Ceramic molding powder, manufacturing method of ceramic molded object, ceramic molded object, and instrument

A ceramic powder containing Zr, Y, and Si, with specific mass ratios, enhances the strength of additive-manufactured ceramic articles through laser irradiation and heating, enabling self-repair and high mechanical strength for various components.

JP2024159508APending Publication Date: 2024-11-08CANON KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024035293
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-03-07
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing ceramic powder for additive manufacturing using zirconium oxide lacks sufficient strength in manufactured objects, necessitating a powder and method that can produce high-strength ceramic shaped articles.

Method used

A ceramic modeling powder composed of oxide particles containing Zr, Y, Si, and optionally Al, with specific mass percentages of ZrO2, Y2O3, SiO2, and Al2O3, is used in an additive manufacturing process involving laser irradiation, followed by a heating step to enhance strength through self-repairing capabilities and improved mechanical properties.

Benefits of technology

The process results in ceramic articles with enhanced mechanical strength, capable of self-repairing cracks and achieving three-point bending strengths of up to 200 MPa or more, suitable for diverse applications including electrical, optical, and mechanical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159508000001_ABST
    Figure 2024159508000001_ABST
Patent Text Reader

Abstract

To provide a technique advantageous for manufacturing a ceramic molded object higher in material strength.SOLUTION: Provided is ceramic molding powder in which oxide particles contain plural elements including at least Zr, Y, Si and, optionally, Al and contain at least particles of silicon monoxide, and α, β, γ satisfy the following: 77.64≤α≤93.06, 4.42≤β≤6.49, and 0.72≤γ≤17.29, when a mass of ZrO2 is represented by the α (mass%), a mass of Y2O3 is represented by the β (mass%), and a mass of SiO2 is represented by the γ (mass%), with respect to the total amount of the mass of the ZrO2, the mass of the SiO2, and a mass of Al2O3, when a content of the Zr is converted to the mass of the ZrO2, a content of the Y is converted to the mass of the Y2O3, a content of the Si is converted to the mass of the SiO2, and a content of the Al is converted to the mass of the Al2O3.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a ceramic shaping powder used when manufacturing a ceramic shaped object by additive manufacturing technology using a laser, a method for manufacturing a ceramic shaped object, a ceramic shaped object, and an apparatus. [Background technology]

[0002] With the development of additive manufacturing technology, there is a demand for the realization of a wide variety of dense ceramic objects using additive manufacturing technology with resin powder or metal powder as raw materials. In recent years, there has been a demand for raw material powders for manufacturing ceramic objects with excellent thermal properties, such as thermal shock resistance and low thermal expansion coefficient. Patent Document 1 proposes the use of zirconium oxide. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-19051 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the powder for additive manufacturing (additive manufacturing) using zirconium oxide disclosed in Patent Document 1 still had room for improvement in terms of the strength of objects that could be manufactured using the powder. There was a demand for a powder for additive manufacturing that could manufacture high-strength objects, and a manufacturing method thereof.

[0005] Therefore, an object of the present disclosure is to provide a technique that is advantageous for producing a ceramic shaped article having higher strength. [Means for solving the problem]

[0006] In order to solve the above problem, the first aspect is: A ceramic modeling powder composed of oxide particles for use in an additive modeling method in which modeling is performed by irradiating a laser beam, the oxide particles include a plurality of elements including at least Zr, Y, Si, and optionally Al, and include at least particles of silicon monoxide; When the Zr content is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 relative to the total mass of ZrO2, Y2O3, SiO2, and Al2O3 is defined as α (mass%), the mass of Y2O3 is β (mass%), and the mass of SiO2 is γ (mass%), the powder for ceramic molding satisfies the following: 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29 The second viewpoint is, a step of disposing oxide particles on a base; an irradiation step of irradiating a part or all of the oxide particles with laser light to melt and solidify the oxide particles at the places irradiated with the laser light, thereby obtaining an intermediate object; a heating step of heat-treating the intermediate object; A method for producing a ceramic shaped object, comprising: The oxide particles contain a plurality of elements including at least Zr, Y, Si, and optionally Al, and contain at least silicon monoxide particles, and when the Zr content is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, when the mass of ZrO2 is defined as α (mass%), the mass of Y2O3 is defined as β (mass%), and the mass of SiO2 is defined as γ (mass%) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3, α, β, and γ satisfy the following: 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29 The third viewpoint is, A ceramic shaped object containing multiple elements including Zr and Si, A region mainly containing Zr and a region mainly containing Si, In an SEM image of a cross section near the center of the ceramic shaped article, at least the region mainly containing Si has a first region and a second region, The first regions have a length to average width ratio of less than 10 and are each 78.5 μm 2 A planar portion having an area of ​​at least The second region is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more, and is a ceramic shaped article in contact with the first region. Also, as a modified example, A ceramic shaped object containing a plurality of elements including Zr, Si, and Al, A region mainly containing Zr, a region mainly containing Si, and a region mainly containing Al, the average value of the Zr SEM-EDS output signal is larger in the region mainly containing Zr than in the region mainly containing Si; An example of a ceramic object is one in which the average value of the SEM-EDS output signal of Si, the average value of the SEM-EDS output signal of Y, and the average value of the SEM-EDS output signal of Al are each larger in the region mainly containing Si than in the region mainly containing Zr. Further, examples of applications include devices including the above-mentioned ceramic shaped object and at least one of an electric part, an optical part, a metal part, and a resin part. Effect of the Invention

[0007] According to this embodiment, it is possible to provide a technique that is advantageous for manufacturing a ceramic object having high strength using additive manufacturing technology. [Brief description of the drawings]

[0008] [Figure 1]1(a) to 1(h) are schematic diagrams showing an example of the method for producing a ceramic shaped article according to this embodiment. [Diagram 2] Fig. 2(a) is a cross-sectional SEM image showing an example of the structural characteristics of the ceramic shaped product of this embodiment. Fig. 2(b) is an elemental mapping image of Zr in the same field of view as the SEM image of Fig. 2(a). Fig. 2(c) is an elemental mapping image of Si in the same field of view as the SEM image of Fig. 2(a). [Diagram 3] Fig. 3(a) is an image showing an example of a cross section of a ceramic shaped object obtained according to the present embodiment, and Fig. 3(b) is an image showing another example of a cross section of a ceramic shaped object obtained according to the present embodiment. [Figure 4] Figure 4(a) is a schematic diagram of Figure 3(a). Figure 4(b) is a schematic diagram showing when a crack occurs due to the application of external stress. Figure 4(c) is a schematic diagram showing when the cracked area has self-repaired by heat treatment. [Diagram 5] 5(a) to 5(h) are element mapping images of Zr, Si, Y, and Al by SEM-EDS evaluation for a number of examples of the ceramic shaped article of this embodiment. [Figure 6] FIG. 6 is a schematic diagram showing another example of the method for producing a ceramic object according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] An embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described with reference to the drawings, but the present embodiment is not limited to the specific example below. <First embodiment> The first embodiment is directed to powder for ceramic shaping. The ceramic molding powder of this embodiment is A ceramic modeling powder composed of oxide particles for use in an additive modeling method in which modeling is performed by irradiating a laser beam, the oxide particles include a plurality of elements including at least Zr, Y, Si, and optionally Al, and include at least particles of silicon monoxide; When the Zr content is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 is defined as α (mass%), the mass of Y2O3 is β (mass%), and the mass of SiO2 is γ (mass%), α, β, and γ satisfy the following: 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29

[0010] The powder for ceramic molding according to this embodiment (hereinafter also referred to as "material powder", "raw powder" or simply "powder") is composed of a plurality of particles independent of each other, and is composed of oxide particles used in additive molding, which performs molding by irradiating laser light. It is preferable that the powder contains zirconium oxide (ZrO2) particles, silicon dioxide (SiO2) particles, silicon monoxide (SiO) particles, and other powder particles. By using the material powder according to this embodiment, it is possible to manufacture articles with excellent mechanical strength. For example, it is suitable for manufacturing ceramic parts that require mechanical strength, such as machine parts, plastic molds, dental parts such as denture materials, and aerospace parts such as turbine materials.

[0011] In the ceramic shaping powder according to the present embodiment, the oxide particles contain at least Zr, Y, Si, and possibly Al. Y (yttrium) is preferably contained as an oxide. In particular, ZrO2 preferably contains Y as Y2O3 (yttrium oxide, yttria) stabilized ZrO2. The content of Y2O3 contained in ZrO2 is preferably 1.5 mol% or more and 10.5 mol% or less. More preferably, it is 2.0 mol% or more and 4.5 mol% or less. In addition, it may exist as an oxide consisting of Si and Y. In this way, the intermediate shaped object made of the ceramic shaping powder can self-repair cracks by heating. ZrO2 containing Y2O3 is also called YSZ (Yttria Stabilized Zirconia, yttria stabilized zirconia, or yttrium stabilized zirconia). In this embodiment, when the concentration of Y2O3 added to ZrO2 is 3 mol%, it is also called 3YSZ, and when it is 4 mol%, it is also called 4YSZ. In the present disclosure, since Si is a metalloid element, it is treated as a type of metallic element.

