Dispersion powder, manufacturing method of the same, heat-ray-shielding resin molding, and heat-ray-shielding laminate
The use of composite tungsten oxide fine particles with controlled dispersant ratios and particle sizes addresses the inefficiencies of existing heat ray shielding technologies, offering high weather resistance and effective near-infrared blocking with minimal visible light reduction.
Patent Information
- Application Number
- JP2023146003
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-09-08
- Publication Date
- 2024-11-08
AI Technical Summary
Existing heat ray shielding technologies face challenges such as high cost, complexity in production, poor adhesion, and lack of weather resistance, leading to inefficiencies in blocking near-infrared rays while maintaining visible light transmission.
A dispersion powder comprising composite tungsten oxide fine particles with a hexagonal crystal structure, modified with an acrylic dispersant, is used to create a heat ray shielding resin molded body and laminate, allowing for high content of heat ray shielding particles and improved weather resistance through controlled particle size and dispersant ratio.
The solution achieves high weather resistance and efficient near-infrared shielding with minimal impact on visible light transmission, reducing energy consumption and providing an environmentally friendly solution for heat ray shielding applications.
Smart Images

Figure 2024159408000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion powder that can be applied to the production of a heat ray shielding resin molding having high weather resistance, etc., a production method thereof, a heat ray shielding resin molding having high weather resistance to which the dispersion powder is applied, and a heat ray shielding laminate having high weather resistance. [Background technology]
[0002] The sunlight entering through so-called openings such as windows and doors of various buildings and vehicles contains ultraviolet rays and infrared rays in addition to visible light. Among the infrared rays contained in the sunlight, near infrared rays with wavelengths of 800 to 2500 nm are called heat rays, and when they enter through openings, they cause the temperature inside the room to rise. To solve this problem, in recent years, in the field of window materials for various buildings and vehicles, there has been a rapid demand for heat ray shielding substrates that can sufficiently let in visible light while shielding heat rays, and suppress the rise in temperature inside the room while maintaining brightness, and many patents related to heat ray shielding substrates have been proposed.
[0003] For example, Patent Documents 1 to 3 propose a heat ray shielding plate in which a heat ray reflective film formed by vapor-depositing a metal or metal oxide on a transparent resin film is bonded to a transparent substrate such as glass, an acrylic plate, or a polycarbonate plate. However, these heat ray shielding plates have the disadvantage that the heat ray reflective film itself is very expensive and requires complicated processes such as a bonding process, resulting in high costs. In addition, since the adhesion between the transparent substrate and the heat ray reflective film is poor, there is also the disadvantage that the film peels off due to changes over time. Furthermore, many heat ray shielding plates have been proposed in which a metal or metal oxide is directly vapor-deposited on the surface of a transparent substrate. However, when manufacturing these heat ray shielding plates, a device that requires high vacuum and highly accurate atmosphere control is required, which causes problems such as poor mass productivity and poor versatility.
[0004] In addition, for example, Patent Documents 4 and 5 propose heat ray shielding plates and films in which organic near infrared absorbing agents, such as phthalocyanine compounds and anthraquinone compounds, are kneaded into thermoplastic transparent resins, such as polyethylene terephthalate resin, polycarbonate resin, acrylic resin, polyethylene resin, and polystyrene resin. However, in these heat ray shielding plates and films, a large amount of near infrared absorbing agent must be blended in order to sufficiently shield heat rays, but the blending of a large amount of near infrared absorbing agent reduces the visible light transmittance, which is a problem that remains. In addition, since an organic compound is used as the near infrared absorbing agent, there are problems with weather resistance when applied to window materials of buildings and vehicles that are constantly exposed to direct sunlight, and it cannot be said that it is necessarily suitable.
[0005] Under such technical background, the present applicant has focused on hexaborides having a large amount of free electrons, and has disclosed in Patent Documents 6 to 8 a coating liquid for forming a heat ray shielding film, which is constituted by dispersing a hexaboride as a heat ray shielding component in an organic solvent and adding various binders, and a heat ray shielding film obtained by applying this coating liquid to various transparent substrates and then curing the coating liquid, etc.
[0006] However, in these inventions, the hexaboride fine particles as the heat ray shielding component are assumed to be dispersed in an organic solvent, and therefore the coating solution for forming the heat ray shielding film is treated as a dangerous material under the Fire Service Act, and there are various restrictions on the transportation of the coating solution for forming the heat ray shielding film, resulting in high transportation costs.
[0007] In addition, when a dispersion of hexaboride microparticles as a heat ray shielding component dispersed in an organic solvent is stored for a long period of time, the microparticles are prone to agglomeration due to Brownian motion, which can result in the formation of precipitates.
[0008] Furthermore, when the hexaboride particles are mixed into the transparent resin material and molded, the hexaboride particles are dispersed in an organic solvent, so it is necessary to mix the hexaboride particles uniformly into the transparent resin material while removing the organic solvent. This poses the problem that the equipment and processes used are complicated and this is not necessarily the optimal method.
[0009] The present applicant has disclosed in Patent Document 9 a highly heat-resistant masterbatch that contains a thermoplastic resin, tungsten oxide microparticles and / or composite tungsten oxide microparticles having a hexagonal crystal structure, and a highly heat-resistant dispersant having a thermal decomposition temperature of 230°C or higher, and satisfies the range of 10≧[weight of highly heat-resistant dispersant / (weight of tungsten oxide microparticles and / or composite tungsten oxide microparticles)]≧0.5. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 61-277437 [Patent Document 2] Japanese Patent Application Publication No. 10-146919 [Patent Document 3] JP 2001-179887 A [Patent Document 4] Japanese Patent Application Publication No. 6-256541 [Patent Document 5] Japanese Patent Application Publication No. 6-264050 [Patent Document 6] Japanese Patent Application Publication No. 11-181336 [Patent Document 7] JP 2000-96034 A [Patent Document 8] JP 2000-169765 A [Patent Document 9] JP 2008-024902 A Summary of the Invention [Problem to be solved by the invention]
[0011] However, in the high heat resistance masterbatch described in Patent Document 9, in order to disperse the tungsten oxide fine particles and / or composite tungsten oxide fine particles, which are heat ray shielding fine particles, in the thermoplastic resin, it was necessary to add a large amount of high heat resistance dispersant. Therefore, the ratio of the heat ray shielding fine particles in the fine particle dispersion powder was low, and there was room for improvement in the content. In addition, Patent Document 9 does not describe weather resistance, leaving room for further study. The present invention has been made under the above-mentioned circumstances, and the problem to be solved by the present invention is to provide a heat-ray shielding resin molding and a heat-ray shielding laminate that have excellent weather resistance, high transmittance in the visible light range, and exhibit excellent heat-ray shielding function, and to provide a dispersion powder for producing them. [Means for solving the problem]
[0012] Under the above circumstances, the inventors conducted research and came up with the idea of a dispersion powder with a large concentration adjustment margin and a manufacturing method thereof by significantly increasing the content of heat-shielding microparticles in the dispersion powder so that it can be adjusted by adding a dilution solvent as appropriate, as well as a heat-shielding resin molding having high weather resistance and a heat-shielding laminate having high weather resistance to which said dispersion powder is applied, and completed the present invention.
