Electrode, manufacturing method thereof, and power storage element
By integrating a fibrous conductive additive with a specific diameter range into the electrode active material layer, the method improves the performance and capacity of power storage elements, addressing the lack of thin fiber conductive agents in existing technologies.
Patent Information
- Application Number
- JP2023070825
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
Smart Images

Figure 2024156399000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode, a manufacturing method thereof, and an energy storage element. [Background technology]
[0002] As an electrode for an electricity storage element using a non-aqueous electrolyte, one has been reported in which the active material layer contains a solid electrolyte and a conductive assistant in addition to an active material.
[0003] In Patent Document 1, Example 1 states, "First, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Composite particles were prepared in which O2 particles (active material particles) were coated with LiNbO3 (oxide-based solid electrolyte). Next, 20 g of the composite particles and 2.4 g of 10LiI-15LiBr-75 (0.75Li2S-0.25P2S5) particles (sulfide-based solid electrolyte···) were charged into a dry kneading device··· and kneading treatment was performed to produce composite active material particles··. The article states that 22.4 g of the composite active material particles were prepared as the positive electrode active material, 0.8 g of 10LiI-15LiBr-75 (0.75Li2S-0.25P2S5) particles as the sulfide-based solid electrolyte, 0.3 g of vapor grown carbon fiber (VGCF) as the conductive material, and 0.15 g of PVdF as the binder. The positive electrode active material, sulfide-based solid electrolyte, conductive material, and binder were adjusted so that the positive electrode active material:sulfide-based solid electrolyte:conductive material:binder = 94.7 mass %:3.4 mass %:1.3 mass %:0.6 mass %, and 13 g of butyl butyrate was added and wet-mixed with an ultrasonic homogenizer to prepare an electrode mixture. (Paragraph
[0019] ) Furthermore, Cited Document 1 states, "All-solid-state lithium secondary batteries were manufactured using the electrode mixtures of Example 1 and Comparative Examples 1 and 2 as positive electrode mixtures. As the raw material for the separator layer (solid electrolyte layer), 10LiI-15LiBr-75 (0.75Li2S-0.25P2S5) particles, which are a sulfide-based solid electrolyte, were prepared. Natural graphite was prepared as the negative electrode active material, 10LiI-15LiBr-75 (0.75Li2S-0.25P2S5) particles as the sulfide-based solid electrolyte, and PVdF as the binder. The negative electrode active material, sulfide-based solid electrolyte, and binder were mixed in a ratio of negative electrode active material:sulfide-based solid electrolyte:binder=64.1% by mass:34.7% by mass:1.2% by mass to prepare a negative electrode mixture. First, a powder compact of 10LiI-15LiBr-75 (0.75Li2S-0.25P2S5) particles was formed as a separator layer. Next, a positive electrode mixture was placed on one side of the powder compact, and a negative electrode mixture was placed on the other side, and then flat-pressed to obtain a laminate. The laminate was then restrained in the stacking direction to produce an all-solid-state lithium secondary battery." (Paragraph
[0022] )
[0004] Patent Document 2 states that "3 g of LPS, 0.2 g of acetylene black as a conductive additive, and 10 g of NMC having an average particle size of 5 μm as an active material were mixed in a ball mill to obtain active material 1 having a coating layer containing LPS and the conductive additive (coating number 1). ... This active material 1, 0.05 g of LSP, and 0.4 g of acetylene black were stirred in a ball mill to obtain active material 2 having a coating layer containing LPS and a conductive additive (coating number 2). This active material 2, 0.1 g of LPS, and 0.4 g of acetylene black were mixed in a ball mill to obtain a composite electrode active material No. 7 having a coating layer containing LPS and a conductive additive (coating times 3)." (Paragraph
[0112] ) Patent Document 2 also states that "An all-solid-state secondary battery No. 1-7 having the layer structure shown in FIG. 1 was produced as follows. ... Zirconia beads were placed in a zirconia container, and 70 g of the composite electrode active material No. 7 synthesized above, 0.9 g of LPS, and 12.3 g of heptane as a dispersion medium were placed in the container. The container was set in a planetary ball mill, and mixing was continued to prepare positive electrode composition 1. ... In a zirconia...container..., 28 g of the LPS synthesized above and 12.3 g of heptane as a dispersion medium were added. The container was set in a planetary ball mill...and mixed. After that, 7.0 g of CGB20 was added as an active material to the container, and the container was similarly set in a planetary ball mill...and mixing was continued to prepare negative electrode composition 1. ... The positive electrode composition 1 prepared above was applied to an aluminum foil (positive electrode current collector) with an applicator... and dried.... After that, a heat press machine was used to apply pressure while heating... to produce a positive electrode sheet having a positive electrode active material layer on the positive electrode current collector. ... The negative electrode composition 1 prepared above was applied to a stainless steel (SUS) foil (negative electrode current collector) by an applicator... and then dried. After that, the negative electrode was pressed while being heated using a heat press machine to produce a negative electrode sheet having a negative electrode active material layer on the negative electrode current collector. ... The document states, "Using the prepared positive electrode sheet and negative electrode sheet... an all-solid-state secondary battery was prepared." (Paragraphs
[0115] to
[0120] )
