Anode for all-solid secondary batteries and all-solid secondary battery
The use of graphite and a binder resin with an ethylene oxide structure in the negative electrode of all-solid-state secondary batteries addresses the issue of ionic conduction network severing, resulting in high capacity and efficient charge/discharge performance.
Patent Information
- Application Number
- JP2023072237
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
AI Technical Summary
All-solid-state secondary batteries face issues with increased battery resistance due to the severing of the ionic conduction network between solid electrolyte particles caused by the expansion and contraction of the negative electrode active material during charging and discharging, leading to lithium dendrite formation and charging troubles.
A negative electrode for all-solid-state secondary batteries comprising graphite as the active material with an average particle diameter of 12 μm or less, a binder resin with an ethylene oxide structure, and a specific content ratio of 30-70% by mass, which enhances lithium ion conductivity and prevents internal short circuits.
The solution results in an all-solid-state secondary battery with high capacity and charge/discharge efficiency, minimizing lithium dendrite precipitation and maintaining stable ionic conduction, thereby improving battery performance.
Smart Images

Figure 2024157716000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state secondary battery having a large capacity and high charge / discharge efficiency, and a negative electrode for constituting the all-solid-state secondary battery. [Background technology]
[0002] In recent years, with the development of portable electronic devices such as mobile phones and notebook personal computers, and the practical application of electric vehicles, there has been a demand for small, lightweight batteries with high capacity and high energy density.
[0003] Currently, lithium secondary batteries, particularly lithium ion secondary batteries, that can meet this demand use lithium-containing composite oxides such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2) as the positive electrode active material, graphite or the like as the negative electrode active material, and an organic electrolyte solution containing an organic solvent and a lithium salt as the non-aqueous electrolyte.
[0004] Furthermore, with the further development of devices in which lithium-ion secondary batteries can be used, there is a demand for lithium-ion secondary batteries with longer life, higher capacity and higher energy density, as well as a high demand for the reliability of longer life, higher capacity and higher energy density lithium-ion secondary batteries.
[0005] However, since the organic electrolyte used in the lithium ion secondary battery contains an organic solvent, which is a flammable substance, the organic electrolyte may generate abnormal heat when an abnormality such as a short circuit occurs in the battery. In addition, with the recent trend toward higher energy density of lithium ion secondary batteries and an increasing amount of organic solvent in the organic electrolyte, there is a demand for even higher reliability of lithium ion secondary batteries.
[0006] In view of the above, all-solid-state lithium secondary batteries that do not use organic solvents are being considered. All-solid-state lithium secondary batteries use a molded body of a solid electrolyte that does not use an organic solvent instead of the conventional organic solvent-based electrolyte, and are highly reliable without the risk of abnormal heat generation of the solid electrolyte.
[0007] In addition, all-solid-state secondary batteries are not only highly safe, but also highly reliable, highly environmentally resistant, and have a long lifespan, so they are expected to be maintenance-free batteries that can contribute to social development while also continuing to contribute to safety and security. By providing all-solid-state secondary batteries to society, we can contribute to the achievement of Goal 3 (Ensure healthy lives and promote well-being for all at all ages), Goal 7 (Ensure access to affordable, reliable, sustainable and modern energy for all), Goal 11 (Make cities and human settlements inclusive, safe, resilient and sustainable), and Goal 12 (Ensure sustainable consumption and production patterns) out of the 17 Sustainable Development Goals (SDGs) established by the United Nations.
[0008] For the negative electrode of an all-solid-state secondary battery, a molded body of a negative electrode mixture containing a solid electrolyte together with a negative electrode active material, or a layer (negative electrode mixture layer) made of the above-mentioned negative electrode mixture formed on a current collector is generally used. However, in such a negative electrode, the expansion and contraction of the negative electrode active material accompanying the charging and discharging of the battery causes the ion conductive network between the solid electrolyte particles in the molded body of the negative electrode mixture or in the negative electrode mixture layer to be cut, resulting in problems such as an increase in battery resistance and charging troubles caused by the precipitation of Li dendrites.
[0009] On the other hand, there have been proposals for all-solid-state secondary batteries using negative electrodes that do not use solid electrolytes (Non-Patent Documents 1 to 4, etc.). Such all-solid-state secondary batteries may be able to avoid the above-mentioned problems that may arise due to the expansion and contraction of the negative electrode active material that accompanies charging and discharging. [Prior art documents] [Non-patent literature]
[0010] [Non-Patent Document 1] ACS Energy Letters, 2020, Vol. 5, pp. 2995-3004 [Non-Patent Document 2] Energy and Environmental Science, 2020, Vol. 13, pp. 908-916 [Non-Patent Document 3] Nature, 2021, vol. 593, pp. 218-222 [Non-Patent Document 4] Advanced Energy and Sustainability Research, 2021, Volume 2, Pages 2100066 Summary of the Invention [Problem to be solved by the invention]
[0011] Incidentally, in recent all-solid-state secondary batteries, the demand for improved characteristics has been increasing due to the widening range of applications, and there is still room for improvement in the above-mentioned techniques.
