface of a conductive substrate such as aluminum and the surface of a through hole provided in the conductive substrate are electrically insulated by a method such as anodizing can be used as the insulating substrate 10. The method of forming the through hole 11 can be any method that can form the through hole 11, such as a laser method, a drilling method, or an etching method. The through hole 11 in FIG. 1 is cylindrical, but the shape of the through hole in the plating method for a through hole according to the present invention is not limited to a cylindrical shape, and may be, for example, a square prism or a polygonal prism. Each shape may have a tapered shape.

[0019] The aspect ratio of the through hole is intended to be 1 when the diameter of the through hole is 1 and the thickness of the insulating substrate is 10 or more, but the plating method for through holes according to the present invention can be suitably used particularly when the diameter of the through hole is 10 μm or less. The upper limit of the thickness of the insulating substrate is not particularly limited when the diameter of the through hole is 1, but the thickness of the insulating substrate can be 250 when the diameter of the through hole is 1 and the aspect ratio of the through hole is high.

[0020] [Process 1] Next, step 1 will be described. Step 1 is a step of forming a conductive metal layer A that covers at least the periphery of and the through hole on the surface of one side A of the insulating base material. No. 2 in Fig. 1 shows a state in which a conductive metal layer A20 that covers at least the periphery of and the through hole 11 on the surface of side A12 of the insulating base material 10 has been formed in step 1.

[0021] Any method can be used for step 1 as long as it is a method capable of forming a conductive metal layer A20 that covers at least the periphery of the through hole 11 and the through hole 11 on the surface of face A12 of the insulating substrate 10. For example, as a first embodiment of step 1, step 1 includes a method of forming a conductive metal layer A20 composed of the conductive metal layer Aa and the conductive metal layer Ab, the conductive metal layer Aa including a step 1a of forming a conductive metal layer Aa at least around the through hole 11 on the surface of face A12 and a step 1b of forming a conductive metal layer Ab that covers the surface of the conductive metal layer Aa and the hole (i.e., the through hole 11 portion) of the conductive metal layer Aa.

[0022] The above-mentioned step 1a can be carried out, for example, as follows. A metal complex containing TiO2 and copper is coated on the surface A12, heated at 200-300°C, and then the coating surface is reduced using a reducing agent or the like. Then, a palladium catalyst is applied to the coating surface, and electroless nickel plating is performed to form the conductive metal layer Aa. Alternatively, after activating the coating surface, electroless copper plating is performed to form the conductive metal layer Aa. Next, as step 1b, for example, a conductive metal layer Ab that covers the surface of the conductive metal layer Aa and the holes of the conductive metal layer Aa can be formed by thickening electrolytic copper plating. In this way, a conductive metal layer A20 consisting of the conductive metal layer Aa and the conductive metal layer Ab can be formed.

[0023] In addition, as a second embodiment of step 1, the conductive metal layer A20 can be formed by laminating a metal foil film on the surface A12. For example, the conductive metal layer A20 can be formed by thermocompression bonding a copper foil having a thickness of 5 to 30 μm onto the surface A12.

[0024] In addition, as a third embodiment of step 1, the conductive metal layer A20 can be formed on the surface A12 by sputtering. For example, the surface A12 is activated in a vacuum by an ion bombardment method, and then titanium or copper is sputtered onto the surface of the surface A12 to form the conductive metal layer A20. Here, the ion bombardment method is a method in which a container containing the insulating base material 10 is degassed to 0.1 Pa or less, and then the container is filled with argon gas to 20-30 Pa, and the argon gas is turned into plasma to clean and activate the surface of the insulating base material 10.

[0025] [Process 2] Next, step 2 will be described. Step 2 is a step of depositing a conductive metal layer B in the direction of a surface B of the insulating base material different from the surface A, using an electrolytic plating method, with the conductive metal layer A as a current-carrying layer, to fill the through-hole. The electrolytic plating method uses a method in which the current density is started from a low current density while stirring the electrolytic plating solution used in the electrolytic plating method with a strong jet so that it circulates in the through-hole, and the current density is increased stepwise as the deposition of the conductive metal layer B progresses. No. 3 in FIG. 1 shows a state in which a conductive metal layer B21 is deposited in the direction of a surface B13 of the insulating base material 10 different from the surface A12 in step 2 to fill the through-hole 11.

