Grouting chemical composition for bedrock solidification

The polyisocyanate component, combining sodium silicate and polyether polyol with diphenylmethane diisocyanate, addresses handling and foaming issues in rock consolidation, ensuring stable workability and reactivity in environments with water leaks, enhancing void filling and efficiency.

JP2024155971AActive Publication Date: 2024-10-31TOSOH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024144073
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-10-31
Estimated Expiration
2040-08-26

AI Technical Summary

Technical Problem

Existing rock consolidation chemicals face issues with poor handling properties at low temperatures, low resin fluidity during foaming, and inadequate void filling in environments with water leaks or springs, leading to reduced efficiency and safety in tunnel excavation.

Method used

A polyisocyanate component comprising a reaction product of a polyol component, including sodium silicate aqueous solution and polyether polyol with a tertiary amine catalyst, combined with diphenylmethane diisocyanate and polyphenylpolymethylene polyisocyanate, to enhance resin fluidity and foamability, ensuring stable workability and reactivity.

Benefits of technology

The solution improves handling properties at low temperatures, ensures resin fluidity during foaming, and enhances foamability, resulting in excellent ground improvement properties with sufficient void filling, even in environments with water leaks or springs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155971000001
    Figure 2024155971000001
  • Figure 2024155971000002
    Figure 2024155971000002
  • Figure 2024155971000003
    Figure 2024155971000003
Patent Text Reader

Abstract

To provide a grouting chemical composition for bedrock solidification, which, due to improved handleability at low temperature, securement of excellent resin flowability during foaming, and improvement in foamability, can secure an excellent soil improvement property through sufficient void filling performance and provide stable workability and reactivity even under an environment of a lot of water leakage and spring water.SOLUTION: Provided is a grouting chemical composition for bedrock solidification, comprising a polyol component (A) and a polyisocyanate component (B). The polyol component (A) comprises an aqueous solution of sodium silicate (A-1), a specific polyether polyol (A-2), and a specific tertiary amine catalyst (A-3). The polyisocyanate component (B) comprises a mixture (B-1) of MDI and polymeric MDI and a reaction product of a specific polyether polyol (B-2) and (B-1). Further, MDI and polymeric MDI in (B-1) have a specific mass ratio and isomers of MDI have a specific mass ratio.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an injection liquid composition that can be used even in environments with a lot of spring water or water leakage. [Background technology]

[0002] As a method for strengthening unstable rock or unstable ground, for example, there is a method called rock bolting, which stabilizes the surrounding ground during tunnel excavation. This method is carried out with the aim of protecting the tunnel structure by fixing and anchoring the bolts with a chemical solution. In the past, inorganic materials such as mortar, which have high strength, have been used as the injection liquid for such rock consolidation. However, these inorganic materials have poor work efficiency because they take a long time to develop strength, and there is also the problem that the materials flow into the water in the event of water leakage or spring water.

[0003] Recently, as tunnel excavation is being carried out in areas prone to water leaks and seepage, there have been increasing cases of injecting chemicals to consolidate rock under the spring water. However, contamination of the spring water by the chemicals and water leaks that cannot be stopped even by injecting the chemicals are hindering the efficiency and safety of the excavation work, and improvements are being called for.

[0004] In order to solve these problems, an inorganic-organic composite soil stabilization liquid, that is, an injection liquid that combines an aqueous silicate solution called water glass with a polyisocyanate composition, is used.

