Decorative sheet

The decorative sheet's laminate structure with controlled erosion rate bonding between resin coat and transparent film layers addresses temperature-induced cracking and peeling, ensuring durability and appearance stability.

JP2024155622AInactive Publication Date: 2024-10-31SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023070495
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-21
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Decorative sheets used for enhancing wall designs suffer from cracks and peeling due to temperature changes, leading to a deterioration in appearance.

Method used

A decorative sheet composed of a laminate structure with a resin coat layer and transparent film, where both layers contain specific resin materials and are bonded with a transition layer having a controlled erosion rate distribution, ensuring strong adhesion and resistance to temperature changes.

Benefits of technology

The laminate structure effectively suppresses cracks and peeling, providing excellent durability against temperature fluctuations, thereby maintaining the appearance of the decorative sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155622000001_ABST
    Figure 2024155622000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet capable of exhibiting excellent durability against a temperature change.SOLUTION: A decorative sheet 10 includes a laminate including a printed layer 14, a clear film 16 and a resin coating layer 20, laminated in this order. The resin coating layer 20 and the clear film 16 respectively include a first resin material and a second resin material. When an erosion rate in a thickness direction of the decorative sheet 10 is measured by projecting polygonal alumina particles to the decorative sheet 10 using a micro slurry jet erosion method, the decorative sheet 10 satisfies a gradient amount of -1.0 / g to 0.0 / g in a region located between the resin coating layer 20 and the clear film 16 in an erosion rate distribution graph showing a relation between an erosion rate and an erosion depth.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative sheet. [Background technology]

[0002] 2. Description of the Related Art In recent years, in the construction of interior and exterior walls of residences such as condominiums, buildings, hotel lobbies, rooms, offices, conference rooms, elevators, etc., decorative sheets having patterns such as wood grain, stone grain, stripe pattern, etc. have been affixed to the walls in order to enhance the design of the walls.

[0003] One such decorative sheet that has been proposed is one in which a decorative printed layer is laminated on the back surface of a transparent film, and further, a resin coating layer that protects the transparent film is laminated on the front surface of the transparent film (see, for example, Patent Document 1).

[0004] A decorative sheet having such a structure has a problem that, after being applied to a wall, temperature changes caused by air temperature changes cause cracks and peeling in the resin coating layer, resulting in a deterioration in appearance. In other words, the reality is that there is a demand for providing decorative sheets having such a structure with better durability against temperature changes. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-24238 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a decorative sheet that exhibits excellent durability against temperature changes. [Means for solving the problem]

[0007] Such an object can be achieved by the present invention described in (1) to (9) below. (1) a printing layer; A transparent film and and a resin coating layer, which are laminated in this order; A decorative sheet characterized in that the resin coating layer and the transparent film contain a first resin material and a second resin material, respectively, and satisfy the following requirement A. Requirement A: When the decorative sheet is subjected to a microslurry jet erosion method in which polygonal alumina particles having an average particle diameter D50 of 0.3 μm are projected onto the decorative sheet from the resin coating layer side with a projection force that results in an erosion rate of 0.481 μm / g for a silicon wafer, and the erosion rate [μm / g] in the thickness direction of the decorative sheet at the position where the polygonal alumina particles were projected is measured, the magnitude of the slope in the region located between the resin coating layer and the transparent film in an erosion rate distribution graph showing the relationship between the erosion rate and the erosion depth, with the erosion rate [μm / g] on the y-axis and the erosion depth [μm], which is the position in the thickness direction showing the erosion rate, on the x-axis, is -1.0 / g or more and 0.0 / g or less.

[0008] (2) The decorative sheet according to (1) above, wherein the transparent film contains polyethylene terephthalate as the second resin material.

[0009] (3) The decorative sheet according to (1) or (2) above, wherein the resin coating layer contains a melamine-based resin as the first resin material.

[0010] (4) The decorative sheet according to any one of (1) to (3) above, wherein the resin coating layer has an average thickness of 5.0 μm or more and 30.0 μm or less.

[0011] (5) A decorative sheet according to any one of (1) to (4) above, wherein the resin coating further contains a matte filler and the surface thereof is configured as an uneven surface having protrusions following the shape of the matte filler.

[0012] (6) The decorative sheet according to the above (5), wherein the matte filler contains at least one of an acrylic resin, a melamine resin, a polystyrene resin, and silica.

[0013] (7) The decorative sheet according to (5) or (6) above, wherein the resin coating layer has a matte filler content of 10% by volume or more and 50% by volume or less.

[0014] (8) The decorative sheet according to any one of (5) to (7) above, wherein the matte filler has a median diameter (D50) of 7.0 μm or more and 50.0 μm or less.

[0015] (9) A decorative sheet according to any one of (1) to (8) above, wherein the laminate further comprises a concealing layer laminated on the side of the printed layer opposite the transparent film. Effect of the Invention

[0016] According to the present invention, it is possible to obtain a decorative sheet that exhibits excellent durability against temperature changes caused by changes in air temperature. [Brief description of the drawings]

[0017] [Figure 1] 1 is a longitudinal sectional view showing an embodiment of a decorative sheet of the present invention. [Diagram 2] 1 is an erosion rate distribution graph showing the relationship between the erosion rate and the erosion depth in the decorative sheets of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The decorative sheet of the present invention will now be described in detail with reference to preferred embodiments shown in the accompanying drawings.

[0019] The decorative sheet 10 of the present invention comprises a printed layer 14, a transparent film 16, and a resin coating layer 20, which are laminated in this order, and the resin coating layer 20 and the transparent film 16 contain a first resin material and a second resin material, respectively, and satisfy the following requirement A.

