Copolymer and method for producing the same
A controlled copolymerization method using specific compounds and initiators achieves precise molecular weight and distribution in α-exomethylene lactone copolymers, resulting in improved heat and solvent resistance.
Patent Information
- Application Number
- JP2023070324
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
AI Technical Summary
The precise control of molecular weight and molecular weight distribution in copolymers containing repeating units derived from α-exomethylene lactone has not been adequately addressed, leading to challenges in achieving controlled polymerization with acyclic (meth)acrylates.
A copolymerization method using a specific combination of compounds represented by formulas (3) and (4), an anionic polymerization initiator, and an organoaluminum compound under controlled conditions to achieve precise control of molecular weight and distribution.
The method enables the production of copolymers with high number average molecular weights and narrow molecular weight distributions, enhancing properties such as heat resistance and solvent resistance.
Smart Images

Figure 2024155533000001 
Figure 2024155533000002 
Figure 2024155533000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a copolymer and a method for producing the same, and more particularly to a copolymer containing a repeating unit derived from an α-exomethylene lactone compound and a method for producing the same. [Background technology]
[0002] Copolymerization of acyclic (meth)acrylate with α-exomethylene lactone results in a polymer with superior heat resistance, solvent resistance, mechanical properties, etc., compared to homopolymers, and therefore various studies have been conducted. Patent Document 1 discloses that a copolymer containing a repeating unit derived from α-methylene-γ-butyrolactone has been obtained by copolymerization of α-methylene-γ-butyrolactone with methyl methacrylate, or copolymerization of α-methylene-γ-butyrolactone with methyl methacrylate and benzyl methacrylate. α-Methylene-γ-butyrolactone is a polymerizable monomer obtained from raw materials derived from plants, and has attracted attention because it can contribute to a carbon-circulating society. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-83035 Summary of the Invention [Problem to be solved by the invention]
[0004] It is known that the molecular weight and molecular weight distribution of a polymer are closely related to the physical properties of the polymer. However, in copolymers containing repeating units derived from α-exomethylene lactone, precise control of the molecular weight and molecular weight distribution has not yet been fully investigated.
[0005] Specifically, the acrylic skeleton of α-exomethylene lactone is more reactive than acyclic (meth)acrylates such as methyl methacrylate due to ring distortion and the acrylic skeleton fixed in s-cis conformation. For this reason, in the copolymerization of α-exomethylene lactone and acyclic (meth)acrylate, the difference in the reactivity of the monomers becomes a challenge in controlling the polymerization. For example, homopolymers with controlled molecular weight and narrow molecular weight distribution have been synthesized by group transfer polymerization of α-methylene-γ-butyrolactone. However, in the copolymerization with methyl methacrylate, only block copolymerization in which methyl methacrylate was polymerized first was successful, and conversely, when α-methylene-γ-butyrolactone was polymerized first, it did not lead to the polymerization of methyl methacrylate, and only homopolymers of α-methylene-γ-butyrolactone were obtained. In other words, it is not possible to induce a cross-propagation reaction to methyl methacrylate from a growing species having a unit derived from α-methylene-γ-butyrolactone as a terminal group. This means that random copolymers of α-methylene-γ-butyrolactone and methyl methacrylate cannot be obtained by group transfer polymerization. In addition, precise copolymerization of α-exomethylene lactone and acrylate has not been reported. Therefore, it is necessary to develop a technology to precisely control the molecular weight and molecular weight distribution of copolymers of α-exomethylene lactone and (meth)acrylate, and to provide polymers with a moderately high molecular weight and a sufficiently narrow molecular weight distribution.
[0006] The present invention has been made in consideration of the above-mentioned problems, and a main object of the present invention is to provide a method for producing a copolymer that contains a repeating unit derived from an α-exomethylene lactone compound and that can provide a copolymer having a precisely controlled molecular weight and molecular weight distribution. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides the following production method for a copolymer and the copolymer.
[0008] A method for producing a copolymer, comprising polymerizing a monomer containing a compound represented by the following formula (3) and a compound represented by the following formula (4) in the presence of a compound represented by the following formula (5) and an anionic polymerization initiator: [ka] (In formula (3), R 10 is a hydrogen atom or a methyl group. 1 represents a hydrocarbyl group having 1 to 20 carbon atoms, which may be substituted with a heteroatom-containing group having at least one element selected from the group consisting of nitrogen, oxygen, sulfur, and halogen. 2 represents a divalent linking group. [ka] (In formula (5), Ar 1 represents a monovalent group in which a benzene ring is bonded to the oxygen atom in the formula, a secondary carbon or a tertiary carbon is bonded to the 2-position and the 6-position carbon of the benzene ring, and a hydrogen atom, a chlorine atom, a fluorine atom, a hydrocarbyl group having 1 to 6 carbon atoms, or a hydrocarbyloxy group having 1 to 6 carbon atoms is bonded to the 4-position carbon. 3 represents an alkyl group having 2 to 10 carbon atoms.
[0009] A copolymer having a repeating unit derived from the compound represented by the above formula (3) and a repeating unit derived from the compound represented by the above formula (4), and having a structure derived from a conjugated acid having an acidity constant (pKa) of 5 or less at its terminal. Effect of the Invention
[0010] According to the present invention, it is possible to provide a copolymer containing a repeating unit derived from an α-exomethylene lactone compound, the molecular weight and molecular weight distribution of which are precisely controlled. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Matters related to the embodiments of the present disclosure will be described in detail below. In this specification, a numerical range described using "~" means that the numerical range described before and after "~" includes the lower limit and upper limit. Unless otherwise specified, each component may be used alone or in combination of two or more types. In this specification, "(meth)acrylic" is a term that includes "acrylic" and "methacrylic".
