Current-voltage nonlinear resistor and manufacturing method thereof

A current-voltage nonlinear resistor with a specific composition and manufacturing process enhances energy withstand capacity and enables miniaturization by using zinc oxide and controlled particle sizes of additives, resulting in improved performance and compact design.

JP2024157203APending Publication Date: 2024-11-07KK TOSHIBA +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023071408
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Current current-voltage nonlinear resistors face challenges in improving energy withstand capacity and achieving miniaturization.

Method used

A current-voltage nonlinear resistor composition comprising zinc oxide as the main component, with specific ratios and particle sizes of antimony oxide, cobalt oxide, nickel oxide, bismuth oxide, manganese oxide, and other additives, along with controlled median diameters, is sintered to form a sintered body with an insulating layer and electrodes, enhancing energy withstand capacity and allowing miniaturization.

Benefits of technology

The described composition and manufacturing process result in a nonlinear resistor with improved energy withstand capacity and potential for miniaturization, achieving higher performance and compact size.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157203000001_ABST
    Figure 2024157203000001_ABST
Patent Text Reader

Abstract

To provide a current-voltage nonlinear resistor and the like, capable of easily improving performance such as energy toleration.SOLUTION: A current-voltage nonlinear resistor according to one embodiment includes a sintered compact of a mixture that contains a primary component raw material (zinc oxide), a first subcomponent raw material (antimony oxide, cobalt oxide, nickel oxide), a second subcomponent raw material (bismuth oxide, manganese oxide), and a third subcomponent raw material (substances containing a trivalent element, substances containing a boron element, substances containing a silver element). In the primary component raw material, a content [ZnOs] of first primary component powder that has a median diameter D50(ZnOs) satisfying D50(ZnOs)≤0.4 μm, and a content [ZnOt] of second primary component powder that has a median diameter D50(ZnOt) satisfying 0.5 μm≤D50(ZnOt)≤0.7 μm satisfy "0.005≤[ZnOs] / [ZnOt]≤0.1". A median diameter D50(Sb+Co+Ni) of the first subcomponent raw material satisfies "D50(Sb+Co+Ni)≤0.4 μm".SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] SUMMARY OF THE DISCLOSURE The present invention relates to a current-voltage nonlinear resistor and a method for making the same. [Background technology]

[0002] Overvoltage protection devices (lightning arresters, surge absorbers, etc.) are used to protect facilities such as power systems and electronic devices from abnormal voltages (surges) caused by lightning strikes. Overvoltage protection devices are equipped with a current-voltage nonlinear resistor. A current-voltage nonlinear resistor exhibits insulating properties when a normal voltage is applied, but when an abnormal voltage is applied, its resistance value drops and it exhibits conductivity.

[0003] The current-voltage nonlinear resistor comprises a sintered body (ceramic body). The sintered body is formed, for example, by sintering a mixture of a main component raw material made of zinc oxide powder and a subcomponent raw material made of powder of a metal oxide other than zinc oxide. In the current-voltage nonlinear resistor, an insulating layer is formed on the side of the sintered body. The insulating layer is provided to prevent flashover when absorbing an abnormal voltage (surge).

[0004] In recent years, there has been a demand for devices equipped with current-voltage nonlinear resistors to have higher performance and smaller size. Accordingly, current-voltage nonlinear resistors are required to have high resistance and excellent nonlinear resistance characteristics, and various techniques have been proposed to achieve this. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2001-307909 A [Patent Document 2] Patent No. 2904178 [Patent Document 3] Patent No. 2933881 [Patent Document 4] Patent No. 2940486 [Patent Document 5] Patent No. 3165410 [Patent Document 6] Patent No. 6937390 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the past, it was difficult to improve the energy tolerance of current-voltage nonlinear resistors, and it was also difficult to sufficiently achieve miniaturization.

[0007] Therefore, an object of the present invention is to provide a current-voltage nonlinear resistor that can easily achieve improvements in performance such as energy tolerance, and a method for manufacturing the same. [Means for solving the problem]

[0008] The current-voltage nonlinear resistor of the embodiment includes a sintered body formed by sintering a mixture containing a main component raw material made of zinc oxide powder, a first minor component raw material made of antimony oxide, cobalt oxide, and nickel oxide powder, a second minor component raw material made of bismuth oxide and manganese oxide, and a third minor component raw material made of powders of a substance containing a trivalent element in its composition, a substance containing elemental boron in its composition, and a substance containing elemental silver in its composition. The mixture contains 85 mol % or more of the main component raw material. The main component raw material includes a first main component powder and a second main component powder having different particle sizes, and the median diameter D50 of the first main component powder is 1.0 mol %. (ZnOs) satisfies the relationship shown in (Equation A), and the median diameter D50 of the second main component powder (ZnOt) satisfies the relationship shown in (Formula B), and the content of the first main component powder [ZnOs] and the content of the second main component powder [ZnOt] satisfy the relationship shown in (Formula C). Median diameter D50 of the first subcomponent raw material (Sb+Co+Ni) satisfies the relationship shown in (Equation D). D50 (ZnOs) ≦0.4μm (Formula A) 0.5μm≦D50(ZnOt) ≦0.7μm (Formula B) 0.005≦[ZnOs] / [ZnOt]≦0.1 (Formula C) D50 (Sb+Co+Ni) ≦0.4μm (Formula D) [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view showing the configuration of a current-voltage nonlinear resistor 10 according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram showing a method for producing the sintered body 20 (see FIG. 1) of the current-voltage nonlinear resistor 10 of this embodiment. [Diagram 3] FIG. 3 is a diagram showing the relationship between D50(Sb+Co+Ni) and D50(ZnOs) and the fracture energy. [Figure 4] FIG. 4 is a diagram showing the relationship between D50(ZnOt) and fracture energy. [Diagram 5] FIG. 5 is a diagram showing the relationship between [ZnOs] / [ZnOt] and fracture energy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [A] Configuration of current-voltage nonlinear resistor 10 FIG. 1 is a cross-sectional view showing the configuration of a current-voltage nonlinear resistor 10 according to an embodiment of the present invention.