[0005] Patent Document 3 describes how, "32.0 parts by mass of LiPS4 powder was added to 30.0 parts by mass of a toluene solvent containing 3.0 parts by mass of ion-conductive polymer A, and the mixture was processed in a planetary ball mill. Further, 60.0 parts by mass of NMC111 was added, and the mixture was processed in the same planetary ball mill, and then vacuum dried to obtain a composite electrode material 1." 95.0 parts by mass of the obtained composite electrode material 1 and 1.0 part by mass of HS-100 were mixed in a mortar. 4.0 parts by mass of VGCF (registered trademark)-H were added thereto, and the mixture was mixed in the mortar to obtain a positive electrode material powder 1. ... A polyethylene die with an inner diameter of 10 mm and a lower punch made of SUS were fixed, 150 parts by mass of LiPS4 powder was placed, and pressure was applied with the upper punch to obtain a solid electrolyte layer. The upper punch was removed, 15 parts by mass of the positive electrode material powder 1 was placed on the solid electrolyte layer, and pressure was applied with the upper punch to obtain a laminate of a solid electrolyte layer and a positive electrode layer. That is, this laminate includes a positive electrode layer made of the positive electrode material powder 1. The upper punch was removed, and a SUS plate with a diameter of 10 mm and a thickness of 100 μm was placed on the laminate in the die. After the upper punch was fitted, the die was inverted upside down. The lower punch (facing up) was removed, and a lithium foil with a diameter of 10 mm and a thickness of 47 μm and two sheets of aluminum foil with a diameter of 10 mm and a thickness of 20 μm were placed in this order on the laminate in the die. After fitting a lower punch onto the aluminum foil, pressure was applied between the lower punch (negative electrode terminal) and the upper punch (positive electrode terminal), and the two were fixed with bolts in this state to obtain a solid-state battery consisting of a negative electrode terminal, an Al foil, a Li foil, a solid electrolyte layer, a positive electrode layer, a SUS plate, and a positive electrode terminal.' (Paragraphs
[0118] to
[0121] ) Patent Document 3 also states that the VGCF (registered trademark)-H used had an average fiber diameter of 150 nm and a ratio of the average fiber length to the average fiber diameter (aspect ratio) of 35 (Paragraph
[0117] ).
[0006] In Patent Document 4, "Li is bonded to the surface of the active material (TiO2) by the following procedure. 1+x Al x Ge 2-x The solid electrolyte represented by the general formula (PO4)3 (x=0.5) and carbon nanofiber VGCF (registered trademark, manufactured by Showa Denko K.K.) were used as a coating. (1) The raw materials for the solid electrolyte (CH3COOLi·2H2O, NH4H2PO4, Al(NO3)3·9H2O, GeO2) were mixed in a solution of ammonia water (0.45 mol / L) in a specified composition ratio. (2) The VGCF was further mixed into the mixture as a conductive additive. (3) Furthermore, TiO2 was mixed into the mixture as an active material. (4) The coating liquid obtained as described above was heated at 100° C. to remove the solvent component. (5) Dry in an oven (260°C) overnight. (6) Prior to firing, the solid electrolyte was vitrified by calcining at 450°C in a nitrogen atmosphere. (7) Heat treatment equivalent to the degreasing process of sheet binder was carried out (500°C for 5 hours in air). (8) Next, the mixture was sintered in a nitrogen atmosphere at 600°C for 2 hours. (9) The obtained coated active material was compressed in a pressure cell, and the electronic conductivity was evaluated. ... The ratio of the active material, the solid electrolyte to be coated, and the VGCF is 89:7:4." (Paragraphs
[0034] to
[0044] )
[0007] Patent Document 5 describes a method for producing a negative electrode mixture layer 132 in the form of a sheet having a thickness of 65 μm: "48.5 parts by mass of a composite material, 48.5 parts by mass of a solid electrolyte (Li3PS4, D50: 8 μm), and 3 parts by mass of VGCF (registered trademark)-H (manufactured by Showa Denko K.K.) were mixed together. This mixture was homogenized by milling using a planetary ball mill. The homogenized mixture was press-molded at 400 MPa by a uniaxial press molding machine using a polyethylene die with an inner diameter of 10 mm and a SUS punch to prepare a negative electrode mixture layer 132 in the form of a sheet having a thickness of 65 μm." ... 55 parts by mass of a positive electrode active material LiCoO2 (manufactured by Nippon Chemical Industry Co., Ltd., D50: 10 μm), 40 parts by mass of a solid electrolyte (Li3PS4, D50: 8 μm), and 5 parts by mass of VGCF (registered trademark)-H (manufactured by Showa Denko K.K.) were mixed. This mixture was homogenized by milling using a planetary ball mill. The homogenized mixture was press-molded by a uniaxial press molding machine using a polyethylene die with an inner diameter of 10 mmφ and a SUS punch to prepare a positive electrode mixture layer 112 as a sheet with a thickness of 65 μm. ... The negative electrode mixture layer 132, solid electrolyte layer 12, and positive electrode mixture layer 112 obtained above were stacked in this order in a polyethylene die having an inner diameter of 10 mm, and were sandwiched from both the negative electrode mixture layer 132 side and the positive electrode mixture layer 112 side with a SUS punch at a pressure of 100 MPa to bond the negative electrode mixture layer 132, solid electrolyte layer 12, and positive electrode mixture layer 112 to obtain a laminate A. The obtained laminate A was once removed from the die, and the negative electrode lead 131a, copper foil (negative electrode current collector 131), laminate A with the negative electrode mixture layer 132 facing downward, aluminum foil (positive electrode current collector 111), and positive electrode lead 111a were stacked in this order in the die, and the laminate was sandwiched from both the negative electrode lead 131a side and the positive electrode lead 111a side with a SUS punch at a pressure of 1 MPa, and the negative electrode lead 131a, copper foil, laminate A, aluminum foil, and positive electrode lead 111a were joined to obtain an all-solid-state lithium-ion secondary battery 1. (Paragraphs
[0110] to
[0112] ) Furthermore, Patent Document 5 describes that artificial graphite SCMG or SiC manufactured by Showa Denko K.K. was placed in a tumbling fluidized coating device, and mixed at room temperature in a nitrogen atmosphere while spraying a solution prepared by dissolving 22.4 mass% tetraisopropyl orthotitanate, 3.3 mass% ethoxylithium, and 14.4 mass% petroleum pitch in 55.9 mass% absolute ethanol, and the resulting mixture was heat-treated to obtain a composite material (paragraph
[0131] , Table 1). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2016-207418 A [Patent Document 2] WO2020 / 203545 [Patent Document 3] WO2021 / 015147 [Patent Document 4] JP 2019-179669 A [Patent Document 5] JP 2021-101421 A Summary of the Invention [Problem to be solved by the invention]
[0009] The conductive assistant contained in the electrodes disclosed in the above prior art documents is in the form of particles or fibers with a relatively large diameter, and an electrode containing a conductive assistant in the form of small fibers has not been reported so far.
