Manufacturing method of iii nitride semiconductor

A method for manufacturing Group III nitride semiconductors through controlled temperature and growth rate stages addresses the challenges of AlN film growth, resulting in high-quality UVC LEDs with reduced dislocation density and lower production costs.

JP2024155681APending Publication Date: 2024-10-31TOYODA GOSEI CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023176099
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-10-11
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The growth of high-quality AlN films is challenging due to high melting point and high N dissociation vapor pressure, leading to poor atomic migration and three-dimensional growth, which is not compatible with general growth equipment, requiring high-temperature equipment that accelerates component deterioration and increases costs.

Method used

A method involving a crystal nucleus layer formation at a lower temperature, followed by low-temperature three-dimensional growth and high-temperature three-dimensional growth, culminating in a two-dimensional growth layer, using controlled temperature and growth rates to form a high-quality Group III nitride semiconductor.

Benefits of technology

This approach allows for the production of high-quality Group III nitride semiconductors suitable for UVC LEDs, reducing threading dislocation density and enabling the use of standard growth equipment, thereby lowering costs and improving yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155681000001_ABST
    Figure 2024155681000001_ABST
Patent Text Reader

Abstract

To provide a III nitride semiconductor with a high quality.SOLUTION: A manufacturing method of a III nitride semiconductor, includes: a crystalline nucleus layer formation step of generating a nucleus 11A of GaN, AlGaN, or AlN onto a sapphire substrate to form a crystalline nucleus layer 11; a low-temperature three-dimensional growing layer formation step of combining crystals from adjacent nuclei 11A by growing AlGaN or AlN from the nucleus 11A at a temperature that is lower than that in the crystalline nucleus layer formation step, and forming a low-temperature three-dimensional growing layer 12A; and a high-temperature three-dimensional growing layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growing layer 12A under a temperature that is higher than that in the low-temperature three-dimensional growing layer formation step, and equal to or lower than that in the crystalline nucleus layer formation step, and forming a high-temperature three-dimensional growing layer 12B.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a Group III nitride semiconductor. [Background technology]

[0002] The ultraviolet wavelength of solid-state light-emitting devices using III-nitride semiconductors corresponds to a wavelength band of approximately 210 to 400 nm. In particular, UVC (wavelength 100 to 280 nm) is known to be effective for sterilization and disinfection, and there is a growing demand for III-nitride semiconductor LEDs that emit ultraviolet light with an emission wavelength corresponding to UVC. Ultraviolet LEDs are configured by forming an AlN layer on a sapphire substrate, and then laminating an n-type layer, light-emitting layer, and p-type layer made of AlGaN on the AlN layer.

[0003] In Non-Patent Document 1, Ga is doped into AlN to produce high-quality Al 0.99 Ga 0.01 It is described that N can be deposited as a film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-154964 A [Patent Document 2] Special Publication No. 2012-522388 [Patent Document 3] JP 2005-72409 A [Patent Document 4] JP 2016-157951 A [Non-patent literature]

[0005] [Non-Patent Document 1] Jpn. J. Appl. Phys. 56 015504 2017 Summary of the Invention [Problem to be solved by the invention]

[0006] AlN is a material with a high melting point and high dissociation vapor pressure of N. At the GaN growth temperature range of 1000 to 1200°C, the migration of atoms during crystal growth is poor, resulting in three-dimensional growth and making it difficult to form a flat crystal surface. In addition, TMAl (trimethylaluminum), the Al source gas, is highly reactive, and TMAl decomposes and reacts to form compounds before reaching the substrate, reducing the raw material concentration that can contribute to crystal growth and making the raw material efficiency worse. For these reasons, growth is performed under reduced pressure, and generally, nuclei are grown at a low temperature of about 1000°C, followed by three-dimensional growth of AlN at about 1200°C, and then AlN is grown and flattened at a high temperature of 1300°C or higher.

[0007] However, general growth equipment cannot withstand such high temperatures, so it is necessary to use growth equipment that can withstand high temperatures. For example, a high-output heating device or an efficient cooling device is required, and the equipment must be made of materials that do not decompose or soften even at high temperatures. High temperatures also accelerate the deterioration of materials. For example, the deterioration of heater materials, susceptors, vacuum packing, etc. is significant. This results in increased running costs.

[0008] Therefore, there was a need for a technology that could deposit high-quality AlN films within the temperature range that could be handled by conventional growth equipment.

[0009] The present invention has been made in view of the above background, and aims to provide a method for producing a high-quality Group III nitride semiconductor. [Means for solving the problem]

[0010] One aspect of the present invention is a crystal nucleation layer formation step of generating nuclei of GaN, AlGaN or AlN on a sapphire substrate to form a crystal nucleation layer; a low-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the nuclei at a temperature lower than that of the crystal nucleus layer formation step, and combining crystals from adjacent nuclei to form a low-temperature three-dimensional growth layer; and a high-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growth layer at a temperature higher than that of the low-temperature three-dimensional growth layer formation step and equal to or lower than the temperature of the crystal nucleus layer formation step to form a high-temperature three-dimensional growth layer.

[0011] Another aspect of the present invention is a crystal nucleation layer formation step of generating nuclei of GaN, AlGaN or AlN on a sapphire substrate to form a crystal nucleation layer; a low-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the nuclei at a growth rate slower than that of the crystal nucleus layer, and merging crystals from adjacent nuclei to form a low-temperature three-dimensional growth layer; and a high-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growth layer at a growth rate that is faster than the low-temperature three-dimensional growth layer and equal to or lower than the growth rate of the crystal nucleus layer to form a high-temperature three-dimensional growth layer. Effect of the Invention

[0012] According to one aspect of the present invention, nuclei of GaN, AlGaN or AlN are generated to form a crystal nucleation layer, and then the temperature is lowered to grow and combine AlGaN or AlN from the nuclei to form a low-temperature three-dimensional growth layer, and then the temperature is raised, thereby making it possible to obtain a high-quality Group III nitride semiconductor. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram showing the configuration of a light-emitting element according to a first embodiment. [Diagram 2] Schematic diagram showing the structure of an AlN layer. [Diagram 3] Schematic diagram showing substrate warpage at each growth stage. [Figure 4] A graph showing the change in temperature and pressure over time when forming an AlN layer. [Diagram 5] AFM images of the surface of each AlN layer. [Figure 6]TEM image showing a cross section of the AlN layer in a direction perpendicular to the main substrate surface. [Figure 7] Graph showing the change in temperature over time when forming an AlN layer. [Figure 8] 1 is a graph showing the change in wafer curvature over time. [Figure 9] 13 is a graph showing the change in temperature over time during the formation of an AlN layer in a comparative example. [Figure 10] 13 is a graph showing the change over time in the curvature of a wafer in a comparative example. [Figure 11] AFM image of the surface of the p-type layer in the deformed morphology. [Figure 12] Graph showing the relationship between the vapor ratio of TMGa and the X-ray half-width of the two-dimensionally grown layer. [Figure 13] Graph showing the a-axis and c-axis values ​​of an AlN layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The method for manufacturing a Group III nitride semiconductor includes a crystal nucleus layer formation step of generating nuclei of GaN, AlGaN or AlN on a sapphire substrate to form a crystal nucleus layer, a low-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the nuclei at a temperature lower than that of the crystal nucleus layer formation step to combine crystals from adjacent nuclei to form a low-temperature three-dimensional growth layer, and a high-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growth layer at a temperature higher than that of the low-temperature three-dimensional growth layer formation step but not higher than the temperature of the crystal nucleus layer formation step to form a high-temperature three-dimensional growth layer.

[0015] The temperature in the crystal nucleus layer formation step may be 1100°C or more and 1200°C or less, the temperature in the low-temperature three-dimensional growth layer formation step may be 900°C or more and 1100°C or less, and the temperature in the high-temperature three-dimensional growth layer formation step may be 1050°C or more and 1200°C or less.

[0016] After the high-temperature three-dimensional growth layer formation step, a two-dimensional growth layer may be formed by growing AlGaN or Ga-doped AlN from the high-temperature three-dimensional growth layer at a temperature equal to or higher than that of the high-temperature three-dimensional growth layer formation step. In this two-dimensional growth layer formation step, the supply amount of Ga may be changed over time. For example, the supply amount is increased from a low supply amount to a high supply amount.

[0017] The temperature in the two-dimensional growth layer forming step may be 1100° C. or more and 1200° C. or less.

