Polyol premix, foam, and insulation chamber
The polyol premix with optimized polyol components and catalysts addresses the poor appearance and moldability issues in water-based polyurethane foam production, achieving high-quality foams for thermal storage.
Patent Information
- Application Number
- JP2023073865
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Existing polyurethane foam production methods using water as a blowing agent often result in poor appearance and moldability issues, as fluorocarbon compounds are expensive and have low supply stability, while water-based methods struggle to achieve good appearance and moldability.
A polyol premix comprising specific types and ratios of polyol components, such as sucrose-based polyether polyol B and aromatic amine polyether polyol C, along with a catalyst like amine catalyst A, and a foam stabilizer with moderate foam regulating power, to optimize the reaction and prevent excessive thickening when mixed with a polyisocyanate component.
The solution enables the production of polyurethane foam with improved appearance and moldability using water as a blowing agent, balancing reaction intensity and foam structure to achieve high-quality foams suitable for thermal storage applications.
Smart Images

Figure 2024158563000001 
Figure 2024158563000002 
Figure 2024158563000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyol premix, a foam, and an insulated cabinet, and more specifically to a polyol premix used in the production of polyurethane foam, a foam produced using such a polyol premix, and an insulated cabinet equipped with such a foam. [Background technology]
[0002] Polyurethane refers to a polymeric compound having a urethane bond (-NH-C(O)O-). Polyurethane is generally obtained by polymerizing the hydroxyl group (-OH) of a polyol with the isocyanate group (-NCO) of a polyisocyanate. It is known that polyurethane exhibits a variety of properties by optimizing the type of polyol and / or polyisocyanate. For this reason, polyurethane is used in various automobile parts, synthetic leather, paints, adhesives, etc. In addition, polyurethane foam, which is made by foaming polyurethane, is used in insulation materials, cushioning materials, etc.
[0003] Among polyurethane foams, those containing closed cells are also called rigid polyurethane foams. Rigid polyurethane foams have excellent heat insulating properties and are therefore highly valued as heat insulating materials for use in rice storage, refrigerators, freezers, vending machines, ships, vehicles, plants, building materials, furniture, etc. Various methods for producing such polyurethane foams have been proposed in the past.
[0004] For example, Patent Document 1 states: (a) Block adduct in which PO and EO are added to sucrose in that order (average functionality 8.0, hydroxyl value 28, content of terminal EO units = 20%): 75 parts by mass, (b) Block adduct in which PO and EO are added to glycerin in that order (average functionality 3.0, hydroxyl value 34, content of terminal EO units = 20%): 12 parts by mass, (c) Polymer polyol obtained by copolymerizing acrylonitrile and styrene in a specified polyol (polymer content 30%, acrylonitrile / styrene ratio (weight ratio) = 65 / 35): 13 parts by mass, (d) Water: 2.0 parts by mass, (e) tertiary amine catalyst: 2.0 parts by mass, (f) 70% diethylene glycol solution of bis(N,N-dimethylamino-2-ethyl) ether: 0.5 parts by mass, and (g) Mixing agent for organic modified polysiloxane: 0.5 parts by mass A polyol mixture comprising: The document describes that by reacting such a polyol mixture with a polyisocyanate component, it is possible to produce thin-walled automotive interior materials that have a good feel to the touch.
[0005] Among polyurethane foams, when producing rigid polyurethane foams, fluorocarbon compounds such as hydrofluorocarbons (HFCs) and hydrofluoroolefins (HFOs) are generally used as blowing agents. Fluorocarbon compounds have the advantage that they are excellent in moldability because they do not react with polyisocyanates, and foams with good appearance can be easily obtained. However, fluorocarbon compounds have low supply stability and are expensive.
[0006] On the other hand, a method of using water as a blowing agent in the production of rigid polyurethane foam is also known. Water is highly stable in supply and inexpensive. However, when water is used as a blowing agent, there is a drawback that moldability is inferior to when a fluorocarbon compound is used, and it is difficult to obtain a foam with a good appearance. Furthermore, even when water is contained as a blowing agent, there have been almost no examples proposed to date of polyol premixes capable of producing rigid polyurethane foams having good appearance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6246235 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a novel polyol premix which is capable of producing a polyurethane foam having a good appearance even when water is used as a blowing agent. Another object of the present invention is to provide a foam produced by using such a polyol premix. Furthermore, another problem to be solved by the present invention is to provide a thermal storage unit equipped with such a foam. [Means for solving the problem]
[0009] In order to solve the above problems, the polyol premix according to the present invention comprises: The composition includes a polyol component, a foam stabilizer, a catalyst, and a blowing agent, The polyol component is Polyether polyol A, Sucrose-based polyether polyol B; Aromatic amine polyether polyol C and Including, The catalyst includes an amine catalyst having a hydroxyl value of 200 mgKOH / g or more.
[0010] The foam according to the present invention is obtained by foaming and curing a mixture containing the polyol premix according to the present invention and a polyisocyanate component. Furthermore, the thermal insulation box according to the present invention includes the foam according to the present invention. Effect of the Invention
[0011] In a polyol premix containing a polyol component, a foam stabilizer, a catalyst, and a blowing agent, by optimizing the types of the polyol component and the catalyst, it is possible to obtain a polyurethane foam, particularly a rigid polyurethane foam, having a good appearance even when water is used as the blowing agent. This is believed to be because optimizing the types of the polyol component and the catalyst suppresses excessive reaction between water and polyisocyanate even when the polyol premix and the polyisocyanate component are mixed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] An embodiment of the present invention will be described in detail below. [1. Polyol premix] The polyol premix according to the present invention contains a polyol component, a foam stabilizer, a catalyst, and a blowing agent. The polyol premix may further contain a flame retardant.