[0012] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an all-solid-state secondary battery having a large capacity and high charge / discharge efficiency, and a negative electrode for constituting the all-solid-state secondary battery. [Means for solving the problem]
[0013] The negative electrode for an all-solid-state secondary battery of the present invention is a negative electrode used in an all-solid-state secondary battery having a solid electrolyte layer, and is characterized in that it has a negative electrode mixture layer on a current collector, the negative electrode mixture layer containing graphite as a negative electrode active material and a binder resin having an ethylene oxide structure in its molecule, the graphite having an average particle size of 12 μm or less, and the negative electrode mixture layer having a content of the binder resin of 30 to 70 mass %.
[0014] The all-solid-state secondary battery of the present invention is characterized in that it has at least one electrode laminate in which a negative electrode and a positive electrode face each other via a solid electrolyte layer, and has the negative electrode for an all-solid-state secondary battery of the present invention as the negative electrode. Effect of the Invention
[0015] According to the present invention, it is possible to provide an all-solid-state secondary battery having a large capacity and high charge / discharge efficiency, and a negative electrode for constituting the all-solid-state secondary battery. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of an all-solid-state secondary battery of the present invention. [Diagram 2] FIG. 2 is a plan view illustrating a schematic configuration of another example of the all-solid-state secondary battery of the present invention. [Diagram 3] 2. FIG. 2 is a cross-sectional view taken along line II in FIG. [Figure 4] FIG. 2 is a diagram showing a Raman spectrum of the negative electrode of the all-solid-state secondary battery in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] <Negative electrode for all-solid-state secondary batteries> The negative electrode for an all-solid-state secondary battery of the present invention has a negative electrode mixture layer on a current collector, the negative electrode mixture layer containing graphite as a negative electrode active material and a binder resin having an ethylene oxide structure (-CH2-CH2-O-) in its molecule.
[0018] The binder resin has binding properties and lithium ion conductivity, and by being present between the negative electrode active material particles in the negative electrode mixture layer, it is possible to impart good lithium ion conductivity to the negative electrode mixture layer.
[0019] The graphite contained in the negative electrode mixture layer as the negative electrode active material may be either natural graphite or artificial graphite (e.g., easily graphitizable carbon such as pyrolytic carbon, mesophase carbon microbeads, or carbon fiber that has been graphitized at 2800°C or higher).
[0020] The negative electrode active material may be graphite alone, or may be graphite and other negative electrode active materials. Examples of other negative electrode active materials that may be used together with graphite include carbon materials such as graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), pyrolytic carbons, cokes, glassy carbons, sintered organic polymer compounds, mesophase carbon microbeads, carbon fibers, and activated carbon; simple substances and compounds (oxides, etc.) containing elements such as Si and Sn, and alloys thereof; and the like.
[0021] However, when graphite is used in combination with other negative electrode active materials as the negative electrode active material, the proportion of graphite in the total amount of the negative electrode active material is preferably 80 mass% or more. Note that, since only graphite may be used as the negative electrode active material, the preferred upper limit of the proportion of graphite in the total amount of the negative electrode active material is 100 mass%.
[0022] The average particle size of the graphite is 12 μm or less, preferably 10 μm or less, and more preferably 8 μm or less, from the viewpoint of making the current distribution in the negative electrode mixture layer and / or at the interface between the negative electrode mixture layer and the solid electrolyte layer uniform and preventing current concentration on specific graphite particles from causing acicular lithium to precipitate and cause an internal short circuit. On the other hand, from the viewpoint of improving the electronic conductivity of the negative electrode mixture layer due to the connection between the graphite particles, the average particle size of the graphite is preferably 1 μm or more, and more preferably 2 μm or more.
[0023] When a material other than graphite is used as the negative electrode active material, the average particle size of the material is also preferably 12 μm or less, and 1 μm or more.
[0024] The content of the negative electrode active material in the negative electrode mixture layer is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more in order to increase the proportion of the negative electrode active material to increase the capacity of the negative electrode and to impart a certain level of electronic conductivity to the negative electrode mixture layer. On the other hand, the content of the negative electrode active material in the negative electrode mixture layer is preferably 70% by mass or less, more preferably 65% by mass or less, and even more preferably 60% by mass or less in order to increase the proportion of the binder resin to impart a certain level of ionic conductivity to the negative electrode mixture layer and to uniformize the current distribution in the negative electrode mixture layer to prevent internal short circuit due to precipitation of acicular lithium.
[0025] The binder resin contained in the negative electrode mixture layer has an ethylene oxide structure in its molecule, and an example of such a binder resin is an ethylene glycol copolymer.
[0026] Examples of ethylene glycol copolymers include those obtained by polymerizing ethylene glycol and a monomer component other than ethylene glycol; those having a main chain obtained by polymerizing a monomer other than ethylene glycol and a side chain having an ethylene oxide structure derived from ethylene glycol (including those having a structure in which main chains obtained by polymerizing a monomer other than ethylene glycol are crosslinked with a chain having an ethylene oxide structure); and the like.
[0027] Specific examples of other monomer components that can be polymerized with ethylene glycol include acrylic acid, acrylic esters, vinyl alcohol, vinylpyrrolidone, butadiene, styrene, and acrylonitrile.
[0028] A specific example of a copolymer having a main chain obtained by polymerizing a monomer other than ethylene glycol and a side chain having an ethylene oxide structure derived from ethylene glycol is an acrylic acid-ethylene glycol copolymer in which the main chains of polyacrylic acid are crosslinked with ethylene oxide chains. The main chain component can be a general binder resin such as polyvinyl alcohol, in addition to polyacrylic acid.