[0012] Furthermore, in the ceramic shaping powder according to this embodiment, when the Zr content is converted to the mass of ZrO2, the Y content is converted to the mass of Y2O3, the Si content is converted to the mass of SiO2, and the Al content is converted to the mass of Al2O3, the mass of ZrO2 is α (mass%), the mass of Y2O3 is β (mass%), and the mass of SiO2 is γ (mass%) relative to the total mass of ZrO2, Y2O3, SiO2, and Al2O3, the following values ​​are satisfied: 77.64≦α≦93.06, 4.42≦β≦6.49, and 0.72≦γ≦17.29. Regarding the composition range γ in terms of SiO2, the lower limit is a value advantageous for maintaining the self-repairing property of cracks possessed by the ceramic shaped object (oxide structure) obtained by this embodiment, and further, when contained as SiO, the value is a value that can fully obtain the function as a laser absorber. The upper limit value is advantageous as one condition for satisfying mechanical strength, particularly a three-point bending strength value of 50 MPa or more. The three-point bending strength value is more preferably 100 MPa or more, and even more preferably 150 MPa or more. The three-point bending strength value can also be 200 MPa or more. The three-point bending strength value may be 1000 MPa or less, 500 MPa or less, or 400 MPa or less.

[0013] Furthermore, the ceramic shaping powder according to the present embodiment preferably contains Al as oxide particles. More preferably, in the composition of the ceramic shaping powder, when the mass of Al2O3 relative to the total mass of ZrO2, Y2O3, SiO2, and Al2O3 is δ (mass%), it is preferable that 0.21≦δ≦9.17. The oxide particles may contain alumina particles, or may contain yttria-stabilized zirconia particles with added alumina. Hereinafter, YSZ containing Al is also referred to as 3YSZ(Al) when the concentration of Y2O3 added is 3 mol% relative to ZrO2.

[0014] ZrO2, SiO2, SiO, Y2O 3、The notation of a compound such as Al2O3 does not limit the composition to the stoichiometric ratio shown, and an error in the composition ratio of the constituent elements within ±30% from the stoichiometric ratio normalized by the metal element is allowed. For example, a compound with a composition ratio of Si:O=1:1.30 is also included in the notation of SiO. In other words, SiO is SiO m (0.7≦m≦1.3).

[0015] The ceramic forming powder of this embodiment contains at least silicon monoxide (SiO) particles. SiO is brown or black, and has a relatively higher light absorption ability for the light (laser light) of the wavelength irradiated during forming than YSZ and SiO2 contained in the ceramic forming powder. When SiO absorbs laser light, Si changes from divalent to tetravalent, and SiO in a metastable state changes to SiO2 in a more stable state, decreasing the light absorption ability for the laser light. By forming a powder in which SiO having such characteristics is added as an absorber to YSZ and silicon dioxide (SiO2), the following effects can be obtained.

[0016] The first effect is that the SiO, which is an absorber, efficiently absorbs the laser light used during manufacturing and becomes hot, which transfers the heat to other compounds present in the area equivalent to the focal size of the laser light, causing a rise in temperature. As a result, the area equivalent to the focal size of the laser light can be effectively heated locally, and the interface between the area where the powder is to be solidified (the area irradiated with the laser light) and the area where it is not to be solidified (the area not irradiated with the laser light) can be made clear, thereby improving the modeling accuracy.

[0017] The second effect is that SiO changes to SiO2, which has low light absorption ability, by irradiation with laser light, and light absorption is suppressed in the part (solidified part) where the powder is solidified by being irradiated with laser light. SiO xIf the light absorption capacity of SiO before the laser irradiation is reduced to 5 / 6 times or less of that of SiO before the laser irradiation, even if the solidified part is irradiated with laser light under the same conditions as during solidification, the solidified part will not be affected to such an extent that the modeling accuracy is deteriorated. That is, since there is almost no absorber in the solidified part, the temperature rise before the laser irradiation does not occur, and even if the powder adjacent to the solidified part is irradiated with laser light, deformation and deterioration of the solidified part are suppressed. As a result, the process margin of the laser irradiation conditions and the like is expanded, and the influence on the modeling accuracy due to the fluctuation of the irradiation conditions can be reduced. In order to obtain sufficient modeling accuracy, it is preferable that the light absorption capacity of SiO alone before the laser irradiation is 1.2 times or more different from the light absorption capacity of the absorber whose composition has changed after the laser irradiation, and it is preferable that the difference is 2 times or more. In this way, if the powder according to this embodiment is selectively irradiated with laser light to perform modeling, the first and second action effects described above can be obtained, and high-precision modeling can be realized. In addition, since SiO is distributed on the market as a negative electrode for lithium-ion secondary batteries, it is also possible to procure it at a lower price than other compounds that can be used as an absorber.

[0018] In the ceramic forming powder of this embodiment, the SiO functioning as an infrared absorbing material has a silicon monoxide particle content of 0.5 volume % or more and 53 volume % or less in oxide particles. More preferably, it is 0.5 volume % or more and 10 volume % or less. The volume composition was calculated by converting from mass and the like using true density. The true density was ZrO2: 5.68 [g / cm 3 ], Y2O3: 5.01 [g / cm 3 ], SiO2: 2.30 [g / cm 3 ], Al2O3: 3.96 [g / cm 3 ], SiO: 2.13 [g / cm 3 Even if this true density is a slightly different value, it does not affect the essence of this embodiment.

[0019] The individual particles contained in the powder for ceramics forming, which are independent from each other, may be a sintered body (sintered particles) of multiple particles, and may be amorphous or crystalline. In this embodiment, the powder being made of multiple compounds includes a case where multiple types of particles made of one type of compound are mixed, and a case where one type or multiple types of particles made of multiple types of compounds are mixed. In the following, to avoid confusion, the particles that are independent from each other contained in the powder are simply called particles, and the particles that make up each particle are called constituent particles. For example, when the powder is made up of sintered particles obtained by sintering ZrO2 particles and Y2O3 particles, the sintered particles are called particles, and the ZrO2 particles and Y2O3 particles that make up the sintered particles are called constituent particles.

[0020] As an example of a powder for ceramic shaping in which each particle contains one type of compound, a powder for ceramic shaping containing the elements Zr, Y, and Si may be a mixture of three types of particles, namely ZrO2 particles, Y2O3 particles, SiO2 particles, and SiO particles.

[0021] Examples of particles constituting the powder for ceramic molding that contain multiple compounds include a state in which one particle is composed of a ZrO2 region, a Y2O3 region, and a SiO2 region, a state in which one particle contains a particle composed of a ZrO2 region and a Y2O3 region, and a particle composed of SiO2, etc. YSZ can be considered as a single compound because Y2O3 is dissolved in ZrO2, but when Al2O3 is contained therein, it is also written as YSZ(Al) in this embodiment, but in this case, it is an example of containing multiple compounds such as YSZ and Al2O3. Therefore, a preferred example of the powder for ceramic shaping in this embodiment is composed of 3YSZ particles, SiO2 particles, SiO particles, or 3YSZ(Al) particles, SiO2 particles, SiO particles, and Al2O3 particles.

[0022] In the powder bed fusion method, when a powder bed layer is formed using a recoater, or when powder is sprayed from a nozzle in the cladding method, it is important that the ceramic shaping powder has a suitable fluidity for these purposes. Therefore, the ceramic shaping powder according to this embodiment preferably has a fluidity index of 40 [sec / 50g] or less. In order to ensure such fluidity, each particle is preferably spherical, but the shape of the particles is not limited to spherical as long as the above fluidity index is satisfied. The fluidity index can be measured, for example, in accordance with JIS Z2502.

[0023] It is particularly preferable that SiO, which functions as an absorber, is contained as particles (SiO particles) independent of other components, regardless of the state in which other compounds are contained in the powder for ceramics molding. A higher light absorption ability can be achieved than when it is contained in one particle together with other compounds. Furthermore, the laser light can easily reach the absorber, and the light absorption ability of the absorber can be efficiently utilized. In addition, if SiO is a particle independent of other components, the particle size of the SiO particles and the particle size of the other particles can be adjusted separately, making it easier to control the fluidity of the powder and easier to control the amount of absorber present within the spot diameter of the irradiated laser light. This point will be explained in detail later. In order to make particles containing SiO and other compounds function as absorbers, it is preferable that 50% or less by volume of the particles is SiO.