[0026] Step 2 can be performed as follows. First, the conductive metal layer A20 is activated. Then, the insulating base material 10 on which the conductive metal layer A20 is formed is immersed in an electrolytic plating solution, and while stirring the electrolytic plating solution with a strong jet so that it circulates in the through-holes 11 using the conductive metal layer A20 as a current-carrying layer, the current density is started from a low current density, and the current density is gradually increased as the deposition of the conductive metal layer B21 progresses.

[0027] In this way, by starting the current density of the electrolytic plating method from a low current density, the conductive metal layer B21 can be deposited without generating voids in the deep part of the through hole 11 having a high aspect ratio, such as a thickness of the insulating substrate 10 of 10 or more when the diameter of the through hole 11 is taken as 1. Then, by increasing the current density stepwise as the deposition of the conductive metal layer B21 progresses and the through hole 11 gradually becomes shallower, the deposition of the conductive metal layer B21 can be accelerated and plating of the through hole 11 can be completed in a short time. That is, at the timing of the stepwise increase in the current density, the aspect ratio of the part where the deposition of the conductive metal layer B21 is performed is smaller than that at the time when the electrolytic plating method was started. Therefore, even if the deposition of the conductive metal layer B21 is accelerated by increasing the current density, the generation of voids can be suppressed.

[0028] The current density in the electrolytic plating method can be increased continuously from a low current density to a high current density. However, it is preferable to increase the current density stepwise according to the deposition amount of the conductive metal layer B21, since this is relatively easy to control. In this case, the number of steps for increasing the current density stepwise is preferably two steps, more preferably three steps, although there is no upper limit to the number of steps.

[0029] In the first stage of the two-stage method, the conductive metal layer B21 is deposited in the deep part of the through hole 11 with a high aspect ratio, so that circulation of the electrolytic plating solution is difficult and voids are likely to occur. Therefore, a low current density is used to suppress the deposition rate of the conductive metal layer B21 so as to prevent voids from occurring. The deposition amount in the first stage is not particularly limited, but can be up to about 1 / 10 of the length of the through hole 11. In the second stage of the two-stage method, the conductive metal layer B21 is deposited until the through hole 11 is completely filled with a current density increased to 5-50 times the current density in the first stage, but is not particularly limited. Thus, in the second stage, the aspect ratio in the part where the conductive metal layer B21 is deposited is small, so that even if the current density is increased, voids are not generated and the conductive metal layer B21 can be deposited at a high speed.

[0030] In the first stage of the three-stage method, the conductive metal layer B21 is deposited in the deep part of the through hole 11 having a high aspect ratio, so that circulation of the electrolytic plating solution is difficult and voids are likely to occur. Therefore, a low current density is used to suppress the deposition rate of the conductive metal layer B21 so as to prevent the generation of voids. The deposition amount in the first stage is not particularly limited, but can be up to about 1 / 10 of the length of the through hole 11. In the second stage of the three-stage method, the current density is increased to about 50 times the current density in the first stage, and the deposition amount of the conductive metal layer B21 can be up to about 5 / 10-6 / 10 of the length of the through hole 11. In the third stage of the three-stage method, the current density is increased to about 80-150 times the current density in the first stage, and the conductive metal layer B21 is deposited until the through hole 11 is completely filled. In this way, in the second and third steps, the aspect ratio of the portion where the conductive metal layer B21 is deposited is small, so that even if the current density is increased, no voids are generated, and the deposition of the conductive metal layer B21 can be performed at high speed. And, since the current density in the third step of the three-step method can be made higher than that in the second step of the two-step method, the three-step method can complete plating of the through hole 11 in a shorter time than the two-step method.

[0031] The amount of stepwise increase in the current density, the number of times the current density is increased, and the timing of the increase are not limited, and the number of steps in which the current density is increased stepwise can be four or more. Depending on the shape and aspect ratio of the through hole 11 and the progress of deposition of the conductive metal layer B21, a suitable method that can suppress the generation of voids and speed up deposition can be used as appropriate, and the above is merely one example.

[0032] In addition, as a method of stirring the electrolytic plating solution with a strong jet so that the electrolytic plating solution circulates in the through-holes, any method can be used as long as the electrolytic plating solution can be circulated in the through-holes. For example, a method can be used in which the electrolytic plating solution is spurted from a nozzle having a drain structure near the blowing part toward the deposition surface of the conductive metal layer B21 in the through-holes 11 while the insulating base material 10 is oscillated by moving it vertically and horizontally at a constant speed in an electrolytic plating solution bath, so that the electrolytic plating solution circulates in the through-holes 11, thereby making the electrolytic plating solution into a high-speed jet-like jet at a flow rate of 4 L / min and stirring the electrolytic plating solution.