[0029] From the viewpoint of ensuring the above-mentioned effects by including a binder resin having an ethylene oxide structure in the molecule in the negative electrode mixture layer, the proportion of the ethylene oxide structure portion in the binder resin is preferably 0.05% by mass or more, and more preferably 0.1% by mass or more. On the other hand, in order to ensure the binding action, the proportion of the ethylene oxide structure portion in the binder resin is preferably 50% by mass or less, more preferably 10% by mass or less, and even more preferably 1% by mass or less.
[0030] Many types of binder resins as described above are commercially available, and such commercially available products can be used for the negative electrode for the all-solid-state secondary battery.
[0031] From the viewpoint of ensuring the effect of its use, the content of the binder resin in the negative electrode mixture layer is 30% by mass or more, preferably 35% by mass or more, and more preferably 40% by mass or more. However, if the content of the binder resin in the negative electrode mixture layer becomes too large, the content of the negative electrode active material becomes small and the capacity of the negative electrode decreases, so the content of the binder resin in the negative electrode mixture layer is 70% by mass or less, preferably 65% by mass or less, and more preferably 60% by mass or less.
[0032] The negative electrode mixture layer can contain binders other than binder resins having an ethylene oxide structure in the molecule. Specific examples include polysaccharides such as starch, polyvinyl alcohol, polyacrylic acid, carboxymethyl cellulose (CMC), hydroxypropyl cellulose, regenerated cellulose, and diacetyl cellulose, and their modified products; thermoplastic resins such as polyvinyl chloride, polyvinylpyrrolidone (PVP), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene, polypropylene, polyamideimide, and polyamide, and their modified products; polyimide; polymers having rubber-like elasticity such as ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), butadiene rubber, polybutadiene, fluororubber, and polyethylene oxide, and their modified products; and the like.
[0033] When the negative electrode mixture layer contains a binder other than a binder resin having an ethylene oxide structure in its molecule, the content thereof is preferably 5 mass % or less.
[0034] Furthermore, the negative electrode mixture layer may contain a conductive assistant such as carbon black (thermal black, furnace black, channel black, ketjen black, acetylene black, etc.) if necessary. When the negative electrode mixture layer contains a conductive assistant, the content is preferably 1 to 5 mass %.
[0035] The current collector for the negative electrode of the all-solid-state secondary battery can be made of copper or nickel foil, punched metal, net, expanded metal, foamed metal, carbon sheet, etc. The thickness of the current collector is preferably 5 to 50 μm.
[0036] A negative electrode for an all-solid-state secondary battery can be manufactured by dispersing a negative electrode active material, a binder resin, and further a binder and a conductive assistant, which are used as necessary, in an organic solvent such as water or N-methyl-2-pyrrolidone (NMP) to prepare a negative electrode mixture-containing composition (slurry, paste, etc.), applying this onto a current collector, drying it, and, if necessary, carrying out pressure molding such as calendaring, thereby forming a negative electrode mixture layer on one or both sides of the current collector.
[0037] The thickness of the negative electrode mixture layer is preferably 5 to 300 μm.
[0038] <All-solid-state secondary battery> The all-solid-state secondary battery of the present invention has at least one electrode laminate in which a negative electrode and a positive electrode face each other via a solid electrolyte layer, and has the negative electrode for an all-solid-state secondary battery of the present invention as the negative electrode.
[0039] A cross-sectional view showing a schematic example of an all-solid-state secondary battery of the present invention is shown in Fig. 1. In the all-solid-state battery 1 shown in Fig. 1, an electrode laminate formed by laminating a positive electrode 10, a negative electrode 20, and a solid electrolyte layer 30 interposed between the positive electrode 10 and the negative electrode 20 is enclosed in an exterior body formed of an exterior can 40, a sealing can 50, and a resin gasket 60 interposed between them, and the negative electrode 20 is the negative electrode for the all-solid-state secondary battery of the present invention. Note that in Fig. 1, the negative electrode 20 is not shown separately as a negative electrode mixture layer and a current collector.
[0040] The sealing can 50 is fitted into the opening of the outer can 40 via a gasket 60, and the open end of the outer can 40 is tightened inward, whereby the gasket 60 comes into contact with the sealing can 50, sealing the opening of the outer can 40 and forming an airtight structure inside the element.
[0041] The outer can and the sealing can can be made of stainless steel or the like. The gasket can be made of polypropylene, nylon, or other materials. If heat resistance is required for the battery's intended use, heat-resistant resins with melting points exceeding 240°C, such as fluororesins such as tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), polyphenylene ether (PEE), polysulfone (PSF), polyarylate (PAR), polyethersulfone (PES), polyphenylene sulfide (PPS), and polyetheretherketone (PEEK), can also be used. If the battery is used in an application that requires heat resistance, a glass hermetic seal can be used for the sealing.
[0042] 2 and 3 are drawings that diagrammatically show another example of the all-solid-state secondary battery of the present invention. Fig. 2 is a plan view of the all-solid-state secondary battery, and Fig. 3 is a cross-sectional view taken along line II in Fig. 2.