[0018] In addition, a method for producing a Group III nitride semiconductor includes a crystal nucleus layer formation step of generating nuclei of GaN, AlGaN or AlN on a sapphire substrate to form a crystal nucleus layer, a low-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the nuclei at a growth rate slower than that of the crystal nucleus layer to combine crystals from adjacent nuclei to form a low-temperature three-dimensional growth layer, and a high-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growth layer at a growth rate faster than that of the low-temperature three-dimensional growth layer but not higher than the growth rate of the crystal nucleus layer to form a high-temperature three-dimensional growth layer.

[0019] The growth rate of the crystal nucleus layer may be 5 nm / min or more and 100 nm / min or less, the growth rate of the low-temperature three-dimensional growth layer may be 2 nm / min or more and 20 nm / min or less, and the growth rate of the high-temperature three-dimensional growth layer may be 5 nm / min or more and 50 nm / min or less.

[0020] The method may further include a two-dimensional growth layer formation step of growing AlGaN or Ga-doped AlN from the high-temperature three-dimensional growth layer at a growth rate equal to or faster than the high-temperature three-dimensional growth layer after the high-temperature three-dimensional growth layer formation step, and the supply amount of Ga may be increased over time in the two-dimensional growth layer formation step.

[0021] The growth rate in the two-dimensional growth layer formation step may be 5 nm / min or more and 50 nm / min or less.

[0022] The crystal nucleus layer forming step may be preceded by a thermal cleaning step of heat-treating the sapphire substrate in a hydrogen-dominated atmosphere at a temperature higher than that in the crystal nucleus layer forming step.

[0023] The core may be AlGaN having an Al composition of 60 to 98%.

[0024] The curvature of the wafer at the end of the two-dimensional growth layer is 50 km. -1 More than 300km -1 It may be the following.

[0025] (Embodiment 1) 1. Structure of the light-emitting element Fig. 1 is a diagram showing the configuration of a light-emitting element according to embodiment 1. As shown in Fig. 1, the light-emitting element according to embodiment 1 has a substrate 10, a crystal nucleus layer 11, a three-dimensional growth layer 12, a two-dimensional growth layer 13, an n-type layer 14, an active layer 15, an electron blocking layer 16, a p-type layer 17, a p-electrode 18, and an n-electrode 19. The light-emitting element according to embodiment 1 is of a flip-chip type, and emits light in the UVC band.

[0026] The substrate 10 is a substrate made of sapphire with a c-plane as the main surface. The plane orientation of the main surface of the sapphire may be an a-plane. Sapphire substrates are large in diameter, low in cost, and transparent to light ranging from deep ultraviolet to visible light in general, and therefore are widely used as substrates for nitride semiconductors and light-emitting devices thereof. In addition, the substrate has an off-angle of 0.1 to 2 degrees in the m-axis or a-axis direction. An anti-reflection film may be provided on the back surface of the substrate 10 (the surface opposite to the crystal nucleus layer 11) to improve the light extraction efficiency. In addition, the surface of the substrate 10 may be provided with irregularities to improve the light extraction efficiency.

[0027] The crystal nucleus layer 11 is located on the substrate 10. The crystal nucleus layer 11 is a layer formed by generating nuclei 11A made of AlN on the surface of the substrate 10 and allowing them to grow three-dimensionally.

[0028] The thickness of the crystal nucleus layer 11 (height of the nuclei 11A) is preferably 1 to 200 nm. If the thickness of the crystal nucleus layer 11 is in this range, the nuclei 11A are sufficiently large, and the quality of the crystal layer formed after the nuclei 11A can be improved. The thickness of the crystal nucleus layer 11 is more preferably 2 to 40 nm, and even more preferably 3 to 30 nm. Since the nuclei 11A are sufficiently large, the density of the nuclei 11A is low. For example, when the thickness of the crystal nucleus layer 11 is in the range of 5 to 100 nm, the density of the nuclei 11A is 3×10 11 / cm -2 It is preferable that:

[0029] The size of the nuclei 11A (average diameter in plan view) is preferably 20 to 50 nm. Here, the diameter is the diameter when the nuclei 11A is converted into a circle of the same area. Also, this is the size of the nuclei 11A when the thickness of the crystal nucleus layer 11 is 5 to 100 nm. By setting the size of the nuclei 11A within this range, the tensile stress can be sufficiently reduced. Also, the variation in size of the nuclei 11A (the difference between the maximum diameter and the average diameter, and the difference between the average diameter and the minimum diameter) is preferably 10 nm or less.

[0030] It is important that the nuclei 11A are large. When the crystal nuclei combine to form a flat film, tensile stress is generated on the surface. Therefore, if the nuclei size is small and the density is high, the stress generated on the surface when they combine to form a flat film is also large. Therefore, it is necessary to reduce the nuclei density. To achieve this, it is effective to increase the nuclei size.

[0031] A low nucleus density has another advantage. Threading dislocations are formed at the interface where the nuclei 11A join together. A low nucleus density also reduces the number of interfaces where the nuclei 11A join together. Therefore, by reducing the nucleus density, it is possible to reduce the formation of threading dislocations, and a high-quality crystal film can be formed.

[0032] The three-dimensional growth layer 12 is located on the crystal nucleus layer 11. The three-dimensional growth layer 12 is made of AlN. The three-dimensional growth layer 12 is a layer in which the nuclei 11A are three-dimensionally grown to combine adjacent nuclei 11A, and the combined AlN is further grown three-dimensionally. The three-dimensional growth layer 12 is a laminate of a low-temperature three-dimensional growth layer 12A and a high-temperature three-dimensional growth layer 12B. The high-temperature three-dimensional growth layer 12B is a layer grown at a higher temperature than the low-temperature three-dimensional growth layer 12A. By combining the nuclei 11A three-dimensionally, rather than growing them into a two-dimensional flat film at once, the stress generated on the surface can be alleviated.

[0033] In the surface of the low-temperature three-dimensionally grown layer 12A, the ratio of flat crystal planes parallel to the main surface of the substrate 10 is preferably smaller than the ratio of obliquely inclined crystal planes. The obliquely inclined planes may be formed of low-order or high-order facet planes, such as {10-11} planes or {11-22} planes.

[0034] The thickness of the low-temperature three-dimensionally grown layer 12A is preferably 100 to 500 nm. Within this range, the nuclei 11A can be sufficiently combined to reduce the dislocation density. The surface roughness RMS of the low-temperature three-dimensionally grown layer 12A is, for example, 10 to 100 nm. The thickness of the low-temperature three-dimensionally grown layer 12A is more preferably 250 to 400 nm, and further preferably 250 to 350 nm.

[0035] In the surface of the high-temperature three-dimensionally grown layer 12B, the proportion of flat crystal planes parallel to the main surface of the substrate 10 is preferably greater than the proportion of obliquely inclined crystal planes. In other words, the high-temperature three-dimensionally grown layer 12B is a flatter film than the low-temperature three-dimensionally grown layer 12A.

[0036] The high-temperature three-dimensional growth layer 12B has a thickness of 750 to 2000 nm. With such a thickness, the nucleus 11A and the low-temperature three-dimensional growth layer 12A can be sufficiently combined without gaps, and the dislocation density can be reduced. The high-temperature three-dimensional growth layer 12B has a more preferable thickness of 1000 to 1750 nm, and further preferably 1250 to 1500 nm.

[0037] Note that voids may be present in the crystals of the crystal nucleus layer 11 and the three-dimensional growth layer 12. The voids are regions that could not be filled by the growth of the nuclei 11A, and are spaces in the crystals filled with carrier gas. The voids can relieve the stress remaining in the film and suppress the occurrence of cracks.

[0038] The two-dimensional growth layer 13 is located on the three-dimensional growth layer 12. The two-dimensional growth layer 13 is a layer in which AlN is grown while Ga is being supplied. The two-dimensional growth layer 13 is made of AlN or AlGaN containing Ga. Ga is supplied as a surfactant that promotes lateral growth during AlN film formation. In order to exert the surfactant effect, the molar ratio of Ga to Al in the formed AlN film needs to be greater than 0. Due to the surfactant effect, the surface of the two-dimensional growth layer 13 is a two-dimensionally flat surface without unevenness due to pits or crystal facets.

[0039] AlN containing Ga is AlN in a state where Ga is dissolved in solid solution, and is AlN containing Ga to such an extent that it does not form a mixed crystal of GaN and AlN. For example, the molar ratio of Ga to Al in the two-dimensional growth layer 13 is greater than 0 and is 0.5% or less.

[0040] The surfactant effect of Ga is also exerted when the Ga content of AlN increases to a level at which a mixed crystal of AlN and GaN (AlGaN) is formed. The level at which a mixed crystal is formed is when the molar ratio of Ga to Al is greater than 0.5%. On the other hand, if the Ga composition of AlGaN becomes too high, there is a high possibility that ultraviolet light from the active layer 15 will be absorbed. Therefore, when the two-dimensionally grown layer 13 is made of AlGaN, it is preferable that the Ga composition be greater than 0.5% and equal to or less than 10%.

