Millable fluorosilicone rubber composition and rubber parts for engine area of transporting machines

A millable fluorosilicone rubber composition with specific organopolysiloxane and silica additives enhances amine resistance, addressing cracking issues and maintaining physical properties for engine-related applications.

JP2024159087AInactive Publication Date: 2024-11-08SHIN ETSU CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023074852
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fluorosilicone rubber compositions face challenges in maintaining physical properties when exposed to amine-based anti-aging agents in fuels and oils, leading to cracking, and the use of certain perfluoroalkyl groups is regulated.

Method used

A millable fluorosilicone rubber composition comprising specific organopolysiloxane, surface-treated reinforcing silica, and organic peroxide, which when cured, provides excellent amine resistance and maintains physical properties.

Benefits of technology

The composition results in a cured fluorosilicone rubber product with minimal deterioration when exposed to amine-based anti-aging agents, suitable for applications near transport aircraft engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159087000001
    Figure 2024159087000001
  • Figure 2024159087000002
    Figure 2024159087000002
  • Figure 2024159087000003
    Figure 2024159087000003
Patent Text Reader

Abstract

To provide a millable fluorosilicone rubber composition capable of obtaining a cured material excellent in amine resistance.SOLUTION: There is provided a millable fluorosilicone rubber composition containing: (A) a raw rubber-state organopolysiloxane represented by the following formula (1): wherein R1 is a group independently selected from alkyl groups having a C number of 1 to 10, aryl groups having a C number of 6 to 10, and aralkyl groups having a C number of 7 to 10, and R2 is an alkenyl group having a C number of 2 to 8; a and b are each an integer of 1 or more; c is an integer of 0 or more; a+b+c=2,000 to 6,000; and a / (a+b+c)=0.3 to 0.8; The bonding of the siloxane units enclosed by a, b and c may be block or random; (B) a surface-treated reinforcing silica having a specific surface area of 50 m2 / g or more by a BET method; and (C) an organic peroxide.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a millable-type fluorosilicone rubber composition and to rubber parts for use around the engine of a transport aircraft, which are made of a cured product of said millable-type fluorosilicone rubber composition. [Background technology]

[0002] Fluorosilicone rubber compositions, which are based on fluorosilicone rubber having 3,3,3-trifluoropropyl groups as side-chain substituents, have excellent solvent resistance in addition to the properties of dimethylsilicone rubber, and are therefore widely used in transportation equipment parts, petroleum-related equipment parts such as diaphragms, O-rings, and oil seal materials.

[0003] However, when fluorosilicone rubber is exposed to amines added to gasoline fuels and oils as antioxidants or rust inhibitors, the siloxane main chain cracks, and the rubber molding is no longer able to maintain its original physical properties. Examples of such amines include various polyether amines, alcohol amines, and alkyl amines.

[0004] As a countermeasure, Patent Document 1 lists a method of preventing deterioration caused by antioxidants by adding an anti-extraction buffer to fluorosilicone rubber. In addition, Patent Document 2 improves fuel oil resistance by using an organopolysiloxane containing a perfluoroalkyl ether group having 4 or more carbon atoms as a base polymer. In addition, Patent Document 3 attempts to improve alcohol fuel oil resistance by adding titanium dioxide and triallyl isocyanurate having an average particle size of 0.1 to 1.0 μm to a fluorosilicone polymer having an unsaturated group at at least one end. Furthermore, Patent Document 4 attempts to improve amine resistance by adding at least one chloride selected from alkali metal chlorides, alkaline earth metal chlorides, and ammonium chloride to a fluorosilicone rubber composition.

[0005] However, even with these methods, it has been difficult to sufficiently prevent cracking of fluorosilicone rubber when it comes into contact with amines.

[0006] In recent years, the Ministry of the Environment has classified organic fluorine compounds as "items requiring monitoring for the protection of human health," restricting compounds containing perfluoroalkyl groups such as PFOS (perfluorooctanesulfonic acid), making it impossible to use long-chain fluoroalkyl groups. As a result, alternative materials are being sought. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 7-252421 [Patent Document 2] Japanese Patent Application Publication No. 5-186700 [Patent Document 3] JP 2000-26735 A [Patent Document 4] JP 2017-222796 A Summary of the Invention [Problem to be solved by the invention]

[0008] In the prior art, there is a problem in that it is difficult to sufficiently prevent cracking of fluorosilicone rubber when it comes into contact with amines which are added as antioxidants or rust inhibitors to gasoline fuels or oils.