[0043] The all-solid-state secondary battery 100 shown in Figures 2 and 3 contains an electrode laminate 200 consisting of a positive electrode, a solid electrolyte layer, and an all-solid-state secondary battery negative electrode of the present invention in a laminate film exterior 500 consisting of two metal laminate films, and the laminate film exterior 500 is sealed at its outer periphery by heat-sealing the upper and lower metal laminate films. In Figure 3, in order to avoid complicating the drawing, the layers constituting the laminate film exterior 500 and the positive electrode, solid electrolyte layer, and negative electrode constituting the electrode laminate are not shown separately.
[0044] The positive electrode of the electrode laminate 200 is connected to a positive electrode external terminal 300 within the battery 100, and although not shown, the negative electrode of the electrode laminate 200 is also connected to a negative electrode external terminal 400 within the battery 100. One end of the positive electrode external terminal 300 and the negative electrode external terminal 400 is drawn out to the outside of the laminate film exterior body 500 so that they can be connected to an external device or the like.
[0045] (positive electrode) As the positive electrode of the all-solid-state secondary battery, for example, there are those composed only of a molded body of a positive electrode mixture containing a positive electrode active material and a conductive assistant, and those having a structure in which a layer (positive electrode mixture layer) composed of a molded body of a positive electrode mixture is formed on a current collector.
[0046] The positive electrode active material is not particularly limited as long as it is a positive electrode active material used in a conventionally known non-aqueous electrolyte secondary battery, that is, an active material capable of occluding and releasing Li ions. Specific examples of the positive electrode active material include LiM r Mn 2-r O4 (where M is at least one element selected from the group consisting of Li, Na, K, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Zr, Fe, Co, Ni, Cu, Zn, Al, Sn, Sb, In, Nb, Ta, Mo, W, Y, Ru, and Rh, and 0 ≦ r ≦ 1), a spinel-type lithium manganese composite oxide represented by r Mn (1-s-r) Ni s M t O (2-u) F v (where M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, 0.8 ≦ r ≦ 1.2, 0 < s < 0.5, 0 ≦ t ≦ 0.5, u + v < 1, -0.1 ≦ u ≦ 0.2, 0 ≦ v ≦ 0.1), a layered compound represented by 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, V, Cr, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ r ≦ 0.5), a lithium cobalt composite oxide represented by 1-r M r O2 (where M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0 ≦ r ≦ 0.5), a lithium nickel composite oxide represented by 1+s M 1-r N r PO4F s(wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5, 0≦s≦1), an olivine-type composite oxide represented by Li2M 1-r N r Examples of such compounds include pyrophosphate compounds represented by the formula: P2O7 (wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5). Among these compounds, only one may be used, or two or more may be used in combination.
[0047] The average particle size of the positive electrode active material is preferably 0.1 μm or more, more preferably 0.5 μm or more, and more preferably 25 μm or less, more preferably 10 μm or less, from the viewpoint of reducing side reactions that cause deterioration of the battery capacity and increasing the density of the electrode. The positive electrode active material may be primary particles or secondary particles formed by agglomeration of primary particles. When the molded body of the positive electrode mixture contains a solid electrolyte, using a positive electrode active material having an average particle size in the above range can provide a large interface with the solid electrolyte, thereby further improving the load characteristics of the battery.
[0048] The average particle diameter of the positive electrode active material and the average particle diameter of graphite and the negative electrode active material other than graphite in this specification are the 50% diameter value (D) in the volume-based integrated fraction when calculating the integral volume from small particles using a particle size distribution measurement device (such as a Microtrac particle size distribution measurement device "HRA9320" manufactured by Nikkiso Co., Ltd.). 50 )
[0049] When the positive electrode mixture compact contains a solid electrolyte, the positive electrode active material preferably has a reaction suppression layer on its surface for suppressing reaction with the solid electrolyte contained in the positive electrode.
[0050] If the positive electrode active material and the solid electrolyte come into direct contact with each other in the positive electrode mixture compact, the solid electrolyte may oxidize to form a resistance layer, which may reduce the ionic conductivity in the compact. By providing a reaction suppression layer that suppresses the reaction with the solid electrolyte on the surface of the positive electrode active material and preventing direct contact between the positive electrode active material and the solid electrolyte, it is possible to suppress the reduction in the ionic conductivity in the compact due to the oxidation of the solid electrolyte.
[0051] The reaction suppression layer may be made of a material that has ion conductivity and can suppress the reaction between the positive electrode active material and the solid electrolyte. Examples of materials that can form the reaction suppression layer include oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti, Zr, Ta, and W, more specifically, Nb-containing oxides such as LiNbO3, Li3PO4, Li3BO3, Li4SiO4, Li4GeO4, LiTiO3, LiZrO3, Li2WO4, and the like. The reaction suppression layer may contain only one of these oxides, or may contain two or more of them, and further, a plurality of these oxides may form a composite compound. Among these oxides, it is preferable to use an Nb-containing oxide, and it is more preferable to use LiNbO3.
[0052] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 2.0 parts by mass per 100 parts by mass of the positive electrode active material, in order to effectively suppress the reaction between the positive electrode active material and the solid electrolyte.
[0053] Methods for forming a reaction suppression layer on the surface of a positive electrode active material include the sol-gel method, the mechanofusion method, the CVD method, the PVD method, and the ALD method.
[0054] The content of the positive electrode active material in the positive electrode mixture compact is preferably 20 to 95 mass %.
