Fabrication of solid material or film from polymerizable liquid
By employing reactive oligomers and monomers with controlled molar bonding ratios, the mechanical properties of single reaction mechanism energy polymerizable resins are enhanced, producing photoplastics with improved toughness and elongation for use in inkjet printing and additive manufacturing.
Patent Information
- Application Number
- JP2024125054
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-09-07
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Single reaction mechanism energy polymerizable resins exhibit poor mechanical properties compared to traditional thermoplastics, such as low toughness, elongation, and tensile strength, due to issues like chain termination, high crosslink density, and difficulty in controlling polymerization rates, which limits their use in applications like inkjet printing and additive manufacturing.
The use of reactive oligomers and monomers with specific molar bonding ratios, along with photoinitiators, to form photoplastics with improved mechanical properties through a single reaction mechanism, allowing for the production of three-dimensional objects with enhanced storage stability and reduced toxicity.
The resulting photoplastics demonstrate mechanical properties comparable to thermoplastics, including high tensile strength and elongation, suitable for applications in inkjet printing and additive manufacturing, while maintaining low viscosity and stability during processing.
Smart Images

Figure 2024156821000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims priority to U.S. Provisional Patent Application No. 15 / 698,059, filed September 7, 2017, which claims the benefit of U.S. Provisional Patent Application No. 62 / 484,103, filed April 11, 2017, and U.S. Provisional Patent Application No. 62 / 484,644, filed April 12, 2017.
[0002] The entire contents of the above applications are incorporated herein by reference.
[0003] The present disclosure relates to materials and methods for producing solid materials or films from liquid materials and objects produced by the methods. More specifically, the present disclosure relates to single reaction mechanism energy polymerizable materials designed as photoplastics. [Background technology]
[0004] Single-reaction mechanism energy polymerizable resins, once cured, generally have inferior mechanical properties compared to traditional thermoplastics. This is the primary reason for the predominance of thermoplastics in many of the materials found and relied upon in manufacturing environments. Specifically, the toughness of thermoplastic materials, including both impact strength, elongation, and tensile strength, is many times greater, if not more, than single-reaction mechanism energy polymerizable materials. Energy-initiated reaction mechanisms are generally free radical polymerizations, but can also be cationic polymerizations. In most cases, polymerization occurs at ambient conditions (25°C, 1 atm). There are four aspects of single-reaction mechanism polymerization that are known to limit mechanical properties:
[0005] 1) Linear polymers are very tough and important for the production of high strength, high elongation thermoplastics such as polyethylene, polypropylene, PET, polycarbonate, and nylon. The main chain structures of these widely used thermoplastics contain many repeat units that occasionally contain high strength structures that provide the ability to stack, align, and weakly bond polymer chains to each other and / or small side or branched chains off the main chain, but these do not generally significantly impede polymer chain entanglement or interchain mobility. The most common reaction mechanism for producing linear polymers by energy-initiated free radical polymerization uses monofunctional monomers. However, these reactions are usually carried out in ambient air, and chain termination reactions due to inhibitions such as dissolved oxygen result in significantly shorter chain lengths than comparable thermoplastics. These linear polymers are also entirely carbon backbone chains, with less entanglement and larger side chains. These features eliminate many of the beneficial low force interactions found in the thermoplastics mentioned above, resulting in a material with low toughness.
[0006] 2) The rate of free radical polymerization produces polymers with very small molecular weights compared to the conventional polymers mentioned above. In the energy polymerization of a single reaction mechanism, the use of difunctional or higher functionality monomers results in non-linear polymers with high crosslink density. Although the molecular weight is very high or even enormous, these highly crosslinked systems generally have very high strength. On the other hand, the elongation is very low because the crosslinks and high density of covalent bonds prevent the polymer chains from moving within the network. For this reason, linear polymers are produced using monofunctional monomers as before. The polymerization of these monomers takes place in three steps: initiation, propagation, and termination. Depending on the energy received by the system during polymerization, the amount of initiator used, and / or the inhibitors, the propagation in the above steps is generally significantly shortened. One reason for the shortened propagation is due to the instability of the generated free radicals, which can react with O2 and other chemical inhibitors resulting in chain termination. Another reason is due to the vitrification that occurs during curing, which limits the mobility of the molecules and, in turn, the conversion rate. For this reason, the number of repeating units in the energy-polymerized monofunctional system of a single reaction mechanism is significantly smaller than that of thermoplastic materials. In the case of such low molecular weights, it is known that the entanglement of linear chains is very small, resulting in a material with significantly low strength.
[0007] 3) One method being explored to circumvent many of the above problems is the use of high molecular weight, generally multifunctional, energetically polymerizable oligomers. These oligomers result in higher molecular weight initiators, resulting in final materials with lower crosslink density and higher overall molecular weight of the polymer chain. However, these high molecular weight oligomers have very high viscosities, which severely limits their use in viscosity-limited applications such as inkjet printing and additive manufacturing.
[0008] 4) Finally, it has been shown that in energy-initiated free radical polymerization, it is very difficult to control the polymerization mechanism and rate of polymerization of species with various free radical-inducing reactive functional groups. To achieve the desired rapid polymerization rate, there is a trade-off between high energy cure and high proportion of photoinitiator. Either of these will essentially result in chain termination and low molecular weight. This makes it very challenging to control the system at the molecular level, and the molecular weight construction, crosslink density distribution, polymer network construction, conversion rate, chain termination, and reaction rate of individual molecular species are not uniform, and the final product shows a wide glass transition temperature (Tg) distribution and unstable mechanical strength.
[0009] Inkjet inks used for printing films on substrates or material jetting in additive manufacturing require very low viscosities at jetting temperatures, typically less than about 20 cPs. Hot melt inks have been used, but liquid inks are generally more suitable for high volume industrial printing. Single reaction mechanism energy polymerizable inks use low viscosity reactive materials to achieve the desired viscosity. The reactive materials have reactive groups that polymerize upon exposure to UV radiation or electron beams after printing. The low viscosity reactive materials in single reaction mechanism energy polymerizable inks typically include low viscosity monomers and possibly low proportions of low viscosity oligomers. Single reaction mechanism energy polymerizable inks may also include low proportions of high viscosity reactive or non-reactive oligomers and polymers. Inkjet inks have traditionally included large amounts of monofunctional monomers, as these have particularly low viscosities. As discussed above, these monofunctional monomers, when polymerized, result in poor performance mechanical properties in the final product.
[0010] In conventional layer-by-layer or three-dimensional manufacturing techniques, the construction of a solid object is carried out in a multi-stage or layer-by-layer manner. In particular, the layer formation is generally carried out by curing a photopolymerizable resin under the application of visible or UV light irradiation. Two techniques are known: in one, a new layer is formed on the upper surface of the growing body, in the other, a new layer is formed on the lower surface of the growing body.
[0011] If a new layer is to be formed on top of the growth body, after each irradiation step the object being built is dropped into a "bath" of resin, a new layer of resin is coated on top, and a new irradiation step is performed. The disadvantage of such a "top-down" technique is that the growth body must be lowered into a (possibly deep) bath of liquid resin and a precise top layer of liquid resin must be reconstructed.
[0012] If new layers are formed below the growth body after each irradiation step, the object under construction is sufficiently separated from the bottom plate during fabrication. Such "bottom-up" techniques may eliminate the need for deep baths in which objects are submerged, by instead lifting the object from a relatively shallow hole or bath. A limitation of both of these deposition techniques is also viscosity, with fluids with viscosities generally below 2000 cPs being required to achieve homogeneous layers at the top or bottom interfaces. In addition, bottom-up techniques favor stiffer materials to obtain homogeneous layer placement and surface finish in the final part. Finally, pot-life stability is important for either technique, since polymerization that can occur without energy initiation can result in defects in parts, or even worse, solidify the entire bath. Such reactions include, for example, many dual reaction mechanism materials offered by Carbon 3D, such as CE220, CE221, EPU40, EPX81, FPU50, RPU60, RPU61, RPU70, etc. Summary of the Invention [Problem to be solved by the invention]
[0013] Therefore, new materials and methods are needed to inkjet print or additively manufacture three-dimensional objects with good mechanical properties along with a single polymerization mechanism that improves pot-life storage stability, reduces the toxicity of the unpolymerized material, and / or reduces the time for thermal post-cure. [Means for solving the problem]
[0014] According to some embodiments, A reactive oligomer, which is at least one of (i) a multifunctional methacrylate oligomer and (ii) a multifunctional acrylate oligomer; a reactive monofunctional monomer, which is at least one of (i) a monofunctional N-vinyl monomer, (ii) a monofunctional vinyl ether monomer, (iii) a monofunctional vinyl ester monomer, (iv) a monofunctional vinyl amide monomer, (v) a styrene monomer, (vi) a monofunctional acrylamide monomer, (vii) a monofunctional (meth)acrylate monomer, (viii) a cyanoacrylate monomer, (ix) a monofunctional vinyl carbonate monomer, (x) a monofunctional acryloyl monomer, and (xi) a monofunctional vinyl carbamate monomer; 16. A free radically polymerizable liquid for forming three-dimensional objects comprising: The molar combination ratio of the reactive ethylenically unsaturated groups of the reactive monofunctional species to the reactive ethylenically unsaturated groups of the reactive polyfunctional species is at least 10: 1. Free-radically polymerizable liquids are energy polymerizable liquids that cure by a single reaction mechanism to form photoplastic materials.
[0015] In additional embodiments of the present disclosure, the polymerizable liquid comprises from about 0.01% to about 15% by weight of a photoinitiator.
[0016] In another embodiment of the present disclosure, the polymerizable liquid has a toughness equal to or greater than the utilization curve defined by the equations: 1) tensile strength (MPa) = -0.75 x elongation + 130 (when the elongation is about 15% to about 95%), 2) tensile strength (MPa) = 4500 / (elongation - 25) - 5 (when the elongation is about 95% to about 500%).
[0017] In another embodiment of the present disclosure, the polymerizable liquid has a toughness equal to or greater than the utilization curve defined by the equations: 1) tensile strength (MPa) = -1 x elongation + 120 (when elongation is less than 105%), 2) tensile strength (MPa) = 2000 / (elongation + 10) - 3 (when elongation is from about 105% to about 550%), 3) tensile strength (MPa) = 0.5 (when elongation is greater than about 550%).
[0018] In another embodiment of the present disclosure, the polymeric material achieves the desired mechanical properties without the input of heat.
[0019] In another embodiment of the present disclosure, the polymerizable liquid comprises at least one of a non-reactive light absorbing pigment, a filler, a polymerization inhibitor, and a polymerization catalyst in an amount of about 0.001% to about 10% by weight.
[0020] In another embodiment of the present disclosure, the polymerizable liquid comprises a non-reactive light absorbing pigment in an amount of about 0.001% to about 10% by weight, and a filler.
[0021] In other embodiments of the present disclosure, the oligomer and monomer react via the same reaction mechanism but have different reaction rates.
[0022] In another embodiment of the present disclosure, the solubility of the monomers and oligomers is altered during polymerization, thereby favoring homopolymerization of either the monomeric or oligomeric species.
[0023] In another embodiment of the present disclosure, the polymerization produces materials with multiple glass transition temperatures.
[0024] In another embodiment of the present disclosure, the polymerization produces a material with two different glass transition temperatures, the Tg of which differs by at least 60°C.
[0025] In another embodiment of the present disclosure, the molar combination ratio of reactive ethylenically unsaturated groups of the reactive monofunctional species to reactive ethylenically unsaturated groups of the reactive multifunctional species is at least 25:1.
[0026] In another embodiment of the present disclosure, the molar combination ratio of reactive ethylenically unsaturated groups of the reactive monofunctional species to reactive ethylenically unsaturated groups of the reactive multifunctional species is at least 30:1.
[0027] In another embodiment of the present disclosure, the polymerizable liquid forms a print on the substrate.
[0028] In other embodiments of the present disclosure, the polymerizable liquid is cured to form a film or three-dimensional object by stereolithography (SLA), digital light projection (DLP), material jetting, or inkjet printing.
[0029] In other embodiments of the present disclosure, the inkjet film or 3D printed layer has a thickness greater than about 30 μm.
[0030] In another embodiment of the present disclosure, the polymerizable liquid has tunable mechanical properties upon curing by varying the energy polymerization conditions.
[0031] In another embodiment of the present disclosure, the polymerizable liquid is non-toxic.
[0032] In other embodiments of the present disclosure, the oligomer has a molecular weight greater than about 1500 g / mol.
[0033] In other embodiments of the present disclosure, the oligomer has a molecular weight greater than about 4000 g / mol.
[0034] In another embodiment of the present disclosure, the monomer is a monofunctional N-vinyl, vinyl ester, or acryloyl selected from the group consisting of N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylformamide, acryloylmorpholine, or vinylcinnamate.
[0035] According to some embodiments, (i) a reactive oligomer which is at least one of: (i) an N-vinyl oligomer having a functionality of 1 or more, (ii) a vinyl ether oligomer having a functionality of 1 or more, (iii) a vinyl ester oligomer having a functionality of 1 or more, (iv) a vinyl amide oligomer having a functionality of 1 or more, (v) a styrene oligomer, (vi) acrylamide oligomer having a functionality of 1 or more, (vii) a (meth)acrylate oligomer having a functionality of 1 or more having a different reaction rate than the (meth)acrylate monomer having a functionality of 1 or more, (viii) a cyanoacrylate oligomer, (ix) a vinyl carbonate oligomer having a functionality of 1 or more, and (x) an acryloyl oligomer having a functionality of 1 or more, (xi) a vinyl carbamate oligomer having a functionality of 1 or more; (i) a reactive monomer that is at least one of N-vinyl monomers of a functionality of 1 or more, (ii) a vinyl ether monomer of a functionality of 1 or more, (iii) a vinyl ester monomer of a functionality of 1 or more, (iv) a vinyl amide monomer of a functionality of 1 or more, (v) a styrene monomer, (vi) acrylamide monomer of a functionality of 1 or more, (vii) a (meth)acrylate monomer of a functionality of 1 or more having a different reaction rate than a (meth)acrylate oligomer of a functionality of 1 or more, (viii) a cyanoacrylate monomer, (ix) a vinyl carbonate monomer of a functionality of 1 or more, (x) an acryloyl monomer of a functionality of 1 or more, and (xi) a vinyl carbamate monomer of a functionality of 1 or more; 23. A method of forming a polymerizable liquid comprising the step of mixing together: The polymerizable liquid is an energy polymerizable liquid that cures to form a photoplastic material by a single reaction mechanism.
[0036] In additional embodiments of the present disclosure, the polymerizable liquid is cured to form a film or three dimensional object by stereolithography (SLA), digital light projection (DLP), material jetting (inkjet printing in 3D), or inkjet printing.
[0037] In other embodiments of the present disclosure, the film or three-dimensional object is a medical device, or a part of footwear, or a part of soft robotics.
[0038] In other embodiments of the present disclosure, the film or three-dimensional object is a hydrogel.
[0039] In another embodiment of the present disclosure, pixel or voxel polymerization is used to obtain different physical properties by varying the energy polymerization conditions.
[0040] In another embodiment of the present disclosure, the method further comprises the step of irradiating the polymerizable liquid with patterned radiation.
[0041] In another embodiment of the present disclosure, the method further comprises the step of admixing a photoinitiator in an amount of about 0.01% to about 15% by weight.
