Positive electrode material for lithium-ion secondary battery, positive electrode for lithium-ion secondary battery, and manufacturing method for positive electrode material for lithium-ion secondary battery

The use of a carbon-coated olivine-type lithium manganese iron phosphate with controlled particle size and pore volume addresses the cracking issue in lithium ion secondary batteries, enabling a higher basis weight and improved battery capacity.

JP2024156422AActive Publication Date: 2024-11-06TOYOTA INDUSTRIES CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023070867
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

The use of olivine-type cathode active materials in lithium ion secondary batteries, particularly olivine-type lithium manganese iron phosphate (LiMnFePO4), results in cracking of the cathode active material layer due to shrinkage during the drying process, limiting the ability to increase the capacity of the battery.

Method used

A positive electrode material composed of olivine-type lithium manganese iron phosphate with a carbon film coating on aggregated primary particles, having a specific particle size and pore volume, is used to form a thick coating film that suppresses cracking and enhances film formability and battery characteristics.

Benefits of technology

The solution allows for a higher basis weight of the positive electrode active material layer, improving film formability and increasing the capacity of the lithium ion secondary battery while maintaining battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156422000001_ABST
    Figure 2024156422000001_ABST
Patent Text Reader

Abstract

To improve both film formability and battery characteristics when the coating weight of a positive electrode active substance layer containing olivine-type lithium manganese iron phosphate is increased.SOLUTION: A positive electrode material for a lithium-ion secondary battery includes a granulated body 10 having: a core 11 composed of olivine-type lithium manganese iron phosphate represented by the general formula LiMnxFeyPO4 (x and y are numerical values satisfying x+y=1, 0<x<1, and 0<y<1 ); and a carbon coating 12 formed on a surface of the core 11. The core 11 has a structure in which primary particles of olivine-type lithium manganese iron phosphate are aggregated. The particle size of the primary particles is 100 nm or less. A pore volume in a pore size range of 2 nm or more and 300 nm or less in the granulated body 10 is 0.2 cm3 / g or less, and a carbon content of the granulated body is 1.8 mass% or more and 3.0 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode material for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a method for producing a positive electrode material for a lithium ion secondary battery. [Background technology]

[0002] Patent Document 1 discloses an electricity storage device including a positive electrode using olivine-type lithium iron phosphate (LiFePO4) as a positive electrode active material. Olivine-type structure positive electrode active materials, such as olivine-type lithium iron phosphate, are positive electrode active materials with excellent thermal stability. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-185920 A Summary of the Invention [Problem to be solved by the invention]

[0004] The positive electrode of the lithium ion secondary battery is manufactured, for example, as follows. First, a positive electrode composite material in a slurry form containing a positive electrode active material, a binder, and a solvent is applied to the surface of a positive electrode current collector. Next, the coating film formed by coating is dried to form a positive electrode active material layer on the surface of the positive electrode current collector. Here, as a method for increasing the capacity of the lithium ion secondary battery, it is considered to increase the basis weight of the positive electrode active material layer by thickly coating the coating film of the positive electrode composite material in the above manufacturing process. However, when an olivine-type structure positive electrode active material is used as the positive electrode active material, there is a problem that the resulting positive electrode active material layer is likely to crack due to shrinkage of the coating film during drying. In particular, when olivine-type lithium manganese iron phosphate (LiMnFePO4) is used among olivine-type structure positive electrode active materials, the above problem is likely to occur. [Means for solving the problem]

[0005] The cathode material for a lithium ion secondary battery for solving the above problems is composed of a core composed of olivine-type lithium manganese iron phosphate represented by the general formula LiMn x Fe y PO4 (where x and y are numerical values satisfying x + y = 1, 0 < x < 1, and 0 < y < 1), and a carbon coating formed on the surface of the core, and the core has a structure in which primary particles of the olivine-type lithium manganese iron phosphate are aggregated. The particle size of the primary particles is 100 nm or less, and the pore volume in the range of pore diameters of 2 nm or more and 300 nm or less in the granulated body is 0.2 cm 3 / g or less, and the carbon content of the granulated body is 1.8% by mass or more and 3.0% by mass or less.

[0006] The cathode for a lithium ion secondary battery for solving the above problems includes a cathode current collector having a first surface and a cathode active material layer formed on the first surface of the cathode current collector, and the cathode active material layer contains the cathode material for the lithium ion secondary battery described above.

[0007] In the cathode for the lithium ion secondary battery described above, the basis weight of the cathode active material layer is preferably 30 mg / cm 2 or more and 100 mg / cm 2 or less. A method for manufacturing a cathode material for a lithium ion secondary battery for solving the above problems includes a step of preparing a slurry containing a pulverized product of olivine-type lithium manganese iron phosphate by pulverizing particles of olivine-type lithium manganese iron phosphate represented by the general formula LiMn x Fe y PO4 (where x and y are numerical values satisfying x + y = 1, 0 < x < 1, and 0 < y < 1) in the presence of an aqueous solvent, a carbon source, and a carboxylic acid, a step of obtaining aggregates of the pulverized product by spray-drying the slurry, and a step of carbonizing the carbon source contained in the aggregates by firing the aggregates.

[0008] In the above-mentioned method for producing a positive electrode material for a lithium ion secondary battery, the carboxylic acid is preferably citric acid. In the method for producing a positive electrode material for a lithium ion secondary battery, the content of the carboxylic acid in the slurry is preferably 2 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the olivine-type lithium manganese iron phosphate. Effect of the Invention

[0009] According to the present invention, it is possible to achieve both improved film formability and improved battery characteristics when the basis weight of a positive electrode active material layer containing olivine-type lithium manganese iron phosphate is increased. [Brief description of the drawings]

[0010] [Figure 1] 1 is a micrograph of a cross section of a granule. [Diagram 2] FIG. 2 is a schematic diagram showing the structure of a primary particle in a cross section of a granule. [Diagram 3] FIG. [Figure 4] 1(a) is a photograph of the positive electrode active material layer using Example 1, and (b) is a photograph of the positive electrode active material layer using Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will now be described with reference to the drawings. In the following, a positive electrode material for a lithium ion secondary battery and a positive electrode of a lithium ion secondary battery will be abbreviated to a positive electrode material and a positive electrode, respectively.

