Wafer processing method

By employing a protective member and forming a second modified layer from the backside to suppress curvature, the method ensures accurate laser beam positioning and successful wafer division into chips.

JP2024157227APending Publication Date: 2024-11-07DISCO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023071458
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The formation of a modified layer on the wafer surface causes the wafer to curve, making it impossible to accurately position the focal point of the laser beam, leading to improper wafer holding and inaccurate layer formation.

Method used

A method involving the use of a protective member on the wafer surface, forming a second modified layer from the backside with a transparent laser beam to suppress curvature, followed by forming a first modified layer as a starting point for division, and applying an external force to divide the wafer into chips.

Benefits of technology

The method effectively suppresses curvature, allowing precise positioning of the laser beam for accurate modified layer formation and successful division into individual chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157227000001_ABST
    Figure 2024157227000001_ABST
Patent Text Reader

Abstract

To provide a wafer processing method for dividing a wafer having a first surface and a second surface on the opposite side and including scheduled division lines on the first surface into individual chips.SOLUTION: A processing method in laser beam radiation means 23 includes the steps of: disposing a protective member on a first surface 10a of a wafer 10; locating a focal point of a laser beam LB with a wavelength having permeability to the wafer from a second surface 10b to the inside of the wafer and radiating the laser beam, thereby forming a first modified layer to be the starting point of division on a side closer to the first surface; applying external force to the wafer to divide the wafer into individual chips; and before the modified layer formation step, in order to prevent a curve that occurs due to swelling on the first surface of the wafer caused by formation of the modified layer, locating the focal point of the laser beam with a wavelength having permeability to a side closer to the second surface of the wafer, thereby forming a second modified layer including at least an annular modified layer 110a.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wafer processing method for dividing a wafer having a first surface and an opposite second surface with dividing lines on the first surface into individual chips. [Background technology]

[0002] Wafers, on whose surface multiple devices such as ICs and LSIs are formed and partitioned along planned division lines, are then divided into individual chips using a laser processing device to form division starting points. These chips are then used in electrical devices such as mobile phones and personal computers.

[0003] The laser processing apparatus includes a chuck table for holding a wafer, a laser beam application means for irradiating a laser beam having a wavelength that is transparent to the wafer held on the chuck table, and a feed means for relatively feeding the chuck table and the laser beam application means for processing, and is capable of forming a modified layer that serves as the starting point for division within the intended division line with high precision (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-000931 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when a modified layer is formed by irradiating the wafer from the back side along the planned dividing line with the focal point of a laser beam positioned close to the front side of the wafer, the front side of the wafer expands overall, causing the wafer to curve in such a way that the front side is convex and the back side is concave, and the wafer is not held properly on the chuck table, so that the focal point of the laser beam cannot be positioned at an appropriate position, and the modified layer cannot be formed accurately at a desired position. This problem is particularly significant when a modified layer is formed close to the front side of the wafer and a crack is extended from the modified layer to the planned dividing line on the front side.

[0006] The present invention has been made in consideration of the above-mentioned facts, and its main technical object is to provide a wafer processing method that can solve the problem that even when the focal point of a laser beam is positioned close to the surface of the wafer and irradiated to form a modified layer that serves as the starting point for division, the front side of the wafer expands and the back side is curved, making it impossible to position the focal point of the laser beam in an appropriate position. [Means for solving the problem]

[0007] In order to solve the above-mentioned main technical problem, according to the present invention, there is provided a wafer processing method for dividing a wafer having a first surface and a second surface opposite thereto, the first surface being provided with a division line, into individual chips, the method comprising: a protective member disposing step of disposing a protective member on the first surface of the wafer; a modified layer forming step of irradiating the wafer from the second surface side of the wafer with a focal point of a laser beam having a wavelength that is transparent to the wafer, positioned inside the division line, to form a first modified layer serving as a starting point for division on the side closer to the first surface; a dividing step of applying an external force to the wafer to divide the wafer into individual chips; and a curvature suppressing step of forming a second modified layer including at least an annular modified layer, prior to the modified layer forming step, by irradiating the wafer from a focal point of a laser beam having a wavelength that is transparent to the wafer, positioned close to the second surface of the wafer, to form a curvature suppressing step.