[0005] For example, Patent Document 1 reports that by using an aqueous silicate solution component containing an amine catalyst and a short-chain diol and diphenylmethane diisocyanate modified with polyether polyol as an injection liquid for rock consolidation, it is possible to improve the long hardening time and strength development time, as well as groundwater and spring water contamination, which are drawbacks of inorganic systems. However, there are concerns about handling, such as the high viscosity of the liquid and poor mixability at low temperatures, and further, there is a concern that the resin fluidity during foaming is low, resulting in poor void filling during injection and making it impossible to ensure the range of ground improvement. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-225951 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above-mentioned background art, and has an object to provide an injection liquid composition for rock consolidation which has improved handleability at low temperatures, ensures resin fluidity during foaming, and improves foaming properties, thereby ensuring excellent ground improvement properties due to sufficient void filling properties, and provides stable workability and reactivity even in environments with frequent water leaks and springs. [Means for solving the problem]

[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a liquid injection composition for rock consolidation agents, which comprises a polyol component (A) containing an aqueous sodium silicate solution and a polyisocyanate component (B) containing a reaction product of diphenylmethane diisocyanate and polyphenylpolymethylene polyisocyanate with a specific monool, and have thus completed the present invention.

[0009] That is, the present invention includes the following embodiments [1] to [5].

[0010] [1] A grout composition for rock consolidation comprising a polyol component (A) and a polyisocyanate component (B), wherein the polyol component (A) comprises an aqueous sodium silicate solution (A-1), a polyether polyol (A-2) having a number average molecular weight of 400 to 2000 and containing 60 to 90 mass% of ethylene oxide units, and a tertiary amine catalyst (A-3) having one active hydrogen, and the polyisocyanate component (B) comprises a mixture (B-1) of diphenylmethane diisocyanate and polyphenylpolymethylene polyisocyanate, and a polyether polyol (A-3) having 60 to 90 mass% of ethylene oxide units. % range of polyether polyol (B-2) having a number average molecular weight of 400 to 2000, and (B-1), wherein the ratio of diphenylmethane diisocyanate to polyphenylpolymethylene polyisocyanate in (B-1) is 50 / 50 to 75 / 25 by mass, and the ratio of 4,4'-diphenylmethane diisocyanate in the diphenylmethane diisocyanate to the sum of 2,2'-diphenylmethane diisocyanate and 2,4'-diphenylmethane diisocyanate is 70 / 30 to 55 / 45 by mass.

[0011] [2] The grout composition for rock consolidation according to the above [1], which contains a dispersion stabilizer in the polyol component (A).

[0012] [3] The injection composition for rock consolidation according to the above [1] or [2], wherein the polyisocyanate component (B) contains a viscosity reducing agent.

[0013] [4] The grout composition for rock consolidation according to any one of [1] to [3] above, wherein the polyisocyanate component (B) contains a foam stabilizer.

[0014] [5] A consolidated body obtained from the grout composition for rock consolidation described in any one of [1] to [4] above. Effect of the Invention

[0015] According to the grout liquid composition for rock consolidation of the present invention, the handling properties at low temperatures are improved, and the resin fluidity during foaming and the foaming properties are improved, thereby ensuring excellent ground improvement properties through sufficient void filling properties, and providing stable workability and reactivity even in environments with frequent water leaks and springs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The grout composition for rock consolidation in the present invention comprises a polyol component (A) (hereinafter also simply referred to as "component (A)") and a polyisocyanate component (B) (hereinafter also simply referred to as "component (B)").

[0017] First, the polyol component (A) will be described.

[0018] The polyol component (A) contains an aqueous sodium silicate solution (A-1) (hereinafter also referred to as (A-1)), a polyether polyol (A-2) (hereinafter also referred to as (A-2)) having a number average molecular weight of 400 to 2000 and containing 60 to 90 mass% ethylene oxide units (hereinafter also referred to as EO units or EO), and a tertiary amine catalyst (A-3) (hereinafter also referred to as (A-3)) having one active hydrogen.

[0019] As (A-1) in the present invention, a commercially available aqueous sodium silicate solution can be used. This sodium silicate is generally represented by the formula Na2O·xSiO2·nH2O. Here, x represents the molar ratio of SiO2 (silicon dioxide) to Na2O (sodium oxide), and in the present invention, it is preferably 2.0 to 3.0, more preferably 2.0 to 2.5, and most preferably 2.0 to 2.4. If x is less than 2.0, when component (A) and component (B) are mixed and cured, foaming properties cannot be ensured, and curing properties may deteriorate. If it exceeds 3.0, the viscosity of the aqueous sodium silicate solution increases, which may deteriorate the mixability with component (B) and may also deteriorate the workability at low temperatures.