[0012] <Cathode materials> 1, the positive electrode material of this embodiment includes a granule 10 having a core 11 made of olivine-type lithium manganese iron phosphate and a carbon coating 12 formed on the surface of the core 11. The positive electrode material may be composed only of the granule 10, or may contain components other than the granule 10 as necessary.

[0013] The olivine-type lithium manganese iron phosphate that constitutes the core 11 is a polyanion compound having an olivine-type structure represented by the general formula LiMn x Fe y PO4. The olivine-type lithium manganese iron phosphate that constitutes the core 11 is a polyanion compound having an olivine-type structure represented by the general formula LiMn x Fe y PO4. In LiMn

[0014] Figure 2 schematically shows the structure of the range indicated by the arrow A in Figure 1. As shown in Figure 2, the core 11 has a structure in which the primary particles 11a of olivine-type lithium manganese iron phosphate are aggregated. Further, the core 11 has pores 11b formed between the plurality of primary particles 11a.

[0015] The particle diameter of the primary particle 11a is 100 nm or less, preferably 80 nm or less. Further, the particle diameter of the primary particle 11a is, for example, 20 nm or more. The particle diameter of the primary particle 11a is a value obtained by the small angle X-ray scattering method (SAXS). More specifically, the particle diameter of the primary particle 11a is defined as the average particle diameter (D50) obtained from the particle diameter distribution of the primary particle 11a assuming the primary particle 11a is spherical.

[0016] In the core 11, the pore volume in the pore diameter range of 2 nm or more and 300 nm or less is 0.2 cm 3 / g or less, preferably 0.15 cm 3 / g or less. Further, the above-mentioned pore volume is, for example, 0.05 cm 3 / g or more, preferably 0.1 cm 3 / g or more. The pore volume can be determined by performing nitrogen adsorption / desorption measurement on the granule 10 and using the BJH (Barrett Joyner Hallenda) method. The pore volume described below refers to the pore volume in the pore diameter range of 2 nm or more and 300 nm or less.

[0017] The carbon content in the granules 10 is 1.8% by mass or more, preferably 1.9% by mass or more, and more preferably 2.0% by mass or more. If the carbon content is less than 1.8%, the carbon coating 12 will not be able to cover the entire surface of the core 11. In this case, the surface of the core 11 will be partially exposed, which will deteriorate the film-forming properties when forming the active material layer described below. The carbon content is 3.0% by mass or less, and preferably 2.7% by mass or less. The carbon content can be measured using a carbon / sulfur analyzer (CS meter).

[0018] The content of the olivine-type lithium manganese iron phosphate in the granules 10 is, for example, 95% by mass or more, and preferably 96% by mass or more. Also, the content is 99% by mass or less, and preferably 98% by mass or less.

[0019] The granules 10 may contain other components in addition to the olivine-type lithium manganese iron phosphate and carbon. In this case, the content of the other components is, for example, 2% by mass or less.

[0020] The average particle size (D50) of the granules 10 is, for example, 3.0 μm or more, and preferably 5.0 μm or more. The average particle size (D50) of the granules 10 is, for example, 30 μm or less, and preferably 20 μm or less. The average particle size of the granules 10 can be measured, for example, using a laser diffraction particle size analyzer.

[0021] <Method of manufacturing positive electrode material> Next, an example of a method for producing a positive electrode material will be described. An example of a method for manufacturing a positive electrode material includes a mixing step, a pulverizing step, a drying step, and a firing step. The positive electrode material is manufactured by sequentially undergoing the mixing step, the pulverizing step, the drying step, and the firing step.

[0022] [Mixing step] The mixing step is a step of producing a first slurry by mixing particles of olivine-type lithium manganese iron phosphate, an aqueous solvent, a carbon source, and a carboxylic acid.

[0023] The particles of olivine-type lithium manganese iron phosphate are particles of a polyanion compound having an olivine-type structure represented by the general formula LiMn x Fe y PO4. In the general formula LiMn x Fe y PO4, x and y are numerical values that satisfy x + y = 1, 0 < x < 1, and 0 < y < 1. Specific examples of the ranges of x and y include the cases where 0.5 ≤ x ≤ 0.9, 0.1 ≤ y ≤ 0.5, and the cases where 0.6 ≤ x ≤ 0.8, 0.2 ≤ y ≤ 0.4. The olivine-type lithium manganese iron phosphate constituting the particles of olivine-type lithium manganese iron phosphate may be one type or two or more types.

[0024] The average particle diameter (D50) of the above particles is, for example, 3.0 μm or more, preferably 5.0 μm or more. Also, the average particle diameter (D50) of the above particles is, for example, 30 μm or less, preferably 20 μm or less.

[0025] Particles of olivine-type lithium manganese iron phosphate can be produced, for example, as follows. First, a first precursor slurry is prepared by mixing a Li source such as lithium hydroxide, a Mn source such as a manganese compound, an Fe source such as an iron compound, and a PO4 source such as orthophosphoric acid with water. Next, the Li source, Mn source, and Fe source contained in the first precursor slurry are pulverized using a pulverizer such as a bead mill. This results in a second precursor slurry containing the pulverized Li source, Mn source, and Fe source. Next, the second precursor slurry is dried by a spray drying method or the like to obtain a particulate dried precursor. The obtained dried precursor is fired at a temperature of, for example, about 500°C to obtain the above particles.