[0013] That is, the first invention according to the present invention is: The present invention relates to a tungsten oxide composite material having a hexagonal crystal structure, a crystallite size of 15 nm or more and 80 nm or less, and a surface-modified acrylic dispersant. The tungsten oxide composite material has a hexagonal crystal structure, a crystallite size of 15 nm or more and 80 nm or less, and a surface-modified acrylic dispersant. The dispersion powder is characterized in that the weight ratio of the dispersant to the composite tungsten oxide fine particles is in the range of 0.3≦(weight of dispersant / weight of composite tungsten oxide fine particles)<3.0. The second invention is The acrylic dispersant is a dispersion powder according to the first aspect of the present invention, characterized in that it has an acidic functional group as a functional group. The third invention is The dispersed powder according to the first or second invention is characterized in that the M element contained in the composite tungsten oxide fine particles is at least one selected from the group consisting of Cs, Rb, K, Tl and Ba. The fourth invention is a composite tungsten oxide microparticle having a hexagonal crystal structure represented by the general formula MxWOy (wherein M element is one or more elements selected from the group 1, group 2 and group 13 elements in the periodic table, 0.1≦x≦1.0, 2.0≦y<4.0) and an acrylic dispersant are added to an organic solvent, and then the resultant is subjected to a pulverization and dispersion treatment to produce a dispersion in which the composite tungsten oxide microparticles have a crystallite diameter of 15 nm or more and 80 nm or less; The method for producing a dispersed powder is characterized in that the organic solvent is removed from the dispersion liquid to produce a dispersed powder in which the weight ratio of the dispersant to the composite tungsten oxide microparticles is in the range of 0.3≦(weight of dispersant / weight of composite tungsten oxide microparticles)<3.0. The fifth invention is The heat ray shielding resin molded body is obtained by diluting and kneading the dispersed powder according to the first or second invention with a thermoplastic resin molding material, and molding the mixture into a predetermined shape. The sixth invention is The heat ray shielding resin molding according to a fifth aspect of the present invention is characterized in that the thermoplastic resin molding material is a polycarbonate resin or an acrylic resin. The seventh invention is The heat ray shielding laminate is characterized in that the heat ray shielding molded resin article according to the fifth invention is laminated with another molded article. Effect of the Invention
[0014] The dispersed powder according to the present invention can be diluted and kneaded with a thermoplastic resin molding material, and further molded into any shape such as a film by a known method such as extrusion molding, injection molding, compression molding, etc. to obtain a heat ray shielding resin molded product having high weather resistance. By applying the obtained heat ray shielding resin molded product having high weather resistance to, for example, automobiles, building windows, carports, arcades, etc., it is possible to block incoming solar energy and reduce the cooling load and the heat sensation felt by people, and is also useful for energy saving and highly useful from an environmental perspective. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The dispersed powder according to the present invention is composed of composite tungsten oxide microparticles having a hexagonal crystal structure and represented by the general formula MxWOy (wherein M element is one or more elements selected from the elements of Groups 1, 2 and 13 of the periodic table, 0.1≦x≦1.0, 2.0≦y<4.0), which have been surface-modified with an acrylic dispersant. The heat-shielding resin molding and heat-shielding laminate according to the present invention are produced using the dispersed powder.
[0016] The dispersion powder, the heat ray shielding molded resin product having high weather resistance, and the heat ray shielding laminate having high weather resistance according to the present invention will be described below in the following order. 1) Composite tungsten oxide particles for use as dispersion powder 2) Manufacturing method of composite tungsten oxide microparticles used for dispersion powder 3) Dispersants used in dispersed powders 4) Manufacturing method of composite tungsten oxide microparticle dispersion liquid used for dispersion powder 5) Manufacturing method of dispersed powder 6) Thermoplastic resins used in heat-shielding resin moldings 7) Method for dispersing powder into thermoplastic resin 8) Method for producing heat ray shielding resin molded body and heat ray shielding laminate
[0017] 1) Composite tungsten oxide particles for use as dispersion powder The composite tungsten oxide microparticles used as a heat ray shielding material in the dispersion powder according to the present invention largely absorb light in the near infrared region, particularly in the vicinity of a wavelength of 1000 nm, and therefore often have a blue-based transmitted color tone. The particle size of the near infrared ray shielding material can be appropriately selected depending on the purpose of use.
[0018] First, when used in applications that require transparency, the composite tungsten oxide microparticles preferably have a dispersion particle diameter of 800 nm or less. Dispersion particle diameters smaller than 800 nm do not completely block light due to scattering, and can maintain visibility in the visible light range while efficiently maintaining transparency at the same time. In particular, when transparency in the visible light range is important, it is preferable to further consider scattering by particles.
[0019] In addition, when the reduction of scattering by the particles is important, the dispersion particle diameter of the composite tungsten oxide microparticles is 200 nm or less, preferably 100 nm or less. The reason is that if the dispersion particle diameter of the dispersion particles is small, the scattering of light in the visible light region of wavelengths of 400 nm to 780 nm due to geometric scattering or Mie scattering is reduced. As a result of the reduction in the scattering of light, it is possible to avoid the near-heat ray shielding resin molded body becoming like cloudy glass, which makes it difficult to obtain clear transparency. That is, when the dispersion particle diameter of the dispersion particles is 200 nm or less, the geometric scattering or Mie scattering is reduced, and the Rayleigh scattering region is reached. In the Rayleigh scattering region, the scattered light is proportional to the sixth power of the particle diameter, so the scattering is reduced with the reduction in the dispersion particle diameter, and the transparency is improved. Furthermore, when the dispersion particle diameter is 100 nm or less, the scattered light is very small, which is preferable. From the viewpoint of avoiding the scattering of light, it is preferable that the dispersion particle diameter is small, and if the dispersion particle diameter is 1 nm or more, industrial production is easy.
[0020] The composite tungsten oxide microparticles are represented by the general formula MxWOy (wherein M element is one or more elements selected from the elements of Groups 1, 2, and 13 in the periodic table, 0.1≦x≦1.0, 2.0≦y<4.0) and have a hexagonal crystal structure. Preferably, the composite tungsten oxide microparticles include M element containing at least one selected from Cs, Rb, K, Tl, and Ba. The amount x of the M element is preferably 0.1 or more and 1.0 or less, and more preferably about 0.33. This is because the value theoretically calculated from the hexagonal crystal structure is 0.33, and preferable optical properties can be obtained with an amount of addition around this value. The range of y is preferably 2.0≦y<4.0.