[0012] <Method for producing copolymer> The production method for the copolymer of the present disclosure (hereinafter also referred to as "the production method") includes a step of polymerizing a monomer (hereinafter also referred to as "α-methylene lactone compound") containing a compound represented by the following formula (3) (hereinafter also referred to as "(meth)acrylic acid ester compound") and a compound represented by the following formula (4) in the presence of a compound represented by the following formula (5) (hereinafter also referred to as "organoaluminum compound") and an anionic polymerization initiator. [ka] (In formula (3), R 10 is a hydrogen atom or a methyl group. 1 represents a hydrocarbyl group having 1 to 20 carbon atoms, which may be substituted with a heteroatom-containing group having at least one element selected from the group consisting of nitrogen, oxygen, sulfur, and halogen. 2 represents a divalent linking group. [ka] (In formula (5), Ar 1 represents a monovalent group in which a benzene ring is bonded to the oxygen atom in the formula, a secondary carbon or a tertiary carbon is bonded to the 2-position and the 6-position carbon of the benzene ring, and a hydrogen atom, a chlorine atom, a fluorine atom, a hydrocarbyl group having 1 to 6 carbon atoms, or a hydrocarbyloxy group having 1 to 6 carbon atoms is bonded to the 4-position carbon. 3 represents an alkyl group having 2 to 10 carbon atoms.
[0013] <Monomer> (Meth)acrylic acid ester compounds In the above formula (3), R 10 From the viewpoint of copolymerizability, R is preferably a hydrogen atom. 1 Examples of the hydrocarbyl group having 1 to 20 carbon atoms represented by the formula (1) include a monovalent saturated or unsaturated chain hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms. In this specification, the alicyclic hydrocarbon group is not limited to being composed only of an alicyclic hydrocarbon structure, and may have a chain structure as part of it. In addition, the aromatic hydrocarbon group is not limited to being composed only of an aromatic ring structure, and may have a chain structure or an alicyclic hydrocarbon structure as part of it.
[0014] R 1 may have any hydrogen atom of the hydrocarbyl group having 1 to 20 carbon atoms substituted with a hetero element-containing group having at least one element selected from the group consisting of nitrogen, oxygen, sulfur, and halogen (hereinafter, simply referred to as a "hetero element-containing group"). Examples of the hetero element-containing group include an oxetanyl group, an oxiranyl group, an amino group, a thiol group, a hydroxyl group, and a halo group (such as a fluoro group, a chloro group, a bromo group, and an iodo group).
[0015] R 1 From the viewpoint of copolymerizability with the α-methylene lactone compound, R is preferably an alkyl group having 1 to 20 carbon atoms which may be substituted with a heteroatom-containing group. From the viewpoint of increasing the reaction rate of the monomer and obtaining a copolymer having a narrower ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn, hereinafter also referred to as "molecular weight distribution"), R 1 R is preferably a substituted or unsubstituted alkyl group having 2 or more carbon atoms, more preferably a substituted or unsubstituted alkyl group having 4 or more carbon atoms, and further preferably a substituted or unsubstituted alkyl group having 8 or more carbon atoms. 1 The alkyl group represented by the formula (I) may be linear or branched.
[0016] Specific examples of the (meth)acrylic acid ester compound represented by the above formula (3) include (meth)acrylic acid alkyl esters, (meth)acrylic acid esters having an alicyclic structure, and (meth)acrylic acid esters having an aromatic ring structure, and the hydrogen atoms of these compounds may be substituted with hetero element-containing groups.
[0017] Further specific examples of the (meth)acrylic acid ester compound represented by the above formula (3) include (meth)acrylic acid alkyl esters which may be substituted with a heteroatom-containing group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-stearyl (meth)acrylate, glycidyl (meth)acrylate, hydroxyethyl (meth)acrylate, 2-dimethylaminoethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 2-bromoethyl (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, and perfluoroethyl (meth)acrylate.
[0018] Examples of the (meth)acrylic acid ester having an alicyclic structure which may be substituted with a heteroatom-containing group include cyclohexyl (meth)acrylate, 2-methylcyclohexyl (meth)acrylate, tricyclo[5.2.1.0](meth)acrylate, and the like. 2,6 ]decan-8-yl, (meth)acrylic acid tricyclo[5.2.1.0 2,5 ]Decan-8-yloxyethyl, isobornyl (meth)acrylate, adamantyl (meth)acrylate, (perfluorocyclohexyl)methyl (meth)acrylate, and (3,4-epoxycyclohexyl)methyl (meth)acrylate. Examples of the (meth)acrylic acid ester having an aromatic ring structure which may be substituted with a heteroatom-containing group include phenyl (meth)acrylate, benzyl (meth)acrylate, and pentafluorophenyl (meth)acrylate.
[0019] Among the above, the (meth)acrylic acid ester compound is preferably an alkyl group having 1 to 20 carbon atoms which may be substituted with a hetero element-containing group, in that the effect of improving heat resistance, solvent resistance, mechanical properties, etc. by introducing a repeating unit derived from an α-methylene lactone compound into a polymer is greater, and a (meth)acrylic acid alkyl ester (i.e., R 1 is an alkyl group), and 1 More preferred are compounds in which is a straight-chain alkyl group.