[0026] The aqueous solvent is water or a mixed solvent of water and a non-aqueous solvent. The water is not particularly limited, but is preferably, for example, ion-exchanged water, which is water treated with an ion-exchange resin, and ultrapure water, which is water treated by a reverse osmosis membrane water purification system. Examples of the non-aqueous solvent constituting the mixed solvent include solvents that are miscible with water, such as lower alcohols, acetone, tetrahydrofuran, ethylene glycol, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, acetonitrile, and dimethylsulfoxide. The non-aqueous solvent may be used alone or in combination of two or more. The volume ratio of water in the mixed solvent is, for example, preferably 50% by volume or more and 99.9% by volume or less, and more preferably 60% by volume or more and 99% by volume or less.

[0027] As the carbon source, for example, an organic compound can be used. As the organic compound, for example, glucose, fructose, galactose, mannose, maltose, sucrose, lactose, glycogen, pectin, alginic acid, glucomannan, chitin, hyaluronic acid, chondroitin, agarose, polyether, polyhydric alcohol, polyvinyl alcohol, polyvinylpyrrolidone, cellulose, starch, gelatin, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, polystyrene sulfonic acid, polyacrylamide, and polyvinyl acetate can be mentioned. As the polyhydric alcohol, for example, polyethylene glycol, polypropylene glycol, polyglycerin, and glycerin can be mentioned. As the carbon source, one kind may be used alone, or two or more kinds may be used in combination.

[0028] Examples of carboxylic acids include citric acid, formic acid, acetic acid, propionic acid, butanoic acid, pentanoic acid, malic acid, fumaric acid, tartaric acid, ascorbic acid, gluconic acid, and polyacrylic acid. Carboxylic acids may be used alone or in combination of two or more. Among these carboxylic acids, it is preferable to use citric acid. Details of this point will be described later.

[0029] Next, the blending amounts of the olivine-type lithium manganese iron phosphate particles, the aqueous solvent, the carbon source, and the carboxylic acid in the first slurry will be described. The amount of the aqueous solvent is, for example, 40 parts by mass or more, preferably 50 parts by mass or more, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles, and is, for example, 80 parts by mass or less, preferably 70 parts by mass or less, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles.

[0030] The amount of the carboxylic acid is, for example, 2 parts by mass or more, preferably 3 parts by mass or more, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The amount of the carboxylic acid is, for example, 15 parts by mass or less, preferably 12 parts by mass or less, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. In addition, within a range below a specific amount, the pore volume of the core 11 of the granule 10 decreases as the amount of the carboxylic acid increases. In addition, the pore size distribution of the core 11 of the granule 10 shifts to the smaller diameter side as the amount of the carboxylic acid increases. Therefore, the pore volume of the core 11 of the granule 10 can be controlled by adjusting the amount of the carboxylic acid.

[0031] In the mixing step, the carbon source is blended with the olivine-type lithium manganese iron phosphate particles so that the total carbon amount, which is the total mass of the carbon in the carbon source and the carbon in the carboxylic acid, is a specific amount. Therefore, the blending amount of the carbon source is, for example, an amount in which the total carbon amount is 1.8 parts by mass or more, preferably 1.9 parts by mass or more, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The blending amount of the carbon source is, for example, an amount in which the total carbon amount is 5.0 parts by mass or less, preferably 3.0 parts by mass or less, per 100 parts by mass of the olivine-type lithium manganese iron phosphate particles. The carbon content of the granules 10 can be controlled by adjusting the total carbon amount based on the blending amount of the carbon source.

[0032] The first slurry may contain other components in addition to the olivine-type lithium manganese iron phosphate particles, the aqueous solvent, the carbon source, and the carboxylic acid, such as a dispersant.

[0033] [Crushing process] The pulverization step is a step of pulverizing the olivine-type lithium manganese iron phosphate particles contained in the first slurry to prepare a second slurry containing the pulverized particles. The pulverization step corresponds to a step of pulverizing the olivine-type lithium manganese iron phosphate particles in the presence of an aqueous solvent, a carbon source, and a carboxylic acid to prepare a second slurry.

[0034] The average particle diameter (D50) of the pulverized product of the above particles is, for example, 20 nm or more, preferably 30 nm or more. The average particle diameter (D50) of the pulverized product of the above particles is, for example, 100 nm or less, preferably 90 nm or less. By reducing the average particle diameter (D50) of the pulverized product of the above particles, the particle diameter of the primary particles 11a of the granules 10 can be reduced.

[0035] The pulverization method used in the pulverization step is not particularly limited as long as it can pulverize the olivine-type lithium manganese iron phosphate particles in the first slurry. Examples of the pulverization method include a method using a pulverizer such as a bead mill, a hammer mill, an agitation mill, a jet mill, or a ball mill. The temperature during pulverization is, for example, 10°C or higher and 50°C or lower.

[0036] Here, when the olivine-type lithium manganese iron phosphate particles are pulverized, some of the metals (Li, Mn, and Fe) contained in the particles are dissolved into the slurry. In the subsequent firing step, the dissolved metals cause necking between the particles of the pulverized material, i.e., between the primary particles 11a constituting the core 11 of the granules 10, with the metals acting as neck portions. If a positive electrode material containing the granules 10 in which a lot of necking occurs is used for the positive electrode of a lithium-ion secondary battery, the battery performance of the lithium-ion secondary battery will be reduced.

[0037] In this embodiment, the occurrence of the necking is suppressed by the first slurry containing carboxylic acid. That is, in the slurry, the eluted metal is captured by carboxylic acid, so that the contact of the eluted metal with the surface of the pulverized olivine-type lithium manganese iron phosphate particles, particularly with the newly formed surface formed by pulverization, is suppressed. As a result, the occurrence of necking between the pulverized particles, in which the eluted metal forms a neck portion, is suppressed.