[0020] In addition, the solid content excluding water from (A-1) is preferably 30 to 50 mass%, more preferably 33 to 42 mass%, further preferably 34 to 41 mass%, and most preferably 35 to 40 mass%. If the solid content of the sodium silicate aqueous solution is too high, it can be adjusted by diluting with water. If the solid content is lower than 30 mass%, when component (A) and component (B) are mixed and cured, foamability cannot be ensured and the mechanical strength of the foam after curing may decrease. If the solid content exceeds 50 mass%, the viscosity of the sodium silicate aqueous solution increases, which may deteriorate the mixability with component (B) and may also deteriorate the workability at low temperatures.

[0021] In the present invention, the solid content of (A-1) refers to the ratio of all components other than water in (A-1).

[0022] As (A-2) in the present invention, a polyol having a number average molecular weight of 400 to 2000 and containing 60 to 90 mass% of EO units in the polyether polyol is used. The number average molecular weight of (A-2) in the present invention is preferably 400 to 1800, more preferably 400 to 1000. If it is less than 400, the fluidity during foaming is poor and the void filling ability is poor. If it exceeds 2000, the groundwater contamination during foaming is deteriorated and the strength of the foam is reduced.

[0023] The EO unit of (A-2) is 60 to 90% by mass, and preferably 60 to 85% by mass. If it is less than 60% by mass, the mixing property of component (A) and component (B) becomes poor, the cells of the foam collapse, and shrink occurs. If it exceeds 90% by mass, the viscosity of component (A) becomes high, and the workability at low temperatures decreases.

[0024] The components other than the EO units in the polyether polyol are not particularly limited, but are preferably polypropylene oxide units (hereinafter, also referred to as PO units or PO).

[0025] In addition to the polyether polyol, a polyester polyol or a glycol may be used in combination without departing from the spirit of the present invention.

[0026] The content of (A-2) in component (A) is preferably 1 to 10% by mass. If it is less than 1% by mass, the foaming property during the reaction may not be ensured, and if it exceeds 10% by mass, the viscosity of component (A) may increase, which may deteriorate the workability and reduce the ground improvement property during chemical injection.

[0027] In the present invention, (A-3) is N,N-dimethylethanolamine, N-methyl-N-(N',N'-dimethylaminoethyl)aminoethanol, N,N-dimethylethoxyethanol, 1,4-diazabicyclo[2.2.2]octane-2-methanol, 6-dimethylamino-1-hexanol, N',N-dimethylethoxy-N'-methyl-N'-ethylmethanol, N'',N''-dimethylamino-N'-methylethylamino-N-methyl-2-propanol, bis(2- dimethylaminoethylamino)-2-propanol, N'-[2-(dimethylamino)ethyl]-N,N-dimethylethylenediamine, 3,3-iminobis(N,N-dimethyl-1-propanamine), N'-[2-(dimethylamino)methyl]-N,N-dimethylmethylenediamine, N,N,N',N'-tetraethyldiethylenetriamine, 2-[2-(dimethylamino)ethoxy]-N-[2-[2-(dimethylamino)ethoxy]ethyl]-ethanamine, and the like.

[0028] In addition, to assist the reaction, tertiary amines not having an active hydrogen group, such as N,N,N',N'-tetramethylhexamethylenediamine, N,N,N',N'-tetramethylpropylenediamine, N,N,N',N',N"-pentamethyldiethylenetriamine, N,N',N'-trimethylaminoethylpiperazine, N,N,N',N'-tetramethylethylenediamine, bis-(dimethylaminoethyl)ether, and N,N',N'-tris(3-dimethylaminopropyl) Hexahydro-S-triazine, 2-methyltriethylenediamine, N,N-dimethylaminoethylmorpholine, dimethylaminopropylimidazole, hexamethyltriethylenetetramine, hexamethyltripropylenetetramine, N,N,N-tris(3-dimethylaminopropyl)amine, N-methyl-N,N-bis(3-dimethylaminopropyl)amine, triethylenediamine, N-methylmorpholine, N-methylimidazole, and the like may also be used in combination.