[0024] When silicon monoxide (SiO) particles do not include regions other than silicon monoxide, the average particle size of the oxide particles other than SiO particles (hereinafter also referred to as base material particles) is preferably 5 μm or more and larger than the average particle size of the SiO particles from the viewpoint of realizing favorable fluidity. More preferably, it is 5 μm or more and 5 times larger than the average particle size of the SiO particles. Also, it is more preferably 10 μm to 200 μm and larger than the average particle size of the SiO particles. Even more preferably, it is 10 μm to 200 μm and 5 times larger than the average particle size of the SiO particles. Also, from the viewpoint of realizing high molding accuracy and from the viewpoint of easy sintering or melting of the powder, the average particle size of the base material particles is preferably 200 μm or less, and more preferably 150 μm or less.

[0025] When the silicon monoxide (SiO) particles do not include regions other than silicon monoxide, the average particle size of the SiO particles is preferably 10 μm or less and 1 / 5 or less of the average particle size of the base material particles. When the SiO particles satisfy this condition, the probability that a plurality of SiO particles are dispersed in the vicinity of the base material particles increases, so that the heat generated by SiO absorbing the laser light is efficiently transferred to the base material particles, and the powder in the laser light irradiated portion is easily melted. Considering the dispersibility of SiO in the powder for ceramic molding and the realization of high packing density, it is preferable that the average particle size of the SiO particles is as small as possible. On the other hand, when the average particle size of the SiO particles is 1 μm or more, scattering into the atmosphere due to irradiation with the laser light is suppressed, and an appropriate amount as an absorber can be maintained in the powder for ceramic molding. Therefore, the average particle size of the SiO particles is preferably 1 μm or more and 10 μm or less and 1 / 5 or less of the average particle size of the base material particles, and more preferably 1 μm or more and less than 5 μm and 1 / 5 or less of the average particle size of the base material particles.

[0026] When silicon monoxide (SiO) particles contain regions other than silicon monoxide, the average particle size is preferably 5 μm or more and 200 μm or less from the viewpoint of realizing fluidity suitable for additive manufacturing. A more preferable average particle size is 5 μm or more and 5 times or more the average diameter of the regions made of SiO contained in the particles. An even more preferable average particle size is 10 μm or more and 5 times or more the average diameter of the regions made of SiO. When silicon monoxide (SiO) particles contain regions other than silicon monoxide, the average particle size of the silicon monoxide particles is preferably 200 μm or less, more preferably 150 μm or less, from the viewpoint of realizing high modeling accuracy and ease of sintering or melting the powder.

[0027] The average particle size of the constituent particles made of SiO in a particle containing SiO and a compound other than SiO is determined by observing the powder with a scanning electron microscope (SEM) or the like, measuring the area of ​​the region made of SiO, and calculating the circle-equivalent diameter of that area. Measurements are taken for multiple (100 or more) regions made of SiO, and the median value is taken as the average particle size of the constituent particles made of SiO.

[0028] In this embodiment, the particle size refers to the circle equivalent diameter (Heywood diameter) of each particle. The average particle size of particles having a specific composition contained in the powder for ceramic molding does not refer to the particle size of each particle, but is the median value of a particle group having the same composition, and does not mean that particles other than the size indicated as the average particle size are not contained in the powder.

[0029] The average particle size of the particles can be calculated in the same way as the average particle size of the constituent particles, by the following method: Observe the powder with a scanning electron microscope (SEM) or the like, measure the area of ​​the particles containing the specific composition for which the average particle size is to be calculated, and calculate the circle-equivalent diameter of that area. This method of calculating the average particle size can be applied regardless of the state of the particles.

[0030] From the viewpoint of realizing a preferable fluidity, the average particle size of the SiO2 particles contained in the SiO2 powder is preferably 5 μm or more and larger than the SiO particles. More preferably, the particle size is 5 μm or more, or 5 times or more than the average particle size of the SiO particles. Even more preferably, the particle size is 10 μm or more, or 5 times or more than the average particle size of the SiO particles. In addition, from the viewpoint of realizing a high molding accuracy and the viewpoint of the ease of sintering or melting the powder, the average particle size of the base material particles is preferably 200 μm or less, more preferably 150 μm or less. On the other hand, SiO2 has high viscosity when melted. Therefore, if the powder for ceramic molding contains a lot of SiO2 with a large particle size, it becomes spherical in the molten state and tends to solidify as it is, so the molded object formed tends to be porous. In order to mold a dense ceramic molded object, the average particle size is preferably 100 μm or less, more preferably 50 μm or less.

[0031] The ceramic shaping powder of this embodiment preferably does not contain a resin binder. This is because the resin binder has a significantly lower melting point than other compounds contained in the powder, and may be explosively burned away by irradiation with a laser beam, causing voids or defects in the shaping region.

[0032] In addition, if the powder contains a sublimable carbon element, the carbon may combine with oxygen to become gas and escape, and the volume occupied by the carbon element may become a void. Furthermore, the carbon element may sublimate and gasify rapidly when irradiated with laser light, which may adversely affect the modeling. Specifically, the rapid gasification may cause stress to be applied to the molten and solidified parts of the ceramic modeling powder, resulting in a deformed model. Therefore, it is preferable that the powder does not basically contain carbon element. It is preferable that the amount of carbon element contained in the powder is small, even if it is not completely zero, and it is particularly preferable that the molar ratio of the carbon element to the metal elements of the multiple compounds contained in the powder is 1000 ppm or less.

[0033] The powder for ceramic shaping according to the present embodiment may be in a crystalline or amorphous state, or may be a mixture of these, etc. In addition, it is not necessary to completely match the composition between the powder and the shaped ceramic object, and differences in the oxidation state, nitridation state, etc. may be acceptable.

[0034] Second Embodiment The second embodiment relates to a method for producing a ceramic shaped object. The method for producing a ceramic object according to the present embodiment includes the steps of: a step of disposing oxide particles on a base; an irradiation step of irradiating a part or all of the oxide particles with laser light to melt and solidify the oxide particles at the places irradiated with the laser light, thereby obtaining an intermediate object; a heating step of heat-treating the intermediate object; A method for producing a ceramic shaped object, comprising: The oxide particles contain a plurality of elements including at least Zr, Y, Si, and optionally Al, and contain at least silicon monoxide particles, and when the Zr content is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 are expressed as α (mass%), β (mass%), and γ (mass%) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3, α, β, and γ satisfy the following: 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29 Each item will be explained below. Note that since each substance has been described above, the explanation may be omitted.

[0035] (Placement process and irradiation process) The ceramic shaping powder of this embodiment is suitable for additive manufacturing, which irradiates the ceramic shaping powder with laser light in accordance with slice data generated based on three-dimensional data of the ceramic object to be manufactured. Specifically, it is used in manufacturing methods using powder bed fusion and cladding. In this manufacturing process, the ceramic object is manufactured by alternately performing the following arrangement step and irradiation step multiple times. The manufacturing method of the ceramic object of this embodiment includes an arrangement step of arranging oxide particles on a base, and an irradiation step of irradiating some or all of the oxide particles with laser light to melt and solidify the oxide particles at the points irradiated with the laser light, thereby obtaining an intermediate object. In the case of using the powder bed fusion method to model, the disposing step and the irradiating step are performed by spreading the ceramic modeling powder of this embodiment on a substrate to a predetermined thickness and then irradiating the substrate with a laser beam. In the case of using the cladding method to model, the disposing step and the irradiating step are performed by ejecting the ceramic modeling powder of this embodiment on a predetermined location and irradiating the predetermined location with a laser beam.

[0036] In the method for producing a ceramic shaped product according to the present embodiment, the powder for ceramic shaping has the following properties: α (mass%), β (mass%), and γ (mass%) of ZrO2, SiO2, and Al2O3, respectively, when the Zr content is converted to the mass of ZrO2, the Y content is converted to the mass of Y2O3, the Si content is converted to the mass of SiO2, and the Al content is converted to the mass of Al2O3. The lower limit of the composition range γ in terms of SiO2 is advantageous for maintaining the self-repairing property of cracks of the ceramic shaped product (oxide structure) obtained by the present embodiment, and furthermore, when contained as SiO, the value is a value that can fully obtain the function as a laser absorber. The upper limit value is advantageous as one condition for satisfying mechanical strength, particularly a three-point bending strength value of 50 MPa or more. The three-point bending strength value is more preferably 100 MPa or more, and even more preferably 150 MPa or more. The three-point bending strength value can also be 200 MPa or more. The three-point bending strength value may be 1000 MPa or less, 500 MPa or less, or 400 MPa or less.

[0037] In the method for manufacturing a ceramic object according to this embodiment, when the oxide particles contain Al and the mass of Al2O3 relative to the total mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 is δ (mass%), it is preferable that δ satisfies 0.21≦δ≦9.17.