[0020] α-Methylene lactone compounds In the above formula (4), R 2 Examples of the divalent linking group represented by the formula (I) include a hydrocarbylene group having 2 to 5 carbon atoms and a divalent group in which any methylene group in the hydrocarbylene group is replaced by -O-, -CO-, -COO-, etc. 2 The hydrocarbylene group having 2 to 5 carbon atoms preferably has a chain structure, and more preferably is a linear or branched alkanediyl group having 2 to 5 carbon atoms.
[0021] R in the above formula (4) 2 Among these, an alkanediyl group having 2 to 5 carbon atoms and a divalent group in which any methylene group in the alkanediyl group is replaced by -O-, -CO-, -COO-, etc. are preferred. 1 -O-CO-R 11 -(However, R 11 is an alkanediyl group having 1 to 4 carbon atoms, and "* 1" represents a bond to the vinyl group side in formula (4). ) is more preferred, and a hydrocarbylene group having 2 to 5 carbon atoms is even more preferred. From the viewpoint of availability of raw materials and copolymerizability with the (meth)acrylic acid ester compound represented by the above formula (3), R 2 Among these, alkanediyl groups having 2 to 4 carbon atoms are preferred, and those having 2 or 3 carbon atoms are particularly preferred.
[0022] Specific examples of the compound represented by the above formula (4) include α-methylene-γ-butyrolactone, α-methylene-δ-valerolactone, [ka] and the like.
[0023] The molar ratio of the (meth)acrylic acid ester compound to the α-methylene lactone compound used in the polymerization is preferably 50 / 50 to 99 / 1 ((meth)acrylic acid ester compound / α-methylene lactone compound). From the viewpoint of precisely controlling the molecular weight and molecular weight distribution with high accuracy while sufficiently imparting the performance derived from the α-methylene lactone compound to the polymer, the molar ratio of the (meth)acrylic acid ester compound to the α-methylene lactone compound is more preferably 55 / 45 to 99 / 1, even more preferably 60 / 40 to 99 / 1, and even more preferably 60 / 40 to 95 / 5.
[0024] In the polymerization, a monomer different from the (meth)acrylic acid ester compound and the α-methylene lactone compound may be used in combination within a range that does not impair the effects of the present disclosure. Specific examples of the monomer include alkyl methacrylate, hydroxyalkyl (meth)acrylate, styrene, ethylene, propylene, 1,3-butadiene, isoprene, and acrylonitrile.
[0025] Of the monomers used in the polymerization, the total amount of the (meth)acrylic acid ester compound and the α-methylene lactone compound used is preferably 80 mol % or more, more preferably 85 mol % or more, even more preferably 90 mol % or more, and still more preferably 95 mol % or more, from the viewpoint of improving controllability of the molecular weight and molecular weight distribution.
[0026] In the polymerization system of the (meth)acrylic acid ester compound and the α-methylene lactone compound according to the present disclosure, it is believed that the polymerization reaction (anionic polymerization) proceeds by the organoaluminum compound used together with the anionic polymerization initiator functioning as a Lewis acid. The organoaluminum compound and the anionic polymerization initiator used in the present production method will be described below.
[0027] <Organoaluminum compounds> The organoaluminum compound is not particularly limited as long as it functions as a co-catalyst. 1 The carbon atoms at the 2-position and 6-position of the benzene ring of the monovalent group represented by the formula: 1 A group having a secondary carbon or a tertiary carbon (hereinafter also referred to as a "specific carbon-containing group") is bonded to the 2-position and the 6-position of the benzene ring of the monovalent group represented by the following formula: 1 The specific carbon-containing groups bonded to the 2-position and the 6-position of the benzene ring of the monovalent group represented by the formula (1) may be the same or different. For example, the specific carbon-containing group bonded to the 2-position of the benzene ring may be a group having a secondary carbon, and the specific carbon-containing group bonded to the 6-position may be a group having a tertiary carbon.
[0028] The specific carbon-containing group is preferably a hydrocarbyl group (more specifically, a hydrocarbyl group having a secondary or tertiary carbon and bonded to a benzene ring via the secondary or tertiary carbon), and specific examples thereof include a monovalent chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Of these, the specific carbon-containing group is preferably a monovalent chain hydrocarbon group, and more preferably a secondary alkyl group or a tertiary alkyl group. Specific examples of preferred specific carbon-containing groups include an isopropyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group.
[0029] In this context, a "secondary carbon" refers to a carbon that is bonded to two hydrocarbon groups, excluding the bond to the benzene ring. A "tertiary carbon" refers to a carbon that is bonded to three hydrocarbon groups, excluding the bond to the benzene ring.
[0030] Ar 1 A hydrogen atom, a chlorine atom, a fluorine atom, a hydrocarbyl group having 1 to 6 carbon atoms, or a hydrocarbyloxy group having 1 to 6 carbon atoms is bonded to the carbon atom at the 4-position of the benzene ring of the monovalent group represented by the following formula: The hydrocarbyl group having 1 to 6 carbon atoms and the hydrocarbyl group in the hydrocarbyloxy group having 1 to 6 carbon atoms include a chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Of these, a chain hydrocarbon group is preferred, and an alkyl group is more preferred.
[0031] R 3 The alkyl group having 2 to 10 carbon atoms represented by the formula (I) may be linear or branched. 3 Specific examples of the aryl group include an ethyl group, an n-propyl group, an isopropyl group, a sec-propyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a 1,1-dimethylbutyl group, an n-pentyl group, an isopentyl group, an n-hexyl group, an isohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.