[0021] Here, a typical example of the composite tungsten oxide material is Cs 0.33 WO3, Rb 0.33 WO3, K 0.33 WO3, Ba 0.33 WO3, etc., and as long as x and y fall within the above ranges, useful near-infrared shielding properties can be obtained.
[0022] 2) Manufacturing method of composite tungsten oxide microparticles used for dispersion powder a) Thermochemical production method The composite tungsten oxide fine particles can be obtained by subjecting a starting tungsten compound material to a heat treatment in an inert gas atmosphere or a reducing gas atmosphere, and then subjecting the material to a mild oxidation treatment.
[0023] The tungsten compound starting material is preferably at least one selected from tungsten trioxide powder, tungsten dioxide powder, tungsten oxide hydrate, tungsten hexachloride powder, ammonium tungstate powder, tungsten oxide hydrate powder obtained by dissolving tungsten hexachloride in alcohol and then drying, tungsten oxide hydrate powder obtained by dissolving tungsten hexachloride in alcohol, adding water to precipitate and drying the precipitate, tungsten compound powder obtained by drying an aqueous solution of ammonium tungstate, and metallic tungsten powder.
[0024] Here, when producing composite tungsten oxide microparticles, it is more preferable to use ammonium tungstate aqueous solution or tungsten hexachloride solution, because the starting material is a solution, and each element can be easily mixed uniformly.By using these raw materials and heat treating them in an inert gas atmosphere or reducing gas atmosphere, composite tungsten oxide microparticles of the above-mentioned particle size can be obtained.
[0025] When producing the composite tungsten oxide microparticles, the M element is further added in the form of a simple element or a compound to the starting tungsten compound material to obtain a starting material for the composite tungsten compound.
[0026] Here, in order to produce a starting material in which each component is mixed uniformly at the molecular level, it is preferable to mix each raw material in the form of a solution. Therefore, it is preferable that the tungsten compound starting material containing element M is soluble in a solvent such as water or an organic solvent. For example, tungstate, chloride salt, nitrate, sulfate, oxalate, oxide, carbonate, hydroxide, etc. containing element M can be mentioned, but is not limited thereto, and any material that can be in a solution state can be used.
[0027] The heat treatment conditions in the inert atmosphere are preferably 650° C. or higher. The starting material heat-treated at has sufficient near-infrared absorption power and is efficient as a heat ray shielding fine particle. As the inert gas, an inert gas such as Ar or N2 can be used.
[0028] On the other hand, as the heat treatment conditions in the reducing atmosphere, it is preferable to first heat treat the starting material in a reducing gas atmosphere at 300°C to 1000°C, and then heat treat it in an inert gas atmosphere at a temperature of 650°C to 1200°C. The reducing gas at this time is not particularly limited, but H2 is preferable. When H2 is used as the reducing gas, the composition of the reducing atmosphere is preferably a mixture of inert gas such as Ar and N2 with H2 at a volume ratio of 0.1% or more, more preferably 0.2% or more. If H2 is 0.1% or more by volume, reduction can be efficiently promoted.
[0029] The composite tungsten oxide microparticles exhibiting the near-infrared shielding function of the present embodiment are preferably surface-treated with at least one selected from the group consisting of silane compounds, titanium compounds, aluminum compounds, and zirconia compounds, and the surfaces of the microparticles are coated with a compound containing one or more of Si, Ti, Zr, and Al, thereby improving weather resistance.
[0030] b) Plasma-based manufacturing method The method for producing composite tungsten oxide microparticles using the plasma method will be described item by item.
[0031] (I) Raw material preparation As the starting material, a raw material mixture of a tungsten compound and an M element compound, or a composite tungsten oxide precursor represented by the general formula MxWOy can be used. As the tungsten compound and the M element compound, the same materials as those explained in the above-mentioned thermochemical production method can be suitably used.
[0032] When preparing a raw material mixture of a tungsten compound and an M element compound as starting materials, the respective raw materials are blended and mixed such that the ratio of the M element to tungsten in the raw material mixture of the tungsten compound and the M element compound is equal to the ratio of x to y in the general formula of the target composite tungsten oxide.
[0033] Further, when using a composite tungsten oxide precursor represented by the general formula MxWOy as a starting material, it is preferable to satisfy 0.001 ≦ x ≦ 1.0 and 2.0 < y. The composite tungsten oxide precursor represented by the general formula MxWOy can be synthesized, for example, by the above-described thermochemical production method.
[0034] (II) Plasma device and reaction conditions As the plasma used for producing the composite tungsten oxide fine particles, for example, any one of a direct current arc plasma, a high-frequency plasma, a microwave plasma, a low-frequency alternating current plasma, or a superposition thereof, or a plasma obtained by an electrical method in which a magnetic field is applied to a direct current plasma, a high-output laser, or a high-output electron beam or ion beam can be used. Hereinafter, a hybrid plasma reactor in which a direct current plasma device and a high-frequency plasma device are superimposed will be described as an example.
[0035] As the carrier gas for transporting the starting material in the reaction step, a mixed gas of an inert gas and an oxygen gas can be used. The plasma can be generated, for example, in an atmosphere of an inert gas alone or a mixed gas of an inert gas and a hydrogen gas. According to the plasma method, for example, composite tungsten oxide fine particles having a single crystal phase can be produced.
[0036] The high-frequency power source is not particularly limited, but for example, a high-frequency power source having a frequency of about 4 MHz and an output of 15 kW or more and 50 kW or less is used.
[0037] When a thermal plasma is used, it is a thermal plasma having a high temperature portion of 10,000 K or more, more preferably 10,000 K or more and 25,000 K or less, and in particular, a plasma capable of controlling the generation time of particles is used.
[0038] (III) Production of composite tungsten oxide particles using plasma The reaction system is evacuated to a vacuum using a vacuum exhaust device. The degree of vacuum is not particularly limited, but for example, it can be evacuated to about 0.1 Pa. After the reaction system is evacuated to a vacuum, the reaction system is filled with argon gas. For example, it is preferable to make the reaction system an argon gas flow system at 1 atmosphere.
[0039] Thereafter, a plasma gas is supplied into the reaction vessel. The plasma gas is not particularly limited, but may be any gas selected from the group consisting of argon gas, a mixed gas of argon and helium (Ar-He mixed gas), a mixed gas of argon and nitrogen (Ar-N2 mixed gas), neon, helium, and xenon.
[0040] The flow rate of the plasma gas supplied is not particularly limited, but may be, for example, 3 L / min to 30 L / min, preferably 3 L / min to 15 L / min.
[0041] On the other hand, outside the plasma region, a sheath gas is supplied from a sheath gas inlet for generating high-frequency plasma and protecting the quartz tube. The type and supply rate of the sheath gas are not particularly limited, but for example, argon gas is supplied at 20 L / min to 50 L / min and hydrogen gas is supplied at 1 L / min to 5 L / min to generate high-frequency plasma.
