Nonaqueous slurry composition for positive electrode
The non-aqueous slurry composition with carbon nanotubes and controlled alkali metal ions addresses the dispersibility and viscosity issues of carbon nanofiber slurries, enabling efficient electrode production with improved properties.
Patent Information
- Application Number
- JP2023074825
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Non-aqueous slurries containing carbon nanofibers exhibit poor dispersibility and high viscosity, leading to poor coating properties and prolonged drying times, necessitating increased solvent use.
A non-aqueous slurry composition for positive electrodes comprising carbon nanotubes, a non-aqueous dispersant, and a non-aqueous polar solvent, with controlled amounts of alkali metal ions, to achieve low viscosity and improved dispersibility.
The composition allows for easy application to electrode substrates, reduces drying time, and results in electrodes with low electrical resistance, high capacity retention, and excellent cycle stability.
Smart Images

Figure 2024159070000001 
Figure 2024159070000002 
Figure 2024159070000003
Abstract
Description
Technical Field
[0001] The present invention relates to a non-aqueous slurry composition suitably used for an electrode for a positive electrode such as a lithium ion secondary battery, and a lithium ion secondary battery having an electrode made using the same as a positive electrode.
Background Art
[0002] In recent years, with the spread of electronic devices, mobility considering the environment, etc., the lithium ion battery market has been attracting attention. A lithium ion battery includes a negative electrode containing an active material that reversibly allows lithium ions to enter and exit, a positive electrode, and a non-aqueous electrolyte that immerses them. The positive electrode is manufactured by applying an electrode slurry composed of an active material, a conductive material, and a binder to a current collector such as an aluminum foil.
[0003] Conventionally, the use of a high specific surface area carbon material, particularly graphite (graphite particles), in a non-aqueous secondary battery including a lithium ion battery has been studied. In particular, it is known to form an intercalation compound in graphite and use the intercalation compound as a secondary battery electrode material, and many techniques have been disclosed.
[0004] For example, Patent Document 1 discloses a secondary battery having a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution. As the active material of the positive electrode, a non-carbonaceous material is used. As the active material of the negative electrode, the BET specific surface area A (m 2 / g) is in the range of 0.1 < A < 100, and the values of the crystal thickness Lc (Å) and the true density ρ (g / cm 3 ) in X-ray diffraction satisfy the conditions 1.80 < ρ < 2.18, 15 < Lc, and 120ρ - 227 < Lc < 120ρ - 189. A secondary battery using a carbonaceous material in this range is described.
[0005] This Patent Document 1 further discloses Li +It is described that when ions and the like are to be incorporated, a carbonaceous material having a certain degree of irregular structure has superior properties, and further, it is described that if the surface area of the carbon material is small, it is undesirable because smooth electrochemical reactions on the electrode surface do not easily proceed, and that if the specific surface area is too large, deterioration in characteristics is observed in terms of cycle life characteristics, self-discharge characteristics, and further current efficiency characteristics, and it is also undesirable.
[0006] In addition, Patent Document 2 describes a conductive assistant having a particle thickness of 0.5 nm to 30 nm and a specific surface area of 50 m 2 / g or more, a carbon material other than the flaky graphite, a dispersant, a binder, etc.
[0007] Patent Document 3 discloses a non-aqueous lithium-type storage element including a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution containing lithium ions, and describes that the negative electrode of the non-aqueous lithium storage element is pre-doped with alkali metal ions, and that the pre-doping method is a method of assembling an electricity storage element using a positive electrode precursor containing an alkali metal compound, a negative electrode, a separator, an exterior body, and a non-aqueous electrolyte solution, and then applying a voltage between the positive electrode precursor and the negative electrode. Patent Document 3 does not mention the improvement of the physical properties of the slurry composition when preparing the positive electrode.
[0008] Furthermore, Patent Document 4 discloses a method for producing a positive electrode active material paste used to form a positive electrode active material layer constituting a lithium ion secondary battery, the method comprising the steps of dispersing a mixture of a conductive assistant such as particulate carbon materials acetylene black and ketjen black, carbon nanofibers as fibrous carbon materials, and vapor-grown carbon fibers, a binder, and an organic solvent using an ultrasonic disperser to obtain a conductive assistant dispersion paste, and mixing the positive electrode active material with the conductive assistant dispersion paste obtained in the previous step. Patent Document 4 does not mention any improvement in the physical properties of the paste. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP-B-4-24831 (Claims, Examples, etc.) [Patent Document 2] JP 2014-182873 A (Claims, Examples, etc.) [Patent Document 3] International Publication No. 2021 / 66174 (Claims, Examples, etc.) [Patent Document 4] JP 2016-103391 A (Claims, Examples, etc.) Summary of the Invention [Problem to be solved by the invention]
[0010] In non-aqueous slurries, carbon nanofibers generally tend to produce slurries with low dispersibility and high viscosity. High viscosity slurries have poor coatability, so the amount of solvent must be increased, which results in longer drying times after coating. For this reason, dispersants are often added, but the improvement effect is limited.