[0020] Requirement A: When the decorative sheet 10 is subjected to a microslurry jet erosion method in which polygonal alumina particles having an average particle diameter D50 of 0.3 μm are projected onto the decorative sheet 10 from the resin coating layer 20 side with a projection force that results in an erosion rate of 0.481 μm / g for a silicon wafer, and the erosion rate [μm / g] in the thickness direction of the decorative sheet 10 at the position where the polygonal alumina particles were projected is measured, the magnitude of the slope in region a located between the resin coating layer 20 and the transparent film 16 in an erosion rate distribution graph showing the relationship between erosion rate and erosion depth, with the erosion rate [μm / g] on the y-axis and the erosion depth [μm], which is the position in the thickness direction showing the erosion rate, on the x-axis, is -1.0 / g or more and 0.0 / g or less.

[0021] Thus, in the present invention, in requirement A, the slope in the erosion rate distribution graph is set to a magnitude within the range of -1.0 / g or more and 0.0 / g or less, which makes it possible to appropriately suppress or prevent cracks or peeling in the resin coat layer 20 due to temperature changes caused by changes in air temperature. Therefore, it is possible to appropriately suppress or prevent deterioration of the appearance caused by cracks or peeling in the resin coat layer 20. Therefore, it can be said that the decorative sheet 10 exhibits excellent durability against temperature changes caused by changes in air temperature.

[0022] Below, each part (each layer) constituting the decorative sheet 10 will be described. Note that below, a case will be described as an example in which the decorative sheet 10 further comprises a concealing layer 12 laminated on the printed layer 14 side in addition to the printed layer 14, transparent film 16, and resin coat layer 20, that is, a case in which the decorative sheet 10 comprises the concealing layer 12, the printed layer 14, the transparent film 16, and the resin coat layer 20, and is configured as a laminate in which these are laminated in this order.

[0023] (Decorative sheet 10) Fig. 1 is a vertical cross-sectional view showing an embodiment of the decorative sheet of the present invention. For convenience of explanation, the upper side of Fig. 1 will be referred to as "upper" and the lower side as "lower".

[0024] (Concealment Layer 12) The concealing layer 12 constitutes the innermost layer located on the wall side when the decorative sheet 10 is applied to a wall, that is, the innermost layer located on the side opposite to the surface of the decorative sheet 10 that is visible to the user.

[0025] By configuring this concealing layer 12 as the innermost layer located on the wall side, the wall, in other words, the application surface to which the decorative sheet 10 is applied, can be concealed from the printing layer 14 located on the opposite side to the wall of the concealing layer 12. As a result, it is possible to appropriately suppress or prevent the wall (application surface) from being viewed from the resin coat layer 20 side, i.e., the front surface side of the decorative sheet 10.

[0026] In addition, when a user views the concealing layer 12 from the resin coating layer 20 side, the concealing layer 12 also has the function of improving the visibility of the pattern in the printed layer 14 or changing the color depending on the combination with the printed layer 14 described below.

[0027] In this embodiment, the concealing layer 12 is a laminate made of a resin film 12a and a metal deposition layer 12b, with the resin film 12a located on the wall side and the metal deposition layer 12b located on the printed layer 14 side.

[0028] The resin film 12a is made mainly of a resin material (fourth resin material) and functions as a base material that supports the metal deposition layer 12b.

[0029] In this specification, the term "main material" refers to a constituent material that is contained in an amount of 50% by weight or more among the constituent materials that constitute the layer (film) that contains this material.

[0030] The resin material is not particularly limited, and examples thereof include thermoplastic resins and curable resin materials. Specific examples thereof include polyolefins such as polyethylene, polypropylene, ethylene-propylene copolymers, and ethylene-vinyl acetate copolymers (EVA), cyclic polyolefins (COP), modified polyolefins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyamides (e.g., nylon 6, nylon 46, nylon 66, nylon 610, nylon 612, nylon 11, nylon 12, nylon 6-12, and nylon 6-66), and polyimides. , polyamide-imide, polycarbonate (PC), poly-(4-methylpentene-1), ionomer, acrylic resin, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylonitrile-styrene copolymer (AS resin), butadiene-styrene copolymer, polyoxymethylene, polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer (EVOH), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polycyclohexane terephthalate Polyesters such as PCT, polyether, polyether ketone (PEK), polyether ether ketone (PEEK), polyetherimide, polyacetal (POM), polyphenylene oxide, modified polyphenylene oxide, polysulfone, polyether sulfone, polyphenylene sulfide, polyarylate, aromatic polyester (liquid crystal polymer), polytetrafluoroethylene, polyvinylidene fluoride, other fluorine-based resins, styrene-based, polyolefin-based, polyvinyl chloride-based, polyurethane-based, polyester-based, polyamide-based, polybutadiene-based, trans-polyisoprene-based, fluorine rubber-based, chlorinated polyethylene-based and other thermoplastic elastomers, epoxy resins, phenolic resins, urea resins, melamine-based resins, unsaturated polyesters, silicone-based resins, urethane-based resins, poly-para-xylylene, polymonochloro-para-xylylene, polydichloro-para-xylylene,Examples of the resin material include polyparaxylylene resins such as polymonofluoroparaxylylene and polymonoethylparaxylylene, or copolymers, blends, and polymer alloys mainly made of these resins. One or more of these resins may be used in combination. Among these, in this embodiment, it is preferable that the resin material is a thermoplastic resin, particularly polyvinyl chloride.

[0031] The metal vapor deposition layer 12 b is laminated on the printed layer 14 side of the resin film 12 a and functions as the main layer of the concealing layer 12 .

[0032] This metal deposition layer 12b is not particularly limited, but examples thereof include those mainly composed of metal oxides, metal nitrides, etc. Examples of metal oxides and metal nitrides include aluminum oxide, silicon oxide, silicon nitride, silicon oxynitride, etc., and one or more of these may be used in combination.

[0033] The average thickness (layer thickness) of the concealing layer 12 composed of the laminate of the metal deposition layer 12b and the resin film 12a is not particularly limited, but is preferably set to about 10.0 μm or more and 300 μm or less, more preferably 50.0 μm or more and 250 μm or less. This ensures that the function of the concealing layer 12 can be imparted.

[0034] In this embodiment, the metal vapor deposition layer 12b is formed on the printed layer 14 side of the resin film 12a (see Figure 1), but the position at which the metal vapor deposition layer 12b is formed is not limited to this, and the metal vapor deposition layer 12b may be formed on the side opposite the printed layer 14 of the resin film 12a.