[0013] [1.1. Ingredients] [1.1.1. Polyol component] The polyol component is one of the main raw materials for producing polyurethane foam. In the present invention, the polyol component is (a) polyether polyol A; (b) sucrose-based polyether polyol B; (c) aromatic amine-based polyether polyol C; Includes. The polyol component further comprises: (d) Polyether polyol D It may also include.
[0014] [A. Polyether polyol A] The term "polyether polyol A" refers to a polyol obtained by addition polymerization of an alkylene oxide to an initiator consisting of a compound having a functionality of 4.0 or more and 5.0 or less, other than sucrose-based polyether polyol B, aromatic amine-based polyether polyol C, and polyether polyol D.
[0015] The polyether polyol A is in particular (a) the number of functional groups is 4.0 or more and 5.0 or less, (b) The hydroxyl value is 300 mgKOH / g or more and 500 mgKOH / g or less. The one is preferred.
[0016] The number of functional groups of the polyether polyol A affects the moldability and appearance of the polyurethane foam. If the number of functional groups of the polyether polyol A is too small, the curing temperature must be increased, and moldability may deteriorate. In addition, the polyurethane foam may shrink during the cooling process after the reaction. Furthermore, if the number of functional groups of the polyether polyol A is too small, the number of reaction points may decrease, and the mechanical strength of the polyurethane foam may decrease. Therefore, the number of functional groups of the polyether polyol A must be 4.0 or more. The number of functional groups is preferably 4.1 or more, or 4.2 or more. On the other hand, if the number of functional groups of the polyether polyol A is too large, the reaction with the polyisocyanate becomes intense, and voids tend to occur in the polyurethane foam. Therefore, the number of functional groups of the polyether polyol A must be 5.0 or less. The number of functional groups is preferably 4.9 or less, or 4.8 or less.
[0017] The hydroxyl value of polyether polyol A affects the mechanical strength and appearance of polyurethane foam. If the hydroxyl value of polyether polyol A is too small, the number of reaction sites decreases, and the mechanical strength of polyurethane foam may decrease. Therefore, the hydroxyl value of polyether polyol A is preferably 300 mgKOH / g or more. The hydroxyl value is more preferably 350 mgKOH / g or more, or 400 mgKOH / g or more. On the other hand, if the hydroxyl value of polyether polyol A is too large, the reaction with polyisocyanate becomes intense, and the polyurethane foam may have a poor appearance. Therefore, the hydroxyl value of polyether polyol A is preferably 500 mg KOH / g or less. The hydroxyl value is more preferably 490 mg KOH / g or less, or 480 mg KOH / g or less.
[0018] [B. Sucrose-based polyether polyol B] "Sucrose-based polyether polyol B" refers to a polyol obtained by addition polymerization of alkylene oxide to sucrose, and is other than polyether polyol A, aromatic amine-based polyether polyol C, and polyether polyol D.
[0019] The sucrose-based polyether polyol B is, in particular, (a) the number of functional groups is 4.0 or more and 5.5 or less, (b) The hydroxyl value is 300 mgKOH / g or more and 500 mgKOH / g or less. The one is preferred.
[0020] The number of functional groups of the sucrose-based polyether polyol B affects the mechanical strength and appearance of the polyurethane foam. If the number of functional groups of the sucrose-based polyether polyol B is too small, the number of reaction sites will be small, and the mechanical strength of the polyurethane foam may decrease. In addition, the polyurethane foam may shrink during the cooling process after the reaction. Therefore, the number of functional groups of the sucrose-based polyether polyol B is preferably 4.0 or more. The number of functional groups is more preferably 4.1 or more, or 4.2 or more. On the other hand, if the number of functional groups of the sucrose-based polyether polyol B is too large, the reaction with the polyisocyanate becomes intense, and the polyurethane foam may have a poor appearance. Therefore, the number of functional groups of the sucrose-based polyether polyol B is preferably 5.5 or less. The number of functional groups is more preferably 5.4 or less, or 5.3 or less.
[0021] The hydroxyl value of the sucrose-based polyether polyol B affects the mechanical strength and appearance of the polyurethane foam. If the hydroxyl value of the sucrose-based polyether polyol B is too small, the number of reaction sites decreases, and the mechanical strength of the polyurethane foam may decrease. Therefore, the hydroxyl value of the sucrose-based polyether polyol B is preferably 300 mgKOH / g or more. The hydroxyl value is more preferably 350 mgKOH / g or more, or 400 mgKOH / g or more. On the other hand, if the hydroxyl value of the sucrose-based polyether polyol B is too large, the reaction with the polyisocyanate becomes intense, and the polyurethane foam may have a poor appearance. Therefore, the hydroxyl value of the sucrose-based polyether polyol B is preferably 500 mg KOH / g or less. The hydroxyl value is more preferably 490 mg KOH / g or less, or 480 mg KOH / g or less.
[0022] The sucrose-based polyether polyol B preferably contains 20 mass% or more of propylene oxide units. The content of propylene oxide units is more preferably 25 mass% or more, or 30 mass% or more. When the sucrose-based polyether polyol B that satisfies such conditions is used, it becomes easier to suppress the appearance defects of the polyurethane foam. However, if the content of propylene oxide units is excessive, it may cause a decrease in the mechanical strength of the polyurethane foam. Therefore, the content of propylene oxide units is preferably 70 mass% or less. The content of propylene oxide units is more preferably 60 mass% or less, or 50 mass% or less.