[0011] There is a demand for further improvement in the physical properties of a slurry composition containing carbon nanofibers when used to prepare an electrode for a lithium ion secondary battery. The problem to be solved by the present invention is to provide a nonaqueous slurry composition for a positive electrode having a low viscosity. [Means for solving the problem]
[0012] The present invention relates to a nonaqueous slurry composition for a positive electrode of a lithium ion secondary battery, comprising at least a positive electrode active material, carbon nanotubes, a nonaqueous dispersant and a nonaqueous polar solvent, and containing a total amount of alkali metal ions other than Li of 5 ppm to 1000 ppm. Effect of the Invention
[0013] The non-aqueous slurry composition of the present invention has a relatively low viscosity, and therefore can be easily applied to a positive electrode substrate. After application, the composition can be easily dried to obtain a positive electrode plate for a lithium battery. Furthermore, an electrode plate obtained by coating and drying the nonaqueous slurry composition for positive electrodes of the present invention has low electrical resistance and is therefore suitable as a positive electrode for a lithium battery.
[0014] More specifically, the non-aqueous slurry composition of the present invention has good dispersibility of carbon nanotubes and excellent coating stability. In addition, the electrode obtained from the non-aqueous slurry composition of the present invention has low electrode sheet resistance, high capacity retention rate after charging and discharging, and high repeated cycle retention rate, and is suitable as a positive electrode for a lithium ion secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The non-aqueous slurry composition for a positive electrode of the present invention comprises at least a positive electrode active material, carbon nanotubes, and a non-aqueous dispersant. The non-aqueous slurry composition for a positive electrode of the present invention may further contain carbon black, graphite, a binder, and a non-aqueous polar solvent.
[0016] Examples of the positive electrode active material include composite oxides of lithium and transition metals such as lithium-nickel composite oxide, lithium-cobalt composite oxide, lithium-manganese composite oxide, lithium-nickel-manganese composite oxide, lithium-nickel-cobalt composite oxide, lithium-nickel-aluminum composite oxide, lithium-nickel-cobalt-aluminum composite oxide, lithium-nickel-manganese-cobalt composite oxide, lithium-nickel-manganese-aluminum composite oxide, and lithium-nickel-cobalt-manganese-aluminum composite oxide; TiS 2 , FeS, MoS 2 Transition metal sulfides such as MnO, V 2 O 5 , V 6 O 13 , TiO 2 and the like, and olivine type lithium phosphate.
[0017] The olivine-type lithium phosphate contains, for example, at least one element selected from the group consisting of Mn, Cr, Co, Cu, Ni, V, Mo, Ti, Zn, Al, Ga, Mg, B, Nb, and Fe, as well as lithium, phosphorus, and oxygen. These compounds may have some elements partially substituted with other elements in order to improve their properties.
[0018] A preferred positive electrode active material is a lithium-nickel composite oxide, and more preferably, the lithium-nickel composite oxide is represented by the formula: LiNiXM1YM 2 Z.O. 2 (M1 and M2 are at least one metal element selected from the group consisting of Al, B, alkali metals, alkaline earth metals, and transition metals; 0.8≦X≦1.0, 0≦Y≦0.2, and 0≦Z≦0.2). These positive electrode active materials may be used alone or in combination of two or more.
[0019] In the positive electrode slurry composition of the present invention, the content of the positive electrode active material is preferably 40 to 70 mass %, more preferably 45 to 65 mass %, based on the total amount of the positive electrode slurry composition, thereby ensuring the capacity of the battery.
[0020] As the carbon nanotube, a carbon nanotube (CNT) having a shape substantially formed by rolling up a single surface of graphite into a cylindrical shape is preferable, and either a single-walled carbon nanotube in which a single surface of graphite is rolled up in one layer, or a multi-walled carbon nanotube in which a single surface of graphite is rolled up in two or more layers can be used.
[0021] From the viewpoint of viscosity, electrical conductivity, and stability of the slurry composition, the average outer diameter of the carbon nanotubes is preferably 1 nm or more and 90 nm or less, more preferably 3 nm or more and 30 nm or less, and even more preferably 3 nm or more and 15 nm or less. Here, the average outer diameter of the carbon nanotubes refers to the arithmetic mean value of the outer diameters of a sufficient number n measured using an image of a transmission electron microscope at a magnification of 100,000 times or more.