[0035] Furthermore, when there is no need for the concealing layer 12 to conceal the wall portion (the application surface to which the decorative sheet 10 is applied) from the printing layer 14, the concealing layer 12 (a laminate of a metal vapor deposition layer 12b and a resin film 12a) having such a configuration may be omitted from being formed as the innermost layer of the decorative sheet 10.

[0036] (Print layer 14) The printed layer 14 is provided with various patterns, such as a wood grain pattern, a stone pattern, a geometric pattern such as a striped pattern, and the like, and is a layer that greatly affects the appearance and aesthetics of the decorative sheet 10, and the patterns are visible when the user views the decorative sheet 10 from the resin coat layer 20 side, i.e., from the front side of the decorative sheet 10. Therefore, the pattern of the printed layer 14 is imparted to the wall portion to which the decorative sheet 10 is attached.

[0037] The printed layer 14 is primarily made of a resin material and contains a colorant. The inclusion of the colorant in the printed layer 14 gives the printed layer 14 various patterns such as a wood grain pattern, a stone pattern, grained processing, and various geometric patterns.

[0038] The resin material (third resin material) contained in the print layer 14 may be, for example, the same resin material (fourth resin material) as exemplified for the resin film 12a. In addition, various pigments, dyes, etc. may be used as the colorant.

[0039] The average thickness (layer thickness) of the printed layer 14 is not particularly limited, but is preferably set to about 0.1 μm or more and 15.0 μm or less, and more preferably about 1.0 μm or more and 5.0 μm or less, so that the function of the printed layer 14 can be reliably imparted.

[0040] (Transparent Film 16) The transparent film 16 is an intermediate layer located between the resin coat layer 20 and the printed layer 14, and the provision of this transparent film 16 in the decorative sheet 10 can impart superior flexibility to the decorative sheet 10. Furthermore, by transmitting light reflected by the printed layer 14, the pattern of the printed layer 14 can be viewed by the user from the resin coat layer 20 side, i.e., the surface of the decorative sheet 10 that is viewed by the user.

[0041] The transparent film 16 contains a resin material (second resin material) as a main material. For example, the resin material may be the same resin material (fourth resin material) as exemplified for the resin film 12a, and among them, polyethylene terephthalate or polyvinyl chloride is preferable, and polyethylene terephthalate is more preferable. This ensures that the transparent film 16 can function as it is.

[0042] The average thickness (layer thickness) of the transparent film 16 is not particularly limited, but is preferably set to about 10.0 μm or more and 300 μm or less, and more preferably about 50.0 μm or more and 200 μm or less, so that the function of the transparent film 16 can be reliably imparted.

[0043] (Resin coat layer 20) When the decorative sheet 10 is attached to a wall, the resin coating layer 20 constitutes the outermost layer located on the side opposite the wall, i.e., the surface (outermost layer) visible to the user, and also functions as a protective layer to protect the transparent film 16.

[0044] In this embodiment, the resin coating layer 20 contains a matte filler 18 and a resin material (first resin material) that serves as a binder resin that holds the matte filler 18 in the resin coating layer 20, and has a convex portion 20a on the surface opposite the transparent film 16 that conforms to the shape of the matte filler 18, such that the surface opposite the transparent film 16 is composed of an uneven surface.

[0045] In this way, by constructing the surface of the resin coating layer 20 opposite the transparent film 16 with an uneven surface having convex portions 20a, it is possible to obtain an anti-diffusion effect that prevents reflected light from being unintentionally diffused in the resin coating layer 20 that constitutes the surface of the decorative sheet 10, thereby making it possible to provide the decorative sheet 10 with reduced gloss and excellent aesthetics.

[0046] In the resin coat layer 20 having such a configuration, the content of the matte filler 18 is preferably 10 volume % or more and 50 volume % or less, and more preferably 20 volume % or more and 35 volume % or less.

[0047] By setting the content of the matte filler 18 in the resin coating layer 20 within the above range, the matte fillers 18 are reliably overlapped in the thickness direction in at least a portion of the resin coating layer 20 as shown in Fig. 1, so that the surface of the resin coating layer 20 can be reliably configured as an uneven surface having protrusions 20a on the surface that follow the shape of the matte filler 18. Therefore, the decorative sheet 10 can be reliably made to have a suppressed gloss and excellent aesthetics.

[0048] Furthermore, if the content of the matte filler 18 is less than 10 volume %, depending on the median diameter of the matte filler 18, the matte fillers 18 may not be able to overlap each other sufficiently in the thickness direction, and as a result, the surface of the resin coating layer 20 may not be able to be configured as an uneven surface having convex portions 20a.

[0049] Furthermore, if the content of the matte filler 18 exceeds 50 volume %, depending on the median diameter of the matte filler 18, excessive areas of overlapping between the matte fillers 18 in the thickness direction may be generated, and more protrusions 20a than necessary may be formed on the surface of the resin coating layer 20, which may result in the effect of suppressing the gloss of the surface of the decorative sheet 10 not being fully achieved.

[0050] In this case, the matte filler 18 has a median diameter (D50) set to preferably about 7.0 μm or more and 50.0 μm or less, more preferably about 8.0 μm or more and 40.0 μm or less, and even more preferably about 8.0 μm or more and 18.0 μm or less.

[0051] The resin coat layer 20 has an average thickness (layer thickness) set to preferably about 5.0 μm or more and 30.0 μm or less, more preferably about 6.0 μm or more and 25.0 μm or less, and even more preferably about 8.0 μm or more and 20.0 μm or less.

[0052] By setting the median diameter (D50) of the matte filler 18 and the average thickness of the resin coating layer 20 within the above ranges, when the matte fillers 18 overlap each other in the thickness direction in at least a part of the resin coating layer 20, the total thickness of the overlapping matte fillers 18 can be reliably set to be greater than the thickness of the resin coating layer 20. Therefore, the convex portion 20a can be more reliably formed on the surface of the resin coating layer 20 opposite the transparent film 16.

