Epoxy resin composition particle, tablet, and method for producing columnar tablet

By incorporating fibrous or acicular fillers and optimizing kneading temperature, the fracture toughness of epoxy resin compositions is improved, addressing gap issues in skewed structures and facilitating stable production of epoxy resin particles and tablets for magnet fixing.

JP2024156626APending Publication Date: 2024-11-06SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024069184
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-22
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Epoxy resin compositions used in fiber-reinforced composite materials exhibit gaps on discontinuous surfaces of molded bodies with skewed structures due to the breaking of magnet fixing materials at corners, leading to instability.

Method used

Incorporating fibrous or acicular fillers and adjusting kneading temperature to enhance the fracture toughness of epoxy resin composition particles, achieving a minimum value of 3.0 MPa m 1/2, which stabilizes the filling process in skewed structures.

Benefits of technology

The enhanced fracture toughness suppresses gap formation in skewed structures, enabling stable production of epoxy resin composition particles and tablets, suitable for magnet fixing applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156626000006
    Figure 2024156626000006
  • Figure 2024156626000007
    Figure 2024156626000007
  • Figure 2024156626000008
    Figure 2024156626000008
Patent Text Reader

Abstract

To provide an epoxy resin composition particle with excellent gap reduction during skewed structure filling.SOLUTION: An epoxy resin composition particle is used for fixing a magnet, and contains an epoxy resin and a fibrous or needle-like filler. The fracture toughness value (K1c) measured by a specified procedure is 3.0 MPa m1 / 2 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing epoxy resin composition particles, tablets, and columnar tablets. [Background technology]

[0002] Various developments have been made so far regarding structural materials made of fiber-reinforced composite materials using epoxy resins. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a material with a fracture toughness of 1.2 to 2.0 MPa m 1 / 2 The epoxy resin is described in Patent Document 1, Examples 1 to 3, etc. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 053937 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of the inventor's investigations, it was confirmed that in the epoxy resin described in Patent Document 1 above, in a molded article having a skew structure, gaps occur at the discontinuous surfaces of the molded article (the misaligned parts of the molded article). [Means for solving the problem]

[0005] When filling a rotor core with a skewed structure, it is thought that the magnet fixing material will break down and create gaps starting from the corners of the magnets, which are areas that hinder its flow. After further investigation, the inventors found that the degree of gaps when filled in a skewed structure can be stably evaluated by using the fracture toughness value of the magnet fixing material as an index. Based on this knowledge, further intensive research led to the discovery that the fracture toughness value of the epoxy resin composition particles can be increased to a predetermined level by using a fibrous or needle-like filler and adopting a moderately high kneading temperature, thereby suppressing the occurrence of gaps when filled in a skewed structure, and thus the present invention was completed.

[0006] According to one aspect of the present invention, there is provided the following method for producing epoxy resin composition particles, tablets, and columnar tablets. [1] Epoxy resin composition particles used for fixing a magnet, Epoxy resin, A fibrous or needle-like filler; Including, The fracture toughness value (K1c) measured by the procedure i below is 3.0 MPa m 1 / 2 The epoxy resin composition particles are as described above. (Step i) Using a transfer molding machine, a molded body is formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175° C., an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the KIc method specified in ASTM D5045-14, the obtained molded body is cut to a length of 50 mm, a width of B5 mm, and a thickness of W10 mm, a notch 3.5 mm deep in the thickness direction is formed in the center of the length direction, and the cured product is obtained by curing at 175°C for 4 hours. Furthermore, a scratch 0.1 mm deep in the thickness direction is made with a razor at the tip of the notch of the cured product to prepare a test piece with a total crack length a = 3.6 mm. After that, a three-point bending test was performed on the obtained test pieces using a tension and compression testing machine at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance of S = 40 mm, and the fracture toughness value (K1c (MPa m 1 / 2 In the following formula, P Q is the maximum load (N). K.I. C =((PQ ×S) / (B×W 3 / 2 ))×f(a / W) where f(a / W) = (3(a / W) 1 / 2 [1.99-(a / W)(1-a / W){2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3 / 2 ) [2] The epoxy resin composition particles according to [1], Epoxy resin composition particles, wherein the number average fiber length of the fibrous or needle-like filler, as measured by the following procedure A, is 5 μm or more and 500 μm or less. (Step A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and the insoluble matter is dispersed on a glass plate, and the filler particles in the insoluble matter are photographed using an optical microscope, and the fiber length is measured using an image analyzer. The average fiber length of the 100 longest fiber particles is defined as the number average fiber length. [3] The epoxy resin composition particles according to [1] or [2], When the number average fiber length of the fibrous or acicular filler measured by the following procedure A is L and the number average fiber diameter of the fibrous or acicular filler measured by the following procedure B is D, Epoxy resin composition particles, having an L / D ratio of 3 or more and 100 or less. (Step A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and the insoluble matter is dispersed on a glass plate, and the fillers in the insoluble matter are photographed using an optical microscope and the fiber length is measured using an image analyzer. The fiber lengths are measured in descending order of length, and the average value of 100 fillers is taken as the number-average fiber length. (Step B) Using a scanning electron microscope, 100 cross sections of the fibrous filler are measured from the cross section of the epoxy resin composition particle, and the average of the smallest diameters of each fiber cross section is calculated as the number average fiber diameter. [4] An epoxy resin composition particle according to any one of [1] to [3], Epoxy resin composition particles, wherein the fibrous or acicular filler comprises one or more selected from the group consisting of wollastonite fibers, glass fibers, metal fibers, carbon fibers, fibrous aluminum oxide, aramid fibers, silicon carbide whiskers, silicon nitride whiskers, and potassium titanate whiskers. [5] An epoxy resin composition particle according to any one of [1] to [4], Epoxy resin composition particles having a spiral flow, measured according to procedure ii below, of 30 cm or greater. (Step ii) Using a low-pressure transfer molding machine, the epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured. [6] An epoxy resin composition particle according to any one of [1] to [5], Epoxy resin composition particles, wherein the content of the fibrous or needle-like filler is 5% by mass or more and 80% by mass or less, based on 100% by mass of the epoxy resin composition particles. [7] An epoxy resin composition particle according to any one of [1] to [6], Epoxy resin composition particles, wherein the epoxy resin comprises a cresol novolac type epoxy resin and / or a bisphenol A type epoxy resin. [8] An epoxy resin composition particle according to any one of [1] to [7], Epoxy resin composition particles comprising one or more curing catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts. [9] An epoxy resin composition particle according to any one of [1] to [8], Epoxy resin composition particles used for molding into tablets through a process of supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material, and a process of cutting the epoxy resin molding material while continuously extruding the molten epoxy resin molding material from an opening at the tip of the extruder to obtain tablets.