[0022] Examples of the form of carbon nanotubes include, but are not limited to, graphite whiskers, filamentous carbon, graphite fibers, ultrafine carbon tubes, carbon tubes, carbon fibrils, carbon microtubes, and carbon nanofibers, and these may be used alone or in combination of two or more types (hereinafter simply referred to as "at least one type").
[0023] The purity of the carbon nanotubes used in the present invention is preferably 90 to 100% by mass, particularly preferably 95 to 100% by mass. The purity of the carbon nanotubes is calculated based on the amount of impurities, with ash content measured according to JIS K 1469 or JIS K 6218 being taken as impurities.
[0024] Specific examples of carbon nanotubes used in the present invention include NC7000 (average outer diameter: 10 nm) manufactured by Nanocyl Corporation, Baytubes C150P (average outer diameter: 11 nm) manufactured by Bayer AG, FloTube 9000 (average outer diameter: 19 nm), FloTube 7320 (average outer diameter: 9 nm), FloTube 7010 (average outer diameter: 9 nm), FloTube 6810 (average outer diameter: 8 nm), FloTube 6120 (average outer diameter: 8 nm), FloTube 6100 (average outer diameter: 8 nm), FloTube 2020 (average outer diameter: 4 nm) manufactured by Cnano Corporation, and MEIJO eDIPS manufactured by Meijo Nano Carbon Co., Ltd. At least one selected from EC2.0 (average outer diameter 2.0 nm), KORBON-A7 (average outer diameter 1.2 nm) manufactured by KORBON Co., Ltd., NFT-7 (average outer diameter 30 nm) manufactured by Koatsu Gas Kogyo Co., Ltd., and NFT-15 (average outer diameter 30 nm) manufactured by Koatsu Gas Kogyo Co., Ltd. can be used.
[0025] In the positive electrode slurry composition of the present invention, the content of carbon nanotubes is preferably 0.05 to 6.00 mass % and more preferably 0.10 to 4.00 mass % based on the total amount of the positive electrode slurry composition, thereby ensuring the capacity of the battery and the fluidity of the slurry composition.
[0026] In the positive electrode slurry composition of the present invention, carbon-based particles other than carbon nanotubes can be blended. As the carbon-based particles other than carbon nanotubes, it is preferable to use one or more types selected from the group consisting of carbon black, graphite, and graphene.
[0027] It is a preferred embodiment to use a combination of carbon nanotubes and flat graphite, in which case the amount of flat graphite is 10% by mass or more relative to the amount of carbon nanotubes to obtain a synergistic effect with the carbon nanotubes, and 2000% by mass or less to ensure the stability of the slurry composition.
[0028] Graphene may be used as the carbon-based particle. Graphene is a one-atom-thick sp 2 It is a sheet-like material of bonded carbon atoms arranged in a honeycomb-like hexagonal lattice structure made up of carbon atoms and their bonds.
[0029] The content of each carbon-based particle is preferably 0.01 to 15.0 mass% in terms of solid content, more preferably 0.05 to 10.0 mass%, further preferably 0.05 to 8.00 mass%, particularly preferably 0.10 to 6.00 mass%, and most preferably 0.50 to 5.0 mass%. By making the content of the carbon-based particles 0.05 mass% or more relative to the total amount of the slurry composition, good conductivity can be ensured when the battery is made, while by making the content 15.0 mass% or less, the stability of the slurry composition can be ensured.
[0030] The slurry composition of the present invention contains a non-aqueous dispersant. The non-aqueous dispersant may be of the polymer type, low molecular type, or inorganic type, but is preferably of the polymer type. More preferably, it is polyvinylpyrrolidone or polyvinyl acetal.
[0031] As the polyvinylpyrrolidone, commercially available polyvinylpyrrolidone can be used. Polyvinylpyrrolidone can act as a dispersant for the active material and the conductive material without being inhibited by alcohol.
[0032] The content of polyvinylpyrrolidone in the aqueous dispersion for forming an electrode layer is, relative to the total amount of the slurry composition for a positive electrode, 0.05% by mass or more, and may be preferably 0.07% by mass or more, 0.10% by mass or more, 0.12% by mass or more, or 0.15% by mass or more, and may be 1.00% by mass or less, and preferably 0.90% by mass or less, 0.80% by mass or less, 0.70% by mass or less, 0.60% by mass or less, 0.50% by mass or less, 0.40% by mass or less, or 0.30% by mass or less.
[0033] The viscosity average molecular weight of polyvinylpyrrolidone may be preferably 5,000 or more, 6,000 or more, 7,000 or more, 8,000 or more, or 10,000 or more, and may be preferably 300,000 or less, 250,000 or less, 230,000 or less, 200,000 or less, 180,000 or less, 150,000 or less, 120,000 or less, 100,000 or less, 90,000 or less, 85,000 or less, 80,000 or less, 75,000 or less, 70,000 or less, or 65,000 or less.