[0008] The second modified layer formed in the curvature suppression step preferably includes a modified layer formed radially in addition to the modified layer formed annularly. The dividing step is preferably a step of grinding the second surface side of the wafer to thin it and dividing the wafer into individual chips starting from the first modified layer formed inside the dividing line. Furthermore, the first surface of the wafer is preferably formed with a device region in which a plurality of devices are partitioned by the dividing line and an outer peripheral surplus region surrounding the device region, and the second modified layer in the curvature suppression step is preferably formed in a region corresponding to the outer peripheral surplus region. Effect of the Invention

[0009] The wafer processing method of the present invention is a wafer processing method for dividing a wafer having a first surface and an opposite second surface with a division line on the first surface into individual chips, the method including a protective member disposing step of disposing a protective member on the first surface of the wafer, a modified layer forming step of irradiating the wafer from the second surface side of the wafer with a focused point of a laser beam having a wavelength that is transparent to the wafer, positioned inside the division line, to form a first modified layer on the side closer to the first surface, which will be a starting point for division, a dividing step of applying an external force to the wafer to divide the wafer into individual chips, and a step of forming a first modified layer of the wafer by the modified layer forming step prior to the modified layer forming step. and a curvature suppression step of irradiating the wafer with a focal point of a laser beam having a wavelength that is transparent to the wafer, located close to the second surface of the wafer, in order to suppress curvature that occurs on the second surface side due to expansion of the first surface side, thereby forming a second modified layer that includes at least annular modified layer.This suppresses the force that causes curvature in the first surface side of the wafer to become convex and the second surface side to become concave, which is generated by performing the modified layer formation step, and provides a wafer processing method that solves the problem that, when performing the modified layer formation step, the focal point of the laser beam is not positioned in an appropriate position, and the first modified layer is not formed in a desired position. [Brief description of the drawings]

[0010] [Figure 1]FIG. 11 is a perspective view showing an embodiment of a protective member disposing step. [Diagram 2] FIG. 2 is a perspective view showing a manner in which a wafer is held on a chuck table of a laser processing apparatus. [Diagram 3] FIG. 2A is a perspective view showing an embodiment of a curvature suppression step, and FIG. 2B is a partially enlarged cross-sectional view of the wafer in the curvature suppression step shown in FIG. [Figure 4] 1A is a schematic plan view and a partially enlarged cross-sectional view showing the configuration of a second modified layer; FIG. 1B is a schematic plan view and a partially enlarged cross-sectional view showing another configuration of the second modified layer; [Diagram 5] (a) A schematic plan view showing a configuration in which a radially modified layer is formed on the second modified layer shown in Figure 4(a), and (b) A schematic plan view showing a configuration in which a radially modified layer is formed on the second modified layer shown in Figure 4(b). [Figure 6] FIG. 2A is a perspective view showing an embodiment of a modified layer forming step, and FIG. 2B is a partially enlarged cross-sectional view of the embodiment shown in FIG. [Figure 7] FIG. 2A is a perspective view showing an embodiment of a dividing step, and FIG. 2B is a perspective view showing a wafer divided into individual chips by the dividing step. [Figure 8] FIG. 11 is a perspective view showing an embodiment of a tape replacement step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of a wafer processing method according to the present invention will be described in detail with reference to the accompanying drawings.

[0012] The workpiece processed by the wafer processing method of this embodiment is, for example, a silicon (Si) wafer 10 having a first surface (hereinafter referred to as "front surface") 10a and an opposite second surface (hereinafter referred to as "back surface") 10b as shown in Fig. 1. On the front surface 10a of the illustrated wafer 10, a device region 16A near the center in which a plurality of devices 12 are partitioned by planned division lines 14, and a peripheral surplus region 16B surrounding the device region 16A are formed. Note that, in Fig. 1, a boundary line 15 that partitions the device region 16A and the peripheral surplus region 16B is shown by a dashed line, but the boundary line 15 is shown for convenience of explanation and is not actually formed on the wafer 10.

[0013] Once the above-described wafer 10 is prepared, as shown in FIG. 1, a protective tape T that functions as a protective member for protecting the devices 12 is provided on the front surface 10a of the wafer 10 (protective member providing step).

[0014] The wafer 10 integrated with the protective tape T by carrying out the protective member disposing step described above is subjected to a modified layer forming step of forming a first modified layer, which will be described later, and a dividing step of dividing the wafer 10 into individual chips using the first modified layer as a starting point for dividing. Here, in this embodiment, in order to prevent the first modified layer formed in the modified layer forming step from expanding the front surface 10a side of the wafer 10 and causing concave curvature on the back surface 10b side, a curvature suppressing step of forming a second modified layer, which will be described below, is carried out before carrying out the modified layer forming step.