[0042] After the hybrid plasma is generated, the raw material is introduced from a raw material powder carrier gas supply port using a carrier gas. The carrier gas is not particularly limited, but for example, a mixed gas consisting of argon gas at 1 L / min to 8 L / min and oxygen gas at 0.001 L / min to 0.8 L / min is used. The supply rate of the starting material from the raw material powder carrier gas supply port is, for example, preferably 1 g / min to 50 g / min, more preferably 1 g / min to 20 g / min.
[0043] The starting material supplied to the plasma instantly evaporates in the plasma and undergoes a condensation process to generate composite tungsten oxide microparticles with an average primary particle size of 100 nm or less. The particle size of the composite tungsten oxide microparticles can be easily controlled by the plasma output, plasma flow rate, amount of supplied raw material powder, etc.
[0044] In order to obtain a desired near-infrared shielding resin molded body using the composite tungsten oxide microparticles produced by the above-described thermochemical production method or plasma-based production method, it is desirable that the powder color of the composite tungsten oxide microparticles satisfy the following conditions in the L*a*b* color system (JIS Z 8729) recommended by the International Commission on Illumination (CIE): L* is 25 to 80, a* is -10 to 10, and b* is -15 to 15.
[0045] By using the composite tungsten oxide fine particles, it is possible to obtain desired optical properties as a near-infrared shielding resin sheet material.
[0046] 3) Dispersants used in dispersed powders Dispersants are used for the purpose of hydrophobizing the surface of composite tungsten oxide particles. Dispersants can be selected according to the dispersion system, which is a combination of composite tungsten oxide particles, dispersion medium, coating resin raw material, etc., but acrylic dispersants are preferred, and those having acidic functional groups as functional groups are more preferred. Examples include hydroxyl groups, carboxyl groups, phosphate groups, and sulfo groups. Carboxyl groups are the most preferred.
[0047] The weight-average molecular weight of the dispersant is 15,000 or more and 80,000 or less, and more preferably 20,000 or more and 40,000 or less. If the weight-average molecular weight is higher than 15,000, the dispersion stability is good and the aggregation of the composite tungsten oxide microparticles is suppressed. If the weight-average molecular weight is lower than 80,000, the composite tungsten oxide microparticles can be easily pulverized.
[0048] The acid value of the dispersant is preferably 3.0 mgKOH / g or more and 20.0 mgKOH / g or less, more preferably 5.0 mgKOH / g or more and 15.0 mgKOH / g or less. If the acid value is higher than 3.0 mgKOH / g, the dispersibility of the composite tungsten oxide microparticles is good. If the acid value is 20.0 mgKOH / g or less, the compatibility of the dispersant with the organic solvent is good, and the dispersibility of the composite tungsten oxide microparticles is good.
[0049] In addition, the glass transition temperature of the dispersant (the temperature at which it softens when heated above a certain temperature) should be between 90° C. and 150° C. If the glass transition temperature is 90° C. or higher, the dispersed powder can be melt-kneaded into the resin at a temperature range of 250° C. to 300° C.
[0050] It has been found that a heat-shielding resin molded body having high weather resistance and a heat-shielding laminate having high weather resistance can be obtained by adjusting the weight ratio of the dispersant to the composite tungsten oxide fine particles to the range of 0.3≦(weight of dispersant / weight of composite tungsten oxide)<3.0, more preferably 0.3≦(weight of dispersant / weight of composite tungsten oxide)≦1.0, 0.3≦(weight of dispersant / weight of composite tungsten oxide)≦0.8, and even more preferably 0.3≦(weight of dispersant / weight of composite tungsten oxide)≦0.5, depending on the amount of acrylic dispersant having an acidic functional group added to the composite tungsten oxide fine particles. As a result, it has become possible to achieve both the viewpoint of obtaining a dispersion powder with a large concentration adjustment margin by significantly increasing the content of the heat-shielding fine particles in the dispersion powder and the viewpoint of obtaining a heat-shielding resin molded body having high weather resistance and a heat-shielding laminate having high weather resistance.
[0051] This is believed to be because the composite tungsten oxide microparticles according to the present invention, which have a large crystallite size, are less likely to suffer damage to the crystal structure due to the effect of preventing the occurrence of loss of constituent elements even when mixed and pulverized during the production of a dispersion liquid, as described below, thereby ensuring high weather resistance. On the other hand, the present inventors have found that when the weight ratio of the dispersant to the composite tungsten oxide microparticles exceeds 3.0, the weather resistance decreases. It is believed that the decrease in weather resistance occurs due to a chemical reaction between the dispersant and the composite tungsten oxide microparticles.
[0052] 4) Manufacturing method of composite tungsten oxide microparticle dispersion liquid used for dispersion powder In the manufacturing process of the composite tungsten oxide microparticle dispersion used to manufacture the dispersed powder, the dispersion can be manufactured by mixing the composite tungsten oxide microparticles, a dispersant, and a dispersion medium. From the viewpoint of reducing the dispersed particle size of the composite tungsten oxide microparticles and dispersing them uniformly in the dispersion, it is preferable to carry out a pulverization process of the composite tungsten oxide microparticles during mixing.
[0053] The dispersion medium may be any one that can disperse the composite tungsten oxide particles and the dispersant to form a dispersion liquid, and various organic compounds can be used. For example, one or more organic solvents selected from aromatic hydrocarbons such as toluene and xylene can be preferably used.
[0054] The mixing means used when mixing and pulverizing the composite tungsten oxide microparticles, the dispersant, and the dispersion medium is not particularly limited, and may be one or more selected from, for example, a bead mill, a ball mill, a sand mill, a paint shaker, an ultrasonic homogenizer, etc. In particular, as the mixing means, it is more preferable to use a media stirring mill such as a bead mill, a ball mill, a sand mill, or a paint shaker using a medium media such as beads, balls, or Ottawa sand. This is because the use of a media stirring mill can make the composite tungsten oxide microparticles have a desired dispersed particle size in a particularly short time, which is preferable from the viewpoint of productivity and suppressing the inclusion of impurities.
[0055] Here, from the viewpoint of making composite tungsten oxide microparticles exhibit transparency and high weather resistance, it is preferable to crush the composite tungsten oxide to a dispersion particle size of 15nm or more and 80nm or less, more preferably 20nm or more and 40nm or less, and even more preferably 30nm or more and 40nm or less.If the crystallite size of composite tungsten oxide microparticles is within this range, the weight ratio of the dispersant to the composite tungsten oxide microparticles is in the above-mentioned predetermined range, and thus the composite tungsten oxide microparticles exhibit both transparency and high weather resistance.
[0056] In order to achieve the above-mentioned object, the concentration of the composite tungsten oxide microparticles in the organic solvent, which is the dispersion medium, is preferably 5 to 50 mass%. If the concentration of the composite tungsten oxide microparticles is 5 mass% or more, the amount of organic solvent to be removed in the post-process can be reduced, and the manufacturing cost can be reduced. In addition, if the concentration of the composite tungsten oxide microparticles is 50 mass% or less, the microparticles do not aggregate, and the viscosity of the liquid does not increase, making it easy to handle.