[0033] [Electrolytic plating solution] Next, the electrolytic plating solution used in the electrolytic plating in step 2 will be described. The electrolytic plating solution used in the electrolytic plating in step 2 is not particularly limited as long as it can be used in the plating method for through holes according to the present invention. For example, when copper is used as the constituent metal of the conductive metal layer B21, an electrolytic copper plating solution having the composition shown below can be used. In this case, for example, a phosphorus-containing copper anode is used, and electrolytic plating can be performed at a bath temperature of 25±5°C, although this is not particularly limited. Here, if the bath temperature is high, decomposition of the electrolytic copper plating solution is promoted and the bath stability is reduced. Although a higher bath temperature promotes copper precipitation, it is necessary to add more additives to ensure bath stability, which increases the cost of step 2. Therefore, it is sufficient to select an appropriate bath temperature.

[0034] Copper sulfate pentahydrate: 200-300g / L. Sulfuric acid: 50-100g / L. Cl - :50ppm. Additives.

[0035] Here, it is preferable to add at least one additive selected from polyethylene glycol (PEG) having a degree of polymerization of 2000-20000, disodium dithiobis(1-propanesulfonate) (SPS), and Janus Green B (JGB) to the electrolytic copper plating solution in advance. A nonionic surfactant such as PEG is added to eliminate variation in the amount of deposition of the conductive metal layer B21 at the position of the through-hole 11 in the insulating substrate 10, and the amount added can be selected according to the size of the insulating substrate 10. When PEG is used in the electrolytic copper plating solution, it is preferable to add PEG at a content of 10 ppm or less. Sulfur-based organic compounds such as SPS are generally used when the current density in the electrolytic plating method is, for example, 200 A / dm 2 It is added in the case of high currents such as 200 A / dm or more to provide effects such as smoothing the surface of the plating film. However, in this electrolytic copper plating solution, 2 It is preferable to use SPS even at a low current density of 100 ppm or less, and it is preferable to add SPS at a content of 50 ppm or more. This is because the quality of the copper of the conductive metal layer B21 is good, and it is smoothed and shiny. The upper limit of the SPS content is not particularly limited, but it is preferable to add SPS at 100 ppm or less. Dyes such as JGB are intended to provide effects such as smoothing the surface of the plating film, but excessive addition makes the plating film brittle, so it is sufficient to select an appropriate amount to add, but when JGB is used in the electrolytic copper plating solution, it is preferable to add SPS at a content of 30 ppm or less.

[0036] [Electrolytic copper plating method] An example of the electrolytic plating method of step 2 will be described using the electrolytic copper plating solution described above, for example, when the diameter of the through hole 11 is 10 μm and the thickness of the insulating substrate 10 is 100 μm, that is, when the diameter of the through hole is 1, the thickness of the insulating substrate is 10 or more. At this time, for example, phosphorus-containing copper can be used for the anode. At this time, for example, an insulating resin is applied to the opposite side of the conductive metal layer A20 from the side in contact with the surface A12 so that deposition does not proceed in the opposite direction to the side in contact with the surface A12 of the conductive metal layer A20. Next, the surface B13 side of the conductive metal layer A20 is activated using dilute sulfuric acid. Then, the conductive metal layer A20 is used as a current-carrying layer, and the current density of the electrolytic plating is, for example, 1 A / dm 2 Then, the conductive metal layer B21 (copper in this case) is deposited, for example, at 10 μm. Then, the current density is increased to, for example, 50 A / dm 2 The current density is then increased to, for example, 100 A / dm2, and the conductive metal layer B21 (copper in this case) is further deposited, for example, to 45 μm. 2 The conductive metal layer B21 (copper in this case) is further deposited to a thickness of, for example, 45 μm inside the through hole 11. In this way, the conductive metal layer B21 can be formed to a thickness of 100 μm in the thickness direction of the insulating base material inside the through hole 11.

[0037] The electrolytic plating method in step 2 described above is merely an example, and the current density at the start of electrolytic plating, the amount and timing of the stepwise increase in current density, and additives can be appropriately selected according to the aspect ratio and shape of the through hole, etc. In this way, by employing the through hole plating method according to the present invention, it is possible to fill a high aspect ratio through hole in an insulating substrate with a conductive metal and fill the hollow portion of the through hole without generating voids in a short time.