[0053] In this specification, the "average thickness" of the resin coating layer 20 refers to the average value of the thickness of the resin coating layer 20 measured in the thickness direction in an area where the protrusions 20a resulting from the matte filler 18 are not formed.

[0054] The resin material (first resin material) contained in the resin coat layer 20 may be, for example, the same resin material (fourth resin material) as that exemplified in the resin film 12a, but among them, a thermoplastic resin or a melamine resin is preferable, and the thermoplastic resin is more preferably an acrylic resin. This allows the resin material to reliably perform the function of a binder resin, and allows the matte filler 18 to be reliably held in the resin coat layer 20.

[0055] The matte filler 18 is mainly made of a resin material or an inorganic material, and the resin material is not particularly limited, but examples thereof include acrylic resin, melamine resin, polystyrene resin, etc., and one or more of these may be used in combination. The inorganic material is not particularly limited, but examples thereof include silica.

[0056] Examples of such matte filler 18 include acrylic resin particles, melamine resin particles, polystyrene resin particles, silica particles, and composite particles of these resins and silica, among which acrylic resin particles or melamine resin particles are preferred, which can improve the visibility of the printing layer 14.

[0057] Specific examples of the matte filler 18 include Metablen (acrylic resin particles, manufactured by Mitsubishi Chemical Corporation), Tuftic (acrylic resin particles, manufactured by Toyobo Co., Ltd.), Techpolymer (acrylic resin particles, manufactured by Sekisui Chemical Industry Co., Ltd.), Techpolymer (polystyrene resin particles, manufactured by Sekisui Chemical Industry Co., Ltd.), silica particles (manufactured by Denka Co., Ltd.), Eposter (melamine resin particles, manufactured by Nippon Shokubai Co., Ltd.), and Optobeads (melamine resin / silica composite particles, manufactured by Nissan Chemical Industries, Ltd.).

[0058] Moreover, it is preferable to use a transparent material for the matte filler 18, the difference in refractive index from the resin material contained in the resin coat layer 20 being 0.2 or less. Here, if the refractive index of the matte filler 18 is significantly different from the refractive index of the resin layer (part of the resin coat layer 20 other than the matte filler 18) mainly composed of the resin material that holds the matte filler 18, the transparency of the resin coat layer 20 decreases, in other words, the clarity of the resin coat layer 20 decreases, and the design of the appearance decreases. Therefore, by setting the refractive index difference to 0.2 or less, the design of the appearance of the resin coat layer 20 can be improved.

[0059] In this case, the refractive index of the resin material contained in the resin coat layer 20 is preferably about 1.4 or more and 1.7 or less, and since the melamine resin preferably used for both the resin coat layer 20 and the matte filler 18 has a refractive index of about 1.6, the refractive index of the matte filler 18 is preferably set to about 1.3 or more and 1.8 or less. This ensures that the magnitude of the refractive index difference between the matte filler 18 and the resin material contained in the resin coat layer 20 can be set to 0.2 or less.

[0060] Furthermore, the difference between the linear expansion coefficient of the resin material contained in the resin coating layer 20 and the linear expansion coefficient of the matte filler 18 is preferably 10×10 -5 / ℃ or less, more preferably 8×10 -5 / ℃ or less, more preferably 5×10 -5 / °C or less. If the difference in linear expansion coefficient is within the above range, the difference in the degree of expansion and contraction in response to temperature changes between the matte filler 18 and the resin material contained in the resin coating layer 20 is small, and the multiple protrusions 20a of the resin coating layer 20 can be maintained. Therefore, the decorative sheet 10 can obtain a surface gloss suppressing effect and an anti-fouling effect.

[0061] Considering the above, a combination in which the resin material contained in the resin coating layer 20 is a melamine-based resin and the resin contained in the matte filler 18 is an acrylic-based resin, or a combination in which the resin material contained in the resin coating layer 20 is a thermoplastic resin and the resin contained in the matte filler 18 is a melamine-based resin, is preferred.

[0062] In addition, when there is no need to suppress the gloss of the decorative sheet 10, i.e., when the surface of the resin coating layer 20 opposite the transparent film 16 does not need to be constructed as an uneven surface having convex portions 20a, but is constructed as a flat surface, the resin coating layer 20 may be constructed of the first resin material as a binder resin without adding the matte filler 18.

[0063] Furthermore, the decorative sheet 10 constituted by a laminate in which the above-mentioned layers are stacked is not limited to the above configuration, and may, for example, be provided with an adhesive layer (not shown) on the surface of the concealing layer 12 opposite the surface facing the printed layer 14, i.e., on the surface of the resin film 12a side of the concealing layer 12. This makes it possible to provide a configuration in which the decorative sheet 10 can be directly attached to a wall, i.e., an application surface, without the need to apply an adhesive or the like to the decorative sheet 10.

[0064] However, there was a problem in that after the decorative sheet 10 was attached to the wall, changes in temperature could cause cracks and peeling to occur in the resin coating layer 20 of the decorative sheet 10, resulting in a deterioration in the appearance of the decorative sheet 10.

[0065] The present inventors have considered these problems and conducted studies, and have found that the occurrence of cracks and peeling in the resin coating layer 20, as described above, is due to the lack of excellent adhesion between the resin coating layer 20 and the transparent film 16 that is the layer below the resin coating layer 20. In addition, by measuring the erosion rate [μm / g], which is measured by projecting polygonal alumina particles in the thickness direction of the decorative sheet 10 using the micro slurry jet erosion method (MSE method), in the region a between the resin coating layer 20 and the transparent film 16, i.e., the interface, it was possible to know the state of bonding (adhesion) in the region a (interface) between the resin coating layer 20 and the transparent film 16.