[0042] According to some embodiments, the article includes an energy-polymerizable liquid that cures by a single reaction mechanism to form a photoplastic material. The energy-polymerizable liquid may be selected from the group consisting of (i) N-vinyl oligomers of one or more functionalities, (ii) vinyl ether oligomers of one or more functionalities, (iii) vinyl ester oligomers of one or more functionalities, (iv) vinyl amide oligomers of one or more functionalities, (v) styrene oligomers, (vi) acrylamide oligomers of one or more functionalities, (vii) (meth)acrylate oligomers of one or more functionalities having a different reaction rate than the (meth)acrylate monomers of one or more functionalities, (viii) cyanoacrylate oligomers, (ix) vinyl carbonate oligomers of one or more functionalities, and (x) acryloyl oligomers of one or more functionalities. (xi) a reactive oligomer which is at least one of a vinyl carbamate oligomer having a functionality of 1 or more, and a reactive monomer which is at least one of (i) an N-vinyl monomer having a functionality of 1 or more, (ii) a vinyl ether monomer having a functionality of 1 or more, (iii) a vinyl ester monomer having a functionality of 1 or more, (iv) a vinyl amide monomer having a functionality of 1 or more, (v) a styrene monomer, (vi) acrylamide monomer having a functionality of 1 or more, (vii) a (meth)acrylate monomer having a functionality of 1 or more having a different reaction rate than the (meth)acrylate oligomer having a functionality of 1 or more, (viii) a cyanoacrylate monomer, (ix) a vinyl carbonate monomer having a functionality of 1 or more, (x) an acryloyl monomer having a functionality of 1 or more, and (xi) a vinyl carbamate monomer having a functionality of 1 or more.
[0043] In additional embodiments of the present disclosure, the polymerizable liquid has tunable mechanical properties upon curing by varying the energy polymerization conditions.
[0044] The present disclosure further provides a method for forming a solid photoplastic material comprising (i) a first component, an energy-polymerizable liquid, and (ii) a second component, an energy-polymerizable liquid, different from the first component, by a single reaction mechanism, in which the components are mixed and polymerized upon exposure to energy to form a solid photoplastic material.
[0045] In some embodiments, the reactive diluent includes acrylates, methacrylates, styrene, acrylic acid, vinyl amides, vinyl ethers, vinyl esters (including derivatives), polymers comprising any one or more of these, combinations of two or more of these (e.g., acrylonitrile, styrene, divinylbenzene, vinyl toluene, methyl acrylate, ethyl acrylate, butyl acrylate, methyl (meth)acrylate, amine (meth)acrylates, and mixtures of two or more of these, as described above).
[0046] In some embodiments, the non-reactive polymer comprises a polymer or polymer blend that does not have a functional group that participates in the polymerization of the bulk material. Many polymers can be used, including but not limited to polyethylene, polypropylene, polycarbonate, polyvinyl chloride, PET, and mixtures of two or more thereof.
[0047] In some embodiments, the first component comprises reactive monomers or oligomers having acrylate functionality, in which embodiment, the first components preferably or necessarily react with each other to form a single polymer network.
[0048] In some embodiments, the second component comprises a reactive monomer or oligomer having (meth)acrylate functionality. In this embodiment, the first components preferably or necessarily react with each other to form a single polymer network.
[0049] In some embodiments, the second component comprises reactive monomers or oligomers having N-vinyl, vinyl ether, acryloyl, vinyl carbonate, vinyl carbamate, vinyl ester, and / or vinyl amide functionality, in which the second components preferably or necessarily react with each other to form a single polymer network.
[0050] In some embodiments, the first component comprises reactive monomers or oligomers having acrylate and / or methacrylate functionality and the second component comprises reactive monomers or oligomers having N-vinyl, vinyl ether, vinyl carbonate, vinyl carbamate, acryloyl, vinyl ester, and / or vinyl amide functionality, in which the components react with each other to form a random copolymer.
[0051] In some embodiments, the first component comprises a reactive monomer or oligomer having acrylate and / or methacrylate functionality, and the second component comprises a reactive monomer or oligomer having N-vinyl, vinyl ether, vinyl carbonate, vinyl carbamate, acryloyl, vinyl ester, and / or vinyl amide functionality. In this embodiment, the components react with each other to form a full IPN, semi-IPN, pseudo-IPN, or dual network. In some embodiments, the three-dimensional object comprises a polymer blend (e.g., IPN, semi-IPN, pseudo-IPN, sequential IPN, simultaneous IPN, dual network) formed from the first component and the second component.
[0052] In some embodiments, the energetically polymerizable liquid of the single reaction mechanism comprises from 1, 2, or 5% to 20, 30, 40, 90, or 99% by weight of the first component; and from 1, 10, 60, 70, or 80% to 95, 98, or 99% by weight of the second component (optionally including one or more additional components). In other embodiments, the energetically polymerizable liquid of the single reaction mechanism comprises from 1, 2, or 5% to 20, 30, 40, 90, or 99% by weight of the second component; and from 1, 10, 60, 70, or 80% to 95, 98, or 99% by weight of the first component (optionally including one or more additional components).
[0053] In some embodiments, the second component is cured simultaneously with the same light as the first component in the same irradiation step.
[0054] In some embodiments, the second component is subsequently cured with light of a different wavelength than the light of the irradiation step.
[0055] In some embodiments, the second component is subsequently cured with light of the same wavelength as the light of the irradiation step.
[0056] In some embodiments, the second component is subsequently cured with an electron beam.
[0057] One particular embodiment of the invention disclosed herein is a method for forming a three-dimensional object comprising a single-reaction mechanism energy-polymerizable liquid, the method comprising the steps of: providing an optically transparent member having a carrier and a build surface, the carrier and the build surface defining a build region therebetween; filling the build region with a polymerizable liquid comprising at least two of (meth)acrylate oligomers, cyanoacrylate monomers, acrylamide monomers, vinyl ether monomers, vinyl ester monomers, N-vinyl monomers, vinyl carbonate monomers, vinyl carbamate monomers, acryloyl monomers, and vinyl amide monomers; irradiating the build region with light through the optically transparent member to form a solid polymer skeleton; releasing the carrier from the build surface to form a three-dimensional intermediate having the same shape as the three-dimensional object or a shape to be incorporated into the three-dimensional object; and then irradiating the three-dimensional intermediate with sufficient energy to form the three-dimensional object from the three-dimensional intermediate.
[0058] In some embodiments, the curable or single reaction mechanism energy polymerizable liquid is changed at least once during the method with a subsequent curable or single reaction mechanism energy polymerizable liquid, optionally cross-reactive with the previous curable or single reaction mechanism energy polymerizable liquid in subsequent polymerizations to form an object having a plurality of structural segments covalently bonded to one another, each having different mechanical properties (e.g., tensile strength).
[0059] A further aspect of the disclosure described herein is a single reaction mechanism energetically polymerizable liquid useful for the production of films or three-dimensional objects comprising (meth)acrylates and their vinyl functional resins by additive manufacturing or inkjet printing. The single reaction mechanism energetically polymerizable liquid is a) at least one component selected from the group of oligomers consisting of: (i) one or more functional acrylate oligomers, (ii) one or more functional (meth)acrylate oligomers, and (iii) one or more functional vinyl oligomers; b) at least one component having a different reaction rate than (a) selected from the vinyl group consisting of: (i) N-vinyl monomers of a functionality of 1 or more, (ii) vinyl ether monomers of a functionality of 1 or more, (iii) vinyl ester monomers of a functionality of 1 or more, (iv) vinyl amide monomers of a functionality of 1 or more, (v) styrene monomers, (vi) acrylamide monomers, (vii) (meth)acrylate monomers, (viii) cyanoacrylate monomers, (ix) vinyl carbonate monomers of a functionality of 1 or more, (x) acryloyl monomers of a functionality of 1 or more, (xi) vinyl carbamate monomers of a functionality of 1 or more; c) one or more photoinitiators d) optionally a reactive diluent; e) optionally a non-reactive polymer; f) optionally, one or more polymerization inhibitors; g) optionally, one or more non-reactive light absorbing pigments or dyes, if present, in an amount of 0.001 to 10% by weight; and h) optional fillers (e.g., reinforcing agents such as silica, carbon fiber, aluminum, core-shell rubber, combinations thereof, etc.); Contains a mixture of.
[0060] A further aspect of the present disclosure is a single reaction mechanism energetically polymerizable liquid useful for the production of films or three-dimensional objects comprising acrylate and its methacrylate functional resins by additive manufacturing or inkjet printing. The single reaction mechanism energetically polymerizable liquid is a) at least one component selected from the oligomer group consisting of one or more functional acrylate oligomers; b) at least one component selected from the methacrylate group consisting of one or more functional methacrylate monomers; c) one or more photoinitiators; d) optionally a reactive diluent; e) optionally a non-reactive polymer; f) optionally, one or more polymerization inhibitors; g) optionally, one or more non-reactive light absorbing pigments or dyes, if present, in an amount of 0.001 to 10% by weight; and h) optional fillers (e.g., reinforcing agents such as silica, carbon fiber, aluminum, core-shell rubber, combinations thereof, etc.); Contains a mixture of.
[0061] In some embodiments, the single reaction mechanism energy polymerizable liquid used in the present invention includes a non-reactive pigment or dye, such as, but not limited to, (i) titanium dioxide (e.g., in an amount of 0.05 or 0.1 to 1 or 5% by weight), (ii) carbon black (e.g., in an amount of 0.05 or 0.1 to 1 or 5% by weight), and / or (iii) an organic UV absorber, such as hydroxybenzophenone, hydroxyphenylbenzotriazole, oxanilide, benzophenone, thioxanthone, hydroxyphenyltriazine, and / or benzotriazole UV absorber (e.g., in an amount of 0.001 or 0.005 to 1, 2, or 4% by weight).
[0062] In some embodiments, a hindered amine light stabilizer, or a Lewis acid, or an oxidizable tin salt is included in the single reaction mechanism energetic polymerizable liquid in an amount effective to promote the formation of a three-dimensional intermediate during manufacture (e.g., 0.01 or 0.1 to 1 or 2 weight percent or more).
[0063] In some embodiments, a hindered amine light stabilizer, or a Lewis acid, or an oxidizable tin salt is included in the single reaction mechanism energetic polymerizable liquid in an amount effective to selectively promote polymerization of the first and / or second components of the polymerizable resin (e.g., 0.01 or 0.1 to 1 or 2 weight percent or more).
[0064] A further aspect of the present disclosure is a three-dimensional object comprising an energy-polymerizable first component and an energy-polymerizable component that has a reaction kinetic difference from the first component and that polymerizes by the same reaction mechanism as the first component, and / or the three-dimensional object is manufactured by an additive manufacturing process.
[0065] A further aspect of the present disclosure is a three-dimensional object comprising an energy-polymerizable first component and an energy-polymerizable component that differs from the first component by its solubility prior to polymerization and that is polymerized by the same reaction mechanism as the first component, and / or the three-dimensional object is manufactured by an additive manufacturing process.
[0066] A further aspect of the invention described herein is a three-dimensional object comprising an energy-polymerizable first component and an energy-polymerizable component that differs from the first component by its solubility after polymerization. Both components are polymerized by the same reaction mechanism and / or the three-dimensional object is manufactured by an additive manufacturing process. If the solubility of the components relative to each other changes during polymerization, phase separation may induce homopolymerization of either component, changing the refractive index of the material.
[0067] A further aspect of the present disclosure is a three-dimensional object comprising an energy-polymerizable first component and an energy-polymerizable component that differs from the first component by 500% molar bond ratio (second component:first component molar bond ratio of 5:1 or more) and that polymerizes via the same reaction mechanism as the first component, and / or the three-dimensional object is manufactured by an additive manufacturing process.
[0068] A further aspect of the present disclosure is a three-dimensional object comprising an energy-polymerizable first component and an energy-polymerizable component that differs from the first component by 700% molar bond ratio (second component:first component molar bond ratio of 7:1 or more) and that polymerizes via the same reaction mechanism as the first component, and / or the three-dimensional object is manufactured by an additive manufacturing process.
[0069] In some embodiments, the object comprises a first component, a third component that is different from the second component and that is curable (or that further reacts, polymerizes or chain extends), where the object has at least a first structural segment and a second structural segment covalently bonded to each other, the first structural segment comprises the curable second component, the second structural segment comprises the curable third component, and both the first structural segment and the second structural segment comprise the same or different photopolymerized first component.
[0070] In some embodiments, the article comprises a polymer blend formed from a first component and a second component.
[0071] The object may have a shape that cannot be formed by injection molding or casting.
[0072] Further areas of applicability will be apparent from the description provided herein. It should be understood that the description and specific examples are for purposes of illustration only and are not intended to limit the scope of the present disclosure.
[0073] The drawings are for illustrative purposes only and are not intended to limit the scope of the disclosure in any way. [Brief description of the drawings]
[0074] [Figure 1A] FIG. 1A is a plot of a single reaction mechanism energetically polymerizable polymer in accordance with the present invention. [Figure 1B] FIG. 1B is another plot of a single reaction mechanism energetically polymerizable polymer in accordance with the present invention. [Figure 1C]FIG. 1C is yet another plot of a single reaction mechanism energetically polymerizable polymer in accordance with the present invention. [Diagram 2] FIG. 2 is a plot of the toxicity profile of a tough polymeric material according to the present invention. [Diagram 3] FIG. 3 shows a classification of IPNs according to the invention. [Figure 4] FIG. 4 shows (a) a full IPN and (b) a semi-IPN according to the present invention, respectively (solid lines=first polymer network, dashed lines=second polymer network). [Diagram 5] FIG. 5 illustrates (a) a quasi-IPN (i.e., two entangled networks with possible weak bonds between the networks) after polymerization of two or more constituent polymerizable resins, and (b) a quasi-IPA (i.e., two entangled networks with covalent chemical crosslinks between the networks) after polymerization of two or more constituent polymerizable resins, in accordance with the present invention. [Figure 6] FIG. 6 shows a dual network with contrasting structures after polymerization of two or more constituent polymerizable resins, where the two networks have no chemical bonds between the networks, and is an example showing the chemical structures of PAMPS and PAAm to form such a structure according to the present invention. [Figure 7] FIG. 7 is a flow diagram illustrating the formation of a continuous IPN after polymerization of two or more constituent polymerizable resins in accordance with the present invention (solid lines=first polymer network, dashed lines=second polymer network). [Figure 8] FIG. 8 is a flow diagram showing the formation of a simultaneous IPN after polymerization of two or more constituent polymerizable resins according to the present invention (solid lines = first polymer network, dashed lines = present second polymer network, open squares and filled circles = different monomers). [Figure 9A] FIG. 9A shows the different molecular weight control of IPN networks in the case of (a) long networks and (b) short networks in accordance with the present invention (solid line=crosslinked polymer network, dashed line=second monomer polymer network). [Figure 9B]FIG. 9B shows the different molecular weight control of monomer segments of random copolymers in the case of (a) long networks and (b) short networks in accordance with the present invention (solid line=crosslinked polymer network, dashed line=second monomer polymer network). [Figure 9C] FIG. 9C shows a chain-extended backbone IPN network using a monomer according to the invention (solid lines = crosslinked network 1, long dashed lines = polymer chains extended by a monomer, short dashed lines = a second monomer network, which may or may not be the same as the chain-extending monomer). [Figure 9D] FIG. 9D shows a second network chain extended with a monomer according to the invention (solid lines=crosslinked network 1, long dashed lines=chain extended monomer network, short dashed lines=second monomer network, a different monomer than the chain extending monomer). [Figure 10A] FIG. 10A shows a semi-IPN polymerization system using two components having energy-polymerizable functional groups with different single reaction mechanisms according to the present invention: I. a multifunctional (meth)acrylate oligomer, and II. a monofunctional vinyl monomer (solid line = polymer network of part I, dashed line = polymer network of part II). [Figure 10B] FIG. 10B shows a full IPN polymerization system using two components having energy-polymerizable functional groups with different single reaction mechanisms according to the present invention: I. multifunctional (meth)acrylate oligomer, II. multifunctional vinyl monomer (solid line = polymer network of part I, dashed line = polymer network of part II). [Figure 10C] FIG. 10C shows a full IPN polymerization system using two components having energetically polymerizable functional groups with different single reaction mechanisms according to the present invention: I. multifunctional (meth)acrylate oligomer, II. multifunctional vinyl oligomer (solid line = polymer network of part I, dashed line = polymer network of part II). [Figure 10D]FIG. 10D shows a semi-IPN polymerization system using two components having energy-polymerizable functional groups with different single reaction mechanisms according to the present invention: I. monofunctional (meth)acrylate monomer, II. multifunctional vinyl oligomer (dashed line = polymer network of part I, solid line = polymer network of part II). [Figure 10E] FIG. 10E shows a full IPN polymerization system using two components with energetically polymerizable functional groups of different single reaction mechanisms according to the present invention: I. multifunctional (meth)acrylate monomer, II. multifunctional vinyl oligomer (solid line = polymer network of part I, dashed line = polymer network of part II). [Figure 10F] FIG. 10F shows a pseudo-IPN polymerization system using two components having energy-polymerizable functional groups with different single reaction mechanisms according to the present invention: I. a monofunctional (meth)acrylate monomer, II. a monofunctional vinyl monomer (solid line = polymer network of part I, dashed line = polymer network of part II). [Figure 11] FIG. 11 shows a plot of the tensile properties of specimens of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0075] The following description is merely exemplary in nature and is in no way intended to limit the disclosure, its application, or uses.