[0041] The Ga supply amount in the two-dimensional growth layer 13 may vary in the thickness direction, and may increase continuously or stepwise as it moves away from the substrate 10. The back side region of the two-dimensional growth layer 13 (the three-dimensional growth layer 12 side) is in a state where Ga is dissolved in AlN, and the front side is in a mixed crystal state of AlN and GaN (i.e., Al 1-x Ga xN) and Al. 1-x Ga x The Ga composition x of N also changes in the thickness direction, and increases continuously or stepwise from 0 to a predetermined value with increasing distance from the substrate 10. The maximum value of the Ga composition x (i.e., the Ga composition x near the surface of the two-dimensionally grown layer 13) is 0.01 to 0.1.

[0042] In this way, the surface vicinity of the two-dimensional growth layer 13 is not AlN but a mixed crystal of AlN and GaN, but the Ga composition x is low enough to allow it to function equivalently to AlN as an underlayer for deep ultraviolet light emitting devices. In addition, the two-dimensional growth layer 13 is flat, has few cracks, and has a low dislocation density. By continuously increasing the Ga ratio, the lattice mismatch with the n-type layer 14 (n-type AlGaN layer) laminated thereon also becomes smaller, which contributes to improving the crystal quality of the n-type layer 14.

[0043] The thickness of the two-dimensional growth layer 13 is 750 to 2000 nm. With such a thickness, the surface of the two-dimensional growth layer 13 is sufficiently flattened. For example, the surface roughness RMS of the two-dimensional growth layer 13 can be set to 0.5 to 5 nm. Step bunching may be present on the surface of the two-dimensional growth layer 13. The thickness of the two-dimensional growth layer 13 is more preferably 1000 to 1750 nm, and further preferably 1250 to 1500 nm.

[0044] The threading dislocation density of the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13 is lower than the threading dislocation density of the crystal nucleus layer 11 and the low-temperature three-dimensional growth layer 12A. The threading dislocation density of the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13 is, for example, 5×10 9 cm -2 The threading dislocation density of the crystal nucleus layer 11 and the low-temperature three-dimensional growth layer 12A is, for example, 1×10 10 cm -2 That's all.

[0045] In addition, the dislocation density of dislocations having an edge dislocation component in the two-dimensionally grown layer 13 is higher than the dislocation density of dislocations having a screw dislocation component. For example, the dislocation density of dislocations having an edge dislocation component is 10 times or more higher.

[0046] In the X-ray diffraction pattern of the two-dimensionally grown layer 13, the full width at half maximum (FWHM) of the (002) diffraction line is, for example, 20 to 200 arcsec, and the full width at half maximum of the (102) diffraction line is, for example, 200 to 800 arcsec.

[0047] The n-type layer 14 is located on the two-dimensionally grown layer 13. The n-type layer 14 is made of n-AlGaN and has a Ga composition higher than the Ga composition of the two-dimensionally grown layer 13. The n-type impurity is Si, and the Si concentration is 5×10 18 ~5×10 19 / cm 3 The n-type layer 14 may be composed of multiple layers.

[0048] The active layer 15 is located on the n-type layer 14. The active layer 15 has an MQW structure in which well layers and barrier layers are alternately and repeatedly stacked. The number of repetitions is, for example, 2 to 5. The well layers are made of AlGaN, and the Al composition is set according to the desired emission wavelength. The barrier layers are AlGaN with a higher Al composition than the well layers. They may also be AlGaInN with a higher band gap energy than the well layers. The active layer 15 may also have an SQW structure.

[0049] The electron blocking layer 16 is located on the active layer 15. The electron blocking layer 16 is made of AlGaN or AlN having a higher Al composition ratio than the barrier layer of the active layer 15. The electron blocking layer 16 may be doped with an impurity to provide p-type. The doping method may be constant or modulated, or may be combined with a non-doped layer. The electron blocking layer 16 prevents electrons injected from the n-electrode 19 from diffusing beyond the active layer 15 toward the p-type layer 17.

[0050] The p-type layer 17 is located on the electron blocking layer 16. The p-type layer 17 is made of p-AlGaN. In the light emitting device of the first embodiment, all the semiconductor layers from the n-type layer 14 to the p-type layer 17 are made of AlGaN, which suppresses the absorption of ultraviolet light emitted from the active layer 15 by the semiconductor layers. The p-type impurity is Mg. The Mg concentration is 1×10 18 / cm 3 That is all. P-type layer 17 may be composed of multiple layers with different Al compositions or Mg concentrations. In that case, the layer in contact with p-electrode 18 may be p-GaN to reduce contact resistance.

[0051] The lowest Al composition in the p-type layer 17 is preferably an Al composition having a band gap that does not absorb the emission wavelength emitted from the active layer 15. For example, if the Al composition of the well layer of the active layer 15 is 40%, the lowest Al composition in the p-type layer 17 is preferably 40% or more. However, since a high Al composition increases the contact resistance with the p-electrode 18, a layer with a composition of 0 to 40% may be laminated as a contact layer in a thin layer in the range of 1 to 50 nm. The layer with a composition of 0 to 40% absorbs the ultraviolet light emitted from the active layer 15, but transmits it to some extent because it is thin. Therefore, a large decrease in the external quantum efficiency of the LED can be avoided.

[0052] Furthermore, layers may be combined in a range of Al composition of 0 to 90%. In that case, it is preferable that the Al composition is set to decrease continuously or stepwise from the active layer 15 side. A superlattice structure may be formed, and the average Al composition may decrease stepwise.

[0053] A groove is provided in a partial area of ​​the surface of the p-type layer 17, the depth of which reaches the n-type layer 14. This groove is for exposing the n-type layer 14 so that an n-electrode 19 can be provided therein.

[0054] The p-electrode 18 is provided on the p-type layer 17. The p-electrode 18 is a reflective electrode that reflects ultraviolet light emitted from the active layer 15 toward the substrate 10 to improve the light extraction efficiency. The material of the p-electrode 18 is Ru, Rh, Ni / Au, Ni / Al, or the like.

[0055] The n-electrode 19 is provided on the n-type layer 14 exposed at the bottom surface of the groove. The material of the n-electrode 19 is Ti / Al, V / Al, or the like.

[0056] 2. Light-emitting device manufacturing method Next, a description will be given of a manufacturing method of the light emitting device according to embodiment 1. The group III nitride semiconductor is formed by MOCVD, and the source gases used are, for example, ammonia as the nitrogen source gas, TMGa (trimethylgallium) or TEGa (triethylgallium) as the Ga source gas, and TMAl (trimethylaluminum) as the Al source gas, and hydrogen or nitrogen as the carrier gas.

[0057] In the following description of the manufacturing method, appropriate reference will be made to Figures 2 to 4. Figure 2 is a diagram showing a schematic diagram of the configuration of each layer at each growth stage up to the formation of the two-dimensionally grown layer 13.

[0058] FIG. 3 is a diagram conceptually showing the warpage of the wafer at each growth stage up to the formation of the two-dimensional growth layer 13. Note that the warpage of the wafer may also occur in a bulk substrate on which nothing is grown. This is because the surface of the substrate 10 is cooled by a carrier gas such as hydrogen, and therefore the temperature is strictly different from that of the back side of the substrate 10, and warpage may occur due to the difference in thermal expansion caused by the temperature difference. Therefore, the depiction of the warpage in FIG. 3 is a conceptual depiction of the behavior caused by the difference in lattice mismatch and thermal expansion coefficient when different materials are laminated, and may be slightly different from the state of warpage that actually occurs. Therefore, FIG. 3 is a conceptual depiction of the stress generated in the film by the lamination of layers and the resulting warpage.

[0059] FIG. 4 is a graph showing the change over time in the growth temperature and the growth pressure until the two-dimensionally grown layer 13 is formed.

[0060] 2-1. Thermal cleaning First, a substrate 10 made of c-plane sapphire is prepared and thermally cleaned in a hydrogen atmosphere at a temperature of 1150 to 1250°C for 1 second to 15 minutes. This removes impurities from the surface of the substrate 10 and flattens it (see Fig. 2(a), Fig. 3(a), and Fig. 4). In Fig. 4, the growth temperature is 1190°C and the pressure is 4 kPa as an example. Also in Fig. 4, the period between this thermal cleaning and the nitridation process in the next step is shown as period T1. It is believed that this thermal cleaning removes oxygen from the surface of the substrate 10, resulting in an Al-rich surface.