[0009] The present invention has been made in order to solve the above problems, and it is an object of the present invention to provide a millable-type fluorosilicone rubber composition which gives a fluorosilicone rubber (cured product) which has excellent amine resistance and undergoes little deterioration in physical properties even when it comes into contact with amine-based antioxidants, etc. contained in fuel, and to provide rubber parts for use around the engine of a transport aircraft, which are made of a cured fluorosilicone rubber.

[0010] In addition, a millable composition refers to a composition that is non-liquid (paste or solid) with no self-fluidity at room temperature (25°C) and can be mixed uniformly under shear stress using a kneading means such as a roll mill. [Means for solving the problem]

[0011] In order to solve the above problems, the present invention provides (A) The following formula (1) [ka] (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkenyl group having 2 to 8 carbon atoms, a and b are each an integer of 1 or more, c is an integer of 0 or more, a+b+c=2,000 to 6,000, and a / (a+b+c)=0.3 to 0.8. The siloxane units bounded by a, b, and c may be bonded in a block or random manner. 100 parts by mass of a raw rubber-like organopolysiloxane represented by the formula: (B) The specific surface area by the BET method is 50 m 2 / g or more of surface-treated reinforcing silica; 10 to 100 parts by mass, (C) Organic peroxide; catalyst amount, The present invention provides a millable type fluorosilicone rubber composition comprising:

[0012] The millable type fluorosilicone rubber composition of the present invention makes it possible to obtain fluorosilicone rubber molded articles (cured products) that exhibit excellent amine resistance and that experience little deterioration in physical properties even when in contact with amine-based antioxidants.

[0013] The present invention also provides rubber parts for use around transport engines, which are made from a cured product of this millable type fluorosilicone rubber composition.

[0014] Rubber parts for use around transport engines made from a cured product of the millable-type fluorosilicone rubber composition of the present invention are preferred because they experience little deterioration in physical properties even when in contact with amine-based antioxidants contained in gasoline fuels and oils. Effect of the Invention

[0015] As described above, the millable-type fluorosilicone rubber composition of the present invention is capable of giving a fluorosilicone rubber molded article (cured product) which exhibits minimal deterioration in physical properties even when in contact with amine-based antioxidants, etc., and such fluorosilicone rubber molded articles are particularly suitable for use in rubber parts for use around transport aircraft engines. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] As mentioned above, there has been a need for the development of a fluorosilicone rubber composition which gives a fluorosilicone rubber molded article (cured product) which exhibits minimal deterioration in physical properties even when in contact with amine-based antioxidants and the like.

[0017] As a result of extensive investigations into the above-mentioned problems, the inventors discovered that by replacing the 3,3,3-trifluoropropylmethylsiloxane units that make up the main chain of the fluorosilicone polymer with 3,3,4,4,5,5,6,6,6-nonafluorohexylmethylsiloxane units, the deterioration of the physical properties of the fluorosilicone rubber due to contact with amine-based antioxidants and the like can be inhibited, leading to the completion of the present invention.

[0018] That is, the present invention provides: (A) The following formula (1) [ka] (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2is an alkenyl group having 2 to 8 carbon atoms, a and b are each an integer of 1 or more, c is an integer of 0 or more, a+b+c=2,000 to 6,000, and a / (a+b+c)=0.3 to 0.8. The siloxane units bounded by a, b, and c may be bonded in a block or random manner. 100 parts by mass of a raw rubber-like organopolysiloxane represented by the formula: (B) The specific surface area by the BET method is 50 m 2 / g or more of surface-treated reinforcing silica; 10 to 100 parts by mass, (C) Organic peroxide; catalyst amount, The millable type fluorosilicone rubber composition contains

[0019] The present invention will be described in detail below, but the present invention is not limited thereto.

[0020] [Component (A)] The component (A) is represented by the following formula (1): [ka] (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkenyl group having 2 to 8 carbon atoms, a and b are each an integer of 1 or more, c is an integer of 0 or more, a+b+c=2,000 to 6,000, and a / (a+b+c)=0.3 to 0.8. The siloxane units bounded by a, b, and c may be bonded in a block or random manner. The organopolysiloxane is a raw rubber-like organopolysiloxane represented by the formula:

[0021] In addition, raw rubber refers to a high polymer that is either a very viscous liquid at room temperature (25° C.) or a non-liquid (paste or solid) that has no self-flowing property.