[0066] And, as a result of further investigation, the inventors of the present invention have found that when a microslurry jet erosion method is used to project polygonal alumina particles having an average particle diameter D50 of 0.3 μm onto the decorative sheet 10 from the resin coat layer 20 side with a projection force that results in an erosion rate of 0.481 μm / g for a silicon wafer, and the erosion rate [μm / g] in the thickness direction of the decorative sheet 10 at the position where the polygonal alumina particles are projected is measured, the erosion rate [μm / g] is plotted on the y-axis and the position in the thickness direction that shows the erosion rate is plotted on the y-axis. The inventors have discovered that when the decorative sheet 10 satisfies the requirement A, in an erosion rate distribution graph showing the relationship between erosion rate and erosion depth, with the x-axis being the erosion depth [μm], the magnitude of the slope in region a located between the resin coating layer 20 and the transparent film 16 is greater than or equal to -1.0 / g and less than or equal to 0.0 / g, the deterioration of the appearance of the decorative sheet 10 caused by cracks and peeling in the resin coating layer 20 due to temperature changes can be appropriately suppressed or prevented, and have thus completed the present invention.

[0067] As described above, in the region a (interface) located between the resin coat layer 20 and the transparent film 16 in the erosion rate distribution graph showing the relationship between the erosion rate and the erosion depth, when an approximation line is obtained by linear approximation using, for example, the least squares method based on the erosion rate [μm / g] measured in the thickness direction (erosion depth [μm]) of the decorative sheet 10, the slope of the approximation line is set to a value within the range of -1.0 / g or more and 0.0 / g or less, so that it can be said that the region a located between the resin coat layer 20 and the transparent film 16 is composed of a transition layer that transitions (shifts) gently from the resin coat layer 20 to the transparent film 16. Therefore, by the region a located between the resin coat layer 20 and the transparent film 16 being composed of such a transition layer, a strong interaction is obtained between the resin coat layer 20 and the transparent film 16. Therefore, the resin coat layer 20 and the transparent film 16 can be bonded with excellent adhesion. Therefore, it is possible to appropriately suppress or prevent cracks or peeling in the resin coat layer 20 due to changes in temperature, and therefore it is possible to appropriately suppress or prevent deterioration of the appearance caused by cracks or peeling in the resin coat layer 20. Therefore, the decorative sheet 10 exhibits excellent durability against changes in temperature.

[0068] In the present invention, the slope of the approximation line may be set to a value within the range of -1.0 / g to 0.0 / g, but is preferably set to a value within the range of -0.6 / g to -0.3 / g. This allows a transition layer to be formed in the region a between the resin coating layer 20 and the transparent film 16, which transitions more gently from the resin coating layer 20 to the transparent film 16, and the above-mentioned effect is more pronounced.

[0069] Furthermore, the approximate straight line preferably satisfies that the maximum and minimum values ​​of the erosion rate are both within a range of 0.3 μm / g to 3.0 μm / g, more preferably 0.5 μm / g to 2.0 μm / g, in the region a located between the resin coating layer 20 and the transparent film 16, i.e., the transition layer. As a result, the transition layer constituting the region a located between the resin coating layer 20 and the transparent film 16 exhibits excellent strength, and from this viewpoint, it is possible to appropriately suppress or prevent the occurrence of cracks or peeling due to temperature changes in this transition layer.

[0070] More specifically, the erosion rate [μm / g] in the thickness direction of the decorative sheet 10 is measured as follows.

[0071] That is, under conditions of room temperature (25°C) x atmospheric pressure (1013 hPa), the decorative sheet 10 is arranged with the resin coating layer 20 on the upper side and the transparent film 16 on the lower side. Then, in this state, with the projection direction being the vertical direction perpendicular to the decorative sheet 10, polygonal alumina particles having an average particle diameter D50 of 0.3 μm are projected from the resin coating layer 20 side from the upper side of the decorative sheet 10 (resin coating layer 20) onto the decorative sheet 10 with a projection distance (separation distance) from the projection position to the surface of the resin coating layer 20 of 4.0 mm.

[0072] At this time, the projection of the polygonal alumina particles is carried out by projecting an aqueous dispersion containing the polygonal alumina particles as fine particles onto the decorative sheet 10, and this aqueous dispersion is prepared by dispersing polygonal alumina particles having an average particle size D50 of 0.3 μm in purified water at a content of 1.0 mass %. The projection force of the polygonal alumina particles onto the decorative sheet 10 is set to a magnitude that results in an erosion rate of 0.481 μm / g for the silicon wafer. This projection force can be adjusted by appropriately setting the projection speed and projection pressure of the aqueous dispersion containing the polygonal alumina particles.

[0073] Furthermore, the erosion depth [μm], which is the position in the thickness direction of the decorative sheet 10 where the erosion rate is measured, i.e., the depth from the surface of the resin coating layer 20 opposite the transparent film 16 to the projection location, is measured using a stylus-type surface profiler at the center of the position where the aqueous dispersion landed in a planar view of the decorative sheet 10, and the erosion rate [μm / g] can be calculated based on the erosion depth [μm] and the amount of projected particles [g] required to reach this erosion depth [μm].

[0074] As described above, a decorative sheet 10 that satisfies requirement A, i.e., a decorative sheet 10 that satisfies that the magnitude of the slope in the region a located between the resin coating layer 20 and the transparent film 16 in the erosion rate distribution graph is between -1.0 / g and 0.0 / g, can be obtained, for example, in a manufacturing method for the decorative sheet 10, by subjecting the surface of the transparent film 16 on which the resin coating layer 20 is to be formed to a hydrophilic treatment such as a corona treatment prior to forming (laminating) the resin coating layer 20 on the transparent film 16. Hereinafter, a manufacturing method for the decorative sheet 10 to which this hydrophilic treatment is applied will be described.

[0075] (Method of manufacturing decorative sheets) The decorative sheet 10 having the above-described configuration can be produced, for example, by laminating a concealing layer 12, a printed layer 14, a transparent film 16, and a resin coating layer 20 containing a matte filler 18 in this order.

[0076] In the following, a method for producing the decorative sheet 10 will be described, in which the layers are laminated in the stated order to produce the decorative sheet 10.