[0029] The content of (A-3) in component (A) is preferably 0.1 to 5% by mass. If it is less than 0.1% by mass, there is a risk of deterioration in curing and reduction in foaming properties, and if it exceeds 5% by mass, it becomes difficult to control the reactivity, and there is a risk of poor injection due to clogging of the resin during injection of the chemical solution.

[0030] In the present invention, additives such as a dispersion stabilizer can be used to ensure the uniformity of component (A) and improve the compatibility between component (A) and component (B). Examples of the dispersion stabilizer include anionic dispersion stabilizers, cationic dispersion stabilizers, and nonionic dispersion stabilizers.

[0031] Examples of the anionic dispersion stabilizer include alkyl carboxylates, alkyl sulfates, alkyl sulfonates, and alkyl phosphates.

[0032] Examples of the cationic dispersion stabilizer include ammonium salts such as benzalkonium chloride.

[0033] Examples of non-ionic dispersion stabilizers include glycerin fatty acid esters, alkyl polyethylene glycols, polyoxyethylene alkyl phenyl ethers, and alkyl glycosides.

[0034] These dispersion stabilizers can be used alone or in combination of two or more.

[0035] Component (B) in the present invention includes a mixture (B-1) (hereinafter also referred to as (B-1)) of diphenylmethane diisocyanate (hereinafter referred to as MDI) and polyphenylpolymethylene polyisocyanate (hereinafter referred to as polymeric MDI), and a reaction product of (B-1) with polyether polyol (B-2) (hereinafter referred to as (B-2)) having a number average molecular weight of 400 to 2000 and containing 60 to 90 mass% of EO units.

[0036] In the present invention, MDI includes various isomers of 4,4'-MDI, 2,4'-MDI and 2,2'-MDI, and polymeric MDI means MDI to which one or more phenyl groups having an isocyanate group are added via a methylene group.

[0037] As for (B-1), the mass ratio of MDI to polymeric MDI is preferably MDI / polymeric MDI=50 / 50 to 75 / 25, more preferably 55 / 45 to 75 / 25. If the mass ratio of MDI is less than 50%, the viscosity of the polyisocyanate increases, which may cause poor handling, whereas if it exceeds 75%, the strength of the foamed resin may decrease.

[0038] The mass ratio of 4,4'-MDI to 2,4'-MDI and 2,2'-MDI in MDI is preferably 70 / 30 to 55 / 45, more preferably 70 / 30 to 60 / 40. If the mass ratio of 2,4'-MDI and 2,2'-MDI is less than 30%, the low temperature stability of the polyisocyanate may deteriorate and solidify, whereas if it exceeds 45%, the strength of the foamed resin may decrease.

[0039] As (B-2), a polyether polyol having a number average molecular weight of 400 to 2000 and containing 60 to 90% by mass of EO units in the polyol is used. The number average molecular weight of (B-2) in the present invention is preferably 400 to 1800, more preferably 400 to 1000. If the number average molecular weight is less than 400, the fluidity during foaming is poor, and the void filling ability is deteriorated. If it exceeds 2000, the strength of the foam is reduced. The EO unit of (B-2) is 60 to 90% by mass, preferably 60 to 85% by mass. If it is less than 60% by mass, the mixing property of component (A) and component (B) becomes poor, the cells of the foam collapse, and shrink occurs. If it exceeds 90% by mass, the viscosity of polyol component (A) becomes high, and the workability at low temperatures decreases.

[0040] The components other than the EO units in the polyether polyol are not particularly limited, but are preferably PO units.

[0041] In addition to the polyether polyol, a polyester polyol or a glycol may be used in combination without departing from the spirit of the present invention.