[0023] [C. Aromatic amine-based polyether polyol C] The term “aromatic amine-based polyether polyol C” refers to a polyol obtained by addition polymerization of an alkylene oxide to an aromatic amine, and is other than polyether polyol A, sucrose-based polyether polyol B, and polyether polyol D.
[0024] The aromatic amine-based polyether polyol C is, in particular, (a) the number of functional groups is 3.0 or more and 5.0 or less, (b) The hydroxyl value is 300 mgKOH / g or more and 500 mgKOH / g or less. The one is preferred.
[0025] The number of functional groups of the aromatic amine-based polyether polyol C affects the moldability and appearance of the polyurethane foam. If the number of functional groups of the aromatic amine-based polyether polyol C is too small, the mechanical strength of the polyurethane foam may decrease, or the polyurethane foam may shrink during the cooling process after the reaction. Therefore, the number of functional groups of the aromatic amine-based polyether polyol C is preferably 3.0 or more. The number of functional groups is more preferably 3.5 or more, or 3.7 or more. On the other hand, if the number of functional groups of the aromatic amine-based polyether polyol C is too large, the polyurethane foam may have poor appearance. Therefore, the number of functional groups of the aromatic amine-based polyether polyol C is preferably 5.0 or less. The number of functional groups is more preferably 4.5 or less, or 4.3 or less.
[0026] The hydroxyl value of the aromatic amine-based polyether polyol C affects the mechanical strength and appearance of the polyurethane foam. If the hydroxyl value of the aromatic amine-based polyether polyol C is too small, the number of reaction points decreases, and the mechanical strength of the polyurethane foam may decrease. Therefore, the hydroxyl value of the aromatic amine-based polyether polyol C is preferably 300 mgKOH / g or more. The hydroxyl value is more preferably 350 mgKOH / g or more, or 400 mgKOH / g or more. On the other hand, if the hydroxyl value of the aromatic amine-based polyether polyol C is too large, the reaction with the polyisocyanate becomes intense, and the polyurethane foam may have a poor appearance. Therefore, the hydroxyl value of the aromatic amine-based polyether polyol C is preferably 500 mgKOH / g or less. The hydroxyl value is more preferably 490 mgKOH / g or less, or 480 mgKOH / g or less.
[0027] [D. Polyether polyol D] "Polyether polyol D" refers to a compound obtained by addition polymerization of an alkylene oxide to an initiator consisting of a compound having a functional group number of 2.1 or more and 3.5 or less, and is other than polyether polyol A, sucrose-based polyether polyol B, and aromatic amine-based polyether polyol C.
[0028] The polyether polyols D are in particular (a) the number of functional groups is 2.1 or more and 3.5 or less, (b) a hydroxyl value of 150 mgKOH / g or more and 500 mgKOH / g or less The one is preferred.
[0029] The number of functional groups of polyether polyol D affects the mechanical strength, appearance, fluidity, and degree of shrinkage of polyurethane foam. If the number of functional groups of polyether polyol D is too small, the mechanical strength of polyurethane foam may decrease, or the polyurethane foam may shrink during the cooling process after the reaction. Therefore, the number of functional groups of polyether polyol D must be 2.1 or more. The number of functional groups is preferably 2.5 or more, or 2.7 or more. On the other hand, if the number of functional groups of the polyether polyol D is too large, the polyurethane foam may have a poor appearance, or the flowability of the raw material mixture may decrease when the polyol premix is mixed with the polyisocyanate component. Therefore, the number of functional groups of the polyether polyol D must be 3.5 or less. The number of functional groups is preferably 3.4 or less, or 3.3 or less.
[0030] The hydroxyl value of polyether polyol D affects the appearance and mechanical strength of polyurethane foam. If the hydroxyl value of polyether polyol D is too small, the number of reaction sites decreases, and the mechanical strength of polyurethane foam may decrease. Therefore, the hydroxyl value of polyether polyol D is preferably 150 mgKOH / g or more. The hydroxyl value is more preferably 200 mgKOH / g or more, 300 mgKOH / g or more, or 400 mgKOH / g or more. On the other hand, if the hydroxyl value of polyether polyol D is too large, the reaction with polyisocyanate becomes intense, and the polyurethane foam may have a poor appearance. Therefore, the hydroxyl value of polyether polyol D is preferably 500 mg KOH / g or less. The hydroxyl value is more preferably 490 mg KOH / g or less, or 480 mg KOH / g or less.
[0031] [1.1.2. Foam stabilizer] The foam stabilizer is used to increase the compatibility of the raw materials and to reduce the surface tension of the raw material mixture, as well as to stabilize bubbles and adjust the bubble structure.
[0032] The type of foam stabilizer affects the cell size within the polyurethane foam. If a foam stabilizer with excessively strong foam-stabilizing power (a foam stabilizer that acts to reduce cell size) is used, the polyurethane foam's insulating properties will increase, but the polyurethane foam's dimensional changes will be greater, making it more likely to have poor appearance. In contrast, when a foam stabilizer having an appropriate foam-stabilizing ability is used, the cell size becomes slightly larger and the heat insulating property is slightly decreased, but the appearance defect is less likely to occur.