[0038] Therefore, from the viewpoint of suppressing the occurrence of necking, it is preferable that the carboxylic acid used in the first slurry has a high ability to capture the eluted metals Li, Mn, and Fe. The binding energies of various carboxylic acids with Li, Mn, and Fe are shown in Table 1 below. The binding energy values ​​shown in Table 1 below are values ​​calculated as the difference in energy before and after the formation of a complex between the carboxylic acid and each of the eluted metals, and the smaller the value, the higher the ability to capture the corresponding eluted metal. The binding energy values ​​shown in Table 1 below are calculated using CAE (Computer Aided Engineering). As shown in Table 1, citric acid has the lowest binding energy with respect to all of the eluted metals Li, Mn, and Fe. Therefore, from the viewpoint of suppressing the occurrence of necking, it is preferable to use citric acid as the carboxylic acid.

[0039] [Table 1] [Drying process] The drying step is a step of obtaining an aggregate of the pulverized material by spray-drying the second slurry. Examples of the spraying method in the spray drying include a spraying method using a disk type, a pressurized nozzle, a pressurized two-fluid nozzle, a pressurized four-fluid nozzle, etc. The spraying temperature in the spray drying is, for example, 180°C or more and 300°C or less.

[0040] [Firing process] The firing step is a step of firing the aggregate obtained in the drying step to carbonize the carbon source contained in the aggregate. The firing conditions in the firing step are not particularly limited as long as the carbon source can be carbonized. The firing temperature in the firing step is, for example, 500°C or higher and 750°C or lower. The firing time in the firing step is, for example, 1 hour or higher and 12 hours or lower. The atmosphere in the firing step is, for example, a non-oxidizing atmosphere. Examples of the non-oxidizing atmosphere include an inert atmosphere such as nitrogen (N2) or argon (Ar), and a reducing atmosphere containing a reducing gas such as hydrogen (H2).

[0041] <Positive electrode> Next, a positive electrode 100 containing the positive electrode material of this embodiment will be described. As shown in FIG. 3, the positive electrode 100 includes a positive electrode current collector 101 having a first surface 101a, and a positive electrode active material layer 102 formed on the first surface 101a of the positive electrode current collector 101.

[0042] [Positive electrode current collector] The positive electrode current collector 101 is a chemically inactive electrical conductor for continuing to pass current through the positive electrode active material layer 102 during discharging or charging of the lithium ion secondary battery. The positive electrode current collector 101 is, for example, in the form of a foil. The thickness of the foil-shaped positive electrode current collector 101 is, for example, 1 μm or more, and preferably 10 μm or more. The thickness of the foil-shaped positive electrode current collector 101 is, for example, 100 μm or less, and preferably 60 μm or less.

[0043] Examples of materials constituting the positive electrode current collector 101 include metal materials, conductive resin materials, and conductive inorganic materials. Examples of the metal materials include copper, aluminum, nickel, titanium, and stainless steel. Examples of the conductive resin materials include resins in which a conductive filler is added to a conductive polymer material or a non-conductive polymer material as necessary. The positive electrode current collector 101 may include multiple layers including one or more layers containing the above metal materials or conductive resin materials.

[0044] An example of the positive electrode current collector 101 is an aluminum current collector. The aluminum current collector may be made of aluminum alone or an aluminum alloy. Examples of the aluminum alloy include an Al-Mn alloy, an Al-Mg alloy, and an Al-Mg-Si alloy.

[0045] The first surface 101a of the positive electrode current collector 101 may be covered with a known protective layer such as a carbon coating layer. The first surface 101a of the positive electrode current collector 101 may be treated by a known method such as plating.

[0046] [Cathode active material layer] The positive electrode active material layer 102 is provided on the first surface 101a of the positive electrode current collector 101. The weight of the positive electrode active material layer 102 is, for example, 20 mg / cm 2 or more, preferably 30 mg / cm 2 The weight of the positive electrode active material layer 102 is, for example, 150 mg / cm 2 or less, preferably 100 mg / cm 2 The thickness of the positive electrode active material layer 102 is, for example, 80 μm or more, and preferably 100 μm or more. The thickness of the positive electrode active material layer 102 is, for example, 1000 μm or less, and preferably 800 μm or less.

[0047] The positive electrode active material layer 102 includes a positive electrode active material capable of absorbing and releasing charge carriers such as lithium ions. The positive electrode active material layer 102 includes the above-mentioned granules 10 as a positive electrode active material. The positive electrode active material layer 102 may include other positive electrode active materials other than the granules 10. Examples of other positive electrode active materials include lithium composite metal oxides having a layered rock salt structure, metal oxides having a spinel structure, and polyanion-based compounds other than olivine-type lithium manganese iron phosphate. The other positive electrode active materials may be used alone or in combination of two or more. When the other positive electrode active materials are included, the mass ratio of the granules 10 to the entire positive electrode active material is preferably 50% or more, and more preferably 90% or more.

[0048] The content of the positive electrode active material in the positive electrode active material layer 102 is not particularly limited. The content of the positive electrode active material in the positive electrode active material layer 102 is, for example, 95 mass % or more, and preferably 96 mass % or more. The content of the positive electrode active material in the positive electrode active material layer 102 is, for example, 99.5 mass % or less, and preferably 99 mass % or less.

[0049] The positive electrode active material layer 102 may further contain, as necessary, a conductive assistant for enhancing electrical conductivity, a binder, an electrolyte (such as a polymer matrix, an ion-conductive polymer, or a liquid electrolyte), an electrolyte supporting salt (lithium salt) for enhancing ion conductivity, and the like.

[0050] The conductive assistant is added to increase the conductivity of the positive electrode 100. Examples of the conductive assistant include acetylene black, carbon black, graphite, and carbon nanotubes.

[0051] Examples of the binder include fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene, and fluorine rubber, thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamideimide, alkoxysilyl group-containing resins, acrylic resins such as polyacrylic acid and polymethacrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, alginates such as sodium alginate and ammonium alginate, water-soluble cellulose ester crosslinkers, and starch-acrylic acid graft polymers. These binders can be used alone or in combination. Examples of the solvent or dispersion medium include water and N-methyl-2-pyrrolidone.