[0055] Examples of the conductive assistant for the positive electrode include carbon materials such as carbon black (thermal black, furnace black, channel black, ketjen black, acetylene black, etc.), graphite (natural graphite, artificial graphite), graphene, vapor-grown carbon fiber, carbon nanofiber, and carbon nanotube; powders of Cu, Ni, Al, Au, and Pd alone or alloys thereof, or porous bodies thereof; and these may be used alone or in combination of two or more. The content of the conductive assistant in the molded body of the positive electrode mixture is preferably 0.1 to 15 mass%.
[0056] The positive electrode mixture compact can contain a solid electrolyte. The solid electrolyte used in the positive electrode mixture compact is not particularly limited as long as it has Li-ion conductivity, and examples of the solid electrolyte that can be used include sulfide-based solid electrolytes, hydride-based solid electrolytes, halide-based solid electrolytes, and oxide-based solid electrolytes.
[0057] Examples of sulfide-based solid electrolytes include particles of Li2S-P2S5, Li2S-SiS2, Li2S-P2S5-GeS2, and Li2S-B2S3-based glass. In addition, thio-LISICON-type electrolytes [Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 Li 12-12a-b+c+6d-e M 1 3+a-b-c-d M 2 b M 3 c M 4 d M 5 12-e X e (However, M 1 is Si, Ge or Sn, M 2 is P or V, M 3 is Al, Ga, Y or Sb, M 4 is Zn, Ca, Ba, M 5is either S or both S and O, X is F, Cl, Br or I, 0 ≦ a < 3, 0 ≦ b + c + d ≦ 3, 0 ≦ e ≦ 3, or an argyrodite type such as Li6PS5Cl, Li 7-f+g PS 6-x Cl x+y (where 0.05 ≦ f ≦ 0.9, -3.0f + 1.8 ≦ g ≦ -3.0f + 5.7), Li 7-h PS 6-h Cl i Br j (where h = i + j, 0 < h ≦ 1.8, 0.1 ≦ i / j ≦ 10.0), etc.] can also be used.
[0058] Examples of the hydride-based solid electrolyte include LiBH4, a solid solution of LiBH4 and the following alkali metal compound (for example, those with a molar ratio of LiBH4 to the alkali metal compound of 1:1 to 20:1). Examples of the alkali metal compound in the solid solution include lithium halides (LiI, LiBr, LiF, LiCl, etc.), rubidium halides (RbI, RbBr, RbF, RbCl, etc.), cesium halides (CsI, CsBr, CsF, CsCl, etc.), lithium amide, rubidium amide, and at least one selected from the group consisting of cesium amide.
[0059] Examples of the halide-based solid electrolyte include monoclinic LiAlCl4, defective spinel-type or layered structure LiInBr4, monoclinic Li 6-3m Y m X6 (where 0 < m < 2 and X = Cl or Br), etc. In addition, for example, known ones described in International Publication No. 2020 / 070958 and International Publication No. 2020 / 070955 can also be used.
[0060] Examples of the oxide-based solid electrolyte include Li2O-Al2O3-SiO2-P2O5-TiO2-based glass ceramics, Li2O-Al2O3-SiO2-P2O5-GeO2-based glass ceramics, garnet-type Li7La3Zr2O 12 , NASICON-type Li1+O Al 1+O Ti 2-O (PO4)3, Li 1+p Al 1+p Ge 2-p (PO4)3, perovskite-type Li 3q La 2 / 3-q Examples include TiO3.
[0061] Among these solid electrolytes, sulfide-based solid electrolytes are preferred because of their high Li-ion conductivity, sulfide-based solid electrolytes containing Li and P are more preferred, and argyrodite-type sulfide-based solid electrolytes, which have particularly high Li-ion conductivity and high chemical stability, are even more preferred.
[0062] The content of the solid electrolyte in the positive electrode mixture compact is preferably 4 to 80 mass %.
[0063] The positive electrode mixture compact may contain a binder, or may not contain a binder in cases where good moldability can be ensured without using a binder, such as in the case of a positive electrode in which a sulfide-based solid electrolyte is contained and the powder of the positive electrode mixture is charged into a molding die and compacted.
[0064] Examples of the binder contained in the positive electrode mixture compact include fluororesins such as PVDF.
[0065] When the positive electrode mixture compact requires a binder, the content is preferably 15% by mass or less, and more preferably 0.5% by mass or more. On the other hand, when the positive electrode mixture compact requires no binder from the viewpoint of moldability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).
[0066] When a current collector is used for the positive electrode, the current collector can be made of a metal foil such as aluminum or stainless steel, a punched metal, a net, an expanded metal, a foamed metal, a carbon sheet, etc. The thickness of the current collector for the positive electrode is preferably 0.1 to 200 μm.
[0067] The positive electrode mixture compact can be formed, for example, by compressing a positive electrode mixture prepared by mixing a positive electrode active material, a conductive assistant, a solid electrolyte, and further a binder added as necessary, by pressure molding or the like.
[0068] In the case of a positive electrode having a current collector, the positive electrode can be produced by bonding a molded body of the positive electrode mixture formed by the above-mentioned method to the current collector by, for example, pressure bonding.