[0038] [Degassing process] It is preferable to have a degassing step between the above-mentioned steps 1 and 2, in which the air in the through holes 11 is degassed. After step 1, the insulating base material 10 is in a state in which the conductive metal layer A20 is formed to cover at least the periphery of the through holes 11 and the through holes 11 on the surface of the face A12 of the insulating base material 10. That is, the face A12 side of the through holes 11 is blocked, and the air in the through holes 11 does not easily escape. Therefore, by carrying out the degassing step to degas the air in the through holes 11, the electrolytic plating solution used in the electrolytic plating can be circulated in the through holes 11.

[0039] The degassing method may be any method capable of degassing the air in the through-holes 11. For example, there may be mentioned a method in which the insulating substrate 10 after the process 1 is immersed in water and ultrasonic vibration is applied to the insulating substrate 10 or the water to degas the air in the through-holes 11. There may also be mentioned a method in which the insulating substrate 10 after the process 1 is immersed in water and the temperature of the water is raised or lowered to expand the air in the through-holes 11 to degas the air in the through-holes 11. There may also be mentioned a method in which the insulating substrate 10 after the process 1 is immersed in water and a container containing the water is evacuated to degas the air in the through-holes 11.

[0040] [Etching process] After the above-mentioned step 2, it is preferable to have an etching step for removing unnecessary parts of the conductive metal layer B21 deposited in the direction of the surface B13 of the insulating base material 10. No. 3 in FIG. 1 shows a state in which the conductive metal layer B21 is deposited in the direction of the surface B13 of the insulating base material 10 different from the surface A12 in step 2 to fill the through-hole 11, but the conductive metal layer B21 is in a state of swelling on the upper part of the surface B13. This is because if such a swelling part of the conductive metal layer B21 is unnecessary, it can be removed in the etching step. No. 4 in FIG. 1 shows a state in which the swelling part of the conductive metal layer B21 on the upper part of the surface B13 is removed in the etching step.

[0041] Any etching method can be used as long as it can remove the unnecessary portion of the conductive metal layer B21. For example, when the electrolytic copper plating described above is performed in step 2, since the conductive metal layer B21 is copper, the unnecessary portion of the conductive metal layer B21 can be removed using an etching solution having the following composition. In this case, the bath temperature is set to 20-30° C., and etching can be performed while rotating the insulating substrate 10 to be etched at 200-1200 rpm.

[0042] Sulfuric acid: 5g / L. H2O2: 50-150g / L. Polyethylene glycol (stabilizer): 5-15g / L.

[0043] 2. Circuit Board Embodiments The circuit board according to the present invention employs a circuit board using an insulating substrate in which the hollow portion of a through hole is filled with a metal by the above-mentioned through hole plating method. The circuit board may be one in which a circuit pattern made of a conductive metal layer is formed on the surface of the insulating substrate before, during, or after the above-mentioned through hole plating method. By employing the above-mentioned through hole plating method, the circuit board according to the present invention can employ through holes with a high aspect ratio, and it is possible to fill the hollow portion of the through hole without generating voids in a short time by filling the high aspect ratio through hole with a conductive metal.

[0044] The circuit board according to the present invention may use a single insulating base material 10 as shown in FIG. 1, or may be a multi-layer circuit board in which multiple insulating base materials 10 produced using the through-hole plating method according to the present invention are laminated and bonded together.

[0045] The embodiment of the present invention described above is one aspect of the present invention, and can be modified as appropriate without departing from the spirit of the present invention. The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. EXAMPLES

[0046] In Example 1, a glass insulating substrate 10 having a thickness of 100 μm and provided with through holes 11 having a diameter of 10 μm was used. After degreasing the glass insulating substrate 10, in the above-mentioned step 1a, a metal complex containing TiO2 and copper was coated on the surface A12, and after heating at 200-300° C., the coating surface was reduced using a reducing agent. Thereafter, a palladium catalyst was applied to the coating surface, and electroless nickel plating was performed to form a conductive metal layer Aa. Next, in the above-described step 1b, the electrolytic copper plating solution shown below was used, phosphorus-containing copper was used as the anode, and electrolytic current density: 150 A / dm 2 By performing thick electrolytic copper plating at 1000 K, a conductive metal layer Ab was formed with a thickness of about 10 μm, covering the surface of the conductive metal layer Aa and the holes of the conductive metal layer Aa. In this way, a conductive metal layer A20 consisting of the conductive metal layer Aa and the conductive metal layer Ab was formed.

