Ingot

By adding C and controlling the cooling rate, the ingot's casting structure is refined, addressing segregation issues and minimizing defects, resulting in a more stable and defect-free titanium ingot.

JP2024155480APending Publication Date: 2024-10-31NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023070234
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing titanium ingots suffer from surface flaws and defects due to segregation of elements like Fe, Al, and Mo during hot working, which are caused by inadequate refinement of the casting structure.

Method used

The ingot is produced by adding an appropriate amount of C and controlling the cooling rate during production to refine the metal structure, reducing both macro-segregation and micro-segregation, thereby minimizing defects.

Benefits of technology

This method results in a titanium ingot with a refined casting structure, reducing surface flaws and defects during hot working, leading to improved manufacturability and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155480000017
    Figure 2024155480000017
  • Figure 2024155480000018
    Figure 2024155480000018
  • Figure 2024155480000019
    Figure 2024155480000019
Patent Text Reader

Abstract

To provide an ingot capable of reducing a segregation of Fe, Al, V, Mo, etc., in a cast structure and inhibiting a surface flaw that might occur in hot processing of an ingot.SOLUTION: An ingot includes, by mass%, 0.100 to 0.900% C, 0 to 7.000% Al, 0 to 7.000% Mo, 0 to 6.000% V, 0 to 5.000% Zr, 0 to 3.000% Sn, 0 to 2.100% Fe, 0 to 0.500% Si, 0 to 0.400% Cr, 0 to 0.400% Ni, 0 to 0.400% Ta, 0 to 0.400% Nb, 0 to 0.200% Mn, 0 to 0.100% Ru, 0 to 0.100% Pd, 0 to 0.200% Cu, 0 to 0.090% B, 0 to 0.090% Hf, 0.400% or less O, 0.300% or less N, 0.110% or less S, 0.110% or less P, 0.035% or less H, and a balance Ti with impurities. An average particle diameter of the cast structure is 90 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to ingots, and in particular to titanium-based ingots. [Background technology]

[0002] Titanium is a metal material that has excellent corrosion resistance, a smaller density than carbon steel, and excellent specific strength (strength per unit weight). Some of the present inventors have proposed a titanium material that contains C instead of rare elements such as Pd, thereby improving corrosion resistance while maintaining high workability (see, for example, Patent Document 1).

[0003] However, when hot working is applied to an ingot of titanium or titanium alloy, surface defects may occur. Usually, when molten titanium or titanium alloy is cast, an ingot is obtained in which Fe, Al, V, Mo, etc. are significantly segregated. The segregation of these elements in such an ingot is undesirable in terms of manufacturability and the stability of product properties, and may cause surface defects. Defects that occur during hot working may cause defects or cracks in subsequent processes such as cold working.

[0004] Patent Document 2 proposes an invention in which vibration is applied to the molten metal during casting to refine the metal structure in the center and surface layer of the ingot in order to prevent the occurrence of surface defects during hot working. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2019 / 198147 [Patent Document 2] JP 2020-121331 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an ingot that can suppress surface defects that may occur due to hot working of the ingot by reducing segregation (both macrosegregation and microsegregation) of elements such as Fe, Al, V, and Mo in the cast structure. [Means for solving the problem]

[0007] As a result of research conducted to solve this problem, it was discovered that by adding an appropriate amount of C to titanium material and keeping the cooling rate during ingot production within a specific range, it is possible to refine the metal structure of the ingot and reduce segregation, thereby suppressing defects during hot processing. The present invention employs the following configuration.

[0008] [1] In weight percent: C: 0.100~0.900%, Al: 0-7.000%, Mo: 0 to 7.000%, V: 0 to 6.000%, Zr: 0 to 5.000%, Sn: 0~3.000%, Fe: 0-2.100%, Si: 0 to 0.500%, Cr: 0~0.400%, Ni: 0 to 0.400%, Ta: 0 to 0.400%, Nb: 0 to 0.400%, Mn: 0 to 0.200%, Ru: 0~0.100%, Pd: 0-0.100%, Cu: 0 to 0.200%, B: 0~0.090%, Hf: 0~0.090%, O: 0.400% or less, N: 0.300% or less, S: 0.110% or less, P: 0.110% or less, H: 0.035% or less, The balance is composed of Ti and impurities. An ingot having an average grain size of 90 μm or less in its cast structure. [2] By weight C: 0.100~0.450%, Fe: 0.010~0.450%, H: 0.015% or less, O: 0.400% or less, N: 0.300% or less, S: 0.030% or less, P: 0.030% or less, Si: 0.500% or less, Mo: 0~1.900%, Al: 0-0.400%, Ta: 0 to 0.200%, Nb: 0 to 0.090%, Ru: 0~0.100%, Pd: 0-0.100%, Ni: 0 to 0.200%, One or more of Mn, Cu, Cr, Sn, and Zr: 0 to 0.200% in total, The balance is composed of Ti and impurities. An ingot having an average grain size of 90 μm or less in its cast structure. [3] The ingot according to [2], wherein the volume fraction of the titanium compound remaining in the ingot is 5 vol% or less. [4] The ingot according to [2] or [3], wherein the average particle size of the titanium compound remaining in the ingot is less than 1 μm. [5] The ingot according to any one of [2] to [4], which satisfies either one or both of the following formula (1) or the following formula (2): [C] max / [C] ave ≦1.4 … (1) [Fe] max / [Fe] ave ≦1.3 … (2) In equations (1) and (2), [C] max , [Fe] max are the maximum concentrations (mass%) of C and Fe in the ingot. ave , [Fe] aveare the average chemical compositions (% by mass) of C and Fe in the ingot, respectively. [6] By weight C: 0.310~0.900%, Al: 4.500%~6.500%, Fe: 0.500%~2.100%, N: 0.050% or less, O: 0.250% or less, Si: 0 to 0.500%, Mo: 0 to 7.000%, Cr: 0~0.400%, Cu: 0-0.090%, Ni: 0 to 0.400%, Hf: 0~0.090%, B: 0~0.090%, Nb: 0 to 0.400%, Ta: 0 to 0.400%, Sn: 0~1.900%, Zr: 0 to 0.400%, Ru: 0~0.100%, Pd: 0 to 0.100% S: 0.080% or less, P: 0.080% or less, H: 0.025% or less, The balance is composed of Ti and impurities. An ingot with an average grain size of 90 μm or less in the cast structure. [7] By weight C: 0.310~0.900%, Al: 2.000%~7.000%, V: 1.500~6.000%, Fe: 0.500% or less, N: 0.050% or less O: 0.250% or less Si: 0 to 0.500%, Mo: 0-7.00%, Cr: 0~0.400%, Cu: 0-0.090%, Ni: 0 to 0.400%, Hf: 0~0.090%, B: 0~0.090%, Nb: 0 to 0.400%, Ta: 0 to 0.400%, Sn: 0~1.900%, Zr: 0 to 0.400%, Ru: 0~0.100%, Pd: 0 to 0.100% S: 0.110% or less, P: 0.110% or less, H: 0.030% or less, The balance is composed of Ti and impurities. An ingot with an average grain size of 90 μm or less in the cast structure. [8] By weight C: 0.310~0.900%, Al: 5.000%~7.000%, Mo: 1.000%~7.000%, Zr: 3.000%~5.000%, Sn: 1.000%~3.000%, Si: 0% to 0.500%, Fe: 0.500% or less, N: 0.050% or less O: 0.250% or less Cr: 0~0.400%, Cu: 0-0.090%, Ni: 0 to 0.400%, Hf: 0~0.090%, B: 0~0.090%, Nb: 0 to 0.400%, Ta: 0 to 0.400%, Ru: 0~0.100%, Pd: 0 to 0.100% S: 0.110% or less, P: 0.110% or less, H: 0.035% or less, The balance is composed of Ti and impurities. An ingot with an average grain size of 90 μm or less in the cast structure. [9] The ingot according to any one of [6] to [8], wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol% or less.

[10] The ingot according to any one of [6] to [9], wherein the average particle size of the titanium compound remaining in the ingot is less than 1 μm.

[11] The ingot according to any one of [6], [8], [9] and

[10] , which satisfies any one or more of the following formulae (3) to (6): [C] max / [C] ave ≦1.4 … (3) [Fe] max / [Fe] ave ≦1.3 … (4) [Al] max / [Al] ave ≦1.3 … (5) [Mo] max / [Mo] ave ≦1.3 … (6) In the formulas (3) to (6), [C] max , [Fe] max , [Al] max , [Mo] max are the maximum concentrations (mass%) of C, Fe, Al, and Mo in the ingot. ave , [Fe] ave , [Al] ave , [Mo] ave are the average chemical compositions (mass%) of C, Fe, Al, and Mo in the ingot, respectively.

[12] The ingot according to any one of [7], [9] and

[10] , which satisfies any one or more of the following formulae (3) to (7): [C] max / [C] ave ≦1.4 … (3) [Fe] max / [Fe] ave ≦1.3 … (4) [Al] max / [Al] ave ≦1.3 … (5) [Mo] max / [Mo] ave ≦1.3 … (6) [V] max / [V] ave ≦1.3 … (7) In the formulas (3) to (7), [C] max , [Fe] max , [Al] max , [Mo] max , [V] max are the maximum concentrations (mass%) of C, Fe, Al, Mo, and V in the ingot. ave , [Fe] ave , [Al] ave , [Mo] ave , [V] ave are the average chemical compositions (mass%) of C, Fe, Al, Mo, and V in the ingot, respectively. Effect of the Invention

[0009] According to the present invention, it is possible to provide an ingot capable of suppressing surface defects that may occur due to hot working of the ingot by reducing the segregation (both macrosegregation and microsegregation) of elements such as Fe, Al, V, and Mo in the cast structure. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram of a facility for producing ingots. [Diagram 2] FIG. 2 is an enlarged schematic diagram of a casting area in a facility for producing ingots. [Diagram 3] FIG. 3 is a schematic diagram illustrating the dimensional relationship of an ingot. [Figure 4] FIG. 4 is a schematic diagram illustrating the relationship between the ingot and the sample collection positions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Titanium is manufactured through a much more complex process than steel, typically ranging from the smelting process to the cold working process.

[0012] Smelting process: The process in which titanium tetrachloride is obtained from titanium-containing ore, which is then reduced with magnesium to produce a sponge-like lump of titanium metal (hereafter referred to as titanium sponge). Casting process: A process in which titanium sponge is mixed with necessary auxiliary materials (such as TiO2 or metallic iron) and then pressed into a titanium briquette, which is then used as an electrode to melt in a vacuum arc melting furnace to produce an ingot; or a process in which titanium sponge or titanium briquette and auxiliary materials are melted in an electron beam melting furnace or plasma arc melting furnace to produce an ingot. Forging or blooming process: A process in which an ingot is hot forged or bloomed to produce slabs (hot rolled material) or billets (materials for hot extrusion, hot forging, etc.). Hot working process: A process in which slabs or billets are heated and then hot rolled, forged, or extruded to produce plates or round bars. Cold working process: The process in which the plate or round bar is further cold rolled, drawn, and drawn to produce thin plate, round bar, wire, etc.

[0013] FIG. 1 shows an example of a facility for carrying out a casting process. This facility is equipped with an electron beam melting furnace, and is equipped with a first electron beam generator, a feed port 4, a mold 5, a second electron beam generator 6, and a vacuum vessel 8 that houses these. The first electron beam generator 2 irradiates sponge titanium or titanium briquettes 1 with an electron beam 2A to melt them into molten titanium. Molten titanium 3 is supplied to the mold 5 from the feed port 4. The molten titanium 3 in the mold 5 is irradiated with an electron beam 6A by a second electron beam generator 6 installed above the mold 5, whereby it is heated. The molten titanium 3 is cooled by the mold 5 to form an ingot 7.