[0057] 5) Manufacturing method of dispersed powder The drying step for obtaining the dispersion powder according to the present invention is a step performed to remove the organic solvent from the dispersion liquid. This step is preferably a method of drying the obtained dispersion liquid under reduced pressure. Specifically, the dispersion liquid is dried under reduced pressure while being stirred using a reduced pressure drying device, and the dispersion powder and the organic solvent component are separated. An example of the device used for the reduced pressure drying is a vacuum stirring type dryer, but any device having the above function may be used, and is not particularly limited. In addition, the pressure of the reduced pressure in the drying step is appropriately selected.
[0058] The reduced pressure drying method is preferable because it improves the efficiency of removing the organic solvent and does not expose the dispersed powder to high temperatures for a long time, which prevents aggregation of the dispersed fine particles. It also increases productivity and makes it easy to recover the evaporated organic solvent, which is preferable from an environmental perspective.
[0059] 6) Thermoplastic resins used in heat-shielding resin moldings The thermoplastic resin used in the present invention is not particularly limited as long as it is a transparent thermoplastic resin having a high light transmittance in the visible light region. For example, the thermoplastic resin may have a visible light transmittance of 50% or more according to JIS R 3106 and a haze of 30% or less according to JIS K7105 when molded into a 3 mm-thick plate-like molded product.
[0060] Specifically, examples of the resin include acrylic resin, polycarbonate resin, polyetherimide resin, polyester resin, polystyrene resin, polyethersulfone resin, fluorine resin, and polyolefin resin. When the heat ray shielding transparent resin substrate is intended to be used as a window material for various buildings and vehicles, acrylic resin, polycarbonate resin, polyetherimide resin, and fluorine resin are more preferable in terms of transparency, impact resistance, weather resistance, and the like.
[0061] The polycarbonate resin is preferably an aromatic polycarbonate. Examples of the aromatic polycarbonate include a polymer obtained by a known method such as interfacial polymerization, melt polymerization, or solid-state polymerization from one or more divalent phenol compounds such as 2,2-bis(4-hydroxyphenyl)propane and 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane and a carbonate precursor such as phosgene or diphenyl carbonate.
[0062] Examples of acrylic resins include polymers or copolymers that use methyl methacrylate, ethyl methacrylate, propyl methacrylate, or butyl methacrylate as the main raw material, and, if necessary, acrylic acid esters having an alkyl group having 1 to 8 carbon atoms, vinyl acetate, styrene, acrylonitrile, methacrylonitrile, etc. as copolymerization components. In addition, acrylic resins that have been polymerized in multiple stages can also be used.
[0063] Examples of the fluorine-based resin include polyethylene fluoride, polyethylene difluoride, polyethylene tetrafluoride, ethylene-ethylene difluoride copolymer, ethylene-ethylene tetrafluoride copolymer, and ethylene tetrafluoride-perfluoroalkoxyethylene copolymer.
[0064] 7) Method for dispersing powder into thermoplastic resin The method for dispersing the powder in the thermoplastic resin can be arbitrarily selected as long as the composite tungsten oxide particles contained in the powder can be uniformly dispersed in the resin. For example, first, a dispersion liquid is prepared by dispersing the dispersed powder in an arbitrary solvent using a method such as a bead mill, a ball mill, a sand mill, or ultrasonic dispersion. Next, the dispersion liquid, a dispersant, powder or pellets of a thermoplastic resin, and other additives as necessary are melt-mixed uniformly while removing the solvent from the dispersion liquid using a mixer such as a ribbon blender, a tumbler, a Nauter mixer, a Henschel mixer, a super mixer, or a planetary mixer, and a kneader such as a Banbury mixer, a kneader, a roll, a kneader ruder, a single-screw extruder, or a twin-screw extruder, to prepare a mixture in which the composite tungsten oxide fine particles are uniformly dispersed in the thermoplastic resin. The temperature during kneading is maintained at a temperature at which the thermoplastic resin used does not decompose.
[0065] As another method, the dispersion powder can be uniformly melt-mixed with powder or pellets of a thermoplastic resin, and, if necessary, with other additives, to prepare a mixture in which the composite tungsten oxide microparticles are uniformly dispersed in the thermoplastic resin. Alternatively, a method can be used in which the dispersion powder, thermoplastic resin powder or pellets, and, if necessary, other additives are melt-mixed uniformly. The dispersion method is not limited to these methods as long as the composite tungsten oxide particles are uniformly dispersed in the thermoplastic resin.
[0066] 8) Method for producing heat ray shielding resin molded body and heat ray shielding laminate Next, the heat ray shielding resin molded article of this embodiment is obtained by diluting and kneading the above-mentioned dispersed powder with a thermoplastic resin molding material, and molding it into a predetermined shape.
[0067] In the present embodiment, since the dispersed powder is used, it is easy to knead it into the thermoplastic resin, and the kneading process during molding of the heat ray shielding resin molded body can be completed in a short time. As a result, the dispersed powder itself is very little thermally deteriorated, and the composite tungsten oxide microparticles are sufficiently dispersed in the near-heat ray shielding resin molded body, so that the visible light transmittance is well secured and an excellent heat ray shielding function is exhibited.
[0068] The heat ray shielding resin molded body can be molded into any shape as required, and can be molded into a flat or curved shape. The thickness of the heat ray shielding resin molded body can be adjusted to any thickness as required. Furthermore, the resin sheet formed into a flat shape can be molded into any shape, such as a spherical shape, by post-processing.
[0069] The method for molding the heat ray shielding resin molded product may be any method such as injection molding, extrusion molding, compression molding, or rotational molding. In particular, a method for obtaining a molded product by injection molding and a method for obtaining a molded product by extrusion molding are preferably used. A method for obtaining a plate-shaped or film-shaped molded product by extrusion molding is produced by taking up a molten thermoplastic resin extruded using an extruder such as a T-die while cooling it with a cooling roll.
[0070] The above-mentioned heat ray shielding resin molded product can be used by itself as a structural material such as window glass, arcade, etc., or can be laminated by any method on other molded products such as inorganic glass, resin glass, resin film, etc., to form an integrated heat ray shielding laminate and used as a structural material. For example, a heat ray shielding laminate having a heat ray shielding function and a shatterproof function can be obtained by laminating and integrating a heat ray shielding resin molded product previously molded into a film shape on inorganic glass by a thermal lamination method.
[0071] It is also possible to obtain a heat ray shielding laminate by laminating and integrating the heat ray shielding resin molded body with another molded body at the same time as molding the heat ray shielding resin molded body by a thermal lamination method, a coextrusion method, a press molding method, an injection molding method, etc. The heat ray shielding laminate can be used as a more useful structural material by effectively utilizing the advantages of each molded body and complementing each other's disadvantages.
