Method of producing sintered porous body, and sintered porous body

The use of organic waste as a void-forming material in a two-stage firing process addresses the challenges of controlling particle size and cost in sintered porous body production, enabling cost-effective and energy-efficient soil creation for plant growth.

JP2024156323APending Publication Date: 2024-11-06OHBAYASHI GUMI LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023070693
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Existing methods for producing sintered porous bodies face challenges in controlling particle size, damaging pores during crushing, and high costs due to the use of limited and expensive industrial materials like artificial graphite powder.

Method used

A method using organic waste as a void-forming material, combined with a two-stage firing process, to produce a sintered porous body with controlled particle size and porosity, eliminating the need for crushing and reducing production costs.

Benefits of technology

The method enables the production of a sintered porous body at a lower cost, with controlled particle size and porosity, suitable for creating a soil environment that supports healthy plant growth by housing microorganisms that decompose organic nitrogen, contributing to energy savings and a potential food cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156323000001_ABST
    Figure 2024156323000001_ABST
Patent Text Reader

Abstract

To produce a sintered porous body from a soil material as a base material easily at a low cost.SOLUTION: A method of producing a sintered porous body for producing a granular sintered porous body from a soil material as a base material, comprises a molding step of obtaining a molded body from a mixture of a void-forming material of a granular shape that disappears by heating and the base material, and a firing step of firing the molded body by raising temperature stepwise, wherein an organic material is used as the void-forming material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a sintered porous body using an earthen material as a base material, and to a sintered porous body. [Background technology]

[0002] An environment suitable for growing agricultural crops is formed by maintaining a suitable biochemical environment in the soil through the metabolism of organic matter in the soil by soil microorganisms, and by maintaining suitable physical environments such as water permeability, air permeability, and water retention. For example, Patent Document 1 discloses a greening system that artificially prepares such an environment.

[0003] The greening system of Patent Document 1 realizes an environment suitable for growing agricultural crops by containing porous ceramic particles. The porous ceramic particles are obtained by mixing clay and a carbon material, adding water, forming the mixture into a plate or block shape, firing it, and then crushing it.

[0004] However, such methods that include a step of crushing the fired product have problems, such as the inability to control the particle size of the porous ceramic particles and the tendency to damage the pores that are favorable for the establishment of microbial groups involved in the production of inorganic nitrogen necessary for plant growth.

[0005] In light of this, the inventors have developed a method for stably producing a sintered porous body having a desired particle size, as shown in Patent Document 2. Specifically, an earthen material is mixed with a pore-forming material, water is added to the mixture, the mixture is granulated to the desired particle size, and the granulated porous body is obtained by firing. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-27503 A [Patent Document 2] Patent Application No. 2021-187316 Summary of the Invention [Problem to be solved by the invention]

[0007] According to the manufacturing method of Patent Document 2, the particle size of the sintered porous body is easily controlled, and the process of crushing the fired product can be omitted, so that damage to the pores can be suppressed. Meanwhile, in manufacturing the sintered porous body, a carbon material is used as a void-forming material. Among carbon materials, artificial graphite powder in particular has a uniform particle size and is a suitable material for easily obtaining the desired pore size and porosity because all impurities disappear when heated.

[0008] However, artificial graphite powder is an industrial product produced by carbonization using large-scale carbonization equipment, and as a result, although it is available on the market, the sellers are limited, and the price is high, which has a significant impact on the production of sintered porous bodies, and the development of an alternative material has been desired.

[0009] The present invention has been made in consideration of the above problems, and a main object of the present invention is to produce a sintered porous body using an earthen material as a base material at low cost and easily. [Means for solving the problem]

[0010] In order to achieve this objective, the method for producing a sintered porous body of the present invention is a method for producing a granular sintered porous body using an earthen material as a base material, and comprises a molding step of obtaining a molded body from a mixture of a powdered void-forming material that disappears when heated and the base material, and a firing step of firing the molded body by gradually increasing the temperature, and is characterized in that an organic material is used as the void-forming material.

[0011] The method for producing a sintered porous body of the present invention is characterized in that the organic material is pulverized and used as the void-forming material.

[0012] The method for producing a sintered porous body of the present invention is characterized in that the organic material is organic waste.