[0022] In the above formula (1), R 1are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms, preferably each having 8 or less carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, isopropyl, and butyl groups, cycloalkyl groups such as cyclohexyl and cyclopentyl groups, aryl groups such as phenyl, tolyl, and xylyl groups, and aralkyl groups such as benzyl and phenylethyl groups. Particularly preferred groups in the present invention are methyl, ethyl, and phenyl groups. An alkenyl group R having 2 to 8 carbon atoms 2 Examples of the alkyl group include a vinyl group and an allyl group, and the vinyl group is particularly preferred.

[0023] Furthermore, in the formula (1), a and b are each an integer of 1 or more, c is an integer of 0 or more, a+b+c=2,000 to 6,000, and a / (a+b+c)=0.3 to 0.8.

[0024] If a+b+c is less than 2,000, the viscosity will be low and the stickiness will increase, significantly impairing the workability of the Millable Rubber. Conversely, if it exceeds 6,000, the viscosity will be high and subsequent addition and compounding will be difficult.

[0025] Furthermore, a / (a+b+c) is 0.3 to 0.8, and preferably 0.3 to 0.7. If it is less than 0.3, sufficient oil resistance cannot be obtained. If it exceeds 0.8, the flexibility of the cured product may decrease, and the tensile strength, tear strength, and elongation at break may be insufficient.

[0026] Furthermore, b / (a+b+c) is preferably 0.1 to 0.3. If it is 0.1 or more, crosslinking proceeds sufficiently, and the product has sufficient hardness and heat resistance, which is preferable. If it is 0.3 or less, there is no risk of the cured product becoming brittle, which is preferable.

[0027] In this organopolysiloxane, R is an alkenyl group having 2 to 8 carbon atoms. 2Each molecule must have three or more of these groups, and the content of these groups is preferably 0.01 to 1 mol % relative to the number of silicon atoms in the molecule, and more preferably 0.02 to 0.5 mol %, and is preferably an alkenyl group, particularly a vinyl group. If the alkenyl group content is 1 mol % or less, the rubber hardness is suitable for practical use, the rubber is less likely to become brittle, and mechanical strength such as tensile strength and tear strength is suitable.

[0028] The organopolysiloxane represented by the above formula (1) can be prepared, for example, from a compound represented by the following formula (2): [ka] The polymerization can be achieved by ring-opening polymerization of a (nonafluorohexyl)methylsiloxane cyclic trimer using a siloxane oligomer represented by the following formula as an initiator. Specifically, an appropriate amount of siloxane oligomer is added to a cyclic organosiloxane, and living polymerization is carried out under sealed conditions at 100°C to 150°C. By adjusting the amount of the above-mentioned siloxane oligomer appropriately during the living polymerization, an organopolysiloxane that has reached the desired degree of polymerization can be obtained.

[0029] The degree of polymerization of the organopolysiloxane is preferably 2,000 to 6,000, more preferably 2,500 to 5,500, particularly preferably 3,000 to 5,500, and even more preferably 3,000 to 5,000. The organopolysiloxane is characterized by being in the form of a so-called raw rubber that has no self-flowability at room temperature (25°C). If the degree of polymerization is less than 2,000, problems such as roll adhesion will occur when the organopolysiloxane is made into a silicone rubber compound, and roll workability will deteriorate. The degree of polymerization in the present invention is determined as the weight-average degree of polymerization from the weight-average molecular weight in terms of polystyrene by gel permeation chromatography (GPC) analysis measured under the following conditions.

[0030] [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperH4000(6.0mmI.D.×15cm×1) TSKgel SuperH3000(6.0mmI.D.×15cm×1) TSKgel SuperH2000(6.0mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (0.5 wt% THF solution)

[0031] The component (A) may be a single type, or a mixture of two or more types differing in molecular weight (degree of polymerization) or molecular structure.

[0032] [(B) Component] The surface-treated reinforcing silica of component (B) acts as a component that imparts excellent mechanical properties to the resulting millable-type fluorosilicone rubber composition. The reinforcing silica may be either precipitated silica (wet silica) or fumed silica (dry silica). In the present invention, the surface-treated reinforcing silica of component (B) has a specific surface area of ​​50 m2 or less as measured by the BET method. 2 / g or more, and preferably 100 to 400m 2 / g. This specific surface area is 50m 2 If the viscosity is less than 400 m / g, the reinforcing effect of component (B) will be insufficient. 2 When the viscosity is not more than 1000g / g, the viscosity does not become too high, and there is no risk of the moldability decreasing, which is preferable.