[0010] Therefore, an object of the present invention is to provide an electrode containing a conductive assistant in the form of fibers having a small diameter. [Means for solving the problem]
[0011] An electrode according to one aspect of the present invention comprises an active material layer containing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less.
[0012] A method for manufacturing an electrode according to another aspect of the present invention includes dry-mixing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less to prepare a dry mixture, adding and mixing a binder and a solvent to the dry mixture to prepare a paste, and applying the paste onto a substrate to form an active material layer.
[0013] An electric storage device according to yet another aspect of the present invention includes the electrode according to the above-mentioned aspect of the present invention, and this electric storage device includes an all-solid-state secondary battery. Effect of the Invention
[0014] According to one aspect of the present invention, an electrode can be provided that contains a conductive assistant in the form of fibers having a small diameter.
[0015] The electrode manufacturing method according to another aspect of the present invention can manufacture an electrode having a high content of fibrous conductive assistant having a small diameter. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a stacked-type all-solid-state secondary battery. [Diagram 2] FIG. 2 is a schematic diagram showing an embodiment of an electricity storage device configured by assembling a plurality of electricity storage elements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] [1] An electrode according to one embodiment of the present invention comprises an active material layer containing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less.
[0018] According to the electrode described in [1] above, an electrode containing a fibrous conductive assistant having a small diameter can be provided.
[0019] [2] In the electrode described in the above [1], the active material layer may be formed by applying a paste.
[0020] According to the electrode described in [2] above, it is possible to reduce the size of the energy storage element.
[0021] [3] In the electrode according to the above [1] or [2], the inorganic solid electrolyte may be a sulfide solid electrolyte.
[0022] According to the electrode described in [3] above, an electricity storage element with excellent characteristics can be obtained.
[0023] [4] In another embodiment of the present invention, a method for manufacturing an electrode includes dry-mixing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less to prepare a dry mixture, adding and mixing a binder and a solvent to the dry mixture to prepare a paste, and applying the paste onto a substrate to form an active material layer.
[0024] According to the electrode manufacturing method described in [4] above, an electrode containing a large amount of thin-diameter fibrous conductive assistant can be manufactured.
[0025] [5] An energy storage device according to yet another embodiment of the present invention includes the electrode according to any one of [1] to [3] above.
[0026] [6] The energy storage element described in [5] above may be an all-solid-state secondary battery.
[0027] The configuration of an electrode, the manufacturing method of an electrode, the configuration of an energy storage element, the configuration of an energy storage device, the manufacturing method of an energy storage element, and other embodiments according to one embodiment of the present invention will be described in detail. Note that the names of the components (components) used in each embodiment may differ from the names of the components (components) used in the background art.
[0028] <Electrode configuration> An electrode according to one embodiment of the present invention (hereinafter simply referred to as "electrode") comprises an active material layer containing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less.
[0029] (electrode active material) The electrode active material is either a positive electrode active material or a negative electrode active material. When the electrode active material contains a positive electrode active material, the active material layer becomes a positive electrode active material layer, and the electrode becomes a positive electrode. On the other hand, when the electrode active material contains a negative electrode active material, the active material layer becomes a negative electrode active material layer, and the electrode becomes a negative electrode.
[0030] The positive electrode active material can be appropriately selected from known positive electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the positive electrode active material for a lithium ion secondary battery. Examples of the positive electrode active material include lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. Examples of the lithium transition metal composite oxides having an α-NaFeO2 type crystal structure include Li[Li x Ni (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Co (1-x) ]O2(0≦x<0.5), Li x Ni γ Mn (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), etc. Lithium transition metal composite oxides with spinel crystal structure include Li x Mn2O4, Li x Ni γ Mn (2-γ) O4, etc. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more may be mixed and used.
[0031] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. In addition, when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. The "average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).