[0069] Alternatively, the positive electrode mixture and a solvent may be mixed to prepare a positive electrode mixture-containing composition, which may be applied onto a substrate such as a current collector or a solid electrolyte layer that faces the positive electrode, dried, and then pressed to form a molded body of the positive electrode mixture.
[0070] It is preferable to select a solvent that does not easily deteriorate the solid electrolyte for use in the positive electrode mixture-containing composition. In particular, since sulfide-based solid electrolytes and hydride-based solid electrolytes undergo chemical reactions with trace amounts of water, it is preferable to use non-polar aprotic solvents such as hydrocarbon solvents such as hexane, heptane, octane, nonane, decane, decalin, toluene, and xylene. In particular, it is more preferable to use an ultra-dehydrated solvent with a water content of 0.001 mass% (10 ppm) or less. In addition, fluorine-based solvents such as "Vertrel (registered trademark)" manufactured by Mitsui DuPont Fluorochemicals, "Zeorolla (registered trademark)" manufactured by Nippon Zeon Co., Ltd., and "Novec (registered trademark)" manufactured by Sumitomo 3M Co., Ltd., as well as non-aqueous organic solvents such as dichloromethane and diethyl ether can also be used.
[0071] The thickness of the positive electrode mixture compact (in the case of a positive electrode having a current collector, the thickness of the positive electrode mixture compact per one side of the current collector; the same applies below) is usually 50 μm or more, but from the viewpoint of increasing the capacity of the battery, it is preferably 200 μm or more. Also, the thickness of the positive electrode mixture compact is usually 2000 μm or less.
[0072] In the case of a positive electrode produced by forming a positive electrode mixture layer on a current collector using a positive electrode mixture-containing composition containing a solvent, the thickness of the positive electrode mixture layer is preferably 50 to 1000 μm.
[0073] (Solid electrolyte layer) The solid electrolyte in the solid electrolyte layer interposed between the positive electrode and the negative electrode can be one or more of the various sulfide-based solid electrolytes, hydride-based solid electrolytes, halide-based solid electrolytes, and oxide-based solid electrolytes exemplified above as those usable for the positive electrode. However, in order to improve the battery characteristics, it is preferable to contain a sulfide-based solid electrolyte, and it is more preferable to contain an argyrodite-type sulfide-based solid electrolyte. It is even more preferable to contain a sulfide-based solid electrolyte in both the positive electrode and the solid electrolyte layer, and it is particularly preferable to use an argyrodite-type sulfide-based solid electrolyte as the sulfide-based solid electrolyte.
[0074] The solid electrolyte layer may have a porous body such as a resin nonwoven fabric as a support.
[0075] The solid electrolyte layer can be formed by a method of compressing a solid electrolyte by pressure molding or the like; a method of applying a composition for forming a solid electrolyte layer, which is prepared by dispersing a solid electrolyte in a solvent, onto a substrate, a positive electrode, or a negative electrode, drying the composition, and, if necessary, performing pressure molding such as pressing.
[0076] It is desirable to select a solvent that is unlikely to deteriorate the solid electrolyte as the solvent used in the solid electrolyte layer-forming composition, and it is preferable to use the same solvent as the various solvents exemplified above as the solvent for the positive electrode mixture-containing composition containing the solid electrolyte.
[0077] The thickness of the solid electrolyte layer is preferably 10 to 500 μm.
[0078] (Laminated electrode body) The all-solid-state secondary battery has a laminate as an electrode laminate, which is made of a positive electrode and a negative electrode facing each other with a solid electrolyte layer interposed therebetween. The all-solid-state secondary battery may use only one of the electrode laminates, or may use a plurality of unit electrode laminates (e.g., 2 to 10) each having a positive electrode, a solid electrolyte layer, and a negative electrode stacked thereon, as necessary. When stacking unit electrode laminates together, a method can be adopted in which the positive electrode of the lower unit electrode laminate and the negative electrode of the upper unit electrode laminate (or the negative electrode of the lower unit electrode laminate and the positive electrode of the upper unit electrode laminate) are usually placed opposite each other, and adjacent unit electrode laminates are connected in series by, for example, interposing a current collector between the two electrodes.
[0079] In addition, when forming the electrode laminate, it is preferable to pressure mold the positive electrode and the negative electrode in a stacked state with the solid electrolyte layer interposed therebetween. This makes it possible to increase the mechanical strength of the electrode laminate and to reduce the contact resistance between the positive electrode and the solid electrolyte layer and the contact resistance between the negative electrode and the solid electrolyte layer.
[0080] (Battery type) The form of the all-solid-state secondary battery may be one having an exterior body composed of an exterior can, a sealing can, and a gasket as shown in FIG. 1, that is, one generally referred to as a coin-type battery or a button-type battery, or one having an exterior body composed of a resin film or a metal-resin laminate film as shown in FIGS. 2 and 3, or one having an exterior body having a metallic, bottomed, tubular (cylindrical or rectangular) exterior can and a sealing structure that seals the opening of the can.
[0081] In the all-solid-state secondary battery, in the Raman spectrum of the negative electrode in the charged state, -1 It is possible to have a peak attributable to Li2C2 in the region.