[0061] The temperature of the thermal cleaning may be higher than that of the crystal nucleus layer forming step described later. The temperature of the thermal cleaning may be more preferably in the range of 1170 to 1230°C, and even more preferably in the range of 1180 to 1210°C. The atmosphere may be dominated by hydrogen, for example, a mixed gas containing 80% or more by volume of hydrogen. The mixed gas may be, for example, a mixed gas of hydrogen and nitrogen. The pressure may be normal pressure, but reduced pressure is preferable, for example, 1 to 80 kPa, preferably 1 to 50 kPa, and even more preferably 1 to 20 kPa. The flow rate of the hydrogen gas or the mixed gas of hydrogen and nitrogen on the substrate 10 may be 5 to 500 m / min (meters / minute), preferably 10 to 300 m / min, and even more preferably 15 to 150 m / min.

[0062] 2-2. Nitriding Next, the temperature is lowered than that of the thermal cleaning, and ammonia is supplied to nitride the Al-rich surface of the substrate 10. The pressure is the same as that of the thermal cleaning. It is preferable that the flow rate of the carrier gas (hydrogen or a mixed gas of hydrogen and nitrogen) is the same as or higher than the optimal range of the thermal cleaning. The flow rate of ammonia is the same as or lower than that of the next process, and the ammonia partial pressure in the carrier gas, which is hydrogen or a mixed gas of hydrogen and nitrogen, is preferably in the range of 0.001 to 0.1 atm, more preferably 0.01 to 0.05 atm. The time of the nitriding process is 0.5 seconds to 10 minutes, more preferably 60 to 300 seconds. An AlN layer (not shown) of one monolayer to several monolayers, which serves as the starting point of nucleation, is formed on the surface of the substrate 10.

[0063] 2-3. Crystal nucleus layer 11 formation process Next, nitrogen source gas and Al source gas are supplied at the same temperature as the nitriding process in the previous step or at a lower temperature than the nitriding process in the previous step, AlN nuclei 11A are generated on the substrate 10, and the nuclei 11A are three-dimensionally grown to form the crystal nucleus layer 11 (see FIG. 2(b) and FIG. 4). In FIG. 4, the period of this step is shown as period T2, and the case of a temperature of 1155°C is shown as an example. The pressure is the same as in the previous step. Conventionally, the nuclei 11A are generated at about 1000°C and three-dimensionally grown, but in the first embodiment, the temperature is set higher than this to enhance the surface migration of the source atoms and form the nuclei 11A larger than conventionally. This makes it possible to achieve high quality of the nuclei 11A made of AlN.

[0064] The lattice mismatch between the nuclei 11A and the substrate 10 made of sapphire causes compressive stress in the crystal nucleus layer 11. However, because the lattice mismatch between the nuclei 11A and the substrate 10 is large, the stress is relieved within a few nm, and the stress at the interface between the substrate 10 and the nuclei 11A is small.

[0065] The crystal nucleus layer 11 is preferably grown three-dimensionally until it has a thickness of 1 to 200 nm, which allows the nuclei 11A to be sufficiently large. The size and density of the nuclei 11A are preferably within the above-mentioned ranges.

[0066] The preferred growth temperature for the crystal nucleus layer 11 is 1100 to 1200°C. By setting the temperature within this range, the nuclei 11A can be made sufficiently large. This is because the surface migration of the raw material atoms can be enhanced. More preferably, it is 1125 to 1190°C, and even more preferably, it is 1150 to 1180°C. It may be the same temperature as that of the previous nitriding process. By making the nuclei 11A larger, the nucleus density is reduced. Therefore, the interface between the nuclei 11A is also reduced. Tensile stress may occur in the film when the nuclei 11A combine and become flat, but by reducing the nucleus density as described above, the stress that occurs after the nuclei 11A combine can be reduced.

[0067] The growth temperature of the crystal nucleus layer 11 may be changed stepwise or continuously. In this case, the average growth temperature may be 1100 to 1200°C.

[0068] The growth rate is preferably 5 to 100 nm / min. By increasing the growth rate, the diameter of the nuclei 11A can be increased. The growth rate is more preferably 10 to 70 nm / min, and further preferably 20 to 50 nm / min.

[0069] The V / III ratio is preferably 5 to 500. By setting the V / III ratio in this range, the growth rate can be controlled within the above range. It is more preferably 5 to 400, and further preferably 5 to 300.

[0070] Although there is a possibility that -c-plane AlN is formed on the nitrided substrate 10, it can be made into a +c-plane by controlling the growth conditions such as a low V / III ratio of the nuclei 11A and a high growth rate. A crystal layer with a +c plane is usually preferable, and even if +c and -c are mixed in the crystal nucleus layer 11, the proportion of -c is small, and +c becomes dominant during the growth process, so that a crystal layer having only a +c-plane surface is finally formed.

[0071] 2-4. Low temperature three-dimensional growth layer 12A formation process When the crystal nucleus layer 11 grows to a predetermined thickness, the growth temperature is lowered to be lower than that in the formation process of the crystal nucleus layer 11 (period T2). This causes the nuclei 11A of the crystal nucleus layer 11 to grow three-dimensionally, and adjacent nuclei 11A are united to form a low-temperature three-dimensionally grown layer 12A (see FIG. 2(c) and FIG. 4). In FIG. 4, the period of this process is shown as period T3, and a case of a temperature of 975°C is shown as an example. The pressure is the same as in the previous process. By uniting the nuclei 11A, threading dislocations can be reduced, and a high-quality low-temperature three-dimensionally grown layer 12A can be formed.

[0072] Here, because the temperature is lower than the formation temperature of the nuclei 11A, the stress acting on the layers up to the low-temperature three-dimensional growth layer 12A becomes compressive stress due to the difference in linear expansion coefficient with the substrate 10 (see FIG. 3(b)). Generally, cracks occur in the growth layer when tensile stress is applied. Since compressive strain occurs in the layers up to the low-temperature three-dimensional growth layer 12A, cracks can be suppressed.

[0073] Furthermore, by lowering the temperature, the low-temperature three-dimensional growth layer 12A can be grown slowly, and the coalescence of the low-temperature three-dimensional growth layer 12A growing from the nuclei 11A can also proceed slowly. Tensile stress may occur when the nuclei 11A coalesce, but since the low-temperature three-dimensional growth layer 12A is grown slowly as described above, cracks due to tensile stress that occur when the low-temperature three-dimensional growth layer 12A on the nuclei 11A coalesce to become a continuous film can also be suppressed.

[0074] The low-temperature three-dimensional growth layer 12A is preferably grown thicker than the crystal nucleus layer 11, for example, until the thickness reaches 200 to 500 nm. By sufficiently merging the nucleus 11A as a starting point so that the nucleus shape changes to a film shape, the threading dislocation density can be reduced. Furthermore, the thicker the low-temperature three-dimensional growth layer 12A is, the more uneven the three-dimensional surface can be. This makes it possible to reduce the threading dislocations that propagate to the growth layer surface by bending the threading dislocations due to the lateral growth promoted in the next and subsequent steps. The thickness is more preferably 250 to 400 nm, and even more preferably 250 to 350 nm.

[0075] The growth temperature of the low-temperature three-dimensionally grown layer 12A is preferably 900 to 1100° C. By setting the temperature at 900° C. or higher, impurities are less likely to enter the crystal, and light absorption can be reduced. The growth temperature is more preferably 950 to 1050° C., and further preferably 975 to 1025° C.

[0076] The growth rate of the low-temperature three-dimensional growth layer 12A is set to be slower than that of the crystal nucleus layer 11. By slowing down the growth rate and slowly coalescing starting from the nuclei 11A, dislocations can be efficiently reduced. In addition, the formation of tensile stress that occurs when planarizing due to the coalescence of the nuclei 11A can be alleviated. The growth rate is preferably 2 to 20 nm / min, more preferably 2 to 15 nm / min, and even more preferably 2 to 10 nm / min.

[0077] The V / III ratio of the low-temperature three-dimensional growth layer 12A is set to be larger than that of the crystal nucleus layer 11, and is preferably set to 500 to 2000. The growth rate can be controlled within the above range, more preferably 750 to 1750, and further preferably 1000 to 1500.

[0078] 2-5. High temperature three-dimensional growth layer 12B formation process When the low-temperature three-dimensional growth layer 12A, which has grown from the nuclei 11A as starting points, is sufficiently united and grows to a predetermined thickness, the growth temperature is set higher than that of the low-temperature three-dimensional growth layer 12A formation step (period T3) and lower than the growth temperature of the crystal nucleus layer 11 formation step, and the high-temperature three-dimensional growth layer 12B is formed by further growing on the low-temperature three-dimensional growth layer 12A (FIG. 2(d)), see FIG. 4). In FIG. 4, the period of this step is shown as period T4, and a case of a temperature of 1155° C. is shown as an example. The pressure is the same as in the previous step.