[0077] Specifically, in this embodiment, the manufacturing method for the decorative sheet 10 includes a step a of forming a printed layer 14 on one side of a transparent film 16 by printing, a step b of forming a resin coating layer 20 on the other side of the transparent film 16, and a step c of laminating the printed layer 14 on one side of the concealing layer 12, and further includes a step d of forming a release layer on the other side of the concealing layer 12.

[0078] First, in step a, a transparent film 16 is prepared, and then the printing layer 14 can be formed by printing on one surface of the transparent film 16 by various printing methods.

[0079] The printing method is not particularly limited, but examples thereof include an inkjet method, a screen printing method, a gravure printing method, and a tacho printing method. The ink usually contains a colorant as a solid content. As the colorant, for example, various pigments and various dyes can be used. The ink may also contain a solvent.

[0080] Next, in step b, a resin coat layer 20 is formed on the surface of the transparent film 16 opposite to the surface on which the print layer 14 is formed.

[0081] This resin coating layer 20 can be formed by forming a layer made of a composition for forming a resin coating layer on the surface of the transparent film 16 using various methods such as an immersion method (dipping), a spray method, a coating method using various coaters such as a kiss coater, a comma coater, a roll coater, a knife coater, or a blade coater, or various printing methods, and then carrying out a curing reaction to form the resin coating layer 20.

[0082] This process In the present invention, prior to forming the resin coating layer 20 on the surface of the transparent film 16 opposite the printed layer 14, the surface of the transparent film 16 on which the resin coating layer 20 is to be formed is subjected to a hydrophilization treatment.

[0083] This makes the surface of the transparent film 16 on which the resin coat layer 20 is to be formed hydrophilic, so that when the resin coat layer 20 is formed on the surface of the transparent film 16 opposite the printed layer 14, the region a between the resin coat layer 20 and the transparent film 16 can be configured as a transition layer that transitions gently from the resin coat layer 20 to the transparent film 16. Therefore, the resulting decorative sheet 10 can be obtained as one that satisfies requirement A. In other words, the decorative sheet 10 can be obtained as one that satisfies that the magnitude of the slope in the region a between the resin coat layer 20 and the transparent film 16 in the erosion rate distribution graph is -1.0 / g or more and 0.0 / g or less.

[0084] The hydrophilization treatment is not particularly limited, but examples thereof include surface modification treatments such as plasma treatment, ultraviolet treatment, ozone treatment, corona treatment, and solvent coating treatment, and one or more of these may be used in combination, with corona treatment being preferred. Corona treatment can relatively easily and uniformly hydrophilize the surface of the transparent film 16.

[0085] The degree of hydrophilization of the surface of the transparent film 16 that has been subjected to hydrophilization treatment can be known, for example, by measuring the contact angle of pure water on the surface of the transparent film 16. The contact angle of pure water on the surface of the transparent film 16 is, for example, preferably 60.0° or less, more preferably 5.0° or more and 55.0° or less, and even more preferably 40.0° or more and 55.0° or less. This means that the surface of the transparent film 16 is appropriately hydrophilized, and the magnitude of the inclination in the region a located between the resin coating layer 20 and the transparent film 16 can be reliably set within the range of -1.0 / g or more and 0.0 / g or less. The contact angle of pure water can be measured, for example, using a contact angle meter (Kyowa Interface Science Co., Ltd., "DM-SA", value measured 6 seconds after 1.5 μL of water is dropped on the film).

[0086] In this embodiment, the composition for forming the resin coat layer used to form the resin coat layer 20 contains at least one of the resin material (first resin material) and its precursor contained in the resin coat layer 20, and a matte filler 18.

[0087] The resin coat layer forming composition can be obtained by, for example, mixing at least one of the resin material and its precursor, the matte filler 18, and, if necessary, a solvent, etc., by a known method. By using a solvent, the composition can easily follow the shape of the matte filler 18, and the convex portion 20a can be efficiently formed. Furthermore, since the resin material or its precursor is dissolved or dispersed, the resin coat layer forming composition can be easily handled. In addition, the adhesion between the transparent film 16 and the resin coat layer 20 can be improved.

[0088] The solvent contained in the composition for forming the resin coat layer is not particularly limited, but a polar solvent can be suitably used.

[0089] The solvent contained in the composition for forming the resin coat layer is not particularly limited, but a polar solvent can be preferably used.

[0090] Specific examples of the polar solvent include water; alcoholic solvents such as methanol, ethanol, and isopropanol; ketone-based solvents such as methyl ethyl ketone and acetone; amide-based solvents such as dimethylformamide (DMF); ether-based solvents such as tetrahydrofuran (THF) and tetrahydropyran; and sulfoxide-based solvents such as dimethyl sulfoxide (DMSO). One or more of these may be used in combination.

[0091] Furthermore, each of the compositions for forming the resin coating layer may contain, as necessary, a catalyst, a release agent, a polymerization initiator, a slip agent (leveling agent), a dispersant, a polymerization accelerator, a polymerization inhibitor, a penetration accelerator, a wetting agent (moisturizing agent), a colorant, a fixing agent, an antifungal agent, a preservative, an antioxidant, a chelating agent, a thickener, an antifoaming agent, a sensitizer (sensitizing dye), and the like.

[0092] <c>Next, in step c, the printed layer 14 is laminated onto the metal vapor deposition layer 12b of the concealing layer 12. The printed layer 14 and the metal vapor deposition layer 12b can also be laminated via an adhesive layer.

[0093] <d>Next, in step d, an adhesive layer and a release layer can be laminated on the resin film 12a of the concealing layer 12. By subjecting the decorative sheet 10 to this step d, when the decorative sheet 10 is applied to a construction surface such as a wall, it can be directly attached to the construction surface via the adhesive layer after peeling the release layer from the decorative sheet 10.

[0094] The decorative sheet of the present invention has been described above, but the present invention is not limited to this, and each part that constitutes the decorative sheet can be replaced with any configuration that can perform the same function.