[0047] Copper sulfate pentahydrate: 250g / L. Sulfuric acid: 50g / L. PEG: 0 ppm. SPS: 50 ppm. JGB: 30 ppm. Cl - :50ppm. Bath temperature: 25±5℃. Stirring method: High speed jet stirring.

[0048] Next, in step 2, electrolytic copper plating was performed using the electrolytic copper plating solution shown below and phosphorus-containing copper as the anode. At this time, the current density was increased stepwise in two steps, with the first step being a current density of 1 A / dm 2 The deposition amount in the first stage was set to 10 μm. Next, the current density in the second stage was set to 5 A / dm 2 The deposition amount in the second stage was set to 90 μm.

[0049] Copper sulfate pentahydrate: 250g / L. Sulfuric acid: 50g / L. PEG: 0 ppm. SPS: 50 ppm. JGB: 30 ppm. Cl - :50ppm. Bath temperature: 25±5℃. Mixing method: rocking and high speed jet mixing (flow rate 4L / min). EXAMPLES

[0050] In Example 2, the same insulating base material 10 as in Example 1 was used, and the same step 1 as in Example 1 was carried out.

[0051] Next, in step 2, electrolytic copper plating was performed using the same electrolytic copper plating solution as in Example 1, and phosphorus-containing copper was used as the anode. At this time, a two-step method was used to increase the current density stepwise, with the first step being a current density of 1 A / dm 2 The deposition amount in the first stage was 10 μm. Next, the current density in the second stage was 50 A / dm 2 The deposition amount in the second stage was set to 90 μm. EXAMPLES

[0052] In Example 3, the same insulating substrate 10 as in Example 1 was used, and the same step 1 as in Example 1 was carried out.

[0053] Next, in step 2, electrolytic copper plating was performed using the same electrolytic copper plating solution as in Example 1, and phosphorus-containing copper was used as the anode. At this time, the current density was increased stepwise in three steps, with the first step being a current density of 1 A / dm 2 The deposition amount in the first stage was 10 μm. Next, the current density in the second stage was 50 A / dm 2 The deposition amount in the second step was set to 45 μm. Next, the current density in the third step was set to 80 A / dm 2 The deposition amount in the third stage was set to 45 μm. EXAMPLES

[0054] In Example 4, the same insulating substrate 10 as in Example 1 was used, and the same step 1 as in Example 1 was carried out.

[0055] Next, in step 2, electrolytic copper plating was performed using the same electrolytic copper plating solution as in Example 1, and phosphorus-containing copper was used as the anode. At this time, the current density was increased stepwise in three steps, with the first step being a current density of 1 A / dm 2 The deposition amount in the first stage was 10 μm. Next, the current density in the second stage was 50 A / dm 2 The deposition amount in the second step was set to 45 μm. Next, the current density in the third step was set to 150 A / dm 2 The amount of precipitation in the third stage was 45 μm.

[0056] Comparative Example 1 In Comparative Example 1, the same insulating substrate 10 as in Example 1 was used, and the same step 1 as in Example 1 was carried out.

[0057] Next, in Comparative Example 1, electrolytic copper plating was performed using a general conformal electrolytic copper plating method with the following electrolytic copper plating solution, using phosphorus-containing copper as the anode. At this time, the current density was 1 A / dm 2 A constant value of was used.

[0058] Copper sulfate pentahydrate: 65g / L. Sulfuric acid: 200g / L. PEG: 1000 ppm. SPS: 6 ppm. JGB: 10 ppm. Cl - :50ppm. Bath temperature: 25±5℃. Mixing method: Air mixing using air bubbles

[0059] Comparative Example 2 In Comparative Example 2, the same insulating substrate 10 as in Example 1 was used, and the same step 1 as in Example 1 was carried out.

[0060] Next, in Comparative Example 2, electrolytic copper plating was performed using a general conformal electrolytic copper plating method with the same electrolytic copper plating solution as in Comparative Example 1, and phosphorus-containing copper was used as the anode. At this time, the current density was 80 A / dm 2 A constant value of was used.

[0061] 〔evaluation〕 X-ray photography was performed on the insulating base material 10 produced in Examples 1-5 and Comparative Examples 1-2. This confirmed that in Examples 1-4 and Comparative Example 1, copper was precipitated in the through hole 11 and there were no voids. In particular, in Example 5, it was confirmed that copper was precipitated in the through hole 11 without voids, despite the high aspect ratio of 1:250. On the other hand, in Comparative Example 2, it was confirmed that copper was not sufficiently precipitated in the through hole 11 and voids were present.