[0011] As shown in FIG. 1, the current-voltage nonlinear resistor 10 includes a sintered body 20, an insulating layer 30, and electrodes 40.

[0012] In the current-voltage nonlinear resistor 10, the sintered body 20 is, for example, disk-shaped, and is insulating when a normal voltage is applied, and when an abnormal voltage higher than the normal voltage is applied, the resistance value drops and the body becomes conductive. The insulating layer 30 is formed of an insulating material so as to cover the side surface (outer peripheral surface) of the sintered body 20. The electrodes 40 are formed of a conductive material so as to cover the respective flat surfaces located on the upper and lower sides of the sintered body 20.

[0013] Although details will be described later, in this embodiment, the sintered body 20 is formed by sintering a mixture obtained by mixing a main component material and a subcomponent material.

[0014] [A-1] Raw materials [A-1-1] Main component raw material (Zn) The main ingredient is zinc oxide powder.

[0015] The mixture contains 85 mol % or more of the main component raw material. In other words, the amount of the main component raw material converted into ZnO [ZnO] in the mixture satisfies the relationship shown in the following (formula a).

[0016] 85mol%≦[ZnO] (formula a)

[0017] [A-1-2] Sub-component raw materials The minor component raw materials include at least a first minor component raw material, a second minor component raw material, and a third minor component raw material. The mixture may further include a fourth minor component raw material in addition to the above.

[0018] [A-1-2-1] First auxiliary ingredient (Sb, Co, Ni) The first minor component raw material is made of powders of antimony oxide, cobalt oxide, and nickel oxide.

[0019] In the mixture, it is preferable that the amount [Sb2O3] converted into Sb2O3, the amount [Co2O3] converted into Co2O3, and the amount [NiO] converted into NiO of the first minor component raw material satisfy the relationships shown in the following (formula b1), (formula b2), and (formula b3).

[0020] 1.0mol%≦[Sb2O3]≦2.5mol% (formula b1) 0.5mol%≦[Co2O3]≦2.0mol% (formula b2) 2.0mol%≦[NiO]≦4.0mol% (formula b3)

[0021] [A-1-2-1-1] Antimony oxide In the first minor component raw material, antimony oxide forms spinel particles together with zinc oxide, which is the main component raw material, and is a component that suppresses the growth of zinc oxide particles during sintering to make them uniform, and is added to improve the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10. If the content ratio of antimony oxide is smaller than the lower limit of the range shown in (Formula b1), the effect of improving the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10 is not fully exerted, and the energy tolerance of the current-voltage nonlinear resistor 10 may deteriorate. If the content ratio of antimony oxide is larger than the upper limit of the range shown in (Formula b1), the insulating components increase inside the sintered body 20, and the characteristics related to the energy tolerance of the current-voltage nonlinear resistor 10 may deteriorate.

[0022] [A-1-2-1-2] Cobalt oxide In the first minor component raw material, cobalt oxide is a component that dissolves in the spinel particles and is added to improve the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10. If the content of cobalt oxide is less than the lower limit of the range shown in (formula b2), the effect of improving the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10 may not be fully achieved. If the content of cobalt oxide is greater than the upper limit of the range shown in (formula b2), the amount of insulating components increases inside the sintered body 20, and the energy tolerance characteristics of the current-voltage nonlinear resistor 10 may deteriorate.

[0023] [A-1-2-1-3] Nickel oxide In the first minor component raw material, nickel oxide is a component that dissolves in the spinel particles and is added to improve the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10. If the content of nickel oxide is less than the lower limit of the range shown in (Formula b3), the effect of improving the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10 may not be fully achieved. If the content of nickel oxide is greater than the upper limit of the range shown in (Formula b3), the amount of insulating components increases inside the sintered body 20, and the energy tolerance characteristics of the current-voltage nonlinear resistor 10 may deteriorate.

[0024] [A-1-2-2] Second auxiliary component raw material (Bi, Mn) The second minor component raw material is made of bismuth oxide and manganese oxide.

[0025] In the mixture, it is preferable that the amount [Bi2O3] calculated as Bi2O3 and the amount [MnO] calculated as MnO of the second minor component raw material satisfy the relationship shown in the following (formula c1) and (formula c2).