[0013] The method for producing a sintered porous body of the present invention is characterized in that the green body is obtained by granulating the mixture.

[0014] The sintered porous body of the present invention is characterized in that it is produced by the method for producing a sintered porous body of the present invention.

[0015] According to the manufacturing method of the sintered porous body and the sintered porous body of the present invention, a powder produced by drying and pulverizing an organic material is used as a void-forming material. This makes it possible to produce a sintered porous body using an earthen material as a base material more cheaply and easily than when an industrial product such as artificial graphite powder is used as a void-forming material. In addition, the carbonization process is omitted in the process of producing the void-forming material, which contributes to energy saving.

[0016] In addition, sintered porous bodies are materials that can create an environment in which microorganisms that break down organic nitrogen and produce inorganic nitrogen as plant nutrition can live, and by immobilizing the microorganisms, they can be used as soil for healthy plant growth. In this sense, if food waste, among organic waste, is used as a pore-forming material, it will be possible to realize a food cycle in which food waste is used to create sintered porous bodies and the sintered porous bodies are used to grow crops. Effect of the Invention

[0017] According to the present invention, by using an organic material as the void-forming material, it becomes possible to inexpensively and easily produce a sintered porous body using an earthen material as a base material. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a diagram showing an outline of a sintered porous body and a sintering program according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing a method for producing a sintered porous body according to an embodiment of the present invention (part 1). [Diagram 3]FIG. 2 is a diagram showing a method for producing a sintered porous body according to an embodiment of the present invention (part 2). [Figure 4] FIG. 1 is a diagram showing an apparatus used for producing a sintered porous body according to an embodiment of the present invention. [Diagram 5] 1 is a graph showing the results of Experiment 1 in the embodiment of the present invention. [Figure 6] 13 is a graph showing the results of Experiment 2 in the embodiment of the present invention. [Figure 7] FIG. 13 is a diagram showing the composition of a molded body used in Experiment 3 in the embodiment of the present invention. [Figure 8] FIG. 13 is a diagram showing a baking program employed in Experiment 3 in the embodiment of the present invention. [Figure 9] FIG. 2 is a diagram showing the state of a sintered porous body using an organic material according to an embodiment of the present invention. [Figure 10] FIG. 4 is a graph showing a particle size accumulation curve of a sintered porous body using an organic material according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention provides a method for inexpensively and easily producing a sintered porous body by using an organic material that has not been carbonized as a void-forming material. The details of the method will be described below with reference to Figs. 1 to 10.

[0020] <<<<Sintered porous body>>>> As shown in Fig. 1(a), the sintered porous body 10 is a fired product of a base material 11 made of an earthen material having a plurality of pores 14, and is manufactured through a process of forming a void-forming material, a molding process, a firing process, and a sieving process. The details of each process will be described later with reference to Fig. 3, but the process is roughly as follows.

[0021] In the forming process of the void-forming material, a non-carbonized organic material is dried and pulverized to obtain a powdered void-forming material 12 having a desired particle size. In the molding process, a base material 11 made of an earthen material and the void-forming material 12 are mixed, and granulated by a wet granulation method to produce a granular compact 13.

[0022] In the firing process, the molded body 13 is fired according to a firing program that employs two-stage firing (stepwise temperature increase) as shown in Fig. 1(b). That is, the molded body 13 produced in the molding process is heated in a low-temperature region, and after the void-forming material 12 is eliminated, the temperature is increased, and then the molded body 13 is heated in a high-temperature region to sinter the base materials 11 together.

[0023] In the sieving step, the sintered porous body 10 obtained in the firing step is sieved to recover the sintered porous body 10 having a particle size range (main range in which particle sizes are distributed) suitable for the intended use.

[0024] The base material 11 used in manufacturing such a sintered porous body 10 is suitably a basaltic soil material whose main components are silica (silicon dioxide SiO2) and alumina (aluminum oxide Al2O3), and examples include processed basalt products and processed lava stone from Mount Fuji.

[0025] In addition, any material that can be sintered by heating for a certain period of time at a temperature higher than the combustion temperature of the organic material used in the void-forming material 12 (the temperature at which the organic material disappears), such as china clay, ceramic base, materials used as fired bricks, or backfill soil or soil generated on-site, can be used as the base material 11.