[0062] Table 1 shows the time required for electrolytic copper plating in step 2 in Examples 1-5 and Comparative Examples 1-2. "Aspect ratio" in Table 1 indicates the aspect ratio of the through hole 11 provided in the insulating base material 10 used in each Example and Comparative Example. "Completion time" in Table 1 indicates the time required for electrolytic copper plating in step 2 on the through hole 11. "Void" in Table 1 indicates the presence or absence of a void (air gap) in which copper is not precipitated in the through hole 11 after completion of electrolytic copper plating in step 2. "-" in Table 1 indicates that the current density is not changed and the current density before "-" is maintained until the electrolytic copper plating is completed. From Table 1, it is clear that the plating method for a through hole according to the present invention can deposit copper and fill the hollow part of the through hole 11 without the generation of voids in a short time compared to the conventional conformal electrolytic copper plating method shown in Comparative Example 1. Furthermore, Comparative Example 2 revealed that in the conventional conformal copper electroplating method, even if the current density is increased to shorten the time required for copper electroplating, voids still occur in the through holes.

[0063] [Table 1] [Industrial Applicability]

[0064] The through-hole plating method of the present invention can fill through holes having a high aspect ratio in an insulating substrate with a conductive metal, thereby filling the hollow portion of the through hole in a short time without generating voids, and can therefore be suitably used as a through-hole plating method for filling a through hole provided in an insulating substrate with a metal to fill the hollow portion of the through hole. [Explanation of symbols]

[0065] 10. Insulating substrate 11 Through hole 12 side A 13 Side B 20 Conductive metal layer A 21 Conductive metal layer B

Claims

1. 1. A plating method for a through hole provided in an insulating base material, the method comprising filling a metal into the through hole to fill a hollow portion of the through hole, the method comprising the steps of: the aspect ratio of the through hole is such that, when the diameter of the through hole is taken as 1, the thickness of the insulating base material is 10 or more; A step 1 of forming a conductive metal layer A on a surface of one side A of the insulating base material, the conductive metal layer A covering at least the periphery of the through hole and the through hole; and step 2 of depositing a conductive metal layer B in a direction of a surface B of the insulating base material different from the surface A by using an electrolytic plating method, with the conductive metal layer A as a current-carrying layer, to fill the through hole. The electrolytic plating method in step 2 is a method for plating a through hole, characterized in that the electrolytic plating solution used in the electrolytic plating method is stirred with a strong jet so as to circulate within the through hole, while the current density is started from a low current density, and the current density is gradually increased as the deposition of the conductive metal layer B progresses.

2. 2. The plating method for a through hole according to claim 1, wherein the electrolytic plating solution is an electrolytic copper plating solution containing copper sulfate pentahydrate and sulfuric acid, the electrolytic copper plating solution contains disodium dithiobis(1-propanesulfonate) as an additive, and the content of the disodium dithiobis(1-propanesulfonate) is 50 ppm or more.

3. The step 1 is a step 1a of forming a conductive metal layer Aa at least around the through hole on the surface of the face A; Step 1b of forming a conductive metal layer Ab covering a surface of the conductive metal layer Aa and holes of the conductive metal layer Aa; The method for plating a through hole according to claim 1 , wherein the conductive metal layer A is formed from the conductive metal layer Aa and the conductive metal layer Ab.

4. The step 1 is The method for plating a through hole according to claim 1 , wherein the conductive metal layer A is formed by laminating a metal foil film.

5. 2. The method for plating a through hole according to claim 1, further comprising a step of degassing air from within the through hole between the step 1 and the step 2.

6. 2. The method for plating a through hole according to claim 1, further comprising, after step 2, an etching step of removing unnecessary portions of said conductive metal layer B deposited in the direction of said surface B.

7. 2. A circuit board comprising an insulating substrate having a through hole filled with a metal by using the through hole plating method according to claim 1.

Citation Information

Patent Citations

  • Anisotropic conductive film and manufacturing method therefor

    JP2002076056A

  • Method for burying plating into through hole and plating device

    JP2006111896A

  • Method of manufacturing through-hole substrate filled with conductive material

    JP2006147971A

  • Plating method

    JP2006328476A

  • Electrolytic copper plating or copper alloy plating bath

    JP2020125539A

Cited By

  • Method for forming via-fill interlayer conductors and circuit board

    JP2026160410A

  • Method for forming via-fill interlayer conductor, and circuit board

    WO2026204233A1