[0079] The high-temperature three-dimensional growth layer 12B is a layer grown to smoothly transition from the three-dimensional growth of the low-temperature three-dimensional growth layer 12A to the two-dimensional growth of the two-dimensional growth layer 13. The high-temperature three-dimensional growth layer 12B is a three-dimensional growth in which the lateral growth is faster than that of the low-temperature three-dimensional growth layer 12A, and the growth temperature of the high-temperature three-dimensional growth layer 12B is higher than that of the low-temperature three-dimensional growth layer 12A, so that the lateral growth is faster than that of the low-temperature three-dimensional growth layer 12A, and the crystals can be further integrated. As a result, the threading dislocations propagating toward the surface can be reduced by bending the threading dislocations laterally, and a crystal film with a low threading dislocation density can be obtained.

[0080] Here, the temperature at which the high-temperature three-dimensional growth layer 12B is formed is higher than the temperature at which the low-temperature three-dimensional growth layer 12A is formed, and tensile stress is generated in the crystal layer up to the high-temperature three-dimensional growth layer 12B during growth of the low-temperature three-dimensional growth layer 12A due to the difference in linear expansion coefficient with the substrate 10 (see FIG. 3(c)). Therefore, it is preferable to grow the high-temperature three-dimensional growth layer 12B not as a completely flat film, but as a three-dimensional surface partially having pits or facets, thereby easing the tensile stress generated on the surface.

[0081] The high-temperature three-dimensionally grown layer 12B is preferably grown thicker than the low-temperature three-dimensionally grown layer 12A, for example, to a thickness of 750 to 2000 nm. In this range, crystals can be further combined to further reduce the threading dislocation density. A more preferred thickness is 1000 to 1750 nm, and even more preferred is 1250 to 1500 nm.

[0082] The growth temperature of the high-temperature three-dimensional growth layer 12B is preferably 1050 to 1200° C. By setting the temperature in this range, the growth mode can be efficiently converted from three-dimensional growth to two-dimensional growth. The temperature is more preferably 1075 to 1175° C., and further preferably 1100 to 1150° C.

[0083] Moreover, the growth rate of the high-temperature three-dimensional growth layer 12B is faster than that of the low-temperature three-dimensional growth layer 12A and is lower than that of the crystal nucleus layer 11, and is preferably 5 to 50 nm / min. By setting the growth rate in this range, the crystals are slowly combined, and the change in the tensile stress generated on the crystal layer surface is made gentle, thereby suppressing the occurrence of cracks when the crystals are combined. The growth rate is more preferably 10 to 40 nm / min, and even more preferably 15 to 30 nm / min.

[0084] The V / III ratio of the high-temperature three-dimensionally grown layer 12B is smaller than that of the low-temperature three-dimensionally grown layer 12A and is equal to or larger than that of the crystal nucleus layer 11, and is preferably 100 to 1000. The growth rate can be controlled within the above range. It is more preferably 150 to 700, and further preferably 200 to 500.

[0085] 2-6. Two-dimensional growth layer 13 formation process When the high-temperature three-dimensional growth layer 12B has grown to a predetermined thickness, Ga source gas is supplied in addition to the nitrogen source gas and Al source gas at the same temperature as or higher than the high-temperature three-dimensional growth layer 12B formation step (period T4) to form a two-dimensional growth layer 13 made of AlN or AlGaN containing Ga (see FIG. 2(e) and FIG. 4). In FIG. 4, the period of this step is shown as period T5. The pressure is the same as in the previous step.

[0086] If Ga is supplied during AlN growth, the Ga atoms, which have a higher surface migration than Al atoms, promote lateral growth in the growth mode of AlN, resulting in two-dimensional growth. Therefore, the crystal can be flattened by the two-dimensional growth layer 13. In addition, the supply amount of Ga is increased continuously and stepwise over time. This allows the lateral growth rate to be increased slowly, easing the change in tensile stress that occurs when the crystals coalesce, thereby suppressing the occurrence of cracks in the two-dimensional growth layer 13.

[0087] The amount of Ga supplied is controlled by the molar ratio of the Ga source gas to the Al source gas, which is preferably 0.05 to 0.5, more preferably 0.08 to 0.4, and further preferably 0.1 to 0.3.

[0088] Although the ratio of Ga source gas is very high, Ga is not actually incorporated into AlN at the above ratio. This is because Ga atoms evaporate more easily than Al atoms on the AlN surface, so the Ga atoms actually incorporated into the AlN crystal are only a few percent, even when the molar ratio of the source gas is 0.3. The higher the growth temperature, the more Ga atoms evaporate preferentially, so even fewer Ga atoms are incorporated into the AlN crystal. Although it depends on the growth temperature and other conditions, the amount of Al grown within the above molar ratio range is about 100%. 1-x Ga x The Ga solid phase ratio of N is about x = 0.01 to 0.1%.

[0089] By applying a continuous and stepwise gradient within the above molar ratio range, the Ga supply rate is increased over time. The two-dimensional growth layer 13 changes from AlN to a mixed crystal of AlN and GaN (Al 1-x Ga x N). Here, the Ga composition is preferably 0.01 to 0.1.

[0090] The two-dimensionally grown layer 13 is preferably grown to a thickness equal to or greater than that of the high-temperature three-dimensionally grown layer 12B, for example, to a thickness of 750 to 2000 nm. Within this range, the surface of the two-dimensionally grown layer 13 can be sufficiently flattened. For example, the surface roughness RMS can be set to 0.5 to 5 nm. A more preferred thickness is 1000 to 1750 nm, and even more preferred is 1250 to 1500 nm.

[0091] The growth temperature of the two-dimensionally grown layer 13 is preferably 1100 to 1200° C. If the temperature is within this range, the two-dimensionally grown layer 13 can be sufficiently flattened. The temperature is more preferably 1120 to 1190° C., and further preferably 1140 to 1180° C. The temperature may be the same as that in the formation process of the crystal nucleus layer 11 and the formation process of the high-temperature three-dimensionally grown layer 12B.

[0092] The growth rate of the two-dimensional growth layer 13 is preferably 5 to 50 nm / min, which is higher than the growth rate of the high-temperature three-dimensional growth layer 12B and lower than the growth rate of the crystal nucleus layer 11. If the growth rate is within this range, the growth rate is sufficiently slow, and the change in tensile stress due to the flattening of the crystal can be made gentle, and the occurrence of cracks can be suppressed. It is more preferably 10 to 40 nm / min, and even more preferably 15 to 30 nm / min.

[0093] The V / III ratio of the two-dimensional growth layer 13 is set to be equal to or lower than the V / III ratio of the high-temperature three-dimensional growth layer 12B and equal to or higher than the V / III ratio of the crystal nucleus layer 11, and is preferably set to 50 to 500. The growth rate can be controlled within the above range. It is more preferably set to 100 to 400, and further preferably set to 150 to 300.

[0094] In addition, the curvature of the wafer at the end of the growth of the two-dimensional growth layer 13 is 50 km. -1 More than 300km -1 It is preferable that the curvature is 100 km or less. Here, the concave warp is a positive value, and the convex warp is a negative value. If the curvature of the wafer is within this range, cracks in the crystal layer can be further suppressed. It is more preferable that the curvature is 100 km or less. -1 More than 200km -1 The following is the result.

[0095] The above manufacturing process makes it possible to obtain a high-quality two-dimensionally grown layer 13 that is flat, has suppressed crack generation, and has a low dislocation density. In particular, the high-quality two-dimensionally grown layer 13 can be obtained at a temperature of 1250° C. or less. Therefore, a general crystal growth device using quartz as a material can be used, and the device cost and running cost can be reduced.

[0096] After the two-dimensionally grown layer 13 is formed, when the temperature is lowered to room temperature, compressive stress is applied to the crystal layers up to the two-dimensionally grown layer 13 due to the difference in linear expansion coefficient with the substrate 10, causing the wafer to warp in a convex shape (see FIG. 3(d)).

[0097] When switching between the periods T1 to T5, it is advisable to temporarily stop the supply of the source gas before changing the temperature, and then to supply the source gas again after changing the temperature to a predetermined temperature.

[0098] The crystal nucleus layer 11, the three-dimensional growth layer 12, and the two-dimensional growth layer 13 are grown under reduced pressure, because TMAl is highly reactive, and reducing the pressure suppresses the reactivity and allows high-quality crystals to be obtained. In the first embodiment, the pressure is constant, but the pressure may be reduced as the growth temperature increases. This allows crystals of higher quality to be obtained.