[0042] The modification rate of component (B) with (B-2) is preferably 0.5 to 10% by mass, more preferably 0.5 to 6.0% by mass. If it is less than 0.5% by mass, the compatibility with polyol component (A) may deteriorate, and the strength of the cured product may decrease when the chemical is injected. If it exceeds 6.0% by mass, the hydrophilicity becomes high, and when it comes into contact with groundwater, it may dissolve in the water, causing cloudiness and foaming, and may contaminate spring water.

[0043] The above (A-2) and (B-2) can be synthesized by a known method, or commercially available products can be used.

[0044] In the present invention, a foam stabilizer may be used in component (B) to stabilize the cell diameter during foaming, and examples of the foam stabilizer include silicon-based foam stabilizers, etc. Examples of silicon-based foam stabilizers include polyoxyalkylenedimethylpolysiloxane copolymers and organopolysiloxanes.

[0045] In the present invention, when a foam stabilizer is used, its content is preferably 3% by mass or less in component (B). If it exceeds 3% by mass, the resin strength may decrease.

[0046] In addition, a viscosity reducing agent for adjusting the viscosity may be used in combination with component (B). Examples of viscosity reducing agents that have excellent compatibility with component (B), viscosity reducing properties, and mixing stability include alkylene carbonates such as propylene carbonate, alkyl ethers such as propylene glycol monomethyl ether acetate, and diethylene glycol monomethyl ether acetate, and esters. From the viewpoints of the working environment and safety, the amount of these to be added is preferably 1 to 5 mass% relative to component (B).

[0047] By using the above-described grout composition for rock consolidation, which is composed of the component (A) and the component (B), a consolidated body having excellent void-filling properties can be obtained. EXAMPLES

[0048] Examples of the present invention will be described in detail below, but the present invention is not limited to these Examples. In the examples, "%" is based on mass unless otherwise specified.

[0049] <Preparation of polyisocyanate component> <Preparation Example 1> In a 1 L reactor equipped with a stirrer, thermometer, cooler and nitrogen gas inlet tube, 525.7 g of polyisocyanate 1, 381.0 g of diisocyanate 1 and 47.6 g of polyol 1 were charged and heated to 80°C. While maintaining the temperature, the mixture was mixed uniformly with a stirring blade and a urethane reaction was carried out for 3 hours. The mixture was then cooled to 60°C, and 38.1 g of diluent and 7.6 g of foam stabilizer were added and stirred for 30 minutes to obtain polyisocyanate composition (B-1a) (NCO content 28.1%, viscosity at 5°C 318 mPa·s, viscosity at 25°C 90 mPa·s).

[0050] <Preparation Example 2> In a 1L reactor equipped with a stirrer, thermometer, cooler, and nitrogen gas inlet tube, 536.1g of polyisocyanate 1, 388.2g of diisocyanate 1, and 30.0g of polyol 1 were charged and heated to 80°C. While maintaining the temperature, the mixture was mixed uniformly with a stirring blade and a urethane reaction was carried out for 3 hours. After that, the mixture was cooled to 60°C, 38.1g of diluent and 7.6g of foam stabilizer were added, and the mixture was stirred for 30 minutes to obtain polyisocyanate composition (B-1b) (NCO content 29.0%, viscosity at 5°C 264mPa·s, viscosity at 25°C 70mPa·s).

[0051] <Preparation Example 3> In a 1 L reactor equipped with a stirrer, thermometer, cooler, and nitrogen gas inlet tube, 536.1 g of polyisocyanate 1, 388.2 g of diisocyanate 1, and 30.0 g of polyol 1 were charged and heated to 80°C. While maintaining the temperature and mixing uniformly with a stirring blade, a urethane reaction was carried out for 3 hours. After that, the mixture was cooled to 60°C, 7.6 g of a foam stabilizer was added, and the mixture was stirred for 30 minutes to obtain polyisocyanate composition (B-1c) (NCO content 29.5%, viscosity at 5°C 342 mPa·s, viscosity at 25°C 97 mPa·s).