[10] An epoxy resin composition particle according to any one of [1] to [9], Epoxy resin composition particles comprising an epoxy resin having a softening point of less than 110°C or a curing agent.

[11] A tablet formed using the epoxy resin composition particles according to any one of [1] to

[10] , 5cm 3 More than 1500cm 3 Tablets having the following volumes:

[12] A step of preparing an epoxy resin composition particle according to any one of [1] to

[11] ; A step of supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material; and a step of cutting the molten epoxy resin molding material into columnar tablets while continuously extruding the molten epoxy resin molding material from an opening at the tip of an extruder, The cross-sectional area of ​​the cylindrical tablet is 3 cm 2 More than 100cm 2 Below is the Method for manufacturing columnar tablets.

[13] A structure using the epoxy resin composition particles described in any one of [1] to

[10] .

[14] A method for producing the structure according to

[13] , comprising the steps of: An injection molding apparatus including an injection unit including a cylinder and a screw inserted into the cylinder, and a mold having a cavity and connected to the injection unit, melting the epoxy resin composition particles in the cylinder to obtain a molten resin composition; a step of injecting a molten resin composition from a tip of the screw to fill the cavity; A method for manufacturing a structure comprising:

[15] A method for producing the structure according to

[13] or

[14] , comprising the steps of: The method for producing a structure, wherein in the filling step, a temperature T of the tip of the screw is 60 to 100°C.

[16] A method for producing a structure according to any one of

[13] to

[15] , comprising the steps of: A method for producing a structure, wherein the temperature inside the cavity is 150 to 180°C in the filling step. Effect of the Invention

[0007] According to the present invention, there are provided epoxy resin composition particles which are excellent in suppressing gaps when filled in a skewed structure, a tablet using the same, and a method for producing a columnar tablet. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a vertical cross-sectional view of an extruder according to an example of the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of an injection molding apparatus according to the present embodiment. [Diagram 3] FIG. 2 is a cross-sectional view for explaining an outline of a tensile / compression testing machine. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.

[0010] The epoxy resin composition particles of this embodiment will be outlined below. The epoxy resin composition particles of the present embodiment contain an epoxy resin and a fibrous or needle-like filler, and have a fracture toughness value (K1c) of 3.0 MPa m as measured by the following procedure i. 1 / 2 It satisfies the above.

[0011] By setting the fracture toughness value (K1c) of the epoxy resin composition particles to be equal to or higher than the above lower limit, it is possible to suppress the occurrence of gaps when a magnet fixing material is filled in a rotor core having a skew structure. The upper limit of the fracture toughness value (K1c) is not particularly limited, but is, for example, 10.0 MPa m 1 / 2 The following may also be used.

[0012] (Measuring procedure for fracture toughness value i) Using a transfer molding machine, a molded body is formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175° C., an injection pressure of 9.8 MPa, and a curing time of 120 seconds. According to the KIc method specified in ASTM D5045-14, the obtained molded body is cut to a length of 50 mm, a width of B5 mm, and a thickness of W10 mm, a notch 3.5 mm deep in the thickness direction is formed in the center of the length direction, and the cured product is obtained by curing at 175°C for 4 hours. Furthermore, a scratch 0.1 mm deep in the thickness direction is made with a razor at the tip of the notch of the cured product to prepare a test piece with a total crack length a = 3.6 mm. After that, a three-point bending test was performed on the obtained test pieces using a tension and compression testing machine at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance of S = 40 mm, and the fracture toughness value (K1c (MPa m 1 / 2 In the following formula, P Q is the maximum load (N). K.I. C =((P Q ×S) / (B×W 3 / 2 ))×f(a / W) where f(a / W) = (3(a / W) 1 / 2 [1.99-(a / W)(1-a / W){2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3 / 2 )}

[0013] In this embodiment, it is possible to control the fracture toughness value by appropriately selecting, for example, the type and amount of each component contained in the epoxy resin composition particles, the preparation method of the epoxy resin composition particles, etc. Among these, for example, improving the kneadability of the material, increasing the fiber length of the fiber filler, etc. can be cited as elements for setting the fracture toughness value in a desired numerical range.

[0014] Such epoxy resin composition particles are used for fixing a magnet. Specifically, a tablet-shaped molding material is produced from the epoxy resin composition particles, and the obtained tablet-shaped molding material can be used for fixing a magnet by a known molding method.

[0015] The epoxy resin composition particles of the present embodiment can be suitably used for producing a tablet-shaped, preferably columnar tablet-shaped, epoxy resin molding material. The epoxy resin composition particles enable stable production of tablet-shaped epoxy resin molding materials.

[0016] A method for producing a tablet-shaped epoxy resin molding material may include, for example, an extrusion molding method including a step of supplying epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material, and a step of cutting the epoxy resin molding material while continuously extruding the molten epoxy resin molding material from an opening at the tip of the extruder to obtain tablets.

[0017] As a specific example of a method for producing the tablet-shaped epoxy resin molding material, an extruder shown in Fig. 1 can be used. Fig. 1 shows a vertical cross-sectional view of an example of the configuration of an extruder. The extruder has a hopper 2 for feeding epoxy resin composition particles 1, a heater 41 for heating the epoxy resin composition particles 1 through a cylinder 43, a screw 42, and a die 5 attached to the tip of the extruder, having an opening with the same shape as a predetermined tablet cross section, and whose temperature is controlled. A temperature regulator 51 for controlling the temperature of the die 5 may be connected to the extruder. The extruder extrudes the epoxy resin composition particles 1 into the cylinder 43 and the input cylinder 43a, and kneads the epoxy resin molding material obtained by melting the epoxy resin composition particles 1 by heating with the screw 42 while extruding. The extruder then continuously extrudes the melt-kneaded epoxy resin molding material from the opening of the die 5. The extruded epoxy resin molding material becomes the extrusion material 6. The extrusion material 6 is cut into a predetermined tablet length with a cutter (not shown) or the like to obtain tablet-shaped epoxy resin molding material (tablets).

[0018] The epoxy resin composition particles 1 include powder and / or granules. For example, relatively coarse particles (granules) are crushed and / or classified to obtain relatively fine particles (powder). The particle shape of the epoxy resin composition particles 1 is not particularly limited and may be spherical, polygonal, irregular, etc. These may be used alone or in combination of two or more kinds.