[0032] A preferred example of the organoaluminum compound is a compound represented by the following formula (5A). [ka] (In formula (5A), R 4 and R 5 R each independently represents a hydrocarbyl group having a secondary or tertiary carbon and bonded to the benzene ring at the secondary or tertiary carbon. 6 R represents a hydrogen atom, a chlorine atom, a fluorine atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. 3 represents an alkyl group having 2 to 10 carbon atoms.
[0033] R 4 and R 5 is preferably a hydrocarbyl group having a tertiary carbon and bonded to a benzene ring at the tertiary carbon, and more preferably an alkyl group having a tertiary carbon and bonded to a benzene ring at the tertiary carbon.
[0034] Specific examples of the organoaluminum compound used in the polymerization include compounds represented by the following formulas (5-1) to (5-8), in which "Et" represents an ethyl group, "iBu" represents an isobutyl group, and "Oc" represents an n-octyl group. [ka]
[0035] In the above polymerization, the amount of the organoaluminum compound used is preferably 0.01 to 10 parts by mole, and more preferably 0.1 to 5 parts by mole, based on 100 parts by mole of the total of the monomers used in the polymerization.
[0036] <Anionic polymerization initiator> As the anionic polymerization initiator, from the viewpoint of sufficiently proceeding with the polymerization reaction between a (meth)acrylic acid ester compound and an α-methylene lactone compound, a salt of an anion of a conjugate acid having an acidity constant (pKa) of 5 or less and an ammonium cation can be preferably used. The acidity constant (pKa) of the anion of the conjugate acid of the anionic polymerization initiator is, for example, 2 or more, and preferably 2.5 or more.
[0037] Specific examples of the anion of the conjugate acid of the anionic polymerization initiator include a carboxylate ion, an azide ion, a 2,4-dinitrophenol ion, etc. From the viewpoint of easy availability of the anionic polymerization initiator, the anion of the conjugate acid of the anionic polymerization initiator is preferably a carboxylate ion or an azide ion, and more preferably a carboxylate ion.
[0038] When the anionic polymerization initiator is a salt of a carboxylate ion and an ammonium cation (hereinafter also referred to as a "carboxylate compound"), the carboxylate compound may be any compound that can function as a polymerization initiator by generating a carboxylate ion in the polymerization system.
[0039] The carboxylate compound is "R 7 COO - N(R 8 )4 + " (wherein R 7 and R 8 Each R independently represents a hydrocarbyl group having 1 to 20 carbon atoms. 8 are the same or different.) Carboxylic acids (R 7 Examples of the carboxylic acid having a substituent group "R -COOH" include aliphatic carboxylic acids and aromatic carboxylic acids. Specific examples of the carboxylic acid include saturated fatty acids such as acetic acid, propionic acid, butyric acid, isobutyric acid, pivalic acid, valeric acid, caproic acid, enanthic acid, caprylic acid, lauric acid, myristic acid, and stearic acid as aliphatic carboxylic acids; unsaturated fatty acids such as oleic acid, linoleic acid, arachidonic acid, eicosapentaenoic acid, and docosahexaenoic acid as aliphatic carboxylic acids. Examples of the aromatic carboxylic acid include benzoic acid and phthalic acid. Of these, saturated fatty acids and aromatic carboxylic acids are preferred, and "R 7a -COOH" (where R 7a is a linear or branched alkyl group having 1 to 12 carbon atoms or a phenyl group.) is more preferable.
[0040] Ammonium (N(R 8 )4 + ) for R 8 is preferably a linear or branched alkyl group having 1 to 12 carbon atoms or a phenyl group. Specific examples of ammonium include tetramethylammonium, tetraethylammonium, diethyldimethylammonium, tetrapropylammonium, tetrabutylammonium, tetrapentylammonium, tetrahexylammonium, tetraheptylammonium, tetraoctylammonium, tetradecylammonium, and tetradodecylammonium.
[0041] Specific examples of the carboxylate compound include compounds obtained by combining any of the carboxy anions derived from the above-mentioned carboxylic acids with ammonium. Examples of such compounds include the compounds represented by the following formulas (6-1) to (6-6). [ka]
[0042] In the above polymerization, the amount of the anionic polymerization initiator used is preferably 0.01 to 10 parts by mole, and more preferably 0.1 to 5 parts by mole, based on 100 parts by mole of the total of the monomers used in the polymerization.
[0043] The polymerization method used in the present production method is not particularly limited, and examples thereof include solution polymerization, suspension polymerization, emulsion polymerization, gas phase polymerization, and bulk polymerization. Among these, solution polymerization is preferred. The polymerization method may be either batch or continuous. In the case of solution polymerization, examples of the organic solvent used in polymerization include hydrocarbons, and specific examples thereof include toluene, xylene, cyclohexane, and methylcyclohexane. Among these, toluene is preferred as the organic solvent used in polymerization. The organic solvent used may be one type or a mixed solvent of two or more types. From the viewpoint of maintaining a balance between productivity and ease of polymerization control, the amount of the organic solvent used is preferably 200 to 3,000 parts by mass per 100 parts by mass of the total of the monomers used in polymerization.