[0014] The mold 5 is capable of casting an ingot having a rectangular cross-sectional shape, or an ingot having a circular cross-sectional shape. Fig. 2 shows an enlarged view of the mold 5. H1 in Fig. 2 is the height of the mold 5, H2 in Fig. 2 is the length of the ingot cooling section, and W is the diameter or width of the ingot.

[0015] The present invention relates to an ingot obtained by the above casting process. The titanium-based ingot of the present invention will be described below. The ingot of the present invention includes both titanium ingots and titanium alloy ingots.

[0016] Conventionally, ingots having a fine cast structure with an average grain size of about 100 μm have been produced by a method of applying vibration between the start of casting and the end of solidification or by a rapid cooling method. However, improvements are required to reduce both macro- and micro-segregation of elements contained in the ingot and to further reduce hot working defects, and the conventional method or a concept that is an extension of the conventional method, which is a technical idea of ​​making improvements between the start of casting and the end of solidification, is insufficient. Therefore, in the present invention, by using a technique and technical idea that are completely different from the conventional method, the average grain size of the cast structure is set to 90 μm or less, and further reduction of alloy element segregation and hot working defects in the ingot is succeeded.

[0017] (Ideas for solving problems) The inventors have found that adding carbon (C) to the material and refining the cast structure are effective in reducing both macrosegregation and microsegregation of elements contained in the ingot and in reducing surface defects caused by hot working (hereinafter referred to as hot working defects). Controlling the cooling rate during casting is effective in refining the cast structure. The term "cast structure" refers to a structure obtained by cooling the solidified structure obtained by solidifying the molten metal to form a transformed structure.

[0018] In general, the formation of a cast structure is composed of the formation of a solidified structure and the formation of a transformed structure. The solidified structure is a structure that occurs when the molten metal is cooled and passes through a solid-liquid coexistence state, and is entirely solidified, and is formed in a temperature range of at least 1400°C. The transformed structure is a structure that undergoes phase transformation and grain growth during the cooling process of the solidified structure, and is formed in the range from the solidification point to 400°C.

[0019] In the present invention, the formation of both the solidified structure and the transformed structure is devised.

[0020] (Ingenuity in the formation of solidified structures) First, the formation of the solidification structure in the present invention will be described. In general, when a molten metal is cooled, a dendritic solid crystallizes out. The formation and development of dendrites has a significant effect on both microsegregation and macrosegregation. Specifically, the presence or absence of secondary dendrite arms and their spacing are important, and the development of secondary arms with narrow spacing reduces both macrosegregation and microsegregation.

[0021] Macrosegregation occurs when alloy elements become concentrated in the liquid phase between secondary dendrites and this concentrated region moves over a long distance due to convection or other factors. Therefore, macrosegregation can be reduced by narrowing the spacing between secondary dendrites to act as a barrier to the movement of atoms distributed in the concentrated region.

[0022] The reduction of microsegregation in the formation of the solidified structure is achieved by narrowing the secondary dendrite arm spacing and shortening the diffusion distance of alloying elements in the enriched regions formed between the secondary dendrite arms. Note that the microsegregation can be further improved not only by the formation of the solidified structure but also by carrying out the first and second cooling steps in the formation of the transformed structure described below.

[0023] Conventional knowledge has suggested that increasing the cooling rate from the start of casting to the solidification point is an effective way to narrow the spacing between secondary dendrite arms. However, titanium and titanium alloys have melting points of 1600°C or higher, and cooling from the start of casting to the solidification point must be performed in an atmosphere that avoids contact between oxygen and the molten metal. This means that there is a limit to how much the spacing between secondary dendrite arms can be narrowed by simply increasing the cooling rate from the start of casting to the solidification point. Therefore, in order to improve the formation of the cast structure, it has been necessary to take measures other than the cooling rate from the start of casting to the solidification point of the molten metal.

[0024] As a result of extensive research, the present inventors have found that the addition of C (carbon) is effective in promoting the growth of secondary dendrite arms in titanium and titanium alloys and in narrowing the secondary dendrite arm spacing.

[0025] (α-type titanium) Generally, in commercially pure titanium, which does not actively add C, dendrites are formed first during solidification. However, in commercially pure titanium, the amount of added elements such as Al and V is small, so the development of secondary dendrite arms is insufficient. Therefore, in the present invention, the amount of C effective for promoting the formation of secondary dendrite arms is 0.100% or more, and more preferably 0.130% or more. If the amount of C is too large, the added C will remain in the cast structure as carbides, causing defects in the manufacturing process. Therefore, the upper limit of the amount of C is 0.450% or less, and more preferably 0.400% or less.

[0026] (α+β titanium alloy) Generally, α+β type alloys that do not actively add C contain relatively large amounts of alloying elements such as Al and V, so that secondary dendrite arms are formed, but the secondary arm spacing is not narrow enough to reduce macrosegregation. Therefore, in the present invention, the necessary amount of C, which is effective for forming sufficiently narrow secondary dendrite arms, is contained, which is 0.310% or more. More preferably, it is 0.400% or more. If the amount of C is too much, the added C will remain in the cast structure as carbides, causing defects in the manufacturing process. Therefore, the upper limit of the amount of C is 0.900% or less, and more preferably, it is 0.850% or less.

[0027] By using the above-mentioned techniques, a solidification structure with reduced macrosegregation and microsegregation can be obtained.

[0028] In addition, in the formation of the solidification structure of α+β type titanium alloy, it is possible to further refine the structure by further preferably containing 0.500% or more of C. When α+β type titanium alloy contains 0.500% or more of C, carbides are crystallized. The crystallized carbides act as nuclei for dendrite formation. The carbides present in large quantities in the molten metal act as nuclei, and dendrite formation occurs in many places, resulting in refinement of the solidification structure. If the C content is appropriate, all of the carbides crystallized in the molten metal will become nuclei for dendrite formation at the stage where solidification is completed, and will not remain. On the other hand, if the C content is too high, carbides will remain, so it is necessary to set a more preferable upper limit according to the alloy composition other than C. A more preferable upper limit of the specific C addition amount is 0.800% or less in the case of α+β type titanium alloy.

[0029] (Ingenuity in the formation of transformed structures) (α+β titanium alloy) In the present invention, phase transformation and grain growth occur during the cooling process of an ingot having a solidification structure in which closely spaced secondary dendrite arms are developed and formed. The formation of transformed structures in the present invention is roughly divided into two. The formation of the first transformed structure is carbide precipitation in the temperature range from the solidification point to 900°C. The formation of the second transformed structure is carbide disappearance, C diffusion, and new crystal grain nucleation in the temperature range from 900°C to 400°C. The cooling process in the temperature range in which the first transformed structure is formed is called the first cooling process, and the cooling process in the temperature range in which the second transformed structure is formed is called the second cooling process. Carbide is precipitated in the first cooling process, and carbide disappearance, C diffusion, and new crystal grain nucleation are achieved in the second cooling process, thereby achieving a finer structure and a reduction in microsegregation compared to the solidification structure.

[0030] (Key Points of the Invention) The key to achieving finer cast structures in the present invention is to satisfy both (I) chemical composition and (II) cooling conditions during casting. (I) and (II) will be described below.

[0031] (I) Chemical composition In the present invention, the incorporation of C is key. The ingot of the present invention has, in mass%, C: 0.100-0.900%, Al: 0-7.000%, Mo: 0-7.000%, V: 0-6.000%, Zr: 0-5.000%, Sn: 0-3.000%, Fe: 0-2.100%, Si: 0-0.500%, Cr: 0-0.400%, Ni: 0-0.400%, Ta: 0-0.400%, Nb: 0 ~0.400%, Mn: 0-0.200%, Ru: 0-0.100%, Pd: 0-0.100%, Cu: 0-0.200%, B: 0-0.090%, Hf: 0-0.090%, O: 0.400% or less, N: 0.300% or less, S: 0.110% or less, P: 0.110% or less, H: 0.035% or less, and the balance consisting of Ti and impurities.

[0032] As described above, the C content of at least 0.100% promotes the formation of secondary dendrite arms, and as described above, the C content of no more than 0.900% prevents the added C from remaining in the cast structure as carbides, suppressing the occurrence of defects during the manufacturing process.

[0033] Elements other than C, namely Al, Mo, V, Zr, Sn, Fe, Si, Cr, Ni, Ta, Nb, Mn, Ru, Pd, Cu, B, Hf, O, N, S, P, and H, are permitted to be contained within the above ranges, which provides the effects of improving strength, suppressing embrittlement, preventing grain boundary cracking, β stabilization, α stabilization, and improving corrosion resistance.

[0034] The appropriate blending ranges of each element vary depending on the alloy type, and are as follows:

[0035] (Chemical composition 1 (assuming that the main metal structure is alpha titanium and the chemical composition is close to that of commercially pure titanium) Chemical composition 1 consists of C: 0.100 - 0.450%, Fe: 0.010 - 0.450%, H: 0.015% or less, O: 0.400% or less, N: 0.300% or less, S: 0.030% or less, P: 0.030% or less, Si: 0.500% or less, Mo: 0 - 1.900%, Al: 0 - 0.400%, Ta: 0 - 0.200%, Nb: 0 - 0.090%, Ru: 0 - 0.100%, Pd: 0 - 0.100%, Ni: 0 - 0.200%, one or more of Mn, Cu, Cr, Sn, Zr: a total of 0 - 0.200%, and the balance being Ti and impurities.

[0036] <C: 0.100 - 0.450%> C shall be 0.100 - 0.450%. Preferably, C is 0.130 - 0.400%. If the chemical composition other than C is within the following ranges, the effects of the invention can be achieved.

[0037] <Fe: 0.010 - 0.450%> Fe is an element contained in sponge titanium or scrap, and when it is dissolved solidly without significant segregation, it contributes to improving the strength of the material. However, if the content of Fe is too high, even when the ingot is cast by the cooling method shown below, the segregation of Fe cannot be completely suppressed, and the defects in the manufacturing process become prominent. Therefore, the upper limit of the content of Fe is 0.450% or less, preferably 0.400% or less. Although it is possible to reduce the content of Fe, it is necessary to use expensive raw materials and the economy is inferior. Therefore, the lower limit of the content of Fe is 0.010% or more, preferably 0.020% or more.

[0038] <H: 0.015% or less> H is an element contained in sponge titanium or scrap, and it causes the material to embrittle by forming a compound with Ti. Therefore, it is better to have less, and the content of H is 0.015% or less, preferably 0.010% or less. Although the lower the content of H is, the better, the lower limit may be, for example, 0.001% or more.

[0039] <O: 0.400% or less> O is an element contained in sponge titanium and scrap, and like C, it dissolves in Ti as an interstitial solid solution element. Although the dissolution of O atoms has a beneficial effect such as improving strength, when the amount of O dissolved increases, the amount of C atoms that can dissolve decreases. Therefore, the content of O is 0.400% or less, preferably 0.350% or less. The lower limit of the content of O may be, for example, 0.001% or more.

[0040] <N: 0.300% or less> N is an element contained in sponge titanium and scrap, and like C, it dissolves in Ti as an interstitial solid solution element. Although the dissolution of N atoms has a beneficial effect such as improving strength, when the amount of N dissolved increases, the amount of C atoms that can dissolve decreases. Therefore, the content of N is 0.300% or less, preferably 0.280% or less. The lower limit of the content of N may be, for example, 0.001% or more.