[0026] On the other hand, the void-forming material 12 can be any organic material that can be pulverized into powder and that disappears when heated for a certain period of time in a specified temperature range. In this embodiment, an example is given in which organic waste is used. Organic waste refers to solid food waste generated from food, such as vegetable waste, brewing waste, fermentation waste, and fish waste, as well as livestock manure, sludge, agricultural residues, and wood waste. In addition, if organic waste cannot be obtained, algae, which has a high carbon dioxide absorption efficiency, may be used.

[0027] <<<<Sintered porous body that can be turned into soil>>>> The sintered porous body 10 can be used as a material for creating soil in which plants can be grown.

[0028] Generally, plants can grow healthily in places where microorganisms that decompose organic nitrogen to produce inorganic nitrogen, which serves as plant nutrition, live. It is known that microorganisms live in environments where the three properties of soil (physical, chemical, and biological) are well-established. In other words, the sintered porous body 10 that can be used as a material for creating soil can be obtained by controlling the particle size range, pore size, and porosity so as to create the three properties of soil and immobilize the microorganisms (soil formation).

[0029] <<<<Method for producing sintered porous body>>> Below, a general procedure for producing a sintered porous body 10 that can be turned into soil by controlling the particle size range, porosity, and pore size will be described with reference to the flow charts shown in Figs.

[0030] <<Step 1: Design of sintered porous body>> In producing the sintered porous body 10, as shown in FIG. 2, first, the particle size range, porosity, and pore size are designed according to the intended use.

[0031] Considering that the sintered porous body 10 that can be turned into soil has a particle size of sand to medium gravel and that pores of a size that can provide a place (home) for the growth of the aforementioned microorganisms are to be created, the particle size range is preferably 0.5 mm to 20 mm, more preferably 1 mm to 9.5 mm. Also, the pore size is preferably, for example, 10 μm or more, and large pores 14 are included.

[0032] Under these conditions, the sintered porous body 10 has a porosity sufficient to create an environment in which the microbial population is established and activated in the pores 14, the ability to supply nutrients to plants is ensured, the soil has a well-balanced three-phase distribution (solid, liquid, and gas phases), and a balanced aerobic and anaerobic environment is achieved.

[0033] ≪≪Step 2: Setting the materials to be used≫≫ <Step 2-1: Selection of base material 11> The soil material to be used as the base material 11 is selected based on the particle size range set in Step 1.

[0034] First, the particle diameter of the compact 13 is set so as to obtain the sintered porous body 10 within the particle diameter range set in Step 1. Then, a soil material capable of producing the compact 13 with this particle diameter is selected. For example, in the case where the sintered porous body 10 capable of being turned into soil is set to a suitable particle diameter range of 1 mm to 9.5 mm, it is preferable to set the particle diameter of the compact 13 to 10 mm or less, taking into account shrinkage during firing.

[0035] The soil material capable of forming such a compact 13 is sintered by heating for a certain period of time at a temperature higher than the combustion temperature of the organic material used in the void-forming material 12, and preferably has a particle size of 2 mm or less and an average particle size (D50) of 10 μm to 200 μm. For example, crushed Osawa stone (processed product of Osawa lava from Mt. Fuji) or simulated lunar regolith sand can be used. Alternatively, a plurality of these soil materials may be mixed and the particle size adjusted for use.

[0036] <Step 2-2: Selection of the void-forming material 12 and setting of the addition ratio of the void-forming material 12> For the void-forming material 12, an organic material that is compatible with the pore diameter set in Step 1 is selected. In addition, the addition ratio of the void-forming material 12 is set based on the porosity requirement shown in Step 1. For the sintered porous body 10 that can be turned into soil, the lower limit of the addition ratio of the void-forming material 12 is preferably set to 10%, more preferably 30%.

[0037] On the other hand, it is preferable to set the upper limit at 50%. This is for the following reason. In producing the sintered porous body 10, the compact 13 is molded by wet granulation in the molding step as described above. The wet granulation method is a method of granulation while adding an appropriate amount of water, and if the addition ratio of the void-forming material 12 exceeds 50%, the amount of water added increases, which may make granulation difficult by the wet granulation method.