[0052] <Manufacturing method of positive electrode> Next, an example of a method for producing the positive electrode 100 will be described. An example of a method for producing the positive electrode 100 includes a mixing step of preparing a positive electrode mixture, and an active material layer forming step of forming a positive electrode active material layer using the positive electrode mixture. The positive electrode 100 is produced by sequentially passing through the mixing step and the active material layer forming step.

[0053] [Preparation process] The preparation step is a step of preparing a positive electrode mixture that will become the positive electrode active material layer 102 when solidified. The positive electrode mixture is a slurry containing a positive electrode active material, an aqueous binder, and an aqueous solvent.

[0054] The positive electrode active material mixed in the positive electrode mixture is the same as the positive electrode active material described in the explanation section for the positive electrode 100 . The content of the positive electrode active material in the positive electrode composite is, for example, 70 parts by mass or more and 99 parts by mass or less, and preferably 90 parts by mass or more and 98 parts by mass or less, when the total mass of the solid contents contained in the positive electrode composite, i.e., the mass of the positive electrode composite excluding the aqueous solvent (hereinafter referred to as the solid content mass), is taken as 100 parts by mass.

[0055] The aqueous binder is a binder that is soluble or dispersible in an aqueous solvent, and is used by mixing the aqueous binder with the positive electrode active material in a dispersed or dissolved state in the aqueous solvent. The aqueous binder is not particularly limited, and any conventionally known material can be used as the aqueous binder contained in the positive electrode active material layer of the lithium ion secondary battery.

[0056] Examples of the aqueous binder include fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene, and fluorine rubber, thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamideimide, alkoxysilyl group-containing resins, acrylic resins such as poly(meth)acrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, alginates such as sodium alginate and ammonium alginate, water-soluble cellulose ester crosslinked bodies, and starch-acrylic acid graft polymers. The aqueous binder contained in the positive electrode active material layer 102 may be one type or two or more types.

[0057] The content of the aqueous binder in the positive electrode mixture is, for example, 1 part by mass to 30 parts by mass, and preferably 1 part by mass to 5 parts by mass, when the solid content mass is 100 parts by mass. The aqueous solvent contained in the positive electrode mixture may be the same as that used in the manufacturing method of the positive electrode material. The content of the aqueous solvent in the positive electrode mixture is not particularly limited, but is, for example, a content that makes the solid content of the positive electrode mixture 30 to 60 mass%.

[0058] The positive electrode mixture may contain optional components, such as a conductive assistant for enhancing electrical conductivity, an electrolyte (polymer matrix, ion-conductive polymer, electrolyte solution, etc.), and an electrolyte supporting salt (lithium salt) for enhancing ion conductivity, as necessary.

[0059] [Active material layer formation process] The active material layer forming step is a step of forming a positive electrode active material layer 102 on the first surface 101a of the positive electrode current collector 101 using the above-mentioned positive electrode mixture.

[0060] In the active material layer formation process, the method of forming the positive electrode active material layer 102 on the first surface 101a of the positive electrode current collector 101 using a slurry positive electrode composite is not particularly limited, and any known method applicable to the formation of a positive electrode 100 comprising a positive electrode current collector 101 and a positive electrode active material layer 102 can be used.

[0061] For example, a positive electrode composite material is applied to a first surface 101a of the positive electrode current collector 101 to a predetermined thickness. Next, the coating film formed by the application is dried and solidified to form the positive electrode active material layer 102. As a method for applying the positive electrode composite material, a conventionally known method such as a roll coating method, a dip coating method, a doctor blade method, a spray coating method, or a curtain coating method can be used.

[0062] <Effects> Next, the effects of this embodiment will be described. (1) The positive electrode material for lithium-ion secondary batteries has the general formula LiMn x Fe yIt includes a granule 10 composed of manganese iron lithium olivine phosphate represented by PO4 (where x and y are numerical values satisfying x + y = 1, 0 < x < 1, and 0 < y < 1), and a carbon coating 12 formed on the surface of the core 11. The core 11 has a structure in which primary particles 11a of manganese iron lithium olivine phosphate are aggregated. The particle diameter of the primary particles 11a is 100 nm or less. The pore volume in the range of pore diameters of 2 nm or more and 300 nm or less in the granule 10 is 0.2 cm 3 / g or less, and the carbon content is 1.8% by mass or more and 3.0% by mass or less.

[0063] The positive electrode material having the above configuration is used as the positive electrode active material contained in the positive electrode active material layer 102 of the positive electrode 100. The positive electrode active material layer 102 of the positive electrode 100 is manufactured by coating a slurry-like positive electrode composite material containing the positive electrode active material on the first surface 101a of the positive electrode current collector 101 and drying the coating film formed by the coating. By using the positive electrode material having the above configuration as the positive electrode active material contained in the positive electrode composite material, even when the coating film is formed thickly to increase the basis weight of the positive electrode active material layer 102, cracks generated in the positive electrode active material layer 102 due to shrinkage of the coating film during drying can be suppressed. That is, by using the positive electrode material having the above configuration, the film-forming property of the positive electrode active material layer 102 can be improved when manufacturing a positive electrode active material layer 102 having a large basis weight, for example, a basis weight of 30 mg / cm 2 or more. In addition, the effect of improving the battery performance based on increasing the basis weight of the positive electrode active material layer 102, for example, the effect of increasing the capacity of the lithium-ion secondary battery can be obtained. Therefore, according to the positive electrode material having the above configuration, it is possible to achieve both improvement in film-forming property and improvement in battery characteristics when the basis weight of the positive electrode active material layer containing manganese iron lithium olivine phosphate is increased.