[0019] In this embodiment, the opening shape of the die 5 attached to the tip of the extruder is the same as the cross-sectional shape of the tablet-shaped epoxy resin molding material (tablet). When the opening shape is circular, the size of the opening shape is, for example, a diameter of 20 mm or more and 200 mm or less, and preferably 40 mm or more and 120 mm or less. The opening shape, including its size, is appropriately selected according to the target tablet shape. The extrusion material 6 extruded from the extruder is cut to a desired length by a cutter. This length is, for example, from 10 mm to 300 mm, and preferably from 20 mm to 200 mm.

[0020] The volume of a tablet (a tablet-shaped epoxy resin molding material) is, for example, 5 cm 3 More than 1500cm 3 Less than 10cm, preferably 3 More than 1000cm 3 The following is the result. The cross-sectional area of ​​a columnar tablet is, for example, 3 cm 2 More than 100cm2 Less than 10cm, preferably 2 Over 95cm 2 The following is the result.

[0021] By using the epoxy resin composition particles of this embodiment, tablet-shaped epoxy resin molding material can be continuously obtained, so that tablet-shaped epoxy resin molding material having a large tablet height can be efficiently produced.

[0022] By using a tablet-shaped epoxy resin molding material and a known molding method such as transfer molding or injection molding, it is possible to manufacture any one of a fixing structure or a sealing structure selected from the group consisting of a magnet fixing structure, an electronic control unit sealing structure, a coil sealing structure, and a stator core sealing structure, as exemplified below. In particular, the epoxy resin composition particles of the present embodiment are preferably used for injection molding. Specifically, it is preferable that the epoxy resin composition particles are used for injection molding by feeding the epoxy resin composition particles into an injection molding device equipped with an injection unit consisting of a cylinder and a screw inserted into the cylinder, and a mold connected to the injection unit and having a cavity. For example, when manufacturing a magnet fixed structure using the epoxy resin composition particles of this embodiment, the epoxy resin composition particles may be introduced into an injection molding machine and melted in a cylinder, and the molten resin may be directly filled between the hole in the mold and the permanent magnet.

[0023] Hereinafter, a method for producing a structure using the epoxy resin composition particles of this embodiment by injection molding will be described with reference to FIG.

[0024] FIG. 2 shows the injection molding apparatus 1 equipped with an injection unit 20 consisting of a cylinder 21 and a screw 22 inserted into the cylinder 21 , and a mold 10 having a cavity 12 . The injection molding apparatus 1 includes a mold 10 having a molding space (cavity 12) including a gate, a runner, and another gate, and an injection molding machine 20 for performing injection molding. The injection molding machine 20 includes, for example, a cylinder 21, a screw 22 rotatable within the cylinder 21, a hopper 23 capable of feeding epoxy resin composition particles into the cylinder 21, a heater 24 for melting and heating the epoxy resin composition particles via the cylinder 21, and a nozzle 25 for sending the epoxy resin composition particles melted and kneaded in the cylinder 21 to the mold 10. 2 shows the screw 22 having the backflow valve 26 at the tip, the screw 22 is not limited to this. The screw 22 may not have the backflow valve 26.

[0025] The method for producing the structure includes a step of melting epoxy resin composition particles in a cylinder 21 to form a molten resin composition, and a step of injecting the molten resin composition from the tip of a screw 22 to fill the cavity 12. That is, first, epoxy resin composition particles are charged into a heated injection molding machine 20. As a result, the epoxy resin composition particles are kneaded by the screw 22 while being heated and melted by the heater 24 in the cylinder 21. The temperature of the tip of the screw 22 in the cylinder 21 is preferably 60 to 100°C from the viewpoint of, for example, adequately heating and melting the epoxy resin composition particles. Next, the molten resin composition melted by the screw 22 is sent while being compressed and kneaded in the direction of the nozzle 25, and the screw 22 moves backward (the opposite direction to the nozzle 25). At this time, back pressure is applied to the screw 22 from the rear, so that pressure can be applied to the molten resin composition that has gathered at the nozzle 25. Then, the molten resin composition that has gathered at the nozzle 25 at the tip of the screw 22 is metered to a set position. Then, the measured molten resin composition is injected into the cavity 12 of the mold 10 through the nozzle 25 by the pressure of the screw 22, by advancing the screw 22 lowered backward. The temperature inside the cavity 12 when the molten resin composition is filled is preferably 150 to 180°C from the viewpoint of appropriately filling the molten resin composition, etc. The molten resin composition is then cured in the cavity 12, and the mold 10 is then opened to remove the structure from the cavity 12.

[0026] For example, when manufacturing a magnet fixing structure using the epoxy resin composition particles of this embodiment, the epoxy resin composition particles may be introduced into an injection molding machine and melted in cylinder 21, and the molten resin may be directly filled between the hole in mold 10 and the permanent magnet.

[0027] With regard to the above-mentioned fixing structure or sealing structure, for example, WO 2012 / 029278 etc. can be referred to as a rotor core to which a magnet is fixed.

[0028] A case where an epoxy resin molding material is used for the magnet fixing structure will be described. The rotor core includes a plurality of holes and a permanent magnet inserted into each of the plurality of holes. The permanent magnet can be fixed to the rotor core by filling the gaps between the holes and the permanent magnets with an epoxy resin molding material.

[0029] The process for producing the fixed structure may be carried out, for example, using a tablet-shaped epoxy resin molding material at a temperature of 120°C or higher and 200°C or lower and a pressure of 3 MPa or higher and 15 MPa or lower, preferably at a temperature of 140°C to 180°C and a pressure of 5 to 12 MPa.

[0030] The lower limit of the spiral flow of the epoxy resin composition particles is, for example, 30 cm or more, and preferably 50 cm or more. On the other hand, the upper limit of the spiral flow of the epoxy resin composition particles is, for example, 250 cm or less, and preferably 200 cm or less. Spiral flow can be measured according to procedure ii below. Using a low-pressure transfer molding machine, epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured.

[0031] The method for producing tablets using the epoxy resin composition particles of the present embodiment is not limited to the above-mentioned extrusion molding method, and compression molding method, transfer molding method, injection molding method, etc. may also be used.

[0032] Each component of the epoxy resin composition particles of this embodiment will be described in detail below.