[0026] 0.1mol%≦[Bi2O3]≦0.8mol% (formula c1) 0.1mol%≦[MnO]≦2.0mol% (formula c2) [A-1-2-2-1] Bismuth oxide In the second minor component raw material, bismuth oxide is a component present in the grain boundaries of zinc oxide, which is the main component raw material, and is added to improve the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10. If the content of bismuth oxide is less than the lower limit of the range shown in (Formula c1), the effect of improving the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10 is not fully exerted, and the energy tolerance of the current-voltage nonlinear resistor 10 may deteriorate. If the content of bismuth oxide is greater than the upper limit of the range shown in (Formula c1), the amount of insulating components inside the sintered body 20 increases, and the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10 may deteriorate.

[0027] [A-1-2-2-2] Manganese oxide In the second minor component raw material, manganese oxide is a component that dissolves in the spinel particles and is added to improve the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10. If the manganese oxide content is less than the lower limit of the range shown in (Formula c1), the effect of improving the nonlinear resistance characteristics of the current-voltage nonlinear resistor 10 may not be fully achieved. If the manganese oxide content is greater than the upper limit of the range shown in (Formula c1), the amount of insulating components increases inside the sintered body 20, and the energy tolerance characteristics of the current-voltage nonlinear resistor 10 may deteriorate.

[0028] [A-1-2-3] Third subcomponent raw material (Al, Ga, In, B, Ag) The third minor component raw material is made of powders of a substance containing a trivalent element in its composition, a substance containing boron (B) in its composition, and a substance containing silver (Ag) in its composition.

[0029] [A-1-2-3-1] Substances containing trivalent elements Here, the substance containing a trivalent element in its composition is a substance containing at least one trivalent element selected from aluminum (Al), gallium (Ga), and indium (In) in its composition, and is, for example, a hydroxide.

[0030] In the mixture, the powder of the material containing the third minor component raw material, trivalent elements (aluminum (Al), gallium (Ga), indium (In)) in its composition is Al 3+ The amount converted into [Al 3+ ], Ga 3+ The converted amount [Ga 3+ ], and In 3+ The amount converted into [In 3+ ] preferably satisfies the relationship shown in the following (Formula d1).

[0031] 0.002mol%≦[Al 3+ ]+[Ga 3+ ]+[In 3+ ]≦0.009mol% (formula d1)

[0032] In the third minor component raw material, the substance containing a trivalent element (aluminum (Al), gallium (Ga), indium (In)) in its composition is a component that dissolves in the particles of zinc oxide, which is the main component raw material, and is added to improve the nonlinear resistance characteristics of current-voltage nonlinear resistor 10. However, if the relationship shown in (formula d1) is not satisfied, the nonlinear resistance characteristics of current-voltage nonlinear resistor 10 may deteriorate.

[0033] [A-1-2-3-2] Substances containing boron (B) / substances containing silver (Ag) In the third minor component raw material, the substance containing boron element (B) in its composition is, for example, an oxide (boron oxide), and the substance containing silver element (Ag) in its composition is, for example, an oxide (silver oxide).

[0034] In the mixture, for the powder of the substance containing elemental boron (B), which is the third minor ingredient, the amount [B2O3] converted to B2O3 preferably satisfies the relationship shown in the following formula (d4). And, for the powder of the substance containing elemental silver (Ag), which is the third minor ingredient, the amount [Ag2O] converted to B2O3 preferably satisfies the relationship shown in the following formula (d5).

[0035] 0.002mol%≦[B2O3]≦0.02mol% (formula d4) 0.002mol%≦[Ag2O]≦0.02mol% (formula d5)

[0036] In the third minor component raw material, the substance containing boron (B) in its composition and the substance containing silver (Ag) in its composition are added to improve the nonlinear resistance characteristics and energy withstand capacity of current-voltage nonlinear resistor 10. However, if the relationships shown in (Equation d4) and (Equation d5) are not satisfied, at least one of the nonlinear resistance characteristics and energy withstand capacity of current-voltage nonlinear resistor 10 may deteriorate.

[0037] [A-1-2-4] Fourth Subcomponent Raw Material (R) The fourth minor component raw material is made of powder of a substance containing at least one rare earth element R from among yttrium, europium, erbium, thulium, gadolinium, dysprosium, holmium, and ytterbium in its composition. The substance containing the rare earth element R in its composition is, for example, an oxide.

[0038] In the mixture, it is preferable that the amount [R2O3] of the fourth minor component raw material calculated as R2O3 satisfies the relationship shown in the following (formula e).

[0039] 0.2mol%≦[R2O3]≦0.7mol% (formula e)

[0040] The fourth minor ingredient material is a component that can improve the nonlinear resistance characteristics and energy tolerance of current-voltage nonlinear resistor 10, and can also increase the resistance of current-voltage nonlinear resistor 10. If the content of the fourth minor ingredient material is less than the lower limit of the range shown in (formula e), the resistance of current-voltage nonlinear resistor 10 may not be sufficiently increased. If the content of the fourth minor ingredient material is greater than the upper limit of the range shown in (formula e), the energy tolerance of current-voltage nonlinear resistor 10 may deteriorate.

[0041] [A-2] Median diameter of raw material The median diameter of the raw material before granules are produced will be described below.