[0038] There is no limitation on the wavelength of the laser light used for modeling, but it is preferable to use a lens or fiber adjusted to a desired focal size, such as a diameter of 10 μm to 2 mm. The focal size is one of the parameters that affect modeling accuracy, and in order to achieve a modeling accuracy of 100 μm (0.1 mm), it is preferable that the line width is approximately the same, and the focal size is preferably 100 μm or less in diameter, although this depends on the situation. The laser light may be irradiated in either a continuous or pulsed form. As the laser light, a laser with a wavelength of approximately 1000 nm, such as an Nd:YAG laser or a Yb fiber laser, can be suitably used. This is because the SiO component exhibits particularly high absorptivity for light with a wavelength of approximately 1 μm.

[0039] 1(a) to 1(h) are conceptual diagrams of a three-dimensional modeling device using a powder bed fusion method (infrared laser melting method). The basic modeling flow of a manufacturing method using an infrared laser melting method that can use the ceramic modeling powder of this embodiment will be described with reference to the schematic diagrams of FIG. 1(a) to FIG. 1(h).

[0040] As shown in FIG. 1(a), first, raw powder 301 is placed on a base 330 installed on a stage 351, and is spread to a predetermined thickness by a roller 352 to form a powder layer 302 as shown in FIG. 1(b). As shown in FIG. 1(c), a laser beam emitted from a laser light source 380 is irradiated onto the powder layer 302 while being scanned by a scanner unit 381 based on slice data generated from shape data of a desired three-dimensional model. In the irradiation range of the laser beam, the raw powder melts and then solidifies, forming a solidified portion 300 corresponding to the slice data for one layer. Next, as shown in FIG. 1(d), the stage 351 is lowered to form a new powder layer 302 on the solidified portion 300, and the laser beam is irradiated based on the slice data as shown in FIG. 1(e). As shown in FIG. 1(f), this series of steps is repeated a number of times according to the slice data to obtain a molded object 310. Finally, as shown in Fig. 1(g), the unsolidified raw material powder 303 is removed, and as shown in Fig. 1(h), if necessary, unnecessary parts of the molded object are removed and the molded object 310 is separated from the base 330. Furthermore, after that, if necessary, a heat treatment may be performed.

[0041] The cladding method will be explained with reference to Fig. 6. The cladding method is a technique in which powder is ejected from multiple powder supply holes 402 in a cladding nozzle 401, and a laser beam 403 is irradiated onto the area where the powder is focused, to successively mold ceramic objects at desired locations. A distinctive feature of the method is that it is possible to mold onto curved surfaces.

[0042] In addition, the atmosphere may be controlled in the manufacturing process. In the manufacturing process, it is preferable to use not only the air atmosphere, but also an inert atmosphere containing nitrogen or other rare gases, an atmosphere containing hydrogen, a reduced pressure atmosphere, or an oxygen atmosphere in which the compounds contained in the powder for ceramic shaping are easily reduced. By controlling the atmosphere in this way, it becomes possible to use a powder containing compounds that are oxidized or reduced from the stoichiometric ratio in the manufacturing of a ceramic shaped product.

[0043] In the manufacturing process of this embodiment as described above, by using the ceramic molding powder of this embodiment, it is possible to obtain a ceramic molded object with stable molding and ensured molding accuracy.

[0044] The ceramic shaped object produced by the ceramic shaping powder according to the present embodiment is not limited to an inorganic material in a crystalline state. As long as the desired physical property values ​​are obtained, a part or a majority of the powder may be in an amorphous state. In addition, the ceramic shaped object may be produced by the above-mentioned production process, including a region close to a metallic state, in which the ceramic shaping powder is reduced.

[0045] (Impregnation process) The method for producing a ceramic object according to this embodiment may include an impregnation step of impregnating the intermediate object with a liquid containing metal components, after the irradiation step and before the heating step. When producing intermediate objects using the infrared laser melting method, the raw material powder is melted by irradiation with an infrared laser and then solidifies. In order to maintain productivity during shape production, it is preferable to increase the laser scanning speed, in which case the part irradiated with the laser is rapidly cooled during solidification. As a result, many fine cracks occur in the intermediate ceramic object due to thermal stress caused by rapid cooling.

[0046] It is possible to complete the production of the ceramic shaped object as it is through a heat treatment process, but it is also preferable to take advantage of the presence of fine cracks and impregnate this part with a modifier for functional modification. For example, it is possible to impregnate Li, Na, K, Mg, Ca, Y, Al, Ti, Zr, Hf, Si, etc. using a metal element-containing liquid and dry or fix it at 600 ° C or less. The metal component-containing liquid preferably contains at least one metal component selected from the group consisting of Li, Na, K, Ca, Y, Al, Zr, and Si, and more preferably contains Al as the metal component. In this way, the three-point bending strength of the ceramic shaped object can be further increased. It is possible to control the amount of fixation to the cracks by the concentration of the metal element-containing liquid and the number of times of impregnation. Therefore, this process allows the modifier to be fixed to the wall surface or between the walls of the cracks.

[0047] In this embodiment, the microcracks in the intermediate object are impregnated with a liquid containing a metal element and then heated to a temperature at which the microcracks can be repaired, thereby modifying the microcracked areas and improving the mechanical strength of the object.

[0048] As an example of the effect of impregnating the intermediate with metal components, the metal element components distributed throughout the intermediate product are diffused over a wide area within the crystals that make up the intermediate product through the microcracks of the intermediate product when heated, and the crystals are recrystallized with a composition that includes the metal element components. This strengthens the bonding force between the crystalline structures of the intermediate product, such as the grain boundaries, and improves the wear resistance of the product. The grain boundaries are the boundaries between crystal grains. Note that crystal grains are sometimes simply referred to as grains.

[0049] As a further example, the intermediate product is composed of a crystalline structure or an amorphous structure formed by irradiation with an energy beam. In the heating step, it is preferable that the metal element component diffuses into the crystalline structure or the amorphous structure and recrystallizes. It is also preferable that the amorphous structure is changed into an amorphous structure having stronger strength. For this reason, the grains constituting the phase originally contained in the intermediate product before heating and the grains constituting the phase containing the metal element component have different grain sizes (e.g., average grain size) after heating. In this way, a phase separation structure is formed consisting of multiple phases whose constituent grains have different average grain sizes, which improves the machinability of the product and enables precise finishing with less chipping.

[0050] Therefore, this embodiment is characterized by modification by introducing metal element components into an intermediate object obtained by melting and solidifying powder with an energy beam, and even if the powder before melting contains metal element components, countless microcracks will be formed in the intermediate object due to thermal stress caused by the temperature difference between melting and solidifying. However, there is no problem if the same metal components are contained in advance as a separate effect. As described above, by carrying out the steps of this embodiment, modification is achieved when microcracks are repaired in the heat treatment step described next, and the mechanical strength of the shaped object can be improved.

[0051] (Heating process) The method for producing a ceramic object according to this embodiment includes a heating step of heat-treating the intermediate object. The powder melted by irradiation with an energy beam such as laser light releases heat to the surroundings, whereby it is cooled and solidified, forming an intermediate object. Ceramics have a smaller thermal diffusivity than metals, so the temperature difference between the melted area and the surrounding area is relatively large. Therefore, when infrared laser melting is used to create a shape without high-temperature residual heat, many microcracks occur in the intermediate object. The microcracks are distributed over the entire intermediate object (surface and interior). When the cross-section of the intermediate object is examined with a scanning electron microscope, most of the microcracks are found to be several nm to several μm wide. The length of the microcracks also varies from several μm to several mm.

[0052] When the intermediate product is subjected to stress, the stress is concentrated in the vicinity of the cracks, and the mechanical strength of the intermediate product is reduced compared to the material in a bulk state. Therefore, it is preferable to repair the microcracks in some way.

[0053] As an example of this embodiment, it was found that by layer-by-layer modeling using a ceramic modeling powder consisting of YSZ particles, SiO2 particles, and SiO particles, microcracks are self-repaired in the firing process after modeling. A region mainly composed of silicon oxide is locally formed inside an intermediate model formed by an additive modeling method in which laser light is irradiated onto this ceramic modeling powder. In a heat treatment process performed after the intermediate model is formed, the region is melted by the heat treatment, penetrates into the microcracks, and fills the microcracks, repairing the cracks. The heat treatment temperature at this time may be 1690°C or higher, and is preferably in the range of 1690°C to 1790°C. Depending on the metal element in the process of impregnating the metal element-containing liquid, the effect of this embodiment can be obtained by selecting an appropriate temperature at which the microcracks can be repaired even at 1690°C or lower.