[0038] <Step 2-3: Selection of void-forming material 12 based on moldability of molded body 13 and hardness after firing> The wet granulation method used in the molding process is a molding method in which a mixture of base material 11 and void-forming material 12 is granulated while adding an appropriate amount of water, and the amount of water added varies depending on the material used for the void-forming material 12.

[0039] If the water content (the weight of water relative to the combined weight of the base material 11 and the void-forming material 12) is high, a slurry will form and granulation will be impossible. Even if granulation is possible, the molded bodies 13 will tend to adhere to each other. The hardness of the molded bodies 13 after sintering will not be suitable for the intended use of the sintered porous body 10.

[0040] For this reason, the moldability of the molded body 13 and the hardness after firing are verified, and an organic material that satisfies these requirements is selected as the void-forming material 12 to manufacture the sintered porous body 10. The sintered porous body 10 that can be turned into soil preferably has a hardness that is not broken when it is transported to the intended plant growth area or when it is spread in the intended plant growth area. The material is selected taking these factors into consideration.

[0041] <<Production of sintered porous bodies: Step 3>> As described above, in Step 2, the soil material that will be the base material 11, the organic material that will be the void-forming material 12, the addition ratio of the void-forming material 12, the particle size of the compact 13, and the amount of water to be added are set, and then, as shown in Figure 3, a sintered porous body 10 that can be turned into soil is produced by the following procedure.

[0042] <Creating the void-forming material: Step 3-0> The organic material to be used as the void-forming material 12 is dried as necessary and then pulverized to obtain a finely pulverized material. This is sieved to obtain a powder to be used as the void-forming material 12. The particle size of the powder is preferably similar to the average particle size ((D50) 10 μm or more and 200 μm or less) of the soil material used as the base material 11, and more preferably, the particle size is about 100 μm. If the powder is pulverized to such a particle size, it is easy to mix homogeneously with the base material 11 when the green body 13 is produced in the above-mentioned molding process, and it is also easy to realize the pores 14 of the sintered porous body 10 designed in Step 1.

[0043] ≪Molding process: Step3-1≫ After mixing the base material 11 and the void-forming material 12, the mixture is granulated by a wet granulation method to form the molded body 13. Any means may be used for the granulation operation by the wet granulation method, but for example, it is preferable to use a pan-type granulator 30 as shown in FIG.

[0044] Specifically, the base material 11 and the void-forming material 12 are dropped into an inclined pan 31 provided in a pan-type granulator 30, and the two are mixed evenly while rotating the pan 31. Next, water 15 is added little by little while rotating the pan 31, and the mixture of the base material 11 and the void-forming material 12 is granulated. Since the mixture of the base material 11 and the void-forming material 12 tends to adhere to the bottom and sides of the pan 31, the adhering matter is scraped off with a scraper 32 or by hand as necessary during granulation.

[0045] As described in Step 2-1, considering the expected particle size range of 1 mm to 9.5 mm for the sintered porous body 10 that can be turned into soil, the particle size of the compact 13 is preferably 10 mm or less. To obtain compacts 13 with a particle size of 10 mm or less by a granulation operation, it is advisable to set the granulation time with a target particle size of about 5 mm and perform the granulation operation. In this way, by forming the compacts 13 into granules in the molding process, post-processing steps such as cutting and crushing that generate powder and granules, which are generally performed after the firing process, can be omitted, greatly improving workability.

[0046] After the molded body 13 is thus molded, it is taken out, for example, into a heat-resistant container 40 and heated for a certain period of time to dry. The drying temperature and drying time are appropriately set while taking into consideration the size and moisture content of the molded body 13 so that no cracks are formed on the surface and the internal moisture is uniform.

[0047] <Firing process Step 3-2> The green body 13 dried in Step 3-1 above is fired. As described above, the firing program employs a two-stage firing (stepwise temperature increase), in which the void-forming material 12 is removed by heating in a low-temperature region for a certain period of time, and then the temperature is increased, and the base material 11 is sintered by heating in a high-temperature region for a certain period of time.