[0032] The positive electrode active material may have another substance having ion conductivity on its surface. Examples of the other substance having ion conductivity include LiNbO3, Li2TiO3, Li2Ti2O5, and Li4Ti5O 12 , Li2ZrO3, LiTaO3, etc. The form of the other substance having ion conductivity on the surface of the positive electrode active material is not limited, and may be, for example, a film-like coating or particles attached thereto.
[0033] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both dry and wet methods.
[0034] The content of the positive electrode active material in the positive electrode active material layer is preferably 20% by mass to 90% by mass, more preferably 30% by mass to 85% by mass, and even more preferably 40% by mass to 80% by mass. By setting the content of the positive electrode active material within the above range, it is possible to achieve both a high energy density and a low resistance of the positive electrode active material layer.
[0035] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for lithium ion secondary batteries. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 , LiTiO 2、Examples of the material include titanium-containing oxides such as TiNb2O7, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0036] "Graphite" refers to graphite that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.
[0037] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.
[0038] Here, the "discharged state" refers to a state in which the negative electrode active material carbon material is discharged so that lithium ions that can be absorbed and released during charging and discharging are sufficiently released. For example, in a single-electrode battery using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode, the state is one in which the open circuit voltage is 0.7 V or more.
[0039] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.
[0040] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.
[0041] Metal Li may exist as pure metal Li consisting essentially of lithium element, or as Li alloy containing other metal elements. Examples of Li alloy include Li-Ag alloy, Li-Zn alloy, Li-Ca alloy, Li-Al alloy, Li-Mg alloy, Li-In alloy, etc. Li alloy may contain multiple metal elements other than lithium element.
[0042] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the production or handling of the negative electrode active material becomes easy. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the active material layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverizing method and the classifying method can be selected, for example, from the methods exemplified for the positive electrode active material.
[0043] When a particulate negative electrode active material is used in the negative electrode active material layer, the content of the negative electrode active material is preferably 20% by mass to 80% by mass, more preferably 30% by mass to 70% by mass. By setting the content of the negative electrode active material in the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0044] (Inorganic solid electrolyte) The inorganic solid electrolyte can be appropriately selected from known inorganic solid electrolytes. For example, sulfide solid electrolytes, halide solid electrolytes, oxide solid electrolytes, etc. can be used as the inorganic solid electrolyte. Among these, sulfide solid electrolytes are preferred because they are easily in contact with the electrode active material by plastic deformation. Sulfide solid electrolytes include Li6PS5Cl, Li2S-P2S5, LiI-Li2S-P2S5, and Li 10 Ge-P2S12 , Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-Li3N, Li2S-SiS2, Li2S-S iS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S 2n (where m and n are positive numbers, and Z is Ge, Zn, or Ga.), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers, and M is any of P, Si, Ge, B, Al, Ga, and In.) The halide solid electrolyte is generally represented by the formula Li x M y Compounds represented by X6 are preferred, and examples thereof include Li3YCl6, Li3YBr6, Li3YI6, Li3InCl6, Li3InBr6, Li3InF6, Li2ZrCl6, Li3ErCl6, Li3ErBr6, Li3DyCl6, Li3DyBr6, Li3GdCl6, Li3GdBr6, Li3HoCl6, Li3HoBr6, Li3LaCl6, Li3LaBr6, Li3NdCl6, Li3NdBr6, Li3ScCl6, Li3ScBr6, Li3ScF6, Li3SmCl6, Li3SmBr6, Li3TbCl6, Li3TbBr6, Li3TmCl6, Li3TmBr6, Li3AlF6, Li3TiF6, Li3GaF6, and Li3GeF6. The oxide solid electrolyte is Li7La3Zr2O 12 , Li 0.5 La 0.5 Examples include TiO3, LiTi2(PO4)3, Li3BO3-Li2CO3, Li3BO3-Li2SO4, etc.
[0045] (fibrous conductive additive) The fibrous conductive assistant has a fiber diameter of 1 nm or more and 5 nm or less. It was expected that a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less would easily aggregate or deform due to its small diameter, and would be difficult to uniformly mix with other components of the active material layer. However, contrary to the above expectation, as shown in the examples described later, it was confirmed that an active material layer containing a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less can be formed, and an electrode containing the active material layer and a storage element having the electrode and capable of charging and discharging can be obtained. As the fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less, for example, single-walled carbon nanotubes (SWCNTs) can be used.
[0046] Here, the fiber diameter of the fibrous conductive assistant is determined by the following procedure. A dispersion liquid is prepared by dispersing the fibrous conductive assistant to be measured in ethanol. The dispersion liquid is dropped onto a specimen stage for observation, the ethanol dispersant is dried, and the fiber diameter is measured by observation with a transmission electron microscope (TEM). To measure the fiber diameter, 60 pieces of fibrous conductive assistant are randomly selected, and the diameter of each piece of fibrous conductive assistant is measured by image analysis. The average value of the measured diameters of the 60 pieces of fibrous conductive assistant is taken as the fiber diameter.