[0072] As described above in detail, by using a dispersed powder consisting of composite tungsten oxide microparticles and a dispersant as a heat ray shielding component, it is possible to provide a heat ray shielding resin molding and a heat ray shielding laminate that have excellent weather resistance and high transmittance in the visible light range and exhibit excellent heat ray shielding function, without using a costly physical film formation method or complicated processes. EXAMPLES
[0073] The present invention will be specifically described using examples, but the present invention is not limited to the following examples.
[0074] The visible light transmittance, 820 nm wavelength transmittance, 1000 nm wavelength transmittance, and 1500 nm wavelength transmittance of the produced heat ray shielding resin molding before and after the weather resistance test were measured using a spectrophotometer UH-4150 manufactured by Hitachi, Ltd. The Δ transmittance (= transmittance after weather resistance test - transmittance before weather resistance test) at each wavelength is an index showing weather resistance performance.
[0075] [Example 1] 17.7g of Cs2CO3 was dissolved in 39.9g of water, and this was added to 82.3g of H2WO4, which was then dried in a vacuum dryer while stirring. The resulting dried powder was sintered for 1 hour at 550°C in a 5% H2 gas atmosphere with N2 gas as a carrier, and then sintered for 1 hour at 800°C in a N2 gas atmosphere to obtain fine particles a. Chemical analysis of fine particles a showed that the composition was Cs 0.33 WO 2.45 The powder X-ray diffraction results show that the hexagonal Cs 0.3 It was WO3.
[0076] Next, 15% by weight of the fine particles a, 6% by weight of an acrylic dispersant having an acidic functional group as a functional group, and 79% by weight of toluene were weighed out, and the mixture was ground and dispersed for 6 hours using a paint shaker containing 0.3 mmφ ZrO2 beads to prepare a composite tungsten oxide fine particle dispersion (liquid A). The crystallite diameter of the composite tungsten oxide fine particles in liquid A was measured and found to be 31.8 nm. After that, the toluene was removed from liquid A using a large vacuum crusher, and a composite tungsten oxide fine particle dispersion powder (dispersion powder A) was obtained.
[0077] The obtained dispersion powder A was added to a polycarbonate resin powder, which is a thermoplastic resin, so that the composite tungsten oxide microparticle concentration was 0.08% by weight, and after uniformly mixing in a blender, it was melt-kneaded in a twin-screw extruder and extrusion molded to a thickness of 1 mm using a T-die. Then, it was heated and pressed to obtain a heat ray shielding resin molded body with a thickness of 0.8 mm in which the composite tungsten oxide microparticles were uniformly dispersed throughout the resin.
[0078] This heat-shielding resin molding was subjected to a xenon weather meter condition (temperature 60°C, relative humidity 50% RH, irradiance 150 W / m 2 An exposure test was carried out under the conditions of 200 hours exposure and 200 hours exposure. After the test, the optical properties were measured, and as shown in Table 1, when the visible light transmittance was 78.8%, the transmittance at a wavelength of 820 nm was 2.6%, the transmittance at a wavelength of 1000 nm was 1.5%, and the transmittance at a wavelength of 1500 nm was 1.3%.
[0079] Example 2 A composite tungsten oxide microparticle dispersion powder (dispersion powder B) according to Example 2 was obtained in the same manner as in Example 1, except that the amount of the acrylic dispersant having an acidic functional group as the functional group was 7.5% by weight and the amount of toluene was 77.5% by weight. A heat ray shielding molded resin product according to Example 2 was prepared in the same manner as in Example 1, except that Dispersion Powder B was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 2 was 32.6 nm. The optical properties of the heat ray shielding resin molding of Example 2 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 78.1%, the transmittance at a wavelength of 820 nm was 2.5%, the transmittance at a wavelength of 1000 nm was 1.6%, and the transmittance at a wavelength of 1500 nm was 1.3%.
[0080] Example 3 A composite tungsten oxide microparticle dispersion powder (dispersion powder C) according to Example 3 was obtained in the same manner as in Example 1, except that the amount of the acrylic dispersant having an acidic functional group as the functional group was 9.0 wt % and the amount of toluene was 76.0 wt %. A heat ray shielding molded resin product according to Example 3 was prepared in the same manner as in Example 1, except that the dispersed powder C was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 3 was 32.3 nm. The optical properties of the heat ray shielding resin molding of Example 3 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 78.7%, the 820 nm Δ transmittance was 2.6%, the 1000 nm Δ transmittance was 1.6%, and the 1500 nm Δ transmittance was 1.3%.
[0081] Example 4 A composite tungsten oxide microparticle dispersion powder (dispersion powder D) according to Example 4 was obtained in the same manner as in Example 1, except that the amount of the acrylic dispersant having an acidic functional group as the functional group was 12.0 wt % and the amount of toluene was 73.0 wt %. A heat ray shielding molded resin product according to Example 4 was prepared in the same manner as in Example 1, except that Dispersion Powder D was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 4 was 32.7 nm. The optical properties of the heat ray shielding resin molding of Example 4 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 78.9%, the 820 nm Δ transmittance was 2.8%, the 1000 nm Δ transmittance was 1.7%, and the 1500 nm Δ transmittance was 1.5%.
[0082] Example 5 38.8g of Cs2CO was dissolved in 16.5g of water, and this was added to 450g of H2WO, which was then dried in a vacuum dryer while stirring. The resulting dried powder was sintered for 1 hour at 570°C in a 5% H2 gas atmosphere with N2 gas as a carrier, then sintered for 1 hour at 800°C in a 1% air atmosphere with N2 gas as a carrier, and then sintered for 0.5 hours at 820°C in a N2 gas atmosphere to obtain microparticles b. Chemical analysis of microparticles b showed that the composition was Cs 0.27 WO 2.86 The powder X-ray diffraction results show that the hexagonal Cs 0.3 It was WO3.
[0083] A composite tungsten oxide microparticle dispersion powder (dispersion powder E) of Example 5 was obtained in the same manner as in Example 1, except that microparticles b were used. Further, a heat ray shielding resin molding of Example 5 was prepared, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 5 was 31.5 nm. The optical properties of the heat ray shielding resin molding of Example 5 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 80.0%, the 820 nm Δ transmittance was 2.9%, the 1000 nm Δ transmittance was 1.8%, and the 1500 nm Δ transmittance was 1.8%.