[0042] [A-2-1] Median diameter of main component raw material and median diameter of first subcomponent raw material The main ingredient raw material, zinc oxide powder, is composed of two types of powder with different particle sizes. The first main ingredient powder has a median diameter of D50 (ZnOs) satisfies the relationship shown in (Equation A), and the median diameter D50 of the second main component powder (ZnOt) satisfies the relationship shown in (Formula B). The content of the first main component powder [ZnOs] and the content of the second main component powder [ZnOt] satisfy the relationship shown in (Formula C).

[0043] D50 (ZnOs) ≦0.4μm (Formula A) 0.5μm≦D50 (ZnOt) ≦0.7μm (Formula B) 0.005≦[ZnOs] / [ZnOt]≦0.1 (Formula C)

[0044] The first subcomponent raw material, which is made of powder of antimony oxide, cobalt oxide, and nickel oxide, has a median diameter of D50 (Sb+Co+Ni) satisfies the relationship shown in (Equation D).

[0045] D50 (Sb+Co+Ni) ≦0.4μm (Formula D)

[0046] Median diameter D50 (Sb+Co+Ni) is a value measured for a mixture of antimony oxide powder, cobalt oxide powder, and nickel oxide powder, and is not the median diameter of each of the antimony oxide powder, cobalt oxide powder, and nickel oxide powder.

[0047] By satisfying the relationships shown in (Formula A), (Formula B) and (Formula C), the reactivity between the main component raw material and the subcomponent raw material can be improved during firing of the mixture. In addition, by satisfying the relationship shown in (Formula D), the subcomponent raw material can be uniformly dispersed in the main component raw material in the mixture slurry. Therefore, in this embodiment, the sinterability of the mixture is improved and the microstructure of the sintered body is made uniform, thereby increasing the density of the sintered body and reducing the porosity of the sintered body. As a result, a current-voltage nonlinear resistor with excellent energy tolerance can be obtained.

[0048] On the other hand, if the relationship is other than that shown in (Formula A), (Formula B), (Formula C), or (Formula D), the reaction between the main component raw materials and the subcomponent raw materials becomes insufficient, and the sinterability decreases, which may result in a deterioration in the energy tolerance of the current-voltage nonlinear resistor.

[0049] In particular, when the lower limit of the range shown in (Formula B) is exceeded or the upper limit of the range shown in (Formula C) is exceeded, the primary particles in the droplets tend to aggregate when the mixture slurry is granulated. This causes the resulting granules to have a hollow shape, and the density of the outer shell of the granules increases, resulting in a decrease in crushability. As a result, when the granules are filled into a mold and pressure-molded at a predetermined density, the hollow parts of the granules may remain as pores. In addition, the pore size of the triple points formed between the granules becomes coarse, which may increase the porosity of the sintered body and decrease the energy tolerance of the current-voltage nonlinear resistor.

[0050] The lower limit of the median diameter of the first main component material and the first subcomponent material is not particularly limited, but is, for example, about 0.1 μm due to production limitations.

[0051] [A-2-2] Median diameter of second subcomponent raw material The second subcomponent raw material, consisting of powder (mixture) of bismuth oxide and manganese oxide, has a median diameter of D50 (Bi+Mn) It is preferable that the relationship shown in (Formula C) is satisfied.

[0052] 0.5μm≦D50 (Bi+Mn) ≦0.7μm (Formula E)

[0053] Median diameter D50 (Bi+Mn) is a value measured for a mixture of bismuth oxide powder and manganese oxide powder, and the median diameter of each of the bismuth oxide powder and the manganese oxide powder differs.

[0054] By satisfying the relationship shown in (Formula E), the minor component raw material can be dispersed more uniformly in the major component raw material in the mixture slurry.

[0055] On the other hand, if the value is less than the lower limit of the range of formula E, it is not easy to achieve uniform dispersion, and the energy tolerance of the current-voltage nonlinear resistor may decrease. Also, if the value is greater than the upper limit of the range of formula E, the nonlinear resistance characteristics of the current-voltage nonlinear resistor may deteriorate.

[0056] [A-2-3] Median diameter of the fourth subcomponent raw material The fourth subcomponent raw material, which is made of powder of a substance containing a rare earth element R in its composition, has a median diameter of D50 (R) It is preferable that the relationship shown in (Formula D) is satisfied.

[0057] D50 (R) ≦0.4μm (Formula F)

[0058] Median diameter D50 (R) is a value measured for a substance containing the rare earth element R in its composition. When there are multiple types of substances containing the rare earth element R in their composition, the median diameter D50 of each of the multiple types of powder is (R)It is preferable that the relationship shown in (Formula F) is satisfied.

[0059] By satisfying the relationship shown in (Formula F), the minor component raw material can be dispersed more uniformly in the major component raw material in the mixture slurry.

[0060] [A-2-4] Measurement of median diameter The above median diameter is a particle size where the cumulative frequency of the particle size is 50%, and is calculated by measuring the particle size distribution using, for example, a laser diffraction / scattering particle size distribution measuring device. The particle size distribution is measured for a slurry obtained by pulverizing the first main component raw material, the second main component raw material, the first minor component raw material, the second minor component raw material, and the fourth minor component raw material under conditions suitable for the specified particle size.

[0061] [B] Manufacturing method of current-voltage nonlinear resistor 10 A method for producing the current-voltage nonlinear resistor 10 (see FIG. 1) of this embodiment will now be described.