[0054] For crack repair, it is important that the repair material of the repair material source melts during heat treatment and seeps from the repair material source into the crack by capillary action, so it is preferable that Si is contained in the ceramics modeling powder for additive manufacturing at 0.72 wt% or more in terms of SiO2. If the amount is less than this, it is not possible to secure a volume sufficient to seep into the crack and backfill it. In addition, even if a cavity occurs in the repair material source in order to backfill the crack, it is not a problem as long as the overall strength is guaranteed. SiO, which functions as a laser light absorber, changes Si from divalent to tetravalent by absorbing laser light, and changes from metastable SiO to more stable SiO2, so the appropriate amount of SiO2 powder to repair cracks is the sum of the amount of SiO2 powder and the amount of SiO powder.

[0055] Furthermore, the ZrO2 particles and SiO2 particles used in this embodiment have a smaller thermal conductivity coefficient than Al2O3 particles, which are common fine ceramic materials. Therefore, heat is transferred from the SiO particles heated by the laser light to the inside of the particles, causing thermal diffusion, and it takes a considerable amount of time for the center temperature to reach the melting point. From this perspective, the average particle size is preferably 100 μm or less, and more preferably 50 μm or less.

[0056] In the method for producing a ceramic shaped product according to the present embodiment, the three-point bending strength of the ceramic shaped product described below is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 150 MPa or more. The three-point bending strength value can be 200 MPa or more. In this way, a ceramic shaped product having higher material strength can be produced. The three-point bending strength value may be 1000 MPa or less, 500 MPa or less, or 400 MPa or less.

[0057] <Third embodiment> The third embodiment relates to a ceramic shaped object. The ceramic shaped object of this embodiment has a portion made of oxides of multiple elements including at least Zr, Y, Si, and optionally Al, within a range of L×M×L (1 μm≦L≦1 mm, 1 μm≦M≦1 mm), When the Zr content in the portion is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, the mass of ZrO2 relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 is defined as α' (mass%), the mass of Y2O3 is β' (mass%), and the mass of SiO2 is γ' (mass%), α', β', and γ' satisfy the following: 77.6≦α'≦93.5 4.4≦β'≦6.5 0.4≦γ'≦17.3 In the ceramic shaped article of the present disclosure, when the mass of Al2O3 relative to the total mass of the ZrO2, the mass of the Y2O3, the mass of the SiO2, and the mass of the Al2O3 is δ' (mass%), it is preferable that δ' satisfies the following: 0.2≦δ'≦8.3

[0058] The explanation of the ranges of α', β', γ', and δ' is omitted because it is the same as the explanation of the ranges of α, β, γ, and δ. The ceramic shaped product of this embodiment preferably has a three-point bending strength of 50 MPa or more, more preferably 100 MPa or more, and even more preferably 150 MPa or more. The three-point bending strength value can also be 200 MPa or more. In this way, a ceramic shaped product with higher strength can be obtained. The three-point bending strength value may be 1000 MPa or less, 500 MPa or less, or 400 MPa or less. Furthermore, the ceramic shaped article of the present disclosure may have a portion within a range of L×M×L (1 μm≦L≦1 mm, 1 μm≦M≦1 mm) that is made of oxides of multiple elements including at least Zr, Y, Si, and possibly Al, and may have a three-point bending strength of 150 MPa or more. The explanation is as follows.

[0059] 2(a) to 2(c) are cross-sectional explanatory views showing a state in which microcracks formed in the intermediate object have been self-repaired after the firing step. FIG. 2(a) is an example of a typical scanning electron microscope (SEM) image of a cross section of a ceramic intermediate object produced using the ceramic powder for additive manufacturing of this embodiment (composed of 3YSZ(Al) particles, SiO2 particles, and SiO particles) after heat treatment at 1730°C. The bright areas in FIG. 2(a) are regions 101 (region z in this embodiment) containing Zr as the main component. The dark areas in FIG. 2(a) are regions 102 containing Si as the main component. The dark areas have at least a length-to-average width ratio of less than 10, and each region is 78.5 μm 2 The first region 104 is a planar portion having an area of ​​10 μm or more (a circle equivalent diameter of 10 μm or more), and the second region 103 (region s in this embodiment) is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more. In this way, in the cross section of the ceramic shaped product, the portion consisting of oxides of multiple elements including at least Zr, Y, Si and possibly Al preferably has a region z mainly containing Zr among the multiple elements, and a region s located between the multiple regions z and mainly containing Si among the multiple elements. Note that the region mainly containing a specific element among the multiple predetermined elements means that the most abundant element among the multiple predetermined elements that can be contained in the region is the specific element, and the most abundant element among the elements contained in the region may be an element other than the multiple predetermined elements (e.g., oxygen). In this embodiment, the multiple predetermined elements may be an element group consisting of only Zr, Y, Si and Al.

[0060] Figures 2(b) and 2(c) are element mapping images (EDS; Energy Dispersive X-ray Spectroscopy) taken using a scanning electron microscope, showing the distribution of Zr and Si, respectively. The area that appears brightest in Figure 2(b) and darkest in Figure 2(c) is region 101, which is mainly composed of Zr. The area that appears brightest in Figure 2(c) and darkest in Figure 2(b) is region 102, which is mainly composed of Si. Region 102 has a length-to-average width ratio of at least less than 10, and each region is 78.5 μm 2 and second regions 103 which are linear portions having an average width of 1 μm or more and a length-to-average width ratio of 10 or more. Regions 102, 103, and 104 contain Si as the main component with some Zr, and correspond to a eutectic composition in the equilibrium phase diagram of ZrO2 and SiO2. Y and Al contained in 3YSZ(Al) may be contained in the region containing Si as the main component.

[0061] As described above, in the heating step of the second embodiment, it is important for the repair of the cracks that the repair material of the repair material source melts during the heat treatment and seeps from the repair material source into the cracks by capillary action. Here, the second region 103 is the portion where the cracks are repaired in the heating step of the second embodiment, and the first region 104 is the repair material source when the cracks are repaired in the heating step of the second embodiment.

[0062] Fig. 3(a) is an enlarged view of a cross section of a shaped object. Fig. 3(a) shows a plurality of regions 101, 103, whose boundaries are indicated by dashed lines. Below, a typical example of the distribution of Zr, Y, Si, and Al in each region will be described. Note that each region may not contain at least any of Zr, Y, Si, and Al. For example, Al may not be present in region 101.

[0063] In FIG. 3(a), region 101 represented by Area#2 is a matrix region. Region 101 contains Zr. Region 101 may contain an amount of Y per unit volume that is less than the amount of Zr per unit volume of region 101. Region 101 may contain an amount of Al per unit volume that is less than the amount of Zr per unit volume of region 101. The amount of Al per unit volume of region 101 may be less than the amount of Y per unit volume of region 101.

[0064] In FIG. 3(a), region 103 represented by Area#1 is a crack repair region (region s in this embodiment). Region 103 contains Si. The amount of Si per unit volume in region 103 may be greater than the amount of Si per unit volume in region 101. Region 103 may contain Al. The amount of Al per unit volume in region 103 may be greater than the amount of Al per unit volume in region 101. Region 103 may contain Y. The amount of Al per unit volume in region 103 may be less than the amount of Si per unit volume in region 103. The amount of Y per unit volume in region 103 may be less than the amount of Si per unit volume in region 103. The amount of Y per unit volume in region 103 may be greater or less than the amount of Al per unit volume in region 103. The amount of Zr per unit volume in region 103 may be less than the amount of Zr per unit volume in region 101, and may be less than the amount of Si per unit volume, the amount of Al per unit volume, and the amount of Y per unit volume in region 101. Region 103 may be an amorphous structure both before and after the heating step in which the intermediate object is heat-treated, but the amorphous structure after the heating step may be stronger than the amorphous structure before the heating step.

[0065] FIG. 3(b) is an enlarged view of a part of the region 103 (part of the region s) in FIG. 3(a). The region 103 includes a plurality of island regions 105 (region r in this embodiment) represented by Area #3 in FIG. 3(b) and an ocean-like region 106 (region t in this embodiment) represented by Area #4 in FIG. 3(b). The ocean-like region 106 separates the plurality of island regions 105. In other words, a continuous ocean-like region 106 is disposed between the plurality of island regions 105. The region s includes a plurality of island regions 105 (region r) and an ocean-like region 106 (region t) separating the plurality of island regions 105 (region r) from one another, and it is preferable that the island region 105 (region r) mainly contains Si. It is preferable that the ocean-like region 106 (region t) contains Al. The ocean-like region 106 may also contain Si, but the amount of Si per unit volume in the ocean-like region 106 may be less than the amount of Si per unit volume in the island-like region 105. The amount of Si per unit volume in the ocean-like region 106 may be less than the amount of Al per unit volume in the ocean-like region 106, but may also be more.