[0041] <S: 0.030% or less> S is an element contained in sponge titanium and scrap. When the amount of S dissolved is large, S atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of S is 0.030% or less, preferably 0.025% or less. Although the lower the content of S, the better, the lower limit may be, for example, 0.001% or more.

[0042] <P: 0.030% or less> P is an element contained in sponge titanium and scrap. When the amount of P dissolved is large, P atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of P is 0.030% or less, preferably 0.022% or less. Although the lower the content of P, the better, the lower limit may be, for example, 0.001% or more.

[0043] <Si: 0.500% or less> Although Si is a useful element for improving strength, it has a small solid solubility limit in Ti and can easily form a compound with Ti. This compound can cause scratches and cracks, so the Si content is preferably low. Therefore, the Si content is 0.500% or less, and preferably 0.420% or less. The lower limit of the Si content may be, for example, 0.001% or more.

[0044] <Mo:0~1.900%> Mo is a β-stabilizing element and affects the segregation of β-stabilizing elements other than Mo. If the Mo content is too high, the segregation of Fe cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Mo content is 1.900% or less, and preferably 1.400% or less. The lower limit of the Mo content is 0% or more, and may be 0.001% or more.

[0045] <Al:0~0.400%> Al is an α-stabilizing element and affects the segregation of α-stabilizing elements other than Al. If the Al content is too high, the segregation of C cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Al content is 0.400% or less, and preferably 0.280% or less. The lower limit of the Al content is 0% or more, and may be 0.001% or more.

[0046] <Ta:0~0.200%> Ta is an effective element for improving oxidation resistance, but if the Ta content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Ta content is 0.200% or less, and preferably 0.150% or less. The lower limit of the Ta content is 0% or more, and may be 0.001% or more.

[0047] <Nb:0~0.090%> Nb is an effective element for improving oxidation resistance, but if the Nb content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Nb content is 0.090% or less, and preferably 0.060% or less. The lower limit of the Nb content is 0% or more, and may be 0.001% or more.

[0048] <Ru:0~0.100%> Although Ru is an effective element for improving corrosion resistance, it tends to concentrate in the β phase, which affects the segregation of β-stabilizing elements other than Ru. If the Ru content is too high, the segregation of Fe cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Ru content is 0.100% or less, and preferably 0.080% or less. The lower limit of the Ru content is 0% or more, and may be 0.001% or more.

[0049] <Pd:0~0.100%> Although Pd is an effective element for improving corrosion resistance, it tends to concentrate in the β phase, which affects the segregation of β-stabilizing elements other than Pd. If the Pd content is too high, the segregation of Fe cannot be suppressed even if the ingot is cast using the cooling method described below, and defects during the manufacturing process become significant. In addition, if the Pd content is too high, a compound is formed with Ti, which causes significant defects and cracks during the manufacturing process. Therefore, the upper limit of the Pd content is 0.100% or less, and preferably 0.090% or less. The lower limit of the Pd content is 0% or more, and may be 0.001% or more.

[0050] <Ni:0~0.200%> Although Ni is an effective element for improving corrosion resistance, if the Ni content is too high, it forms a compound with Ti, which causes noticeable scratches and cracks during the manufacturing process. Therefore, the upper limit of the Ni content is 0.200% or less, preferably 0.180% or less. The lower limit of the Ni content is 0% or more, and may be 0.001% or more.

[0051] <One or more of Mn, Cu, Cr, Sn, and Zr: a total of 0 to 0.200%> Containing one or more of Mn, Cu, Cr, Sn, and Zr has the advantage of improving corrosion resistance. However, the effect is not exerted if the total content of Mn, Cu, Cr, Sn, and Zr is too high. Therefore, the upper limit of the total content of one or more of Mn, Cu, Cr, Sn, and Zr is 0.200% or less, preferably 0.180% or less. The lower limit of the total content of these elements is 0% or more, and it may also be 0.001% or more.

[0052] Next, when assuming the chemical composition of an α + β type titanium alloy, etc., it is preferable to set the ranges of the chemical compositions of "Chemical Composition 2", "Chemical Composition 3", and "Chemical Composition 4" described below.

[0053] (Chemical Composition 2) Chemical Composition 2 is composed of C: 0.310 to 0.900%, Al: 4.500% to 6.500%, Fe: 0.500% to 2.100%, N: 0.050% or less, O: 0.250% or less, Si: 0 to 0.500%, Mo: 0 to 7.000%, Cr: 0 to 0.400%, Cu: 0 to 0.090%, Ni: 0 to 0.400%, Hf: 0 to 0.090%, B: 0 to 0.090%, Nb: 0 to 0.400%, Ta: 0 to 0.400%, Sn: 0 to 1.900%, Zr: 0 to 0.400%, Ru: 0 to 0.100%, Pd: 0 to 0.100%, S: 0.080% or less, P: 0.080% or less, H: 0.025% or less, and the balance consists of Ti and impurities.

[0054] <C: 0.310 to 0.900%> In the case of Chemical Composition 2, C is set to 0.310 to 0.900%. Preferably, C is 0.400 to 0.850%, and more preferably, C is 0.500 to 0.800%. The invention's effect can be achieved as long as the chemical composition other than C is within the following ranges.

[0055] <Al: 4.500% to 6.500%> Al is an α-stabilizing element and affects not only the segregation of Al itself but also the segregation of α-stabilizing elements other than Al. If the Al content is too high, even when the ingot is cast by the cooling method shown below, the segregation of C or Al cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the upper limit of the Al content is 6.500% or less, preferably 6.200% or less. If the Al content is too low, even when the ingot is cast by the cooling method shown below, the grain refinement is not sufficient. Therefore, the lower limit of the Al content is 4.500% or more, preferably 4.750% or more.

[0056] <Fe: 0.500 - 2.100%> Fe is an element contained in sponge titanium and scrap, and when it is dissolved without significant segregation, it contributes to the improvement of the strength of the material. However, if the Fe content is too high, even when the ingot is cast by the cooling method shown below, the segregation of Fe cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the upper limit of the Fe content is 2.100% or less, preferably 1.900% or less. Although it is possible to reduce the Fe content, even when the ingot is cast by the cooling method shown below, the grain refinement is not sufficient, so the lower limit of the Fe content is 0.500% or more, preferably 0.700% or more.

[0057] <N: 0.050% or less> N is an element contained in sponge titanium and scrap, and like C, it dissolves in Ti as an interstitial solid solution element. Although the dissolution of N atoms has a beneficial effect on strength improvement, etc., when the amount of N dissolved increases, the amount of C atoms that can dissolve decreases. Therefore, the N content is 0.050% or less, preferably 0.030% or less. The lower limit of the N content may be, for example, 0.001% or more.

[0058] <O: 0.250% or less> O is an element contained in titanium sponge and scrap, and dissolves in Ti as an interstitial solid solution element, similar to C. Although the dissolution of O atoms has a positive effect on improving strength, the amount of C atoms that can dissolve decreases as the amount of O dissolved increases. Therefore, the O content is 0.250% or less, and preferably 0.220% or less. The lower limit of the O content may be, for example, 0.001% or more.

[0059] <Si:0~0.500%> Although Si is a useful element for improving strength, it has a small solid solubility limit in Ti and can form a compound with Ti. This compound can cause scratches and cracks, so the Si content is preferably low. Therefore, the Si content is 0.500% or less, and preferably 0.420% or less. The lower limit of the Si content is 0% or more, and may be 0.001% or more.

[0060] <Mo:0~7.000%> Mo is a β-stabilizing element and affects the segregation of β-stabilizing elements other than Mo. If the Mo content is too high, the segregation of Fe or Mo cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Mo content is 7.000% or less, and preferably 6.600% or less. The lower limit of the Mo content is 0% or more, and may be 0.001% or more.

[0061] <Cr:0~0.400%> Although Cr is an effective element for improving corrosion resistance, it affects the segregation of β-stabilizing elements other than Cr. If the Cr content is too high, even if the ingot is cast using the cooling method described below, the segregation of Fe or Mo cannot be suppressed completely, and defects in the manufacturing process become significant. Therefore, the upper limit of the Cr content is 0.400% or less, and preferably 0.350% or less. The lower limit of the Cr content is 0% or more, and may be 0.001% or more.

[0062] <Cu:0~0.090%> Cu has the advantage of improving corrosion resistance, but if the Cu content is too high, this effect is not exerted. Also, if the Cu content is too high, it may form a compound with Ti and cause scratches and cracks. Therefore, the upper limit of the Cu content is 0.090% or less, preferably 0.060% or less. The lower limit of the Cu content is 0% or more, and may be 0.001% or more.

[0063] <Ni:0~0.400%> Although Ni is an effective element for improving corrosion resistance, if the Ni content is too high, it forms a compound with Ti, which causes noticeable scratches and cracks during the manufacturing process. Therefore, the upper limit of the Ni content is 0.400% or less, preferably 0.350% or less. The lower limit of the Ni content is 0% or more, and may be 0.001% or more.

[0064] <Hf:0~0.090%> Although Hf is an effective element for improving oxidation resistance, if the Hf content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Hf content is 0.090% or less, and preferably 0.075% or less. The lower the Hf content, the better, but the lower limit is 0% or more, and may be 0.001% or more.

[0065] <B:0~0.090%> Although B is an effective element for improving oxidation resistance, if the B content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. In addition, if the B content is too high, it may form a compound with Ti, causing defects and cracks. Therefore, the upper limit of the B content is 0.090% or less, and preferably 0.070% or less. The lower limit of the B content is 0% or more, and may be 0.001% or more.

[0066] <Nb:0~0.400%> Nb is an effective element for improving oxidation resistance, but if the Nb content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Nb content is 0.400% or less, and preferably 0.360% or less. The lower limit of the Nb content is 0% or more, and may be 0.001% or more.

[0067] <Ta:0~0.400%> Ta is an effective element for improving oxidation resistance, but if the Ta content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Ta content is 0.400% or less, and preferably 0.250% or less. The lower limit of the Ta content is 0% or more, and may be 0.001% or more.

[0068] <Sn:0~1.900%> Sn has the advantage of improving corrosion resistance, but if the Sn content is too high, this effect is not exerted. Therefore, the upper limit of the Sn content is 1.900% or less, preferably 0.200% or less. The lower limit of the Sn content may be, for example, 0.001% or more.

[0069] <Zr:0~0.400%> Zr has the advantage of improving corrosion resistance, but if the Zr content is too high, this effect is not exerted. Therefore, the upper limit of the Zr content is 0.400% or less, preferably 0.200% or less. The lower limit of the Zr content is 0% or more, and may be 0.001% or more.

[0070] <Ru:0~0.100%> Although Ru is an element effective for improving corrosion resistance, it tends to concentrate in the β phase and affects the segregation of β-stabilizing elements other than Ru. If the Ru content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe or Mo cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the upper limit of the Ru content is 0.100% or less, preferably 0.080% or less. The lower limit of the Ru content is 0% or more, and may be 0.001% or more.

[0071] <Pd: 0 to 0.100%> Although Pd is an element effective for improving corrosion resistance, it tends to concentrate in the β phase and affects the segregation of β-stabilizing elements other than Pd. If the Pd content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe or Mo cannot be completely suppressed, and defects in the manufacturing process become prominent. Also, if the Pd content is too high, compounds with Ti are formed, and defects and cracks in the manufacturing process become prominent. Therefore, the upper limit of the Pd content is 0.100% or less, preferably 0.090% or less. The lower limit of the Pd content is 0% or more, and may be 0.001% or more.