[0099] 2-7. Device structure formation process Next, n-type layer 14, active layer 15, electron blocking layer 16, and p-type layer 17 are laminated in this order on the two-dimensionally grown layer. A partial region of p-type layer 17 is then dry etched to form a groove reaching n-type layer 14. Then, p-electrode 18 is formed on p-type layer 17, and n-electrode 19 is formed on n-type layer 14 exposed at the bottom of the groove. In this manner, the light-emitting device according to embodiment 1 shown in FIG. 1 is manufactured.

[0100] In the first embodiment, the light emitting device is fabricated using the high-quality two-dimensionally grown layer 13 as the base layer, which makes it possible to improve the light emitting efficiency of the light emitting device, reduce the driving voltage, and improve the yield.

[0101] In the first embodiment, the light-emitting device is fabricated by successively growing the semiconductor layers on the two-dimensional growth layer 13. However, the production may be terminated at the stage where the two-dimensional growth layer 13 is grown, and the device may be used as an AlN template substrate.

[0102] In the first embodiment, the switching of the periods T1 to T5 from the formation of the nuclei 11A to the formation of the two-dimensionally grown layer 13 is controlled by the growth temperature, but it may be controlled by the growth rate. The growth rate can be controlled by, for example, the growth temperature and the V / III ratio.

[0103] 3. Experimental Results Next, various experimental results relating to the first embodiment will be described.

[0104] Experiment 1 A sample was prepared on a substrate 10, in which a crystal nucleus layer 11, a low-temperature three-dimensional growth layer 12A, a high-temperature three-dimensional growth layer 12B, and a two-dimensional growth layer 13 were formed at each stage. The growth temperature and growth pressure were as shown in the graph of FIG. 4. The crystal nucleus layer 11 had a growth rate of 30 nm / min and a thickness of 50 nm, the low-temperature three-dimensional growth layer 12A had a growth rate of 4 nm / min and a thickness of 250 nm, the high-temperature three-dimensional growth layer 12B had a growth rate of 18 nm / min and a thickness of 1300 nm, and the two-dimensional growth layer 13 had a growth rate of 18 nm / min and a thickness of 1400 nm. In the two-dimensional growth layer 13, the molar ratio of TMGa to TMAl was continuously changed from 13% to 30%.

[0105] 5 shows AFM images of the surfaces of the crystal nucleus layer 11, the low-temperature three-dimensional growth layer 12A, the high-temperature three-dimensional growth layer 12B, and the two-dimensional growth layer 13. Fig. 5(a) shows the surface of the crystal nucleus layer 11, Fig. 5(b) shows the surface of the low-temperature three-dimensional growth layer 12A, Fig. 5(c) shows the surface of the high-temperature three-dimensional growth layer 12B in the early growth stage, Fig. 5(d) shows the surface of the high-temperature three-dimensional growth layer 12B in the later growth stage, and Fig. 5(e) shows the surface of the two-dimensional growth layer 13.

[0106] As shown in Fig. 5(a), it can be seen that large nuclei 11A with a diameter of about 40 nm are generated. As shown in Fig. 5(b) to Fig. 5(d), it can be seen that the nuclei 11A grow and adjacent nuclei merge with each other. As shown in Fig. 5(e), it can be seen that the surface of the two-dimensionally grown layer 13 is flat and has steps.

[0107] Figure 6 is a TEM image showing a cross section perpendicular to the main surface of substrate 10 for the layered structure from substrate 10 to two-dimensional growth layer 13. As shown in Figure 6, it can be seen that threading dislocations are greatly reduced by the coalescence of nuclei 11A in low-temperature three-dimensional growth layer 12A, and that threading dislocations are further reduced in high-temperature three-dimensional growth layer 12B, resulting in a very low threading dislocation density in two-dimensional growth layer 13. Figures 5 and 6 show that high-quality AlN that is flat and has low dislocation density and suppressed crack generation has been obtained.

[0108] Experiment 2 A sample was prepared in which a crystal nucleus layer 11, a low-temperature three-dimensional growth layer 12A, a high-temperature three-dimensional growth layer 12B, and a two-dimensional growth layer 13 were formed in this order on a substrate 10. The change in growth temperature over time was as shown in the graph of FIG. 7. The crystal nucleus layer 11 had a growth temperature of 1100 to 1150°C and a thickness of 140 nm, the low-temperature three-dimensional growth layer 12A had a growth temperature of 1000°C and a thickness of 120 nm, and the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13 had a growth temperature of 1150°C and a thickness of 2600 nm. In FIG. 7, there are sections in which the temperature is constant at 400°C at the beginning and end of growth, but this is because the thermometer used for temperature measurement was compatible with high temperatures and could not measure temperatures below 400°C, and the temperature actually dropped to room temperature.

[0109] During the preparation of the sample for experiment 2, the warpage of the wafer was observed in situ. Figure 8 is a graph showing the change in the curvature of the wafer over time. A positive curvature value indicates concave warpage, and a negative curvature value indicates convex warpage. The periods T2 to T5 in Figure 8 are the same as those in Figure 4, with T2 being the process of forming the crystal nucleus layer 11, T3 being the process of forming the low-temperature three-dimensional growth layer 12A, and T4 and T5 being the processes of forming the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13.

[0110] As shown in FIG. 8, from the growth of the crystal nucleation layer 11 to the growth of the two-dimensional growth layer 13, except during the growth of the low-temperature three-dimensional growth layer 12A, the warpage is approximately constant with respect to time, and the curvature is 50 km. -1 is kept to a minimum.

[0111] The increase in warpage before the growth of the crystal nucleus layer 11 is caused by the temperature difference between the back surface of the substrate 10 that is in contact with the susceptor and the front surface of the substrate 10 that is in contact with the gas. The warpage of the wafer temporarily decreases during the growth of the low-temperature three-dimensional growth layer 12A. This is because the difference in thermal expansion coefficient between the substrate 10 and the crystal layer causes a shift in the direction of compressive strain. Thereafter, the warpage increases again during the growth of the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13, which is also caused by the difference in thermal expansion coefficient.

[0112] Here, since the growth temperatures of the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13 are approximately the same as the growth temperature of the crystal nucleus layer 11, the warping is also approximately the same during the growth of the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13 as during the growth of the crystal nucleus layer 11.

[0113] In this manner, the tensile strain increases when the temperature is higher than the reference temperature of the growth temperature of the crystal nucleus layer 11, and the compressive strain increases when the temperature is lower than the reference temperature. Therefore, the strain in the entire crystal layer depends on the growth temperature of the crystal nucleus layer 11 that is first formed on the substrate 10 and the growth temperatures of the subsequent crystal layers.

[0114] In order to prevent cracks from occurring in the crystal layer, it is important that no tensile strain occurs in the crystal layer. To achieve this, the crystal layer is grown on the crystal nucleus layer 11 at a temperature equal to or lower than the growth temperature of the crystal nucleus layer 11.

[0115] When the temperature is returned to room temperature after the growth of the two-dimensional growth layer 13 is completed, the wafer warps convexly due to the difference in thermal expansion coefficient between the substrate 10 and the crystal layer, but no cracks occur because the crystal is subjected to compressive strain.

[0116] It should be noted that the low-temperature three-dimensionally grown layer 12A is provided to reduce the threading dislocation density, but it is understood that the formation of the low-temperature three-dimensionally grown layer 12A can also suppress cracks.

[0117] Experiment 3 As a comparative example, a sample was prepared in which a crystal nucleus layer 11, a high-temperature three-dimensional growth layer 12B, and a two-dimensional growth layer 13 were successively formed on a substrate 10. The change in growth temperature over time was as shown in the graph of FIG. 9. The crystal nucleus layer 11 had a growth temperature of 950-1000°C and a thickness of 140 nm, while the high-temperature three-dimensional growth layer 12B and the two-dimensional growth layer 13 had growth temperatures of 1150°C and a thickness of 2600 nm. The difference from Experiment 2 is that the crystal nucleus layer 11 was grown at a lower temperature than in Experiment 2, and that the low-temperature three-dimensional growth layer 12A was not provided.

[0118] During the preparation of the sample for this experiment 3, the warpage of the wafer was observed in situ. Figure 10 is a graph showing the change in the curvature of the wafer over time. As shown in Figure 10, the warpage of the wafer increases monotonically with time, and when the curvature reaches 200 km, -1 Thus, when the crystal nucleus layer 11 is grown at a low temperature and then heated to form a crystal layer, tensile strain is formed in the film, and as the crystal layer grows (as the film thickness increases), the strain accumulates and the concave warpage increases. This causes cracks to form in the crystal layer. The cracks that occur remain even after growth is completed, leading to deterioration of device characteristics and yield.