[0033] In the present invention, the type of foam stabilizer is not particularly limited, but the foam stabilizer is preferably a silicone-based foam stabilizer. In order to suppress poor appearance, the foam stabilizer preferably contains a compound having a hydroxyl group at the molecular end.
[0034] In order to prevent poor appearance, the foam stabilizer is (a) polyalkylene oxide-methylsiloxane copolymer (OR terminal), (b) dimethylpolysiloxane-polyoxyalkylene copolymer (OH-terminated), and (c) Dimethylpolysiloxane-polyoxyalkylene copolymer (OR terminal) At least one selected from the group consisting of is preferred. These have a moderate foam-stabilizing power and are therefore effective in suppressing poor appearance. Dimethylpolysiloxane-polyoxyalkylene copolymer (OH terminal) is particularly preferred as the foam stabilizer.
[0035] Catalyst The polyol premix according to the present invention contains an amine catalyst A as a catalyst. "Amine catalyst A" refers to a catalyst made of an amine compound having a hydroxyl value of 200 mgKOH / g or more.
[0036] Polyol premix contains, in addition to amine catalyst A, (a) a foaming catalyst, and / or (b) Triazine catalyst It may further include.
[0037] [A. Amine catalyst A] The amine catalyst A is a resinification catalyst (a catalyst that contributes more to the resinification reaction than to the foaming reaction). When the amine catalyst A is used as the resinification catalyst, the polyurethane foam is less likely to have poor appearance compared to when a resinification catalyst other than the amine catalyst A is used.
[0038] The hydroxyl value of the amine catalyst A affects the appearance of the polyurethane foam. If the hydroxyl value of the amine catalyst A is too small, the appearance may be poor. Therefore, the hydroxyl value of the amine catalyst A must be 200 mg KOH / g or more. The hydroxyl value is preferably 210 mg KOH / g or more. On the other hand, if the hydroxyl value of the amine catalyst A is too large, the polyurethane foam may have a poor appearance. Therefore, the hydroxyl value of the amine catalyst A is preferably 500 mgKOH / g or less. The hydroxyl value is more preferably 300 mgKOH / g or less, or 250 mgKOH / g or less.
[0039] The weight average molecular weight of the amine catalyst A affects the appearance of the polyurethane foam. If the weight average molecular weight of the amine catalyst A is too small, the polyurethane foam may have poor appearance. Therefore, the weight average molecular weight of the amine catalyst A is preferably 300 or more. The weight average molecular weight is preferably 400 or more, or 500 or more. On the other hand, if the weight average molecular weight of the amine catalyst A is too large, poor appearance may occur. Therefore, the weight average molecular weight of the amine catalyst A is preferably 2000 or less. The weight average molecular weight is more preferably 1000 or less, or 700 or less.
[0040] Examples of the amine catalyst A include (a) Methylamine-1,6-hexanediol polycondensate (HO-[R1-N(R2)] n -R1-OH, where R1 is a hexamethylene group, R2 is a methyl group, n is 3.5 (average degree of polymerization), and hydroxyl value: 217 mg KOH / g; (b) N,N-dimethylaminohexanol (hydroxyl value: 380 mg KOH / g), etc.
[0041] [B. Foaming catalyst] When water is used as the blowing agent, the polyol premix preferably further contains a foaming catalyst (a catalyst that contributes more to the foaming reaction than to the resinification reaction) as a catalyst. In the present invention, the type of foaming catalyst is not particularly limited, and an optimal catalyst can be selected depending on the purpose.
[0042] Examples of the foaming catalyst include: (a) bis(2-dimethylaminoethyl) ether, (b) 2,3-dimorpholinodiethyl ether, (c) pentamethyldiethylenetriamine, etc.
[0043] [C. Triazine catalysts] The triazine catalyst is a type of resinification catalyst. The polyol premix may further contain a triazine catalyst as a catalyst. The triazine catalyst has the effect of further improving the curing property when the polyol premix is reacted with the polyisocyanate. Examples of triazine catalysts include: (a) N,N',N"-dimethylaminopropylhexahydrotriazine, (b) hexahydrotriazine, etc.
[0044] [1.1.4. Foaming agents] The term "foaming agent" refers to an additive for generating bubbles in the raw material mixture during the process in which the liquid raw material mixture is resinified. In the present invention, the blowing agent is (a) A physical blowing agent that generates gas upon pressure reduction or heating; or (b) Chemical foaming agents that generate gas by thermal decomposition or chemical reaction Either of the above may be used.
[0045] Examples of physical foaming agents include: (a-1) Hydrocarbons such as cyclopentane, isopentane, and normal pentane, (a-2) Halogen-based compounds such as methylene chloride, trichlorofluoromethane, dichlorodifluoromethane, nonafluorobutyl methyl ether, pentafluoroethyl methyl ether, and pentafluoroisopropyl methyl ether; (a-3) Hydrofluoroolefins (HFOs), hydrochloroolefins (HCFOs), hydrofluorocarbons (HFCs) etc.
[0046] Examples of chemical foaming agents include: (b-1) Water that reacts with isocyanate groups to generate CO2; (b-2) Azodicarbonamide that generates nitrogen, carbon monoxide, carbon dioxide, or ammonia gas upon thermal decomposition etc.
[0047] Among these, the blowing agent is preferably water, which is suitable as a blowing agent because it has high supply stability and is inexpensive. The polyol premix preferably contains only water as a blowing agent, but may contain a blowing agent other than water instead of or in addition to water.