[0047] When the fibrous conductive assistant is collected by dismantling the storage element, the following procedure is adopted. The storage element is dismantled to remove the electrodes, and an active material layer containing the fibrous conductive assistant is collected. The active material layer is treated with an acid such as hydrochloric acid that dissolves the electrode active material and the inorganic solid electrolyte, thereby dissolving the electrode active material and the inorganic solid electrolyte contained in the active material layer, and removing them by filtration. The filtered residue is further treated with water or ethanol to dissolve the inorganic solid electrolyte remaining in the residue, and further removed by filtration. By this operation, even if the inorganic solid electrolyte contains a sulfide solid electrolyte, the inorganic solid electrolyte can be sufficiently removed. Next, the filtered residue is treated with a non-polar solvent such as butyl butyrate to dissolve the resin components such as the binder contained in the residue, and further removed by filtration. In this way, the fibrous conductive assistant can be collected. In addition, if the electrode active material and the oxide solid electrolyte are not sufficiently removed, the microwave decomposition treatment may be performed to a degree that does not affect the fiber diameter of the fibrous conductive assistant.
[0048] The lower limit of the content of the fibrous conductive assistant in the active material layer is preferably 0.2 mass% or more, more preferably 0.25 mass% or more, even more preferably 0.3 mass% or more, and even more preferably 0.4 mass% or more. The upper limit of the content of the fibrous conductive assistant in the active material layer is preferably 10 mass% or less, more preferably 5 mass% or less. By setting the content of the fibrous conductive assistant in the above range, the energy density of the energy storage element can be increased.
[0049] (Other components of the active material layer) The active material layer contains optional components such as a binder, a thickener, and a filler, as necessary.
[0050] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.
[0051] The content of the binder in the active material layer is preferably from 0.1% by mass to 10% by mass, more preferably from 0.5% by mass to 9% by mass. By setting the content of the binder in the above range, the electrode active material can be stably maintained.
[0052] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, the functional group may be deactivated in advance by methylation or the like.
[0053] The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, and mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof.
[0054] When the active material layer is a positive electrode active material layer, it may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, I, etc., typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, etc., and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, W, etc., as components other than the positive electrode active material, fibrous conductive assistant, binder, thickener, filler, and solid electrolyte.
[0055] When the active material layer is a negative electrode active material layer, it may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, I, etc., typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, etc., and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, W, etc., as components other than the negative electrode active material, fibrous conductive assistant, binder, thickener, filler, and solid electrolyte.
[0056] (base material) The active material layer may be formed directly on a conductive substrate or via an intermediate layer. Whether or not the active material layer has "conductivity" is determined by whether the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 7 The threshold value is Ω·cm.
[0057] When the electrode is a positive electrode, the material of the substrate is a metal such as aluminum, titanium, tantalum, stainless steel, or an alloy thereof. Among these, aluminum or an aluminum alloy is preferred from the viewpoints of potential resistance, high conductivity, and cost. Examples of the substrate of the positive electrode include foil, vapor deposition film, mesh, and porous material, and foil is preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the substrate of the positive electrode. Examples of aluminum or aluminum alloy include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).
[0058] When the electrode is a positive electrode, the average thickness of the substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and to increase the energy density per volume of the energy storage element.
[0059] When the electrode is a negative electrode, the material of the substrate is copper, nickel, stainless steel, nickel-plated steel, aluminum, or other metals or alloys thereof, carbonaceous materials, etc. Among these, copper or copper alloys are preferred. Examples of the substrate of the negative electrode include foil, vapor deposition film, mesh, and porous material, and foil is preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the substrate of the negative electrode. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0060] When the electrode is a negative electrode, the average thickness of the substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the energy storage element.
[0061] The intermediate layer is a layer disposed between the substrate and the active material layer. The intermediate layer contains a conductive assistant such as carbon particles to reduce the contact resistance between the substrate and the active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.
[0062] The active material layer may be formed by applying a paste. By forming the active material layer by applying a paste, the thickness of the active material layer can be made thin. In addition, the productivity of the electrode is improved. Until now, it was thought that it was more difficult to form an active material layer containing a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less by applying a paste than when other methods are adopted. This is because, when forming an active material layer containing an inorganic solid electrolyte by applying a paste, a non-polar solvent is used as a solvent in the paste to suppress the reaction with the inorganic solid electrolyte. Since a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less has low dispersibility in a non-polar solvent, it was expected that a uniform paste could not be obtained and an active material layer could not be formed by applying a paste. However, contrary to the above expectation, as shown in the examples described later, it was confirmed that an active material layer can be formed by applying a paste, and an electrode containing the active material layer and an electric storage element equipped with the electrode and capable of charging and discharging can be obtained.
[0063] Whether the active material layer is formed by applying a paste is judged by whether the active material layer contains a binder. When the active material layer is formed by pressing, a binder is not necessary, whereas when the active material layer is formed by applying a paste, a binder is necessary. Therefore, when the active material layer contains a binder, it can be strongly inferred that the active material layer is formed by applying a paste. The following procedure is adopted to identify the binder in the active material layer. The active material layer is collected from the electrodes taken out by dismantling the energy storage element, and the binder is dissolved by dispersing it in a non-polar solvent such as butyl butyrate and stirring it. The filtrate can be subjected to pyrolysis gas chromatography / mass spectrometry (Py-GC / MS) to confirm the presence and type of binder.
[0064] <Electrode manufacturing method> An electrode manufacturing method according to one embodiment of the present invention (hereinafter also simply referred to as the "electrode manufacturing method") includes dry-mixing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less to prepare a dry mixture, adding a binder and a solvent to the dry mixture and mixing them to prepare a paste, and applying the paste onto a substrate to form an active material layer.