[0034] The viscosity average molecular weight can be measured, for example, by the method for measuring molecular weight described in Kobunshi Ronbunshu, vol. 38, No. 7, pp. 457-463 (July, 1981), that is, by the following procedure: (1) The sample is added to an excess of acetone for precipitation purification. This procedure is repeated twice, and then the sample is dried under reduced pressure until the odor of acetone disappears. (2) Prepare an aqueous solution of the purified sample, and use an Ubbelohde viscometer (water, 120 seconds) to calculate the viscosity average molecular weight using the following formula.
number
[0035] The above formula is the relational expression between the intrinsic viscosity [η] and the viscosity average molecular weight obtained by substituting the constants K and a in the following Mark-Kuhn-Houwink formula (Mark-Houwink-Sakurada formula) with reference to the above-mentioned collection of papers. It should be noted that other methods may be used to measure the viscosity average molecular weight as long as the measurement method can give equivalent results.
[0036] <Polyvinyl acetal> The polyvinyl acetal in the positive electrode slurry composition of the present invention is a vinyl copolymer represented by the following chemical formula (1) and having an acetal group, an acetyl group, and a hydroxyl group as substituted functional groups. [ka] (In the formula, l, m, and n are positive numbers, and R is an alkyl group having 1 to 20 carbon atoms.)
[0037] Without wishing to be bound by theory, in the FT-IR (Fourier transform infrared spectroscopy) spectrum obtained by total attenuation measurement (ATR method) of polyvinyl acetal, -1 The intensity of the peak at 2950 cm -1 It is believed that the intensity of the peak at is large due to the proportion of the sum of the acetal group and the acetyl group, that is, the sum of the values of l and m in the above chemical formula (1). In the FT-IR spectrum, 1650 cm -1 Peak intensity at 2950cm -1 The ratio of peak intensities at indicates the relative proportion of acetal groups.
[0038] The polyvinyl acetal of the present invention has a peak at 1650 cm as measured by FT-IR. -1 Intensity of the peak near 2950 cm -1is equal to or greater than 50. This ratio may be equal to or greater than 50, 55 or greater, 60 or greater, 65 or greater, 70 or greater, 75 or greater, 80 or greater, 85 or greater, 90 or greater, 95 or greater, or 100 or greater. If this ratio is less than 50, the effect of the present invention will not be exhibited, which is not preferable.
[0039] In addition, the polyvinyl acetal of the present invention has a peak at 3400 cm as measured by the FT-IR. -1 The intensity of the peak at 3400 cm is increased due to the proportion of hydroxyl groups, i.e., the value of n in the above chemical formula (1). -1 Intensity of the peak at 2950 cm -1 The ratio of the peak intensities at 3400 cm is considered to indicate the relative proportion of acetal groups. -1 Intensity of the peak at 2950 cm -1 is preferably 2.0 or more, and may be 2.5 or more, or 3.0 or more.
[0040] It is believed that the relatively large proportion of acetal groups leads to a stronger tendency for the polyvinyl acetal as a whole to be hydrophobic, which results in a high affinity for graphite. As a result, the positive electrode slurry composition can be easily heated at a low shear rate, for example at 0.1 to 100°C. -1 The viscosity at the time of the reaction can be reduced.
[0041] In the slurry composition for a positive electrode of the present invention containing such polyvinyl acetal, -1 Viscosity at 1000s -1 is preferably 1000 or less, and more desirably 900 or less, 800 or less, 700 or less, 600 or less, or 550 or less.
[0042] In the measurement of the viscosity ratio, the shear rate is set to 0.1 -1 From 1000s -1 The shear rate was then changed to 1000 s with a logarithmic slope over 20 s.-1 From 0.ls -1 The viscosity was measured over a total of 40 seconds by changing the shear rate to 1000 s with a logarithmic gradient over 20 seconds. The viscosity measured 20 seconds after the start of the measurement was -1 The viscosity measured at 40 seconds was taken as the shear rate of 0.1 s -1 The viscosity was set to .
[0043] The content of the acetal groups in the substituted functional groups of the polyvinyl acetal in the present invention can be 70 mass% or more, 75 mass% or more, 80 mass% or more, 81 mass% or more, 82 mass% or more, or 83 mass% or more, based on the total amount of substituted functional groups of the polyvinyl acetal.
[0044] The number of carbon atoms in the alkyl group constituting R in the above chemical formula (1) is not particularly limited, and may be 1 or more, 3 or more, 5 or more, 7 or more, or 9 or more, and may be 20 or less, 18 or less, 16 or less, 14 or less, or 12 or less. In particular, the polyvinyl acetal in the present invention may be polyvinyl butyral in which the number of carbon atoms in the alkyl group constituting R is 3.