[0048] [1.1.5. Flame retardants] The polyol premix may further contain a flame retardant. The type of flame retardant is not particularly limited, and an optimal one can be selected depending on the purpose. Examples of flame retardants include: (a) phosphorus-based flame retardants such as phosphoric acid esters, red phosphorus, and phosphate-containing flame retardants, such as tris(1-chloro-2-propyl)phosphate and triethylphosphate; (b) Bromine-containing flame retardants; (c) boron-containing flame retardants; (d) antimony-containing flame retardants; (e) metal hydroxides, etc.
[0049] [1.2. Content] [1.2.1. Polyol component] In the present invention, the "content (mass %)" of the ith polyol (i≧1) contained in the polyol component refers to the proportion of the mass of the ith polyol to the total mass of the polyol component.
[0050] [A. Content of polyether polyol A] If the content of polyether polyol A is too low, the viscosity of the polyol premix increases excessively, and the polyurethane foam may have poor appearance or poor physical properties due to poor mixing of the raw materials. Therefore, the content of polyether polyol A is preferably 60.0 mass% or more. The content is more preferably 65.0 mass% or more, or 70.0 mass% or more. On the other hand, if the content of polyether polyol A is excessive, the mechanical strength of the polyurethane foam may decrease, and therefore the content of polyether polyol A is preferably 90.0 mass% or less.
[0051] [B. Content of sucrose-based polyether polyol B] If the content of sucrose-based polyether polyol B is too low, the mechanical strength of the polyurethane foam may decrease. Therefore, the content of sucrose-based polyether polyol B is preferably 1.0 mass% or more. The content is more preferably 3.0 mass% or more, or 5.0 mass% or more. On the other hand, if the content of sucrose-based polyether polyol B is excessive, the polyurethane foam may have poor appearance. Therefore, the content of sucrose-based polyether polyol B is preferably 25.0 mass% or less. The content is more preferably 20.0 mass% or less, 15.0 mass% or less, or 10.0 mass% or less.
[0052] [C. Content of aromatic amine-based polyether polyol C] If the content of aromatic amine-based polyether polyol C is too low, the curability of the polyol premix may decrease. Therefore, the content of aromatic amine-based polyether polyol C is preferably 1.0 mass% or more. The content is more preferably 3.0 mass% or more, or 5.0 mass% or more. On the other hand, if the content of aromatic amine-based polyether polyol C is excessive, the polyurethane foam may have poor appearance. Therefore, the content of aromatic amine-based polyether polyol C is preferably 25.0 mass% or less. The content is more preferably 20.0 mass% or less, 15.0 mass% or less, or 10.0 mass% or less.
[0053] [D. Content of polyether polyol D] The content of polyether polyol D may be zero. In general, the higher the content of polyether polyol D, the lower the viscosity of the polyol premix, and the less likely the polyurethane foam will have poor appearance. In order to obtain such an effect, the content of polyether polyol D is preferably 5.0 mass% or more. The content is more preferably 6.0 mass% or more. On the other hand, if the content of polyether polyol D is excessive, the mechanical strength of the polyurethane foam may decrease. Therefore, the content of polyether polyol D is preferably 10.0 mass% or less. The content is more preferably 9.0 mass% or less, or 8.0 mass% or less.
[0054] [1.2.2. Components other than polyols] The "content (parts by mass)" of components other than polyol contained in the polyol premix (foam stabilizer, amine catalyst A, foaming catalyst, triazine catalyst, blowing agent, flame retardant, etc.) refers to the mass of the components other than polyol when the total mass of the polyol components is taken as 100.
[0055] [A. Content of foam stabilizer] If the content of the foam stabilizer is too low, the polyurethane foam may have a poor appearance, and therefore the content of the foam stabilizer is preferably 3.0 parts by mass or more. On the other hand, if the content of the foam stabilizer is excessive, the flame retardancy may decrease. Therefore, the content of the foam stabilizer is preferably 6.0 parts by mass or less. The content is more preferably 5.0 parts by mass or less, or 4.0 parts by mass or less.
[0056] [B. Content of amine catalyst A] If the content of the amine catalyst A is too low, the polyurethane foam may have poor appearance. Therefore, the content of the amine catalyst A is preferably 1.0 part by mass or more. The content is more preferably 2.0 parts by mass or more, or 3.0 parts by mass or more. Similarly, if the content of the amine catalyst A is excessive, the polyurethane foam may have poor appearance. Therefore, the content of the amine catalyst A is preferably 10.0 parts by mass or less. The content is more preferably 7.0 parts by mass or less, or 4.0 parts by mass or less.
[0057] [C. Foaming catalyst content] When water is used as a blowing agent, if the content of the foaming catalyst is too small, the flowability of the raw material mixture when the polyol premix and the polyisocyanate component are mixed may decrease. Therefore, the content of the foaming catalyst is preferably 0.1 parts by mass or more. The content is more preferably 0.2 parts by mass or more. On the other hand, if the content of the foaming catalyst is excessive, the polyurethane foam may have a poor appearance. Therefore, the content of the foaming catalyst is preferably 1.0 part by mass or less. The content is more preferably 0.5 part by mass or less.
[0058] [D. Triazine catalyst content] The content of the triazine-based catalyst may be zero. However, when a triazine-based catalyst is further added to the polyol premix, the curability of the polyurethane foam may be improved. In order to obtain high curability, the content of the triazine-based catalyst is preferably 0.2 parts by mass or more. On the other hand, if the content of the triazine-based catalyst is excessive, the polyurethane foam may have poor appearance. Therefore, the content of the triazine-based catalyst is preferably 0.4 parts by mass or less. The content is more preferably 0.3 parts by mass or less.