[0048] The set temperature of the low temperature region is set based on the combustion temperature of the organic material used in the void-forming material 12, and the heating time is set to the heating time required to raise the temperature to the center of the compact 13 and eliminate the void-forming material 12. The set temperature of the high temperature region is set based on the sintering temperature of the soil material used in the base material 11, and the heating time is set to the heating time required to raise the temperature to the center of the compact 13 and sinter the base material 11.

[0049] In this way, by adopting a two-stage firing process, the heating time can be easily controlled, which makes it easy to avoid problems such as the occurrence of molten parts on the surface of the compact 13 and the remaining unsintered parts inside. Therefore, it is possible to stably obtain a high-quality sintered porous body 10, as shown in Fig. 1(a), in which pores 14 are formed all the way to the center where the void-forming material 12 has disappeared.

[0050] <Sieving process: Step 3-3> After firing the green body 13 in Step 3-2 above, sieving is performed to recover the sintered porous body 10 having a desired particle size range. Since the green body 13 is granulated in Step 3-1 to a particle size that takes into account the particle size range required for the sintered porous body 10, the sintered porous body 10 having a desired particle size range can be efficiently obtained, and the sintered porous body 10 can be obtained at a high recovery rate.

[0051] As described in Step 1, the particle size range of the sintered porous bodies 10 that can be turned into soil is set to 1 mm or more and 9.5 mm or less, and sieving is performed to recover sintered porous bodies 10 in this range. As a result, the recovered sintered porous bodies 10 contain many large pores 14 with pore sizes of 10 μm or more, and the particle size range is adjusted to 1 mm or more and 9.5 mm or less. In this way, it is possible to obtain sintered porous bodies 10 with sizes ranging from sand to fine gravel, which have significantly improved air permeability, water permeability, and water retention properties compared to the soil material used as the base material 11.

[0052] In addition, the recovered sintered porous body 10 has a porosity that is sufficient to create an environment in which a group of microorganisms that decompose organic nitrogen and generate inorganic nitrogen as a nutrient for plants can live. Therefore, the sintered porous body 10 that can be turned into soil can be used as soil in which plants can grow healthily by immobilizing a group of microorganisms.

[0053] <<<<Reference Example: When artificial graphite powder is used as the void-forming material>>>> As a reference example, artificial graphite powder was used as the void-forming material 12, and the results of producing a sintered porous body 10 according to the above procedure are shown below.

[0054] Artificial graphite powder (grain size approximately 100 μm, volume average value approximately 125 μm) was used as the void-forming material 12, and lunar regolith imitation sand (grain size 2 mm or less, D50 ≒ 70 μm) was used as the base material 11 to create a green body 13 with an additive ratio of 30% void-forming material 12. This green body 13 was heated in a low-temperature range of 800°C or 900°C for 10 hours, then heated again, and then heated in a high-temperature range of 1100°C for 1 hour, thereby undergoing a two-stage firing process.

[0055] As a result, it becomes possible to stably manufacture a high-quality sintered porous body 10 that is sintered to the inside, as shown in Fig. 9. The size of the voids at this time was about 100 µm. Using these results as a guide, the following verification was carried out on the sintered porous body 10 when organic waste was used as the void-forming material 12.

[0056] <<<<<Example: When organic waste is used as a void-forming material>>>> In this embodiment, "coffee grounds" and "green tea leaves" are used as organic waste. Also, "rice husk charcoal" is used as a comparative example. "Coffee grounds" are the residue left over after grinding coffee beans to brew coffee, and "green tea leaves" are the tea leaves left over after brewing green tea. On the other hand, "rice husk charcoal" is a biomass-derived carbonized material made by carbonizing rice husks.

[0057] <Experiment 1: Verification of obtaining powder of desired particle size from organic waste> In the experiment, the above-mentioned "coffee grounds" and "green tea leaves" were thoroughly dried at 105°C, and then finely pulverized to obtain finely pulverized materials. The pulverization method was to use a crush mill to pulverize each, and then a vibration mill or a planetary ball mill as appropriate. Furthermore, the obtained finely pulverized materials were sieved to obtain powder particles with a particle size that can be used as the void-forming material 12.