[0065] According to this electrode manufacturing method, an electrode containing a large amount of thin-diameter fibrous conductive assistant can be manufactured. In addition, an active material layer having superior strength compared to other methods can be formed. Furthermore, by using an electrode obtained by this electrode manufacturing method, an electric storage device having a large initial discharge capacity can be obtained.
[0066] (Preparation of dry mix) The dry mixture is prepared by dry mixing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less. By dry mixing, a dry mixture is obtained in which the inorganic solid electrolyte and the fibrous conductive assistant are attached to the surface of the electrode active material. Various dry composite devices can be used for the dry mixing. Examples of dry composite devices include Nobilta (registered trademark) NOB-MINI manufactured by Hosokawa Micron Corporation and Hybridization System (registered trademark) NHS manufactured by Nara Machinery Co., Ltd.
[0067] (Preparation of paste) The paste is prepared by adding a binder and a solvent to the dry mixture obtained by dry mixing and mixing them. When the inorganic solid electrolyte contains a sulfide solid electrolyte, the solvent to be used is preferably an aliphatic hydrocarbon such as heptane or decane, an aromatic hydrocarbon such as toluene, tetralin, cumene, mesitylene, or anisole, dibutyl ether, diisobutyl ketone, or butyl butyrate. The binder to be used is not particularly limited as long as it is soluble in the above solvent, and for example, polyvinylidene fluoride (PVDF) or styrene butadiene rubber (SBR) can be used. The amount of the solvent used in the paste during the preparation of the paste is preferably 10% by mass or more and 60% by mass or less, more preferably 20% by mass or more and 40% by mass or less. By setting the content of the solvent within the above range, the viscosity of the obtained paste becomes appropriate, and an active material layer having a uniform composition and thickness can be obtained. For mixing, a general mixer such as a dissolver, homomixer, kneader, roll mill, sand mill, attritor, ball mill, vibrator mill, high-speed impeller mill, ultrasonic homogenizer, or shaker can be used.
[0068] When preparing the paste, a fibrous conductive assistant may be added to the dry mixture in addition to the binder and the solvent. The fibrous conductive assistant used in this case may be the fibrous conductive assistant with a fiber diameter of 1 nm to 5 nm used in preparing the dry mixture, or may be a fibrous conductive assistant with a different material, diameter, or length. Examples of the fibrous conductive assistant used in preparing the paste include single-walled carbon nanotubes (SWCNTs), multi-walled carbon nanotubes (MWCNTs), and vapor-grown carbon fibers.
[0069] (Formation of active material layer) The active material layer is formed by applying the prepared paste onto a substrate and drying it. For example, a doctor blade method, a die coating method, a gravure coating method, a spray coating method, an electrostatic coating method, or a bar coating method can be used to form the active material layer.
[0070] <Configuration of Energy Storage Element> An energy storage element (hereinafter, also simply referred to as "energy storage element") according to one embodiment of the present invention comprises an electrode body having a positive electrode, a negative electrode, and a solid electrolyte, and a container for accommodating the same. The electrode body is usually of a laminated type in which a plurality of positive electrodes and a plurality of negative electrodes are laminated with separators interposed therebetween. The electrode body may also be of a so-called "bipolar type" in which a positive electrode active material layer is formed on one surface of a substrate, and a negative electrode active material layer is formed on the other surface.
[0071] FIG. 1 shows an all-solid-state secondary battery 10 as an example of a power storage element. The all-solid-state secondary battery 10 is a secondary battery in which a positive electrode 1 and a negative electrode 2 are arranged with a solid electrolyte layer 3 interposed therebetween. The positive electrode 1 has a positive electrode substrate 4 and a positive electrode active material layer 5. The negative electrode 2 has a negative electrode substrate 7 and a negative electrode active material layer 6. In the all-solid-state secondary battery 10 shown in FIG. 1, the negative electrode active material layer 6, the solid electrolyte layer 3, the positive electrode active material layer 5, and the positive electrode substrate 4 are laminated in this order on the negative electrode substrate 7. The solid electrolyte layer 3 contains a solid electrolyte. As the solid electrolyte, the above-mentioned inorganic solid electrolytes that can be used for electrodes can be used.
[0072] <Configuration of the power storage device> The energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) formed by assembling a plurality of energy storage elements in a power source for an automobile such as an electric vehicle (EV), a hybrid vehicle (HEV), or a plug-in hybrid vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, it is sufficient that the technology of the present invention is applied to at least one energy storage element included in the energy storage unit. 2 shows an example of a power storage device 30 in which power storage units 20, each of which is an assembly of two or more electrically connected all-solid-state secondary batteries 10, are further assembled. The power storage device 30 may include a bus bar (not shown) that electrically connects the two or more all-solid-state secondary batteries 10, a bus bar (not shown) that electrically connects the two or more power storage units 20, and the like. The power storage unit 20 or the power storage device 30 may include a status monitoring device (not shown) that monitors the status of the one or more all-solid-state secondary batteries 10.
[0073] <Method of manufacturing the energy storage element> The manufacturing method of the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, manufacturing a positive electrode and a negative electrode by the above-mentioned electrode manufacturing method, forming a solid electrolyte layer, and stacking the positive electrode and the negative electrode with the solid electrolyte layer interposed therebetween to form an electrode body. The electrode body can also be manufactured by stacking a positive electrode base material, a mixed powder of components of a positive electrode active material layer, a mixed powder of components of a solid electrolyte layer, a mixed powder of components of a negative electrode active material layer, and a negative electrode base material in this order, and simultaneously compression-molding them.