[0072] <S: 0.080% or less> S is an element contained in sponge titanium and scrap. When the solid solution amount of S is large, S atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of S is 0.080% or less, preferably 0.070% or less. Although the lower the content of S, the better, the lower limit may be, for example, 0.001% or more.

[0073] <P: 0.080% or less> P is an element contained in sponge titanium and scrap. When the solid solution amount of P is large, P atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of P is 0.080% or less, preferably 0.065% or less. Although the lower the content of P, the better, the lower limit may be, for example, 0.001% or more.

[0074] <H: 0.025% or less> H is an element contained in titanium sponge and scrap, and forms a compound with Ti, which causes the material to become embrittled. Therefore, the less the better, and the H content is 0.025% or less, and preferably 0.020% or less. The lower the H content, the better, but the lower limit may be, for example, 0.001% or more.

[0075] (Chemical composition 3) Chemical composition 3 is: C: 0.310-0.900%, Al: 2.000%-7.000%, V: 1.500-6.000%, Fe: 0.500% or less, N: 0.050% or less, O: 0.250% or less, Si: 0-0.500%, Mo: 0-7.00%, Cr: 0-0.400%, Cu: 0-0.090%, Ni: 0-0.400 %, Hf: 0-0.090%, B: 0-0.090%, Nb: 0-0.400%, Ta: 0-0.400%, Sn: 0-1.900%, Zr: 0-0.400%, Ru: 0-0.100%, Pd: 0-0.100%, S: 0.110% or less, P: 0.110% or less, H: 0.030% or less, balance: Ti and impurities.

[0076] <C:0.310~0.900%> In chemical composition 3, C is 0.310 to 0.900%. Preferably, C is 0.400 to 0.850%, and more preferably, C is 0.500 to 0.800%. If the chemical composition other than C is within the following ranges, the effect of the invention can be achieved.

[0077] <Al:2.000%~7.000%> Al is an α-stabilizing element and affects not only the segregation of Al itself but also the segregation of α-stabilizing elements other than Al. If the Al content is too high, the segregation of C or Al cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Al content is 7.000% or less, and preferably 6.800% or less. If the Al content is too low, the crystal grains are not sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the lower limit of the Al content is 2.000% or more, and preferably 2.250% or more.

[0078] <V: 1.500 to 6.000%> V is a β-stabilizing element and affects the segregation of β-stabilizing elements other than V. If the V content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe, Mo, or V cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the upper limit of the V content is 6.000% or less, preferably 5.650% or less. If the V content is too low, even when the ingot is cast by the cooling method shown below, the grain refinement is not sufficient. Therefore, the lower limit of the V content is 1.500% or more, preferably 6.000% or more.

[0079] <Fe: 0.500% or less> Fe is an element contained in sponge titanium or scrap, and when dissolved in solid solution without significant segregation, it contributes to improving the strength of the material. However, if the Fe content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the Fe content is 0.500% or less, preferably 0.300% or less. The Fe content may be 0.001% or more.

[0080] <N: 0.050% or less> N is an element contained in sponge titanium or scrap, and like C, it dissolves in Ti as an interstitial solid solution element. Although the dissolution of N atoms has a good effect such as improving strength, when the amount of N dissolved increases, the amount of C atoms that can dissolve decreases. Therefore, the N content is 0.050% or less, preferably 0.030% or less. The N content may be 0.001% or more.

[0081] <O: 0.250% or less> O is an element contained in titanium sponge and scrap, and dissolves in Ti as an interstitial solid solution element, similar to C. Although the dissolution of O atoms has a positive effect on improving strength, the amount of C atoms that can dissolve decreases as the amount of O dissolved increases. Therefore, the O content is 0.250% or less, and preferably 0.220% or less. The O content may be 0.001% or more.

[0082] <Si:0~0.500%> Although Si is a useful element for improving strength, it has a small solid solubility limit in Ti and can form a compound with Ti. This compound can cause scratches and cracks, so the Si content is preferably low. Therefore, the Si content is 0.500% or less, and preferably 0.420% or less. The Si content may be 0.001% or more.

[0083] <Mo:0~7.000%> Mo is a β-stabilizing element and affects the segregation of β-stabilizing elements other than Mo. If the Mo content is too high, even if the ingot is cast using the cooling method described below, the segregation of Fe, Mo, or V cannot be suppressed completely, and defects in the manufacturing process become significant. Therefore, the upper limit of the Mo content is 7.000% or less, and preferably 6.600% or less. The lower limit of the Mo content is 0% or more, and may be 0.001% or more.

[0084] <Cr:0~0.400%> Although Cr is an effective element for improving corrosion resistance, it affects the segregation of β-stabilizing elements other than Cr. If the Cr content is too high, even if the ingot is cast using the cooling method described below, the segregation of Fe, Mo, or V cannot be suppressed completely, and defects in the manufacturing process become significant. Therefore, the upper limit of the Cr content is 0.400% or less, and preferably 0.350% or less. The lower limit of the Cr content is 0% or more, and may be 0.001% or more.

[0085] <Cu:0~0.090%> Cu has the advantage of improving corrosion resistance, but if the Cu content is too high, this effect is not exerted. Also, if the Cu content is too high, it may form a compound with Ti and cause scratches and cracks. Therefore, the upper limit of the Cu content is 0.090% or less, preferably 0.060% or less. The lower limit of the Cu content is 0% or more, and may be 0.001% or more.

[0086] <Ni:0~0.400%> Although Ni is an effective element for improving corrosion resistance, if the Ni content is too high, it forms a compound with Ti, which causes noticeable scratches and cracks during the manufacturing process. Therefore, the upper limit of the Ni content is 0.400% or less, preferably 0.350% or less. The lower limit of the Ni content is 0% or more, and may be 0.001% or more.

[0087] <Hf:0~0.090%> Although Hf is an effective element for improving oxidation resistance, if the Hf content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Hf content is 0.090% or less, and preferably 0.075% or less. The lower limit of the Hf content is 0% or more, and may be 0.001% or more.

[0088] <B:0~0.090%> Although B is an effective element for improving oxidation resistance, if the B content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. In addition, if the B content is too high, it may form a compound with Ti, causing defects and cracks. Therefore, the upper limit of the B content is 0.090% or less, and preferably 0.070% or less. The lower limit of the B content is 0% or more, and may be 0.001% or more.

[0089] <Nb:0~0.400%> Nb is an effective element for improving oxidation resistance, but if the Nb content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Nb content is 0.400% or less, and preferably 0.360% or less. The lower limit of the Nb content is 0% or more, and may be 0.001% or more.

[0090] <Ta:0~0.400%> Ta is an effective element for improving oxidation resistance, but if the Ta content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Ta content is 0.400% or less, and preferably 0.250% or less. The lower limit of the Ta content is 0% or more, and may be 0.001% or more.

[0091] <Sn:0~1.900%> Sn has the advantage of improving corrosion resistance, but if the Sn content is too high, this effect is not exerted. Therefore, the upper limit of the Sn content is 1.900% or less, preferably 0.200% or less. The lower limit of the Sn content is 0% or more, and may be 0.001% or more.

[0092] <Zr:0~0.400%> Zr has the advantage of improving corrosion resistance, but if the Zr content is too high, this effect is not exerted. Therefore, the upper limit of the Zr content is 0.400% or less, preferably 0.200% or less. The lower limit of the Zr content is 0% or more, and may be 0.001% or more.

[0093] <Ru:0~0.100%> Although Ru is an element effective in improving corrosion resistance, it tends to concentrate in the β phase and affects the segregation of β-stabilizing elements other than Ru. If the Ru content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe, segregation of Mo, or segregation of V cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the upper limit of the Ru content is 0.100% or less, preferably 0.080% or less. The lower limit of the Ru content is 0% or more, and may be 0.001% or more.

[0094] <Pd: 0 to 0.100%> Although Pd is an element effective in improving corrosion resistance, it tends to concentrate in the β phase and affects the segregation of β-stabilizing elements other than Pd. If the Pd content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe, segregation of Mo, or segregation of V cannot be completely suppressed, and defects in the manufacturing process become prominent. Also, if the Pd content is too high, compounds with Ti are formed, and defects and cracks in the manufacturing process become prominent. Therefore, the upper limit of the Pd content is 0.100% or less, preferably 0.090% or less. The lower limit of the Pd content is 0% or more, and may be 0.001% or more.

[0095] <S: 0.110% or less> S is an element contained in sponge titanium and scrap. When the solid solution amount of S is large, S atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of S is 0.110% or less, preferably 0.090% or less. The content of S may be 0.001% or more.

[0096] <P: 0.110% or less> P is an element contained in sponge titanium and scrap. When the solid solution amount of P is large, P atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of P is 0.110% or less, preferably 0.085% or less. The content of P may be 0.001% or more.

[0097] <H: 0.030% or less> H is an element contained in titanium sponge and scrap, and forms a compound with Ti, which causes the material to become embrittled. Therefore, the less H, the better, and the H content is 0.030% or less, preferably 0.024% or less. The H content may be 0.001% or more.

[0098] (Chemical composition 4) Chemical composition 4 is C: 0.310-0.900%, Al: 5.000%-7.000%, Mo: 1.000%-7.000%, Zr: 3.000%-5.000%, Sn: 1.000%-3.000%, Si: 0%-0.500%, Fe: 0.500% or less, N: 0.050% or less, O: 0.250% or less, Cr: 0-0.40 0%, Cu: 0-0.090%, Ni: 0-0.400%, Hf: 0-0.090%, B: 0-0.090%, Nb: 0-0.400%, Ta: 0-0.400%, Ru: 0-0.100%, Pd: 0-0.100%, S: 0.110% or less, P: 0.110% or less, H: 0.035% or less, balance: Ti and impurities.

[0099] <C:0.310~0.900%> In chemical composition 4, C is 0.310 to 0.900%. Preferably, C is 0.400 to 0.850%, and more preferably, C is 0.500 to 0.800%. If the chemical composition other than C is within the following ranges, the effect of the invention can be achieved.

[0100] <Al:5.000%~7.000%> Al is an α-stabilizing element and affects not only the segregation of Al itself but also the segregation of α-stabilizing elements other than Al. If the Al content is too high, the segregation of C or Al cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Al content is 7.000% or less, preferably 6.400% or less. If the Al content is too low, the grains are not sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the lower limit of the Al content is 5.000% or more, preferably 5.200% or more.

[0101] <Mo:1.000~7.000%> Mo is a β-stabilizing element and affects not only the segregation of Mo itself but also the segregation of β-stabilizing elements other than Mo. If the Mo content is too high, the segregation of Fe or Mo cannot be suppressed even if the ingot is cast using the cooling method described below, and defects in the manufacturing process become significant. Therefore, the upper limit of the Mo content is 7.000% or less, and preferably 6.400% or less. If the Mo content is too low, the crystal grains are not sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the lower limit of the Mo content is 1.000% or more, and preferably 0.780% or more.

[0102] <Zr:3.000%~5.000%> Zr has the effect of reducing the grain size of the ingot, and if the Zr content is too low, the grains will not be sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the lower limit of the Zr content is 3.000% or more, and preferably 3.480% or more. If the Zr content is too high, the grains will not be sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the upper limit of the Zr content is 5.000% or less, and preferably 4.500% or less.

[0103] <Sn:1.000%~3.000%> Sn has the effect of reducing the grain size of the ingot, and if the Sn content is too low, the grains will not be sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the lower limit of the Sn content is 1.000% or more, and preferably 1.200% or more. If the Sn content is too high, the grains will not be sufficiently refined even if the ingot is cast using the cooling method described below. Therefore, the upper limit of the Sn content is 3.000% or less, and preferably 2.650% or less.