[0059] [E. Water (foaming agent) content] When water is used as a blowing agent, if the water content is too low, the density of the polyurethane foam may become excessively high. Therefore, the water content is preferably 1.0 part by mass or more. The content is more preferably 3.0 parts by mass or more, or 5.0 parts by mass or more. On the other hand, if the water content is excessive, the density may be excessively low, and the mechanical strength may be reduced. In addition, when a polyurethane foam is formed on the surface of a substrate, the adhesion between the substrate and the polyurethane foam may be reduced. Therefore, the water content is preferably 15.0 parts by mass or less. The content is more preferably 10.0 parts by mass or less, or 7.0 parts by mass or less.
[0060] [F. Flame retardant content] The content of the flame retardant may be zero. However, if a flame retardant is further added to the polyol premix, the flame retardancy of the polyurethane foam may be improved. In order to obtain high flame retardancy, the content of the flame retardant is preferably 15.0 parts by mass or more. The content is more preferably 20.0 parts by mass or more, or 25.0 parts by mass or more. On the other hand, if the content of the flame retardant is excessive, the content of the components necessary for the urethane reaction will be relatively small, and the curing property of the polyurethane foam may be reduced. Therefore, the content of the flame retardant is preferably 30.0 parts by mass or less. The content is more preferably 29.0 parts by mass or less, or 28.0 parts by mass or less.
[0061] [2. Foam] The foam according to the present invention can be obtained by foaming and curing a mixture containing the polyol premix according to the present invention and a polyisocyanate component.
[0062] [2.1. Polyol premix] The polyol premix according to the present invention contains a polyol component, a foam stabilizer, a catalyst, and a blowing agent. Details of the polyol premix are as described above, and therefore will not be described here.
[0063] [2.2. Polyisocyanate component] In the present invention, the type of polyisocyanate component is not particularly limited. The polyisocyanate component may contain one type of polyisocyanate, or may contain two or more types of polyisocyanates.
[0064] The polyisocyanate is (a) Aromatic isocyanate compounds, aliphatic isocyanate compounds, or alicyclic isocyanate compounds, (b) Modified products of the above compounds etc.
[0065] Examples of aromatic isocyanate compounds include: Diphenylmethane diisocyanate (MDI), Crude diphenylmethane diisocyanate, tolylene diisocyanate (TDI), Naphthalene diisocyanate (NDI), p-Phenylene diisocyanate (PPDI), Xylene diisocyanate (XDI), Tetramethylxylene diisocyanate (TMXDI), Tolidin diisocyanate (TODI) and the like.
[0066] Among these, MDI is suitable as a polyisocyanate for producing polyurethane foam. MDI is a polyisocyanate that is divided into three isomers: 2,2'-diphenylmethane diisocyanate (2,2'-MDI), 2,4'-Diphenylmethane diisocyanate (2,4'-MDI), and 4,4'-Diphenylmethane Diisocyanate (4,4'-MDI) The polyisocyanate may contain any one of these isomers, or may contain two or more of them.
[0067] Examples of the aliphatic isocyanate compound include: Hexamethylene diisocyanate (HDI), Lysine diisocyanate (LDI), Examples include lysine triisocyanate (LTI).
[0068] Examples of the alicyclic isocyanate compound include: Isophorone diisocyanate (IPDI), Cyclohexyl diisocyanate (CHDI), water-added XDI (H6XDI), Water added MDI(H 12 MDI) etc.
[0069] Examples of modified isocyanate compounds include urethane-modified, dimer-, trimer-, carbodiimide-modified, allophanate-modified, biuret-modified, urea-modified, isocyanurate-modified, oxazolidone-modified, and isocyanate-terminated prepolymers of isocyanate compounds.
[0070] [2.3. Reaction] When the polyol premix and the polyisocyanate component are mixed in a predetermined ratio and the raw material mixture is heated to a predetermined temperature, the raw material mixture foams and hardens to obtain the foam according to the present invention. The reaction method, reaction conditions, etc. are not particularly limited, and the optimal ones can be selected depending on the purpose.
[0071] [3. Warm storage] The thermal insulation cabinet according to the present invention includes the foam according to the present invention. In the thermal insulation cabinet, the foam is used as a heat insulating material. Examples of the thermal insulation cabinet include rice cabinets, refrigerators, freezers, and the like.
[0072] [4. Effect] In the case of producing polyurethane foam containing closed cells (rigid polyurethane foam), it is relatively easy to produce polyurethane foam with good appearance by using a fluorocarbon compound as a blowing agent. However, the supply stability of the fluorocarbon compound is low and it is expensive. On the other hand, water as a blowing agent has a high supply stability and is inexpensive. However, when water is used as a blowing agent, the polyurethane foam tends to have a poor appearance. This is thought to be because the viscosity tends to increase when the polyol premix and the polyisocyanate are mixed.
[0073] In contrast, in a polyol premix containing a polyol component, a foam stabilizer, a catalyst, and a blowing agent, if the types of the polyol component and the catalyst are optimized, a polyurethane foam with a good appearance can be obtained even when water is used as the blowing agent. This is thought to be because optimizing the types of the polyol component and the catalyst makes it difficult for the polyol premix to thicken even when it is mixed with a polyisocyanate.