[0062] FIG. 2 is a flow diagram showing a method for producing the sintered body 20 (see FIG. 1) of the current-voltage nonlinear resistor 10 of this embodiment.

[0063] 2, in this embodiment, when producing the sintered body 20, the steps of preparing a mixture (ST10), preparing a slurry (ST20), preparing granules (ST30), preparing a compact (ST40), firing (ST50), and cooling (ST60) are sequentially carried out. Each step will be described in detail in turn.

[0064] [B-1] Preparation of mixture (ST10) In producing the sintered body 20, as shown in FIG. 2, first, a mixture is produced (ST10).

[0065] Here, the mixture is obtained by mixing the main component raw material and the subcomponent raw material in the above-mentioned ratio.

[0066] The main component raw material is made of zinc oxide powder. The minor component raw materials include at least a first minor component raw material, a second minor component raw material, and a third minor component raw material. The first minor component raw material is made of antimony oxide, cobalt oxide, and nickel oxide powder. The second minor component raw material is made of bismuth oxide and manganese oxide. The third minor component raw material is made of powders of a substance containing a trivalent element in its composition, a substance containing boron (B) in its composition, and a substance containing silver (Ag) in its composition.

[0067] In addition to the above, the mixture may further contain a fourth minor component raw material. The fourth minor component raw material is made of powder of a substance containing at least one rare earth element R from among yttrium, europium, erbium, thulium, gadolinium, dysprosium, holmium, and ytterbium in its composition.

[0068] [B-2] Preparation of slurry (ST20) Next, as shown in FIG. 2, slurry is prepared (ST20).

[0069] Here, the mixture prepared above, a solvent, and a binder are charged into a wet grinding device, and the mixture is ground to prepare a slurry.

[0070] Specifically, the mixture, the solvent, and the binder are fed into a wet grinding device so that the content of the mixture is, for example, in the range of 30% by weight to 60% by weight. The solvent is, for example, water, and the binder is, for example, polyvinyl alcohol. After preparing a solution by dissolving the binder in the solvent, the solution is fed into the wet grinding device together with the mixture.

[0071] Then, the particles contained in the slurry are pulverized using a wet pulverization device so that the median diameter of the particles contained in the slurry satisfies the relationships shown in the above-mentioned (Formula A), (Formula B), (Formula C), and (Formula D). It is preferable that the pulverization is further performed so that the median diameter of the particles contained in the slurry satisfies the relationships shown in the above-mentioned (Formula E) and (Formula F).

[0072] The wet grinding device is, for example, a circulation type, and grinding is performed by stirring with a stirring rotor in a vessel containing zirconia beads. Here, the diameter of the zirconia beads is, for example, in the range of 0.05 mm to 0.3 mm. The bead filling rate in the vessel is, for example, in the range of 35% to 95%. The rotation speed of the stirring rotor is, for example, in the range of 500 rpm to 1500 rpm. The circulation flow rate is, for example, in the range of 5 L / min to 50 L / min. The median diameter of the particles contained in the slurry can be arbitrarily adjusted by changing each condition (such as the diameter of the zirconia beads).

[0073] [B-3] Preparation of granules (ST30) Next, as shown in FIG. 2, granules are prepared (ST30).

[0074] Here, the slurry prepared above is sprayed using a sprayer such as a spray dryer to produce granules. In other words, the particles contained in the slurry are linked together to increase their size. The sprayer may be, for example, a rotating disk type or a pressurized nozzle type.

[0075] The granules are prepared so that the median diameter D50_k is in the range of 45 μm to 90 μm (45 μm≦D50_k≦90 μm). The median diameter of the granules is also calculated by measuring the particle size distribution using, for example, a laser diffraction / scattering type particle size distribution measuring device.

[0076] If the median diameter of the granules is less than the lower limit of the specified range, the surface area of ​​the granules will increase, which will cause the flowability of the granules to deteriorate and the number of pores at the triple junctions formed between the granules to increase, which may increase the porosity of the sintered body and reduce the energy withstand capacity of the current-voltage nonlinear resistor. If the median diameter of the granules exceeds the upper limit of the specified range, the size of the pores at the triple junctions formed between the granules will become coarse, which may increase the porosity of the sintered body and reduce the energy withstand capacity of the current-voltage nonlinear resistor.

[0077] [B-4] Preparation of molded body (ST40) Next, as shown in FIG. 2, a molded body is produced (ST40).

[0078] Here, the granules prepared above are molded into a molded body using a molding machine, such as a hydraulic press molding machine, and the molded body is, for example, cylindrical.

[0079] The compact is heated to remove the solvent and binder. The heating conditions are, for example, a heating temperature in the range of 350° C. to 500° C. and a heating time in the range of 1 hour to 3 hours.

[0080] [B-5] Firing (ST50) Next, as shown in FIG. 2, baking is carried out (ST50).

[0081] Here, the molded body produced above is fired. The firing conditions are, for example, a firing temperature in the range of 900°C to 1300°C, and a firing time of, for example, 2 hours or more. The firing is carried out, for example, by using a tunnel-type continuous furnace. The firing is carried out by placing the molded body inside a refractory container made of alumina, mullite, or the like.