[0044] The polymerization temperature is preferably within the range of -30°C to 50°C, more preferably within the range of -20°C to 40°C, and even more preferably within the range of -10°C to 20°C. In this production method, even when the polymerization temperature is set to a relatively high temperature of -10°C to 20°C, a (meth)acrylic acid ester compound / α-methylene lactone compound copolymer having a number average molecular weight (Mn) of 20,000 or more and a molecular weight distribution (Mw / Mn) of 1.0 to 3.0 can be obtained. From the viewpoint of performing polymerization under as mild conditions as possible while precisely controlling the molecular weight and molecular weight distribution, the polymerization temperature is preferably -7°C or more, more preferably -5°C or more. In addition, from the viewpoint of suppressing side reactions, the polymerization temperature is preferably 15°C or less, more preferably 10°C or less. The polymerization reaction is preferably performed under a pressure sufficient to substantially keep the monomer in a liquid phase.
[0045] According to the present production method described above, the copolymer of the present disclosure, that is, a copolymer having a repeating unit derived from the compound represented by the above formula (3) (hereinafter also referred to as "repeating unit (U1)") and a repeating unit derived from the compound represented by the above formula (4) (hereinafter also referred to as "repeating unit (U2)") and having a structure derived from a conjugated acid having an acidity constant (pKa) of 5 or less at its terminal, can be obtained by a polymerization reaction under relatively mild temperature conditions. The copolymer obtained by the present production method is preferably a random copolymer of the repeating unit (U1) and the repeating unit (U2).
[0046] The content of the repeating unit (U1) in the copolymer of the present disclosure is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more, based on the total amount of repeating units constituting the copolymer, from the viewpoint of improving control of molecular weight characteristics. In addition, from the viewpoint of improving the heat resistance, solvent resistance, mechanical properties, etc. of the polymer by introducing a sufficient amount of repeating unit (U2) into the copolymer, and from the viewpoint of improving the usefulness as a biomass-derived polymer, the content of the repeating unit (U1) is preferably 99 mol% or less, more preferably 95 mol% or less, and even more preferably 90 mol% or less, based on the total amount of repeating units constituting the copolymer. In this specification, the "repeating unit" refers to a monomer unit that mainly constitutes the main chain structure of the polymer, and is a unit that is contained in multiple units in one molecule.
[0047] The content of the repeating unit (U2) in the copolymer of the present disclosure is preferably 1 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more, based on the total amount of repeating units constituting the copolymer, from the viewpoint of introducing a sufficient amount of the repeating unit (U2) into the copolymer to improve the heat resistance, solvent resistance, mechanical properties, etc. of the polymer, and from the viewpoint of improving the usefulness as a biomass-derived polymer. Moreover, the content of the repeating unit (U2) is preferably 50 mol% or less, more preferably 40 mol% or less, and even more preferably 30 mol% or less, based on the total amount of repeating units constituting the copolymer, from the viewpoint of introducing a sufficient amount of the repeating unit (U2) into the copolymer while improving the controllability of the molecular weight properties of the polymer.
[0048] In the copolymer of the present disclosure, the total amount of the repeating units (U1) and (U2) is preferably 80 mol % or more, more preferably 85 mol % or more, even more preferably 90 mol % or more, and still more preferably 95 mol % or more, based on the total amount of repeating units constituting the copolymer.
[0049] The number average molecular weight (Mn) of the copolymer of the present disclosure is preferably 20,000 or more. When the number average molecular weight (Mn) is 20,000 or more, the polymer tends to have better strength, heat resistance, and processability. The number average molecular weight (Mn) of the copolymer of the present disclosure is preferably 22,000 or more, and more preferably 25,000 or more. In addition, the number average molecular weight (Mn) of the copolymer of the present disclosure is preferably 3,000,000 or less, and more preferably 2,000,000 or less, from the viewpoint of improving fluidity, processability, and flexibility. In this specification, the molecular weight of the polymer (including the copolymer) is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).
[0050] The molecular weight distribution (Mw / Mn) of the copolymer of the present disclosure is preferably 1.0 to 3.0. From the viewpoint of controlling the molecular weight distribution at a higher level, the molecular weight distribution (Mw / Mn) is preferably 2.7 or less, more preferably 2.5 or less, even more preferably 2.3 or less, even more preferably 2.0 or less, and even more preferably 1.9 or less.
[0051] The copolymer of the present disclosure and the copolymer obtained by the present production method described above are expected to exhibit a high refractive index and have excellent transparency, heat resistance, and solvent resistance due to the inclusion of a repeating unit derived from α-exomethylene lactone. In addition, the α-exomethylene lactone compound used in the polymerization is a polymerizable monomer that can be obtained from a raw material derived from a plant. Therefore, the copolymer of the present disclosure and the copolymer obtained by the present production method are expected to contribute to a carbon-circulating society and to be applied to a wide range of applications, such as optical components, electrical devices, automotive components, building components, and medical instruments.