[0015] When performing the curvature suppression step of this embodiment, the above-mentioned wafer 10 is transported to a laser processing device 20 (only a part of which is shown) shown in Fig. 2 and placed on a chuck table 21 with the protective tape T side facing downward and the back surface 10b side facing upward. The chuck table 21 includes a frame 21b and an adsorption chuck 21a surrounded by the frame 21b. The adsorption chuck 21a is formed of a porous member having air permeability, and the frame 21b is connected to a suction means (not shown). By operating the suction means, a negative pressure is generated in the adsorption chuck 21a, and the wafer 10 can be sucked and held.

[0016] 3(a), the laser processing device 20 includes, in addition to the chuck table 21, a laser beam application means 23 for applying a laser beam LB to the wafer 10 held on the chuck table 21, an X-axis feed means for relatively feeding the chuck table 21 and the laser beam application means 23 in the X-axis direction, a Y-axis feed means for relatively feeding the chuck table 21 and the laser beam application means 23 in the Y-axis direction perpendicular to the X-axis direction, a rotary drive means for rotating the holding means in the direction indicated by the arrow R1, and an alignment means including an infrared CCD camera for applying infrared rays toward the chuck table 21 and receiving reflected light of the reflected infrared rays (all of which are not shown). The laser beam LB applied by the laser beam application means 23 is a laser beam having a wavelength that is transparent to silicon constituting the wafer 10.

[0017] The wafer 10 held by suction on the chuck table 21 is positioned directly below the alignment means by the X-axis feed means and imaged, and the processing position where the first modified layer is formed in the modified layer forming step described below and the processing position where the second modified layer is formed in the curvature suppression step are detected. Information on the detected processing positions is stored in a control means (not shown).

[0018] Based on the information of the processing position where the second modified layer is formed detected by the alignment means described above, the condenser 23a of the laser beam application means 23 is positioned at the processing start position where the second modified layer is formed. The processing position where the second modified layer is formed is set in an area corresponding to the outer peripheral surplus area 16B described above as shown in FIG. 3(a), and the condenser 23a of the laser beam application means 23 is positioned at a predetermined processing start position of the outer peripheral surplus area 16B. As shown in FIG. 3(b), the focal point of the laser beam LB irradiated from the laser beam application means 23 is positioned inside the wafer 10 and close to the back surface 10b side exposed upward when viewed in the thickness direction of the wafer 10. The position where the focal point is positioned is set in the inner outer peripheral surplus area 16B avoiding, for example, the area 1.0 to 2.0 mm from the outer peripheral end so as to avoid the chamfered portion 10c (see FIG. 3(b)) that forms the outer peripheral end side of the wafer 10.

[0019] As described above, once the focal point of the laser beam LB has been positioned, the laser beam application means 23 is operated to apply the laser beam LB as shown in Fig. 3(a), and the chuck table 21 is rotated in the direction indicated by the arrow R1 to form an annular modified layer 110a as a second modified layer as shown in Fig. 3(b). The annular modified layer 110a is an annular modified layer formed in the outer peripheral excess region 16B in plan view as shown in Fig. 4(a), and its center is formed to coincide with the center of the wafer 10.

[0020] The laser processing conditions performed by the laser processing device 20 to form the above-mentioned annular modified layer 110a are set, for example, as follows. Wavelength: 1342nm Repetition frequency: 90kHz Average output: 1.2W Circumferential feed speed: 500mm / sec

[0021] 3(b), when viewed in the thickness direction of the wafer 10, by forming the annular modified layer 110a at a position close to the back surface 10b side, a force acts on the wafer 10 to curve the back surface 10b side in a convex manner. In this way, when the above-mentioned annular modified layer 110a is formed on the wafer 10, a force acts on the wafer 10 to curve the front surface 10a in a concave manner, but since a closed space is formed between the suction chuck 21a of the chuck table 21 and the front surface 10a, the negative suction pressure acting on the suction chuck 21a does not escape to the outside, and the wafer 10 is appropriately sucked and held on the chuck table 21.

[0022] In the above embodiment described based on Fig. 3 and Fig. 4(a), one annular modified layer 110a is formed in the region corresponding to the outer peripheral surplus region 16B as the second modified layer, but the form of the second modified layer is not limited to this. For example, as shown in Fig. 4(b), in addition to the above-mentioned annular modified layer 110a formed in the outer peripheral surplus region 16B, an annular modified layer 110b concentric with the annular modified layer 110a may be formed by the same processing procedure as the above-mentioned annular modified layer 110a, to form two annular modified layers 110a, 110b. Furthermore, it is not limited to forming the above-mentioned two annular modified layers, and three or more annular modified layers may be formed.