[0052] <Preparation Example 4> In a 1 L reactor equipped with a stirrer, thermometer, cooler and nitrogen gas inlet tube, 525.7 g of polyisocyanate 1, 381.0 g of diisocyanate 1 and 47.6 g of polyol 3 were charged and heated to 80°C. While maintaining the temperature and mixing uniformly with a stirring blade, a urethane reaction was carried out for 3 hours. After that, it was cooled to 60°C, 38.1 g of diluent and 7.6 g of foam stabilizer were added, and the mixture was stirred for 30 minutes to obtain polyisocyanate composition (B-1d) (NCO content 29.6%, viscosity at 5°C 281 mPa·s, viscosity at 25°C 72 mPa·s).

[0053] <Preparation Example 5> In a 1 L reactor equipped with a stirrer, thermometer, cooler and nitrogen gas inlet tube, 536.1 g of polyisocyanate 1, 388.2 g of diisocyanate 1 and 30.0 g of polyol 2 were charged and heated to 80°C. While maintaining the temperature, the mixture was mixed uniformly with a stirring blade and a urethane reaction was carried out for 3 hours. After that, the mixture was cooled to 60°C, 38.1 g of diluent and 7.6 g of foam stabilizer were added, and the mixture was stirred for 30 minutes to obtain polyisocyanate composition (B-1e) (NCO content 30.6%, viscosity at 5°C 188 mPa·s, viscosity at 25°C 61 mPa·s).

[0054] <Preparation Example 6> In a 1 L reactor equipped with a stirrer, thermometer, cooler, and nitrogen gas inlet tube, 813.9 g of polyisocyanate 1, 111.2 g of diisocyanate 1, and 17.8 g of polyol 3 were charged and heated to 80°C. While maintaining the temperature and mixing uniformly with a stirring blade, a urethane reaction was carried out for 3 hours. After that, the mixture was cooled to 60°C, 38.1 g of diluent and 7.6 g of foam stabilizer were added, and the mixture was stirred for 30 minutes to obtain polyisocyanate composition (B-1f) (NCO content 28.6%, viscosity at 5°C 711 mPa·s, viscosity at 25°C 140 mPa·s).

[0055] <Preparation Example 7> In a 1L reactor equipped with a stirrer, thermometer, cooler, and nitrogen gas inlet tube, 778.0g of polyisocyanate 1, 146.3g of diisocyanate 1, and 30.0g of polyol 1 were charged and heated to 80°C. While maintaining the temperature, the mixture was mixed uniformly with a stirring blade and a urethane reaction was carried out for 3 hours. After that, the mixture was cooled to 60°C, 38.1g of diluent and 7.6g of foam stabilizer were added, and the mixture was stirred for 30 minutes to obtain polyisocyanate composition (B-1g) (NCO content 28.4%, viscosity at 5°C 621mPa·s, viscosity at 25°C 120mPa·s).

[0056] [Table 1]

[0057] The ingredients in Table 1 are as follows: Polyisocyanate 1: MDI / polymeric MDI = 40 / 60 (PA ratio), 2,4'-MDI and 2,2'-MDI to 4,4'-MDI ratio in MDI = 3 / 97, NCO content 31.0% (product name: MR-200, manufactured by Tosoh Corporation) Diisocyanate 1: MDI / polymeric MDI = 100 / 0 (PA ratio), 2,4'-MDI and 2,2'-MDI to 4,4'-MDI ratio in MDI = 55 / 45, NCO content 33.5% (product name: Millionate NM, manufactured by Tosoh Corporation) Polyol 1: PO / EO polyether polyol, number average molecular weight 400, EO content 75% Polyol 2: PO / EO polyether polyol, number average molecular weight 4000, EO content 20% Polyol 3: PO-based polyether polyol, number average molecular weight 400, EO content 0% Foam stabilizer: Siloxane-polyalkylene oxide copolymer (product name: NIAXSILICONEY-16136, manufactured by MOMENTIVE) Diluent: Propylene carbonate (product name: Propylene Carbonate S, manufactured by BASF) The MDI / polymeric MDI ratio of Polyisocyanate 1 and Diisocyanate 1 is the peak area ratio (PA ratio) obtained by GPC measurement, and is expressed as (MDI monomer peak area) / (sum of peak areas of MDI oligomers other than MDI monomer).