[0052] According to the present disclosure described above, the following means are provided. [Means 1] A method for producing a copolymer, comprising polymerizing a monomer containing a compound represented by the above formula (3) and a compound represented by the above formula (4) in the presence of a compound represented by the above formula (5) and an anionic polymerization initiator. [Means 2] The method for producing a copolymer according to [Means 1], wherein the anionic polymerization initiator is a salt of an anion of a conjugate acid having an acidity constant (pKa) of 5 or less and an ammonium cation. [Means 3] The method for producing a copolymer according to [Means 1] or [Means 2], wherein the anion of the conjugate acid is a carboxylate ion, an azide ion or a 2,4-dinitrophenol ion. [Means 4] The method for producing a copolymer according to any one of [Means 1] to [Means 3], wherein the polymerization temperature is from -10 to 20°C. [Means 5] The method for producing the copolymer according to any one of [Means 1] to [Means 4], wherein the monomers are polymerized in an organic solvent. [Means 6] R in the above formula (3) 1is an alkyl group having 1 to 20 carbon atoms which may be substituted with the hetero element-containing group. [Means 7] R in the above formula (4) 2 is an alkanediyl group having 2 to 5 carbon atoms or 1 -O-CO-R 11 -(However, R 11 is an alkanediyl group having 1 to 4 carbon atoms, and "* 1 " represents a bond to the vinyl group in formula (4). The method for producing a copolymer according to any one of [Means 1] to [Means 6] above. [Means 8] The method for producing a copolymer according to any one of [Means 1] to [Means 7], wherein the use ratio of the compound represented by the above formula (3) and the compound represented by the above formula (4) is 50 / 50 to 99 / 1 in terms of molar ratio (compound represented by the above formula (3) / compound represented by the above formula (4)). [Means 9] A copolymer having a repeating unit derived from the compound represented by the above formula (3) and a repeating unit derived from the compound represented by the above formula (4), and having a structure derived from a conjugated acid having an acidity constant (pKa) of 5 or less at its terminal. EXAMPLES
[0053] The present invention will be described in detail below based on examples, but is not limited to these examples. In the examples and comparative examples, "parts" and "%" are based on mass unless otherwise specified. The method for measuring the molecular weight of the polymer is shown below.
[0054] [Measurement of molecular weight of polymer]: Using a gel permeation chromatograph (product name: HLC-8420GP, manufactured by Tosoh Corporation) and a differential refractometer as a detector, measurements were carried out under the following conditions, and the molecular weight was calculated as a standard polystyrene equivalent value. Column: 2 units of "GMHXL-SP" (manufactured by Tosoh Corporation), column temperature: 40°C Mobile phase: tetrahydrofuran, flow rate: 1.0 mL / min Sample concentration: 10mg / 20mL
[0055] 1. Preparation of initiator (carboxylate compound) (Preparation of initiator 1) In a dried eggplant flask, 19.9 g of tetrabutylammonium hydroxide as an ammonium salt in a 10% methanol solution and 0.79 g of pivalic acid were added and heated at 50°C for 1 hour, after which 10 mL of toluene was added and azeotropic dehydration was carried out. After azeotropic dehydration was carried out three times, nitrogen replacement was carried out, and 28 mL of deoxygenated toluene was added, and activated molecular sieves were added to make a dehydrated toluene solution of about 0.25 M. This was used as a dehydrated toluene solution containing initiator 1 for the production of copolymers.
[0056] (Preparation of initiator 2) In a dry recovery flask, 19.9 g of a 10% methanol solution of tetrabutylammonium hydroxide as an ammonium salt was added, and 0.48 g of acetic acid was added, and the same operation as for initiator 1 was carried out to obtain a dehydrated toluene solution of about 0.25 M. This was used as a dehydrated toluene solution containing initiator 2 for the production of a copolymer.
[0057] (Preparation of initiator 3) In a dry recovery flask, 19.9 g of a 10% methanol solution of tetrabutylammonium hydroxide as an ammonium salt and 0.71 g of isobutyric acid were added, and the same operation as for initiator 1 was carried out to obtain a dehydrated toluene solution of about 0.25 M. This was used as a dehydrated toluene solution containing initiator 3 for the production of a copolymer.
[0058] (Preparation of initiator 4) In a dry recovery flask, 28.5 g of a 10% methanol solution of tetrahexylammonium hydroxide as an ammonium salt was added, and 0.79 g of pivalic acid was added, and the same operation as for initiator 1 was carried out to obtain a dehydrated toluene solution of about 0.25 M. This was used as a dehydrated toluene solution containing initiator 4 for the production of a copolymer.
[0059] (Preparation of initiator 5) In a dry recovery flask, 28.5 g of a 10% methanol solution of tetrahexylammonium hydroxide as an ammonium salt was added, and 0.71 g of isobutyric acid was added, and the same operation as for initiator 1 was carried out to obtain a dehydrated toluene solution of about 0.25 M. This was used as a dehydrated toluene solution containing initiator 5 in the production of a copolymer.
[0060] (Preparation of initiator 6) In a dry recovery flask, 28.5 g of a 10% methanol solution of tetrahexylammonium hydroxide as an ammonium salt was added, and 0.98 g of benzoic acid was added, and the same operation as for initiator 1 was carried out to obtain a dehydrated toluene solution of about 0.25 M. This was used as a dehydrated toluene solution containing initiator 6 for the production of a copolymer.
[0061] 2. Preparation of aluminum catalyst (organoaluminum compound) (Preparation of Al catalyst 1) A dried Schlenk flask was purged with nitrogen, 16.5 g of 2,6-di-tert-butylphenol was placed in it, and after evacuation, deoxygenated toluene was added to make a 2 M toluene solution. In addition, 18 mL of a 1.0 mol / L toluene solution of triisobutylaluminum was added to another dried Schlenk flask, and after cooling to 0°C, a solution of 2,6-di-tert-butylphenol in an amount of 2 molar equivalents to aluminum was added dropwise, and the mixture was left overnight at room temperature with stirring to prepare a 0.5 M toluene solution of Al catalyst 1.