[0076] The present invention will now be described more fully with reference to the accompanying drawings, in which like numbers refer to like elements throughout. In the figures, certain lines, layers, components, elements or features may be bolded for clarity. Where used, dashed lines indicate optional functions or operations unless otherwise noted.
[0077] When an element is described as being "on," "attached," "connected," "coupled with," "in contact with," etc., it is understood to be directly on, attached to, connected to, coupled with, and / or in contact with other elements, and that intervening elements may be present. On the other hand, when an element is described as being, for example, "directly on other elements," "directly attached to other elements," "directly connected to other elements," "directly coupled to other elements," "directly in contact with other elements," there are no intervening elements. It will be understood by one of ordinary skill in the art that a description of a structure or feature that is located adjacent to another feature may have overlapping or underlying portions of the adjacent feature.
[0078] To simplify the description of the relationship of an element or feature to other elements or features when shown in the figures, spatial terms such as "below," "upper," and the like may be used herein. Spatial terms are understood to encompass different orientations of the device in use or operation in addition to the orientation shown in the figures. For example, if the device in the figures is turned upside down, an element described as "below" another element or feature would be placed "above" the other element or feature. Thus, for example, the term "below" can encompass both an orientation of above and below. The device may be oriented in different directions (rotated 90 degrees or at other orientations), and the spatial terms used herein will be interpreted accordingly. Similarly, terms such as "upward," "downward," "vertically," "horizontally," and the like are used herein for descriptive purposes only, unless otherwise noted.
[0079] "Shape imparted" refers to cases where the shape of the intermediate object changes slightly between its formation and the subsequent formation of the three-dimensional product, typically due to shrinkage (e.g., ∼1, 2, or 4% by volume), expansion (e.g., ∼1, 2, or 4% by volume), removal of support structures, or the introduction of a shaping step (e.g., intentional bending, stretching, drilling, grinding, cutting, polishing, or other intentional shaping after formation of the intermediate product and prior to the subsequent formation of the three-dimensional product). As noted above, the three-dimensional intermediate may be washed as desired prior to further polymerization and / or before, during, or after any intervening shaping steps.
[0080] The polymerized material may assume the desired mechanical properties without the input of heat. The polymerized material may also be heated. Heating may be active (e.g., in an oven, such as an electric oven, gas oven, solar oven, etc.) or passive (such as at ambient temperature). Active heating is generally more rapid than passive heating and is preferred in some embodiments, although passive heating, such as simply maintaining the intermediate at ambient temperature long enough to effect further polymerization, is preferred in some embodiments.
[0081] Voxels represent values on a regular grid in three-dimensional space. Similar to pixels in a bitmap, voxels themselves do not usually have their location (coordinates) explicitly coded along with their value. Instead, a voxel's location is inferred based on its position relative to other voxels (i.e., its position within the data structures that make up a single volumetric image). In contrast to pixels and voxels, points and polygons are often explicitly represented by the coordinates of their vertices. A direct consequence of this difference is that polygons can efficiently represent simple 3D structures with significant empty or uniformly filled space, while voxels excel at representing non-uniformly filled and regularly sampled spaces.
[0082] In contrast to polymers, which in principle have an unlimited number of monomers, oligomers are molecular complexes consisting of a small number of monomer units. Dimers, trimers, and tetramers are, for example, oligomers composed of two, three, and four monomers, respectively.
[0083] Single reaction mechanism energy polymerization, single reaction mechanism energy polymerizability, single reaction mechanism energy polymerized, single reaction mechanism energy polymerization, single reaction mechanism energy irradiation, single reaction mechanism energy irradiation refers to inducing polymerization by either actinic radiation, UV light, visible light, or electrons. Examples of such include UV light (100 nm to 405 nm), visible light (405 nm to 700 nm), or electron beams. A non-exhaustive list of exemplary light sources for carrying out the present invention includes LEDs, laser diodes, laser beams, lamps (such as halogen lamps, Xe, Xe-Hg lamps), LED lasers or LED projectors used in additive manufacturing, LCD, LED or plasma screens that emit visible light, mobile or tablet devices. The polymerization is carried out by a single reaction mechanism such as free radical, cationic, Michael addition, sequential, or click chemistry.
[0084] Photoplastics are materials formed by the energetic polymerization of liquid materials with a single reaction mechanism. Compared to existing photopolymers, photoplastics have mechanical properties comparable to materials known as thermoplastics, as shown, for example, in Figures 1A, 1B, 1C, and 2. Photoplastics can exhibit physical and mechanical properties superior to or equivalent to high-performance thermoplastics such as nylon 6, polycarbonate, PET, polypropylene, polyethylene, and a wide range of thermoplastic copolymers. In addition, photoplastics can exhibit physical and mechanical properties superior to or equivalent to other high-performance rubbers such as silicone and vulcanized natural rubber. Photoplastics can take the form of various polymer networks, including, but not limited to, interpenetrating networks and random copolymer networks.
[0085] Interpenetrating Networks. Interpenetrating networks, or interpenetrating polymer networks, or IPNs, refer to polymers that contain two or more networks that are at least partially entangled (but not necessarily covalently bonded to each other) on a polymer scale. These IPNs can take a variety of forms in their embodiments: full, semi, or pseudo. In some embodiments, these networks are also referred to as dual networks (DNs). Finally, in some embodiments, either or both sequential or simultaneous processes may be used to construct these networks. Examples of different classifications of IPNs are shown in FIG. 3.
[0086] Interpenetrating polymer networks (IPNs) are a method used in polymer science to prepare composite materials from two immiscible or miscible raw materials. The final product consists of two networks that are independently cross-linked by chemical or physical bonds. In such systems, the two phases are continuous in space and each is in contact with all parts of the sample's space.
[0087] As shown in Figure 4, full and semi-IPNs differ based on whether crosslinking is present in one or both of the respective components. Herein, less than 1% crosslinking is defined as a full IPN network, and 1%-99% partial crosslinking is defined as a semi-IPN network. Semi-IPNs contain separable linear and / or branched networks. Pseudo-IPNs have polymer chains that fill or grow into the internal voids of a pre-existing structure or network.
[0088] Pseudo-IPNs, as seen in Figure 5, represent a special category of rotaxanes that usually undergo partial or complete phase separation because the linear chains are thermodynamically incompatible with the crosslinking components and usually have sufficient molecular mobility to phase separate spontaneously.
[0089] The dual network (DN) seen in Figure 6 is known as a concept different from full, semi, or pseudo IPNs. Although IPNs do not have a significant improvement in mechanical strength compared to the original single network structure, they can combine various physical and chemical properties such as cell adhesion, water absorption, biocompatibility, and biodegradability. DN gels differ from fiber-reinforced hydrogels, which consist of a mechanically tough "dry" component (hydrophobic plastic) and a mechanically weak "wet" component (hydrophilic gel), in that the tough dry component essentially determines the mechanical properties of the composite, while the hydrophilic component acts as a water absorbent but does not practically function to improve mechanical strength. The high strength of DN gels is due to the nonlinear effect of the binary structure, rather than a linear combination of the two component networks as in common IPNs and fiber-reinforced hydrogels. Although the two networks are both mechanically weak, i.e., the first network is stiff and brittle and the second network is soft and ductile, the DN gels they are composited with are stiff but not brittle, ductile but not soft.
[0090] These interpenetrating polymer networks can be obtained by a simultaneous method, shown in FIG. 8, where all chemicals are mixed together and reacted at the same time, or by a sequential method, shown in FIG. 7. Sequential polymerization can be performed in stages, where a premixed resin has the components to be polymerized in the first step, with the backbone network swollen with unpolymerized material to be polymerized in the next step. Sequential network polymerization can also rely on swelling of a presynthesized network in a solution containing the second polymer to be crosslinked. In the latter case, a high porosity of the first network can be useful to obtain a sufficient content of the second polymer in the composite to be produced. Thus, for aqueous systems such as hydrogels, freeze-drying can be a suitable method to effectively remove the retained water and form macroporous sponges.
[0091] As shown in Figure 9, the molecular weight of each network in the IPN can be controlled. Various factors can be used to control the molecular weight of each network, such as the relative ratio of each component in the system, the relative ratio of components to initiator, and the relative ratio of components to inhibitor. In addition, when UV energy is used for polymerization, the power consumption and light energy can be used to control the molecular weight.
[0092] IPNs, semi-IPNs, pseudo-IPNs, and dual networks can be detected by two different glass transition temperatures measured by DMA or DSC.
[0093] In some embodiments, the material has low toxicity. Toxic materials are often used to obtain thermoplastic-like properties in dual polymeric materials and are also shown in FIG. 2. Toxic materials are substances that are toxic or have potential health effects. Toxic materials can usually cause physiological damage if ingested or inhaled by humans. There are various concerns about chemicals such as low molecular weight amines, e.g., trimethylolpropane poly(oxypropylene) triamine or 4,4'-methylene bis(2-methylcyclohexylamine). There are also various concerns about chemicals with isocyanate functionality.
[0094] Non-limiting examples of hindered amine light stabilizers useful in the practice of the present invention include 2,2,6,6-tetramethylpiperidine derivatives, 1,6-hexanediamine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-, polymers with 2,4,6-trichloro-1,3,5-triazine, reaction products of N-butyl-1-butanamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine, butanedioic acid 1,4-dimethyl ester, polymers with 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol. mer, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate + methyl(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, 2,2,6,6-tetramethyl-4-piperidinyl stearate (fatty acid mixture), 1,6-hexanediamine, N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-, polymers with 2,4,6-trichloro-1,3,5-triazine, and reaction products with 2,4,4-trimethyl-2-pentanamine.
[0095] Oxidizable tin salts useful in the practice of the present invention include, but are not limited to, stannous butanoate, stannous octanoate, stannous hexanoate, stannous heptanoate, stannous linoleate, stannous phenylbutyrate, stannous phenylstearate, stannous phenyloleate, stannous nonanoate, stannous decanoate, stannous undecenoate, stannous dodecanoate, stannous stearate, stannous oleate, stannous octanoate, dibutyltin dilaurate, dibutyltin dioleate, dibutyltin distearate, dipropyltin dilaurate, dipropyltin dioleate, dipropyltin distearate, dibutyltin dihexanoate, and combinations thereof. See U.S. Patent Nos. 5,298,532, 4,421,822, and 4,389,514, the disclosures of which are incorporated herein by reference. In addition to the oxidizable tin salts mentioned above, Lewis acids, such as those described in Chu et al., Macromolecular Symposia, Vol. 95, No. 1, pp. 233-242 (June 1995), are known to enhance the polymerization rate of free radical polymerizations, which is incorporated herein by reference.
[0096] Any suitable filler may be utilized in the various embodiments described herein depending on the desired properties of the part or object being manufactured. Thus, the fillers may be solid or liquid, organic or inorganic, including reactive and non-reactive rubbers: siloxanes, acrylonitrile butadiene rubbers; reactive and non-reactive thermoplastics (including but not limited to poly(etherimides), maleimide-styrene terpolymers, polyarylates, polysulfones, polyethersulfones, etc.); inorganic fillers such as silicates (talc, clay, silica, mica, etc.), glass, carbon nanotubes, graphene, carbon fibers, metals, cellulose nanocrystals, etc., and combinations of all of the above. Suitable fillers include reinforcing agents such as core-shell rubbers, as described below.
[0097] Reinforcing agents. One or more polymeric and / or inorganic reinforcing agents, such as those described in US Patent Publication No. 20150215430, the entire contents of which are incorporated herein by reference, can be used as fillers in the present invention. The reinforcing agent may be in the form of particles and uniformly dispersed in the polymerization product. The particles may be less than 5 microns (μm) in diameter. Without being limited thereto, such reinforcing agents include elastomers, branched polymers, hyperbranched polymers, dendrimers, rubbery polymers, rubbery copolymers, block copolymers, core-shell particles, oxides or inorganic materials, such as clays, polyhedral oligomeric silsesquioxanes (POSS), carbonaceous materials (e.g., carbon black, carbon nanotubes, carbon nanofibers, fullerenes), ceramics and silicon carbide, which may or may not be surface modified or functionalized. Block copolymers include, for example, those described in U.S. Patent No. 6,894,113, the entire contents of which are incorporated herein by reference, and include "NANOSTRENGTH®" SBM (polystyrene-polybutadiene-polymethacrylate) and AMA (polymethacrylate-polybutylacrylate-polymethacrylate), both manufactured by Arkema. Other suitable block copolymers include FORTEGRA® and the amphiphilic block copolymers described in U.S. Patent No. 7,820,760, the entire contents of which are incorporated herein by reference.Known core-shell particles include, for example, core-shell (dendrimer) particles having compositions as described in US Patent Publication No. 20100280151 (Nguyen et al., Toray Industries, Inc., 2010) for amine branched polymers in which the shell is grafted to a core polymer polymerized with a polymerizable monomer containing an unsaturated carbon-carbon bond; core-shell rubber particles as described, for example, in EP Patent Publication No. 1632533 and EP Patent Publication No. 2123711, the entire contents of which are incorporated herein by reference; and the "KaneAce MX" product line, which are particle / epoxy blends having a polymer core polymerized with a polymerizable monomer such as butadiene, styrene, other unsaturated carbon-carbon bond monomers, or combinations thereof, and particles having a polymer shell that can be mixed with an epoxy, typically polymethyl methacrylate, polyglycidyl methacrylate, polyacrylonitrile, or similar polymers as further described below. Also suitable as block copolymers in the present invention are the "JSR SX" series, which are carboxylated polystyrene / polyvinylbenzene manufactured by JSR Corporation; "Kureha Paraloid" EXL-2655, which is a butadiene alkyl methacrylate styrene copolymer (manufactured by Kureha Corporation); "Stafiloid" AC-3355 and TR-2122, which are acrylate methacrylate copolymers (both manufactured by Takeda Pharmaceutical Co., Ltd.); and "PARALOID" EXL-2611 and EXL-3387, which are butyl acrylate methyl methacrylate copolymers (both manufactured by Rohm & Haas). Suitable oxide particles include, for example, NANOPDX®, which is manufactured by nanoresins AG. It is a master blend of functionalized nanosilica particles and epoxy.