[0033] The reinforcing silica of component (B) is surface-treated with an organosilicon compound such as silanol-containing organopolysiloxane, organopolysilazane, chlorosilane, alkoxysilane, etc. These reinforcing silicas may be used alone or in combination of two or more.

[0034] The amount of reinforcing silica (B) added is 10 to 100 parts by mass, preferably 15 to 80 parts by mass, and more preferably 20 to 70 parts by mass, per 100 parts by mass of the organopolysiloxane (A). If the amount added is outside the above range, not only will the processability of the silicone rubber composition decrease, but the mechanical properties of the cured silicone rubber will also be insufficient.

[0035] [(C) component] Examples of organic peroxides include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, 2,4-dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-butyl peroxide, t-butyl perbenzoate, and 1,6-hexanediol-bis-t-butylperoxycarbonate.

[0036] The amount of organic peroxide blended is a catalytic amount relative to 100 parts by mass of component (A), and is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass. A blend amount of 0.1 parts by mass or more relative to 100 parts by mass of component (A) is preferred because sufficient curing is achieved, while an addition of 10 parts by mass or less is preferred because discoloration of the cured silicone rubber due to decomposition residues of the organic peroxide can be prevented.

[0037] [Other ingredients] In addition to the above-mentioned components, the millable fluorosilicone rubber composition of the present invention may optionally contain, as necessary, fillers such as crushed quartz, crystalline silica, diatomaceous earth, calcium carbonate, etc., colorants, tear strength improvers, acid acceptors, thermal conductivity improvers such as alumina and boron nitride, release agents, and filler dispersants such as various alkoxysilanes, particularly phenyl-containing alkoxysilanes and their hydrolysates, diphenylsilanediol, carbon functional silane, and other fillers and additives known in thermosetting silicone rubber compositions.

[0038] [Method of producing the composition] The millable type fluorosilicone rubber composition of the present invention can be obtained by mixing the components constituting the composition using a known mixer such as a kneader, a Banbury mixer, a twin roll mixer, etc. When using a composition containing the above-mentioned components (A) to (C) as the millable type fluorosilicone rubber composition, it is preferable to first mix components (A) and (B) to obtain a mixture, and then add component (C) to the mixture.

[0039] When the composition containing the components (A) to (C) further contains other components, it is preferable to first mix the components (A), (B), and the other components to obtain a mixture, and then add the component (C) to the mixture.

[0040] [Curing conditions] The millable type fluorosilicone rubber composition of the present invention can be cured by a known curing method under known curing conditions. Specifically, the composition can be cured by heating at a temperature of usually 25 to 200° C., preferably 80 to 160° C. The heating time may be about 0.5 minutes to 5 hours, and particularly about 1 minute to 3 hours. The millable type fluorosilicone rubber composition of the present invention may be cured under pressure.

[0041] [Cured product] As described above, the composition of the present invention can be cured to obtain a cured product. This cured product exhibits excellent amine resistance and is less susceptible to deterioration in physical properties even when in contact with an amine-based antioxidant. The cured product of the composition of the present invention is suitable for rubber parts for use in the vicinity of transport engines. Rubber parts for use in the vicinity of transport engines made of such a cured product are preferred because they are less susceptible to deterioration in physical properties even when they come into contact with amine-based antioxidants contained in gasoline fuels, oils, etc. EXAMPLES

[0042] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.

[0043] [Oil resistance measurement] The hardness (Durometer A) and initial volume change rate (%) of the cured products of the millable type fluorosilicone rubber compositions prepared in the following Examples and Comparative Examples were measured in accordance with JIS K 6249:2003. The test sheets were immersed in IRM903 (manufactured by Japan San Oil) at 150°C for 70 hours, after which the hardness and volume change rate were measured. The results are shown in Table 1.

[0044] [Amine resistance measurement] For the millable type fluorosilicone rubber compositions prepared in the following examples and comparative examples, the obtained full compounds were pressure molded at 165°C for 10 minutes, cured, and then post-cured at 200°C for 4 hours to prepare small cylindrical test pieces for measuring compression set with a diameter of 13 mm and a height of 6.3 mm. The measurement method was based on JIS K 6262:2013 to measure the initial value of compression set. The test pieces were immersed at room temperature for 168 hours at 120°C in a 1% by mass IRM903 solution of N,N'-di-sec-butyl-p-phenylenediamine or a 10% ethanol solution of N,N'-bis(salicylidene)-1,2-propanediamine in a 25% compressed state, and then cooled to measure the compression set.