[0064] (2) The manufacturing method of the positive electrode material for a lithium-ion secondary battery is represented by the general formula LiMn x Fe yParticles of olivine-type lithium manganese iron phosphate represented by PO4 (where x and y are numerical values satisfying x + y = 1, 0 < x < 1, and 0 < y < 1) are pulverized in the presence of an aqueous solvent, a carbon source, and a carboxylic acid to produce a slurry (corresponding to the second slurry) containing pulverized particles of olivine-type lithium manganese iron phosphate (corresponding to the pulverization step), a step of obtaining aggregates of the pulverized product by spray-drying the slurry (corresponding to the drying step), and a step of carbonizing the carbon source contained in the aggregates by firing the aggregates (corresponding to the firing step).

[0065] According to the above configuration, since the above particles are pulverized in an aqueous solvent and in the presence of a carboxylic acid, the eluted metal eluted during pulverization is captured by the carboxylic acid. When the eluted metal is captured by the carboxylic acid, contact of the eluted metal with the surface of the pulverized product of the olivine-type lithium manganese iron phosphate particles, particularly with the newly formed surface formed by pulverization, is suppressed. As a result, the occurrence of necking with the eluted metal as the neck portion between the particles of the pulverized product is suppressed. And as a result of suppressing the occurrence of necking, a decrease in the battery performance of the lithium-ion secondary battery due to necking can be suppressed. Also, compared with the case where a carboxylic acid is added after pulverizing the particles of olivine-type lithium manganese iron phosphate, the pore volume in the pore diameter range of 2 nm or more and 300 nm or less in the granulated body 10 can be reduced.

[0066] (3) The carboxylic acid is citric acid. Citric acid has a high ability to capture Li, Mn, and Fe, which are eluted metals during pulverization. Therefore, the effect of (2) above can be obtained more significantly.

[0067] (4) The content of the carboxylic acid in the slurry is 10 parts by mass or less with respect to 100 parts by mass of the olivine-type lithium manganese iron phosphate. In this case, a granulated body 10 with a small pore volume in the pore diameter range of 2 nm or more and 300 nm or less in the granulated body 10 can be manufactured.

[0068] <Modified Example> This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.

[0069] In the method for producing a positive electrode material, the timing of adding the carboxylic acid may be changed. For example, in the mixing step, a first slurry containing olivine-type lithium manganese iron phosphate particles, an aqueous solvent, and a carbon source is prepared. Then, in the pulverizing step, a process is performed to pulverize the olivine-type lithium manganese iron phosphate particles contained in the first slurry while adding a carboxylic acid or a solution of a carboxylic acid. In this case, too, the particles are pulverized in an aqueous solvent in the presence of a carboxylic acid, so that the effect of suppressing the occurrence of necking due to the carboxylic acid capturing the eluted metal can be obtained. EXAMPLES

[0070] Hereinafter, a more specific embodiment of the above embodiment will be described. <Preparation of olivine-type lithium manganese iron phosphate> A first precursor slurry was obtained by mixing pure water (12000 ml), LiOH (245 g) as a Li source, MnCO3 (840 g) as a Mn source, Fe2C2O4 (401 g) as an Fe source, and H3PO4 (1125 g) as a PO4 source. After adding beads (medium particles) with a diameter of 0.3 mm to the obtained first precursor slurry, the Li source, Mn source, and Fe source contained in the first precursor slurry were pulverized using a bead mill. As a result, a second precursor slurry containing pulverized products of the Li source, Mn source, and Fe source was obtained. The pulverization process using the bead mill was performed so that the average particle diameter (D50) of the Li source, Mn source, and Fe source was within the range of 50 nm to 1000 nm. Next, the second precursor slurry was dried and granulated using a spray dryer (drying outlet temperature: 200° C.) to obtain a dried precursor product. The dried precursor was heated at 500°C for 6 hours in a N2 atmosphere to obtain LiMn 0.75 Fe 0.25 The olivine-type lithium manganese iron phosphate represented by PO4 was obtained.

[0071] <Preparation of granules> [Example 1] The olivine-type lithium manganese iron phosphate (45 g), fructose as a carbon source, and citric acid (2 g) as a carboxylic acid were mixed in pure water (405 ml) to obtain a first slurry. The amount of fructose was set so that the total carbon amount, which is the sum of the carbon in fructose and the carbon in citric acid, was 2.5 parts by mass per 100 parts by mass of the olivine-type lithium manganese iron phosphate.

[0072] After adding beads (medium particles) having a diameter of 0.1 mm to the obtained first slurry, the olivine-type lithium manganese iron phosphate contained in the first slurry was pulverized using a bead mill. As a result, a second slurry containing pulverized olivine-type lithium manganese iron phosphate was obtained. The pulverization process using the bead mill was carried out so that the average particle diameter (D50) of the olivine-type lithium manganese iron phosphate was within a range of 60 nm to 100 nm.

[0073] Next, the second slurry was dried and granulated using a spray dryer (drying outlet temperature: 200°C) to obtain an aggregate of the above-mentioned ground material. The obtained aggregate was heated at 650°C for 6 hours in a N2 atmosphere to carbonize the fructose and citric acid contained in the aggregate. As a result, a granule of Example 1 was obtained, which had a core composed of olivine-type lithium manganese iron phosphate and a carbon coating formed on the surface of the core.

[0074] [Examples 2 to 10 and Comparative Examples 1 to 4] Examples 2 to 10 and Comparative Examples 1 to 4 are examples in which the blending amount of citric acid was changed. Granules of Examples 2 to 10 and Comparative Examples 1 to 4 were obtained by the same method as Example 1, except that the blending amounts of citric acid and fructose in the first slurry were changed. The blending amount of citric acid in each example is as shown in Table 2 below. The blending amount of fructose in each example was adjusted to an amount such that the total carbon amount was 2.5 parts by mass per 100 parts by mass of the olivine-type lithium manganese iron phosphate, in accordance with the blending amount of citric acid.