[0066] Furthermore, the island region 105 may also contain Al, but the amount of Al in the island region 105 may be less than the amount of Al in the ocean-like region 106. The amount of Al per unit volume in the island region 105 may be less than the amount of Si per unit volume in the island region 105. Furthermore, the ocean-like region 106 may contain Y. The amount of Y per unit volume in the ocean-like region 106 may be more than the amount of Y per unit volume in the region 101. The island region 105 may also contain Y, but the amount of Y per unit volume in the island region 105 may be less than the amount of Y per unit volume in the ocean-like region 106.

[0067] The composition of the powder for ceramic molding or the ceramic molded object can be measured by inductively coupled plasma atomic emission spectrometry (ICP-AES). Measurement may be performed within a planar area of ​​a square of M (μm) × N (μm) or a three-dimensional area of ​​a square prism of L (μm) × M (μm) × N (μm). Here, L, M, and N are, for example, 1 μm or more, 5 μm or more, 10 μm or more, 50 μm or more, 100 μm or more, 1000 μm or less, and 500 μm or less. Figures 2 and 3 also show the cross-sectional structure of a square prism of these dimensions.

[0068] <Fourth embodiment> The fourth embodiment is a ceramic shaped object. The ceramic shaped object of the present embodiment is a ceramic shaped object containing a plurality of elements including Zr and Si, A region mainly containing Zr and a region mainly containing Si, In an SEM image of a cross section near the center of the ceramic shaped object, at least the region mainly containing Si has a first region and a second region, The first regions have a length to average width ratio of less than 10 and are each 78.5 μm 2 A planar portion having an area of ​​at least The second region is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more, and is in contact with the first region.

[0069] In this specification, zirconium dioxide may be referred to as zirconia or ZrO2, silicon dioxide as silica or SiO2, yttrium oxide as yttria or Y2O3, and aluminum oxide as alumina or Al2O3. Silicon dioxide has several different crystal forms, but when the state of amorphous, crystalline, or crystalline structure does not matter, it will be simply referred to as silicon dioxide or silica, or by the chemical formula SiO2.

[0070] FIG. 2(a) shows a typical scanning electron microscope (SEM) image of a cross section of a ceramic object 100 mainly containing Zr and Si, which is produced by a direct molding method and is composed of ZrO2 and SiO2 as main oxides, after heat treatment at 1730°C. The typical scanning electron microscope (SEM) image of a cross section of a ceramic object here refers to, for example, an SEM image of a cross section near the center of the ceramic object. The bright area in FIG. 2(a) is a region 101 mainly containing Zr. The dark area in FIG. 2(a) is a region 102 mainly containing Si. The region 101 mainly containing Zr and the region 102 mainly containing Si can be distinguished by partial SEM-EDS measurement of the same SEM image or SEM-EDS mapping observation in the same field of view as the SEM image. In addition, the region mainly containing a specific element among the predetermined elements means that the most abundant element among the predetermined elements that can be contained in the region is the specific element, and the most abundant element among the elements contained in the region may be an element other than the predetermined elements (e.g., oxygen). In this embodiment, the predetermined elements may be an element group consisting of only Zr, Y, Si, and Al.

[0071] The dark regions have at least one nebula with a length-to-average width ratio of less than 10 and a diameter of 78.5 μm. 2 The first region 104 is a planar portion having an area of ​​10 μm or more (a circle equivalent diameter of 10 μm or more), and the second region 103 is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more. The planar portion of the first region and the linear portion of the second region refer to the shape (appearance) in the SEM image seen in SEM observation of the cross section, and do not refer to the three-dimensional structure inside the ceramic shaped object. In this embodiment, the ratio of length to average width refers to the ratio of length to average width, that is, length / average width. Here, the length refers to the longitudinal distance of the first region or the second region, and the average width refers to the average value of the distance in the direction perpendicular to the longitudinal direction.

[0072] Figures 2(b) and 2(c) are element mapping images (EDS; Energy Dispersive X-ray Spectroscopy) obtained using a scanning electron microscope, showing the distribution of Zr and Si, respectively. The region that appears brightest in Figure 2(b) and darkest in Figure 2(c) is region 101 that mainly contains Zr. The region that appears brightest in Figure 2(c) and darkest in Figure 2(b) is region 102 that mainly contains Si. Regions 102 have a length-to-average width ratio of at least less than 10, and each region is 78.5 μm 2 The first region 104 is a planar portion having an area of ​​78.5 μm or more, and the second region 103 is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more, the second region 103 being in contact with the first region 104. 2 By having an area of ​​78.5 μm or more, the first region can serve as a reservoir for a substance mainly containing Si, and the ceramic object can have self-repairing properties. 2 or greater, and the second region has an average width of 1 μm or greater and a ratio of length to average width of 10 or greater, the ceramic shaped article can have higher strength.

[0073] FIG. 4(a) is a schematic diagram of FIG. 2(a). Now, assume that the structure is as shown in FIG. 4(a) and a crack 201 occurs as shown in FIG. 4(b) due to external stress during use. At this time, when the ceramic molded product 100 is heat-treated in the above-mentioned temperature range, the first region 104, which has a composition close to a eutectic composition of zirconia and silica (eutectic point 1687°C) and whose melting point is within this temperature range, softens or melts. The molten component spreads from the first region 104 to the crack 201 by the capillary phenomenon, and the crack is repaired by an oxide mainly containing Si, and a new second region 103 is formed as shown in FIG. 4(c). In this way, the ceramic molded product 100 of this embodiment has a function of self-repairing by performing heat treatment again in the range of 1690°C to 1790°C even if a crack occurs, and the ceramic molded product after heat treatment can be restored to the same mechanical strength as the original. This characteristic is an effect obtained due to the presence of the second region 103 in particular among the region 102 that is included in the ceramic object 100 and that mainly contains Si.

[0074] In the ceramic shaped product of this embodiment, the second region 103 included in the ceramic shaped product 100, the new second region 103 which is a self-repaired portion of the crack, and the first region 104 can be observed at least in one place by observing a two-dimensional plane of 2 mm × 2 mm. The second region 103 has an average width of 1 μm or more and a ratio of length to average width of 10 or more, so it can be distinguished from regions not caused by cracks. Here, the average width is, for example, an average value obtained by measuring the width 202 of the second region at five or more places. Also, the average width is, for example, an average value obtained by measuring the width 203 of the first region at five or more places. When the second region 103 extends in a curved shape rather than in a straight line, the length measured along the curve is used. It is preferable to calculate the area of ​​the first region 104, and the value is 78.5 μm 2 The first region 104 and the second region 103 actually have a three-dimensional structure, but in order to allow evaluation to be substituted by cross-sectional observation, it is also preferable to calculate the average value of a plurality of corresponding parts present in an observation region of 2 × 2 mm.

[0075] As described above, the ceramic object 100 of this embodiment is characterized by having an inherent function of self-repairing cracks 201 that occur later. This function occurs when a material mainly containing Si seeps out of the first region 104 into the cracks 201 due to capillary action, which may result in a decrease in the material mainly containing Si in the first region 104 and the generation of voids. This is because the cracks 201, which have a large impact on the mechanical strength, are repaired, and the generation of voids in the first region 104 is relatively unproblematic.

[0076] Furthermore, the ceramic shaped product of this embodiment preferably contains Y and, in some cases, Al. In particular, the region 101 mainly containing Zr is preferably composed of ZrO2, and further preferably contains Y as Y2O3-stabilized ZrO2. The Y2O3 contained in ZrO2 is preferably 1.5 mol% or more and 10.5 mol% or less, and more preferably 2.0 mol% or more and 4.5 mol% or less. In addition, in the region 102 mainly containing Si, it may be present as an oxide consisting of Si and Y.

[0077] In the ceramic shaped product of the present embodiment, when the Zr content is converted into the mass of ZrO2, the Si content is converted into the mass of SiO2, the Y content is converted into the mass of Y2O3, and the Al content is converted into the mass of Al2O3, it is preferable that α', β', and γ' satisfy the following when the mass of ZrO2 is α' (mass %), the mass of Y2O3 is β' (mass %), and the mass of SiO2 is γ' (mass %) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3: 77.6≦α'≦93.5 4.4≦β'≦6.5 0.4≦γ'≦17.3 In this way, the ceramic shaped article of this embodiment can have high strength while maintaining the ability to self-repair cracks.

[0078] With respect to the composition range in terms of SiO2, if the composition is equal to or greater than the lower limit, the self-repairing property of the cracks of the ceramic shaped product of this embodiment can be maintained, and if the composition is equal to or less than the upper limit, high mechanical strength can be achieved. The three-point bending strength value is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 150 MPa or more. The three-point bending strength value can be 200 MPa or more. The three-point bending strength value may be 1000 MPa or less, 500 MPa or less, or 400 MPa or less.