[0104] <Si:0~0.500%> Although Si is an element useful for improving strength, etc., its solubility limit in Ti is small and it can form a compound with Ti. Since this compound can cause defects and cracks, it is better to have a lower Si content. Therefore, the Si content is 0.500% or less, preferably 0.420% or less. The lower limit of the Si content is 0% or more, and it may also be 0.001% or more.

[0105] <Fe: 0.500% or less> Fe is an element contained in sponge titanium and scrap, and when it is dissolved without significant segregation, it contributes to improving the strength of the material. However, if the Fe content is too high, even when the ingot is cast by the cooling method shown below, the segregation of Fe cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the Fe content is 0.500% or less, preferably 0.400% or less. The lower limit of the Fe content may also be 0.001% or more.

[0106] <N: 0.050% or less> N is an element contained in sponge titanium and scrap, and like C, it dissolves in Ti as an interstitial solid solution element. Although the dissolution of N atoms has a good effect on improving strength, etc., when the amount of N dissolved increases, the amount of C atoms that can dissolve decreases. Therefore, the N content is 0.050% or less, preferably 0.030% or less. The lower limit of the N content may also be 0.001% or more.

[0107] <O: 0.250% or less> O is an element contained in sponge titanium and scrap, and like C, it dissolves in Ti as an interstitial solid solution element. Although the dissolution of O atoms has a good effect on improving strength, etc., when the amount of O dissolved increases, the amount of C atoms that can dissolve decreases. Therefore, the O content is 0.250% or less, preferably 0.220% or less. The lower limit of the O content may also be 0.001% or more.

[0108] <Cr: 0 to 0.400%> Although Cr is an effective element for improving corrosion resistance, it affects the segregation of β-stabilizing elements other than Cr. If the Cr content is too high, even if the ingot is cast using the cooling method described below, the segregation of Fe and Mo cannot be suppressed completely, and defects in the manufacturing process become significant. Therefore, the upper limit of the Cr content is 0.400% or less, and preferably 0.350% or less. The lower limit of the Cr content is 0% or more, and may be 0.001% or more.

[0109] <Cu:0~0.090%> Cu has the advantage of improving corrosion resistance, but if the Cu content is too high, this effect is not exerted. Also, if the Cu content is too high, it may form a compound with Ti and cause scratches and cracks. Therefore, the upper limit of the Cu content is 0.090% or less, preferably 0.060% or less. The lower limit of the Cu content is 0% or more, and may be 0.001% or more.

[0110] <Ni:0~0.400%> Although Ni is an effective element for improving corrosion resistance, if the Ni content is too high, it forms a compound with Ti, which causes noticeable scratches and cracks during the manufacturing process. Therefore, the upper limit of the Ni content is 0.400% or less, preferably 0.350% or less. The lower limit of the Ni content is 0% or more, and may be 0.001% or more.

[0111] <Hf:0~0.090%> Although Hf is an effective element for improving oxidation resistance, if the Hf content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Hf content is 0.090% or less, and preferably 0.075% or less. The lower limit of the Hf content is 0% or more, and may be 0.001% or more.

[0112] <B:0~0.090%> Although B is an effective element for improving oxidation resistance, if the B content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. In addition, if the B content is too high, it may form a compound with Ti, causing defects and cracks. Therefore, the upper limit of the B content is 0.090% or less, and preferably 0.070% or less. The lower limit of the B content is 0% or more, and may be 0.001% or more.

[0113] <Nb:0~0.400%> Nb is an effective element for improving oxidation resistance, but if the Nb content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Nb content is 0.400% or less, and preferably 0.360% or less. The lower limit of the Nb content is 0% or more, and may be 0.001% or more.

[0114] <Ta:0~0.400%> Ta is an effective element for improving oxidation resistance, but if the Ta content is too high, even if the ingot is cast using the cooling method described below to obtain an appropriate grain size, the crystal grains tend to become large just below the scale formed in the manufacturing process, and defects in the manufacturing process become noticeable. Therefore, the upper limit of the Ta content is 0.400% or less, and preferably 0.250% or less. The lower limit of the Ta content is 0% or more, and may be 0.001% or more.

[0115] <Ru:0~0.100%> Although Ru is an element effective in improving corrosion resistance, it has a tendency to concentrate in the β phase and affects the segregation of β-stabilizing elements other than Ru. If the Ru content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe, segregation of Mo, or segregation of V cannot be completely suppressed, and defects in the manufacturing process become prominent. Therefore, the upper limit of the Ru content is 0.100% or less, preferably 0.080% or less. The lower limit of the Ru content is 0% or more, and may be 0.001% or more.

[0116] <Pd: 0~0.100%> Although Pd is an element effective in improving corrosion resistance, it has a tendency to concentrate in the β phase and affects the segregation of β-stabilizing elements other than Pd. If the Pd content is too high, even when the ingot is cast by the cooling method shown below, segregation of Fe, segregation of Mo, or segregation of V cannot be completely suppressed, and defects in the manufacturing process become prominent. Also, if the Pd content is too high, compounds with Ti are formed, and defects and cracks in the manufacturing process become prominent. Therefore, the upper limit of the Pd content is 0.100% or less, preferably 0.090% or less. The lower limit of the Pd content is 0% or more, and may be 0.001% or more.

[0117] <S: 0.110% or less> S is an element contained in sponge titanium and scrap. When the solid solution amount of S is large, S atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of S is 0.110% or less, preferably 0.090% or less. The lower limit of the S content may be 0.001% or more.

[0118] <P: 0.110% or less> P is an element contained in sponge titanium and scrap. When the solid solution amount of P is large, P atoms tend to segregate at grain boundaries and grain boundary cracking is likely to occur. Therefore, the content of P is 0.110% or less, preferably 0.085% or less. The lower limit of the P content may be 0.001% or more.

[0119] <H: 0.035% or less> H is an element contained in titanium sponge and scrap, and forms a compound with Ti, which causes the material to become embrittled. Therefore, the less the better, and the H content is 0.035% or less, preferably 0.028% or less. The lower limit of the H content may be 0.001% or more.

[0120] (II) Cooling method The ingot of the present invention is manufactured through a casting process. In the casting process, for example, sponge titanium previously manufactured through a refining process or the like is mixed with necessary auxiliary materials (TiO2, etc. and metallic iron), and then press-molded into titanium briquettes, which are then used as electrodes to melt in a vacuum arc melting furnace, and the molten metal is cast to manufacture an ingot. Alternatively, sponge titanium or titanium briquettes are melted in an electron beam melting furnace or a plasma arc melting furnace, and the molten metal is cast to manufacture an ingot.

[0121] In the present invention, when forming the molten metal, the C (carbon) content is adjusted, and the cooling rate is controlled during casting.

[0122] The cooling method in the casting process in the present invention includes a first cooling process and a second cooling process. In the first cooling process, the average cooling rate from the solidification point of the ingot to 900°C is 1.00°C / s or more. The upper limit of the average cooling rate is preferably 10.00°C / s or less, and more preferably 2.50°C / s or less. In the second cooling process, the average cooling rate from 900°C to 400°C is 0.001°C / s or more and 0.500°C / s or less. This makes it possible to make the average grain size of the cast structure 90 μm or less. It is difficult to make the average grain size of the cast structure 90 μm or less by only one of the first cooling process and the second cooling process.

[0123] In order to realize the above average cooling rate, the following measures (A) to (C) are taken, for example.

[0124] (A) In order to keep the average cooling rate from the freezing point to 900°C within the above range, the cooling capacity of the coolant used to cool the mold is increased. In other words, a coolant with a specific heat of 4.00 kJ / (kg·K) or more is used as the circulating coolant for cooling the mold. One example of a coolant is water. In addition, the thermal conductivity of the mold's constituent material is 20.0 W / (m·K) or more, the coolant temperature is 50°C or less, and the circulation rate of the coolant is 2 tons / h or more.

[0125] (B) In order to keep the average cooling rate from the solidification point to 900°C within the above range, the ratio of the cross-sectional area of ​​the ingot to the surface area inside the mold (cross-sectional area of ​​the ingot / surface area inside the mold) is set to 0.8 or less. As shown in Figures 2 and 3, the cross-sectional area of ​​the ingot is the area of ​​a cross section perpendicular to the casting direction, assuming that the direction in which the ingot is extracted from the mold is the casting direction. The surface area inside the mold is the surface area of ​​the inner surface of the mold.

[0126] For example, as shown in FIG. 3(a), if the ingot is cylindrical, and the diameter of the ingot is W1 and the height of the ingot is H x In this case, the cross-sectional area of ​​the ingot and the surface area inside the mold are calculated by the following formulas.

[0127] Ingot cross-sectional area = (W1 / 2) · (W1 / 2) · π

[0128] Surface area of ​​the mold interior = W1 H x π

[0129] Ingot cross-sectional area / mold internal surface area = W1 / (4·H x )

[0130] As shown in FIG. 3(b), the ingot is a rectangular parallelepiped, and the width of the ingot is W2, the thickness of the ingot is D, and the height of the ingot is H. x In this case, the cross-sectional area of ​​the ingot and the surface area inside the mold are calculated by the following formulas.

[0131] Ingot cross-sectional area = W2·D

[0132] Surface area of ​​the mold interior = 2(W2+D) H x

[0133] Ingot cross-sectional area / mold upper surface area = W2·D / {2H x ·(W2+D)}

[0134] H x : Height of mold (m) W1: diameter of ingot (m) W2: Width of ingot (m) D: Thickness of the ingot when the shape is rectangular (m) π: Pi

[0135] In addition, W1, W2, H x There are no particular limitations on D, and it is sufficient that the cross-sectional area of ​​the ingot / the surface area inside the mold is 0.8 or less.

[0136] (C) In order to keep the casting cooling rate range from 900°C to 400°C within the above range, the emissivity of the ingot cooling section (corresponding to symbol H2) shown in the schematic diagram of FIG. 2 is set to 0.4 or less.

[0137] As shown in FIG. 2, the ingot 7 reaches a temperature range of 900°C to 400°C after being extracted from the mold 5, so that the ingot 7 in this temperature range does not come into contact with other solids including the mold 5. However, the ingot 7 in a high temperature state after casting needs to be kept in a vacuum to prevent oxidation of titanium. Therefore, the ingot 7 after casting is placed in a vacuum container 8 as shown in FIG. 1, and a cover member for heat insulation may be installed near the ingot in the vacuum container 8. The cover member may be made of any material as long as it can withstand high temperatures of several hundred degrees and can be used in a vacuum, but the emissivity of the ingot 7 changes depending on the selection of the cover member. To make the emissivity 0.4 or less, for example, stainless steel having metallic luster is used as the cover member for the ingot 7. In addition, it is preferable to adjust the distance between the ingot 7 and the cover member in order to make the emissivity 0.4 or less.

[0138] The emissivity is the value measured in the atmosphere at 400°C. A contact thermometer and a radiation thermometer are used to measure the temperature of an object heated to 400°C, and the emissivity of the radiation thermometer is set so that the difference is within 10°C. The set emissivity is the emissivity in this invention.

[0139] Of the above-mentioned conditions (A) to (C), the cooling conditions required to obtain the ingot of this embodiment can be realized by adopting any of the combination of (A) and (C), the combination of (B) and (C), or all of the combinations of (A), (B), and (C).