[0075] [Comparative Examples 5 to 7] Comparative Examples 5 to 7 are examples in which a coarse pulverization treatment was mainly carried out using a bead mill. A granule of Comparative Example 5 was obtained in the same manner as in Example 1, except that the amount of citric acid was set to 0, and the pulverization process using a bead mill was performed so that the average particle size (D50) of the olivine-type lithium manganese iron phosphate was within the range of 60 nm or more and 150 nm or less.

[0076] A granule of Comparative Example 6 was obtained in the same manner as in Example 5, except that the pulverization treatment using a bead mill was carried out so that the average particle size (D50) of the olivine-type lithium manganese iron phosphate was within the range of 100 nm or more and 120 nm or less.

[0077] A granule of Comparative Example 7 was obtained in the same manner as in Example 5, except that the pulverization treatment using a bead mill was performed so that the average particle size (D50) of the olivine-type lithium manganese iron phosphate was within the range of 140 nm or more and 160 nm or less.

[0078] [Comparative Examples 8 to 9] Comparative Examples 8 and 9 are examples in which the amount of fructose, which is a carbon source, was increased. Granules of Comparative Example 8 were obtained in the same manner as in Example 5, except that the total carbon amount was adjusted to 3.2 parts by mass per 100 parts by mass of olivine-type lithium manganese iron phosphate.

[0079] Granules of Comparative Example 9 were obtained in the same manner as in Example 5, except that the total carbon amount was adjusted to 5.1 parts by mass per 100 parts by mass of olivine-type lithium manganese iron phosphate.

[0080] [Comparative Example 10] Comparative Example 10 is an example in which the timing of mixing citric acid was changed. The granules of Comparative Example 10 were obtained in the same manner as in Example 1, except that citric acid (2 g) was not mixed into the first slurry, but was mixed into the second slurry after the pulverization treatment using a bead mill.

[0081] <Analysis of granules> For the granules of each Example and Comparative Example, the primary particle size, the pore volume in the pore size range of 2 nm to 300 nm, and the carbon content were measured. The results are shown in Table 2.

[0082] The particle size of the primary particles was determined as follows. Using the SAXS method, the particle size distribution of the primary particles was determined assuming that the primary particles were spherical. The average particle size (D50) was calculated from the determined particle size distribution, and this value was taken as the particle size of the primary particles.

[0083] The pore volume was determined as follows. The pores of the positive electrode active material were measured using a specific surface area / pore distribution measurement device. The cumulative pore distribution of the granules was determined in the pore diameter range of 2 nm to 300 nm by analysis using the BJH method. The pore diameter was plotted on the horizontal axis and the cumulative pore volume on the vertical axis, and the pore volume in the pore diameter range of 2 nm to 300 nm was calculated from the difference between the cumulative pore volumes for pore diameters of 2 nm and 300 nm.

[0084] The carbon content was measured using a carbon-sulfur analyzer. <Preparation of positive electrode> The positive electrode mixture was applied to one surface of an aluminum foil having a thickness of 15 μm. The applied positive electrode mixture was dried to prepare a positive electrode in which a positive electrode active material layer was formed on one surface of a positive electrode current collector. As the positive electrode mixture, a slurry containing the granules (positive electrode active material) of each Example and Comparative Example, carbon nanotubes (conductive assistant), carboxymethyl cellulose (binder), and styrene-butadiene rubber (binder) in a solid content mass ratio of 98.25:0.05:0.4:1.3 and using water as a solvent was used. The basis weight of the positive electrode active material layer in each of the prepared positive electrodes was measured. As a result, the measured values ​​were all about 65 to 75 mg / cm. 2 It was.

[0085] <Evaluation of film-forming properties> The surface state of the positive electrode active material layer in each of the prepared positive electrodes was visually evaluated. The results are shown in Table 2. The evaluation criteria are as follows. For reference, FIG. 4(a) shows a photograph of the positive electrode active material layer using Example 1, in which the film-formability was evaluated as "○", and FIG. 4(b) shows a photograph of the positive electrode active material layer using Comparative Example 1, in which the film-formability was evaluated as "×".

[0086] "◯": No cracks were found on the surface of the positive electrode active material layer. "X": Cracks were present on the surface of the positive electrode active material layer. <Electrochemical Testing> Among the prepared positive electrodes, a positive electrode half cell was prepared using the positive electrode that was evaluated as "○" in the film forming property evaluation. A separator was sandwiched between the prepared positive electrode (evaluation electrode) cut into 25 mm square and a negative electrode made of a 200 μm thick metal lithium foil cut into 27 mm square to prepare an electrode body battery. The electrode body battery was housed in a laminate as an exterior material, and a non-aqueous electrolyte was injected and the exterior material was sealed to obtain a half cell for electrochemical testing. A glass filter manufactured by Hoechst Celanese was used as the separator. As the non-aqueous electrolyte, a non-aqueous electrolyte was used in which lithium hexafluorophosphate was dissolved to a concentration of 1M in a mixed solvent of ethylene carbonate and diethyl carbonate mixed at a volume ratio of 1:1.

[0087] The prepared positive electrode half cell was charged at 25° C. and a constant current of 0.05 C to 4.3 V, and discharged to 3.0 V. The discharge capacity at this time was measured. The results are shown in Table 2.

[0088] [Table 2] As shown in Table 2, the granules of Examples 1 to 10 satisfy all of the following three conditions.

[0089] Condition 1: The particle size of the primary particles is 100 nm or less. Condition 2: Pore volume is 0.2 cm 3 / g or less. Condition 3: The carbon content is 3.0 mass % or less.

[0090] No cracks were found on the surface of the positive electrode active material layer formed using the granules of Examples 1 to 10 as the positive electrode active material. The discharge capacity when the granules of Examples 1 to 10 were used as the positive electrode active material was 147 to 149.1 mAh / g.