[0079] The ceramic shaped product of this embodiment preferably contains Al, and when the mass of Al2O3 relative to the total mass of the ZrO2, the mass of the Y2O3, the mass of the SiO2, and the mass of the Al2O3 is δ' (mass%), it is preferable that δ' satisfies the following: 0.2≦δ'≦8.3 In this way, the ceramic shaped article of this embodiment can have high strength while maintaining the ability to self-repair cracks.

[0080] The reason why the ceramic shaped product of this embodiment has high strength while maintaining the self-repairing property of cracks is that the Y2O3 concentration of the Y2O3-stabilized ZrO2 in the ceramic shaped product is important, and it is necessary that Si and Al form compounds with Y that do not exclude amorphous matter and play the role of adjusting the Y2O3 concentration in ZrO2. Therefore, the relative relationship between the concentrations of Y and Al in the region 101 that mainly contains Zr and the concentrations of Y and Al in the region 102 that mainly contains Si becomes important. In particular, the present embodiment is characterized by the following three patterns, which differ only slightly in the process of producing the ceramic object.

[0081] (1) In a cross section near the center of the ceramic object, the average value of the SEM-EDS output signal of Zr, the average value of the SEM-EDS output signal of Y, and the average value of the SEM-EDS output signal of Al may be larger in a region mainly containing Zr than in a region mainly containing Si, and the average value of the SEM-EDS output signal of Si may be larger in a region mainly containing Si than in a region mainly containing Zr. This is regarded as the type of the ceramic object being type (III). In this embodiment, the SEM-EDS output signal refers to the integrated intensity of the peak of the characteristic X-rays of the target elements (Zr, Y, Al, Si), and the average value of the SEM-EDS output signal refers to the average value of the SEM-EDS output signal in a region mainly containing Zr or Si.

[0082] (2) In a cross section near the center of the ceramic object, the average value of the SEM-EDS output signal of Zr and the average value of the SEM-EDS output signal of Y may be larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of Si and the average value of the SEM-EDS output signal of Al may be larger in the region mainly containing Si than in the region mainly containing Zr. This is regarded as the type of the ceramic object (II).

[0083] (3) In a cross section near the center of the ceramic object, the average value of the SEM-EDS output signal of Zr may be larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of Si, the average value of the SEM-EDS output signal of Y, and the average value of the SEM-EDS output signal of Al may each be larger in the region mainly containing Si than in the region mainly containing Zr. This is deemed to be the type of the ceramic object (I).

[0084] In the above relative comparison by type, the order of the three-point bending strength that can be high is type (I)>type (II)>type (III). This means that in Table 1, when the three-point bending strength of the ceramic molded object type of type (I) is the maximum value in Example 37, the three-point bending strength of the ceramic molded object type of type (II) is the maximum value in Example 14, and the three-point bending strength of the ceramic molded object type of type (III) is the maximum value in Example 11, the maximum value of the three-point bending strength is type (I)>type (II)>type (III). As mentioned above, it is more preferable that the relative concentrations of Y and Al are high in the region mainly containing Si compared to the region mainly containing Zr. When Al is contained in the raw material powder, it may exist as a region mainly containing Al (region 107 in FIG. 5(h)), but the type can be determined by the region mainly containing Zr and the region mainly containing Si. The three-point bending strength value is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 150 MPa or more. The three-point bending strength value can be 200 MPa or more. The three-point bending strength value may be 1000 MPa or less, 500 MPa or less, or 400 MPa or less.

[0085] Fig. 3(a) is an enlarged view of a cross section of a shaped object. Fig. 3(a) shows a plurality of regions 101, 103, whose boundaries are indicated by dashed lines. Below, a typical example of the distribution of Zr, Y, Si, and Al in each region will be described. Note that each region may not contain at least any of Zr, Y, Si, and Al. For example, Al may not be present in region 101.

[0086] In FIG. 3(a), region 101 represented by Area#2 is a matrix region. Region 101 contains Zr. Region 101 may contain an amount of Y per unit volume that is less than the amount of Zr per unit volume of region 101. Region 101 may contain an amount of Al per unit volume that is less than the amount of Zr per unit volume of region 101. The amount of Al per unit volume of region 101 may be less than the amount of Y per unit volume of region 101.

[0087] In FIG. 3(a), region 103 represented by Area#1 is a crack repair region. Region 103 contains Si. The amount of Si per unit volume in region 103 may be greater than the amount of Si per unit volume in region 101. Region 103 may contain Al. The amount of Al per unit volume in region 103 may be greater than the amount of Al per unit volume in region 101. Region 103 may contain Y. The amount of Al per unit volume in region 103 may be less than the amount of Si per unit volume in region 103. The amount of Y per unit volume in region 103 may be less than the amount of Si per unit volume in region 103. The amount of Y per unit volume in region 103 may be greater or less than the amount of Al per unit volume in region 103. The amount of Zr per unit volume of region 103 may be less than the amount of Zr per unit volume of region 101, and may be less than the amount of Si per unit volume, the amount of Al per unit volume, and the amount of Y per unit volume of region 101.

[0088] FIG. 3(b) is an enlarged view of a part of the region 103 in FIG. 3(a). The region 103 includes a plurality of island regions 105 represented by Area #3 in FIG. 3(b) and a sea-like region 106 represented by Area #4 in FIG. 3(b). The sea-like region 106 separates the plurality of island regions 105. In other words, a continuous sea-like region 106 is disposed between the plurality of island regions 105. The region 103 includes a plurality of island regions 105 and a sea-like region 106 separating the plurality of island regions 105 from each other, and it is preferable that the island region 105 mainly contains Si. It is preferable that the sea-like region 106 contains Al. The sea-like region 106 may also contain Si, but the amount of Si per unit volume of the sea-like region 106 may be less than the amount of Si per unit volume of the island region 105. The amount of Si per unit volume of the ocean-like region 106 may be less than the amount of Al per unit volume of the ocean-like region 106, but it may also be more than that.

[0089] Furthermore, the island region 105 may also contain Al, but the amount of Al in the island region 105 may be less than the amount of Al in the ocean-like region 106. The amount of Al per unit volume in the island region 105 may be less than the amount of Si per unit volume in the island region 105. Furthermore, the ocean-like region 106 may contain Y. The amount of Y per unit volume in the ocean-like region 106 may be more than the amount of Y per unit volume in the region 101. The island region 105 may also contain Y, but the amount of Y per unit volume in the island region 105 may be less than the amount of Y per unit volume in the ocean-like region 106.

[0090] <Modification> The modified example is different from the fourth embodiment in that the ceramic shaped object must contain Al, and the modified example is similar to the fourth embodiment in other respects, so a description of the other points will be omitted. The ceramic shaped object of the modified example is a ceramic shaped object containing a plurality of elements including Zr, Si, and Al, A region mainly containing Zr, a region mainly containing Si, and a region mainly containing Al, the average value of the Zr SEM-EDS output signal is larger in the region mainly containing Zr than in the region mainly containing Si; The average value of the SEM-EDS output signal of the Si, the average value of the SEM-EDS output signal of the Y, and the average value of the SEM-EDS output signal of the Al are each larger in the region mainly containing Si than in the region mainly containing Zr.

[0091] In the ceramic shaped product of the modified example, when the Zr content is converted into the mass of ZrO2, the Si content is converted into the mass of SiO2, the Y content is converted into the mass of Y2O3, and the Al content is converted into the mass of Al2O3, it is preferable that α', β', γ', and δ' satisfy the following when the mass of ZrO2 is α' (mass%), the mass of Y2O3 is β' (mass%), the mass of SiO2 is γ' (mass%), and the mass of Al2O3 is δ' (mass%) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3. 77.6≦α'≦93.5 4.4≦β'≦6.5 0.4≦γ'≦17.3 0.2≦δ'≦8.3 In this way, the ceramic shaped article of this embodiment can have high strength while maintaining the ability to self-repair cracks.

[0092] <Application Examples> An application example of the present disclosure relates to an instrument. The instrument as an application example includes a ceramic shaped object and at least one of an electric component, an optical component, a metal component, and a resin component. Various devices can be configured by combining a mechanical part that is a ceramic molded object with at least one of an electric part, an optical part, a metal part, and a resin part. The mechanical part is, for example, a link part used as a hand or an arm, but may also be a transmission part such as a gear, a cam, or an axis, or a coupling part such as a screw. The mechanical part of this embodiment can also be used as a heat-resistant part or a fire-resistant part. The device having the mechanical part can be a printing device or an office device such as an inkjet printer, a laser printer, a scanner, a copier, or a multifunction device. The device can be an imaging device such as a camera, a display, or a projector. The device can be an optical device such as an interchangeable lens or a binocular. The device can be a medical device such as an X-ray device, a CT, an MRI, or an endoscope. The device can be an industrial device such as an exposure device, a film forming device, a generator, or a robot. The device can be various mobile devices or transportation devices such as an automobile, an aircraft, or a ship. The device can also be a scientific device such as a nuclear reactor (nuclear fusion reactor, nuclear fission reactor), an accelerator, or a space device such as a rocket or an artificial satellite. EXAMPLES

[0093] Table 1 shows a list of examples and comparative examples of this embodiment. The table shows the material system notation of the raw material powder in the infrared laser melting method and the composition of the raw material powder (ZrO 2、 Y2O 3、The conversion values ​​for SiO2 and Al2O3 (SiO was converted as SiO2) are listed, along with the metal element notation of the modifier during the impregnation process, the number of impregnations, the firing temperature, and the results of the three-point bending strength test (based on JIS R1601:2008, where n=2 average) are listed.

