Rubber-metal laminated gasket material
The use of p,p'-dibenzoylquinone dioxime and N,N'-m-phenylene dimaleimide crosslinking agents in rubber-metal laminated gasket materials addresses the challenge of forming a highly crosslinked rubber layer under atmospheric conditions, enhancing sealing performance and reducing costs.
Patent Information
- Application Number
- JP2023072916
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing rubber-metal laminated gasket materials face challenges in forming a highly crosslinked rubber layer under atmospheric conditions without using organic peroxide as a crosslinking agent, leading to decreased sealing performance due to deformation under compressive stress.
A rubber-metal laminated gasket material is developed using p,p'-dibenzoylquinone dioxime and N,N'-m-phenylene dimaleimide crosslinking agents with hydrogenated nitrile rubber, allowing crosslinking under atmospheric conditions, enhancing the crosslinking degree and reducing material costs.
The solution achieves a highly crosslinked rubber layer with improved sealing performance and reduced material costs, maintaining sealing integrity under stress and eliminating rubber peeling issues.
Smart Images

Figure 2024158066000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber-metal laminate gasket material, and more particularly to a rubber-metal laminate gasket material in which a highly cross-linked rubber layer is formed on a metal plate in the air without using an organic peroxide as a cross-linking agent. [Background technology]
[0002] Rubber-metal laminated gasket materials, in which (hydrogenated) nitrile rubber or fluororubber is laminated on one or both sides of a metal plate, are subjected to strong compressive stress on the rubber laminate surface. If the rubber cannot withstand this fastening stress and deforms, the surface pressure will decrease, making it difficult to achieve the intended sealing function.
[0003] In such rubber-metal laminated gasket materials, fluororubber is often used in the rubber layer of cylinder head gaskets, which serve as a part for sealing between the engine and the block, to ensure heat resistance. However, due to the unstable supply of fluororubber raw materials and the soaring prices in recent years, there is a demand for cheaper materials with a more stable supply.
[0004] Here, as disclosed in Patent Documents 1 and 2, organic peroxide crosslinking using a peroxide such as hydrogenated nitrile rubber is effective in obtaining high heat resistance. However, organic peroxide crosslinking does not proceed unless in a sealed environment or in the absence of oxygen. Therefore, if the reaction site can be kept under an inert gas atmosphere at all times, peroxide crosslinking can be performed in an open space. However, this requires the continuous supply of a specified inert gas, which increases the production cost of the rubber molded body.
[0005] In light of the above circumstances, there is a demand for a rubber-metal laminate gasket material that is produced without using an organic peroxide crosslinking agent. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] WO 2019 / 093081 A1 [Patent Document 2] WO 2020 / 175151 A1 [Patent Document 3] Japanese Patent Application Publication No. 7-165953 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a rubber-metal laminate gasket material in which a rubber layer with a high degree of cross-linking is formed on a metal plate in the air without using an organic peroxide as a cross-linking agent for the rubber. [Means for solving the problem]
[0008] The object of the present invention is achieved by a rubber-metal laminated gasket material in which a crosslinked rubber layer of a hydrogenated nitrile rubber composition containing 1 to 30 parts by weight of a p,p'-dibenzoylquinone dioxime crosslinking agent and 10 parts by weight or less of an N,N'-m-phenylenedimaleimide crosslinking aid per 100 parts by weight of hydrogenated nitrile rubber is formed on a metal plate. Effect of the Invention
[0009] By using p,p'-dibenzoylquinone dioxime as a crosslinking agent for hydrogenated nitrile rubber, and preferably further blending N,N'-m-phenylenedimaleimide crosslinking aid, it is possible to obtain rubber with a high degree of crosslinking in the air.
[0010] Another advantage of hydrogenated nitrile rubber is that it is less expensive than fluororubber.
[0011] By forming a crosslinked rubber layer of such a rubber composition on a metal plate, it is possible to obtain an excellent effect of forming a gasket material having a high degree of crosslinking of the rubber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] When used as a gasket material, the metal plate may be a mild steel plate, a stainless steel plate, an aluminum plate, an aluminum die-cast plate, or the like. The stainless steel plate may be SUS301, SUS301H, SUS304, SUS430, or the like. The plate thickness is generally about 0.1 to 2 mm, since it is used as a gasket. In this case, the metal plate is preferably used after surface roughening and / or alkaline degreasing.