[0045] The absorbance at 320 nm of a 10% by mass N-methylpyrrolidone (NMP) solution of the polyvinyl acetal in the present invention may be preferably 0.25 or more, 0.30 or more, 0.35 or more, 0.40 or more, 0.45 or more, 0.50 or more, 0.55 or more, 0.60 or more, or 0.65 or more in terms of the viscosity and stability over time of the dispersion, and among them, 0.50 or more is preferable in terms of improving dispersibility. This absorbance may be 0.90 or less, 0.85 or less, 0.80 or less, 0.75 or less, or 0.70 or less. In addition, in measuring this absorbance, the absorbance of NMP is used as a blank.
[0046] The shear rate of the 10% by mass NMP solution of the polyvinyl acetal of the present invention is 76.6 s -1The viscosity at may be 10.0 mPa·s or more, 15.0 mPa·s or more, 20.0 mPa·s or more, or 21.0 mPa·s or more, and may be 70.0 mPa·s or less, 65 mPa·s or less, 60.0 mPa·s or less, 55.0 mPa·s or less, 50 mPa·s, 45.0 mPa·s or less, 40.0 mPa·s or less, 35.0 mPa·s or less, 33.0 mPa·s or less, 3.0 mPa·s or less, or 30.0 mPa·s or less. This viscosity can be measured using a cone-plate viscometer for a measurement time of 60 seconds.
[0047] The mass average molecular weight of the polyvinyl acetal of the present invention measured by gel permeation chromatography is preferably 100,000 or less in order to further exert the effects of the present invention. This mass average molecular weight may be 90,000 or less, 85,000 or less, 80,000 or less, 75,000 or less, 70,000 or less, 65,000 or less, 60,000 or less, 55,000 or less, or 50,000 or less. Such a mass average molecular weight reduces the viscosity of the polyvinyl acetal solution, and as a result, the aggregation of the obtained graphite can be suppressed. This mass average molecular weight may be 10,000 or more, 15,000 or more, 20,000 or more, 25,000 or more, 30,000 or more, 35,000 or more, or 40,000 or more. This mass average molecular weight obtained by gel permeation chromatography is a converted value obtained using polystyrene as a standard polymer.
[0048] In the positive electrode slurry composition of the present invention, the content of the non-aqueous dispersant may be 0.1 mass% or more, 0.3 mass% or more, 0.5 mass% or more, 0.7 mass% or more, or 0.9 mass% or more, and may be 10.0 mass% or less, 8.0 mass% or less, 5.0 mass% or less, 3.0 mass% or less, 2.7 mass% or less, 2.4 mass% or less, 2.1 mass% or less, 1.8 mass% or less, or 1.5 mass% or less, based on the total mass of the positive electrode slurry composition. This ensures the fluidity of the slurry composition.
[0049] In the production of the non-aqueous slurry composition for positive electrodes of the present invention, a non-aqueous dispersant containing alkali metal ions in a total amount of preferably 30 ppm to 3000 ppm, more preferably 30 ppm to 2000 ppm, and even more preferably 40 ppm to 1000 ppm can be used. However, when calculating the total amount of the alkali metal ion concentration, the concentration of lithium ions is not included. Some commercially available non-aqueous dispersants contain a considerable amount of alkali metal ions, and these can be used.
[0050] One or more of commercially available non-aqueous dispersants can be used in combination so that the total amount of alkali metal ions in the positive electrode slurry composition is a predetermined concentration, thereby adjusting the alkali metal ion content of the slurry composition.
[0051] The non-aqueous slurry composition for a positive electrode of the present invention is further mixed with a binder and applied to a positive electrode substrate such as an aluminum foil. The binder enhances the adhesion between the applied positive electrode composition and the positive electrode substrate, and polyvinylidene fluoride (PVDF) is used, for example.
[0052] The positive electrode slurry composition of the present invention may further contain other components, such as a solid electrolyte such as a sulfide solid electrolyte, an oxide solid electrolyte, a dry polymer electrolyte, a gel polymer electrolyte, or a quasi-solid electrolyte.
[0053] The non-aqueous slurry composition for a positive electrode of the present invention contains a non-aqueous polar solvent. As the non-aqueous polar solvent, an organic solvent having polarity is used. The non-aqueous polar solvent used in the present invention does not substantially contain water. The content of water is, for example, preferably 2000 ppm or less, more preferably 1500 ppm or less, and even more preferably 1000 ppm or less. If the non-aqueous polar solvent contains a large amount of water, it will cause the decomposition of the positive electrode active material that coexists, which is not preferable.