[0095] For example, in the above embodiment, the concealing layer 12 is shown as being composed of a resin film 12a and a metal vapor deposition layer 12b, but the concealing layer 12 is not limited to such a configuration and can be composed, for example, of a laminate of a resin film 12a and a separately prepared metal layer, or can be composed of a single layer consisting of only a colored resin film 12a, or can be composed of a single layer consisting of a resin film 12a that has been whitened by internal voids. EXAMPLES

[0096] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.

[0097] 1. Preparation of raw materials First, the raw materials used in the production of the decorative sheet 10 of each of the Examples and Comparative Examples are shown below.

[0098] The melamine resin constituting the resin coating layer 20 The melamine-based resin was synthesized by the following method. First, the raw material melamine and formalin were charged in a reaction vessel in a predetermined mixing ratio, and after adding a catalyst, the temperature was raised to the boiling point and refluxed. After confirming that the melamine had been completely dissolved, the reaction reached its end point, and the resin solid content was prepared by dehydration treatment and cooled. The melamine-based resin was synthesized by this method.

[0099] Matte filler 18 constituting the resin coating layer 20 Melamine resin particles (manufactured by Nippon Shokubai Co., Ltd., "Eposter", median diameter (D50): 9.0 μm, refractive index: 1.68, linear expansion coefficient (10 -5 / ℃):4)

[0100] 2. Manufacturing of the decorative sheet 10 Example 1 First, a polyethylene terephthalate (PET) film having an ink receiving layer was prepared as the transparent film 16. This transparent film had a thickness of 38.0 μm.

[0101] Next, a printed layer 14 was formed in a predetermined pattern (woodgrain pattern) by an inkjet method on the surface of the transparent film 16 on which the ink receiving layer was provided.

[0102] When forming the printed layer 14 with the wood grain pattern, an ink containing a colorant and an acrylic resin as a UV-curable resin was used to adjust the appearance to have a wood grain pattern. After the ink was ejected by the inkjet method, the ink that had landed on the transparent film 16 was irradiated with UV rays to cure it. This resulted in the printing layer 14 having a thickness of 3 μm.

[0103] Next, the surface of the transparent film 16 opposite to the surface on which the printed layer 14 was formed was subjected to a corona treatment to make the surface hydrophilic. The contact angle of pure water on the corona-treated surface, i.e., the surface on which the resin coating layer 20 was to be formed, was 51.4°.

[0104] Next, a resin composition containing 100% by volume of melamine resin (reaction molar ratio: 1.4, resin solid content: 50% by mass) and 13% by volume of matte filler 18 (melamine resin particles, manufactured by Nippon Shokubai Co., Ltd., "Eposter") was applied to the surface of the transparent film 16 opposite to the surface on which the printed layer 14 was provided, i.e., the surface of the transparent film 16 that had been subjected to corona treatment, to form a coating film. The coating film was then dried for 90 seconds in a hot air dryer at 120°C to obtain a first B-stage layer (a resin coating layer 20 composed of a material containing a B-stage curable resin (melamine resin) and matte filler 18 (acrylic resin particles)).

[0105] As a result of the above, a laminate was obtained in which the printed layer 14, the transparent film 16, and the B-stage layer (the resin coat layer 20 containing the matte filler 18) were laminated together.

[0106] On the other hand, aluminum was evaporated onto the surface of a white polyvinyl chloride film (80 μm, resin film 12a) made of a material containing titanium oxide by resistance heating evaporation to form a metal evaporated layer 12b (thickness 0.1 μm), thereby obtaining a concealing layer 12.

[0107] Next, the printed layer 14 of the obtained laminate was laminated on the metal deposition layer 12b of the concealing layer 12, and the obtained laminate was heated and pressurized for 40 minutes at 140° C. and 2 MPa. This resulted in a decorative sheet 10 (melamine decorative sheet) of Example 1, in which a resin coating layer 20 (average thickness: 10.0 μm) made of a hard resin material, a transparent film 16 (thickness: 38.0 μm), a printed layer 14 (thickness: 3.0 μm), and a concealing layer 12 (thickness: 80.1 μm) were laminated in this order (see FIG. 1).

[0108] The average thickness (μm) of each layer was measured by observing the cross section using an electron microscope (manufactured by JEOL Ltd., “JSM-7401F”).

[0109] The surface of the resin coat layer 20 was formed as an uneven surface having protrusions 20a that conformed to the shape of the matte filler.

[0110] Example 2 The decorative sheet 10 of Example 2 was manufactured in the same manner as Example 1, except that the conditions for the corona treatment on the side of the transparent film 16 opposite the side on which the printed layer 14 was formed were changed so that the contact angle of pure water on the surface of the corona-treated side was set to 54.7°.

[0111] Comparative Example 1 The decorative sheet 10 of Comparative Example 1 was manufactured in the same manner as in Example 1, except that the corona treatment was omitted on the side of the transparent film 16 opposite the side on which the printed layer 14 was formed, and the contact angle of pure water on the surface on which the corona treatment was omitted was set to 68.0°.

[0112] 3. Evaluation The decorative sheets 10 of the respective Examples and Comparative Examples were evaluated by the following methods.

[0113] <Measurement of erosion rate of decorative sheet 10 by MSE method> First, under conditions of room temperature (25°C) x atmospheric pressure (1013 hPa), the decorative sheets 10 of the examples and comparative examples were arranged with the resin coating layer 20 on the upper side and the transparent film 16 on the lower side. Then, in this state, using an MSE testing device (Palmeso, "A203"), polygonal alumina particles having an average particle diameter D50 of 0.3 μm were projected onto the decorative sheet 10 from the resin coating layer 20 side from the upper side of the decorative sheet 10 (resin coating layer 20), with the projection direction being the vertical direction perpendicular to the decorative sheet 10, and the projection distance (separation distance) from the projection position to the surface of the resin coating layer 20 being 4.0 mm.

[0114] The polygonal alumina particles were projected by using a nozzle with a diameter of 1 mm to project an aqueous dispersion containing the polygonal alumina particles as fine particles onto the decorative sheet 10. The aqueous dispersion used was prepared by dispersing polygonal alumina particles with an average particle diameter D50 of 0.3 μm in purified water at a content of 1.0 mass %. The projection force of the polygonal alumina particles projected from the nozzle with a diameter of 1 mm onto the decorative sheet 10 was set to a magnitude that resulted in an erosion rate of 0.481 μm / g for the silicon wafer.