[0074] <Other embodiments> The energy storage element of the present invention is not limited to the above-described embodiment, and various modifications may be made without departing from the scope of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and a part of the configuration of one embodiment may be replaced with the configuration of another embodiment or a well-known technique. Furthermore, a part of the configuration of one embodiment may be deleted. Also, a well-known technique may be added to the configuration of one embodiment.
[0075] In the above embodiment, the case where the energy storage element is used as a chargeable and dischargeable all-solid-state secondary battery (for example, a lithium-ion all-solid-state secondary battery) having a solid electrolyte layer has been described, but the type, shape, size, capacity, etc. of the energy storage element are arbitrary. The present invention can also be applied to various secondary batteries, electric double layer capacitors, lithium ion capacitors, and other capacitors. EXAMPLES
[0076] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0077] [Example 1] (Preparation of electrodes) The positive electrode active material is LiNi 0.5 Co 0.2 Mn 0.3 A powder (average particle size 10 μm) composed of particles in which the surface of lithium transition metal composite oxide particles represented by O2 (NCM523) was coated with LiNbO3 was prepared. A sulfide solid electrolyte represented by the composition formula Li6PS5Cl was prepared as a solid electrolyte. Single-walled carbon nanotubes (SWCNTs) (TUBALL, manufactured by Kusumoto Chemical Co., Ltd.) were prepared as a fibrous conductive assistant with a fiber diameter of 1 nm to 5 nm. The solid electrolyte, the fibrous conductive assistant, and butyl butyrate in which SBR was dissolved as a binder were added and kneaded to prepare a paste. The amount of the fibrous conductive assistant in the paste was 0.2 mass% relative to the positive electrode active material. The ratio of each component in the paste was (positive electrode active material): (solid electrolyte): (fibrous conductive assistant): (binder) = 76: 22.8: 0.2: 1 in terms of solid content. The obtained paste was applied to an aluminum foil (average thickness 20 μm) as a positive electrode substrate using a multi-applicator (MA100, manufactured by Cortec Co., Ltd.) so that the solid content was 15 mg cm -2 More than 25mg cm -2 The coating was performed as follows. The coating was dried in a dryer in an argon atmosphere set at a temperature at which butyl butyrate volatilized, to form a positive electrode active material layer on the positive electrode substrate. The positive electrode active material layer was punched out into a circle with a diameter of 10 mm to obtain the positive electrode according to Example 1.
[0078] (Fabrication of Energy Storage Element) As the solid electrolyte, a powder of a sulfide solid electrolyte represented by the composition formula Li6PS5Cl was prepared. 80 mg of the sulfide solid electrolyte was inserted into a ceramic powder molding machine with an inner diameter of 10 mm, and pressure molding was performed by uniaxial pressing at room temperature for several seconds at a pressure of 100 MPa to form a solid electrolyte layer. After releasing the pressure, the positive electrode according to Example 1 was placed on one side of the solid electrolyte layer, and pressure molding was performed at 160°C for 5 minutes at a pressure of 360 MPa. After releasing the pressure, indium foil (average thickness 300 μm, diameter 8 mm, manufactured by Nilaco) and lithium foil (average thickness 300 μm, diameter 6 mm, manufactured by Honjo Metal Co., Ltd.) as a negative electrode, and SUS316 foil (manufactured by Nilaco) as a negative electrode substrate were placed on the surface opposite to the bonding surface of the positive electrode, and bonded by uniaxial pressing at room temperature for several seconds at a pressure of 50 MPa. This was removed from the ceramic powder molding machine to obtain an all-solid-state secondary battery as an energy storage element according to Example 1.
[0079] [Comparative Example 1] An attempt was made to prepare an electrode in the same manner as in Example 1, except that the amount of fibrous conductive additive in the paste was 0.4 mass% relative to the positive electrode active material, and the ratio of each component in the paste was (positive electrode active material):(solid electrolyte):(fibrous conductive additive):(binder)=76:22.6:0.4:1 in terms of mass ratio of solid content. However, a uniform paste was not obtained, and an active material layer could not be formed on the substrate.
[0080] [Example 2] (Preparation of electrodes) The positive electrode active material is LiNi 0.5 Co 0.2 Mn 0.3A powder (average particle size 10 μm) composed of particles in which the surface of a lithium transition metal composite oxide particle represented by O2 (NCM523) was coated with LiNbO3 was prepared. A sulfide solid electrolyte represented by the composition formula Li6PS5Cl was prepared as a solid electrolyte. Single-walled carbon nanotubes (SWCNTs) (TUBALL, manufactured by Kusumoto Chemical Co., Ltd.) were prepared as a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less. In a glove box in an argon atmosphere, the positive electrode active material, the solid electrolyte, and the SWCNTs were dry-mixed in a mass ratio of (positive electrode active material):(solid electrolyte):(SWCNT) = 95:4.2:0.8 using a dry composite device (Nobilta (registered trademark) NOB-MINI, manufactured by Hosokawa Micron Corporation), to obtain a dry mixture in which the solid electrolyte and the fibrous conductive assistant were attached to the surface of the positive electrode active material particles. The solid electrolyte, the fibrous conductive assistant, and butyl butyrate in which SBR was dissolved as a binder were added to this dry mixture and kneaded to prepare a paste. The amount of the fibrous conductive assistant in the paste was 0.2 mass% relative to the positive electrode active material. The ratio of each component in the paste was (positive electrode active material):(solid electrolyte):(fibrous conductive assistant):(binder)=76:22:1:1 in terms of mass ratio of solid content. The obtained paste was applied to a positive electrode substrate in the same manner as in Example 1, and then dried and punched to obtain a positive electrode according to Example 2.