[0023] In addition to forming the annular modified layers 110a and 110b, the second modified layer may include a radially formed modified layer 120a or 120b as shown in Figs. 5(a) and 5(b). The radial modified layers 120a and 120b are formed in the peripheral excess region 16B, similar to the annular modified layers 110a and 110b, and are formed on the second surface of the wafer 10, i.e., on the side closer to the back surface 10b, when viewed in the thickness direction of the wafer 10. Fig. 5(a) shows a wafer 10 having one annular modified layer 110a as shown in Fig. 4(a) on which a radial modified layer 120a is formed, and Fig. 5(b) shows a wafer 10 having two annular modified layers 110a and 110b as shown in Fig. 4(b) on which a radial modified layer 120b is formed. By forming such radial modified layers 120a, 120b, a stronger force acts on the wafer 10 to curve the back surface 10b side into a convex shape. The curvature suppression step is completed by forming the second modified layer as described above.

[0024] As described above, after the curvature suppression step is performed, a modified layer forming step of forming a first modified layer is performed, which will be described below with reference to FIGS. 6(a) and 6(b).

[0025] The modified layer forming step is a step of forming a first modified layer which is a starting point for dividing the wafer 10 into individual chips, and as shown in FIG. 6(a), it can be performed by the laser processing device 20 which has performed the above-mentioned curvature suppression step while holding the wafer 10 on the chuck table 21. When performing the modified layer forming step of this embodiment, the predetermined direction of the dividing line 14 is aligned in the X-axis direction based on the dividing line 14 detected by the above-mentioned alignment means. Next, the condenser 23a of the laser beam application means 23 is positioned at the processing start position of the predetermined dividing line 14, and the laser beam is irradiated from the back surface 10b side of the wafer 10 by positioning the focusing point on the inside of the wafer 10 corresponding to the dividing line 14 and close to the front surface 10a, and the above-mentioned X-axis feed means is operated to feed the wafer 10 together with the holding means in the X-axis direction for processing, thereby forming a first modified layer 130 along the predetermined dividing line 14 of the wafer 10. As shown in Fig. 6(b), the first modified layer 130 is formed on the first surface, i.e., the side closer to the front surface 10a, in the thickness direction of the wafer 10. For convenience of explanation, the above-mentioned annular modified layers 110a and 110b are omitted in Fig. 6(a).

[0026] After the first modified layer 130 is formed along the position corresponding to the predetermined dividing line 14 as described above, the Y-axis feed means is operated to index and feed the wafer 10 in the Y-axis direction by the interval of the dividing line 14, and the unprocessed dividing line 14 adjacent in the Y-axis direction is positioned directly under the condenser 23a. The dividing lines 14 of the wafer 10 in this embodiment are formed at intervals of 5 mm corresponding to the dimensions of the chips constituting the device 12, and the interval when indexing and feeding in the Y-axis direction is 5 mm. Then, in the same manner as described above, the focusing point of the laser beam LB is positioned inside the wafer 10 corresponding to the dividing line 14 and close to the front surface 10a, and the laser beam LB is irradiated, and the wafer 10 is processed and fed in the X-axis direction to form the first modified layer 130. In the same manner, the wafer 10 is processed and fed in the X-axis direction and the Y-axis direction to form the first modified layer 130 along all the dividing lines 14 along the X-axis direction. Next, the wafer 10 is rotated 90 degrees to align the unprocessed division lines 14 perpendicular to the division lines 14 on which the first modified layers 130 have already been formed, in the X-axis direction. Then, the focal point of the laser beam LB is positioned and irradiated in the same manner as described above inside the wafer 10 corresponding to each of the remaining division lines 14, thereby forming modified layers 130 inside the wafer 10 corresponding to all of the division lines 14 formed on the wafer 10, and the modified layer forming process is thereby completed.