[0058] As a result, powder particles of 212 μm or less were obtained from the finely ground "coffee grounds," and powder particles of 150 μm or less were obtained from the finely ground "green tea leaves." On the other hand, powder particles of 150 μm or less were obtained from the finely ground "rice husk charcoal," which was used as a comparative example. The particle size distribution of these powder particles is shown in Figures 5(a) to (c).

[0059] As described above, it was possible to obtain powder particles (particle size of about 100 μm) similar to artificial graphite powder from all of the "coffee grounds," "green tea leaves," and "rice husk charcoal." Therefore, in Experiment 2, an experiment was conducted to verify the heating temperature required to eliminate the void-forming material 12 when these were used as the void-forming material 12.

[0060] <Experiment 2: Verification of heating temperature required to eliminate void-forming material 12> In the experiment, the powder obtained in <Experiment 1> was heated and the temperature and mass transitions were observed for "coffee grounds," "green tea leaves," and "rice husk charcoal" (comparative example), to confirm the temperature at which the powder was completely burned. The results are shown in Figures 6(a)-(c) as temperature transition curves and mass loss curves.

[0061] For the powder of "rice husk charcoal" used as a comparative example, looking at the inflection point (TG) and heat generation peak (DTA) of the mass loss curve in Figure 6(c), the mass starts to decrease gradually with increasing temperature, but decreases significantly at around 300°C. It then reaches an exothermic peak at 394.5°C, and is completely combusted at around 450°C.

[0062] Looking at the inflection point (TG) and heat generation peak (DTA) of the mass loss curve in Figure 6(a) for the powdered "coffee grounds," the mass starts to decrease gradually as the temperature rises, then decreases significantly at around 250°C. It then reaches an exothermic peak at 491.3°C, and is completely combusted at around 500°C.

[0063] Looking at the inflection point (TG) and heat generation peak (DTA) of the mass loss curve in Figure 6(b) for the powdered "green tea leaves," the mass starts to decrease gradually as the temperature rises, and then decreases significantly at around 250°C. After that, the heat generation peaks at around 512.9°C, and the powder is completely combusted.

[0064] From the above results, when organic waste is used as the void-forming material 12, the suitable heating temperature for eliminating the void-forming material 12 is preferably 300° C. or higher and 600° C. or lower, and more preferably about 450° C. to 550° C. With reference to these temperatures, the following experiment was carried out to create a firing program employing two-stage firing, which is applied when using an organic material as the void-forming material 12 and producing a sintered porous body 10 that can be turned into soil.

[0065] <Experiment 3: Creating a baking program> In the experiment, first, a green body 13 with an addition ratio of 30% of the void-forming material 12 was produced by the procedure explained in the molding process of Step 3-1. FIG. 7 shows the composition when the green body 13 was produced.

[0066] Lunar regolith imitation sand (grain size 2 mm or less, D50 ≒ 70 μm) was used for the base material 11, and "coffee grounds" and "green tea leaves" obtained as powder in <Experiment 1> were used as the void-forming material 12 as examples. For the "coffee grounds", powder of 212 μm or less obtained by sifting finely ground material was used as the void-forming material 12, and for the "green tea leaves", powder of 150 μm or less obtained by sifting finely ground material was used as the void-forming material 12.

[0067] As a comparative example, the powdered material obtained in <Experiment 1>, "rice husk charcoal", was used as the void-forming material 12 to produce a compact 13. "Rice husk charcoal", powdered material of 150 μm or less obtained by sieving finely pulverized material, was used as the void-forming material 12.

[0068] The firing program was set based on the results of the above-mentioned <Experiment 2>. Specifically, for the "coffee grounds," the heating temperature in the low-temperature region was set to two cases, 500°C (Case 1) and 800°C (Case 2), and the heating time was set to 10 hours for both, as shown in Figures 7 and 8(a). In addition, the set temperature of the high-temperature region was set to 1100°C based on the sintering temperature of the crushed product of simulated lunar regolith sand, and the heating time was set to 1 hour.

[0069] For "green tea leaves," the heating temperature in the low-temperature region was set to 500°C, and the heating time was set for three cases: 1 hour (case 3), 3 hours (case 4), and 5 hours (case 5), as shown in Figures 7 and 8(b). The temperature in the high-temperature region was set to 1100°C, based on the sintering temperature of the crushed and processed lunar regolith simulant sand, and the heating time was set to 1 hour.