[0013] A primer layer is preferably formed on the metal plate. As the primer layer, generally commercially available chemical solutions or known techniques can be used as they are, such as Ti / Al-based coatings, zinc phosphate coatings, iron phosphate coatings, coating-type chromate coatings, compounds of metals such as vanadium, zirconium, titanium, molybdenum, tungsten, manganese, zinc, and cerium, inorganic coatings such as oxides of these metals, and organic coatings such as silane, phenolic resin, epoxy resin, and polyurethane, but preferably, a primer layer containing an organometallic compound having at least one chelate ring and an alkoxyl group, a primer layer to which a metal oxide or silica is further added, and more preferably, a primer layer to which a hydrolysis condensation product of an amino group-containing alkoxysilane and a vinyl group-containing alkoxysilane is added to these primer layer forming components is used. This hydrolysis condensation product can also be used alone.
[0014] Examples of the organometallic compound include organoaluminum compounds such as ethyl acetoacetate aluminum diisopropylate, aluminum tris(ethyl acetoacetate), aluminum monoacetylacetonate bis(ethyl acetoacetate), and aluminum tris(acetylacetate); organo-titanium compounds such as isopropoxytitanium bis(ethyl acetoacetate), 1,3-propanedioxytitanium bis(ethyl acetoacetate), diisopropoxytitanium bis(acetylacetonate), and titanium tetra(acetylacetonate); and organo-zirconium compounds such as di-n-butoxyzirconium bis(acetylacetonate) and di-n-butoxyzirconium bis(ethyl acetoacetate). Preferably, the compounds are represented by the general formula: TIFF2024158066000001.tif84166R: Lower alkyl groups such as CH3, C2H5, n-C3H7, i-C3H7, n-C4H9, and i-C4H9 n: an integer between 1 and 4 An organic titanium compound having a chelate ring represented by the following formula and an alkoxyl group is used.
[0015] The surface treatment agent that forms the primer layer is applied to the metal sheet surface at a rate of approximately 30 to 1,000 mg / m by immersion, spraying, brush printing, roll coating, or other methods. 2 , preferably about 100 to 1,000 mg / m 2 After drying at room temperature or with hot air, it is baked at about 100 to 250°C for about 1 to 20 minutes.
[0016] On the primer layer applied to the metal plate and dried, a resin-based vulcanizing adhesive such as a thermosetting phenolic resin or an epoxy resin is applied as a rubber adhesive. As the thermosetting phenolic resin, any thermosetting phenolic resin such as cresol novolac type phenolic resin, cresol resol type phenolic resin, or alkyl-modified type phenolic resin can be used. As the epoxy resin, a cresol novolac type epoxy resin is preferably used, and in this case, a bisphenol novolac type phenolic resin is used as a curing agent, and an imidazole compound is used as a curing catalyst.
[0017] These resin-based vulcanizing adhesives are generally prepared as organic solvent solutions with component concentrations of about 1 to 5% by weight using alcohol-based organic solvents such as methanol, ethanol, isopropanol, etc., or ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, etc., either alone or in a mixture. They are applied in a manner similar to that for surface treatment agents, and are applied at a concentration of about 100 to 2,500 mg / m 2 After drying at room temperature or with hot air, the coating is baked at about 100 to 250°C for about 1 to 20 minutes.
[0018] Onto the vulcanized adhesive layer thus formed, an unvulcanized rubber compound is applied in the form of a solution in an organic solvent, such as alcohols (e.g., methanol, ethanol, etc.), ketones (e.g., methyl ethyl ketone, methyl isobutyl ketone, etc.), aromatic hydrocarbons (e.g., toluene, xylene, etc.), or a mixture of these.
[0019] The applied unvulcanized rubber layer is dried at room temperature or about 100°C for about 1 to 15 minutes, and after the organic solvent has been evaporated, it is heated and vulcanized at about 150 to 230°C for about 0.5 to 30 minutes, during which pressure may also be applied for vulcanization as necessary.
[0020] The hydrogenated nitrile rubber may have any degree of hydrogenation. For example, commercially available products such as Terban 3446 manufactured by LANXESS and Zanvar ZN35256 manufactured by Zannan may be used as they are.