[0074] For example, when a sucrose-based polyether polyol B having a large number of functional groups is used as the polyol component, if the type and / or content of other components contained in the polyol premix is inappropriate, the polyurethane foam may have a defective appearance. In contrast, when a sucrose-based polyether polyol B having a small number of functional groups is used, the defective appearance is less likely to occur.
[0075] When amine catalyst A (higher glycol-based amine catalyst) is used as the resinification catalyst, the appearance defect is less likely to occur. This is thought to be because amine catalyst A has an appropriate hydroxyl value and a good balance between resinification activity and foaming activity, so that the resinification reaction and foaming reaction proceed in a well-balanced manner.
[0076] When polyether polyol D having a high hydroxyl value and low molecular weight is further used as the polyol component, the occurrence of defective appearance may be reduced. This is believed to be due to an increase in crosslink density.
[0077] Furthermore, when a foam stabilizer with strong foam stabilizing power (e.g., dimethylpolysiloxane-polyoxyalkylene copolymer (OR terminal)) is used as a foam stabilizer, the polyurethane foam may have a poor appearance. In contrast, when a foam stabilizer with slightly weaker foam stabilizing power is used (e.g., a compound with hydroxyl groups at the molecular end, such as dimethylpolysiloxane-polyoxyalkylene copolymer (OH terminal)) is used, the foam is less likely to have a poor appearance. This is thought to be because foam stabilizers with OH terminals, which have moderate foam stabilizing power, have moderate fluidity and therefore are able to suppress the generation of voids caused by the collapse of the edges of the polyurethane foam compared to foam stabilizers with OR terminals, which have strong foam stabilizing power. EXAMPLES
[0078] (Examples 1 to 6, Comparative Examples 1 to 4) [1. Preparation of polyol premix] The following polyether polyol A was used. (a) Polyether polyol A1: Functional group number 4, hydroxyl value 400 mg KOH / g, product name "PE-400", manufactured by SKC
[0079] As the sucrose-based polyether polyol B, the following was used. (a) Sucrose-based polyether polyol B1: Functional group number 5.4, hydroxyl value 450 mgKOH / g, viscosity 15,000 mPa·s (B-type viscosity measurement temperature: 25°C), product name "SR-453", manufactured by SKC (b) Sucrose-based polyether polyol B2: Functional group number 4.4, hydroxyl value 460 mgKOH / g, viscosity 5,000 mPa·s (B-type viscosity measurement temperature: 25°C), product name "EXCENOL 100S", manufactured by AGC Corporation
[0080] As the aromatic amine-based polyether polyol C, the following was used. (a) Aromatic amine polyether polyol C1: Functional group number 4, hydroxyl value 400 mgKOH / g, viscosity 16,000 mPa·s (B-type viscosity measurement temperature: 25°C), product name "LUPRANOL VP9345", manufactured by BASF (b) Aromatic amine polyether polyol C2: Functional group number 4, hydroxyl value 400 mgKOH / g, viscosity 17,000 mPa·s (B-type viscosity measurement temperature: 25°C), product name "POLYOL RA-401", manufactured by SKC (c) Aromatic amine polyether polyol C3: Functional group number 4, hydroxyl value 400 mgKOH / g, viscosity 8,500 mPa·s (B-type viscosity measurement temperature: 25°C), product name "LUPRANOL VP9234", manufactured by BASF
[0081] The following polyether polyol D was used. (a) Polyether polyol D1: Functional group number 3, hydroxyl value 160 mg KOH / g, molecular weight 1,000, product name "LUPRANOL TP1000", manufactured by BASF (b) Polyether polyol D2: Functional group number 3, hydroxyl value 400 mg KOH / g, molecular weight 430, product name "EXCENOL 430", manufactured by AGC Corporation
[0082] The other polyols used were as follows: (a) Sorbitol-based polyether polyol E1: Functional group number 6, hydroxyl value 450 mgKOH / g, product name "SANNIX SP-750", manufactured by Sanyo Chemical Industries, Ltd.
[0083] The following flame retardants were used: (a) Flame retardant A: Tris(1-chloro-2-propyl)phosphate (b) Flame retardant B: triethyl phosphate
[0084] The following foam stabilizers were used: (a) Foam stabilizer A: Dimethylpolysiloxane-polyoxyalkylene copolymer (OH group terminal), product name "SF2937F", manufactured by Dow Toray Co., Ltd. (b) Foam stabilizer B: Dimethylpolysiloxane-polyoxyalkylene copolymer (OR terminal), product name "SF2938F", manufactured by Dow Toray Co., Ltd. (c) Foam stabilizer C: Dimethylpolysiloxane-polyoxyalkylene copolymer (OH terminal), product name "SZ1711", manufactured by Dow Toray Co., Ltd. (d) Foam stabilizer D: Dimethylpolysiloxane-polyoxyalkylene copolymer (OR terminal), product name "SZ1677", manufactured by Dow Toray Co., Ltd.