[0084] Example 6 17.7 g of Cs2CO3 was dissolved in 39.9 g of water, and this was added to 82.3 g of H2WO4 and dried in a vacuum dryer with stirring to obtain dry powder a. A hybrid plasma reactor in which DC plasma and high-frequency plasma were superimposed was used, and the reaction system was evacuated to about 0.1 Pa (about 0.001 torr) using a vacuum exhaust device, and then completely replaced with argon gas to create a flow system at 1 atmosphere. Then, argon gas was flowed at 8 L / min from the plasma generation gas supply port to generate DC plasma. The DC power input was 6 kW. Furthermore, argon gas was flowed in a spiral shape at 40 L / min and hydrogen gas at 3 L / min from the sheath gas supply port along the inner wall of the water-cooled quartz tube as gas for high-frequency plasma generation and for protecting the quartz tube, and high-frequency plasma was generated. The high-frequency power input was 45 kW. After the hybrid plasma was generated in this way, the obtained dry powder a was fed into the plasma at a rate of 2 g / min from the raw material powder feeder using a mixed gas of 3 L / min argon gas and 0.15 L / min oxygen gas as a carrier gas. As a result, the raw material evaporated instantly, condensed in the plasma tail flame, and pulverized to obtain fine particles c. Chemical analysis of the particle c shows that its composition is Cs 0.31 WO 3.21 The powder X-ray diffraction results are , hexagonal Cs 0.3 It was WO3.
[0085] A composite tungsten oxide microparticle dispersion powder (dispersion powder F) of Example 6 was obtained in the same manner as in Example 1, except that microparticles c were used. Further, a heat ray shielding resin molding of Example 6 was prepared, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 6 was 24.6 nm. The optical properties of the heat ray shielding resin molding of Example 6 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 79.2%, the 820 nm Δ transmittance was 3.4%, the 1000 nm Δ transmittance was 2.0%, and the 1500 nm Δ transmittance was 1.9%.
[0086] [Example 7] Composite tungsten oxide particles d according to Example 7 were obtained in the same manner as in Example 1, except that the molar ratio of K2CO3 and H2WO4 was set to 0.33 when preparing the raw materials. 0.33 WO 2.45 The powder X-ray diffraction results showed that the hexagonal K 0.3 It was WO3. A composite tungsten oxide fine particle dispersion powder (dispersion powder G) according to Example 7 was obtained in the same manner as in Example 1, except that fine particles d were used. A heat ray shielding molded resin product according to Example 7 was prepared in the same manner as in Example 1, except that Dispersion Powder G was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 7 was 31.6 nm. The optical properties of the heat ray shielding resin molding of Example 7 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 78.0%, the transmittance at a wavelength of 820 nm was 3.4%, the transmittance at a wavelength of 1000 nm was 2.2%, and the transmittance at a wavelength of 1500 nm was 2.0%.
[0087] [Example 8] Composite tungsten oxide fine particles e according to Example 8 were obtained in the same manner as in Example 1, except that the molar ratio of Rb2CO3 and H2WO4 was set to Rb / W = 0.33 when preparing the raw materials. 0.33 WO 2.45 The powder X-ray diffraction results showed that hexagonal Rb 0.33 It was WO3. A composite tungsten oxide fine particle dispersion powder (dispersion powder H) according to Example 8 was obtained in the same manner as in Example 1, except that fine particles e were used. A heat ray shielding molded resin product according to Example 8 was prepared in the same manner as in Example 1, except that the dispersion powder H was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 8 was 32.2 nm. The optical properties of the heat ray shielding resin molding of Example 8 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 79.9%, the 820 nm Δ transmittance was 2.9%, the 1000 nm Δ transmittance was 2.1%, and the 1500 nm Δ transmittance was 2.0%.
[0088] [Example 9] Composite tungsten oxide microparticles g according to Example 9 were obtained in the same manner as in Example 1, except that Tl(NO3)33H2O and H2WO4 were mixed in a Tl / W molar ratio of 0.33 when preparing the raw materials. 0.33 WO 2.45 The powder X-ray diffraction results showed that the hexagonal Tl 0.3 It was WO3. A composite tungsten oxide fine particle dispersion powder (dispersion powder I) according to Example 9 was obtained in the same manner as in Example 1, except that fine particles g were used. A heat ray shielding molded resin product according to Example 9 was prepared in the same manner as in Example 1 except that Dispersion Powder I was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 9 was 32.6 nm. The optical properties of the heat ray shielding resin molding of Example 9 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 79.4%, the 820 nm Δ transmittance was 3.0%, the 1000 nm Δ transmittance was 2.2%, and the 1500 nm Δ transmittance was 2.0%.
[0089] Example 10 Composite tungsten oxide microparticles h according to Example 10 were obtained in the same manner as in Example 1, except that BaCO3 and H2WO4 were used in a Ba / W molar ratio of 0.33 when preparing the raw materials. 0.33 WO 2.45 The powder X-ray diffraction results showed that the hexagonal Ba 0.3 It was WO3. A composite tungsten oxide fine particle dispersion powder (dispersion powder J) according to Example 10 was obtained in the same manner as in Example 1, except that fine particles h were used. A heat ray shielding molded resin product according to Example 10 was prepared in the same manner as in Example 1 except that the dispersion powder J was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 10 was 32.5 nm. The optical properties of the heat ray shielding resin molding of Example 10 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 78.0%, the 820 nm Δ transmittance was 3.7%, the 1000 nm Δ transmittance was 2.6%, and the 1500 nm Δ transmittance was 2.0%.
[0090] Example 11 Except for using an acrylic resin as the thermoplastic resin, a heat ray shielding molded resin according to Example 11 was obtained in the same manner as in Example 1. Thereafter, exposure was performed under the same conditions as in Example 1 to evaluate the optical properties. As shown in Table 1, when the visible light transmittance was 80.8%, the Δ transmittance at a wavelength of 820 nm was 3.4%, the Δ transmittance at a wavelength of 1000 nm was 2.5%, and the Δ transmittance at a wavelength of 1500 nm was 2.0%.
[0091] [Example 12] A composite tungsten oxide microparticle dispersion powder (dispersion powder K) according to Example 12 was obtained in the same manner as in Example 1, except that the acrylic dispersant having an acidic functional group as the functional group was 15.0 wt % and the toluene was 70.0 wt %. A heat ray shielding molded resin product according to Example 12 was prepared in the same manner as in Example 1 except that the dispersion powder K was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 12 was 32.2 nm. The optical properties of the heat ray shielding resin molding of Example 12 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 79.1%, the 820 nm Δ transmittance was 3.7%, the 1000 nm Δ transmittance was 2.2%, and the 1500 nm Δ transmittance was 1.9%.
[0092] [Example 13] A composite tungsten oxide microparticle dispersion powder (dispersion powder L) according to Example 13 was obtained in the same manner as in Example 1, except that the acrylic dispersant having an acidic functional group as the functional group was 4.5% by weight and the toluene was 80.5% by weight. A heat ray shielding molded resin product according to Example 13 was prepared in the same manner as in Example 1 except that the dispersion powder L was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 13 was 32.2 nm. The optical properties of the heat ray shielding resin molding of Example 13 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 78.0%, the 820 nm Δ transmittance was 2.3%, the 1000 nm Δ transmittance was 1.4%, and the 1500 nm Δ transmittance was 1.3%.