[0140] By satisfying the chemical composition described in (I) above and the cooling conditions described in (II) above, both macrosegregation and microsegregation are reduced, and the solidified structure is refined.

[0141] In this embodiment, it is sufficient to satisfy the above (I) and (II), and the melting method in the melting step is not limited. Any melting method such as VAR, EBR, or PAM for melting titanium or titanium alloys may be used, and the shape and structure of the hearth are not limited.

[0142] (Problem-solving mechanisms) Hereinafter, the mechanism for reducing macrosegregation, the mechanism for reducing microsegregation, and the mechanism for refining the cast structure in the ingot manufacturing method of the present embodiment will be described.

[0143] (Macrosegregation reduction mechanism) Macrosegregation is reduced by forming a solidification structure. The formation of secondary dendrite arms and narrowing the spacing between the secondary dendrite arms are important for reducing macrosegregation. The cause of macrosegregation is that alloy elements are concentrated in the liquid phase between secondary dendrites, and this concentrated area moves over a long range due to convection, etc. Therefore, by narrowing the spacing between secondary dendrites to act as a barrier to movement, macrosegregation can be reduced.

[0144] Adding carbon is effective in forming secondary dendrite arms and narrowing the secondary dendrite arm spacing. Compared to other elements contained in titanium and titanium alloys, carbon has an equilibrium distribution coefficient that is significantly different from 1.0, so it diffuses significantly from the solid phase to the liquid phase in a solid-liquid coexistence state. As carbon diffuses from the solid phase to the liquid phase, the development of secondary arms becomes more pronounced and the secondary dendrite arm spacing also narrows. As a result of the narrowing of the secondary dendrite arm spacing, macrosegregation is reduced.

[0145] (Mechanism for reducing microsegregation) The reduction of microsegregation is related to both the formation of solidification structure and the formation of transformation structure. Microsegregation occurs when the secondary dendrite arms are formed, and alloy element enriched regions remain between the secondary dendrite arms, near the tip of the secondary dendrite arms, near the tip of the primary dendrite arms, etc., and these alloy element enriched regions become microsegregation in the ingot. The narrowing of the secondary dendrite arms in the formation of the solidification structure functions as a barrier to the movement of the alloy element enriched regions and is effective in reducing macrosegregation, but the alloy element enriched regions remain as microsegregation, which is not sufficient for reducing microsegregation. In order to sufficiently reduce microsegregation, in the formation of the transformation structure after the formation of the solidification structure, the structure is refined to minimize segregation by satisfying both the first cooling step conditions and the second cooling step conditions, and further, the segregation elements are sufficiently diffused in these cooling steps, thereby reducing microsegregation.

[0146] (Mechanism of Refining Cast Structure) The cast structure is refined in the formation of a transformed structure when the C content is in the entire range of the above chemical composition 1, and when the C content of the above chemical compositions 2 to 4 is 0.31 to 0.50%. Furthermore, the cast structure is refined in the formation of the solidified structure and the transformed structure when the C content of the above chemical compositions 2 and 3 is 0.50-0.90% and when the C content of the above chemical composition 3 is 0.50-0.80%.

[0147] The refinement of the cast structure in the formation of the transformed structure, which is common to all of the above chemical compositions 1 to 4, is achieved by controlling the formation and disappearance of carbides (C solid solution) during the cooling process.

[0148] First, we will explain the role of the C content in refining the cast structure of the present invention and the reason for specifying the amount of C. Next, we will explain the reason for specifying the average cooling rate from the solidification point to 900°C and the reason for specifying the average cooling rate from 900°C to 400°C.

[0149] The role of C in the present invention is to form carbides in the first cooling step in the formation of a transformed structure, and to function as a nucleation site for fine crystal grains in the process in which the carbides disappear in the second cooling step.

[0150] The transformation structure is formed by cooling the solidified structure, but the solidified structure of the present invention does not have carbides. In the first cooling step in which the solidified structure is cooled, carbides precipitate due to a decrease in the C solid solubility limit. However, the first cooling step alone does not result in the precipitation of carbides, thereby not achieving the refinement of the cast structure. The refinement of the cast structure is achieved by further cooling the structure in which carbides have been precipitated in the first cooling step in the second cooling step, causing the carbides to disappear, and forming new crystal grains. The carbides precipitated in the first cooling step disappear as the C atoms in the carbides diffuse into the parent phase in the second cooling step. When the carbides disappear, new crystal grains nucleate. Generally, the new crystal grains are very small at the nucleation stage, but they grow, which is not sufficient for refinement. However, in the present invention, the C atoms diffused into the parent phase suppress the grain growth by the drag effect, thereby suppressing the nucleation of new crystal grains, and a fine cast structure can be obtained.

[0151] In order to achieve refinement of the cast structure through the above mechanism, the chemical composition and the average cooling rate must be within a range in which the precipitation of carbides in the first cooling step, the diffusion of C atoms in the carbides, the disappearance of carbides, and the nucleation of new crystal grains in the second cooling step all occur, and therefore it is important not only to set the chemical composition within the range explained in (I) above as the range for sufficiently causing all of the above structural changes, but also to control the average cooling rates in the first cooling step and the second cooling step.

[0152] In the first cooling step, it is necessary to precipitate carbides (or leave the crystallized carbides). In an alloy composition close to that of commercially pure titanium, if the average cooling rate in the first cooling step is too fast, carbide precipitation is insufficient. On the other hand, if the average cooling rate in the first cooling step is too slow, carbides precipitate but grow too large, resulting in insufficient disappearance of carbides and nucleation of new crystal grains in the second cooling step. For these reasons, the appropriate average cooling rate range for the first cooling step is the range explained in (II).

[0153] In the second cooling step, it is necessary to achieve all of the following: diffusion of C atoms in carbide into the matrix, disappearance of carbide, and nucleation of new crystal grains. If the average cooling rate in the second cooling step is too fast, the diffusion of C atoms in carbide into the matrix is ​​insufficient, so that disappearance of carbide and nucleation of new crystal grains are insufficient, and the grain size of the cast structure specified in the present invention cannot be satisfied. On the other hand, if the average cooling rate in the second cooling step is too slow, although the diffusion of C atoms in carbide into the matrix, disappearance of carbide, and nucleation of new crystal grains are all sufficiently achieved, the nucleated grains grow too much, and the grain size of the cast structure specified in the present invention cannot be satisfied. For the above reasons, the range of the average cooling rate in the second cooling step is set to the range described in (II).

[0154] (Method of measuring average grain size of cast structure and average grain size of cast structure) The average crystal grain size of the cast structure is measured by taking samples near the center of the ingot, near the surface layer of the side of the ingot, near the center of the top of the ingot, and near the center of the bottom of the ingot, and the cut surface of each sample is mirror-polished and then etched with a mixture of an aqueous hydrogen fluoride solution and an aqueous nitric acid solution in any ratio to reveal the grain boundaries, as shown in the schematic diagram of Figure 4. Figure 4(a) is a perspective view of a cylindrical or rectangular ingot, Figure 4(b) is a schematic cross-sectional view of section I in Figure 4(a), Figure 4(c) is a schematic cross-sectional view of section II in Figure 4(a), and Figure 4(e) is a schematic cross-sectional view of section III in Figure 4(a).

[0155] The vicinity of the center of the ingot refers to the center position of the cross section (cross section II) at the midpoint between the top and bottom surfaces of the ingot, as shown in Figures 4(a) and 4(d). The vicinity of the surface layer of the side surface of the ingot refers to a position 10 mm deep from the surface of the side surface of the ingot, as shown in Figures 4(a) and 4(d). The vicinity of the center of the top of the ingot refers to a position 10 mm deep from the center of the top surface of the ingot (cross section I), as shown in Figures 4(a) and 4(c). The vicinity of the center of the bottom of the ingot refers to a position 10 mm deep from the center of the bottom surface of the ingot (cross section III), as shown in Figures 4(a) and 4(e). Samples are taken from each position. The top surface is the rear surface when viewed in the casting direction, and the bottom surface is the front surface when viewed in the casting direction.

[0156] Thereafter, the structure of the sample is observed and photographed using a digital camera, a microscope, an optical microscope, and a SEM (scanning electron microscope), and the average crystal grain size is calculated by the cutting method specified in JIS G 0551:2020. In order to determine the magnification of the photograph for observation, the structure of the sample is first observed at magnifications of 1x, 24x, 50x, 100x, 200x, 500x, and 1000x. The magnification at which an image containing 5 to 100 crystal grains in the observation field is obtained is adopted as the magnification for calculating the average crystal grain size. If an image containing 5 to 100 crystal grains is obtained at two or more magnifications, the observation result at the higher magnification is adopted. Note that if the crystal grain size is large and the photograph does not contain 5 or more crystal grains in the observation field even when photographed at 1x, the photograph taken at 1x magnification is adopted. At least five visual fields are surveyed for each sampling position, for a total of at least 20 visual fields. The average of the average grain sizes at each sampling position is defined as the "average grain size of the cast structure at each sample sampling position," and the average of the average grain sizes at all sampling positions is defined as the "average grain size of the entire cast structure" of this invention.

[0157] The average crystal grain size means the "average crystal grain size of the entire cast structure," and is desirably 90 μm or less.

[0158] The average grain size of the cast structure may vary significantly depending on the sampling position, but it is desirable that the ratio of the average grain size (average grain size of the cast structure at each sampling position) / (average grain size of the entire cast structure) be in the range of 0.70 to 1.40.

[0159] (Titanium compounds) The ingot of the present embodiment may contain a titanium compound in the cast structure. The titanium compounds that may be contained in the ingot of the present invention include carbides and titanium compounds other than carbides.

[0160] (carbide) In the present invention, it is desirable to eliminate all carbides in the second cooling step. If such carbides remain in the ingot, they may become the starting point of cracks in the subsequent hot working. The carbides are mainly TiC, but the type is not limited thereto. The carbides remaining in the ingot after the second cooling step can be almost completely eliminated by heating for hot working the slab or billet obtained from the ingot.

[0161] (Ti compounds other than carbides) Depending on the chemical composition of the ingot, Ti compounds other than carbides may be present in the ingot after the second cooling step of the present invention. For example, Ti2Cu, Ti2Ni, Ti3Al, TiAl, TiB, etc. As with carbides, these can also be the starting point of cracks in the subsequent hot working, so it is desirable to have fewer of them. Note that, if the chemical composition is within the range of 1 to 4 described above in (I), they can be almost completely eliminated by heating for hot working the slab or billet obtained from the ingot.

[0162] In the ingot of the present invention, the volume fraction of titanium compounds (carbides and titanium compounds other than carbides) is preferably 5 vol% or less, and the average particle size of the titanium compounds is preferably less than 1 μm.

[0163] The volume fraction and average particle size of the titanium compounds (carbides and titanium compounds other than carbides) can be measured by the following method.

[0164] For both the volume fraction and the average particle size, measurement and observation samples are taken from near the center of the ingot, near the surface layer of the side of the ingot, near the center of the top of the ingot, and near the center of the bottom of the ingot, as shown in the schematic diagram in Figure 4.

[0165] "Near the center of the ingot" refers to the center of the cross section at the midpoint between the top and bottom of the ingot. "Near the surface of the side of the ingot" refers to a position 10 mm deep from the surface of the side of the ingot. "Near the center of the top of the ingot" refers to a position 10 mm deep from the center of the top surface of the ingot. "Near the center of the bottom of the ingot" refers to a position 10 mm deep from the center of the bottom surface of the ingot. Samples are taken from each position. Note that the top surface is the rear surface when viewed in the casting direction, and the bottom surface is the front surface when viewed in the casting direction.