[0033] [Epoxy resin] The epoxy resin composition particles contain an epoxy resin. Examples of epoxy resins include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, and bisphenol A novolac resin, and resol-type phenolic resin; novolac-type epoxy resins such as phenol novolac-type epoxy resin and cresol novolac-type epoxy resin; bisphenol-type epoxy resins such as bisphenol A-type epoxy resin and bisphenol F-type epoxy resin; aromatic glycidylamine-type epoxy resins such as N,N-diglycidylaniline, N,N-diglycidyltoluidine, diaminodiphenylmethane-type glycidylamine, and aminophenol-type glycidylamine; hydroquinone-type epoxy resins; biphenyl-type epoxy resins; and stilbene. Examples of epoxy resins include epoxy resins such as aralkyl type epoxy resins, such as phenol aralkyl type epoxy resins having a phenylene and / or biphenylene skeleton, and naphthol aralkyl type epoxy resins having a phenylene and / or biphenylene skeleton, and aliphatic epoxy resins such as vinylcyclohexene dioxide, dicyclopentadiene oxide, and alicyclic epoxy resins such as alicyclic diepoxy-adipade. These may be used alone or in combination of two or more. Among these, the epoxy resin preferably contains a cresol novolac type epoxy resin and / or a bisphenol A type epoxy resin.

[0034] Moreover, the epoxy resin preferably has a softening point of less than 80°C. The softening point is measured by the ball and ring method.

[0035] The content of the epoxy resin is preferably from 5% by mass to 40% by mass, more preferably from 10% by mass to 20% by mass, based on the total amount of the epoxy resin composition particles.

[0036] [Hardening agent] The epoxy resin composition particles may include a curing agent that cures the epoxy resin. As the curing agent, for example, a phenol resin-based curing agent is preferably used. Examples of the phenol resin-based curing agent include novolac type resins such as phenol novolac resin, cresol novolac resin, and naphthol novolac resin; multifunctional phenol resins such as triphenol methane type phenol resin; modified phenol resins such as terpene modified phenol resin and dicyclopentadiene modified phenol resin; aralkyl type resins such as phenol aralkyl resins having a phenylene skeleton and / or biphenylene skeleton, and naphthol aralkyl resins having a phenylene and / or biphenylene skeleton; and bisphenol compounds such as bisphenol A and bisphenol F. These may be used alone or in combination of two or more. Such a phenol resin-based curing agent provides a good balance of flame resistance, moisture resistance, electrical properties, curability, storage stability, and the like.

[0037] Further, examples of the curing agent that can be used in combination include polyaddition type curing agents and condensation type curing agents.

[0038] Examples of the polyaddition type curing agent include aliphatic polyamines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylenediamine (MXDA), aromatic polyamines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS), as well as polyamine compounds including dicyandiamide (DICY) and organic acid dihydrazides; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polyphenol compounds such as novolac-type phenolic resins and phenol polymers; polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins.

[0039] Examples of the condensation type curing agent include resol resins, urea resins such as methylol group-containing urea resins, and melamine resins such as methylol group-containing melamine resins.

[0040] Moreover, the hardener preferably has a softening point of less than 110°C, more preferably less than 105°C. The softening point is measured by the ball and ring method.

[0041] The phenolic resin as the curing agent and the epoxy resin are preferably mixed so that the equivalent ratio (EP) / (OH) between the number of epoxy groups (EP) in the epoxy resin composition particles and the number of phenolic hydroxyl groups (OH) in the total phenolic resin is 0.8 or more and 1.3 or less. When the equivalent ratio is within the above range, sufficient curing properties can be obtained when molding the obtained epoxy resin composition particles. However, when a resin other than the phenolic resin that can react with the epoxy resin is used in combination, the equivalent ratio can be appropriately adjusted.

[0042] [Inorganic filler] (fibrous or needle-like filler) The epoxy resin composition particles contain a fibrous or needle-like filler as an inorganic filler.

[0043] The lower limit of the number average fiber length of the fibrous or needle-like filler is, for example, 5 μm or more, preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more, which can improve the strength of the material. On the other hand, the upper limit of the number average fiber length of the fibrous or needle-like filler is, for example, 500 μm or less, preferably 450 μm or less, and more preferably 400 μm or less, which can improve the moldability of the material.

[0044] When the number average fiber length of the fibrous or needle-like filler is L and the number average fiber diameter of the fibrous or needle-like filler is D, the aspect ratio is defined as L / D. The lower limit of L / D of the fibrous or needle-like filler is, for example, 3 or more, preferably 10 or more, and more preferably 15 or more. This can further improve the flexural modulus and toughness. On the other hand, the upper limit of L / D of the fibrous or needle-like filler is, for example, not more than 100, preferably not more than 70, and more preferably not more than 50. This can improve the moldability of the material.

[0045] (Procedure A for measuring number average fiber length) After the epoxy resin composition particles are dissolved in acetone to remove the resin component, the insoluble matter is dispersed on a glass plate, the filler in the insoluble matter is photographed using an optical microscope, and the fiber length is measured using an image analyzer. The average value of the fiber lengths of the 100 fillers starting from the longest fiber length is taken as the number-average fiber length.

[0046] (Measurement Procedure B for Number Average Fiber Diameter) Using a scanning electron microscope, 100 cross sections of the fibrous filler are measured from the cross section of an epoxy resin composition particle, and the average of the smallest diameters of each fiber cross section is calculated as the number average fiber diameter.

[0047] The fibrous or acicular filler may include, for example, one or more selected from the group consisting of wollastonite fiber, glass fiber, metal fiber, carbon fiber, fibrous aluminum oxide, aramid fiber, silicon carbide whisker, silicon nitride whisker, and potassium titanate whisker. Among these, it is preferable to include at least one of wollastonite fiber and glass fiber, and it is more preferable to include wollastonite fiber.

[0048] The lower limit of the content of the fibrous or needle-like filler is, for example, 5% by mass or more, preferably 10% by mass or more, and more preferably 30% by mass or more, based on 100% by mass of the epoxy resin composition particles. This can further improve the flexural modulus and toughness. On the other hand, the upper limit of the content of the fibrous or needle-like filler is not particularly limited, but may be 80% by mass or less, preferably 75% by mass or less, based on 100% by mass of the epoxy resin composition particles.

[0049] The lower limit of the content of the fibrous or needle-like filler in all inorganic fillers is, for example, 30% by mass or more, preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 72% by mass or more. This can further improve the flexural modulus and toughness. On the other hand, the upper limit of the content of the fibrous or needle-like filler in all the inorganic fillers is not particularly limited, but may be 100 mass % or less.

[0050] (Inorganic fillers other than fibrous or acicular fillers) The epoxy resin composition particles may contain inorganic fillers other than the fibrous or acicular filler. The other inorganic filler is not particularly limited as long as it has a shape such as a spherical shape, a polygonal shape, an irregular shape, etc. Specifically, the other inorganic filler is preferably one having an aspect ratio of 2 or less, and more preferably one having a spherical shape.