[0081] (Fabrication of Energy Storage Element) An all-solid-state secondary battery according to Example 2 was obtained in the same manner as in Example 1, except that the positive electrode according to Example 2 was used.
[0082] [Example 3] A positive electrode and an all-solid-state secondary battery according to Example 3 were obtained in the same manner as in Example 2, except that the fibrous conductive assistant added to the dry mixture during the preparation of the paste was a multi-walled carbon nanotube (MWCNT) having a fiber diameter of 10 nm to 20 nm (C2150, manufactured by Tokyo Chemical Industry Co., Ltd.).
[0083] [Example 4] A positive electrode and an all-solid-state secondary battery according to Example 4 were obtained in the same manner as in Example 2, except that the fibrous conductive assistant added to the dry mixture when preparing the paste was vapor-grown carbon fiber having a fiber diameter of 150 nm (VGCF (registered trademark), manufactured by Showa Denko K.K.).
[0084] [Example 5] A positive electrode and an all-solid-state secondary battery according to Example 5 were obtained in the same manner as in Example 2, except that the fibrous conductive assistant added to the dry mixture during the preparation of the paste was carbon nanofiber (CNF) (Sigma-Aldrich, 719781) having a fiber diameter of 100 nm.
[0085] <Evaluation> (Strength of active material layer) The strength of the active material layer in the positive electrode according to each Example was evaluated by the following procedure. Each of the positive electrodes according to Examples 1 to 5 was cut into a size of 2 cm x 2 cm using a trimming cutter to prepare a test piece. The test piece was wrapped around a glass bottle with a diameter of 4 cmφ, and the presence or absence of peeling of the active material layer was observed to evaluate the strength.
[0086] As a result of the above evaluation, peeling of the active material layer from the substrate was confirmed in the positive electrode of Example 1, whereas peeling of the active material layer from the substrate was not confirmed in each of the positive electrodes of Examples 2 to 4.
[0087] (Initial discharge capacity) For the all-solid-state secondary batteries according to each example, an initial charge and discharge was carried out at 50° C. in the following manner, and the initial discharge capacity was measured. Constant current / constant voltage charging was performed with a charging current of 0.1 C and a charge cut-off voltage of 3.75 V. The charge was terminated when the charging current reached 0.025 C. A rest period of 10 minutes was then provided. After that, constant current discharging was performed with a discharge current of 0.1 C and a discharge cut-off voltage of 2.25 V, and the discharge capacity was recorded as the initial discharge capacity. The obtained initial discharge capacity values are shown in Table 1, together with the type of fibrous conductive assistant used in producing the positive electrode and its mass percentage relative to the positive electrode active material.
[0088] [Table 1]
[0089] As shown in Table 1, it was confirmed that an active material layer containing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less can be formed, and an electrode containing the active material layer and a chargeable and dischargeable electricity storage element having the electrode can be obtained. In particular, it was confirmed that an electricity storage element having a large initial discharge capacity can be obtained by an electrode produced through dry mixing of an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less to produce a dry mixture, adding and mixing a binder and a solvent to the dry mixture to produce a paste, and applying the paste onto a substrate to form an active material layer. [Explanation of symbols]
[0090] 1 positive electrode 2 negative electrode 3 Solid electrolyte layer 4. Positive electrode substrate 5 Cathode active material layer 6 Negative electrode active material layer 7. Negative electrode substrate 10 All-solid-state secondary battery 20 Energy Storage Unit 30 Energy storage device
Claims
1. electrode active material, Inorganic solid electrolytes, and A fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less. An active material layer containing An electrode comprising:
2. The electrode according to claim 1 , wherein the active material layer is formed by applying a paste.
3. 2. The electrode of claim 1, wherein the inorganic solid electrolyte is a sulfide solid electrolyte.
4. Dry-mixing an electrode active material, an inorganic solid electrolyte, and a fibrous conductive assistant having a fiber diameter of 1 nm or more and 5 nm or less to prepare a dry mixture; adding and mixing a binder and a solvent to the dry mixture to form a paste; and Applying the paste onto a substrate to form an active material layer. A method for manufacturing an electrode, comprising:
5. An energy storage element comprising the electrode according to claim 1 .
6. The energy storage element according to claim 5 , which is an all-solid-state secondary battery.
Citation Information
Patent Citations
Electrode mixture
JP2016207418A
Method for manufacturing all-solid battery, and all-solid battery
JP2019179669A
Composite material, manufacturing method thereof, negative electrode material for lithium ion secondary battery, negative electrode, and secondary battery
JP2021101421A
Composite electrode active material, electrode composition, electrode sheet for all-solid-state secondary battery and all-solid-state secondary battery, and methods for manufacturing composite electrode active material, electrode sheet for all-solid-state secondary battery, and all-solid-state secondary battery
WO2020203545A1
Composite electrode material, electrode layer, and solid-state battery
WO2021015147A1