[0082] The negative electrode for an all-solid-state secondary battery of the present invention is unlikely to cause a short circuit caused by Li dendrites even when an all-solid-state secondary battery (all-solid-state secondary battery of the present invention) using the negative electrode is charged until LiC2 is generated, and thus good charge / discharge efficiency can be achieved while increasing the capacity of the all-solid-state secondary battery. Here, when irradiated with excitation light having a wavelength of 532 nm used in laser Raman spectroscopy, LiC2 decomposes to generate Li2C2, and therefore, in the Raman spectrum of the negative electrode when the all-solid-state secondary battery is in a charged state, the peak of LiC2 is 1800 to 1900 cm -1 The presence of a peak attributed to Li2C2 in this region suggests that LiC2 is being generated in the negative electrode of the all-solid-state secondary battery in this charged state. If no problems such as short circuits occur in this state, it can be determined that the battery is a high-capacity battery that can be used satisfactorily even when charged to a deeper depth of charge.
[0083] The laser Raman spectroscopy of the negative electrode in the charged state is measured, for example, using a confocal laser Raman microscope (RAMANTouch, manufactured by Nanophoton) and an airtight cell (LIBcell, manufactured by Nanophoton). As the charging conditions of the battery before measurement, the capacity is calculated based on the content of the positive electrode active material in the positive electrode, and constant current charging is performed at 0.01C until a preset upper limit voltage is reached. After the upper limit voltage is reached, constant voltage charging is performed by continuously applying the upper limit voltage for 100 hours, thereby obtaining a battery having a negative electrode in a charged state. The charged battery is disassembled in a glove box in an Ar gas environment with a dew point of -60°C or less, and the current collector is peeled off from the negative electrode. The sample is cut out so that the negative electrode mixture layer remaining on the solid electrolyte layer side or the current collector side faces the quartz window plate of the airtight cell, and sealed in the airtight cell. An excitation laser light with a wavelength of 532 nm is irradiated, and the negative electrode mixture layer is observed using an objective lens (with a glass correction ring) with a magnification of 50 times or more. The signal intensity of the peak assigned to Li2C2 is the signal intensity at the peak position (peak top wave number) of the peak assigned to Li2C2 and the signal intensity at 1750 cm -1 The signal intensity is calculated as the difference between the signal intensity at
[0084] The flat all-solid-state secondary battery of Example 1 described later was subjected to laser Raman spectroscopy analysis of the negative electrode in the charged state under the above conditions, and the results are shown in FIG. -1 It can be seen that there is a peak assigned to Li2C2 in this region.
[0085] The all-solid-state secondary battery of the present invention has a high capacity and excellent charge / discharge efficiency, and therefore can be used in a variety of applications in which non-aqueous electrolyte secondary batteries are used, including applications in which such characteristics are required. In addition, the negative electrode for the all-solid-state secondary battery of the present invention can constitute the all-solid-state secondary battery of the present invention. EXAMPLES
[0086] The present invention will be described in detail below with reference to examples, although the present invention is not limited to the following examples.
[0087] Example 1 Natural graphite with an average particle size of 7.5 μm was used as the negative electrode active material, and polyacrylic acid "10CLPAH (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., polyethylene oxide content 0.15% by mass)" having a cross-linked structure was used as the binder resin, and dispersed in pure water at a mass ratio of 1:1 by ultrasonic waves. The obtained slurry was applied to a copper foil with a thickness of 8 μm at a speed of 9 mm / sec using an applicator with a gap of 120 μm to form a negative electrode mixture layer. Next, a heat drying treatment was performed at 60°C for 12 hours under vacuum, and then the negative electrode was punched out with a punch with a diameter of 9 mm. The content ratio of the negative electrode active material in the negative electrode mixture layer was 50% by mass, and the basis weight of the negative electrode mixture was 1.4 mg / cm. 2 It was decided.
[0088] <Formation of solid electrolyte layer> 20 mg of Li6PS5Cl as a solid electrolyte was placed in a mold with an inner diameter of 9 mm and 2 × 10 3 kgf / cm 2 The solid electrolyte layer was formed by molding at a pressure of 1000 MPa.
[0089] <Preparation of positive electrode> 0.86g of lithium and 38.7g of pentaethoxyniobium were mixed in 394g of dehydrated ethanol to prepare a coating solution for forming a reaction suppression layer. Next, the coating solution for forming a reaction suppression layer was applied to 1000g of a positive electrode active material (LiCoO2) at a rate of 2g per minute using a coating device using a rolling fluidized bed. The obtained powder was heat-treated at 350°C to obtain a positive electrode material having a reaction suppression layer formed on the surface thereof, the reaction suppression layer being composed of 2 parts by mass of LiNbO3 per 100 parts by mass of the positive electrode active material.
[0090] On the solid electrolyte layer prepared in the mold, 91 mg of a positive electrode mixture obtained by mixing the positive electrode material, carbon black, and a solid electrolyte (Li6PS5Cl) in a mass ratio of 66:4:30 was placed. 3 kgf / cm 2 The mixture was molded under a pressure of 1000 MPa to form a positive electrode mixture layer (positive electrode).
[0091] <Formation of negative electrode and preparation of electrode laminate> The negative electrode was placed on the solid electrolyte layer not in contact with the positive electrode such that the solid electrolyte layer and the negative electrode mixture layer were in contact with each other. 3 kgf / cm 2 A positive electrode / solid electrolyte layer / negative electrode laminate was obtained by pressing at a pressure of 1000 MPa.