[0058] The GPC measurement conditions are as follows. (1) Measuring instrument: HLC-8220 (manufactured by Tosoh Corporation) (2) Column: TSKgel (Tosoh Corporation) G3000H-XL G2500H-XL G2000H-XL G1000H-XL (3) Carrier: THF (tetrahydrofuran) (4) Detector: RI (refractive index) detector (5) Temperature: 40℃ (6)Flow rate: 1.000ml / min (7) Calibration curve: Standard polystyrene (Tosoh Corporation) ·F-80 (molecular weight: 7.06×10 5 , molecular weight distribution: 1.05) ·F-20 (molecular weight: 1.90×10 5 , molecular weight distribution: 1.05) ·F-10 (molecular weight: 9.64×10 4 , molecular weight distribution: 1.01) ·F-2 (molecular weight: 1.81×10 4 , molecular weight distribution: 1.01) ·F-1 (molecular weight: 1.02×10 4 , molecular weight distribution: 1.02) ·A-5000 (molecular weight: 5.97×10 3 , molecular weight distribution: 1.02) ·A-2500 (molecular weight: 2.63×10 3 , molecular weight distribution: 1.05) ·A-500 (molecular weight: 5.0×10 2 , molecular weight distribution: 1.14) (8) Sample solution concentration: 0.5% THF solution.

[0059] <Preparation of polyol component> The polyol component was prepared according to the composition shown in Table 2.

[0060] [Table 2]

[0061] The ingredients in Table 2 are as follows: Sodium silicate aqueous solution 1: solid content 37.5%, molar ratio (SiO2 / Na2O) = 2.0 (product name: No. 1 sodium silicate Q0, manufactured by Toso Sangyo Co., Ltd.) Sodium silicate aqueous solution 2: solid content 36.5%, molar ratio (SiO2 / Na2O) = 2.0 (product name: No. 1 sodium silicate R0, manufactured by Toso Sangyo Co., Ltd.) Polyol 1: PO / EO polyether polyol, number average molecular weight 400, EO content 75% Polyol 2: PO / EO polyether polyol, number average molecular weight 4000, EO content 20% Polyol 3: PO-based polyether polyol, number average molecular weight 400, EO content 0% Polyol 4: EO-based polyether polyol, number average molecular weight 400, EO content 100% 1,3-BG: 1,3-butanediol, molecular weight 90 MPD: 3-methyl-1,5-pentanediol, molecular weight 118 TMAEE: N-methyl-N-(N',N'-dimethylaminoethyl)aminoethanol (product name: TOYOCATRX5, manufactured by Tosoh Corporation) · TEDA: Triethylenediamine (product name: TEDAL33, manufactured by Tosoh Corporation).

[0062] <Reaction behavior and various evaluation methods> A foaming test was carried out using the polyol component (A) and polyisocyanate component (B) in the formulation shown in Table 3 (liquid temperature: 5°C, stirring conditions: 300 rpm x 10 seconds using a Three-One motor, liquid temperature: 20°C, stirring conditions: 350 rpm x 10 seconds using a Three-One motor, liquid temperature: 25°C, stirring conditions: 400 rpm x 10 seconds using a Three-One motor). The results are shown in Table 3.

[0063] [Table 3]

[0064] In the reactivity test, "free foaming" refers to mixing components (A) and (B) in a 1 L cup under the above conditions, mixing and stirring, and allowing foaming to occur in the cup. "Foaming in water" refers to mixing components (A) and (B) in a 1 L cup under the above conditions, mixing and stirring, and then quickly pouring 100 mL of the mixed liquid into another 1 L cup containing 500 mL of water, and stirring the water vigorously with a stirring rod for 30 seconds to allow foaming.