[0119] (Modification of the first embodiment) As the nucleus 11A in the first embodiment, AlGaN or GaN may be used instead of AlN. If GaN or AlGaN is used, the difference in lattice constant with the sapphire substrate 10 becomes larger, and the strain relaxation at the interface between the substrate 10 and the nucleus 11A becomes larger. In addition, when the nucleus 11A is made of AlGaN or GaN, the lattice constant of the low-temperature three-dimensional growth layer 12A formed thereon has a higher Al composition than the nucleus 11A, so that the low-temperature three-dimensional growth layer 12A grown on the nucleus 11A receives tensile strain. This is because the growing crystal is formed in conformity with the lattice constant of the base. Therefore, it is possible to relax the compressive strain generated after the low-temperature three-dimensional growth layer 12A due to the thermal stress of the substrate and the crystal layer generated when the growth is completed and the temperature becomes room temperature.

[0120] In addition, in the strain relaxation at the interface between the substrate 10 and the nuclei 11A, the nuclei 11A are formed discretely, not in a film shape, so that the occurrence of cracks is suppressed. In addition, the low-temperature three-dimensional growth layer 12A formed on the crystal nuclei layer 11 receives tensile stress from the crystal nuclei layer 11 due to the difference in lattice constant, but the occurrence of cracks due to the tensile stress is suppressed because of the three-dimensional growth. As a result of the above, the threading dislocation density of the two-dimensional growth layer 13 can be reduced.

[0121] Furthermore, when the nuclei 11A are made of GaN or AlGaN, the surfactant effect of Ga allows the nuclei 11A to be made larger, and the nucleus density to be reduced. As described above, a low nucleus density allows the tensile stress generated on the surface when the nuclei combine to form a flat film to be reduced. In addition, the number of meeting surfaces where the nuclei 11A combine is reduced, which reduces the formation of threading dislocations, and allows the formation of a high-quality crystal film.

[0122] The core 11A may be GaN doped with Al. The core 11A is preferably AlGaN rather than GaN, and the Al composition is preferably 60% or more and 98% or less. This allows the strain to be further relaxed and the core 11A to be larger. More preferably, it is 60% or more and 98% or less.

[0123] When the nucleus 11A is GaN or AlGaN containing Ga, the substrate 10 can be easily separated by laser lift-off. In other words, since the band gap energy is smaller than that of AlN, it is easy to make the crystal nucleus layer 11 absorb laser light. In addition, since Ga has a very low melting point compared to Al, the crystal nucleus layer 11 becomes liquid when decomposed by irradiation with laser light. Therefore, when the crystal nucleus layer 11 contains Ga, the substrate 10 can be easily separated. Thus, when the nucleus 11A is GaN or AlGaN containing Ga, the crystal nucleus layer 11 is effective as a sacrificial layer for laser lift-off.

[0124] When the cores 11A are made of GaN or AlGaN, the size of the cores 11A is preferably 20 to 100 nm. By setting the size of the cores 11A in this range, the tensile stress can be sufficiently reduced. In addition, the variation in size of the cores 11A (the difference between the maximum diameter and the average diameter, and the difference between the average diameter and the minimum diameter) is preferably 20 nm or less.

[0125] Moreover, when the nucleus 11A is made of GaN or AlGaN, the thickness of the crystal nucleus layer 11 is preferably 5 to 100 nm. Since the nucleus 11A is larger than when the nucleus 11A is made of AlN, the crystal nucleus layer 11 is also thicker. As a result of the larger nucleus 11A, the quality of the crystal layer formed after the nucleus 11A can be further improved. A more preferable thickness of the crystal nucleus layer 11 is 5 to 50 nm. When the nucleus is AlGaN and the Ga composition is high, the crystals become more mobile by annealing, and it becomes easier to enlarge the nucleus by solid phase growth. The size of the nucleus immediately before growing the three-dimensional growth layer can be increased by annealing, and the density can also be reduced.

[0126] In addition, when the core 11A is made of GaN or AlGaN, the density of the core 11A is 3×10 11 / cm -2 It is preferable that the density of the cores 11A is 1.5×10 or less. Since the cores 11A are larger than those in the case of AlN, the density of the cores 11A is also smaller than those in the case of AlN. 11 / cm -2 Less than 1×10, more preferably11 / cm -2 In addition, when the nuclei 11A are GaN or AlGaN, the nuclei 11A can be enlarged by annealing. That is, the nuclei density can be increased to 1×10 11 / cm -2 It can be as follows:

[0127] In the first embodiment, the low-temperature three-dimensional growth layer 12A is made of AlN, but it may be made of AlGaN instead of AlN. However, from the viewpoint of strain relaxation and crystallinity, it is preferable that the difference between the Al composition of the low-temperature three-dimensional growth layer 12A and the Al composition of the crystal nucleus layer 11 is 40% or less.

[0128] In the first embodiment, the high-temperature three-dimensional growth layer 12B is AlN, but may be AlGaN instead of AlN. However, from the viewpoint of strain relaxation and crystallinity, it is preferable that the difference in Al composition between the high-temperature three-dimensional growth layer 12B and the low-temperature three-dimensional growth layer 12A is 30% or less.

[0129] In addition, in the first embodiment, the two-dimensional growth layer 13 is AlN, but it may be AlGaN instead of AlN. However, from the viewpoint of strain relaxation and crystallinity, it is preferable that the difference between the Al composition of the two-dimensional growth layer 13 and the Al composition of the high-temperature three-dimensional growth layer 12B is 20% or less.

[0130] In addition, the crystal layers below the two-dimensional growth layer 13 must have an Al composition that does not absorb light if the device formed on the two-dimensional growth layer 13 is a light-emitting device. If the device to be formed on the two-dimensional growth layer 13 is an ultraviolet light-emitting LED, the Al composition of the two-dimensional growth layer 13 is preferably the same as or greater than the Al composition of the n-type layer of the LED.

[0131] For the above reasons, most of the device structure is often formed with an Al composition lower than that of the two-dimensional growth layer 13. In order to relieve the strain in the device structure, it is preferable to change the lattice mismatch difference stepwise. It is preferable that the Al composition of the layers subsequent to the three-dimensional growth layer 12, excluding the crystal nucleus layer 11, is reduced stepwise. In this way, the strain on the device structure can be relieved.

[0132] The lower the Al composition of the nucleus 11A, the more the lattice constant changes from AlN to that of GaN. That is, the larger the in-plane lattice constant. Therefore, the three-dimensional growth layer 12 formed on the nucleus 11A and having a larger Al composition than the Al composition of the nucleus 11A receives tensile strain from the nucleus 11A. The lower the Al composition of the nucleus 11A, the larger the in-plane lattice constant of the three-dimensional growth layer 12 tends to be. The three-dimensional growth layer 12 receives tensile strain during growth, increasing the possibility of crack formation, so there is an optimal value for the Al composition difference between the nucleus 11A and the three-dimensional growth layer 12, as described above. The tensile strain formed after the three-dimensional growth layer 12 during growth becomes compressive strain due to the difference in thermal expansion coefficient with the substrate 10 made of sapphire when growth is completed and the temperature is raised to room temperature. However, as in the case of growth, the larger the lattice constant of the nucleus 11A, the more the compressive strain generated after the three-dimensional growth layer 12 at room temperature is alleviated.

[0133] Furthermore, when the nucleus 11A is made of GaN or AlGaN, the thickness of the two-dimensionally grown layer 13 is preferably 0.5 to 5 μm. The surface of the two-dimensionally grown layer 13 can be sufficiently flattened. For example, the surface roughness RMS can be set to 0.5 to 5 nm. The thickness of the two-dimensionally grown layer 13 is more preferably 1 to 3 μm.

[0134] Even when the nucleus 11A is made of GaN or AlGaN, the threading dislocation density of the two-dimensionally grown layer 13 is 5×10 11 cm -2 or less, and good quality crystals can be obtained. Furthermore, the full width at half maximum (FWHM) of the (002) diffraction line in rocking curve measurement in X-ray diffraction of the two-dimensionally grown layer 13 can be, for example, 100 to 300 arcsec, and the full width at half maximum of the (102) diffraction line can be, for example, 300 to 600 arcsec. This is because the full width at half maximum can be sufficiently reduced by reducing the threading dislocation density.

[0135] When the nuclei 11A are made of GaN or AlGaN, the growth conditions such as the growth temperature and growth rate of each layer can be in the same range as in the first embodiment.

[0136] Next, experimental results regarding the modified embodiment will be described.