[0098] Core-shell rubber. Core-shell rubber is a particulate material (particle) with a rubber-like core. Such materials are known and described in U.S. Patent Application Publication No. 20150184039 and U.S. Patent Application Publication No. 20150240113, the entire contents of which are incorporated herein by reference, as well as U.S. Patent Nos. 6,861,475, 7,625,977, 7,642,316, and 8,088,245.
[0099] In some embodiments, the core-shell rubber particles are nanoparticles (i.e., have an average particle size of less than 1000 nanometers (nm)). Typically, the average particle size of core-shell rubber nanoparticles is less than 500 nm, such as less than 300 nm, less than 200 nm, less than 100 nm, or even less than 50 nm. Typically, such particles are spherical, so the particle size is the diameter. However, if the particle is not spherical, the particle size is defined as the longest dimension of the particle.
[0100] In some embodiments, the rubbery core may have a Tg of less than -25°C, more preferably less than -50°C, and even more preferably less than -70°C. The Tg of the rubbery core may be significantly less than -100°C. The core-shell rubber also has at least one shell portion with a Tg of 50°C or greater. "Core" refers to the interior of the core-shell rubber. The core may form the center of the core-shell particle, or the interior shell or region of the core-shell rubber. The shell is the portion of the core-shell rubber that is outside the rubbery core. The shell portion(s) typically form the outermost portion of the core-shell rubber particle. The shell material may be grafted to the core and may be crosslinked. The rubber core may constitute 50-95% by weight or 60-90% by weight of the core-shell rubber particle.
[0101] The core of the core-shell rubber may be a polymer or copolymer of a conjugated diene such as butadiene, or a lower alkyl acrylate such as n-butyl-, ethyl-, isobutyl-, or 2-ethylhexyl acrylate. The core polymer may further contain up to 20% by weight of other copolymerized monounsaturated monomers such as styrene, vinyl acetate, vinyl chloride, methyl methacrylate, etc. The core polymer may be crosslinked. The core polymer may contain up to 5% of copolymerized graft-linking monomers having two or more heterogeneous reactive unsaturated sites (provided that at least one reactive site is non-conjugated), such as diallyl maleate, monoallyl fumarate, allyl methacrylate, etc.
[0102] The core polymer may be a silicone rubber. This material often has a glass transition temperature below −100° C. Core-shell rubbers with silicone rubber cores include those available under the trade name Genioperl from Wacker Chemie, Munich, Germany.
[0103] The shell polymer, which may be chemically grafted or crosslinked to the rubbery core, may be polymerized from at least one lower alkyl methacrylate, such as methyl methacrylate, ethyl methacrylate, or t-butyl methacrylate. Homopolymers of such methacrylate monomers may be used. Additionally, up to 40% by weight of the shell polymer may be formed from other monovinylidene monomers, such as styrene, vinyl acetate, vinyl chloride, methyl acrylate, ethyl acrylate, butyl acrylate, and the like. The molecular weight of the grafted shell polymer may be from 20,000 to 500,000.
[0104] One suitable type of core-shell rubber is one that has reactive groups on the shell polymer that can react with an epoxy resin or an epoxy resin hardener. Glycidyl groups are suitable. The glycidyl groups are provided by monomers such as glycidyl methacrylate.
[0105] An example of a suitable core-shell rubber is of the type described in EP 1 632 533 A1 (published in 2007 / 0027233), the entire contents of which are incorporated herein by reference. As described therein, the core-shell rubber particles comprise a crosslinked rubber core, which is most often a crosslinked copolymer of butadiene, and a shell, which is preferably a copolymer of styrene, methyl methacrylate, glycidyl methacrylate, and optionally acrylonitrile. The core-shell rubber is preferably dispersed in a polymer or epoxy resin, as described in the literature. Suitable core-shell rubbers include, but are not limited to, those sold under the name Kaneka Kane Ace by Kaneka Corporation, such as the Kaneka Kane Ace 15 and 120 series products, such as Kaneka Kane Ace MX120, Kaneka Kane Ace MX153, Kaneka Kane Ace MX154, Kaneka Kane Ace MX156, Kaneka Kane Ace MX170, and Kaneka Kane Ace MX257, and Kaneka Kane Ace MX120 core-shell rubber dispersions, and mixtures thereof.
[0106] I. Single-reaction mechanism energetically polymerizable liquids have advantages over conventional IPN systems because two or more parts can be premixed or combined in the liquid state. However, the components are referred to herein as Part A and Part B. Part A
[0107] As described herein, the polymerization system includes a first polymerization system (sometimes referred to herein as "Part A") that is polymerized by energy radiation, typically light, and sometimes ultraviolet (UV) radiation. Any suitable polymerizable liquid may be used as the first component. The liquid (sometimes referred to herein as "liquid resin", "ink", or simply "resin") may include monomers or preferentially oligomers, particularly photopolymerizable and / or free radical polymerizable monomers or oligomers, suitable initiators, such as free radical initiators, and combinations thereof. Examples include, but are not limited to, acrylic, methacrylic, vinyl, acrylamide, styrene, olefin, halogenated olefin, cyclic alkene, maleic anhydride, alkene, alkyne, carbon monoxide, functionalized oligomers, multifunctional cutosite monomers, functionalized PEG, and combinations thereof. Non-limiting examples of liquid resins, monomers and initiators include those described in U.S. Pat. Nos. 8,232,043, 8,119,214, 7,935,476, 7,767,728, 7,649,029, International Publication No. 2012129968, China Patent No. 102715751, and Japan Patent Application Publication No. 2012210408, the entire contents of which are incorporated herein by reference.
[0108] Hydrogels. In some embodiments, suitable resins include photopolymerizable hydrogels such as poly(ethylene glycol) (PEG) and gelatin. PEG hydrogels have been used to deliver a variety of biologics, such as growth factors. However, a major challenge facing PEG hydrogels that are crosslinked by chain-growth polymerization is the potential for irreversible protein damage. Inclusion of affinity binding peptide sequences in the monomer-resin solution prior to photopolymerization to allow sustained delivery improves conditions that maximize the release of biologics from photopolymerized PEG diacrylate hydrogels. Gelatin is a biopolymer frequently used in the food, cosmetic, pharmaceutical, and photography industries. Gelatin is obtained by thermal denaturation or chemical and physical degradation of collagen. There are three types of gelatin, including those found in animals, fish, and humans. Gelatin obtained from the skin of cold-water fish is considered safe for use in pharmaceutical applications. UV or visible light can be used to crosslink appropriately modified gelatin. Methods for crosslinking gelatin include polymer derivatives obtained from dyes such as Rose Bengal.
[0109] Acid-catalyzed polymerizable liquids. In some embodiments, as described above, single reaction mechanism energy polymerizable liquids include free radical polymerizable liquids (where the inhibitor can be oxygen, as described below), while in other embodiments, single reaction mechanism polymerizable liquids include polymerizable liquids that are polymerized by acid catalysis or cationically. In such embodiments, the polymerizable liquids include monomers that contain groups suitable for acid catalysis, such as epoxide groups, vinyl ether groups, etc. Thus, suitable monomers include olefins, such as methoxyethene, 4-methoxystyrene, styrene, 2-methylprop-1-ene, 1,3-butadiene; heterocyclic monomers (including lactones, lactams, and cyclic amines), such as oxiranes, thietanes, tetrahydrofurans, oxazolines, 1,3-dioxepanes, oxetan-2-ones, and combinations thereof. Suitable (generally ionic or non-ionic) photoacid generators (PAGs) may be included in the acid-catalyzed polymerizable liquid, including, but not limited to, onium salts, sulfonium and iodonium salts, such as diphenyl iodide hexafluorophosphate, diphenyl iodide hexafluoroarsenate, diphenyl iodide hexafluoroantimonate, diphenyl p-methoxyphenyl triflate, diphenyl p-toluenyl triflate, diphenyl p-isobutylphenyl triflate, diphenyl p-tert-butylphenyl triflate, triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroarsenate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium triflate, dibutylnaphthylsulfonium triflate, and the like, and mixtures thereof.See, e.g., U.S. Pat. Nos. 7,824,839, 7,550,246, 7,534,844, 6,692,891, 5,374,500, and 5,017,461, the entire contents of which are incorporated herein by reference, and also see Photoacid Generator Selection Guide for the electronics industry and energy curable coatings (BASF 2010), the entire contents of which are incorporated herein by reference.
[0110] Photopolymerizable silicones. Suitable resins include photopolymerizable silicones. UV-polymerizable silicone rubbers, such as Siliopren® UV-polymerizable silicone rubbers, can be used as well as LOCTITE® polymerizable silicone adhesive sealants. Applications include optical instruments, medical and surgical instruments, exterior lighting and enclosures, electrical connectors / sensors, fiber optics, gaskets, and molds.
[0111] Biodegradable resins. Biodegradable resins are particularly important for the application of implantable devices or temporary features for drug delivery, such as biodegradable screws and stents (U.S. Patent Nos. 7,919,162 and 6,932,930, the entire contents of which are incorporated herein by reference). Biodegradable copolymers of lactic and glycolic acid (PLGA) are dissolved in PEG di(meth)acrylate to provide transparent resins suitable for use. Polycaprolactone and PLGA oligomers can be functionalized with acrylic or methacrylic groups to provide effective resins for use.
[0112] Photopolymerizable polyurethanes. Particularly useful materials are photopolymerizable polyurethanes, including polyureas and copolymers of polyurethanes and polyureas (e.g., poly(urethane-ureas)). Photopolymerizable polyurethane / polyurea compositions containing (1) a polyurethane based on an aliphatic diisocyanate, poly(hexamethylene isophthalate glycol) and optionally 1,4-butanediol, (2) a multifunctional acrylic ester, (3) a photoinitiator, and (4) an antioxidant can be formulated to be hard, abrasion-resistant, and stain-resistant materials (U.S. Pat. No. 4,337,130, the entire contents of which are incorporated herein by reference). Photopolymerizable thermoplastic polyurethane elastomers incorporate photoreactive diacetylenic diols as chain extenders.
[0113] High performance resin. In some embodiments, a high performance resin is used. Such high performance resin may require heating to melt and / or reduce viscosity, as described above and further below. Such resins include, but are not limited to, resins for materials sometimes called liquid crystal polymers of ester, esterimide, and esteramide oligomers, as described, for example, in U.S. Pat. Nos. 7,507,784 and 6,939,940, the entire contents of which are incorporated herein by reference. Since such resins are sometimes used as high temperature thermosetting resins, the present invention further includes a suitable photoinitiator, such as benzophenone, anthraquinone, and fluoroenone initiators (including their derivatives), to initiate crosslinking upon irradiation, as described further below.
[0114] Additional Resin Examples: Resins particularly useful for dental applications include EnvisionTEC's Clear Guide, EnvisionTEC's E-Denstone Material. Resins particularly useful for hearing aid applications include EnvisionTEC's e-Shell 300 series resins. Particularly useful resins include EnvisionTEC's HTM140IV high temperature molding material for direct use with vulcanized rubber in molding / casting applications. Particularly useful materials for making tough, hard parts include EnvisionTEC's RC31 resin. Particularly useful resins for investment casting applications include EnvisionTEC's Easy Cast EC500 resin and MadeSolid FireCast resin.
[0115] Photoplastic materials can exhibit qualities that are particularly useful for use in the dental industry. The increased toughness of photoplastics compared to traditional (meth)acrylate and vinyl ether based materials suggests that they may perform well in some dental applications. Photoplastics can be formulated and processed to improve biocompatibility compared to traditional SLA materials.
[0116] Additional Resin Components. The liquid resin or polymerizable material may have solid particles suspended or dispersed therein. Any suitable solid particles may be used depending on the final product being produced. The particles may be metallic, organic / polymeric, inorganic, or composites or mixtures thereof. The particles may be non-conductive, semi-conductive, or conductive (such as metallic and non-metallic or polymeric conductors), and the particles may be magnetic, ferromagnetic, paramagnetic, or non-magnetic. The particles may be any suitable shape, such as spherical, elliptical, cylindrical, etc. The particles may be any suitable size (e.g., ranging from 1 nm to 20 μm average diameter).
[0117] The particles may include active agents or imaging compounds, as described below, which may also be provided dissolved or solubilized in a liquid resin, as described below. For example, magnetic or paramagnetic particles or nanoparticles may be used.
[0118] Depending on the particular purpose of the product being manufactured, the liquid resin may have additional components solubilized such as pigments, dyes, active or pharmaceutical compounds, imaging compounds (e.g., fluorescent, phosphorescent, radioactive), etc. Without being limited thereto, such additional components may include, for example, proteins, peptides, nucleic acids (DNA, RNA) such as siRNA, sugars, small organic compounds (drugs and drug-like compounds), combinations thereof, etc.
[0119] Light absorbers. In some embodiments, the single-reaction mechanism energy polymerizable liquid for carrying out the present invention includes a pigment or dye that absorbs light, particularly UV light. Suitable examples of such light absorbers include, but are not limited to, (i) titanium dioxide (e.g., in an amount of 0.05 or 0.1 to 1 or 5 wt %), (ii) carbon black (e.g., in an amount of 0.05 or 0.1 to 1 or 5 wt %), and / or (iii) organic UV absorbers such as hydroxybenzophenone, hydroxyphenylbenzotriazole, oxanilide, benzophenone, thioxanthone, hydroxyphenyltriazine, and / or benzotriazole UV absorbers (e.g., Mayzo BLS1326) (e.g., in an amount of 0.001 or 0.005 to 1, 2, or 4 wt %). Suitable organic UV absorbers include, but are not limited to, those described in U.S. Pat. Nos. 3,213,058, 6,916,867, 7,157,586, and 7,695,643, the disclosures of which are incorporated herein by reference.
[0120] Polymerization Inhibitors. Inhibitors or polymerization inhibitors for use in the present invention may be in liquid or gaseous state. In some embodiments, gaseous inhibitors are preferred. In some embodiments, liquid inhibitors such as oils or lubricants (e.g., fluorinated oils such as perfluoropolyethers) may be used as inhibitors (or as release layers to maintain the liquid interface). The specific inhibitors will vary depending on the monomers being polymerized and the polymerization reaction. For free radical polymerization monomers, oxygen is a convenient inhibitor, provided in gaseous state such as air, oxygen-rich gas (sometimes preferably including additional inert gases to reduce flammability in some embodiments), or pure oxygen gas in some embodiments. Free radical scavengers or inhibitors such as MEHQ (monomethyl ether hydroquinone) and PTZ (phenothiazine) may also be used to inhibit polymerization. In addition, stable radical compounds capable of scavenging free radicals may be used to inhibit radical polymerization. In alternative embodiments, such as where the monomers are polymerized by a photoacid generating initiator, the inhibitor may be a base such as ammonia, trace amines (e.g., methylamine, ethylamine, di- and trialkylamines, e.g., dimethylamine, diethylamine, trimethylamine, triethylamine), and the like, carbon dioxide, or mixtures or combinations thereof.
[0121] Polymerizable liquid carrying living cells. In some embodiments, a single reaction mechanism energy polymerizable liquid carries living cells as particles. Such polymerizable liquids are generally aqueous, may be hydrogen peroxide, and may be considered "emulsions" in which the living cells are the dispersed phase. Suitable living cells may be plant cells (e.g., monocotyledonous, dicotyledonous), animal cells (e.g., mammalian, avian, amphibian, reptilian cells), microbial cells (e.g., prokaryotic, eukaryotic, protozoan, etc.). The cells may be differentiated cells or corresponding to any type of tissue (e.g., blood, cartilage, bone, muscle, endocrine glands, exocrine glands, epithelium, endothelium, etc.), or may be undifferentiated cells such as stem cells or progenitor cells. In such embodiments, the polymerizable liquid may be one that forms a hydrogel, including, but not limited to, those described in U.S. Pat. Nos. 7,651,683, 7,651,682, 7,556,490, 6,602,975, and 5,836,313, the entire contents of which are incorporated herein by reference.