[0085] The following catalysts were used: (a) Catalyst A (imidazole catalyst): N,N,N',N'-tetramethylethylenediamine approx. 12%, 1-methylimidazole approx. 48%, polyoxypropylene monoallyl ether approx. 40% (b) Catalyst B (foaming catalyst): 70% bis(2-dimethylaminoethyl) ether, 30% dipropylene glycol
[0086] (c) Catalyst C (triazine catalyst): N,N',N"-dimethylaminopropylhexahydrotriazine (d) Catalyst D (foam catalyst): pentamethyldiethylenetriamine (e) Catalyst E (balance catalyst): N,N,N',N'-tetramethyl-1,6-hexanediamine
[0087] (f) Catalyst F (amine catalyst A): methylamine-1,6-hexanediol polycondensate (HO-[R1-N(R2)] n -R1-OH, where R1 is a hexamethylene group, R2 is a methyl group, n is 3.5 (average degree of polymerization), hydroxyl value: 217 mg KOH / g) (g) Catalyst G (amine catalyst B): N,N-dimethyldodecylamine (h) Catalyst H (foam catalyst): 2,2-dimorpholinodiethyl ether
[0088] The foaming agent used was water. The above raw materials were mixed in a predetermined ratio to obtain polyol premixes. Table 1 shows the raw material composition of each polyol premix.
[0089] [Table 1]
[0090] [2. Polyisocyanate] The following polyisocyanates were used: (a) Polyisocyanate A: Crude diphenylmethane diisocyanate, NCO content 31%, product name "LUPRANATE M20S", manufactured by BASF
[0091] 3. Test Method [3.1. Molding and appearance evaluation] A mold (2 m bread mold) with inner dimensions of 200 mm × 2000 mm × t50 mm was used for the foam molding. A predetermined amount of polyol premix and a predetermined amount of polyisocyanate were mixed. Table 2 shows the mass of polyisocyanate relative to the total mass shown in Table 1, and the isocyanate index.
[0092] [Table 2]
[0093] The obtained raw material mixture was poured into a 2 m bread mold maintained at 50° C., and the raw material mixture was foamed and cured in the mold. After a predetermined time (15 minutes) had elapsed, the mold was removed to obtain a polyurethane foam. Furthermore, the appearance of the obtained polyurethane foam was visually evaluated. The evaluation was performed on the tip shape, upper surface, and lower surface. Table 3 shows the evaluation criteria for appearance.
[0094] [Table 3]
[0095] 3.2. Reactivity The polyol premix and polyisocyanate were each adjusted to a temperature of 25°C. Then, each raw material was charged into a container measuring 150 mm in length, 150 mm in width, and 150 mm in height, and the polyol premix and polyisocyanate were mixed. The blending ratio of each raw material was the same as that in Table 2. The mixture was stirred at 3600 rpm for 5 seconds using a stirrer. Furthermore, the cream time, gel time, and rise time of the raw material mixture were measured in accordance with JIS A 9511.
[0096] The "cream time" refers to the time when the mixture begins to swell, as determined by visual observation. "Gel time" refers to the time from the start of mixing to the start of hardening of the resin. "Rise time" refers to the time when the foam stops rising as visually confirmed.
[0097] The resulting mixture was then foamed and cured to obtain a polyurethane foam for density measurement. After curing for one day, the free density of the polyurethane foam was measured in accordance with JIS A 9511.
[0098] [4. Results] The results are shown in Table 4. From Table 4, the following can be seen. (1) In Comparative Example 1, poor appearance occurred. This is believed to be due to the use of Catalyst A, as well as the use of raw materials such as sucrose-based polyol (SR453) with many functional groups, glycerin-based polyol (TP1000) with low crosslink density (low number of functional groups relative to the molecular weight), and foam stabilizer A (SF2937F) with too strong foam stabilizing power. (2) In Comparative Example 2, poor appearance occurred. This is believed to be due to the use of Catalyst E, as well as the use of sucrose-based polyol (SR453) with many functional groups, glycerin-based polyol (TP1000) with low crosslink density (low number of functional groups relative to the molecular weight), and foam stabilizer B (SF2938F) with OR terminals as raw materials.
[0099] (3) Poor appearance occurred in Comparative Example 3. This is believed to be due to the use of sorbitol-based polyol (SP-750) as a raw material. (4) In Comparative Example 4, poor appearance occurred. This is believed to be due to the use of Catalyst E and the addition amount of TDA-based polyol (VP9234) being too large at 20 parts. (5) Examples 1 to 6 all had better appearance than Comparative Examples 1 to 6. (6) Examples 5 to 6 had better appearances than Examples 1 to 4. This is believed to be due to the use of foam stabilizer C (SZ1711) having an OH terminal with a moderately strong foam stabilizing power.
[0100] [Table 4]
[0101] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]
[0102] The polyol premix according to the present invention can be used as a raw material for producing polyurethane foams used as insulating materials for rice storage, refrigerators, freezers, vending machines, ships, vehicles, plants, building materials, furniture, etc.
Claims
1. The composition includes a polyol component, a foam stabilizer, a catalyst, and a blowing agent, The polyol component is Polyether polyol A; Sucrose-based polyether polyol B; Aromatic amine-based polyether polyol C; Including, The catalyst includes an amine catalyst having a hydroxyl value of 200 mgKOH / g or more. Polyol premix.
2. The polyol premix according to claim 1 , wherein the sucrose-based polyether polyol B contains 20 mass % or more of propylene oxide units.
3. The content of the sucrose-based polyether polyol B is 1.0 mass% or more and 25.0 mass% or less, The content of the aromatic amine-based polyether polyol C is 1.0 mass% or more and 25.0 mass% or less. The polyol premix of claim 1.
4. The catalyst further comprises a triazine-based catalyst; The foam stabilizer contains a compound having a hydroxyl group at the molecular end. The polyol premix of claim 1.
5. A foam obtained by foaming and curing a mixture containing the polyol premix according to claim 1 and a polyisocyanate component.
6. A thermal insulation box comprising the foam according to claim 5.
Citation Information