[0166] The volume fraction is calculated by measuring the diffraction peaks of carbides, Ti compounds other than carbides, and other phases by X-ray diffraction, and using the reference intensity ratio method. One measurement is taken at each sample collection position, for a total of four measurements, and the volume fraction at each measurement position is calculated. The volume fractions at all collection positions are averaged to determine the volume fraction of carbides and Ti compounds other than carbides in the ingot.

[0167] The average particle diameter is measured by mirror-polishing the cut surface of each sample, and then etching it with a mixture of an aqueous hydrogen fluoride solution and an aqueous nitric acid solution in an arbitrary ratio to reveal the grain boundaries. The etching time is 1 to 60 seconds. The structure is then observed and photographed using an optical microscope and a scanning electron microscope (SEM). The magnification for observation and photography is 50 to 1000 times. If the particles are spherical, the particle diameter is 0.5 μm or more, and if the particles are not spherical, the short axis length of the particles is 0.5 μm or more. The observation target is particles observed at these magnifications, and the magnification at which there are 1 to 30 particles in one field of view is adopted. The particle diameter is measured by comparing with the scale bar when observed at the adopted magnification, if the particles are spherical, and if the particles are not spherical, the short axis length of the particles is measured, and the particle diameter is taken as the particle diameter. At the adopted magnification, observation and particle diameter measurements are performed for 5 or more fields of view for each sampling position, and the average particle diameter at each sampling position is calculated. The average particle size of all the sampling positions is averaged to obtain the average particle size of the ingot.

[0168] (Effects of the Invention) (Reduction of segregation of C, Fe, Al, V, and Mo) The above mechanism makes it possible to obtain a cast structure with an average crystal grain size of 90 μm or less. In the process of refining the cast structure, it is possible to produce an ingot with reduced segregation of C, Fe, Al, V, Mo, etc. Segregation of these elements is divided into macrosegregation and microsegregation, but in the present invention, both types of segregation can be reduced.

[0169] The degree of macrosegregation and microsegregation is evaluated by the segregation ratio index. The segregation ratio index is calculated by the following formulas (a) to (e). The appropriate range of the following formulas varies depending on the chemical composition. In the case of chemical composition 1, the present invention is satisfied if formula (a) is 1.4 or less and formula (b) is 1.3 or less.

[0170] In the case of chemical composition 2, the present invention is satisfied if the formula (a) is 1.4 or less, the formula (b) is 1.3 or less, the formula (c) is 1.3 or less, and the formula (e) is 1.3 or less.

[0171] In the case of chemical composition 3, the present invention is satisfied if the formula (a) is 1.4 or less, the formula (b) is 1.3 or less, the formula (c) is 1.3 or less, the formula (d) is 1.3 or less, and the formula (e) is 1.3 or less.

[0172] In the case of chemical composition 4, the present invention is satisfied if the formula (a) is 1.4 or less, the formula (b) is 1.3 or less, the formula (c) is 1.3 or less, and the formula (e) is 1.3 or less.

[0173] [C] max / [C] ave … (a) [Fe] max / [Fe] ave … (b) [Al] max / [Al] ave … (c) [V] max / [V] ave … (d) [Mo] max / [Mo] ave … (e)

[0174] [C] max / [C] aveWhen this value is large, it means that there are areas with a high C content locally. In areas with a high C content locally, titanium carbide forms, and the titanium carbide may remain even after cooling. Titanium carbide is hard, and it is undesirable because scratches and cracks tend to occur at the areas where titanium carbide forms and in the surrounding area. Also, in areas with a high C content locally, even if titanium carbide does not form, the material hardens due to solid solution strengthening. Therefore, it is undesirable because scratches and cracks tend to occur at the areas with a high C content locally and in the surrounding area. Therefore, [C] max / [C] ave is preferably 1.4 or less.

[0175] [Fe] max / [Fe] ave , [Al] max / [Al] ave , [V] max / [V] ave , [Mo] max / [Mo] ave Similarly, in areas where these elements are locally abundant, the material becomes hard due to solid solution strengthening, and scratches and cracks tend to occur in the areas where these elements are locally abundant and in the surrounding areas, which is undesirable. max / [Fe] ave , [Al] max / [Al] ave , [V] max / [V] ave , [Mo] max / [Mo] ave are each preferably 1.3 or less.

[0176] In formulas (a) to (e), [C] ave , [Fe] ave , [Al] ave , [V] ave , [Mo] aveThe mean chemical composition (mass%) of C, Fe, Al, V, and Mo in the ingot are measured by common component analysis methods such as ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometer). The sample ring for measurement is taken from the bottom of the ingot after it has been cast and cooled. The analytical sample is the chips cut with a shaper or similar tool from a position 5mm or more deep from the casting surface at the bottom. This sample is dissolved in acid and analyzed by ICP-OES or similar tools.

[0177] [C] max , [Fe] max , [Al] max , [V] max , [Mo] max means the maximum concentration (mass%) of C, Fe, Al, V, and Mo in the ingot. These are measured by EPMA analysis (Electron Probe Micro Analyzer). Measurement samples for EPMA analysis are taken from near the center of the ingot, near the surface layer of the side of the ingot, near the center of the top of the ingot, and near the center of the bottom of the ingot, as shown in the schematic diagram of Figure 4.

[0178] "Near the center of the ingot" refers to the center of the cross section at the midpoint between the top and bottom of the ingot. "Near the surface of the side of the ingot" refers to a position 10 mm deep from the surface of the side of the ingot. "Near the center of the top of the ingot" refers to a position 10 mm deep from the center of the top surface of the ingot. "Near the center of the bottom of the ingot" refers to a position 10 mm deep from the center of the bottom surface of the ingot. Samples are taken from each position. Note that the top surface is the rear surface when viewed in the casting direction, and the bottom surface is the front surface when viewed in the casting direction.

[0179] Analyze at least 5 fields of view for each sample taken from each sampling location, for a total of 20 fields of view or more. The largest analytical value among the 20 analytical fields is taken as the maximum chemical composition, and each is [C] max , [Fe] max , [Al] max , [V] max , [Mo] maxThe measurement conditions for the EPMA analysis are not particularly limited, and an example is an acceleration voltage of 10 to 15 kV. In addition, in order to determine the magnification during analysis, first, observation is performed at magnifications of 50x, 100x, 200x, 500x, and 1000x. Then, the magnification at which an image containing 2 to 20 crystal particles in the observation field is obtained is adopted for the EPMA analysis. When 2 to 20 crystal particles are included at two or more magnifications, the observation result at the higher magnification is adopted. Before performing the EPMA analysis, the sample is observed at the same magnification as the magnification during analysis, and a field of view that does not contain compound particles is selected to perform the EPMA analysis.

[0180] (Reduction of hot working defects) Generally, the finer the structure, the more the hot working defects are suppressed. In the present invention, the finer the cast structure, the less defects there are during hot working such as blooming and forging. By reducing the defects during hot working, the occurrence of defects and cracks in the subsequent processes is suppressed, making it possible to manufacture high quality products.

[0181] The evaluation of hot working defects can be carried out by the following method. After the ingot is heated in the atmosphere, it is hot worked, and the front and back surfaces of the hot worked material are observed with the naked eye to evaluate the length and amount of defects. For example, if a defect with a length of 10 mm or more is confirmed, it is evaluated as failing, and if no defect is confirmed, it is evaluated as passing. The amount of defects can be evaluated as failing if the area ratio of the defect part on the front and back surfaces of the hot worked material exceeds 5%, and passing if it is 5% or less. The atmospheric heating conditions before hot working are not particularly limited, and may be performed under conditions such as a soaking temperature of 700 to 900 ° C and a holding time of 10 to 400 minutes. The hot working method is also not particularly limited, and may be performed under conditions such as a hot rolling reduction of 20 to 90% for an ingot with a thickness of 500 mm.

[0182] (Reduction of C content in ingot) In general, ingots are rarely used as structural parts as they are, and are often used after being processed into plates, bars, wire rods, and shapes. Depending on the application, it may be desirable to reduce the amount of carbon in the final product. In such cases, it is possible to produce hot-worked materials with a low carbon content from ingots having the above-mentioned cast structure by taking the following measures.

[0183] Specifically, the α case is formed on the surface layer by heating before and after the above-mentioned hot working, C is concentrated in the α case, and then the surface α case is removed by machining, pickling, or the like. Usually, the α case contains a lot of O due to the atmosphere, but in the present invention, the C in the material is affected by diffusing to the surface layer of the material, and the α case in the present invention is formed from not only O but also a high-C α phase. By removing the formed α case by cutting or pickling, it is possible to obtain a material with reduced macro-segregation and micro-segregation while suppressing the amount of C, and reduced hot working defects. The conditions for forming the α case are a soaking temperature of 700°C to 900°C and a holding time of 20 minutes to 400 minutes, so that a high-C α case can be formed on the surface layer of the material, and then removed by cutting or pickling. EXAMPLES

[0184] (Sample manufacturing conditions) Ingots having the chemical compositions shown in Tables 1A, 1B, 3A, 3B, 5A, 5B, 7A, and 7B were cast using an electron beam melting furnace, and 8 tons of ingots were produced by cooling at the cooling rates shown in Tables 2A, 2B, 4A, 4B, 6A, 6B, 8A, and 8B. The produced ingots were evaluated by the following method. The cooling rates shown in Tables 2A, 2B, 4A, 4B, 6A, 6B, 8A, and 8B are all average cooling rates. Regarding the evaluation of hot working defects, the produced ingots were forged and hot rolled to form 5 mm thick hot rolled sheets, which were then used for the evaluation.

[0185] In Tables 1A, 1B, 3A, 3B, 5A, 5B, 7A, and 7B, the notation "<0.001" indicates that the element is not intentionally contained. In addition, the formulas (a), (b), (c), (d), and (e) in Tables 2A, 2B, 4A, 4B, 6A, 6B, 8A, and 8B are as follows: [C] max / [C] ave … (a) [Fe] max / [Fe] ave … (b) [Al] max / [Al] ave … (c) [V] max / [V] ave … (d) [Mo] max / [Mo] ave … (e)

[0186] (Evaluation method) (Method for measuring average grain size of cast structure) To measure the average crystal grain size of the cast structure, samples were taken from near the center of the ingot, near the surface of the ingot, near the top of the ingot, and near the bottom of the ingot. The cut surfaces of each sample were mirror-polished, and then etched with a mixture of an aqueous hydrogen fluoride solution and an aqueous nitric acid solution in any ratio to reveal the grain boundaries. The structure of the sample was then observed and photographed using a digital camera, a microscope, an optical microscope, and an SEM (scanning electron microscope), and the average crystal grain size was calculated using the cutting method specified in JIS G 0551:2020. To determine the magnification of the photographs for observation, the structure of the sample was first observed at magnifications of 1x, 24x, 50x, 100x, 200x, 500x, and 1000x. The magnification at which an image containing 5 to 100 crystal grains in the observation field was obtained was adopted as the observation magnification for calculating the average crystal grain size. When images containing 5 to 100 crystal grains were obtained at two or more magnifications, the observation results at the higher magnification were used. Note that when the crystal grain size was large and the image was taken at 1x magnification, the photograph taken at 1x magnification was used when the observation field did not contain 5 or more crystal grains. At least 5 fields were taken for each sampling position, for a total of 20 fields or more, and the average of the average grain sizes at each sampling position was taken as the "average grain size of the cast structure at each sample sampling position," and the average of the average grain sizes at all sampling positions was taken as the "average grain size of the entire cast structure" of the present invention.