[0122] II. Single-reaction mechanism energetic polymeric liquids: Part B
[0123] As mentioned above, in some embodiments of the present invention, the single reaction mechanism energy polymerizable liquid includes a first energy polymerizable component (sometimes referred to herein as "Part A") and a second component (sometimes referred to herein as "Part B") that cures by energy polymerization in the same reaction mechanism as the first component, typically by further reaction, polymerization, or chain extension. Many of these embodiments can be implemented. Note that below, where a specific acrylate, such as a methacrylate, is described, other acrylates can also be used. Note that below, where a specific vinyl, such as an N-vinyl, is described, other vinyls can also be used. Figure 10 illustrates the formation of various IPNs that can occur between acrylate-functional and vinyl-functional materials. These include semi-IPNs (Figures 10A, 10D) when monofunctional monomers are used with multifunctional monomers or oligomers, full IPNs (Figures 10B, 10C, 10E) when multifunctional monomers or oligomers are used with oligomeric multifunctional monomers, and pseudo-IPNs (Figure 10F) when monofunctional monomers are used with monofunctional monomers.
[0124] Chemistry of Part A. As mentioned above, in some embodiments of the invention, the resin has a first component called "Part A". Part A comprises a mixture of monomers and / or oligomers and / or prepolymers that are polymerizable upon exposure to actinic radiation or light. The resin may have one or more functionalities. The purpose of Part A is to "lock" the shape of the material or object being formed or to form a backbone for one or more additional components (e.g., Part B). What is important is that there is at least the minimum amount of Part A required to maintain the shape of the material or object being formed after the initial cure. In some embodiments, this amount corresponds to less than 10, 20, or 30% by weight of the total resin (polymerizable liquid) composition.
[0125] In some embodiments, moiety A is capable of reacting to form a crosslinked polymer network or a solid homopolymer.
[0126] Suitable reactive end groups for the component, oligomer, or prepolymer of part A include, but are not limited to, for example, acrylate, methacrylate, α-olefin, N-vinyl, vinylamide, cyanoacrylate, acrylamide, methacrylamide, acryloyl, styrene, epoxide, thiol, 1,3-dienes, vinyl halides, acrylonitrile, vinyl esters, maleimides, and vinyl ethers, vinyl carbonates, vinyl carbamates.
[0127] An aspect of the curing of Part A is to provide a scaffold onto which a second reactive resin component, called "Part B," can be cured in a second step (which can occur simultaneously with or after the curing of Part A). This second reaction preferably occurs without significantly distorting the initial shape defined during the curing of Part A, as would otherwise occur in the desired initial shape.
[0128] In certain embodiments, the cure of part A is continuously inhibited during printing in certain areas with oxygen or amines or other reactive species, forming a liquid interface between the cured parts and an inhibitor-permeable film or window (e.g., accomplished by continuous liquid interphase / interface printing).
[0129] Chemistry of Part B. Part B may comprise a mixture of monomers and / or prepolymers having reactive end groups that participate in a second cure reaction during or after the cure reaction of Part A. In some embodiments, Part A and Part B may be premixed, Part B may be added to Part A simultaneously so that it is present during exposure to the energy radiation, or Part B may be injected into the material or object in a subsequent step after polymerization of Part A. Methods used to cure Part B include, but are not limited to, for example, exposing the material or object to light of a different wavelength than that which polymerized Part A, or light of the same wavelength as that which polymerized Part A, or electrons in the case of electron beam polymerization (or a combination thereof).
[0130] Suitable reactive end groups for the component, monomer, or prepolymer of part B include, but are not limited to, for example, acrylate, methacrylate, α-olefin, N-vinyl, vinylamide, cyanoacrylate, vinyl carbonate, vinyl carbamate, acrylamide, methacrylamide, styrene, epoxide, thiol, 1,3-dienes, vinyl halides, acryloyl, acrylonitrile, vinyl ester, maleimide, and vinyl ether.
[0131] Those of skill in the art will recognize other suitable reactive species for part B. Components of part B useful for forming polymers are described in the Concise Polymeric Materials Encyclopedia and the Encyclopedia of Polymer Science and Technology, the entire contents of which are incorporated herein by reference.
[0132] Organic peroxides. In some embodiments, organic peroxides can be included in the single reaction mechanism energy polymerizable liquid or resin, for example, to promote reaction of double bonds that may remain unreacted during thermal and / or microwave irradiation polymerization. Such organic peroxides can be included in the resin or polymerizable liquid in any suitable amount, such as from 0.001 or 0.01 or 0.1% by weight to 1, 2 or 3% by weight. Suitable organic peroxides include, but are not limited to, 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane (e.g., LUPEROX 101®), dilauroyl peroxide (e.g., LUPEROX LP®), benzoyl peroxide (e.g., LUPEROX A98®), bis(tert-butyldioxyisopropyl)benzene (e.g., VulCUP R®), and combinations thereof. Such organic peroxides are available from a variety of suppliers, including but not limited to Arkema (420 rue d'Estienned'Orves, 92705 Colombes Cedex, France).
[0133] Catalysts. Other catalysts known to those skilled in the art that can affect the rate of polymerization of the other part A or B may be used to adjust the energy polymerization rate of a single reaction mechanism for either or both of parts A and B (e.g., metal catalysts such as peroxides, tin catalysts, and / or amine catalysts; platinum or tin catalysts for silicone resins; ruthenium catalysts for ring-opening metathesis polymerization resins; copper catalysts for click chemistry resins, and the like (these catalysts contact the article as a liquid aerosol, such as by immersion), or aminoplast-containing resins such as those containing N-(alkoxymethyl)acrylamides, hydroxyl groups, blocked acid catalysts).
[0134] Inhibitors. In some embodiments, other inhibitors known to those skilled in the art that can affect the rate or initiation of polymerization of part A or part B may be used to adjust the initiation or polymerization rate of the energy of a single reaction mechanism of either or both of part A and part B.
[0135] In some embodiments, the reaction rate of one component is significantly slower than the other. This can be achieved by choosing raw materials with significantly different reactivities or by using an inhibitor that preferentially inhibits one component. By slowing the reaction rate, one component can be more completely polymerized before the other component is completely polymerized. In some embodiments, this can result in the formation of a continuous IPN.
[0136] In some embodiments, the solubility of the second component in the first component changes during polymerization of the first component. Generally, all components are soluble in the liquid state. In some embodiments, while the first component is polymerizing to form a solid, the solubility of the other liquid components changes, resulting in solid-liquid phase separation at the nano-, micro-, and macro-levels. This phase separation can be seen by a change in the refractive index of the material. This phase separation can change the reaction selectivity of the components and promote homopolymerization. This phase separation can change the mechanical properties of the material, such as the elasticity and rebound of an elastomer.
[0137] In some embodiments, the solubility of the second component in the other components changes during polymerization of the second component. Generally, all components are soluble in the liquid state. In some embodiments, while one component is polymerizing to form a solid, the solubility of the other liquid components does not change significantly. As the second component polymerizes to form a solid, the solubility in the second component changes, resulting in solid-state phase separation at the nano-, micro-, and macro-levels. This phase separation can be evidenced by a change in the refractive index of the material. This phase separation can change the mechanical properties of the material, such as the elasticity and rebound of an elastomer.
[0138] In some embodiments of the present invention, it may be useful to use photoplastics in acoustical or sound deadening applications. IPN materials are known to exhibit interesting and unique acoustic absorption, sound and vibration properties over a wide temperature range.
[0139] In some embodiments of the invention, part A is composed of a high elongation urethane-based (meth)acrylate oligomer. Part A, which is UV-polymerizable, is blended with part B, which is composed mainly of monofunctional n-vinyl monomers, and used to solidify objects into desired shapes using 3D printing with high reaction rates and selective reaction pathways as described herein, resulting in a scaffold for part B in a single-reaction mechanism energetically polymerizable liquid. This scaffold is generally very elastic but weak. After printing, the object is further polymerized by single-reaction mechanism energetic polymerization, which polymerizes the second component and forms a strong linear, semi-crosslinked or fully crosslinked IPN through the scaffold, resulting in an elastomer-containing object.
[0140] Bonding of formed objects. In some embodiments, it may be useful to define the shape of multiple objects by curing part A, arrange these objects in a specific configuration so that there are hermetic seals between the objects, and then polymerize a secondary cure of part B. In this way, strong bonds can be provided between the parts during manufacturing. A particularly useful example is in forming and bonding sneaker components.
[0141] Fusion of particles as Part B. In some embodiments, "Part B" may simply comprise small particles of preformed polymer. After curing of Part A, the object may be heated above the glass transition temperature of Part B to polymerize the encapsulated polymer particles.
[0142] Photocleavable End Groups. In some embodiments, reactive species of part A are cleaved upon exposure to energy to generate new reactive species after curing of part A. The newly formed reactive species can further react with part B in a secondary solidification.
[0143] Methods for mixing components. In some embodiments, the components may be mixed sequentially before being introduced to the build plate of the printer. This can be done using a multi-barrel syringe and mixing nozzle. For example, part A may include a UV-polymerizable di(meth)acrylate resin and part B may include or consist of a vinyl monomer. It is usually possible to premix both parts A and B thoroughly before application, since they are highly shelf stable even when all components are mixed. Shelf stability can be defined as having a viscosity within 10% of the original viscosity in the premixed bottle at ambient conditions for 1, 2, 3, or 4 years. This can be simulated by high temperature stability at 60° C. for 1, 2, 3, or 4 weeks. However, if necessary, a second syringe barrel would contain the material of part B. Furthermore, when the resin is introduced to the printer in this manner, a fixed time is defined between mixing all components and curing of part A or part B.
[0144] Other Additive Manufacturing Techniques It will be apparent to one skilled in the art that the materials described in this invention are useful in other additive manufacturing techniques such as fused deposition modeling (FDM), selective laser sintering (SLS), and inkjet printing.
[0145] In some embodiments, moiety A comprises acrylate, methacrylate, styrene, acrylic acid, N-vinyl, acryloyl, vinyl amide, vinyl ether, vinyl carbonate, vinyl carbamate, vinyl ester (including derivatives thereof), polymers comprising any one or more of the foregoing, and combinations of two or more of the foregoing (e.g., acrylonitrile, styrene, divinylbenzene, vinyl toluene, methyl acrylate, ethyl acrylate, butyl acrylate, methyl (meth)acrylate, amine (meth)acrylate, and mixtures of any two or more of the foregoing, as described above (see, e.g., U.S. Patent Application Publication No. 20140072806, the entire contents of which are incorporated herein by reference).
[0146] In some embodiments, part B comprises acrylate, methacrylate, styrene, acrylic acid, N-vinyl, vinylamide, acryloyl, vinyl ether, vinyl carbonate, vinyl carbamate, vinyl ester (including derivatives thereof), polymers comprising any one or more of the foregoing, and combinations of two or more of the foregoing (e.g., acrylonitrile, styrene, divinylbenzene, vinyl toluene, methyl acrylate, ethyl acrylate, butyl acrylate, methyl (meth)acrylate, amine (meth)acrylate, and mixtures of any two or more of the foregoing, as described above (see, e.g., U.S. Patent Application Publication No. 20140072806, the entire contents of which are incorporated herein by reference).
[0147] Elastomers. Particularly useful embodiments in the practice of the present invention are directed to the formation of elastomers. Using conventional liquid UV-polymerizable precursors, it is difficult to achieve tough, high-elongation, high-strength elastomers. However, through the formation of IPN networks, elastomers with properties equal to or better than known polyurethanes, silicones, natural rubbers, etc. can be formed under single-reaction mechanism energy polymerization. These single-reaction mechanism energy polymerized elastomers can have elongations of >750% and / or tensile strengths of >20 MPa.
[0148] In some embodiments, as described in more detail above, the single reaction mechanism energetically polymerizable liquid comprises: a) 5 or 20 or 40% to 60 or 80 or 90% by weight of part A; b) 10 or 20% to 30 or 40 or 50 or 60 or 70% by weight of part B; c) 0.1 or 0.2% to 1, 2 or 4 or 8% by weight of photoinitiator; d) optional additional materials, such as dyes, fillers (e.g., silica), surfactants, etc. Because these single reaction mechanism energetically polymerizable liquids do not polymerize upon mixing, an advantage of some embodiments of the invention is that they can be pre-formulated and the filling step can be carried out by pouring or supplying the polymerizable liquid to the build area from a single source (e.g., a single reservoir containing the polymerizable liquid in a pre-mixed form), thus eliminating the need for separate reservoirs or modified equipment to provide mixing capabilities.
[0149] In some embodiments, the three-dimensional object produced by this process is foldable or compressible (i.e., elastic (e.g., having a Young's modulus at room temperature of about 0.001, 0.01, or 0.1 GPa to about 1, 2, or 4 GPa, and / or a tensile strength at maximum load at room temperature of about 0.01, 0.1, or 1 to about 50, 100, or 500 MPa, and / or an elongation at break at room temperature of about 10, 20, 50, or 100% to 1000, 2000, or 5000% or more).
[0150] In some embodiments, after forming an intermediate molded product having polyurethane oligomer as a backbone by the energy polymerization of a single reaction mechanism, the whole material is subjected to another energy polymerization when the IPN of the second component is polymerized. The time required for this energy polymerization varies depending on the energy source, temperature, size, shape and density of the product, but is typically from 1 second to several hours, depending on the specific energy of the single reaction mechanism used and the size of the product.
[0151] Generally, the film or three-dimensional product produced by the single reaction mechanism of the above method includes (i) a linear or semi-crosslinked or fully crosslinked energy polymerized network, (ii) a fully or semi-crosslinked energy polymerized polymer constructed from monomers or oligomers having energy polymerizable functional groups, or (iii) a combination thereof, for example, as an IPN, semi-IPN, simultaneous IPN, sequential IPN, dual network, or a combination thereof. In some embodiments, the film or three-dimensional product may include unreacted photoinitiator remaining in the film or three-dimensional formed object. For example, in some embodiments, 0.1 or 0.2 wt % to 1, 2, or 4 wt % of photoinitiator may remain in the film or three-dimensional formed object, and the photoinitiator may be present in even smaller or trace amounts only. In some embodiments, the film or three-dimensional product may include fragments of the reacted photoinitiator. For example, in some embodiments, the fragments of the reacted photoinitiator may be remnants of the first polymerization that forms the intermediate product. For example, 0.1 or 0.2 wt % to 1, 2 or 4 wt % of the reacted photoinitiator fragments may remain in the film or three-dimensional formed object, and even smaller or only trace amounts of the reacted photoinitiator fragments may be present. In an exemplary embodiment, the film or three-dimensional formed object produced by a single reaction mechanism may include all or any combination of crosslinked or linear energy polymerized networks, different crosslinked energy polymerized networks, unreacted photoinitiator, and reacted photoinitiator materials.
[0152] These materials can be used in bottom-up additive manufacturing techniques such as the continuous liquid interface printing techniques described herein and other additive manufacturing techniques described above and below.
[0153] These materials can be used in inkjet printing manufacturing techniques such as the piezoelectric printing techniques described herein and other inkjet printing techniques described above and below.