[0062] (Preparation of Al catalyst 2) A dried Schlenk flask was purged with nitrogen, 18.9 g of 2,6-di-tert-butyl-4-methoxyphenol was placed in it, and the same procedure as for Al catalyst 1 was carried out to prepare a 0.5 M toluene solution of Al catalyst 2.
[0063] (Preparation of Al catalyst 3) A dried Schlenk flask was purged with nitrogen, 17.6 g of 2,6-di-tert-butyl-4-methylphenol was placed in it, and the same procedure as for Al catalyst 1 was carried out to prepare a 0.5 M toluene solution of Al catalyst 3.
[0064] (Preparation of Al catalyst 4) A dried Schlenk flask was purged with nitrogen, 7.1 g of 2,6-di-tert-butyl-4-methoxyphenol was placed in it, and after evacuation, deoxygenated toluene was added to make a 2 M toluene solution. In addition, 15 mL of a 1.0 mol / L toluene solution of triethylaluminum was added to another dried Schlenk flask, and after cooling to 0°C, a solution of 2,6-di-tert-butylphenol in an amount of 2 molar equivalents to aluminum was added dropwise, and the mixture was left overnight at room temperature with stirring to prepare a 0.5 M toluene solution of Al catalyst 4.
[0065] (Preparation of Al catalyst 5) A dried Schlenk flask was purged with nitrogen, and 7.1 g of 2,6-di-tert-butyl-4-methoxyphenol and 2.6 g of isobutyl alcohol were placed in it. After evacuation, deoxygenated toluene was added to prepare a 1 M toluene solution. In addition, 15 mL of a 1.0 mol / L toluene solution of triethylaluminum was added to another dried Schlenk flask, and after cooling to 0°C, a solution of 2,6-di-tert-butylphenol and isobutyl alcohol, each of which was 1 molar equivalent to aluminum, was added dropwise, and the mixture was left overnight at room temperature with stirring to prepare a 0.5 M toluene solution of Al catalyst 5.
[0066] (Preparation of Al catalyst 6) A dried Schlenk flask was purged with nitrogen, 5.2 g of isobutyl alcohol was placed in it, and after evacuation, deoxygenated toluene was added to prepare a 2 M toluene solution. In addition, 15 mL of a 1.0 mol / L toluene solution of triethylaluminum was added to another dried Schlenk flask, and after cooling to 0°C, a solution of 2 molar equivalents of isobutyl alcohol relative to aluminum was added dropwise, and the mixture was left overnight at room temperature with stirring to prepare a 0.5 M toluene solution of Al catalyst 5.
[0067] 3. Preparation of copolymer Example 1 After replacing the dried two-neck flask with nitrogen, 15 mL of deoxygenated toluene was added, 1.3 mL of ethyl acrylate, and 0.26 mL of α-methylene-γ-butyrolactone were added and stirred. After cooling to 0°C, 1.5 mL of Al catalyst 1 was added and stirred, while 0.60 mL of initiator 1 was added, and polymerization was started at 0°C. After 5 minutes, 1.0 mL of 20 vol% ethanol in toluene was added to stop the reaction, and a copolymer consisting of α-methylene-γ-butyrolactone and ethyl acrylate was obtained. After polymerization, the reaction solution was analyzed by gas chromatography (GC), and the reaction rate was calculated from the remaining monomer. In addition, the reaction solution was reprecipitated with methanol to extract the polymer, which was then redissolved in tetrahydrofuran and the molecular weight was calculated by gel permeation chromatography (GPC).
[0068] Example 2 A copolymer consisting of α-methylene-γ-butyrolactone and n-butyl acrylate was obtained by the same operation as in Example 1 except that 1.71 mL of n-butyl acrylate was used instead of ethyl acrylate in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0069] Example 3 A copolymer consisting of α-methylene-γ-butyrolactone and n-hexyl acrylate was obtained by the same operation as in Example 1 except that 2.11 mL of n-hexyl acrylate was used instead of ethyl acrylate in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0070] Example 4 A copolymer consisting of α-methylene-γ-butyrolactone and n-octyl acrylate was obtained by the same operation as in Example 1 except that 2.51 mL of n-octyl acrylate was used instead of ethyl acrylate in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0071] Example 5 A copolymer consisting of α-methylene-γ-butyrolactone and n-dodecyl acrylate was obtained in the same manner as in Example 1, except that 3.32 mL of n-dodecyl acrylate was used instead of ethyl acrylate in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0072] Example 6 A copolymer consisting of α-methylene-γ-butyrolactone and n-stearyl acrylate was obtained by the same operation as in Example 1, except that 3.89 mL of n-stearyl acrylate was used instead of ethyl acrylate in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0073] Example 7 A copolymer consisting of α-methylene-γ-butyrolactone and n-stearyl acrylate was obtained in the same manner as in Example 6, except that the amount of α-methylene-γ-butyrolactone was changed to 0.60 mL and the amount of n-stearyl acrylate was changed to 2.66 mL in Example 6. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0074] (Examples 8 to 12) Using initiators 2 to 6 as initiators, copolymers consisting of α-methylene-γ-butyrolactone and ethyl acrylate were obtained in the same manner as in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0075] (Examples 13 to 15) Using Al catalysts 2 to 4 as catalysts, copolymers consisting of α-methylene-γ-butyrolactone and ethyl acrylate were obtained in the same manner as in Example 1. After polymerization, the reaction rate was calculated from the residual monomer in the same manner as in Example 1, and the molecular weight was calculated by GPC.