[0092] <Fabrication of flat all-solid-state secondary batteries> A sealing can (negative electrode can) with a gasket fitted therein, a wave washer, a 100 μm-thick stainless steel disk, the electrode laminate, a 0.05 mm-thick carbon sheet, and an outer can (positive electrode can) were stacked in that order, and the outer can was crimped to seal. A heat treatment was then performed for 2 hours in a constant temperature bath at 115° C. to obtain a flat all-solid-state secondary battery.
[0093] Example 2 A flat all-solid-state secondary battery was produced in the same manner as in Example 1, except that the temperature of the heat treatment was changed to 150°C.
[0094] Comparative Example 1 A negative electrode was produced in the same manner as in Example 1, except that the negative electrode active material was changed to acetylene black having an average particle size of 35 nm. The content of the negative electrode active material in the negative electrode mixture layer was 50 mass %, and the weight per unit area of the negative electrode was 0.8 mg / cm. 2 Using this negative electrode, a flat all-solid-state secondary battery was produced in the same manner as in Example 1, except that the heat treatment temperature was changed to 150°C.
[0095] Comparative Example 2 A negative electrode was produced in the same manner as in Example 1, except that the negative electrode active material was changed to natural graphite having an average particle size of 15 μm. The content of the negative electrode active material in the negative electrode mixture layer was 50 mass %, and the weight per unit area of the negative electrode was 1.9 mg / cm. 2 A flat all-solid-state secondary battery was produced in the same manner as in Example 1, except that this negative electrode was used.
[0096] Comparative Example 3 A negative electrode was produced in the same manner as in Example 1, except that the ratio of the negative electrode active material to the binder resin in the slurry was changed to 1:3 by mass. The content of the negative electrode active material in the negative electrode mixture layer was 25 mass %, and the weight per unit area of the negative electrode was 1.8 mg / cm. 2 A flat all-solid-state secondary battery was produced in the same manner as in Example 1, except that this negative electrode was used.
[0097] Comparative Example 4 A negative electrode was produced in the same manner as in Example 1, except that the ratio of the negative electrode active material to the binder resin in the slurry was changed to 3:1 by mass. The content of the negative electrode active material in the negative electrode mixture layer was 75 mass %, and the weight per unit area of the negative electrode was 1.5 mg / cm. 2 A flat all-solid-state secondary battery was produced in the same manner as in Example 1, except that this negative electrode was used.
[0098] Comparative Example 5 A flat all-solid-state secondary battery was produced in the same manner as in Example 1, except that a negative electrode mixture layer was not formed on the copper foil, and the copper foil having a thickness of 8 μm was used as the negative electrode as it was.
[0099] The coulombic efficiency of the batteries of the examples and comparative examples was measured as follows. A program was created in which each battery was charged at a constant current of 0.01C based on the positive electrode active material, and when the upper limit voltage (4.3V) was reached, constant voltage charging was performed, and each battery was charged using this program. The total time of constant current charging and constant voltage charging was 100 hours, and even if an internal short circuit occurred during constant current charging or constant voltage charging and the battery voltage dropped, charging was continued for 100 hours without regard to this. After measuring the open circuit voltage for 10 minutes for each battery after charging, a constant current discharge was performed at 0.1C to determine the discharge capacity. The value of the discharge capacity / the charge capacity was calculated as the coulombic efficiency (charge / discharge efficiency). These evaluation results are shown in Table 1 together with the configuration of the negative electrode and the heat treatment temperature of the battery.
[0100] [Table 1]
[0101] As shown in Table 1, the flat all-solid-state secondary batteries of Examples 1 and 2, which have negative electrodes with appropriate average particle diameters of the negative electrode active material and binder resin content ratios, exhibited higher Coulombic efficiency than the batteries of Comparative Examples 1 to 5, which had inappropriate values for these values. [Explanation of symbols]
[0102] 1,100 All-solid-state secondary battery 10 positive electrode 20 negative electrode 30 Solid electrolyte layer 40 Outer can 50 sealed cans 60 Gasket 200 Electrode body 300 Positive external terminal 400 Negative external terminal 500 Laminated film exterior
Claims
1. A negative electrode for use in an all-solid-state secondary battery having a solid electrolyte layer, The negative electrode mixture layer includes graphite as a negative electrode active material and a binder resin having an ethylene oxide structure in its molecule, and the negative electrode mixture layer is disposed on a current collector. The average particle size of the graphite is 12 μm or less, The negative electrode for an all-solid-state secondary battery, wherein the content of the binder resin in the negative electrode mixture layer is 30 to 70 mass %.
2. 2. The negative electrode for an all-solid-state secondary battery according to claim 1, wherein the graphite has an average particle size of 1 μm or more.
3. 2. The negative electrode for an all-solid-state secondary battery according to claim 1, wherein the binder resin has an ethylene oxide structure content of 0.05 mass % or more.
4. An all-solid-state secondary battery having at least one electrode laminate in which a negative electrode and a positive electrode face each other via a solid electrolyte layer, An all-solid-state secondary battery comprising the anode for an all-solid-state secondary battery according to any one of claims 1 to 3 as the anode.
5. In the Raman spectrum of the negative electrode in a charged state, -1 Li in the area 2 C 2 The all-solid-state secondary battery according to claim 4 , having a peak attributable to