[0070] As with the "coffee grounds", the comparative example "rice husk charcoal" had its heating temperature set to two low-temperature ranges, 500°C (case 1) and 800°C (case 2), and both heating times were set to 10 hours. The high-temperature range was set to 1100°C, based on the sintering temperature of the crushed product of simulated lunar regolith sand, and its heating time was set to 1 hour.

[0071] <Experiment 4: Verification of the finish of the sintered porous body 10> FIG. 9 shows the external appearance and an electron microscope photograph of the sintered porous body 10 obtained as a result of firing according to the above firing program.

[0072] First, when "rice husk charcoal" was used as a comparative example, the low temperature range was set to 500°C and heating was performed for 10 hours (Case 1), and a granular sintered porous body 10 having sufficient hardness that did not easily crumble due to impact, etc. was recovered. On the other hand, in Case 2, where the low temperature range was set to 800°C and heating was performed for 10 hours, a granular sintered porous body 10 was recovered, but the strength was insufficient.

[0073] When the sintered porous body 10 produced in the above (Case 1) was observed under an electron microscope, no cinders were found in the pores formed by the disappearance of the "rice husk charcoal." Furthermore, analysis revealed that the largest pores were about 100 μm in size, the porosity was about 45%, and the dry density was 1.4 g / m 3 This porosity and dry density are approximately the same as those of the sintered porous body 10 in which the artificial graphite powder shown as the reference example was used as the void-forming material 12.

[0074] When "coffee grounds" were used, as in the case of using "rice husk charcoal" as a comparative example, the low temperature range was set to 500°C and heating was performed for 10 hours (Case 1), and a granular sintered porous body 10 having sufficient hardness that does not easily crumble due to impact, etc. was recovered. On the other hand, when the low temperature range was set to 800°C and heating was performed for 10 hours (Case 2), a granular sintered porous body 10 was recovered, but the strength was insufficient.

[0075] When the sintered porous body 10 produced in the above (Case 1) was observed under an electron microscope, no cinders were found in the pores formed by the disappearance of the "coffee grounds". Furthermore, analysis revealed that the largest pores were about 150 μm, the porosity was about 55%, and the dry density was 1 g / m. 3 This pore and void ratio is slightly larger than that of the case where "rice husk charcoal" was used. In other words, it is slightly larger than that of the case where the artificial graphite powder shown as the reference example was used.

[0076] When "green tea leaves" were used, the low temperature range was set to 500°C and heating was performed for 3 hours (Case 4), and a granular sintered porous body 10 having sufficient hardness to not easily crumble due to impact, etc. was recovered. On the other hand, when the low temperature range was set to 500°C and heating was performed for 1 hour (Case 3), a granular sintered porous body 10 was recovered, but it was brittle enough to be crushed with fingers. Furthermore, when the low temperature range was set to 500°C and heating was performed for 5 hours (Case 5), although it was not as brittle as Case 3, its strength was insufficient.

[0077] When the sintered porous body 10 produced in the above (Case 4) was observed under an electron microscope, no cinders were found in the pores formed when the "green tea leaves" disappeared. In addition, analysis revealed that the largest pores were about 150 μm, the porosity was about 60%, and the dry density was 1 g / m. 3 It can be seen that when "green tea leaves" were used, the pores and porosity formed in the sintered porous body 10 were approximately the same as when "coffee grounds" were used.

[0078] <Experiment 5: Verification of particle size distribution of sintered porous body 10> FIGS. 10(a) and 10(b) show the particle size distribution of the sintered porous body 10 of FIG. 9, which was determined to have sufficient hardness in the above-mentioned <<Experiment 4>>.

[0079] As shown in Figure 10(a), in the sintered porous body 10 using "rice husk charcoal", the particle size is 4.75 to 9.5 mm in about 50%. On the other hand, when "coffee grounds" are used, the particle size is 1.0 to 4.75 mm in about 50%, and a sintered porous body 10 with a smaller particle size can be obtained compared to the case where "rice husk charcoal" is used.