[0051] Examples of other inorganic fillers include silica, alumina, kaolin, talc, clay, mica, rock wool, glass powder, glass flakes, glass beads, silicon carbide, silicon nitride, aluminum nitride, carbon black, graphite, titanium dioxide, calcium carbonate, calcium sulfate, barium carbonate, magnesium carbonate, magnesium sulfate, barium sulfate, etc. These may be used alone or in combination of two or more. As the silica, fused silica such as fused crushed silica and fused spherical silica, crystalline silica, etc. are used.

[0052] Average particle size of inorganic filler D 50 is preferably 0.01 μm or more and 75 μm or less, and more preferably 0.05 μm or more and 50 μm or less. By setting the average particle size of the inorganic filler within the above range, the filling property in the mold is improved. Furthermore, by setting the upper limit of the average particle size of the inorganic filler to 75 μm or less, the filling property is further improved. Average particle size D 50 was determined as the volume-converted average particle diameter using a laser diffraction measuring device RODOS SR type (SYMPATEC HEROS & RODOS).

[0053] The content of the inorganic filler is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 65% ​​by mass or more, and particularly preferably 75% by mass or more, based on the total amount of the epoxy resin composition particles. On the other hand, the content of the inorganic filler is preferably 93% by mass or less, more preferably 91% by mass or less, and further preferably 90% by mass or less, based on the total amount of the epoxy resin composition particles.

[0054] In addition, when an inorganic filler is used in combination with a metal hydroxide such as aluminum hydroxide or magnesium hydroxide, or an inorganic flame retardant such as zinc borate, zinc molybdate, or antimony trioxide, as described below, it is desirable that the total amount of the inorganic flame retardant and the inorganic filler is within the range of the content of the inorganic filler.

[0055] [Curing catalyst] The epoxy resin composition particles may contain a curing catalyst if necessary. As the curing catalyst, it is preferable to use one or more catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts.

[0056] As the imidazole catalyst, it is preferable to use imidazoles, for example. Examples of the imidazoles include imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxyimidazole, 2-phenyl-4,5-dihydroxydimethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. The compound may include one or more selected from imidazole compounds such as midazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2-phenylimidazole, and an isocyanuric acid adduct of 2-methylimidazole.

[0057] When the curing catalyst contains an imidazole-based catalyst, the lower limit of the content of the imidazole-based catalyst is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and particularly preferably 0.05 mass% or more, based on the total amount of the epoxy resin composition particles. The upper limit of the content of the imidazole catalyst is preferably 2.0% by mass or less, more preferably 1.0% by mass or less, and particularly preferably 0.5% by mass or less, based on the total amount of the epoxy resin composition particles.

[0058] Examples of phosphorus-based catalysts include phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds.

[0059] Examples of organic phosphines that can be used in the epoxy resin composition particles include primary phosphines such as ethylphosphine and phenylphosphine; secondary phosphines such as dimethylphosphine and diphenylphosphine; and tertiary phosphines such as trimethylphosphine, triethylphosphine, tributylphosphine, and triphenylphosphine.

[0060] Examples of the tetra-substituted phosphonium compound that can be used in the epoxy resin composition particles include compounds represented by the following general formula (4).

[0061] [ka] (In the above general formula (4), P represents a phosphorus atom. 4 , R 5 , R 6 and R 7represents an aromatic group or an alkyl group. A represents an anion of an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on an aromatic ring. AH represents an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on an aromatic ring. x and y are numbers from 1 to 3, z is a number from 0 to 3, and x=y.

[0062] The compound represented by the general formula (4) can be obtained, for example, but not limited to, as follows. First, a tetra-substituted phosphonium halide, an aromatic organic acid, and a base are mixed uniformly in an organic solvent to generate an aromatic organic acid anion in the solution system. Next, water is added to precipitate the compound represented by the general formula (4). In the compound represented by the general formula (4), R bonded to the phosphorus atom 4 , R 5 , R 6 and R 7 is preferably a phenyl group, AH is a compound having a hydroxyl group on an aromatic ring, i.e., a phenol, and A is an anion of the phenol. Examples of the phenol include monocyclic phenols such as phenol, cresol, resorcin, and catechol, condensed polycyclic phenols such as naphthol, dihydroxynaphthalene, and anthraquinol, bisphenols such as bisphenol A, bisphenol F, and bisphenol S, and polycyclic phenols such as phenylphenol and biphenol.

[0063] Examples of the phosphobetaine compound used as the curing catalyst include compounds represented by the following general formula (5).

[0064] [ka] (In the above general formula (5), R 8 is an alkyl group having 1 to 3 carbon atoms, R 9 represents a hydroxyl group. f is a number from 0 to 5, and g is a number from 0 to 3.)

[0065] The compound represented by the general formula (5) can be obtained, for example, as follows. First, a triaromatic substituted phosphine, which is a tertiary phosphine, is contacted with a diazonium salt to substitute the triaromatic substituted phosphine for the diazonium group of the diazonium salt. However, the method is not limited thereto.

[0066] An example of an adduct of a phosphine compound and a quinone compound used as a curing catalyst is a compound represented by the following general formula (6).

[0067] [ka] (In the above general formula (6), P represents a phosphorus atom. 10 , R 11 and R 12 R represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and may be the same or different. 13 , R 14 and R 15 represents a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, and may be the same or different; R 14 and R 15 may be bonded to form a cyclic structure.)

[0068] The phosphine compound used in the adduct of the phosphine compound and the quinone compound is preferably, for example, triphenylphosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, trinaphthylphosphine, tris(benzyl)phosphine, etc., which is unsubstituted or has a substituent such as an alkyl group or an alkoxy group on the aromatic ring, and examples of the substituent such as the alkyl group or alkoxy group include those having a carbon number of 1 to 6. From the viewpoint of availability, triphenylphosphine is preferred.

[0069] As the quinone compound used in the adduct of the phosphine compound and the quinone compound, benzoquinone and anthraquinones can be mentioned, and among them, p-benzoquinone is preferred from the viewpoint of storage stability.

[0070] The method for producing an adduct of a phosphine compound and a quinone compound is to contact and mix the organic tertiary phosphine and the benzoquinone in a solvent in which both can dissolve, to obtain the adduct. The solvent is preferably a ketone such as acetone or methyl ethyl ketone, which has low solubility in the adduct, but is not limited thereto.

[0071] In the compound represented by the general formula (6), R bonded to the phosphorus atom 10 , R 11 and R 12 is a phenyl group, and R 13 , R 14 and R 15 is a hydrogen atom, that is, a compound obtained by adding 1,4-benzoquinone and triphenylphosphine, is preferred in terms of decreasing the hot elastic modulus of the cured product of the epoxy resin composition particles.

[0072] An example of an adduct of a phosphonium compound and a silane compound used as a curing catalyst is a compound represented by the following general formula (7).