[0045] The following components were used as component (A): (A-1): Organopolysiloxane raw rubber represented by the following formula, consisting of 66.53 mol % dimethylsiloxane units, 0.27 mol % methylvinylsiloxane units, 33.00 mol % methylnonafluorohexylmethylsiloxane units, and 0.03 mol % methylvinylsiloxy units (number of vinyl groups per molecule: 18), and having an average degree of polymerization of 6,000. [ka]

[0046] (A-2): Organopolysiloxane raw rubber having an average degree of polymerization of 6,000, consisting of 33.70 mol% dimethylsiloxane units, 0.27 mol% methylvinylsiloxane units, 66.00% methylnonafluorohexylmethylsiloxane units, and 0.03 mol% methylvinylsiloxy units (number of vinyl groups per molecule: 18), as shown in the following formula: [ka]

[0047] (A-3): Organopolysiloxane raw rubber represented by the following formula, consisting of 33.20 mol% dimethylsiloxane units, 0.20 mol% methylvinylsiloxane units, 66.47% methylnonafluorohexylmethylsiloxane units, and 0.13 mol% methylvinylsiloxy units (number of vinyl groups per molecule: 6), and having an average degree of polymerization of 2,022. [ka]

[0048] The following components were used as component (B): (B):Specific surface area 130m 2 / g of dry silica (manufactured by Nippon Aerosil Co., Ltd., product name: Aerosil 130)

[0049] The following components were used as component (C): (C) 2,5-Dimethyl-2,5-di(t-butylperoxy)hexane

[0050] [Example 1] 100 parts by mass of component (A-1) were mixed with 40 parts by mass of component (B) and 10 parts by mass of diphenylsilanediol as a dispersant, and the mixture was uniformly kneaded with a two-roll mill, heat-treated at 150°C for 4 hours, and then mixed with a two-roll mill to obtain the silicone-based compound A1, which serves as the base. 0.8 parts by mass of paste containing 80% by mass of component (C) (corresponding to 0.64 parts by mass of component (C) relative to 100 parts by mass of component (A-1)) was added to 100 parts by mass of the obtained compound A1, and the mixture was uniformly mixed with a two-roll mill to obtain a silicone rubber full compound (fluorosilicone rubber composition). Test sheets and cured products were prepared from the obtained composition, and various physical properties were evaluated. The results are shown in Table 1.

[0051] [Example 2] 100 parts by mass of component (A-2) were mixed with 40 parts by mass of component (B) and 10 parts by mass of diphenylsilanediol as a dispersant, and the mixture was uniformly kneaded with a two-roll mill, heat-treated at 150°C for 4 hours, and then mixed with a two-roll mill to obtain the silicone-based compound A2. 0.8 parts by mass of paste containing 80% by mass of component (C) (corresponding to 0.64 parts by mass of component (C) per 100 parts by mass of component (A-2)) was added to 100 parts by mass of the obtained compound A2, and the mixture was uniformly mixed with a two-roll mill to obtain a silicone rubber full compound (fluorosilicone rubber composition). Test sheets and cured products were prepared from the obtained composition, and various physical properties were evaluated. The results are shown in Table 1.

[0052] [Example 3] 100 parts by mass of component (A-3) were mixed with 40 parts by mass of component (B) and 10 parts by mass of diphenylsilanediol as a dispersant, and the mixture was uniformly kneaded with a two-roll mill, heat-treated at 150°C for 4 hours, and then mixed with a two-roll mill to obtain the silicone-based compound A3 as the base. 0.8 parts by mass of paste containing 80% by mass of component (C) (corresponding to 0.64 parts by mass of component (C) per 100 parts by mass of component (A-3)) was added to 100 parts by mass of the obtained compound A3, and the mixture was uniformly mixed with a two-roll mill to obtain a silicone rubber full compound (fluorosilicone rubber composition). Test sheets and cured products were prepared from the obtained composition, and various physical properties were evaluated. The results are shown in Table 1.