[0054] Examples of the non-aqueous polar solvent to be used include alkylene glycols such as ethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,5-pentanediol, 2,5-hexanediol, 3-methyl-1,3-butanediol, 2-methylpentane-2,4-diol, 3-methylpentane-1,3,5-triol, and 1,2,3-hexanetriol; polyalkylene glycols such as polyethylene glycol and polypropylene glycol;
[0055] Examples of the alkyl ether include glycerols such as glycerol, diglycerol, and triglycerol; lower alkyl ethers of glycols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, and diethylene glycol mono-n-butyl ether; amides such as N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidalidinone, dimethylformamide, and dimethylacetamide; ketones such as acetone; and esters such as ethylene carbonate, ethyl methyl carbonate, and dimethyl methyl carbonate.
[0056] The non-aqueous polar solvent used in the present invention is preferably an aprotic polar solvent, more preferably an amide or an ester, and even more preferably N-methyl-2-pyrrolidone.
[0057] The non-aqueous slurry composition of the present invention contains a total amount of alkali metal ions of 5 ppm to 1000 ppm, preferably 5 ppm to 800 ppm, and more preferably 10 ppm to 500 ppm. The alkali metal ion content is the sum of the concentrations of each alkali metal ion excluding Li. In the present invention, the concentration of alkali metal ions does not include Li. + The concentration of ions is not included.
[0058] Conventionally, it has been believed that the smaller the content of metal ions other than the metal ions constituting the positive electrode, the better the battery characteristics. On the other hand, in the present invention, the non-aqueous slurry composition that is the raw material for the positive electrode contains alkali metal ions in a predetermined amount range. That is, the positive electrode obtained from the non-aqueous slurry composition of the present invention contains alkali metal ions in a certain amount range, which unexpectedly results in good battery characteristics.
[0059] The method for introducing the alkali metal ions into the non-aqueous slurry composition for a positive electrode at the above-mentioned concentration is not limited, but is preferably carried out by blending a non-aqueous dispersant containing an appropriate concentration of alkali metal ions.
[0060] The amount of alkali metal ions contained in the non-aqueous slurry composition for a positive electrode and the non-aqueous dispersant can be determined by inductively coupled plasma (ICP) emission spectrometry. + , K + The sum of the concentrations of alkali metal ions belonging to Group I of the periodic table in the slurry composition is referred to as the total amount of alkali metal ions.
[0061] The non-aqueous slurry composition of the present invention is a slurry with a relatively low viscosity. Although the mechanism by which the viscosity of the slurry composition is reduced is not clear, it is presumed that a certain amount of alkali metal ions contained in the slurry reduces the Coulomb force due to the surface charge between the carbon nanotubes, and increases the affinity between the carbon nanotube chains and the non-aqueous polar solvent.
[0062] In addition, the positive electrode plate of a lithium battery obtained by coating the non-aqueous slurry composition for a positive electrode of the present invention has a low current resistance. Although the mechanism by which the electrical resistance of the electrode plate decreases is not clear, it is presumed that the alkali metal ions contained in the slurry reduce the Coulomb force due to the surface charge between the carbon nanotubes and increase the fluidity of the carbon nanotube chains, thereby increasing the contact between the carbon nanotubes and the active material, as described above.
[0063] The non-aqueous slurry composition for a positive electrode of the present invention is prepared by putting its components, that is, at least a positive electrode active material, carbon nanotubes, a non-aqueous dispersant, and a non-aqueous polar solvent, into a dispersing machine and mixing them. The non-aqueous slurry composition for a positive electrode of the present invention contains a total amount of 5 ppm to 1000 ppm of alkali metal ions, and these alkali metal ions can be supplied from the non-aqueous dispersant.
[0064] That is, another aspect of the present invention is a method for producing a nonaqueous slurry composition for a positive electrode, the method comprising the step of mixing at least a positive electrode active material, carbon nanotubes, a nonaqueous dispersant, and a nonaqueous polar solvent using a disperser, the nonaqueous dispersant containing a total amount of alkali metal ions excluding Li of 30 ppm to 3000 ppm.
[0065] When preparing the non-aqueous slurry composition for a positive electrode of the present invention, it is preferable to use a dispersing machine with a large beating force, which allows the active material to be crushed in parallel with dispersing the solid particles in the non-aqueous polar solvent.
[0066] Examples of the dispersing machine to be used include homomixers, high-pressure homogenizers, ultra-high-pressure homogenizers, ultrasonic dispersion processors, planetary mixers, combimixes, kneaders, centrifugal mixers, Henschel mixers, ball mills, bead mills, thin-film rotary high-speed agitators, screw mixers, paddle mixers, disperser mixers, turbine mixers, propeller mixers, blenders, ultrasonic homogenizers, colloid mills, pebble mills, beaters, disk refiners, conical refiners, double disk refiners, grinders, etc. It is also preferable to use two or more types of dispersing machines in combination.