[0154] An article composed of an interpenetrating polymer network (IPN) formed from an energetic polymerizable liquid by a single reaction mechanism.
[0155] In some embodiments, single kinetic energetic polymerizable liquids, including single kinetic systems such as those described above, are also useful in forming films and three-dimensional articles, including IPNs.
[0156] In a non-limiting example, the energetic polymerizable liquid and method steps of the single reaction mechanism are selected such that the film or three-dimensional object comprises:
[0157] Sol-gel compositions. This can be done using amine (ammonia) permeable windows or semi-permeable members. In the system described here, tetraethyl orthosilicate (TEOS), epoxy (diglycidyl ether of bisphenol A), and 4-aminopropyltriethoxysilane are added to a free radical crosslinker. During the process, the free radical crosslinker contains the above reactants that polymerize and react in a later separate process or stage. The reaction requires the presence of water and acid. A photoacid generator (PAG) may be added to the above mixture to promote the reaction of the silica-based network. Note that if only TEOS is included, the end result is a silica (glass) network. The temperature is then increased to remove the organic layer, leaving behind a silica structure that is difficult to prepare by traditional methods. This process allows the preparation of many variants (different polymer structures) in addition to epoxies, such as urethanes, functionalized polyols, and silicone rubbers.
[0158] Hydrophobic-hydrophilic IPNs, such as hydrophobic-hydrophilic networks for improving tissue and blood compatibility of biomedical components. Poly(N-vinylpyrrolidone) is an example of a hydrophilic component. Polybutadiene is an example of a hydrophobic component.
[0159] Conductive polymer. To produce the conductive part, aniline and ammonium persulfate are incorporated into the polymerizable liquid with a single reaction mechanism energy. The reaction system polymerizes and can be initiated to polyaniline after post-treatment with acid (e.g. HCl vapor).
[0160] Natural product-based IPNs. Many natural product-based IPNs are known, based on triglyceride oils such as castor oil, or gelatin, or polyvinyl alcohol. These can be incorporated into the energetic polymerizable liquid in a single reaction mechanism. Upon completion of the part, these can form additional IPNs. Glycerol can of course also be used.
[0161] Continuous IPN In some embodiments, the backbone crosslinked network is swollen with monomer and a free radical photoinitiator and an optional crosslinker, and then polymerized.
[0162] Simultaneous IPN: In some embodiments, both networks are formed in a first polymerization step.
[0163] III.Products
[0164] A. Three-dimensional (3D) object
[0165] The three-dimensional object produced by the methods and processes of the present invention may be a final, finished or substantially finished product, or may be an intermediate product that is subjected to further manufacturing steps such as surface treatment, laser cutting, electrical discharge machining, etc. Intermediate products include products that can be further additively manufactured in the same or different equipment. For example, fault lines or secants can be intentionally introduced into an ongoing "build" by disrupting and restoring the slope of the polymerization zone to stop one area of the final product, or simply because certain areas or "builds" of the final product are weaker than others.
[0166] Many different products can be produced by the methods and apparatus of the present invention, including large scale models or prototypes, small custom products, miniature or microminiature products or devices, including, but not limited to, medical devices such as hearing aids, stents, drug delivery depots, functional structures, microneedle arrays, fibers and rods such as waveguides, micromechanical devices, microfluidic devices, and implantable medical devices.
[0167] Thus, in some embodiments, the articles of manufacture may have heights from 0.1 or 1 mm to 10 or 100 mm or more, and / or maximum widths from 0.1 or 1 mm to 10 or 100 mm or more. In other embodiments, the articles of manufacture may have heights from 10 or 100 nm to 10 or 100 μm or more, and / or maximum widths from 10 or 100 nm to 10 or 100 μm or more. These are merely examples. The maximum diameters and maximum widths will vary depending on the particular instrument configuration and light source resolution and may be adjusted depending on the particular purpose of the embodiment or article being manufactured.
[0168] In some embodiments, the height to width ratio of the product is at least 2:1, 10:1, 50:1, or 100:1 or more, and the width to height ratio is 1:1, 10:1, 50:1, or 100:1 or more.
[0169] As described further below, in some embodiments, the article of manufacture has at least one or more holes or grooves formed therein.
[0170] The processes described herein can produce products having a variety of different properties. In some embodiments, the products are rigid, while in other embodiments, the products are flexible and resilient. In some embodiments, the products are solid. In other embodiments, the products are gels, such as hydrogels. In some embodiments, the products have shape memory (i.e., they generally return to their previous shape after deformation unless deformed to the point of structural failure). In some embodiments, the products are unitary (i.e., formed from one single reaction mechanism energy polymerizable liquid). In some embodiments, the products are composite (i.e., formed from two or more different single reaction mechanism energy polymerizable liquids). The particular properties will be determined by factors such as the choice of single reaction mechanism energy polymerizable liquid used.
[0171] In some embodiments, the manufactured product or article produced has at least one protrusion (or "protrusion"), such as a bridging element between two supports, or a cantilever element protruding from one substantially vertical support. The unidirectional and continuous nature of some embodiments of the process significantly reduces the problem of fault or cleavage lines forming between layers when each layer is polymerized substantially complete and a substantial time interval occurs before the next pattern is exposed. Thus, in some embodiments, the method is particularly advantageous for reducing or eliminating the number of such protruding support structures that are manufactured simultaneously with the article.
[0172] B. Examples of 3D object structures and shapes
[0173] In an exemplary embodiment, the three-dimensional object can be imparted with thousands or millions of shape variations during formation to form a three-dimensional (3D) object. In an exemplary embodiment, the pattern generator generates different patterns of light irradiation to activate photoinitiators in the polymerization gradient regions to impart different shapes as the object is obtained from the polymerization gradient. In an exemplary embodiment, the pattern generator can have high resolution with millions of pixel elements that can be changed to change the shape imparted. For example, the pattern generator can be a DLP with more than 1,000, 2,000, or 3,000 or more rows and / or more than 1,000, 2,000, or 3,000 or more columns of micromirrors, or LCD panel pixels that can be used to change the shape. As a result, the object can be imparted with very fine variations or gradations along the length of the object. In an exemplary embodiment, this allows complex three-dimensional objects with substantially continuous surfaces without cleavage lines or seams to be formed at high speed. In some examples, the three-dimensional object formed may be imparted with more than 100, 1000, 10000, 100000, or 1 million shape changes without tear lines or seams over the length of the object formed of more than 1 mm, 1 cm, 10 cm, or more, or over the entire length of the molded object. In exemplary embodiments, objects can be continuously formed from the polymerization gradient at rates of more than 1, 10, 100, 1000, 10000 microns per second or more.
[0174] In exemplary embodiments, this allows complex three-dimensional (3D) objects to be formed. In some exemplary embodiments, the 3D formed object has a complex non-injection moldable shape. This shape may not be easily formed by injection molding or casting. For example, this shape may not be formed by a mold that fits together to form a cavity into which a fill material is injected and polymerized, as in traditional two-part molding. For example, in some embodiments, the 3D formed object may include closed or partially open cavities, repeating unit cells, or open or closed cell foam structures that are not suitable for injection molding, and may include hundreds, thousands, or millions of these structures or interconnected networks of these structures. However, in exemplary embodiments, these shapes may be 3D formed using the methods described herein utilizing a wide range of properties such as a wide range of elastomeric properties, tensile strength, and elongation at break due to the use of dual polymerized materials and / or IPNs to form these structures. In exemplary embodiments, the 3D object may be formed without tear lines, parting lines, seams, sprues, gate marks, or ejector pin marks that may be present in injection molding or other conventional techniques. In some embodiments, the 3D formed object can have a continuous surface texture (smoothness, pattern, or roughness) without moldings or other printed features (such as cleavage lines, parting lines, seams, sprues, gate marks, or ejector pin marks) over 1 mm, 1 cm, 10 cm, or more, or over the entire length of the formed object. In an exemplary embodiment, a complex 3D object can be formed such that there are no discontinuous layers visible in the completed 3D object or easily detectable from the printing process over 1 mm, 1 cm, 10 cm, or more, or over the entire length of the formed object. For example, the printing occurs due to the tilting of the polymerization area (from which the 3D object will be generated when exposed to the various patterns projected from the pattern generator), so that the various shapes imparted by the pattern generator during printing may not be visible or detectable as different layers when the 3D object is completed.The 3D object resulting from this process, which may also be referred to as a 3D printed object, may be formed by continuous liquid interphase printing without the discrete layers and tear lines associated with some 3D printing processes.
[0175] In some embodiments, the 3D formed object may include one or more repeating structural elements to form the 3D object, such as, for example, closed cavities, partially closed cavities, repeating unit cells or networks of unit cells, foam cells, Kelvin foam cells or other open or closed cell foam structures, cross structures, overhanging structures, cantilevers, microneedles, fibers, paddles, protrusions, pins, dimples, rings, tunnels, tubes, shells, panels, beams (including I-beams, U-beams, W-beams, cylindrical beams), struts, ties, channels (open, closed or partially closed), waveguides, triangular structures, tetrahedrons or other pyramidal shapes, cubes, octahedrons, octagonal prisms, icosahedrons, rhomboidal triocahedrons or other polyhedral shapes or modules (including Kelvin minimum surface tetrahedrons, prisms or other polyhedral shapes), pentagons, hexagons, octagons and other polygonal structures or prisms, polygonal meshes or other three dimensional structures. In some embodiments, the 3D formed object may include any combination of these structures, or an interconnected network of these structures. In exemplary embodiments, the structure of all or a portion of the 3D formed object corresponds (or substantially corresponds) to one or more Bravais lattice or unit cell structures, such as cubic (including simple, body-centered, or face-centered), tetragonal (including simple or body-centered), monoclinic (including simple or baso-centered), orthorhombic (including simple, body-centered, face-centered, or baso-centered), rhombohedral, hexagonal, triclinic structures, etc. In exemplary embodiments, the 3D shaped object corresponds (or substantially corresponds) to one or more Bravais lattices or unit cell structures, such as a catenoid, helicoid, gyroid or lysinoid, other Thirty Periodically Minimal Surfaces (TPMS), or other shapes from a related family (or Bonnet family), or a Schwarz P ("Primitive") or Schwarz D ("Diamond"), Schwarz H ("Hexagonal") or Schwarz CLP ("Crossed layers of parallels") surface, an argyle or diamond pattern, a lattice or other pattern or structure.
[0176] In an exemplary embodiment, the pattern generator can be programmed to rapidly change during printing to impart different shapes to the polymerization gradient with high resolution. As a result, any of the above structural elements can be formed with a wide range of dimensions and characteristics, and the above structural elements can be repeated or combined with other structural elements to form a 3D object. In an exemplary embodiment, the 3D formed object can include a single three-dimensional structure, or can include more than 1, 10, 100, 1000, 10000, 100000, 1000000, or more of these structural elements. The structural elements can be repeated structural elements of similar shapes, or can be a combination of different structural elements, and can be any of the above or other regular or irregular shapes. In exemplary embodiments, each of these structural elements may have a structural dimension of at least 10 nm, 100 nm, 10 μm, 100 μm, 1 mm, 1 cm, 10 cm, 50 cm, or more, and may have a structural dimension of less than 50 cm, 10 cm, 1 cm, 1 mm, 100 μm, 10 μm, 100 nm, 10 nm, or less. In exemplary embodiments, the height, width, or other dimension of the structure may be in the range of about 10 nm to about 50 cm or more, or any range encompassed therein. As used herein, "any range encompassed therein" means any range within the stated range. For example, the following ranges: 10 nm to 1 μm, 1 μm to 1 mm, 1 mm to 1 cm, 1 cm to 50 cm, or any other ranges and range groups within the above ranges, are all encompassed within the range of about 10 nm to about 50 cm, and are described herein. In exemplary embodiments, each structural element may have a structural dimension of at least about 10 nm, and may have a structural dimension of less than 50 cm, 10 cm, 1 cm, 1 mm, 100 μm, 10 μm, 100 nm, 10 nm, or less. 3 ~about 50cm 3 In an exemplary embodiment, each structural element may form a 3D object with a volume ranging from about 10 nm to about 50 cm or more, or any range subsumed therein. In an exemplary embodiment, each structural element may form a cavity, or hollow region, or gap between faces of the structural element with a dimension ranging from about 10 nm to about 50 cm or more, or any range subsumed therein, or 3 ~about 50cm 3, or greater, or any range subsumed therein, may be defined within the region of the 3D formed object.
[0177] The structural elements may be of similar size, or may vary in size throughout the volume of the 3D formed object, may increase or decrease in size (gradual or stepwise) from one side of the 3D formed object to the other, and elements of different shapes may be intermixed in regular or irregular patterns (e.g., a 3D elastomeric foam with open and / or closed cell cavities of different sizes intermixed in the foam).
[0178] In some embodiments, the 3D formed object may have an irregular shape with protrusions, bridging elements, or asymmetry, or may have an offset center of gravity in the direction in which it is formed. For example, the 3D formed object may be asymmetric. In an exemplary embodiment, the 3D formed object may not have rotational symmetry on any axis, but only on a single axis. In an exemplary embodiment, the 3D formed object may not have plane symmetry on any plane through the 3D formed object, but only on a single plane. In an exemplary embodiment, the 3D object may have an offset center of gravity. For example, the center of gravity of the 3D formed object may not be at the location center of the object. In some examples, the center of gravity may not be located along the central axis of the object. For example, the 3D formed object may be a shoe sole or insole that generally follows the contour of a foot. The shoe sole or insole may be tilted to the right or left and have different widths at the heel and toe. As a result, the 3D formed object in this example is not plane symmetric left-right and front-back. However, a uniformly flat shoe sole or insole may be symmetrical from top to bottom. In another example, a shoe sole or insole may be flat on one side and contoured to accommodate the arch of the foot on the other side, resulting in no symmetrical top to bottom. Other 3D formed objects for shapes or devices for wearables, prosthetics, or body structures may have similar asymmetries and / or offset centers of gravity. For example, a 3D formed object for a dental mold or dental implant may substantially match the shape of a tooth and may not be symmetrical on any side. Another example is a 3D molded component for soft robotics, such as a grip, handle, or internally pressurized material that may contact an object to pick it up, lift, or move it. The elastomeric material described in this example may be particularly useful for soft robotics applications. In other examples, 3D molded components for wearable devices such as athletic wear, such as left and right curved shin guards, rigid shin guards, or foam pads or inserts for use between a helmet or other wearable component and the body, may closely conform to the shape of the body and have corresponding asymmetries. These are merely examples, and many 3D molded objects may be asymmetric or have an offset center of gravity.In exemplary embodiments, if there is significant asymmetry or protruding elements (such as arms, bridge elements, cantilevers, brush fibers, etc.) or if the desired structural elements are elastomeric, they may deform during 3D printing or subsequent polymerization. For example, if a large amount of non-UV polymerizable elastomeric resin material is included, gravity may cause deformation before final polymerization. Some elastomeric compositions with highly asymmetric or protruding shapes may be prone to deformation while the scaffold formed by the UV polymerizable material during 3D printing (from the first polymerization in the dual polymerization process) helps to fix the shape. In some embodiments, the UV polymerizable material in the composition may be adjusted to form a stronger scaffold to avoid deformation. In other exemplary embodiments, objects with asymmetric shapes and / or offset centers of gravity may be formed in pairs (or other combinations) with connectors that are later removed, especially when the 3D formed objects or protruding elements are relatively long. In one example, an elastomeric 3D object may be formed along its length, may have asymmetric, offset center of gravity, and / or may have protruding elements that are transverse to its length and are greater than 10%, 20%, 30%, 40%, 50%, or more of its length. For example, a 3D formed object may have a length of about 1 cm to 50 cm, or more, or any range therein, and may have lateral or side asymmetric or protruding elements of about 1 cm to 50 cm, or more, or any range therein. In an exemplary embodiment, two or more of these objects may be formed together to provide support for the transverse or protruding elements until the elastomeric material is polymerized to separate the objects. For example, two shoe soles (e.g., rotated and inverted shoe soles formed together with a small removable connector between them) may be formed in pairs such that the shoe soles support each other during formation (when formed along its length). In other embodiments, other supports may be formed and removed after polymerization of the elastomeric material.