[0021] The p,p'-dibenzoylquinone dioxime crosslinking agent is used in a ratio of 1 to 30 parts by weight, preferably 5 to 20 parts by weight, per 100 parts by weight of hydrogenated nitrile rubber. If the p,p'-dibenzoylquinone dioxime crosslinking agent is used in a ratio less than this, sufficient crosslinking cannot be performed, and the rubber will dissolve when immersed in KOS-2 oil or the like. On the other hand, if it is used in a ratio greater than this, the time it takes for the rubber paste to solidify will be shortened, the rubber paste life will not be satisfied, and it will solidify in a few hours, making its production difficult.
[0022] In the hydrogenated nitrile rubber composition containing the p,p'-dibenzoylquinone dioxime crosslinking agent, preferably, an N,N'-m-phenylenedimaleimide crosslinking aid can be further used in an amount of 10 parts by weight or less, preferably 2 to 8 parts by weight, per 100 parts by weight of the hydrogenated nitrile rubber. If the N,N'-m-phenylenedimaleimide crosslinking aid is used in a proportion greater than this, the time until the rubber paste solidifies becomes shorter, the rubber paste life cannot be satisfied, and the rubber paste solidifies within a few hours, making production difficult.
[0023] The hydrogenated nitrile rubber composition consisting of the above components contains magnesium oxide in an amount of about 7 parts by weight or less, preferably about 3 to 5 parts by weight, per 100 parts by weight of hydrogenated nitrile rubber. By adding magnesium oxide in a specific ratio, roll processability during kneading is improved, and bagging can be suppressed. However, if magnesium oxide is used in a ratio greater than this, adhesion to the roll increases, and workability deteriorates.
[0024] The average particle size of the magnesium oxide is not particularly limited, and for example, magnesium oxide having a particle size of about 1.0 to 30.0 μm may be used. In addition, the magnesium oxide may be surface-treated, such as with a fatty acid.
[0025] From the viewpoint of blister resistance against water or LLC, it is preferable to mix about 70 to 150 parts by weight of titanium oxide per 100 parts by weight of hydrogenated nitrile rubber. However, if the mixing ratio is more than this, the rubber hardness becomes too high and the sealing property deteriorates. The average particle size of titanium oxide is not particularly limited, and for example, about 0.15 to 0.30 μm is used.
[0026] By incorporating titanium oxide, the blister resistance of vulcanization-molded cylinder head gaskets and the like can be improved, eliminating the problem of rubber peeling from the gasket inside the engine and improving the problem.
[0027] The use of other fillers such as calcium carbonate and silica is permitted as long as it does not impair the object of the present invention. In order to ensure sealing properties, it is preferable that the D hardness measured with a JIS D durometer corresponding to ISO 7619-1 is 35 or more and 65 or less.
[0028] The organic solvent solution of the hydrogenated nitrile rubber composition containing the above components is formed on a metal plate as a crosslinked rubber layer having a laminated rubber thickness of about 10 to 125 μm, preferably 15 to 65 μm. If the laminated rubber thickness is thinner than this, it becomes difficult to maintain the sealing property, while if it is thicker than this, the rubber is likely to flow.
[0029] If necessary, an anti-tack agent can be applied to the surface of the crosslinked rubber layer. The anti-tack agent is used for the purpose of preventing adhesion between rubbers or between rubber and metal, and any agent can be used as long as it can form a coating on the vulcanized rubber layer, such as silicone-based, fluorine-based, graphite-based, amide, paraffin or other wax-based, polyolefin-based or polybutadiene-based agents, but preferably an anti-tack agent consisting of a liquid 1,2-polybutadiene hydroxyl group-containing material, 1,2-polybutadiene isocyanate group-containing material, and an organic solvent dispersion of a polyolefin-based resin is used (Patent Document 3). EXAMPLES
[0030] The present invention will now be described with reference to examples.
[0031] Examples 1 to 7, Comparative Examples 1 to 4 A Ti / Al primer (Ti compound: Matsumoto Fine Chemical's ORGATIX TC-100 / Al compound: Nissan Chemical Industries' AS-520-A; weight ratio 40:60) was applied to both sides of a degreased stainless steel plate (0.2 mm thick) and baked at 200°C for 10 minutes to form a lower primer layer. An adhesive mainly composed of epoxy resin was applied to the lower primer layer and baked at 200°C for 5 minutes to form a cover coat layer. A rubber paste coating liquid was applied to the cover coat layer and vulcanized at 215°C for 12 minutes to form a rubber layer, producing a rubber-metal laminated gasket material.