[0080] As shown in Figure 10(b), when "green tea leaves" are used, the sintered porous body 10 has a particle size of 1.0 to 4.75 mm accounting for approximately 70% and less than 1.0 mm accounting for approximately 20%. This means that a sintered porous body 10 with a smaller particle size can be obtained compared to when "coffee grounds" are used.

[0081] As described above, when lunar regolith imitation sand is used for the base material 11 and "coffee grounds" is used for the void-forming material 12, a two-stage firing is performed with a firing program (case 1) in which the low-temperature region is set to 500°C and heating is performed for 10 hours. When "green tea leaves" are used, a two-stage firing is performed with a firing program (case 4) in which the low-temperature region is set to 500°C and heating is performed for 3 hours.

[0082] This makes it possible to stably produce a high-quality sintered porous body 10 that is sintered to the inside at low cost and easily, compared to the case of using an industrial product such as artificial graphite powder as the void-forming material 12. In addition, since the carbonization process is omitted in the production process of the void-forming material 12, this contributes to energy saving.

[0083] The firing program may be set by appropriately adjusting the temperature of the low temperature region and the heating time depending on the organic waste to be used as the void-forming material 12. Furthermore, the crushing means for crushing the organic waste to produce a powder that can be used as the void-forming material 12 is not limited in any way.

[0084] The method for producing a sintered porous body and the sintered porous body 10 of the present invention are not limited to the above-described embodiment, and various modifications are possible without departing from the spirit of the present invention.

[0085] For example, in the present embodiment, in the manufacturing method of the sintered porous body 10, a mixture of the void-forming material 12 and the base material 11 is granulated to obtain the molded body 13, but a method of obtaining the molded body 13 without the granulation step may be adopted.

[0086] In addition, in the present embodiment, an example is given of the case of producing a sintered porous body 10 that can be turned into soil, but the present invention is not limited to this. By appropriately designing and producing the particle size range, pore size, and porosity according to the above-mentioned method for producing a sintered porous body, it is possible to produce a sintered porous body 10 that can be used for a desired purpose by employing an organic material as the void-forming material 12.

[0087] Furthermore, although the above examples show the use of "coffee grounds" and "green tea leaves" as organic waste from among organic materials, it is also possible to use inedible parts such as rice husks, potato skins, and root vegetable skins, as well as inedible parts such as leaves, stems, and roots of crops and plants. By using such inedible parts, the sintered porous body 10 can be manufactured using the inedible parts, and the sintered porous body 10 can be used to cultivate agricultural crops such as vegetables, thereby contributing to the production of agricultural crops using inedible biomass.

[0088] In other words, if food waste such as coffee grounds, green tea leaves, or inedible parts are used as the void-forming material 12, it will be possible to realize a food cycle in which the food waste is used to create a sintered porous body 10 and the created sintered porous body 10 is then used to grow crops.

[0089] When an organic material is used as the void-forming material 12, the heating time in the low temperature range may be appropriately set according to the type of organic material when creating a firing program. Also, the organic material may be pulverized using an appropriate pulverizing means, and a powder having a desired particle size may be obtained from the pulverized material. [Explanation of symbols]

[0090] 10 Sintered porous body 11 Base material 12 Void forming material 13 Molded body 14 Pore 15 water 30 Pan-type Granulator 31 Bread 32 Scraper 40 Heat-resistant container

Claims

1. A method for producing a granular sintered porous body using a soil material as a base material, comprising the steps of: a molding step of obtaining a green body from a mixture of the powder-like void-forming material, which disappears when heated, and the base material; A firing step of firing the molded body by gradually increasing the temperature, A method for producing a sintered porous body, characterized in that an organic material is used as the void-forming material.

2. The method for producing a sintered porous body according to claim 1, The method for producing a sintered porous body, comprising crushing the organic material and using the crushed organic material as the void-forming material.

3. The method for producing a sintered porous body according to claim 1, A method for producing a sintered porous body, wherein the organic material is organic waste.

4. The method for producing a sintered porous body according to claim 1, The method for producing a sintered porous body, wherein the green body is obtained by granulating the mixture.

5. A sintered porous body produced by the method for producing a sintered porous body according to any one of claims 1 to 4.

Citation Information