[0082] In addition, the heating rate at which the temperature for removing the solvent (first temperature) is increased to the temperature for firing (second temperature) is preferably 25°C / hour or more and 100°C / hour or less, from the viewpoints of temperature uniformity inside the fired object and the firing process lead time.

[0083] [B-6] Cooling (ST60) Next, as shown in FIG. 2, cooling is performed (ST60).

[0084] Here, the sintered compact 20 (see FIG. 1) is obtained by cooling the sintered compact described above. Note that the cooling rate from the sintering temperature (second temperature) is preferably 100° C. / hour or more and 200° C. / hour or less, from the viewpoints of temperature uniformity inside the sintered object and the sintering process lead time.

[0085] [B-7] Formation of insulating layer 30 and electrode 40 As described above, after the sintered body 20 is produced, the insulating layer 30 and the electrodes 40 are formed (see FIG. 1).

[0086] In forming the insulating layer 30, for example, an inorganic insulator such as glass frit, which is an electrical insulating material, is applied or sprayed onto the side surface of the sintered body 20. Then, a heat treatment is performed at a temperature in the range of 300° C. to 500° C. for 1 to 5 hours, thereby forming the insulating layer 30.

[0087] In forming the electrode 40, the upper and lower end faces of the sintered body 20 are polished, and then a conductive layer is formed on the polished surfaces as the electrode 40. The conductive layer is formed by, for example, thermal spraying.

[0088] This results in the manufacture of a current-voltage nonlinear resistor 10 with excellent energy tolerance.

[0089] The order in which the insulating layer 30 and the electrodes 40 are formed is not particularly limited. EXAMPLES

[0090] Examples will be described below with reference to Tables 1 to 4.

[0091] [Table 1]

[0092] [Table 2]

[0093] Tables 1 and 2 are tables for explaining the relationships shown in the above-mentioned (Formula A), (Formula B), (Formula C), and (Formula D). In the "Sample No." column of Tables 1 and 2, samples without an * mark indicate cases where the relationships shown in (Formula A), (Formula B), (Formula C), and (Formula D) are satisfied, and samples with an * mark indicate cases where at least one of the relationships among (Formula A), (Formula B), (Formula C), and (Formula D) is not satisfied. The samples shown in Tables 1 and 2 are D50 (Bi+Mn) is 0.4 μm.

[0094] [Table 3]

[0095] Table 3 is a table for explaining the relationship shown in the above-mentioned (Formula E). In the "Sample No." column of Table 3, samples without an * mark indicate cases where the relationship shown in (Formula E) is satisfied, and samples with an * mark indicate cases where the relationship shown in (Formula E) is not satisfied.

[0096] [Table 4]

[0097] Table 4 is a table for explaining the relationship shown in the above-mentioned (Formula F). In the "Sample No." column of Table 4, samples without an * mark indicate cases where the relationship shown in (Formula F) is satisfied, and samples with an * mark indicate cases where the relationship shown in (Formula F) is not satisfied.

[0098] [1] Sample preparation The procedures for producing the samples shown in Tables 1 to 4 will be explained in order.

[0099] [1-1] Samples No. 1 to 60 [1-1-1] Preparation of mixture (ST10; see Figure 2) In the preparation of samples No. 1 to No. 60, a mixture was first prepared by mixing the main component raw materials and each of the subcomponent raw materials in the ratios shown below.

[0100] (Main ingredient raw material) Zinc oxide (ZnO): Remainder

[0101] (First Subcomponent Raw Material) Antimony oxide (Sb2O3): 1.5mol% Cobalt oxide (Co2O3): 1.5mol% Nickel oxide (NiO): 3.0 mol%

[0102] (Second sub-ingredient) Bismuth oxide (Bi2O3): 0.7 mol% Manganese oxide (MnO): 1.5 mol%

[0103] (Third sub-ingredient) Substances containing trivalent elements (Gallium (Ga)): 0.006 mol% Substances containing boron (B) in their composition (B2O3): 0.015mol% Substances containing silver (Ag) in their composition (Ag2O): 0.015 mol%

[0104] [1-1-2] Preparation of slurry (ST20; see Figure 2) Next, a slurry was prepared by putting the mixture prepared above, a solvent, and a binder into a circulation type wet grinding device and grinding the mixture to prepare a slurry.

[0105] Specifically, water was prepared as a solvent, polyvinyl alcohol or the like was prepared as a binder, and the mixture, the solvent, and the binder were placed in a vessel of a wet grinding device so that the content of the mixture was 40% by weight.

[0106] In the circulation type wet grinding apparatus, the mixture was ground by stirring in a vessel containing zirconia beads. Here, the grinding conditions (diameter of zirconia beads, bead filling rate in the vessel, rotation speed of the stirring rotor, circulation flow rate, and mixing time) were changed for each of Samples No. 1 to 60. In this way, the mixture was mixed uniformly to produce slurries for each of Samples No. 1 to 60.

[0107] Using a laser diffraction / scattering type particle size distribution measuring device, the value D50 for (Equation A) was measured for each of the slurries of Samples No. 1 to 60. (ZnOs) , Value D50 for (Formula B) (ZnOt) , the value ([ZnOs] / [ZnOt]) for (Formula C), and the value (D50 (Sb+Co+Ni) ) was calculated (see Tables 1 and 2).