[0065] Cream time: The time (seconds) from when you start mixing and stirring the polyol component (A) and the polyisocyanate component (B) until the mixture becomes cloudy and creamy and the liquid level rises. Rise time: The time (seconds) from the start of mixing and stirring the polyol component (A) and the polyisocyanate component (B) until the mixture foams and reaches its maximum height.

[0066] Foaming ratio: The foaming ratio during free foaming is calculated using the following formula. Expansion ratio (times) = volume of molded product after expansion (cm 3 ) / volume of mixture before foaming (cm 3 ) A free foaming ratio of 5.0 or more at each temperature is considered to be good. In the case of underwater foaming, a free foaming ratio of 4.0 or more is considered to be good.

[0067] - Water turbidity after foaming: In the underwater foaming test, the turbidity of the water was measured with a turbidity meter (TURBIDIMETER2100N, manufactured by HACH) as an index of water pollution after the rise time had ended. A turbidity of 20 NTU or less is considered to be good.

[0068] - Water foaming after foaming: In the underwater foaming test, the foaming of water is measured as an index of water pollution after the rise time has finished. 125mL of the water used in the underwater foaming test after the rise time has finished is placed in a 250mL polyethylene bottle, sealed, shaken vigorously for 10 seconds, and then left to stand. The time (seconds) until the foam disappears from the water surface is expressed. A time of 60 seconds or less is considered good.

[0069] Foaming speed: When foaming in a 1L cup, the time it takes from the cream time until the cup is full is calculated using the following formula.

[0070] Foaming rate ( / sec) = 100 / (reaction time from start of mixing to filling 1L cup (sec) - cream time (sec)) At a liquid temperature of 25°C, a foaming rate of 14.0 or less is considered to be good.

Claims

[Claim 1] The grout composition for rock consolidation is composed of a polyol component (A) and a polyisocyanate component (B), in which the polyol component (A) contains an aqueous sodium silicate solution (A-1), a polyether polyol (A-2) having a number average molecular weight of 400 to 2000 and containing 60 to 90% by mass of ethylene oxide units, and a tertiary amine catalyst (A-3) having one active hydrogen, and the polyisocyanate component (B) contains a mixture (B-1) of diphenylmethane diisocyanate and polyphenylpolymethylene polyisocyanate, and a polyether polyol (A-3) having 60 to 90% by mass of ethylene oxide units. The injection liquid composition for rock consolidation comprises a reaction product of polyether polyol (B-2) having a number average molecular weight of 400 to 2000, the number average molecular weight being in the range of 400 to 2000, and (B-1), wherein the ratio of diphenylmethane diisocyanate to polyphenylpolymethylene polyisocyanate in (B-1) is 50 / 50 to 75 / 25 by mass, and the mass ratio of 4,4'-diphenylmethane diisocyanate in the diphenylmethane diisocyanate to the sum of 2,2'-diphenylmethane diisocyanate and 2,4'-diphenylmethane diisocyanate is 70 / 30 to 55 / 45 by mass.

Citation Information

Patent Citations

  • Soil-stabilizing composition for polyurethane-based expanded resin and soil stabilization using the composition

    JP1997183898A

  • Chemical grouting agent composition for soil coagulation, and water siopping by soil stabilization and strengthening using the same

    JP1999116955A

  • Injectable chemical solution composition for stabilizing and strengthening soil or artificial construction, and water barrier constructing method for stabilizing and strengthening soil or artificial construction using the composition

    JP2001303054A

  • Impregnating agent composition for consolidation of rock bed or ground, and soil-stabilizing and enhancing water sealing construction method using the same

    JP2017155076A

  • Grouting agent composition for soil stabilization, and stabilizing and strengthening water cutoff method using the same