[0053] [Comparative Example 1] In Example 1, the (A-1) component was replaced with 100 parts by mass of organopolysiloxane raw rubber (A-4) consisting of 99.85 mol% dimethylsiloxane unit, 0.125 mol% methylvinylsiloxane unit, and 0.025 mol% dimethylvinylsiloxy unit (number of vinyl groups in one molecule: 10) and an average degree of polymerization of 6,000, and 40 parts by mass of the (B) component and 10 parts by mass of diphenylsilanediol as a dispersant were added and uniformly kneaded with a two-roll mill, heat-treated at 150°C for 4 hours, and then mixed and plasticized with a two-roll mill to obtain a silicone-based compound A4 as a base. Thereafter, a full compound of silicone rubber (fluorosilicone rubber composition) was prepared from the obtained compound A4 in the same manner as in Example 1, and a test sheet and a cured product were prepared from the obtained composition, and various physical properties were evaluated. The results are shown in Table 1.

[0054] [Comparative Example 2] In Example 1, component (A-1) was replaced with organopolysiloxane raw rubber (A-5) represented by the following formula: 0.15 mol% dimethylsiloxane unit, 0.37 mol% methylvinylsiloxane unit, 99.48 mol% methyltrifluoropropyl unit, 0.025 mol% dimethylvinylsiloxy unit, and 0.025 mol% dimethylhydroxysiloxy unit (number of vinyl groups in one molecule: 16), with an average degree of polymerization of 4,021. 40 parts by mass of component (B) and 10 parts by mass of diphenylsilanediol as a dispersant were added, and the mixture was uniformly kneaded using a two-roll mill, heat-treated at 150°C for 4 hours, and then mixed and plasticized using a two-roll mill to obtain the base silicone base compound A5. Thereafter, a silicone rubber full compound (fluorosilicone rubber composition) was prepared from the obtained compound A5 in the same manner as in Example 1, and test sheets and cured products were prepared from the obtained composition, and various physical properties were evaluated. The results are shown in Table 1. [ka]

[0055] [Comparative Example 3] In Example 1, component (A-1) was replaced with organopolysiloxane raw rubber (A-6) represented by the following formula: 49.74 mol% dimethylsiloxane unit, 0.37 mol% methylvinylsiloxane unit, 49.84 mol% methyltrifluoropropyl unit, 0.025 mol% dimethylvinylsiloxy unit, and 0.025 mol% dimethylhydroxysiloxy unit (number of vinyl groups in one molecule: 16), with an average degree of polymerization of 4,021. 40 parts by mass of component (B) and 10 parts by mass of diphenylsilanediol as a dispersant were added, and the mixture was uniformly kneaded using a two-roll mill, heat-treated at 150°C for 4 hours, and then mixed and plasticized using a two-roll mill to obtain the base silicone base compound A6. Thereafter, a silicone rubber full compound (fluorosilicone rubber composition) was prepared from the obtained compound A6 in the same manner as in Example 1, and test sheets and cured products were prepared from the obtained composition, and various physical properties were evaluated. The results are shown in Table 1. [ka]

[0056] [Table 1]

[0057] In the oil resistance measurement, Examples 1 to 3 were superior to the comparative examples, except that the volume change rate was equivalent to that of Comparative Example 2. As for the compression set measured for amine resistance, Examples 1 to 3 were better than each of the comparative examples. As for Comparative Example 2, which was equivalent in the volume change rate, the compression set measured after immersion in a 1% by mass IRM903 solution of N,N'-di-sec-butyl-p-phenylenediamine was significantly inferior to the examples. That is, it is clear that Examples 1 to 3 are superior to the Comparative Example in amine resistance, and achieve both excellent oil resistance and amine resistance.

[0058] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. (A) Formula (1) below 【Chemistry 1】 (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 is an alkenyl group having 2 to 8 carbon atoms, a and b are each an integer of 1 or more, c is an integer of 0 or more, a+b+c=2,000 to 6,000, and a / (a+b+c)=0.3 to 0.

8. The bonds of the siloxane units bounded by a, b, and c may be block or random. Raw rubber-like organopolysiloxane represented by the formula: 100 parts by mass, (B) A material with a specific surface area of ​​50 m2 measured by the BET method 2 / g or more of surface-treated reinforcing silica; 10 to 100 parts by mass, (C) Organic peroxide; catalytic amount, A millable type fluorosilicone rubber composition comprising:

2. 2. A rubber part for use around the engine of a transport aircraft, which comprises a cured product of the millable type fluorosilicone rubber composition of claim 1.

Citation Information

Patent Citations

  • Fluorosilicone polymer, processes for the production thereof and composition containing it

    EP0255957A2

  • Production of fluorosilicone polymer

    JP1988041535A

  • Polymerization of silicone polymer

    JP1988137924A

  • Production of fluorosilicone copolymer

    JP1988152634A

  • Production of crosslinkable fluorosilicone polymer

    JP1988152635A