[0108] [1-1-3] Preparation of granules (ST30; see Figure 2) Next, granules were produced. Here, the slurry produced above was sprayed using a spray dryer to produce granules. The granules were produced so that the median diameter D50_k was in the range of 45 μm to 90 μm (45 μm≦D50_k≦90 μm).

[0109] [1-1-4] Preparation of molded body (ST40; see Figure 2) Next, a green compact was produced by molding the granules produced above into a cylindrical shape (diameter: 40 mm, thickness: 40 mm) using a hydraulic press molding machine.

[0110] The compact was then heated at a heating temperature of 500° C. for a heating time of 2 hours to remove the solvent and binder from the compact.

[0111] [1-1-5] Firing (ST50; see Figure 2) Next, firing was performed. Here, the molded body was placed inside a refractory container made of mullite in a tunnel-type continuous furnace. Then, the temperature was raised to 1,050°C at a heating rate of 100°C / hour, and the molded body was fired for 3 hours.

[0112] [1-1-6] Cooling (ST60; see Figure 2) Next, cooling was carried out. Here, after the temperature was lowered to 750° C., the temperature was further lowered at a cooling rate of 100° C. / hour. As a result, a sintered body 20 (see FIG. 1) was obtained.

[0113] [1-1-7] Formation of insulating layer 30 and electrode 40 As described above, after the sintered body 20 was produced, the insulating layer 30 and the electrodes 40 were formed (see FIG. 1).

[0114] In forming the insulating layer 30, a glass frit was applied to the side surface of the sintered body 20, and then a heat treatment was performed at a temperature of 500° C. for two hours.

[0115] In forming the electrode 40, the upper and lower end faces of the sintered body 20 were polished, and then aluminum was sprayed onto the polished faces.

[0116] In the manner described above, the current-voltage nonlinear resistors 10 of Samples No. 1 to No. 60 were produced.

[0117] [1-2] Samples No. 61 to 71 Samples No. 61 to 71 have values ​​related to (Equation E) (D50 (Bi+Mn) ) are the values ​​shown in Table 3. (Sb+Co+Ni) , D50 (ZnOs) , D50 (ZnOt) , and [ZnOs] / [ZnOt] was prepared to be the same as that of sample No. 29.

[0118] [1-3] Samples No. 72 to 103 In preparing samples No. 72 to 103, as shown in Table 4, a substance containing at least one rare earth element R selected from yttrium, europium, erbium, thulium, gadolinium, dysprosium, holmium, and ytterbium in its composition was added as a fourth minor component raw material in the preparation of the mixture (ST10; see FIG. 2). As shown in Table 4, the substance containing the rare earth element R in its composition is an oxide. In preparing samples No. 72 to 103, the mixture contained an oxide of the rare earth element R, and the value (D50 (R) ) are the values ​​shown in Table 4. (Sb+Co+Ni) , D50 (ZnOs) , D50 (ZnOt) , and [ZnOs] / [ZnOt] were fabricated to be similar to those of sample No. 66.

[0119] [2] Sample evaluation method For samples No. 1 to 103, as shown in Tables 1 to 4, the varistor voltage (V1mA) and energy tolerance (average energy for breakdown (J / cm 3 ) was evaluated.

[0120] [2-1] Varistor voltage (V1mA) The varistor voltage (V1mA) was measured in accordance with JEC0202-1994. Specifically, the voltage measured when a power-frequency current of 1mA was passed through the sample was determined as the varistor voltage (V1mA).

[0121] [2-2] Energy tolerance (average energy to break (J / cm 3 ) The energy tolerance was evaluated by applying a 4 / 10μs impulse current to the sample. In the energy tolerance test, the sample was subjected to a 400J / cm2 impulse current until it broke. 3 to about 50 J / cm 3The energy was gradually increased and impulse current was applied. Between applications, the specimens were cooled to room temperature. Here, energy tolerance tests were conducted on each of the 10 specimen pieces, and the average fracture energy value obtained from multiple energy tolerance tests was calculated as the "average fracture energy." Note that the higher the fracture energy value, the better the energy tolerance.

[0122] [3] Evaluation results [3-1] Samples No. 1 to 60 Figure 3 shows the D50 (Sb+Co+Ni) and D50 (ZnOs) FIG. 4 is a graph showing the relationship between D50 and fracture energy. (ZnOt) FIG. 5 shows the relationship between the [ZnOs] / [ZnOt] ratio and the fracture energy. ) 3 to 5 show the relationship between the fracture energy and the specimen No. in Table 1 or Table 2.

[0123] As can be seen from the results in Figures 3 to 5 and Tables 1 and 2, in samples No. 1 to 60, when the relationships shown in (Equation A) and (Equation B) are satisfied (samples not marked with an *), the average fracture energy is 750 J / cm 3 From these results, it is clear that current-voltage nonlinear resistors that satisfy the relationships shown in (Equation A), (Equation B), (Equation C), and (Equation D) have excellent energy tolerance and can be made smaller.