[0187] The case where the "average crystal grain size of the entire cast structure" exceeded 90 μm was evaluated as "x", and the case where the "average crystal grain size of the entire cast structure" was 90 μm or less was evaluated as "good".

[0188] The evaluation of carbides and Ti compounds other than carbides was carried out by the following method. For both the volume fraction and average grain size, measurement and observation samples were taken from near the center of the ingot, near the surface layer of the side of the ingot, near the center of the top of the ingot, and near the center of the bottom of the ingot. The volume fraction was calculated from the reference intensity ratio method using commercially available software, measuring the diffraction peaks of carbides, Ti compounds other than carbides, and other phases by X-ray diffraction. One measurement was taken at each sample collection position, for a total of four measurements, and the volume fraction of each phase was calculated at each measurement position.

[0189] When any of the volume fractions calculated at each sample collection position exceeded 5 vol%, it was evaluated as × (fail), and when it was 5 vol% or less at all sample collection positions, it was evaluated as ◯ (pass).

[0190] The average particle size was measured by mirror-polishing the cut surface of each sample, and then etching the sample with a mixture of an aqueous hydrogen fluoride solution and an aqueous nitric acid solution in an arbitrary ratio to reveal the grain boundaries. The etching time was 1 to 60 seconds. The structure of the sample was then observed with a digital camera, a microscope, an optical microscope, and a SEM (scanning electron microscope). In order to determine the magnification for the analysis, the sample was first observed at magnifications of 1x, 24x, 50x, 100x, 200x, 500x, and 1000x. If the particles were spherical, the particle diameter was 0.5 μm or more, and if the particles were not spherical, the particle diameter was 0.5 μm or more. The magnification at which an image containing 5 to 30 particles in the observation field was obtained was used to calculate the average particle size. The average particle size was determined by comparing the particle diameter with the scale bar when observed at the adopted magnification, if the particle was spherical, and the short axis length of the particle if the particle was not spherical. At the adopted magnification, observation and particle size measurement were performed for each sampling position, with 5 or more visual fields for a total of 20 or more visual fields, and the average particle size at each sampling position was calculated. Note that if the observation included 5 to 30 particles at two or more magnifications, the observation result at the higher magnification was used. At each sampling position, an average particle size of 1 μm or more was evaluated as × (fail), and an average particle size of less than 1 μm was evaluated as ◯ (pass).

[0191] The evaluation of hot working defects was carried out by the following method. The ingot was subjected to atmospheric heating and then hot working, and the front and back surfaces of the material after hot working were observed with the naked eye to evaluate the length and amount of defects. The length of the defects was evaluated as × (fail) if a defect of 10 mm or more was confirmed, and 〇 (pass) if no defect was confirmed. The amount of defects was evaluated as × (fail) if the area ratio of the defects on the front and back surfaces of the material after hot working exceeded 5%, and 〇 (pass) if it was 5% or less. The atmospheric heating conditions before hot working were a soaking temperature of 800°C and a holding time of 40 minutes. The hot working method involved hot rolling a forged material with a thickness of 100 mm with a total reduction of 95%.

[0192] [Table 1A]

[0193] [Table 1B]

[0194] [Table 2A]

[0195] [Table 2B]

[0196] [Table 3A]

[0197] [Table 3B]

[0198] [Table 4A]

[0199] [Table 4B]

[0200] [Table 5A]

[0201] [Table 5B]

[0202] [Table 6A]

[0203] [Table 6B]

[0204] [Table 7A]

[0205] [Table 7B]

[0206] [Table 8A]

[0207] [Table 8B]

[0208] As shown in Tables 1A to 8B, in the examples of the present invention, both the length and amount of flaws were rated as "◯," and the occurrence of surface flaws was successfully suppressed.

[0209] On the other hand, as shown in Tables 1A to 8B, in the comparative examples in which the chemical components were outside the range of the invention or the manufacturing conditions were outside the preferred range, at least one of the length and amount of scratches was marked as "X," and the occurrence of surface scratches could not be suppressed.

Claims

1. In mass percent, C: 0.100-0.900%, Al: 0-7.000%, Mo: 0-7.000%, V: 0-6.000%, Zr: 0-5.000%, Sn: 0-3.000%, Fe: 0-2.100%, Si: 0 to 0.500%, Cr: 0-0.400%, Ni: 0 to 0.400%, Ta: 0-0.400%, Nb: 0 to 0.400%, Mn: 0 to 0.200%, Ru: 0-0.100%, Pd: 0 to 0.100%, Cu: 0-0.200%, B: 0 to 0.090%, Hf: 0 to 0.090%, O: 0.400% or less, N: 0.300% or less, S: 0.110% or less, P: 0.110% or less, H: 0.035% or less, The balance is composed of Ti and impurities. An ingot having an average grain size of 90 μm or less in a cast structure.

2. By mass% C: 0.100-0.450%, Fe: 0.010-0.450%, H: 0.015% or less, O: 0.400% or less, N: 0.300% or less, S: 0.030% or less, P: 0.030% or less, Si: 0.500% or less, Mo: 0 to 1.900%, Al: 0-0.400%, Ta: 0-0.200%, Nb: 0 to 0.090%, Ru: 0-0.100%, Pd: 0 to 0.100%, Ni: 0-0.200% One or more of Mn, Cu, Cr, Sn, and Zr: 0 to 0.200% in total, The balance is composed of Ti and impurities. An ingot having an average grain size of 90 μm or less in a cast structure.

3. 3. The ingot according to claim 2, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less.

4. 3. The ingot according to claim 2, wherein the average particle size of the titanium compound remaining in the ingot is less than 1 μm.

5. 3. The ingot according to claim 2, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less, and an average particle size of the titanium compound is less than 1 μm.

6. The ingot according to any one of claims 2 to 5, which satisfies either one or both of the following formula (1) and the following formula (2): [C] max / [C] ave ≦1.4 … (1) [Fe] max / [Fe] ave ≦1.3 … (2) In the formulas (1) and (2), [C] max [Fe] max are the maximum concentrations (mass%) of C and Fe in the ingot. ave [Fe] ave are the average chemical compositions (mass%) of C and Fe in the ingot, respectively.

7. By mass% C: 0.310-0.900%, Al: 4.500% to 6.500%, Fe: 0.500% to 2.100%, N: 0.050% or less, O: 0.250% or less, Si: 0 to 0.500%, Mo: 0-7.000%, Cr: 0-0.400%, Cu: 0 to 0.090%, Ni: 0 to 0.400%, Hf: 0 to 0.090%, B: 0 to 0.090%, Nb: 0 to 0.400%, Ta: 0-0.400%, Sn: 0-1.900%, Zr: 0 to 0.400%, Ru: 0-0.100%, Pd: 0-0.100% S: 0.080% or less, P: 0.080% or less, H: 0.025% or less, The balance is Ti and impurities. An ingot having an average grain size of 90 μm or less in its cast structure.

8. By mass% C: 0.310-0.900%, Al: 2.000% to 7.000%, V: 1.500-6.000%, Fe: 0.500% or less, N: 0.050% or less O: 0.250% or less Si: 0 to 0.500%, Mo: 0-7.00%, Cr: 0-0.400%, Cu: 0 to 0.090%, Ni: 0 to 0.400%, Hf: 0 to 0.090%, B: 0 to 0.090%, Nb: 0 to 0.400%, Ta: 0-0.400%, Sn: 0-1.900%, Zr: 0 to 0.400%, Ru: 0-0.100%, Pd: 0-0.100% S: 0.110% or less, P: 0.110% or less, H: 0.030% or less, The balance is composed of Ti and impurities. An ingot having an average grain size of 90 μm or less in its cast structure.

9. By mass% C: 0.310-0.900%, Al: 5.000% to 7.000%, Mo: 1.000% to 7.000%, Zr: 3.000% to 5.000%, Sn: 1.000% to 3.000%, Si: 0% to 0.500%, Fe: 0.500% or less, N: 0.050% or less O: 0.250% or less Cr: 0-0.400%, Cu: 0 to 0.090%, Ni: 0-0.400%, Hf: 0 to 0.090%, B: 0 to 0.090%, Nb: 0 to 0.400%, Ta: 0-0.400%, Ru: 0-0.100%, Pd: 0-0.100% S: 0.110% or less, P: 0.110% or less, H: 0.035% or less, The balance is composed of Ti and impurities. An ingot having an average grain size of 90 μm or less in its cast structure.

10. 8. The ingot according to claim 7, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less.

11. 9. The ingot according to claim 8, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less.

12. 10. The ingot according to claim 9, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less.

13. 8. The ingot according to claim 7, wherein the average particle size of the titanium compound remaining in the ingot is less than 1 μm.

14. 9. The ingot according to claim 8, wherein the average particle size of the titanium compound remaining in the ingot is less than 1 μm.

15. 10. The ingot according to claim 9, wherein the average particle size of the titanium compound remaining in the ingot is less than 1 μm.

16. 8. The ingot according to claim 7, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less, and an average particle size of the titanium compound is less than 1 μm.

17. 9. The ingot according to claim 8, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less, and an average particle size of the titanium compound is less than 1 μm.

18. 10. The ingot according to claim 9, wherein a volume fraction of the titanium compound remaining in the ingot is 5 vol % or less, and an average particle size of the titanium compound is less than 1 μm.

19. The ingot according to any one of claims 7, 9, 10, 12, 13, 15, 16, and 18, which satisfies any one or more of the following formulas (3) to (6): [C] max / [C] ave ≦1.4 … (3) [Fe] max / [Fe] ave ≦1.3 … (4) <h2 style=";text-align:left;direction:ltr">[Al]<h2 style=";text-align:left;direction:ltr"> max <h2 style=";text-align:left;direction:ltr"> / [Al]<h2 style=";text-align:left;direction:ltr"> ave <h2 style=";text-align:left;direction:ltr"> ≦1533 … (5) [Mo] max / [Mo] ave ≦1.3 … (6) However, in formulas (3) to (6), [C] max [Fe] max [Al] max , [Mo] max are the maximum concentrations (mass%) of C, Fe, Al, and Mo in the ingot. ave [Fe] ave [Al] ave , [Mo] ave are the average chemical compositions (mass%) of C, Fe, Al, and Mo in the ingot, respectively.

20. The ingot according to any one of claims 8, 11, 14, and 17, which satisfies any one or more of the following formulas (3) to (7): [C] max / [C] ave ≦1.4 … (3) [Fe] max / [Fe] ave ≦1.3 … (4) <h2 style=";text-align:left;direction:ltr">[Al]<h2 style=";text-align:left;direction:ltr"> max <h2 style=";text-align:left;direction:ltr"> / [Al]<h2 style=";text-align:left;direction:ltr"> ave <h2 style=";text-align:left;direction:ltr"> ≦1533 … (5) [Mo] max / [Mo] ave ≦1.3 … (6) [V] max / [V] ave ≦1.3 … (7) In the formulas (3) to (7), [C] max [Fe] max [Al] max , [Mo] max , [V] max are the maximum concentrations (mass%) of C, Fe, Al, Mo, and V in the ingot. ave [Fe] ave [Al] ave , [Mo] ave , [V] ave are the average chemical compositions (mass%) of C, Fe, Al, Mo, and V in the ingot, respectively.

Citation Information

Patent Citations

  • Method and apparatus for producing titanium ingot

    JP2020121331A

  • Titanium alloy and production method therefor

    WO2019198147A1

Cited By

  • Titanium alloy plate and preparation method thereof

    CN120366616A

  • Titanium alloy plate and preparation method thereof

    CN120366616B