[0067] The non-aqueous slurry composition of the present invention has a relatively low viscosity as a slurry, and therefore can be easily applied to a positive electrode substrate. After application, the composition can be easily dried to obtain a positive electrode plate for a lithium battery. Furthermore, an electrode plate obtained by coating and drying the nonaqueous slurry composition for positive electrodes of the present invention can be used as a positive electrode for a lithium ion secondary battery having low resistance, enduring high C-rate charge / discharge, and excellent cycle characteristics. EXAMPLES
[0068] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to these.
[0069] <<Preparation of carbon nanotube dispersion liquid>> <Production Example 1> 100 parts by mass of a carbon nanotube (FT7010, manufactured by Cnano), 1 part by mass of polyvinylpyrrolidone (PVP resin 1) as a dispersant, and 95 parts by mass of N-methyl-2-pyrrolidone as a solvent were dispersed using a high-pressure homogenizer (dispersion pressure 100 MPa, 10 passes) to prepare 100 parts by mass of a carbon nanotube (CNT) dispersion.
[0070] <Production Examples 2 to 7> A carbon nanotube dispersion liquid was prepared in the same manner as in Example 1, except that the same amount of polyvinylpyrrolidone or polyvinyl butyral shown in Table 1 was used instead of PVP resin 1 as a carbon nanotube dispersant. As the polyvinylpyrrolidone, PVP resin 2, PVP resin 3 or PVP K-30 was used, and as the polyvinyl butyral, PVB resin 1, PVB resin 2 or PVB resin 3 was used.
[0071] The proportions of each functional group in the total amount of substituted functional groups contained in the polyvinyl butyral used are as follows: PVB resin 2: polyvinyl butyral containing 83% by mass of acetal groups, 3% by mass of acetyl groups, and 14% by mass of vinyl alcohol groups PVB resin 3: polyvinyl butyral containing 78% by mass of acetal groups, 3% by mass of acetyl groups, and 19% by mass of vinyl alcohol groups
[0072] <<Preparation of non-aqueous slurry composition for positive electrode>> Examples 1 to 4 and Comparative Examples 1 to 3 20 parts by mass of the carbon nanotube dispersion liquid produced in Production Examples 1 to 7, 1.5 parts by mass of acetylene black as a conductive material, and 100 parts by mass of LiNi as a positive electrode active material. 0.5 Co 0.2 Mn 0.3 O 2 100 parts by mass of a nonaqueous slurry composition for a positive electrode was prepared by dispersing 2 parts by mass of polyvinylidene fluoride (Solef5130, manufactured by Solvay) as a binder and 30 parts by mass of N-methyl-2-pyrrolidone as a solvent using a planetary mixer.
[0073] Properties of Carbon Nanotube Dispersion and Non-Aqueous Slurry Composition <Alkali metal ion content> The concentrations of alkali metal ions other than Li were measured and summed up for each of the carbon nanotube dispersions and the non-aqueous slurry compositions prepared using the same using a sequential ICP emission spectrometer. The results are shown in Tables 1 and 2.
[0074] <viscosity> Each of the carbon nanotube dispersions and the non-aqueous slurry compositions prepared using the same were measured using a rheometer (Anton Paar, Modular Compact Rheometer MCR102, diameter 50 mm-2° cone) at a sample temperature of 25° C. and a shear rate of 0.1 s -1 and 1000s -1 The viscosity at each point was measured. That is, shear rate 0.1 s -1 From 1000s -1 The shear rate was then changed to 1000 s with a logarithmic slope over 20 s. -1 From 0.1s -1 The viscosity was measured over a total of 40 seconds by changing the shear rate to 1000 s with a logarithmic gradient over 20 seconds. -1 The viscosity was measured at 40 seconds and the shear rate was 0.1 s -1The results are shown in Tables 1 and 2.
[0075] <Coating stability> The obtained non-aqueous slurry composition was applied to one side of an aluminum foil at a wet film thickness of 100 μm using a comma coater with a coating width of 200 mm to a thickness of 10 m. Streaks that appeared on the obtained coating film and were 10 mm or longer in length were regarded as defects and evaluated according to the following criteria. When multiple streaks appeared, the total length of each was used as the criteria. The results are shown in Table 2. Evaluation criteria: ◎: No streaks longer than 10 mm were present. ○: The total muscle length was 10 mm or more and less than 50 mm. △: The total muscle length was 50 mm or more and less than 100 mm. ×: The total length of the muscle was 100 mm or more.