[0027] The laser processing conditions performed by the above-described laser processing device 20 to form the first modified layer 130 that will be the starting point of division are set, for example, as follows: Although not shown, when forming the first modified layer 130, the processing conditions may be set so that a crack extending from the first modified layer 130 to the surface 10a is formed. Wavelength: 1342nm Repetition frequency: 90kHz Average output: 1.2W Machining feed speed: 700mm / sec

[0028] In the modified layer forming step described above, the first modified layer 130, which is the starting point for dividing the wafer 10 into individual chips, is formed on the side close to the front surface 10a of the wafer 10. As a result, the front surface 10a side of the wafer 10 expands overall, and a force acts on the wafer 10 to cause the wafer 10 to be curved such that the front surface 10a side is convex and the back surface 10b side is concave. However, in this embodiment, the above-mentioned curvature suppression step is performed before the modified layer forming step is performed, and a force is generated to cause the wafer 10 to be curved such that the back surface 10b side is convex and the front surface 10a side is concave. As a result, the force to cause the wafer 10 to be curved such that the front surface 10a side is convex and the back surface 10b side is concave, which occurs by performing the modified layer forming step described above, is suppressed. This solves the problem that the wafer 10 is curved when the modified layer forming step is performed, and the focal point of the laser beam LB is not positioned at an appropriate position, and the first modified layer 130 is not formed at a desired position.

[0029] After the first modified layer 130 is formed by the modified layer forming step described above, a dividing step is performed in which an external force is applied to the wafer 10 to divide it into individual chips. The dividing step is performed, for example, as described below with reference to Figures 7(a) and (b). Note that the first modified layer 130 and the second modified layers 110a and 110b are omitted in Figures 7(a) and (b).

[0030] When carrying out the division step, the wafer 10 on which the first modified layer 130 has been formed by the modified layer forming step is transported to a grinding device 30 (only a part of which is shown) shown in Fig. 7. The grinding device 30 includes a chuck table 31 and a grinding means 32 for grinding and thinning the back surface 10b of the wafer 10 held by suction on the chuck table 31. The grinding means 32 includes a rotating spindle 33 rotated by a rotation drive mechanism (not shown), a wheel mount 34 attached to the lower end of the rotating spindle 33, and a grinding wheel 35 attached to the wheel mount 34 and having a plurality of grinding wheels 36 arranged in an annular shape on the lower surface side.

[0031] The side of the wafer 10 to which the protective tape T is attached is placed on the chuck table 31 and held by suction. The rotating spindle 33 of the grinding means 32 is rotated in the direction indicated by the arrow R3 in FIG. 7(a) at, for example, 6000 rpm, while the chuck table 31 is rotated in the direction indicated by the arrow R4 at, for example, 300 rpm. Then, while supplying grinding water onto the back surface 10b of the wafer 10 by a grinding water supplying means (not shown), the grinding stone 36 is brought into contact with the back surface 10b of the wafer 10, and the grinding wheel 35 is fed downward for grinding at a grinding feed rate of, for example, 1 μm / sec. At this time, grinding can be carried out while measuring the thickness of the wafer 10 by a contact or non-contact measuring gauge (not shown), and the back surface 10b of the wafer 10 is ground by a predetermined amount. As a result, the wafer 10 is thinned and an external force is applied, causing cracks to extend toward the front surface 10a along the first modified layer 130, and the wafer 10 is divided into individual chips 12'. Once the wafer 10 is divided into individual chips 12' and formed to a predetermined thickness, the grinding means 30 is stopped, and after cleaning, drying, and other steps (not shown), the dividing step of dividing the wafer 10 into individual chips 12' is completed, and the wafer processing method of this embodiment is completed.

[0032] When the wafer 10 is divided into individual chips 12' by the above-mentioned wafer processing method, a tape replacement step may be performed as necessary, as described below with reference to FIG. 8. When performing the tape replacement step, an annular frame F having an opening Fa capable of accommodating the wafer 10 as shown in FIG. 8 is prepared, and the back surface 10b side of the wafer 10 subjected to the above-mentioned division step is positioned in the center of the opening Fa with the back surface 10b side facing downward. Next, the wafer 10 and the frame F are supported by an adhesive tape T2 that adheres both the back surface 10b of the wafer 10 and the back surface of the frame F. When the wafer 10 is supported by the frame F via the adhesive tape T2 as shown in the figure, the protective tape T1 is peeled off from the front surface 10a of the wafer 10 to expose it as shown in the figure. With the above, the tape replacement step is completed. As a result, the wafer 10 is supported on the frame F via the adhesive tape T2, exposing the surface 10a, making it easier to pick up the individually separated chips 12' from the wafer 10 and, for example, making it easier to carry out the next bonding process.