[0179] C. Example Materials and Compositions of 3D Objects
[0180] In exemplary embodiments, the 3D formed object produced by the single reaction mechanism may have any of the above shapes or structures, for example, an IPN, semi-IPN, simultaneous IPN, or sequential IPN, or a combination thereof, which may comprise, consist of, or consist essentially of (i) a linear, semi-, or fully crosslinked energy-polymerized network, (ii) a fully or semi-crosslinked energy-polymerized polymer constructed from monomers or oligomers containing energy-polymerizable functional groups, or (iii) a combination thereof, and / or (iv) a photoinitiator, such as unreacted photoinitiator and / or reacted photoinitiator fragments.
[0181] In some exemplary embodiments, the 3D formed object may include sol-gel compositions, hydrophobic or hydrophilic compositions, phenolic resoles, cyanate esters, polyimides, conductive polymers, natural product-based IPNs, sequential IPNs, simultaneous IPNs, and polyolefins, as described above.
[0182] In exemplary embodiments, the 3D formed object may have any of the shapes or structures described above, and may include, consist of, or consist essentially of different materials with different tensile strengths or other different properties in different regions of the 3D formed object. In exemplary embodiments, the different materials may be selected from any of the above. In some exemplary embodiments, the manufacturing process of the product may be stopped or interrupted one or more times to change the single-reaction mechanism energetic polymerizable liquid. In exemplary embodiments, the 3D formed object may include multiple materials (e.g., thermoplastic or thermosetting polyurethanes, polyureas, or copolymers thereof, or silicone rubbers, or epoxies, or combinations thereof) with different tensile strengths, as described further below. The interruption may create a fault line or plane in the intermediate, but if the later single-reaction mechanism energetic polymerizable liquid is reactive with the first in that second polymerizable material, the two different segments of the intermediate will cross-react during the second polymerization (e.g., by heating or microwave irradiation) and covalently bond to each other. Thus, for example, any of the materials described herein can be sequentially modified to form a product having multiple different segments with different tensile strength properties, yet the product is a single product with the different segments covalently bonded to one another.
[0183] In exemplary embodiments, the above-mentioned photoplastic materials or combinations thereof may comprise a majority of the weight of the 3D formed object, and may constitute more than 50%, 60%, 70%, 80% or 90% by weight of the 3D formed object.
[0184] In exemplary embodiments, the 3D formed object produced by a single reaction mechanism may have any of the above shapes or structures, for example, an IPN, semi-IPN, simultaneous IPN, or sequential IPN, or a combination thereof, which may comprise, consist of, or consist essentially of (i) a linear, semi-crosslinked, or fully crosslinked energy polymerized network, (ii) a fully or semi-crosslinked energy polymerized polymer constructed from monomers or oligomers containing energy polymerizable functional groups, or (iii) a combination thereof, and may constitute a majority of the 3D formed object, or may constitute more than 50%, 60%, 70%, 80%, or 90% by weight of the 3D formed object.
[0185] In some embodiments, the 3D formed object may include sol-gel compositions, hydrophobic or hydrophilic compositions, phenolic resoles, cyanate esters, polyimides, conductive polymers, natural product-based IPNs, continuous IPNs, and polyolefins as described above.
[0186] D. Examples of film materials
[0187] Any material that is applied to a substrate by flexography, lithography, gravure, offset, spray coating, roll coating, curtain coating, inkjet deposition, stamping, brush.
[0188] These films can come in a variety of sizes. The American Society for Testing and Materials (ASTM) defines a film as a plastic sheet that is 0.25 mm thick or less. Sheet material that is thicker than 0.25 mm is considered sheet. Sheet extrusion produces materials for use in most thermoforming operations. However, anything over 0.25 mm can be considered a film as long as it is permanently attached to a substrate.
[0189] Examples of photoinitiators and photoinitiator fragments. In some embodiments, the film or 3D formed object may include unreacted photoinitiator remaining in the film or 3D formed object. For example, in some embodiments, 0.1 or 0.2% to 1, 2, or 4% by weight of photoinitiator may remain in the film or 3D formed object, or the photoinitiator may be present in lesser or trace amounts only. In some embodiments, the film or 3D formed object may include reacted photoinitiator fragments. For example, in some embodiments, the reacted photoinitiator fragments may be residues of a first polymerization that forms an intermediate product. For example, 0.1 or 0.2% to 1, 2, or 4% by weight of reacted photoinitiator fragments may remain in the film or 3D formed object, or the reacted photoinitiator fragments may be present in lesser or trace amounts only.
[0190] In an exemplary embodiment, since the system is composed, in part, of monomers and oligomers polymerizable by exposure to UV light, the final product may contain residual photoinitiator molecules and photoinitiator fragments.
[0191] In some embodiments, photopolymerization involves the chemical changes described below. In the first step, initiation, UV light cleaves the initiator into active radical fragments. These active radical fragments then react with the "M" group of the monomer. In the propagation stage, the active monomer reacts with additional monomers that add to the growing polymer chain. Finally, termination occurs by either recombination or disproportionation.
[0192] start
[0193] Initiator + h v →R'
[0194] R'+M→RM'
[0195] growth
[0196] RM'+M n→RM' n+1
[0197] Stop
[0198] join
[0199] RM' n +'M m R → RM n M m R
[0200] Disproportionation
[0201] RM' n +'M m R → RM n +M m R
[0202] In an exemplary embodiment, a 3D formed object produced by the processes described herein may include the following chemicals after the object is formed:
[0203] Latent unreacted photoinitiator. Photoinitiators are rarely 100% consumed in photopolymerization. Because of this, products typically contain unreacted photoinitiator incorporated throughout the solid object.
[0204] A by-product photoinitiator that is covalently attached to the polymer network. In an exemplary embodiment, the photoinitiator can include:
[0205] Benzoyl chromophore based: these systems take the form:
[0206] [ka]
[0207] where "R" is any number of elements such as H, O, C, N, S, etc. These initiators cleave to form:
[0208] [ka]
[0209] where "." represents a free radical. Any of these components can initiate polymerization and thus become covalently bonded to the polymer network.
[0210] [ka]
[0211] Examples of such initiators are given below.
[0212] [ka]
[0213] Morpholinos and aminoketones. These systems take the form:
[0214] [ka]
[0215] where "R" is any number of elements such as H, O, C, N, S, etc. These initiators cleave to form:
[0216] [ka]
[0217] where "." represents a free radical. Any of these components can initiate polymerization and thus become covalently bonded to the polymer network.
[0218] [ka]
[0219] Examples of such initiators are given below. [ka]
[0220] Benzoylphosphine oxide. These systems take the form:
[0221] [ka]
[0222] where "R" is any number of elements such as H, O, C, N, S, etc. These initiators cleave to form:
[0223] [ka]
[0224] where "." represents a free radical. Any of these components can initiate polymerization and thus become covalently bonded to the polymer network.
[0225] [ka]
[0226] Examples of such initiators are given below.
[0227] [ka]
[0228] Amines. Many photoinitiators can be used in combination with amines. Here, the photoinitiator in an excited state serves to abstract a hydrogen atom from the amine, thereby generating an active radical. This radical can then initiate polymerization and thus become incorporated into the polymer network that is formed. This process is shown below:
[0229] [ka]
[0230] Any of these active species can then form an active polymer chain, resulting in the following structure:
[0231] [ka]
[0232] Other Systems: Other classes of photoinitiators that can be used to generate such materials and generate fragments that are covalently attached to the polymer network that is formed include triazines, ketones, peroxides, diketones, azides, azo derivatives, disulfide derivatives, disilane derivatives, thiol derivatives, diselenide derivatives, diphenyl ditelluride derivatives, digermane derivatives, distannane derivatives, carbon-germanium compounds, carbon-silicon derivatives, sulfur-carbon derivatives, sulfur-silicon derivatives, peresters, Barton ester derivatives, hydroxamic and thiohydroxamic acids and esters, organic borates, organometallic compounds, titanocenes, chromium complexes, alumate complexes, carbon-sulfur or sulfur-sulfur iniferter compounds, oxyamines, aldehydes, acetals, silanes, phosphorus-containing compounds, borane complexes, thioxanthone derivatives, coumarins, anthraquinones, fluorenones, ferrocenium salts. These photoinitiators may also be oligomeric or polymeric in that they are attached to larger molecules to reduce the mobility, hazard, etc. of the initiator species.
[0233] Detection. Detection of the unique chemical signature of the photoinitiator fragments in the polymerized polymeric mass can be accomplished by a number of spectroscopic techniques. Specific techniques that are useful, either alone or in combination, include UV-Vis spectroscopy, fluorescence spectroscopy, infrared spectroscopy, nuclear magnetic resonance spectroscopy, mass spectrometry, atomic absorption spectroscopy, Raman spectroscopy, and X-ray photoelectron spectroscopy.
[0234] E. Examples of 3D object characteristics
[0235] The structural properties of the 3D formed object can be selected along with the properties of the materials that form the 3D object and provide a wide range of properties for the 3D object. Complex shapes with desired material properties can be formed using the materials and methods described above in this application to form a wide range of 3D objects.
[0236] In some embodiments, the 3D formed object may be rigid, for example having a Young's modulus (MPa) in the range of about 800-4500 or any range therein, a tensile strength (MPa) in the range of about 30-150 or any range therein, an elongation at break (%) in the range of about 1-100 or any range therein, and / or an IZOD impact strength with notch geometry in the range of 10-200 J / m or any range therein. Non-limiting examples of such rigid 3D formed objects may include fasteners; electronics housings; gears, propellers, and impellers; wheels, machinery housings; tools, and other rigid 3D objects.
[0237] In some embodiments, the 3D formed object may be semi-rigid, for example having a Young's modulus (MPa) in the range of about 300-3500 or any range therein, a tensile strength (MPa) in the range of about 20-90 or any range therein, an elongation at break (%) in the range of about 20-300 or 600 or any range therein, and / or an IZOD impact strength with notch geometry in the range of about 30-400 J / m or any range therein. Non-limiting examples of such semi-rigid 3D formed objects can include structural elements; hinges, such as living hinges; boat and ship hulls and decks; wheels; bottles, jars, and other containers; pipes, liquid tubes and connectors, and other semi-rigid 3D objects.
[0238] In some embodiments, the 3D shaped object may be elastomeric, e.g., having a Young's modulus (MPa) in the range of about 0.25-300 or any range therein, a tensile strength (MPa) in the range of about 0.5-30 or any range therein, a breaking elongation (%) in the range of about 50-1500 or any range therein, and / or a tear strength in the range of about 10-200 kN / m or any range therein. Non-limiting examples of such elastomeric 3D shaped objects may include footwear soles, heels, innersoles, midsoles; bushings and gaskets; soft robotics components; cushioning; electronics housings, and other elastomeric 3D objects. EXAMPLES
[0239] Examples 1-3 below provide comparative exemplary materials for the formation of products having a variety of different tensile properties ranging from elastomeric to semi-rigid to flexible as described above, with all tensile data measured according to ASTM D638, Type 4 specimens. These examples are shown in Figures 1A and 1B along with all known, commercially available, single kinetic energy polymerizable materials.
[0240] [Table 1]
[0241] [Table 2]
[0242] [Table 3]
[0243] A further example of the use of energetic polymerizable liquids with a single reaction mechanism to produce photoplastics.
[0244] [Table 4]
[0245] [Table 5]
[0246] [Table 6]
[0247] [Table 7]
[0248] [Table 8]
[0249] Although 1-vinyl-2-pyrrolidone and N-vinylcaprolactam are shown in the examples above, many other monomers can be used with desirable results, including but not limited to N-vinylformamide, acryloylmorpholine, or vinyl cinnamate.
[0250] <Example #5 Calculation of molar bond ratio>
[0251]
number
[0252] First, the number of moles of each ingredient in a given mass or volume of material is determined.
[0253]
number
[0254] The moles of each component multiplied by its functionality gives the number of moles of each binding species in the composition.
[0255]
number
[0256] Dividing the total moles of bonds contributed by monofunctional species by the total moles of bonds contributed by multifunctional species gives the molar bond ratio.
[0257]
number
[0258] Calculation of Molar Bond Numbers. Exemplary calculations of the molar bond ratios for Examples #4-#8 are shown below.
[0259] [Table 9]
[0260] [Table 10]
[0261] [Table 11]
[0262] [Table 12]
[0263] [Table 13]
[0264] In Example #8, the molar bond ratio of monofunctional to polyfunctional species is at least 1000% (molar bond ratio of monofunctional to polyfunctional species is 10:1 or more).
[0265] In Example #7, the molar bond ratio of monofunctional to polyfunctional species is at least 3000% (the molar bond ratio of monofunctional to polyfunctional species is 30:1 or greater).
[0266] Molar Bond Ratio. Molar bond ratio is the ratio of the number of functional groups contributed by a single different molecular species to the number of functional groups (sites available for reaction / polymerization) contributed by different molecular species in a closed system. It is the relative ratio between the different molecules and takes into account their relative weight % in the composition, molecular weight, and functionality (number of functional groups per molecule).
[0267] Molar Bond Ratio. One particularly useful definition of molar bond ratio used to characterize photoplastic materials compares the number of functional groups contributed to the composition: the sum of monofunctional reactive species to the sum of polyfunctional reactive species. The molar bond ratio is the ratio of the number of functional groups contributed by monofunctional species to the number of functional groups (sites available for reaction / polymerization) contributed by polyfunctional species in a closed system. This is the relative ratio of different monofunctional and polyfunctional species, taking into account their relative weight % in the composition, molecular weight, and functionality (number of functional groups per molecule). Monofunctional species are defined as molecules that contain one functional group that will form a covalent bond in the fully polymerized material. Polyfunctional species are defined as molecules that contain more than one functional group that will form a covalent bond in the fully polymerized material. For a given system, the molar bond ratio is calculated only for those functional groups that will become covalent bonds when the material is polymerized. For example, if a monomer contains one acrylate group and one epoxide group in a 100% free radical polymerization reaction, and only the acrylate group reacts, the monomer is considered to be monofunctional. If the same molecule is considered, but the material is polymerized using both free radical and cationic polymerization methods, the monomer is considered to have two functional groups since both the acrylate and epoxide groups form covalent bonds in the final polymer structure, and therefore the system is considered to be multifunctional. Molar bond ratio is also one way to consider the crosslink density of a polymeric material.
[0268] The crosslink density of a polymeric material greatly influences its final physical and mechanical properties. In general, highly crosslinked polymers exhibit weaker mechanical behavior than polymers with lower crosslink density. Crosslink density is a useful physical property that can be used as an alternative to characterize a material as a photoplastic.