[0076] <Electrode sheet resistance> The obtained non-aqueous slurry composition was applied to one side of a PET film (Lumira #100-T60, manufactured by Toray Industries, Inc.) with an applicator so that the liquid film was 50 μm, and then dried at room temperature for 30 minutes, and then further dried at 80° C. for 5 minutes to obtain an electrode layer. The sheet resistance (kΩ / □) of the produced electrode layer was measured using an apparatus consisting of a probe with a probe gap of 10 mm and a low resistance meter (Milliohm HiTester 3227, manufactured by Hioki E.E. Corporation). The results are shown in Table 2.
[0077] <Capacity retention rate after 10C charge / discharge> The obtained non-aqueous slurry composition was applied to one side of an aluminum foil with a wet film thickness of 100 μm using a comma coater with a coating width of 200 mm, and dried for 5 minutes in a drying oven at 100° C. to obtain an electrode. Five coin secondary batteries were fabricated using the obtained electrode as the positive electrode, a carbonate-based solvent as the electrolyte, a polypropylene film as the separator, and metallic lithium as the counter electrode.
[0078] The discharge capacity (a) of the produced coin secondary battery was measured when it was charged and discharged once at a charge / discharge rate of 1C, and then the discharge capacity (b) of the battery was measured when it was charged and discharged once at a charge / discharge rate of 10C, and the capacity retention rate after 10C charge / discharge was calculated using Equation 2. The average value for the five coin secondary batteries was calculated, and this was taken as the capacity retention rate after 10C charge / discharge (%). The results are shown in Table 2.
[0079]
number
[0080] <100 cycles maintenance rate> The five coin secondary batteries thus produced were used to measure the initial discharge capacity (A) and the 100th discharge capacity (B) after 100 cycles of 10C charge and discharge, and the 100 cycle retention rate was calculated using Equation 3. The average value for the five coin secondary batteries was calculated, and the 100 cycle retention rate was evaluated by applying the average value to the following evaluation criteria. The results are shown in Table 2.
[0081]
number
[0082] Evaluation criteria: ◎: 98% or more ○: 95% to less than 98% △: 85% to less than 95% ×: Less than 85%
[0083] The composition and physical properties of each carbon nanotube dispersion are shown in Table 1, and the composition and physical properties of each non-aqueous slurry composition are shown in Table 2.
[0084] [Table 1]
[0085] [Table 2]
[0086] As is clear from the results in Table 2 above, the nonaqueous slurry compositions of Examples 1 to 4, which are within the scope of the present invention, were confirmed to produce lithium ion secondary battery positive electrodes having excellent coating stability and good electrode sheet resistance, capacity retention rate after charge and discharge, and discharge capacity retention rate, as compared with the nonaqueous slurry compositions of Comparative Examples 1 to 3, which are outside the scope of the present invention. [Industrial Applicability]
[0087] The non-aqueous slurry composition of the present invention has excellent dispersibility and electrical conductivity, and is particularly suitable for producing a positive electrode of a lithium ion secondary battery. A lithium ion secondary battery having a positive electrode made using the non-aqueous slurry composition of the present invention exhibits improved performance.
Claims
1. At least a positive electrode active material, carbon nanotubes, a non-aqueous dispersant, and a non-aqueous polar solvent are included, A non-aqueous slurry composition for a positive electrode of a lithium ion secondary battery, comprising a total of 5 ppm to 1000 ppm of alkali metal ions other than Li.
2. 2. The non-aqueous slurry composition according to claim 1, wherein the non-aqueous dispersant is at least one member selected from the group consisting of polyvinylpyrrolidone and polyvinyl acetal.
3. The non-aqueous slurry composition according to claim 1 or 2, further comprising carbon black, graphite, and a binder.
4. A method for producing a non-aqueous slurry composition for a lithium ion secondary battery positive electrode, comprising the steps of: mixing at least a positive electrode active material, carbon nanotubes, a non-aqueous dispersant, and a non-aqueous polar solvent using a dispersing machine; The total content of alkali metal ions excluding Li in the nonaqueous positive electrode slurry composition is 5 ppm to 1000 ppm. A method for producing a non-aqueous slurry composition for a positive electrode of a lithium ion secondary battery.
5. The method according to claim 4, wherein the total content of alkali metal ions excluding Li in the non-aqueous dispersant is 30 ppm to 3000 ppm.
6. A lithium ion secondary battery having a positive electrode made from the nonaqueous slurry composition according to claim 3.
Citation Information
Patent Citations
Test device
JP1992024831A
Nonaqueous secondary battery electrode-forming material, nonaqueous secondary battery electrode, and nonaqueous secondary battery
JP2014182873A
Method for manufacturing positive electrode active material paste for lithium ion secondary battery
JP2016103391A
Non-aqueous lithium power storage element
WO2021066174A1