[0115] Furthermore, the erosion depth [μm], i.e., the depth from the surface of the resin coating layer 20 opposite the transparent film 16 to the projection site, was measured using a stylus-type surface profiler (manufactured by Palmeso, "PU-EU2") at the center of the position where the aqueous dispersion landed in a planar view of the decorative sheet 10.

[0116] At this time, the contact of the stylus surface profilometer had a tip R of 2.0 μm, and the load of the contact was set to 150 μN. The measurement conditions of the stylus surface profilometer using this contact were set to measurement magnification: 10,000 times, measurement length: 3.0 mm, and measurement speed: 0.2 mm / sec. The erosion rate [μm / g] was calculated based on the measured erosion depth [μm] and the amount of projected particles [g] required to reach this erosion depth [μm].

[0117] For the erosion rate [μm / g] obtained as described above, an erosion rate distribution graph was created showing the relationship between the erosion rate and the erosion depth, with the erosion rate [μm / g] on the y-axis and the erosion depth [μm] on the x-axis. In this erosion rate distribution graph, the erosion depth [μm] in the region a (interface) located between the resin coating layer 20 and the transparent film 16 and the erosion rate [μm / g] measured at this erosion depth [μm] were linearly approximated to a straight line using the least squares method, and the slope of this straight line (approximation line) was obtained.

[0118] <Evaluation of durability of decorative sheet 10 against temperature changes> For each of the decorative sheets 10 in the examples and comparative examples, a durability test was conducted in which the sheets were placed under conditions of 60°C and 90% RH for 3 hours, followed by placing them under conditions of -10°C for 3 hours, with this cycle being repeated up to 61 times.

[0119] In this durability test, the appearance (presence or absence of cracks) and the presence or absence of peeling of the resin coating layer 20 were visually inspected after 20 cycles, 35 cycles, 45 cycles, and 61 cycles, and the results were evaluated according to the following evaluation criteria.

[0120] Evaluation criteria In the decorative sheet 10 after each cycle, A: Neither the occurrence of cracks nor peeling of the resin coating layer 20 is observed. B: Only cracks were observed, but there was no problem with use as a decorative sheet. C: Clear cracks were observed, affecting use as a decorative sheet. D: Both cracking and peeling of the resin coating layer 20 were observed. It is clearly not suitable for use as a decorative sheet.

[0121] The evaluation results of the decorative sheets 10 of the examples and comparative examples obtained as described above are shown in the following Table 1 and Fig. 2. Fig. 2 is an erosion rate distribution graph showing the relationship between the erosion rate and the erosion depth in the decorative sheets of Example 1 and Comparative Example 1.

[0122] [Table 1]

[0123] As shown in Table 1 and FIG. 2, in Examples 1 and 2, the magnitude of the slope in the region a in the erosion rate distribution graph, which is located between the resin coating layer 20 and the transparent film 16, is greater than or equal to -1.0 / g and less than or equal to 0.0 / g, i.e., requirement A is satisfied. As a result, it was shown that the occurrence of cracks or peeling in the resin coating layer 20 due to temperature changes can be appropriately suppressed or prevented.

[0124] In contrast, in Comparative Example 1, the magnitude of the slope in the region a was greater than -1.0 / g and less than 0.0 / g, i.e., requirement A was not satisfied, and therefore it became clear that cracks and peeling would occur in the resin coating layer 20 due to temperature changes. [Explanation of symbols]

[0125] 10 Decorative Sheet 12 Hidden Layer 12a Resin film 12b Metal evaporated layer 14 Printing layer 16 Transparent Film 18 Matte Filler 20 Resin Coating Layer 20a Convex part a) Region between the resin coating layer and the transparent film< / d> < / c>

Claims

1. A printing layer; A transparent film and and a resin coating layer, which are laminated in this order; A decorative sheet characterized in that the resin coating layer and the transparent film contain a first resin material and a second resin material, respectively, and satisfy the following requirement A. Requirement A: When the decorative sheet is subjected to a microslurry jet erosion method in which polygonal alumina particles having an average particle diameter D50 of 0.3 μm are projected onto the decorative sheet from the resin coating layer side with a projection force that results in an erosion rate of 0.481 μm / g for a silicon wafer, and the erosion rate [μm / g] in the thickness direction of the decorative sheet at the position where the polygonal alumina particles were projected is measured, the magnitude of the slope in the region located between the resin coating layer and the transparent film in an erosion rate distribution graph showing the relationship between the erosion rate and the erosion depth, with the erosion rate [μm / g] on the y-axis and the erosion depth [μm], which is the position in the thickness direction showing the erosion rate, on the x-axis, is -1.0 / g or more and 0.0 / g or less.

2. The decorative sheet according to claim 1 , wherein the transparent film contains polyethylene terephthalate as the second resin material.

3. The decorative sheet according to claim 1 , wherein the resin coat layer contains a melamine-based resin as the first resin material.

4. 4. The decorative sheet according to claim 3, wherein the resin coating layer has an average thickness of 5.0 μm or more and 30.0 μm or less.

5. 2. The decorative sheet according to claim 1, wherein said resin coat further contains a matte filler, and the surface thereof is configured as an uneven surface having protrusions following the shape of said matte filler.

6. 6. The decorative sheet according to claim 5, wherein said matte filler contains at least one of an acrylic resin, a melamine resin, a polystyrene resin, and silica.

7. 6. The decorative sheet according to claim 5, wherein the resin coating layer has a content of the matte filler of 10% by volume or more and 50% by volume or less.

8. 6. The decorative sheet according to claim 5, wherein the matte filler has a median diameter (D50) of 7.0 μm or more and 50.0 μm or less.

9. The decorative sheet according to claim 1 , wherein the laminate further comprises a concealing layer laminated on the side of the printed layer opposite the transparent film.