[0093] [Example 14] A heat ray shielding resin molded body according to Example 14 was obtained in the same manner as in Example 1, except that the fine particles a were pulverized and dispersed for 20 hours using a paint shaker. Thereafter, an exposure test was carried out under the same conditions as in Example 1, and the optical properties were evaluated. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 14 was 15.0 nm. The optical properties of the heat ray shielding resin molding of Example 14 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 80.3%, the 820 nm Δ transmittance was 3.8%, the 1000 nm Δ transmittance was 2.7%, and the 1500 nm Δ transmittance was 2.1%.
[0094] [Example 15] A heat ray shielding resin molded body according to Example 15 was obtained in the same manner as in Example 1, except that the fine particles a were pulverized and dispersed for 1 hour using a paint shaker. Thereafter, an exposure test was carried out under the same conditions as in Example 1, and the optical properties were evaluated. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Example 15 was 80 nm. The optical properties of the heat ray shielding resin molding of Example 15 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 79.8%, the 820 nm Δ transmittance was 2.0%, the 1000 nm Δ transmittance was 1.0%, and the 1500 nm Δ transmittance was 1.0%.
[0095] [Comparative Example 1] A composite tungsten oxide microparticle dispersion powder (dispersion powder M) according to Comparative Example 1 was obtained in the same manner as in Example 1, except that the acrylic dispersant having an acidic functional group as the functional group was 45.0 wt % and the toluene was 35.0 wt %. A heat ray shielding molded resin body according to Comparative Example 1 was prepared in the same manner as in Example 1, except that Dispersion Powder M was used, and an exposure test was carried out under the same conditions as in Example 1 to evaluate the optical properties. The crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Comparative Example 1 was 32.9 nm. The optical properties of the heat ray shielding resin molding of Comparative Example 1 after the exposure test were measured. As shown in Table 1, when the visible light transmittance was 79.2%, the 820 nm Δ transmittance was 5.6%, the 1000 nm Δ transmittance was 3.1%, and the 1500 nm Δ transmittance was 2.6%.
[0096] [Comparative Example 2] A composite tungsten oxide microparticle dispersion according to Comparative Example 1 was prepared in the same manner as in Example 1, except that the acrylic dispersant having an acidic functional group as a functional group was 3.0% by weight, and the toluene was 82.0% by weight. However, the crystallite diameter of the composite tungsten oxide microparticles in the composite tungsten oxide microparticle dispersion liquid according to Comparative Example 2 was 96.3 nm, and since pulverization did not progress to the desired particle size at the stage of preparing the dispersion liquid, the test was terminated.
[0097] [Comparative Example 3] An attempt was made to produce a heat-shielding resin molded body of Example 15 in the same manner as in Example 1, except that the fine particles a were pulverized and dispersed for 25 hours using a paint shaker. However, since the dispersion liquid gelled, the test was terminated without proceeding to the production of a heat-shielding resin molded body and the evaluation of its optical properties.
[0098] 〔evaluation〕 According to the results shown in Table 1, it was confirmed that the heat ray shielding resin moldings of Examples 1 to 15 after the weather resistance test had a visible light transmittance of 78.0% or more, a Δ transmittance at a wavelength of 820 nm of 3.8% or less, a Δ transmittance at a wavelength of 1000 nm of 2.7% or less, and a Δ transmittance at a wavelength of 1500 nm of 2.1% or less. On the other hand, the heat ray shielding resin molding of Comparative Example 1 has a visible light transmittance of 78.0% or more, but the Δ transmittance at wavelength 820 nm exceeds 3.8%, the Δ transmittance at wavelength 1000 nm exceeds 2.7%, and the Δ transmittance at wavelength 1500 nm exceeds 2.1%, and it was confirmed that the Δ transmittance in the near infrared region is high. Furthermore, in Comparative Example 2, the grinding did not progress to the desired particle size at the dispersion liquid preparation stage. Furthermore, in Comparative Example 3, gelation occurred at the dispersion liquid preparation stage, and the heat ray shielding resin molding was not prepared and the optical properties were not evaluated.
[0099] [Table 1]
Claims
1. The present invention relates to a tungsten oxide nanoparticle having a hexagonal crystal structure, a crystallite size of 15 nm or more and 80 nm or less, and a surface-modified acrylic dispersant, the nanoparticle being represented by a general formula MxWOy (wherein M element is one or more elements selected from the group 1, group 2 and group 13 elements in the periodic table, and 0.1≦x≦1.0, 2.0≦y<4.0), and the like; A dispersion powder characterized in that a weight ratio of the dispersant to the composite tungsten oxide fine particles is in the range of 0.3≦(weight of dispersant / weight of composite tungsten oxide fine particles)<3.
0.
2. 2. The dispersion powder according to claim 1, wherein the acrylic dispersant has an acidic functional group as a functional group.
3. 3. The dispersion powder according to claim 1, wherein the M element contained in the composite tungsten oxide fine particles is at least one element selected from the group consisting of Cs, Rb, K, Tl, and Ba.
4. a composite tungsten oxide microparticle having a hexagonal crystal structure represented by the general formula MxWOy (wherein M element is one or more elements selected from the elements of Groups 1, 2, and 13 in the periodic table, 0.1≦x≦1.0, 2.0≦y<4.0) and an acrylic dispersant are added to an organic solvent, and then a pulverization and dispersion process is performed to produce a dispersion in which the composite tungsten oxide microparticles have a crystallite diameter of 15 nm or more and 80 nm or less; The method for producing a dispersed powder, comprising removing the organic solvent from the dispersion liquid to produce a dispersed powder in which the weight ratio of the dispersant to the composite tungsten oxide microparticles is in the range of 0.3≦(weight of dispersant / weight of composite tungsten oxide microparticles)<3.
0.
5. 3. A heat ray shielding resin molded article, which is obtained by diluting and kneading the dispersed powder according to claim 1 or 2 with a thermoplastic resin molding material, and molding the mixture into a predetermined shape.
6. 6. The heat ray shielding resin molding according to claim 5, wherein the thermoplastic resin molding material is a polycarbonate resin or an acrylic resin.
7. A heat ray shielding laminate, comprising the heat ray shielding molded resin product according to claim 5 laminated with another molded product.
Citation Information
Patent Citations
Highly heat-resistant masterbatch, heat ray-shielding transparent resin molding, and heat ray-shielding transparent laminate
JP2008024902A
Fine particle dispersing liquid excellent in high temperature stability and fine particle dispersion
JP2020172407A
Haet ray-shielding resin sheet material
JP2022100880A
Absorber microparticle dispersion with excellent long-term stability, object containing dispersed absorber microparticles, and production methods therefor
WO2019093525A1
Heat-ray reflecting resin glass
JP1986277437A
Cited By
Heat-ray-blocking composition, heat-ray-blocking resin molded body, heat-ray-blocking resin laminate, and method for producing dispersion powder
WO2026134277A1