[0032] The rubber cement coating liquid has the following composition: Hydrogenated nitrile rubber (LANXESS product Telban 3446) 100 parts by weight Carbon black (Tokai Carbon Products Seast GS) 85 〃 Titanium oxide (Ishihara Sangyo Co., Ltd. product Type A100) 130 Same Magnesium oxide (Kyowa Chemical Products #150) 4 Same Stearic acid (Miyoshi Oil Products DTST) 1 〃 Anti-aging agent (Ouchi Shinko Chemical Products Nocrac ODA) 2 Same p,p'-Dibenzoylquinonedioxime crosslinking agent Specified amount Same (Ouchi Shinko Chemical Products Barnoc DGM) N,N'-m-phenylenedimaleimide crosslinking agent Specified amount Same (Ouchi Shinko Chemical Products Barnoc PM) The above components were kneaded using a kneader and an open roll, and the resulting kneaded product (composition) was dissolved and dispersed in a mixed solvent of toluene and methyl ethyl ketone to prepare a rubber paste coating liquid with a solid content concentration of 20% by weight.
[0033] The produced gasket materials were evaluated and measured for the following items. Rubber thickness change rate: Rubber-metal laminated gasket material, Osaka Organic Chemical Industry Co., Ltd. KOS-2 The rubber was immersed in oil at 100°C for 4 hours, and the degree of cross-linking was measured before and after the test. Measure the thickness change rate Preferably 60% or less Martens hardness: Shimadzu Dynamic Ultra Micro Hardness Tester DUH-211S was used to measure rubber Metal laminated gasket material, load speed 1.48mN / sec, indentation Tests were conducted at a depth of 5 μm to measure the microhardness of the rubber layer surface. 5~30N / mm 2 It is preferable that Rubber glue life: Measure the time it takes for the rubber glue to harden after the rubber material is dissolved. Preferably 168 hours or more
[0034] The results obtained are shown in the following Tables 1 and 2. In Comparative Example 1, the rubber layer dissolved, and the rubber thickness could not be measured. Table 1 Working Example 1 2 3 4 5 6 7 [Additional ingredients] Barnoc DGM 5 5 15 20 20 1 30 Barnoc PM 0 5 5 0 3 10 10 [Measurement results] Rubber thickness change rate (%) 51 48 23 18 17 58 13 Martens hardness (N / mm 2 ) 8.5 13.2 17.2 22.1 27.5 5.2 30.3 Rubber glue life (hours) ≧168 ≧168 ≧168 ≧168 ≧168 ≧168 ≧168 Table 2 Comparative Example 12 3 4 [Additional ingredients] Barnock DGM 0 30 35 35 Barnoc PM 10 15 5 15 [Measurement results] Rubber thickness change rate (%) - 14 16 13 Martens hardness (N / mm 2 ) 3.8 30.1 23.4 32.1 Rubber glue life (hours) ≧168 16 16 16
Claims
1. A rubber-metal laminated gasket material in which a crosslinked rubber layer of a hydrogenated nitrile rubber composition is formed on a metal plate, the crosslinked rubber layer being made of a hydrogenated nitrile rubber composition containing 100 parts by weight of hydrogenated nitrile rubber, 1 to 30 parts by weight of a p,p'-dibenzoylquinone dioxime crosslinking agent, and 10 parts by weight or less of an N,N'-m-phenylenedimaleimide crosslinking aid.
2. 2. The rubber-metal laminate gasket material according to claim 1, further comprising a hydrogenated nitrile rubber composition containing 7 parts by weight or less of magnesium oxide.
3. 3. The rubber-metal laminated gasket material according to claim 1, wherein the thickness of the laminated rubber is 10 to 125 μm.
4. Martens hardness measured using a dynamic microhardness tester is 5 to 30 N / mm 2 3. The rubber-metal laminate gasket material according to claim 1 or 2, which is
5. 3. The rubber-metal laminate gasket material according to claim 1, further comprising a primer layer and a resin-based vulcanized adhesive layer interposed between the metal plate and the crosslinked rubber layer.
6. A cylinder head gasket made of the rubber-metal laminate gasket material according to claim 1 or 2.
Citation Information
Patent Citations
Surface treating agent for cured rubber
JP1995165953A
Gasket material
WO2019093081A1
Hydrogenated NBR composition
WO2020175151A1