[0073] [ka] (In the above general formula (7), P represents a phosphorus atom, and Si represents a silicon atom. 16 , R 17 , R 18 and R 19 Each of R represents an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group, and may be the same or different. 20 is the group Y 2 and Y 3 is an organic group that bonds to 21 is the group Y 4 and Y 5It is an organic group that bonds with Y. 2 and Y 3 represents a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure. 4 and Y 5 represents a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. 20 , and R 21 may be the same or different, and Y 2 , Y 3 , Y 4 and Y 5 may be the same or different. 1 is an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group.

[0074] In the general formula (7), R 16 , R 17 , R 18 and R 19 Examples of the alkyl group include a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, a naphthyl group, a hydroxynaphthyl group, a benzyl group, a methyl group, an ethyl group, an n-butyl group, an n-octyl group, and a cyclohexyl group. Among these, an aromatic group having a substituent such as an alkyl group, an alkoxy group, or a hydroxyl group, such as a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, or a hydroxynaphthyl group, or an unsubstituted aromatic group is more preferable.

[0075] In addition, in the general formula (7), R 20 is Y 2 and Y 3 Similarly, R 21 is the group Y 4 and Y 5 It is an organic group that bonds with Y. 2 and Y 3is a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure. 4 and Y 5 is a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. 20 and R 21 may be the same or different, and the group Y 2 , Y 3 , Y 4 , and Y 5 may be the same or different. In the general formula (7), -Y 2 -R 20 -Y 3 - and -Y 4 -R 21 -Y 5 The group represented by - is composed of a group formed by releasing two protons from a proton donor. As the proton donor, an organic acid having at least two carboxyl groups or hydroxyl groups in the molecule is preferable, an aromatic compound having at least two carboxyl groups or hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferable, and an aromatic compound having at least two hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferable. Examples of the proton donor include catechol, pyrogallol, 1,2-dihydro- Examples of the hydroxynaphthalene include xynaphthalene, 2,3-dihydroxynaphthalene, 2,2'-biphenol, 1,1'-bi-2-naphthol, salicylic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, chloranilic acid, tannic acid, 2-hydroxybenzyl alcohol, 1,2-cyclohexanediol, 1,2-propanediol, and glycerin. Of these, catechol, 1,2-dihydroxynaphthalene, and 2,3-dihydroxynaphthalene are more preferred.

[0076] In addition, Z in the general formula (7) 1represents an organic group or an aliphatic group having an aromatic ring or a heterocyclic ring, and specific examples thereof include aliphatic hydrocarbon groups such as methyl group, ethyl group, propyl group, butyl group, hexyl group, and octyl group; aromatic hydrocarbon groups such as phenyl group, benzyl group, naphthyl group, and biphenyl group; glycidyloxy groups such as glycidyloxypropyl group, mercaptopropyl group, and aminopropyl group; mercapto group; and reactive substituents such as an alkyl group having an amino group and a vinyl group. Among these, the methyl group, the ethyl group, the phenyl group, the naphthyl group, and the biphenyl group are more preferable in terms of thermal stability.

[0077] The method for producing an adduct of a phosphonium compound and a silane compound is to add and dissolve a silane compound such as phenyltrimethoxysilane and a proton donor such as 2,3-dihydroxynaphthalene in a flask containing methanol, and then drip a sodium methoxide-methanol solution at room temperature while stirring. Then, a solution of a tetra-substituted phosphonium halide such as tetraphenylphosphonium bromide dissolved in methanol is dripped at room temperature while stirring, and crystals are precipitated. The precipitated crystals are filtered, washed with water, and vacuum dried to obtain an adduct of a phosphonium compound and a silane compound. However, the method is not limited to this.

[0078] The content of the curing catalyst is preferably 0.05% by mass or more, more preferably 0.08% by mass or more, and particularly preferably 0.10% by mass or more, based on the entire epoxy resin composition particles. By making the content of the curing catalyst equal to or more than the above lower limit, the curability of the epoxy resin composition particles during transfer molding can be effectively improved. On the other hand, the content of the curing catalyst is preferably 2.0% by mass or less, more preferably 1.0% by mass or less, and particularly preferably 0.5% by mass or less, based on the entire epoxy resin composition particles. By making the content of the curing catalyst equal to or less than the above upper limit, the fluidity during sealing can be improved, which contributes to improving the filling property.

[0079] [wax] The epoxy resin composition particles may contain wax as a release agent, if necessary. Examples of waxes include natural waxes such as carnauba wax, synthetic waxes such as ester wax, montan acid ester wax, and oxidized polyethylene wax, and higher fatty acids such as zinc stearate and metal salts thereof.

[0080] The amount of wax blended is, for example, 0.05% by mass or more and 2.0% by mass or less, based on the entire epoxy resin composition particles. The lower limit of the amount of wax blended is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, based on the entire epoxy resin composition particles. The upper limit of the amount of wax blended is preferably 1.5% by mass or less, more preferably 1.0% by mass or less, based on the entire epoxy resin composition particles. By blending the wax in the above range, the obtained epoxy resin composition particles have excellent fluidity and filling property during transfer molding.

[0081] [Coupling agent] The epoxy resin composition particles may contain a coupling agent such as a silane coupling agent, if necessary. Coupling agents include, for example, epoxy silane, amino silane, ureido silane, mercapto silane, and the like.

[0082] Examples of epoxy silanes include γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, and β-(3,4 epoxycyclohexyl)ethyltrimethoxysilane. Examples of aminosilanes include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenylγ-aminopropyltriethoxysilane, N-phenylγ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-6-(aminohexyl)3-aminopropyltrimethoxysilane, and N-(3-(trimethoxysilylpropyl)-1,3-benzenedimethanane. Examples of ureidosilanes include γ-ureidopropyltriethoxysilane and hexamethyldisilazane. Primary aminosilanes include A latent aminosilane coupling agent in which the amino site is protected by reacting with a ketone or aldehyde may be used. The aminosilane may have a secondary amino group. Examples of mercaptosilane include γ-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and silane coupling agents that exhibit the same function as a mercaptosilane coupling agent by thermal decomposition, such as bis(3-triethoxysilylpropyl)tetrasulfide and bis(3-triethoxysilylpropyl)disulfide. These silane coupling agents may be blended after being hydrolyzed in advance. These silane coupling agents may be used alone or in combination of two or more.

[0083] From the viewpoint of continuous moldability, mercaptosilane is preferred, from the viewpoint of fluidity, aminosilane is preferred, and from the viewpoint of adhesion, epoxysilane is preferred.