[0269] The production of the product may be stopped or interrupted one or more times to modify the single-reaction mechanism energetic polymerizable liquid. In an exemplary embodiment, the 3D formed object includes multiple materials with different tensile strengths. The interruption may cause a fault line or plane to form in the intermediate, but if the next single-reaction mechanism energetic polymerizable liquid is reactive with the first in that second polymerizable material, then the two different segments of the intermediate cross-react (e.g., by heat or microwave irradiation) during the second polymerization and covalently bond to each other. Thus, for example, any of the materials described herein can be sequentially modified to form a single product with different segments covalently bonded to each other, but with multiple different segments with different tensile strengths. In some embodiments, the 3D object can be formed from multiple regions with different materials and properties. For example, the 3D formed object may have one or more regions formed from a first material or a first group of one or more materials having a tensile strength (MPa) in the range of about 30-100 or any range encompassed herein, and / or one or more regions formed from a second material or a second group of one or more materials having a tensile strength (MPa) in the range of about 20-70 or any range encompassed herein, and / or one or more regions formed from a third material or a third group of one or more materials having a tensile strength (MPa) in the range of about 0.5-30 or any range encompassed herein, or any combination thereof. For example, the 3D object may have 1-10 or more (or any range encompassed herein) different regions having different tensile strengths selected from any of the materials and tensile strengths listed above. For example, a hinge may be formed, and the hinge may include a rigid segment, a second elastic segment coupled thereto, and a third rigid segment coupled thereto, by sequentially changing the energy polymerizable liquid of a single reaction mechanism during the formation of the 3D intermediate. A shock absorber or vibration dampener may be formed in a similar manner, and the second segment may be either elastic or semi-rigid. A single rigid funnel and flexible hose assembly may be formed in a similar manner.
[0270] In some embodiments, a single reaction mechanism energy polymerizable resin can be used to tune the mechanical properties even within the same photoplastic material / object (see FIG. 11). This can be achieved by modifying the energy polymerization of the photoplastic material to change the reactivity or reaction mechanism of the system. For example, the polymerization mechanism and polymerization rate can be changed by changing the light irradiation, light energy, light wavelength, or by using an electron beam. This is due in part to the different polymerizable functional groups contained in the resin and their reactivity or non-reactivity with the same or different functional groups, which can change the molecular weight and network of the final polymer. This is also due in part to the homogeneous initiation that can polymerize all the functional groups in the photoplastic material. By controlling these process parameters, different mechanical properties can be achieved by using one resin to build different chemical structures: full IPN, semi-IPN, pseudo-IPN, dual network, and random copolymer, each of which in turn has different mechanical properties. In addition, the ability to achieve different mechanical properties can be optimized by selecting specific stoichiometric ratios of the components. 4 mJ / cm per layer 2 3D print specimens 1, 2, 4, and 5 with a layer thickness of 100 μm using a 395 nm LED. 25 mJ / cm per layer. 2 3D print specimens 6 and 7 with a 100 μm layer thickness using a 395 nm LED. All specimens are 3D printed with a 5 J / cm 2 The samples are post-cured with a broad spectrum mercury lamp. Differences in the mechanical properties are observed, with Young's modulus varying from 10 MPa to 70 MPa for the different print conditions. This represents a seven-fold difference in Young's modulus. Additionally, the elongation appears to differ by approximately 10-20%. Finally, the Shore D for the first group of samples is ~15, while the Shore D for the second group of samples is ~40. All specimens have the same composition as Example 8 above.
[0271] Furthermore, the various polymer networks, molecular weights, liquid-solid, solid-solid solubility or phase separation of the above structures can be tuned and controlled by the above process parameters. This allows for significant changes in the mechanical properties of one resin, either on a pixel-by-pixel basis in a film or on a voxel-by-voxel basis in an object. Specifically, in additive manufacturing, VAT polymerization typically occurs with a laser in a projector or screen light source. These and next-generation light sources can be controlled to emit lower wattage or lower energy on a pixel-by-pixel basis. This allows for three-dimensional control of voxel polymerization, allowing for objects with different mechanical properties in three-dimensional space. This greatly expands the capabilities of all additive manufacturing machines for 3D objects.
[0272] The core of SLA and DLP 3D printing methods use bottom-up printing techniques. An equally useful method used for 3D printing is top-down bath printing. Bottom-up and top-down printing each have their own distinct advantages and disadvantages. The quality and success rate of building a part with bottom-up 3D printing is heavily influenced and limited by the green strength of the printed part. Green strength includes the strength, stiffness, and dimensional stability of the 3D printed part in its green state in the 3D printer prior to any additional post-curing methods that result in high conversion of reactive components. If the green strength or mechanical integrity of the 3D printed object overcomes the potential deformation effects of gravity, unwanted adhesion to the resin bath bottom, and other build-up in bottom-up 3D printing systems, the 3D printed object tends to print with high quality and stability. The effect of green strength on print quality in bottom-up systems can be greatly influenced by the geometry of the 3D printed part and the printing conditions. Top-down bath printing techniques reduce the effect of some properties, such as green strength, on the success of the printing process. Top-down bath printing techniques keep the printed part in a bath of constituent liquid material during printing, which acts as a buffer against gravity to the printed part. Thus, the printed part may exhibit a "floating" behavior due to the comparable density of the printed part and the surrounding fluid. The floating ability of the printed part in the resin layer reduces the resultant force applied from gravity to the part during printing, especially when the green strength is low and / or the adhesion of the interlayer is low in the green state. Also, the viscosity of top-down bath resins may impart undesirable forces to the green part during printing, resulting in deformation and the introduction of defects. To reduce the risk of deformation due to solid-liquid interactions, low viscosity resins of 750 cP or less are desirable. One potential advantage of photoplastics in top-down printing techniques is that they can be formulated to low viscosity. Photoplastic materials can have low green strength, which suggests that top-down bath printing is a more suitable method than bottom-up printing.
[0273] F. Example of adding 3D objects
[0274] The above methods, structures, materials, compositions, and properties can be used to 3D print a virtually limitless number of manufactured articles, including, but not limited to, medical devices and implantable medical devices such as stents, drug delivery systems, catheters, bladders, breast implants, testicular implants, pectoral implants, eye implants, contact lenses, dental aligners, microfluidics, seals, shrouds, and other applications requiring biocompatibility, functional structures, microneedle arrays, fibers, rods, waveguides, micromechanical devices, microfluidic devices, fasteners, electronic device housings, gears, propellers, impellers, wheels, mechanical device housings, tools, structural members, hinges including living hinges, boats, ship hulls and decks, wheels, bottles, jars, and other containers, pipes, fluid lines and connectors, soles, heels, inner soles, and midsoles of footwear, boots, etc. 3D objects such as ... Any of the above structures, materials, and properties can be combined to form a 3D object, such as the 3D formed object described above.These are merely examples, and many other 3D objects can be formed using the methods and materials described herein.
[0275] IV. ALTERNATIVE METHODS AND APPARATUS
[0276] Although the present invention is preferably practiced by stereolithography, material jetting, or inkjet printing, as described in detail above and in more detail below, in some embodiments, other methods and apparatus for bottom-up or top-down 3D manufacturing may be used, such as layer-by-layer manufacturing, including, but not limited to, those described in U.S. Pat. Nos. 5,236,637, 5,391,072, 5,529,473, 7,438,846, 7,892,474, 8,110,135, U.S. Patent Application Publication Nos. 2013 / 0292862 and 2013 / 029521, and International Publication No. WO2015 / 164234, the entire contents of which are incorporated herein by reference.
[0277] The advantages of photoplastic materials are many but can be summarized as follows: The ability to achieve engineered thermoplastic properties and performance with energy polymerizable materials. Manufacturing techniques where the use of thermoplastics is severely limited by the need to melt the thermoplastic and deposit / mold it into the desired shape. Manufacturing techniques using energy polymerizable materials are almost unlimited as long as there is an energy source available for polymerization. These techniques include inkjet printing, 3D printing, molding, lamination, etc.
[0278] The description of the disclosure is merely exemplary in nature and variations that do not depart from the gist of the disclosure are intended to be within the scope of the disclosure. Such variations should not be regarded as a departure from the spirit and scope of the disclosure.
Claims
1. A reactive oligomer, which is at least one of (i) a multifunctional methacrylate oligomer and (ii) a multifunctional acrylate oligomer; and a reactive monofunctional monomer which is at least one of (i) a monofunctional N-vinyl monomer, (ii) a monofunctional vinyl ether monomer, (iii) a monofunctional vinyl ester monomer, (iv) a monofunctional vinyl amide monomer, (v) a styrene monomer, (vi) a monofunctional acrylamide monomer, (vii) a monofunctional (meth)acrylate monomer, (viii) a cyanoacrylate monomer, (ix) a monofunctional vinyl carbonate monomer, (x) a monofunctional acryloyl monomer, and (xi) a monofunctional vinyl carbamate monomer; A free radical polymerizable liquid for forming three-dimensional objects comprising: a molar bond ratio of reactive ethylenically unsaturated groups of the reactive monofunctional species to reactive ethylenically unsaturated groups of the reactive multifunctional species of at least 10:1; The free radical polymerizable liquid for forming three-dimensional objects is an energy polymerizable liquid that cures by a single reaction mechanism to form a photoplastic material.
2. 10. The polymerizable liquid of claim 1, further comprising about 0.01% to about 15% by weight of a photoinitiator.
3. 2) tensile strength (MPa) = 4500 / (elongation - 25) - 5 (when elongation is about 95% to about 500%).
4. 2) tensile strength (MPa) = 2000 / (elongation + 10) - 3 (when elongation is about 105% to about 550%); 3) tensile strength (MPa) = 0.5 (when elongation is more than about 550%).
5. 10. The polymerizable liquid of claim 1, wherein the polymerized material assumes predetermined mechanical properties without the input of heat.
6. 10. The polymerizable liquid of claim 1, further comprising at least one of a non-reactive light absorbing pigment, a filler, a polymerization inhibitor, and a polymerization catalyst in an amount of about 0.001% to about 10% by weight.
7. 10. The polymerizable liquid of claim 1, further comprising a non-reactive light absorbing pigment in an amount of about 0.001% to about 10% by weight, and a filler.
8. 10. The polymerizable liquid of claim 1, wherein said oligomer and said monomer react by the same polymerization mechanism but have different reaction rates.
9. 10. The polymerizable liquid of claim 1, wherein the solubility of the monomer and oligomer changes during polymerization, thereby favoring homopolymerization of either the monomer or oligomeric species.
10. 10. The polymerizable liquid of claim 1, wherein upon polymerization a material having multiple glass transition temperatures is produced.
11. 10. The polymerizable liquid of claim 1, wherein the polymerization produces a material having two different glass transition temperatures that differ by at least 60 degrees Celsius.
12. 10. The polymerizable liquid of claim 1, wherein the molar combination ratio of reactive ethylenically unsaturated groups of the reactive monofunctional species to reactive ethylenically unsaturated groups of the reactive multifunctional species is at least 25:
1.
13. 13. The polymerizable liquid of claim 12, wherein the molar combination ratio of reactive ethylenically unsaturated groups of the reactive monofunctional species to reactive ethylenically unsaturated groups of the reactive multifunctional species is at least 30:
1.
14. The polymerizable liquid of claim 1 which forms a print on a substrate.
15. 10. The polymerizable liquid of claim 1 that is cured to form a film or three-dimensional object by stereolithography (SLA), digital light projection (DLP), material jetting, or inkjet printing.
16. 16. The polymerizable liquid of claim 15, wherein the inkjet film or 3D printed layer has a thickness greater than about 30 μm.
17. 10. The polymerizable liquid of claim 1, having mechanical properties upon curing that are tunable by varying the energy polymerization conditions.
18. 10. The polymerizable liquid of claim 1 which is non-toxic.
19. 10. The polymerizable liquid of claim 1 , wherein the oligomer has a molecular weight greater than about 1500 g / mole.
20. 20. The polymerizable liquid of claim 19, wherein the oligomer has a molecular weight greater than about 4000 g / mole.
21. 2. The polymerizable liquid of claim 1, wherein the monomer is a monofunctional N-vinyl, vinyl ester, or acryloyl selected from the group consisting of N-vinylpyrrolidone, N-vinylcaprolactam, N-vinylformamide, acryloylmorpholine, or vinylcinnamate.
22. a reactive oligomer which is at least one of: (i) an N-vinyl oligomer having one or more functionalities, (ii) a vinyl ether oligomer having one or more functionalities, (iii) a vinyl ester oligomer having one or more functionalities, (iv) a vinyl amide oligomer having one or more functionalities, (v) a styrene oligomer, (vi) an acrylamide oligomer having one or more functionalities, (vii) a (meth)acrylate oligomer having one or more functionalities that has a different reaction rate than the (meth)acrylate monomer having one or more functionalities, (viii) a cyanoacrylate oligomer, (ix) a vinyl carbonate oligomer having one or more functionalities, and (x) an acryloyl oligomer having one or more functionalities, (xi) a vinyl carbamate oligomer having one or more functionalities; (i) one or more functional N-vinyl monomers, (ii) one or more functional vinyl ether monomers, (iii) one or more functional vinyl ester monomers, (iv) one or more functional vinyl amide monomers, (v) styrene monomers, (vi) one or more functional acrylamide monomers, (vii) one or more functional (meth)acrylate monomers having a different reaction rate than the one or more functional (meth)acrylate oligomers, (viii) cyanoacrylate monomers, (ix) one or more functional vinyl carbonate monomers, (x) one or more functional acryloyl monomers, and (xi) one or more functional vinyl carbamate monomers; 1. A method of forming a polymerizable liquid comprising mixing together A method for forming a polymerizable liquid, wherein the polymerizable liquid is an energy polymerizable liquid capable of being cured by a single reaction mechanism to form a photoplastic material.
23. 23. The method of claim 22, wherein the polymerizable liquid is cured to produce a film or three dimensional object by stereolithography (SLA), digital light / projection (DLP), material jetting (inkjet printing in 3D), or inkjet printing.
24. 24. The method of claim 23, wherein the film or three-dimensional object is a medical device, or a part of footwear, or a part of soft robotics.
25. 24. The method of claim 23, wherein the film or three-dimensional object is a hydrogel.
26. 22. The method of claim 21, wherein pixel or voxel polymerization is used to obtain different physical properties by varying the energy polymerization conditions.
27. 23. The method of claim 22, further comprising irradiating the polymerizable liquid with patterned radiation.
28. The method of claim 22 further comprising mixing a photoinitiator in an amount of about 0.01% to about 15% by weight.
29. 1. An article comprising an energy-polymerizable liquid that hardens by a single reaction mechanism to form a photoplastic material, comprising: The energetically polymerizable liquid is a reactive oligomer which is at least one of: (i) an N-vinyl oligomer having one or more functionalities, (ii) a vinyl ether oligomer having one or more functionalities, (iii) a vinyl ester oligomer having one or more functionalities, (iv) a vinyl amide oligomer having one or more functionalities, (v) a styrene oligomer, (vi) an acrylamide oligomer having one or more functionalities, (vii) a (meth)acrylate oligomer having one or more functionalities that has a different reaction rate than the (meth)acrylate monomer having one or more functionalities, (viii) a cyanoacrylate oligomer, (ix) a vinyl carbonate oligomer having one or more functionalities, and (x) an acryloyl oligomer having one or more functionalities, (xi) a vinyl carbamate oligomer having one or more functionalities; (i) one or more functional N-vinyl monomers, (ii) one or more functional vinyl ether monomers, (iii) one or more functional vinyl ester monomers, (iv) one or more functional vinyl amide monomers, (v) styrene monomers, (vi) one or more functional acrylamide monomers, (vii) one or more functional (meth)acrylate monomers having a different reaction rate than the one or more functional (meth)acrylate oligomers, (viii) cyanoacrylate monomers, (ix) one or more functional vinyl carbonate monomers, (x) one or more functional acryloyl monomers, and (xi) one or more functional vinyl carbamate monomers; An article made from
30. 30. The article of claim 29, wherein the polymerizable liquid upon curing has mechanical properties that are tunable by varying the energy polymerization conditions.