[0076] Comparative Example 1 After replacing the air in a dried two-neck flask with nitrogen, 15 mL of deoxygenated toluene was added, followed by 1.3 mL of ethyl acrylate and 0.26 mL of α-methylene-γ-butyrolactone, and the mixture was stirred. After cooling to 0°C, 0.60 mL of initiator 1 was added, and polymerization was started at 0°C. However, the polymerization reaction did not proceed under these conditions, and the desired copolymer could not be obtained.
[0077] Comparative Example 2 After replacing the air in a dried two-neck flask with nitrogen, 15 mL of deoxygenated toluene was added, followed by 1.3 mL of ethyl acrylate and 0.26 mL of α-methylene-γ-butyrolactone, and the mixture was stirred. After cooling to 0°C, 1.5 mL of Al catalyst 5 was added and 0.60 mL of initiator 1 was added while stirring, and polymerization was started at 0°C. However, the polymerization reaction did not proceed under these conditions, and the desired copolymer could not be obtained.
[0078] Comparative Example 3 A polymerization reaction between α-methylene-γ-butyrolactone and ethyl acrylate was carried out in the same manner as in Comparative Example 2, except that Al catalyst 6 was used instead of Al catalyst 5. However, the polymerization reaction did not proceed under these conditions, and the target copolymer could not be obtained.
[0079] Comparative Example 4 After replacing the air in a dried two-neck flask with nitrogen, 15 mL of deoxygenated toluene was added, followed by 1.3 mL of ethyl acrylate and 0.58 mL of methyl adamantyl methacrylate, and the mixture was stirred. After cooling to 0°C, 1.5 mL of Al catalyst 6 was added and 0.60 mL of initiator 1 was added while stirring, and polymerization was started at 0°C. However, under these conditions, the polymerization reaction did not proceed, and the desired copolymer could not be obtained.
[0080] The polymerization conditions in Examples 1 to 15 and Comparative Examples 1 to 4, as well as the number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the copolymers obtained by polymerization are shown in Table 1. In Table 1, the monomer ratio (mol%) indicates the ratio of each monomer to the total amount of monomers used in the polymerization. In Comparative Examples 1 to 4, the polymerization reaction did not proceed, so the number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) columns are marked with "-".
[0081] [Table 1]
[0082] As can be seen from the results shown in Table 1, according to Examples 1 to 15, even when copolymerization using a (meth)acrylic acid ester compound and an α-methylene lactone compound was carried out under mild temperature conditions, copolymers having a high molecular weight, number average molecular weight (Mn) of 20,000 or more and a narrow molecular weight distribution of 3.0 or less could be obtained.
Claims
1. A method for producing a copolymer, comprising polymerizing a monomer containing a compound represented by the following formula (3) and a compound represented by the following formula (4) in the presence of a compound represented by the following formula (5) and an anionic polymerization initiator. [Case 1] (In formula (3), R 10 is a hydrogen atom or a methyl group. 1 represents a hydrocarbyl group having 1 to 20 carbon atoms, which may be substituted with a heteroatom-containing group having at least one element selected from the group consisting of nitrogen, oxygen, sulfur, and halogen. 2 represents a divalent linking group. [Case 2] (In formula (5), Ar 1 represents a monovalent group bonded to the oxygen atom in the formula through a benzene ring, in which a secondary carbon or a tertiary carbon is bonded to the carbon at the 2-position and the 6-position of the benzene ring, respectively, and a hydrogen atom, a chlorine atom, a fluorine atom, a hydrocarbyl group having 1 to 6 carbon atoms, or a hydrocarbyloxy group having 1 to 6 carbon atoms is bonded to the carbon at the 4-position. 3 represents an alkyl group having 2 to 10 carbon atoms.
2. 2. The method for producing a copolymer according to claim 1, wherein the anionic polymerization initiator is a salt of an anion of a conjugate acid having an acidity constant (pKa) of 5 or less and an ammonium cation.
3. The method for producing a copolymer according to claim 2, wherein the anion of the conjugate acid is a carboxylate ion, an azide ion or a 2,4-dinitrophenol ion.
4. The method for producing the copolymer according to claim 1, wherein the polymerization temperature is from -10 to 20°C.
5. The method for producing the copolymer according to claim 1 , wherein the monomers are polymerized in an organic solvent.
6. R in the above formula (3) 1is an alkyl group having 1 to 20 carbon atoms which may be substituted with the heteroatom-containing group,
7. R in the above formula (4) 2 is an alkanediyl group having 2 to 5 carbon atoms or * 1 -O-C-O-R 11 - (However, R 11 is an alkanediyl group having 1 to 4 carbon atoms, and "* 1 " represents a bond to the vinyl group in formula (4).
8. The method for producing a copolymer according to claim 1, wherein a molar ratio of the compound represented by formula (3) to the compound represented by formula (4) is 50 / 50 to 99 / 1.
9. A copolymer having a repeating unit derived from a compound represented by the following formula (3) and a repeating unit derived from a compound represented by the following formula (4), and having a structure derived from a conjugated acid having an acidity constant (pKa) of 5 or less at its terminal. [C3] (In formula (3), R 10 is a hydrogen atom or a methyl group. 1 represents a hydrocarbyl group having 1 to 20 carbon atoms, which may be substituted with a heteroatom-containing group having at least one element selected from the group consisting of nitrogen, oxygen, sulfur, and halogen. 2 represents a divalent linking group.
Citation Information
Patent Citations
Method for producing copolymer
JP2022083035A