[0084] The lower limit of the content of the coupling agent such as silane coupling agent that can be used in the epoxy resin composition particles is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and particularly preferably 0.1% by mass or more, based on the entire epoxy resin composition particles. If the lower limit of the content of the coupling agent such as silane coupling agent is within the above range, the interfacial strength between the epoxy resin and the inorganic filler is not reduced, and good vibration resistance can be obtained. In addition, the upper limit of the content of the coupling agent such as silane coupling agent is preferably 1% by mass or less, more preferably 0.8% by mass or less, and particularly preferably 0.6% by mass or less, based on the entire epoxy resin composition particles. If the upper limit of the content of the coupling agent such as silane coupling agent is within the above range, the interfacial strength between the epoxy resin and the inorganic filler is not reduced, and good vibration resistance can be obtained. In addition, if the content of the coupling agent such as silane coupling agent is within the above range, the water absorption of the cured product of the epoxy resin composition particles is prevented from increasing.

[0085] [Other additives] In addition to the above components, the epoxy resin composition particles of the present embodiment may further contain other additives such as colorants, flame retardants, stress reducing agents, etc. These may be used alone or in combination of two or more.

[0086] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0087] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0088] (Examples 1 to 5, Comparative Example 1) <Preparation of Epoxy Resin Composition Particles> The material mixture in which each component was mixed according to the mixing amounts shown in Table 1 below was kneaded with a heated roll, cooled into a sheet shape, and crushed to obtain epoxy resin composition particles (granular molding material). The kneading conditions for the heated roll were a rotation speed of 20 rpm, a temperature of 120° C., and a kneading time of 5 to 10 minutes.

[0089] Comparative Example 2 Except for changing the temperature of the heated roll kneading conditions to 90° C., the same procedure as in Example 1 was followed according to the blending amounts and components in Table 1 to obtain epoxy resin composition particles (granular molding material).

[0090] Details of each component in Table 1 are as follows. Fibrous or needle-like filler 1: Glass fiber (manufactured by Nitto Boseki, CS3E479) Fibrous or needle-like filler 2: Wollastonite fiber (NYCO, NYAD325) Spherical inorganic filler 1: Glass beads (Unitika, Unibeads UB-13L) Spherical inorganic filler 2: Fused silica (Fumitec, FMT-15C) Colorant: Carbon black (Mitsubishi Chemical, #750B) Low stress agent: Epoxy polyether modified silicone oil (Toray Dow Corning, FZ-3730) Epoxy resin: Cresol novolac type epoxy resin (DIC, N-673) Softening point 78℃ Hardener 1: Phenol-based hardener (novolac-type phenolic resin, manufactured by Sumitomo Bakelite Co., Ltd., PR-51470) Softening point: 104°C Hardener 2: Phenol-based hardener (novolac-type phenolic resin, manufactured by Sumitomo Bakelite Co., Ltd., PR-HF-3) Softening point: 80°C Curing catalyst: Imidazole catalyst (2-phenyl-4,5-dihydroxyimidazole, Shikoku Chemical Industry Co., Ltd., 2PHZ-PW) Release agent: Ester wax (Clariant Chemical Japan, Ricowax OP) Coupling agent: Aminosilane coupling agent (Shin-Etsu Chemical Co., Ltd., KBE-903)

[0091] <Number average fiber length> After the epoxy resin composition particles were dissolved in acetone to remove the resin components, the insoluble matter was dispersed on a glass plate, and the fillers in the insoluble matter were photographed using an optical microscope and the fiber length was measured using an image analyzer. The average value of the fiber lengths of the 100 fillers, starting from the longest fiber length, was taken as the number average fiber length (μm).

[0092] [Table 1]

[0093] The obtained epoxy resin composition particles were evaluated for the following items.

[0094] <Spiral Flow> Using a low pressure transfer molding machine (KTS-15, manufactured by Kotaki Seiki Co., Ltd.), the obtained epoxy resin composition particles were injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a pressure retention time of 120 seconds, and the flow length was measured.

[0095] <Bending test: Flexural modulus> The epoxy resin composition particles obtained above were compressed into tablets, which were then injected into a transfer molding machine at a mold temperature of 175°C, injection pressure of 9.8MPa, and curing time of 120 seconds to obtain test pieces of a cured product measuring 10mm wide x 4mm thick x 80mm long. The flexural modulus (GPa) of the obtained test piece at room temperature was measured in accordance with JIS K 6911.

[0096] <k1c> Using a transfer molding machine, a molded body was formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175° C., an injection pressure of 9.8 MPa, and a curing time of 120 seconds. The obtained molded product was cut to a length of 50 mm, width B of 5 mm, and thickness W of 10 mm, and a notch of 3.5 mm in the thickness direction was formed in the center of the length direction, and cured at 175°C for 4 hours to obtain a cured product. Furthermore, a scratch of 0.1 mm in the thickness direction was made with a razor at the tip of the notch of the cured product, and a test piece with a total crack length a = 3.6 mm was prepared. Then, as shown in FIG. 3, a three-point bending test was performed on the obtained test piece 10 using a tension and compression tester (STB-1225S Tensilon manufactured by Orientec Co., Ltd.) at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance S of 40 mm. The fracture toughness value (K1c (MPa m 1 / 2 In the following formula, P Q is the maximum load (N). The tension and compression testing machine in FIG. 3 is equipped with a loading pin 12 having a diameter of 10 mm and two round supports 14 with R processing. K.I. C =((P Q ×S) / (B×W 3 / 2 ))×f(a / W) where f(a / W) = (3(a / W) 1 / 2 [1.99-(a / W)(1-a / W){2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3 / 2 ) The fracture toughness values ​​calculated as above are shown in Table 1.

[0097] <Evaluation of gaps during filling> Forty electromagnetic steel sheets, each 130 mm in diameter and 0.35 mm in thickness, were stacked together, and magnets were inserted into the holes in the stacked steel sheets. The above unit was counted as one stage, and a total of five stages were stacked with a phase shift of 2 mm in circumferential length for stages of different heights to prepare a rotor structure with a skew structure. The workpiece was attached to the mold, and using a transfer molding machine, the above epoxy resin composition particles were injected into the hole in the rotor structure and the space between the magnet under conditions of a mold temperature of 175°C, an injection pressure of 4 MPa, and a pressure retention time of 180 seconds. The presence or absence of gaps in each stage of the obtained molded body was confirmed by a gap gauge. If a 0.02 mm gap gauge cannot be inserted, it is considered good, and if a gap gauge of 0.02 mm or more can be inserted, it is considered bad. In the above-mentioned evaluation of the gap during filling, Examples 1 to 5 showed good results, while Comparative Examples 1 and 2 showed poor results.