[0091] In contrast, the granules of Comparative Examples 1 to 4 satisfy Conditions 1 and 3, but do not satisfy Condition 2 regarding the pore volume due to their large pore volume. In the positive electrode active material layers formed using the granules of Comparative Examples 1 to 4 as the positive electrode active material, cracks were confirmed on the surface. From these results, in order to ensure good film formability when forming a positive electrode active material layer with a large basis weight, it is necessary to make the pore volume 0.2 cm or less. 3 It can be seen that it is effective to keep the value at / g or less.

[0092] On the other hand, the granules of Comparative Examples 5 to 7 satisfy Conditions 2 and 3, but do not satisfy Condition 1 because the particle diameter of the primary particles is large. No cracks were observed on the surface of the positive electrode active material layer formed using the granules of Comparative Examples 5 to 7 as the positive electrode active material. However, the discharge capacity when the granules of Comparative Examples 5 to 7 were used as the positive electrode active material was 132 to 141 mAh / g, which was significantly lower than the discharge capacity when the granules of Examples 1 to 10 were used as the positive electrode active material.

[0093] The granules of Comparative Examples 8 to 9 satisfy Condition 1 and Condition 2, but do not satisfy Condition 3 due to their high carbon content. No cracks were observed on the surface of the positive electrode active material layer formed using the granules of Comparative Examples 8 to 9 as the positive electrode active material. However, the discharge capacity when the granules of Comparative Examples 8 to 9 were used as the positive electrode active material was 133.5 to 139.9 mAh / g, which was significantly lower than the discharge capacity when the granules of Examples 1 to 10 were used as the positive electrode active material.

[0094] The above results when the granules of Comparative Examples 5 to 9 were used show that the effect of increasing the capacity of a lithium ion secondary battery cannot be obtained only by forming a positive electrode active material layer having a large basis weight. 3 / g or less, it is also necessary to keep the primary particle size at 100 nm or less and the carbon content at 3.0 mass % or less.

[0095] Next, the relationship between the amount of citric acid and the pore volume of the resulting granules will be considered. Referring to the results of Examples 1 to 10 and Comparative Examples 1 to 3, in the range of 10 parts by mass or less per 100 parts by mass of olivine-type lithium manganese iron phosphate, the pore volume of the resulting granules decreases as the amount of citric acid increases. On the other hand, the pore volume of the granules of Comparative Example 4, in which the amount of citric acid is 15 parts by mass, increases to more than twice the pore volume of the granules of Examples 8 to 10, in which the amount of citric acid is 10 parts by mass. From this result, it can be seen that the pore volume of the granules can be reduced by increasing the amount of carboxylic acid such as citric acid, but when the amount of carboxylic acid is increased to a specific amount or more, the pore volume of the granules increases.

[0096] Next, the timing of mixing citric acid will be considered. Comparative Example 10 is an example in which citric acid is not mixed into the first slurry, but is mixed into the second slurry after the pulverization treatment. The pore volume of the granules of Comparative Example 10 is 1.5 times larger than the pore volume of the granules of Example 1, which differs only in the timing of mixing citric acid. From this result, it can be seen that in order to reduce the pore volume, it is necessary to perform the pulverization treatment in the presence of a carboxylic acid such as citric acid. [Explanation of symbols]

[0097] 10...Granules 11. Core 11a...Primary particle 11b…pore 12...Carbon coating 100...Positive electrode 101...Positive electrode current collector 101a...first surface 102...Cathode active material layer

Claims

1. General formula LiMn x Fe y P.O. 4 (x and y are numbers satisfying x+y=1, 0<x<1, 0<y<1), and a granule having a core made of an olivine-type lithium manganese iron phosphate represented by the formula (x and y) and a carbon coating formed on a surface of the core, the core has a structure in which primary particles of the olivine-type lithium manganese iron phosphate are aggregated, The particle diameter of the primary particles is 100 nm or less, The pore volume in the pore diameter range of 2 nm to 300 nm in the granules is 0.2 cm 3 / g or less, The granules have a carbon content of 1.8% by mass or more and 3.0% by mass or less.

2. a positive electrode current collector having a first surface; a positive electrode active material layer formed on the first surface of the positive electrode current collector, The positive electrode active material layer comprises the positive electrode material for lithium ion secondary batteries according to claim 1 .

3. The weight of the positive electrode active material layer is 30 mg / cm 2 100mg / cm or more 2 3. The positive electrode for a lithium ion secondary battery according to claim 2, wherein:

4. General formula LiMn x Fe y P.O. 4 (x and y are numerical values ​​satisfying x+y=1, 0<x<1, 0<y<1), in the presence of an aqueous solvent, a carbon source, and a carboxylic acid, to prepare a slurry containing the pulverized product of the olivine-type lithium manganese iron phosphate; obtaining an agglomerate of the pulverized material by spray drying the slurry; and calcining the aggregates to carbonize the carbon source contained in the aggregates.

5. The method for producing a positive electrode material for a lithium ion secondary battery according to claim 4, wherein the carboxylic acid is citric acid.

6. 6. The method for producing a positive electrode material for a lithium ion secondary battery according to claim 4 or 5, wherein the content of the carboxylic acid in the slurry is 2 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the olivine-type lithium manganese iron phosphate.

Citation Information

Patent Citations

  • Modified ultralow-temperature lithium iron phosphate composite material, positive electrode material and preparation method thereof

    CN113097456A

  • Olivine structure positive electrode material, preparation method and application thereof, and lithium ion battery

    CN113363483A

  • Method for preparing lithium iron manganese phosphate positive electrode material from phosphated residues

    CN115010107A

  • Lithium ferric manganese phosphate precursor, lithium ferric manganese phosphate, preparation methods of lithium ferric manganese phosphate precursor and lithium ferric manganese phosphate, electrode and battery

    CN115611254A

  • Olivine-type lithium transition metal oxide and manufacturing method therefor

    JP2015143189A