[0137] A sample was fabricated by successively growing a crystal nucleus layer 11, a low-temperature three-dimensional growth layer 12A made of AlN, a high-temperature three-dimensional growth layer 12B made of AlN, and a two-dimensional growth layer 13 made of Ga-doped AlN on a substrate 10, and further stacking an n-type layer 14, an active layer 15, an electron block layer 16, and a p-type layer 17 on the two-dimensional growth layer 13. A plurality of samples were fabricated for the crystal nucleus layer 11 by varying the gas phase ratio of TMGa to the total of TMGa and TMAl (hereinafter, referred to as the gas phase ratio of TMGa). The gas phase ratio of TMGa was set to four values: 0%, 13.9%, 30.3%, and 46.5%. The Al composition in the AlGaN crystal at this time was 100%, 98%, 93%, and 89%, respectively. The thickness of each layer and the growth conditions were the same as those in the experiment of the first embodiment.

[0138] FIG. 11 is an AFM image of the surface of the p-type layer 17. As shown in FIG. 11, it can be seen that the surface flatness is higher when the TMGa gas phase ratio is 46.5% than when the TMGa gas phase ratio is 0% to 30.3%. In addition, when the RMS of the surface is calculated, it is 7.95 nm when the TMGa gas phase ratio is 0%, 8.61 nm when it is 13.9%, 7.97 nm when it is 30.3%, and 4.96 nm when it is 46.5%, and it can be seen that the surface flatness is higher when the TMGa gas phase ratio is 46.5%. In this way, it was found that by lowering the Al composition of the nucleus 11A, the crystal distortion is relaxed, three-dimensional growth is suppressed, and the surface flatness of the crystal layer is improved.

[0139] In addition, the rocking curve in X-ray diffraction of the two-dimensional growth layer 13 was measured, and the full width at half maximum (FWHM) of the (002) diffraction line and the (102) diffraction line was obtained. FIG. 12 is a graph showing the relationship between the gas phase ratio of TMGa and the full width at half maximum. As shown in FIG. 12, it was found that the full width at half maximum of both the (002) diffraction line and the (102) diffraction line becomes smaller as the gas phase ratio of TMGa increases (the Al composition decreases). This is considered to be because the lower the Al composition of the nuclei 11A, the larger the nuclei 11A becomes and the lower the nucleus density, resulting in a lower threading dislocation density. By making the nuclei 11A AlGaN, the three-dimensional growth layer 12 grown thereon is subjected to tensile strain due to the lattice mismatch difference, increasing the possibility of cracks occurring, but the surfactant effect of Ga makes it possible to make the nuclei 11A larger and the nucleus density smaller, so it is considered that the tensile stress occurring on the surface when the nuclei 11A are combined to form a flat film is also alleviated.

[0140] Next, the values ​​of the lattice constants of AlN in the low-temperature three-dimensional growth layer 12A and the high-temperature three-dimensional growth layer 12B were calculated from the X-ray diffraction data. FIG. 13 is a graph showing the a-axis and c-axis values ​​of the low-temperature three-dimensional growth layer 12A, the high-temperature three-dimensional growth layer 12B, and theoretical AlN. In addition, in the graph of FIG. 13, the diagonal line descending to the lower right indicates the direction in which the lattice constant of AlGaN at a given Al composition changes when strain occurs due to stress. In addition, in the graph of FIG. 13, the diagonal line ascending to the upper right indicates the direction in which the lattice constant changes due to a change in the Al composition.

[0141] 13, it can be seen that the lattice constant approaches the theoretical value of AlN as the gas phase ratio of TMGa increases (as the Al composition of the nuclei 11A decreases), which indicates that the compressive strain of AlN in the low-temperature three-dimensionally grown layer 12A and the high-temperature three-dimensionally grown layer 12B is relaxed as the Al composition of the nuclei 11A decreases. [Explanation of symbols]

[0142] 10: Substrate 11: Crystal nucleation layer 12: Three-dimensional growth layer 13: Two-dimensional growth layer 14:N-type layer 15:Active layer 16: Electron block layer 17:p-type layer 18:p electrode 19:n electrode

Claims

1. a crystal nucleation layer forming step of generating nuclei of GaN, AlGaN or AlN on a sapphire substrate to form a crystal nucleation layer; a low-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the nuclei at a temperature lower than that of the crystal nucleus layer formation step, and combining crystals from adjacent nuclei to form a low-temperature three-dimensional growth layer; and a high-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growth layer at a temperature higher than that of the low-temperature three-dimensional growth layer formation step and equal to or lower than the temperature of the crystal nucleus layer formation step to form a high-temperature three-dimensional growth layer.

2. The temperature of the crystal nucleus layer formation step is 1100° C. or more and 1200° C. or less, The temperature of the low-temperature three-dimensional growth layer formation process is 900° C. or more and 1100° C. or less, The method for producing a Group III nitride semiconductor according to claim 1 , wherein the temperature in the high-temperature three-dimensional growth layer formation step is 1050° C. or higher and 1200° C. or lower.

3. 3. The method for producing a Group III nitride semiconductor according to claim 1 or 2, further comprising, after the high-temperature three-dimensional growth layer formation step, a two-dimensional growth layer formation step of growing AlGaN or Ga-doped AlN from the high-temperature three-dimensional growth layer at a temperature equal to or higher than that of the high-temperature three-dimensional growth layer formation step to form a two-dimensional growth layer.

4. The method for producing a Group III nitride semiconductor according to claim 3 , wherein in the two-dimensionally grown layer forming step, the supply rate of Ga is increased with time.

5. The method for producing a Group III nitride semiconductor according to claim 3 , wherein the temperature in the two-dimensionally grown layer forming step is 1100° C. or more and 1200° C. or less.

6. The curvature of the wafer at the end of the growth of the two-dimensional growth layer is 50 km. -1 More than 300km -1 The method for producing a Group III nitride semiconductor according to claim 3 , wherein:

7. a crystal nucleation layer forming step of generating nuclei of GaN, AlGaN or AlN on a sapphire substrate to form a crystal nucleation layer; a low-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the nuclei at a growth rate slower than that of the crystal nucleus layer, and merging crystals from adjacent nuclei to form a low-temperature three-dimensional growth layer; and a high-temperature three-dimensional growth layer formation step of growing AlGaN or AlN from the low-temperature three-dimensional growth layer at a growth rate that is faster than the low-temperature three-dimensional growth layer and is equal to or lower than the growth rate of the crystal nucleus layer to form a high-temperature three-dimensional growth layer.

8. The growth rate of the crystal nucleus layer is 5 nm / min or more and 100 nm / min or less, The growth rate of the low-temperature three-dimensional growth layer is 2 nm / min or more and 20 nm / min or less, The method for producing a Group III nitride semiconductor according to claim 7 , wherein the growth rate of the high-temperature three-dimensionally grown layer is 5 nm / min or more and 50 nm / min or less.

9. 9. The method for producing a Group III nitride semiconductor according to claim 7 or 8, further comprising, after the high-temperature three-dimensional growth layer formation step, a two-dimensional growth layer formation step of growing AlGaN or Ga-doped AlN from the high-temperature three-dimensional growth layer at a growth rate equal to or higher than the high-temperature three-dimensional growth layer to form a two-dimensional growth layer.

10. The method for producing a Group III nitride semiconductor according to claim 9 , wherein in the two-dimensionally grown layer forming step, the supply rate of Ga is increased with time.

11. The method for producing a Group III nitride semiconductor according to claim 9 , wherein a growth rate in the two-dimensionally grown layer formation step is not less than 5 nm / min and not more than 50 nm / min.

12. The curvature of the wafer at the end of the growth of the two-dimensional growth layer is 50 km. -1 More than 300km -1 The method for producing a Group III nitride semiconductor according to claim 9 , wherein:

13. 8. The method for producing a Group III nitride semiconductor according to claim 1, further comprising, before the crystal nucleus layer forming step, a thermal cleaning step of heat-treating the sapphire substrate in a hydrogen-dominated atmosphere at a temperature higher than that in the crystal nucleus layer forming step.

14. 8. The method for producing a Group III nitride semiconductor according to claim 1, wherein the nucleus is AlGaN having an Al composition of 60 to 98%.

Citation Information

Patent Citations

  • Epitaxial substrate, manufacturing method thereof, semiconductor laminate structure, and pit generation suppression method in epitaxial substrate front surface

    JP2005072409A

  • Ultraviolet light-emitting diode device and method for manufacturing the same

    JP2012522388A

  • Semiconductor wafer and method of manufacturing the same

    JP2016157951A

  • Crystal substrate, ultraviolet emission element, and manufacturing method thereof

    JP2017154964A