[0098] The above results show that the epoxy resin composition particles of Examples 1 to 5 exhibited higher K1c values ​​than those of Comparative Examples 1 and 2, and thus suppressed the occurrence of gaps when filled into a skew structure. Such epoxy resin composition particles of Examples 1 to 5 can be suitably used for fixing a magnet. [Explanation of symbols]

[0099] 1. Epoxy resin composition particles 2. Hopper 41 Heater 42 Screw 43 Cylinder 43a Input cylinder 5 Dice 51 Temperature controller 6 Extrusion Materials 10 Test Pieces 12 Loading pin 14 Round fulcrum 100 injection molding equipment 15 Mold 16 Cavity 20 injection molding machine 21 Cylinder 22 Screw 23 Hopper 24 Heater 25 Nozzles 26 Backflow valve 30. Automotive Electronic Control Unit 32 Wiring board 34 Sealing resin 36 Electronic Components 38 Connection terminal 40 through hole

Claims

1. Epoxy resin composition particles used for fixing a magnet, Epoxy resin, A fibrous or needle-like filler; Including, The fracture toughness value (K1c) measured by the following procedure i is 3.0 MPa m 1/2 The epoxy resin composition particles are as described above. (Step i) Using a transfer molding machine, a molded body is formed from the epoxy resin composition particles under molding conditions of a mold temperature of 175° C., an injection pressure of 9.8 MPa, and a curing time of 120 seconds. The resulting molded product was cut to a length of 50 mm, a width B of 5 mm, and a thickness W of 10 mm, and a notch 3.5 mm deep in the thickness direction was formed in the center of the length direction, followed by curing at 175° C. for 4 hours to obtain a cured product, which was then cut with a razor to a depth of 0.1 mm in the thickness direction at the tip of the notch in the cured product to produce a test specimen with a total crack length a = 3.6 mm. Thereafter, a three-point bending test was performed on the obtained test piece using a tension and compression tester at a measurement temperature of 25°C, a speed of 10 mm / min, and a support distance S of 40 mm, and the fracture toughness value (K1c (MPa m 1/2 In the following formula, P Q is the maximum load (N). K.I. C = ((P Q x S) / (B x W 3/2 ) × f (a / W) where f(a / W)=(3(a / W) 1/2 [1.99-(a / W) (1-a / W) {2.15-3.9(a / W)+2.7(a / W) 2 ]) / (2{1+2(a / W)}{1-(a / W)} 3/2 )

2. Epoxy resin composition particles according to claim 1, Epoxy resin composition particles, wherein the number average fiber length of the fibrous or needle-like filler, as measured by the following procedure A, is 5 μm or more and 500 μm or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and the insoluble matter is dispersed on a glass plate, and the filler particles in the insoluble matter are photographed using an optical microscope and the fiber length is measured using an image analyzer. The average fiber length of the 100 longest fiber particles is defined as the number-average fiber length.

3. Epoxy resin composition particles according to claim 1 or 2, When the number average fiber length of the fibrous or acicular filler measured by the following procedure A is L and the number average fiber diameter of the fibrous or acicular filler measured by the following procedure B is D, Epoxy resin composition particles, wherein L / D is 3 or more and 100 or less. (Procedure A) The epoxy resin composition particles are dissolved in acetone to remove the resin component, and the insoluble portion is dispersed on a glass plate, and the fillers in the insoluble portion are photographed using an optical microscope and the fiber length is measured using an image analyzer. The fiber lengths are measured in descending order of length, and the average value of 100 fillers is taken as the number-average fiber length. (Procedure B) Using a scanning electron microscope, 100 cross sections of the fibrous filler are measured from the cross section of the epoxy resin composition particle, and the average of the smallest diameters of the respective fiber cross sections is calculated as the number average fiber diameter.

4. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles, wherein the fibrous or acicular filler comprises one or more selected from the group consisting of wollastonite fibers, glass fibers, metal fibers, carbon fibers, fibrous aluminum oxide, aramid fibers, silicon carbide whiskers, silicon nitride whiskers, and potassium titanate whiskers.

5. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles having a spiral flow, measured according to the following procedure ii, of 30 cm or more. (Step ii) Using a low-pressure transfer molding machine, the epoxy resin composition particles are injected into a spiral flow measurement mold conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and the flow length (cm) is measured.

6. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles, wherein the content of the fibrous or needle-like filler is 5% by mass or more and 80% by mass or less, based on 100% by mass of the epoxy resin composition particles.

7. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles, wherein the epoxy resin comprises a cresol novolac type epoxy resin and / or a bisphenol A type epoxy resin.

8. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles comprising one or more curing catalysts selected from the group consisting of imidazole-based catalysts and phosphorus-based catalysts.

9. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles used for molding into tablets through a process of supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material, and a process of cutting the epoxy resin molding material while continuously extruding the molten epoxy resin molding material from an opening at the tip of the extruder to obtain tablets.

10. Epoxy resin composition particles according to claim 1 or 2, Epoxy resin composition particles comprising an epoxy resin having a softening point of less than 110°C or a curing agent.

11. A tablet formed using the epoxy resin composition particles according to claim 1 or 2, 5 cm 3 More than 1500cm 3 Tablets having the following volumes:

12. A step of preparing the epoxy resin composition particles according to claim 1 or 2; A step of supplying the epoxy resin composition particles to a heated extruder and kneading them while melting them to obtain an epoxy resin molding material; and a step of cutting the molten epoxy resin molding material into columnar tablets while continuously extruding the molten epoxy resin molding material from an opening at the tip of an extruder, The cross-sectional area of ​​the cylindrical tablet is 3 cm 2 More than 100cm 2 Below is the Method for manufacturing columnar tablets.

13. A structure using the epoxy resin composition particles according to claim 1 or 2.

14. A method for producing the structure according to claim 13, comprising the steps of: Using an injection molding apparatus including an injection unit including a cylinder and a screw inserted into the cylinder, and a mold having a cavity and connected to the injection unit, melting the epoxy resin composition particles in the cylinder to obtain a molten resin composition; a step of injecting a molten resin composition from a tip of the screw to fill the cavity; A method for manufacturing a structure comprising:

15. A method for producing the structure according to claim 14, comprising the steps of: The method for producing a structure, wherein in the step of filling, a temperature T of the tip of the screw is 60 to 100° C.

16. A method for producing the structure according to claim 14, comprising the steps of: A method for manufacturing a structure, wherein in the filling step, the temperature inside the cavity is 150 to 180°C.

Citation Information

Patent Citations

  • Epoxy resin, epoxy resin composition, epoxy resin cured product and composite material

    WO2020053937A1