[0124] D50 (ZnOs) ≦0.4μm (Formula A) 0.5μm≦D50 (ZnOt) ≦0.7μm (Formula B) 0.005≦[ZnOs] / [ZnOt]≦0.1 (Formula C) D50 (Sb+Co+Ni) ≦0.4μm (Formula D)

[0125] [3-2] Samples No. 61 to 71 As can be seen from the results in Table 3, in samples No. 61 to 71, when the relationship shown in (Equation E) was further satisfied (samples without an * mark), the average fracture energy was 850 J / cm 3 From these results, it is clear that a current-voltage nonlinear resistor that further satisfies the relationship shown in (Equation E) has excellent energy tolerance and can be made smaller.

[0126] 0.5μm≦D50 (Bi+Mn) ≦0.7μm (Formula E)

[0127] [3-3] Samples No. 72 to 103 As can be seen from the results in Table 4, in samples No. 72 to 103, when the relationship shown in (Equation F) was further satisfied (samples without an * mark), the average fracture energy was 850 J / cm 3 At the same time, the varistor voltage (V1mA) is 900V / mm or more. From these results, it is clear that a current-voltage nonlinear resistor that further satisfies the relationship shown in (Equation F) has excellent energy tolerance and can be made smaller.

[0128] D50 (R) ≦0.4μm (Formula F)

[0129] <Other> Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0130] 10: current-voltage nonlinear resistor, 20: sintered body, 30: insulating layer, 40: electrode

Claims

1. A main component raw material consisting of zinc oxide powder; a first minor component raw material consisting of antimony oxide, cobalt oxide, and nickel oxide powder; a second minor component raw material consisting of bismuth oxide and manganese oxide; A third subcomponent raw material consisting of powders of a substance containing a trivalent element in its composition, a substance containing a boron element in its composition, and a substance containing a silver element in its composition; A current-voltage nonlinear resistor having a sintered body formed by sintering a mixture containing The mixture is The main component raw material is contained in an amount of 85 mol% or more, The main component raw material is The powder contains a first main component powder and a second main component powder, each having a different particle size; Median diameter D50 of the first main component powder (ZnOs) satisfies the relationship shown in (Formula A), Median diameter D50 of the second main component powder (ZnOt) satisfies the relationship shown in (Equation B), The content [ZnOs] of the first main component powder and the content [ZnOt] of the second main component powder satisfy the relationship shown in (Formula C), The median diameter D50 of the first subcomponent raw material (Sb+Co+Ni) satisfies the relationship shown in (Formula D). Current-voltage nonlinear resistor. D50 (ZnOs) ≦0.4μm ……(Formula A) 0.5μm≦D50 (ZnOt) ≦0.7μm ……(Formula B) 0.005≦[ZnOs] / [ZnOt]≦0.1 (Formula C) D50 (Sb+Co+Ni) ≦0.4μm ……(Formula D)

2. The median diameter D50 of the second subcomponent raw material (Bi+Mn) satisfies the relationship shown in (Equation E).

2. The current-voltage nonlinear resistor according to claim 1. 0.5μm≦D50 (Bi+Mn) ≦0.7μm ……(Formula E)

3. The mixture is A fourth subcomponent raw material made of powder of a substance containing at least one rare earth element R from among yttrium, europium, erbium, thulium, gadolinium, dysprosium, holmium, and ytterbium in its composition. Further comprising The median diameter D50 of the fourth subcomponent raw material (R) satisfies the relationship shown in (Formula F).

3. The current / voltage nonlinear resistor according to claim 1 or 2. D50 (R) ≦0.4μm ……(Formula F)

4. A method for producing a current-voltage nonlinear resistor, comprising the steps of: mixing a main component raw material made of zinc oxide powder; a first subcomponent raw material made of antimony oxide, cobalt oxide, and nickel oxide powder; a second subcomponent raw material made of bismuth oxide and manganese oxide; and a third subcomponent raw material made of powders of a substance containing a trivalent element in its composition, a substance containing elemental boron in its composition, and a substance containing elemental silver in its composition; and sintering the mixture to obtain a sintered body, The mixture is The main component raw material is contained in an amount of 85 mol% or more, The main component raw material is The powder contains a first main component powder and a second main component powder, each having a different particle size; Median diameter D50 of the first main component powder (ZnOs) satisfies the relationship shown in (Formula A), Median diameter D50 of the second main component powder (ZnOt) satisfies the relationship shown in (Equation B), The content [ZnOs] of the first main component powder and the content [ZnOt] of the second main component powder satisfy the relationship shown in (Formula C), The median diameter D50 of the first subcomponent raw material (Sb+Co+Ni) satisfies the relationship shown in (Formula D). A method for manufacturing a current-voltage nonlinear resistor. D50 (ZnOs) ≦0.4μm ……(Formula A) 0.5μm≦D50 (ZnOt) ≦0.7μm ……(Formula B) 0.005≦[ZnOs] / [ZnOt]≦0.1 (Formula C) D50 (Sb+Co+Ni) ≦0.4μm ……(Formula D)

Citation Information

Patent Citations

  • Current-voltage nonlinear resistor

    JP2001307909A

  • Voltage non-linear resistor and lightning arrester

    JP2904178B2

  • Voltage nonlinear resistor, method for manufacturing the same, and surge arrester equipped with the voltage nonlinear resistor.

    JP2933881B2

  • Voltage non-linear resistor, method for manufacturing voltage non-linear resistor, and lightning arrester

    JP2940486B2

  • High resistance voltage non-linear resistor and lightning arrester using the same

    JP3165410B2