[0033] In the above embodiment, the annular modified layers 110a, 110b and the radial modified layers 120a, 120b constituting the second modified layer are formed in the peripheral surplus region 16B of the wafer 10, but the present invention is not limited to forming the second modified layer in the peripheral surplus region 16B. That is, instead of forming the second modified layer in the peripheral surplus region 16B, the second modified layer may be formed in the device region 16A, or in addition to forming the second modified layer in the peripheral surplus region 16B, a modified layer that functions as a second modified layer may also be formed in the device region 16A. The second modified layer formed in the device region 16A may be an annular modified layer or a radial modified layer, as in the above embodiment. In this way, when the second modified layer is formed in the device region 16A in the curvature suppression step, the second modified layer is formed at a depth position where the second modified layer formed in the device region 16A is removed when the back surface 10b is ground using the grinding device 30 to divide the chip into individual chips 12'. The second modified layer formed in the device region 16A may interfere with the application of a laser beam when forming the first modified layer in the modified layer formation step. Therefore, when forming the second modified layer in the curvature suppression step, it is preferable not to form the second modified layer at a position that intersects with the planned division line 14. This avoids the problem that the second modified layer interferes with the laser processing when forming the first modified layer in the modified layer formation step.

[0034] The dividing step of the present invention is not limited to dividing the wafer 10 into individual chips 12' by grinding and thinning the back surface 10b side of the wafer 10 with the grinding device 30 described above. For example, instead of grinding the back surface 10b of the wafer 10 with the grinding device 30 described above, as described based on FIG. 8, a tape replacement step may be performed to support the wafer 10 on the frame F via the adhesive tape T2, and the adhesive tape T2 may be radially expanded to apply an external force to the wafer 10, thereby dividing the wafer 10 into individual chips 12' along the first modified layer 130 described above. Alternatively, the wafer 10 may be placed on a flexible mat and a roller (not shown) may be rolled against the back surface 10b of the wafer 10 to apply a pressing force as an external force, thereby dividing the wafer 10 into individual chips 12' starting from the first modified layer 130.

[0035] As described above, various combinations are possible for the region in which the second modified layer is formed in the curvature suppression process and the method of performing the division process. However, when the division process is performed without grinding the back surface 10b of the wafer 10 with a grinding device 30, for example, when the tape replacement process described based on Figure 8 is performed by radially expanding the adhesive tape T2 to divide the wafer into individual chips 12', it is preferable to avoid forming a second modified layer in the device region 16A in which the device 12 is formed. [Explanation of symbols]

[0036] 10: Wafer 10a: Surface (first surface) 10b: Back side (second side) 10c: Chamfered part 12: Device 12': Chip 14: Planned division line 15: Borderline 16A: Device area 16B: Surplus outer area 20: Laser processing equipment 21: Chuck table 21a: Suction chuck 21b: Frame 23: Laser beam irradiation means 23a: Concentrator 30: Grinding equipment 31: Chuck table 32: Grinding means 35: Grinding wheel 36: Grinding wheel 110a, 110b: Annular modified layer (second modified layer) 120a, 120b: Radial modified layer (second modified layer) 130: First modified layer F: Frame T1: Protective tape T2: Adhesive tape

Claims

1. A wafer processing method for dividing a wafer having a first surface and an opposite second surface, the first surface being provided with a dividing line, into individual chips, the method comprising the steps of: a protective member providing step of providing a protective member on a first surface of the wafer; a modified layer forming step of irradiating the wafer from the second surface side of the wafer with a focused point of a laser beam having a wavelength that is transparent to the wafer, the focused point being positioned within the intended dividing line, to form a first modified layer on the side close to the first surface, the first modified layer being a starting point for dividing the wafer; a dividing step of dividing the wafer into individual chips by applying an external force to the wafer; The wafer processing method includes a curvature suppression step, which is performed prior to the modified layer formation step, of positioning a focal point of a laser beam having a wavelength that is transparent to the wafer near the second surface of the wafer and irradiating the laser beam, in order to suppress curvature that occurs on the second surface of the wafer due to expansion of the first surface of the wafer caused by the modified layer formation step, thereby forming a second modified layer including at least annular modified layer.

2. 2. The wafer processing method according to claim 1, wherein the second modified layer formed in the curvature suppressing step includes a modified layer formed radially in addition to a modified layer formed annularly.

3. The wafer processing method according to claim 1, wherein the dividing step comprises grinding the second surface side of the wafer to thin it and dividing the wafer into individual chips starting from the first modified layer formed inside the intended dividing line.

4. A device region in which a plurality of devices are partitioned by division lines and a peripheral excess region surrounding the device region are formed on the first surface of the wafer; 2. The wafer processing method according to claim 1, wherein the second modified layer in the curvature suppression step is formed in a region corresponding to the outer peripheral excess region.

Citation Information

Patent Citations

  • Laser machining apparatus

    JP2007000931A