[0094] [Table 1]

[0095] Table 2 shows the material system notation of the raw powder used in the infrared laser melting method, and a relative comparison of the areas mainly containing Zr and the areas mainly containing Si in the SEM-EDS mapping image, with areas with large EDS signals indicated as "○" and areas with small EDS signals indicated as "×", and the results are shown by type of ceramic object, and finally by whether or not cracks have self-repairing ability, indicated as "○" or "×". More details will be given later.

[0096] [Table 2]

[0097] Common points in the production of ceramic objects shown in the examples are described below. The inorganic powder used in the infrared laser melting method was basically made up of three types of particles: zirconia particles, silica particles, and silicon monoxide particles. For the zirconia particles, two types of particles were used: yttrium-stabilized zirconia 4YSZ (TZ-4YS, manufactured by Tosoh Corporation) with a median particle size of 40 μm, and yttrium-stabilized zirconia 3YSZ(Al) (TZ-B30, manufactured by Tosoh Corporation) with a median particle size of 30 μm. For the silica particles, SiO2 (amorphous silica HS304, manufactured by Nippon Steel Chemical & Material Co., Ltd.) with a median particle size of 28 μm was used, for the silicon monoxide particles, SiO (manufactured by Japan NER) with a median particle size of 5 μm was used, and for the alumina particles, Al2O3 (CB-A20S, manufactured by Showa Denko K.K.) with a median particle size of 24 μm was used.

[0098] For each of the examples and comparative examples, the above particles were mixed to obtain the composition of the powder for ceramic molding shown in Table 1 and used. For the infrared laser melting method, a 3D Systems ProXDMP100 was used, and an intermediate object was produced as a precursor to the ceramic object under the common conditions of a layer thickness of 20 μm, a laser power of 30 W, and a scan speed of 160 mm / sec. The shape of the object produced was 5 mm wide x 5 mm thick x 38 mm long.

[0099] Thereafter, for Examples 1, 2, and 19 to 29, the intermediate objects were immersed in various metal component-containing liquids and allowed to penetrate to the inside under reduced pressure. As the metal component-containing liquid, an Al-containing impregnation liquid (Aluminasol 520-A, manufactured by Nissan Chemical Industries, Ltd.) was used in Examples 1, 2, and 19 to 23; an LiSi-containing impregnation liquid (lithium silicate 35, manufactured by Nippon Chemical Industry Co., Ltd.) was used in Example 24; an Na-containing impregnation liquid (sodium polyacrylate 45% in water, manufactured by GELEST Inc.) was used in Example 25; a K-containing impregnation liquid (potassium methoxyethoxide solution, manufactured by Sigma-Aldrich) was used in Example 26; a Ca-containing impregnation liquid (calcium methoxyethoxide, 20% in methoxyethanol, manufactured by GELEST Inc.) was used in Example 27; an Y-containing impregnation liquid (yttrium methoxyethoxide, 15-18% in methoxyethanol, manufactured by GELEST Inc.) was used in Example 28; and two types of impregnation liquids, the Y-containing impregnation liquid and the Al-containing impregnation liquid, were used in Example 29.

[0100] Furthermore, the intermediate object was immersed in the metal component-containing liquid and the pressure was reduced to allow the metal component-containing liquid to penetrate into the fine cracks, after which a drying process was performed at 600°C. Table 1 shows the number of times the process was repeated. Note that 0.5 times refers to the case where the impregnation liquid was diluted by two times. The heat treatment was performed at a maximum temperature of 1690°C to 1790°C, and was held for 20 minutes.

[0101] <Evaluation> [Three-point bending strength test] The bending strength of high-strength ceramics was measured for structures fabricated using direct molding methods (powder bed fusion or infrared laser melting) using the JIS R1601:2008 test method for three-point bending strength test of fine ceramics. The three-point bending strength test was conducted in accordance with JIS R1601:2008, with n=2 as the average. The test piece size was 3mm x 4mm x 38mm, and the bending strength test was performed with the following conditions: test piece width W=4mm, test piece thickness T=3mm, support distance L=30mm, and indentation speed 0.5mm / min. If the maximum load (N) at which the test piece breaks is P, the bending strength [MPa] is calculated as follows: (3×P×L) / (2×W×T 2 The average bending strength obtained from two test pieces prepared under the same conditions was then calculated. The results are shown in Table 1.

[0102] [Cross-section SEM observation and SEM-EDS measurement signal] A 3mm x 4mm cross section near the center of the test piece that broke in the three-point bending strength test was cut to a thickness of about 2mm using a diamond wire saw or a low-speed precision cutting machine. The test piece was fixed to a polishing jig, and the 3mm x 4mm cross section of the test piece was precision polished. Polishing was performed by gradually changing the grain size of the abrasive from coarse to fine, and polishing was performed in the order of 6μmφ, 3μmφ, and 1μmφ diamond paste, and finally buffed with colloidal silica, followed by ultrasonic cleaning to ensure that no abrasive remained on the polished surface. SEM observation (SEM observation of the cross section) was performed on the polished surface, and SEM-EDS mapping of Si, Al, Zr, and Y was obtained for the field of view observed by SEM. In the SEM-EDS measurement signals in Table 2, the areas mainly containing Zr and the areas mainly containing Si from the results of SEM-EDS are marked with "○" when Si, Al, Zr, and Y are present in relatively large amounts, and marked with "×" when they are present in relatively small amounts.

[0103] [Ceramics modeling type] The type of ceramic object was determined from the results of SEM observation of the cross section and SEM-EDS measurement signals. The results are shown in Table 2. Details about types (I), (II), and (III) are as described above. Examples marked "II or III" in Table 2 are examples where the ceramic object types are a mixture of types (II) and (III). Figure 5 shows a typical SEM-EDS element mapping image.

[0104] [Crack repairability] In the ceramic shaped object of this embodiment, for example, a three-point bending strength test is performed, and new cracks are generated by impact. For the test pieces broken in the three-point bending strength test, SEM observation and SEM-EDS analysis of the cross section were performed before and after performing the same process as the heating process shown in the method for producing a ceramic shaped object again, to confirm whether the cracks were repaired and the second region was further formed. In Table 2, for examples in which it was confirmed that the cracks were repaired by the second heating process, the repairability of the cracks is indicated as "○" in Table 2, and for examples in which it was not confirmed that the cracks were repaired by the second heating process, the repairability of the cracks is indicated as "×" in Table 2.

[0105] [Composition analysis of ceramic objects] The composition of the ceramic molded object is determined by ICP atomic emission spectrometry (inductively coupled plasma atomic emission spectrometry) of the test piece. The test piece is wrapped in a plastic bag, crushed with a hammer, and diluted by acid decomposition. For acid decomposition, 3 ml of HBF4 liquid, 3 ml of H2SO4 liquid, 3 ml of water, and 20 to 30 mg of the sample are mixed and kept at a maximum temperature of 230°C for 30 minutes. This solution is measured by ICP-AES to quantify the element ratio. A portion of the crushed material is taken and dissolved in two solutions by acid decomposition. ICP-AES measurement is performed twice for each solution, and the average value of the four ICP-AES measurement results is calculated. The results are shown in Table 3.

[0106] [Table 3]

[0107] Example 1 In Example 1, the powder for molding was composed of Zr, Y, and Si as elements, and 10 g of 4YSZ particles was weighed out at a ratio of 0.77 g of SiO2 particles and 0.124 g of SiO particles, and mixed uniformly to form an inorganic material powder having the composition ratio shown in Table 1, which was then used to mold an intermediate product that would become a ceramic product. The cracks in the intermediate product were impregnated with Al as a modifier three times, and the product was heat-treated at a heat treatment temperature (firing temperature in Table 1) of 1730°C, and processed into a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to form a test specimen for a three-point bending strength test. Two of these test specimens were subjected to a three-point bending strength test. The average value of the three-point bending strength was 157 MPa.

[0108] Example 2 A test specimen for a three-point bending strength test was prepared in the same manner as in Example 1, except that the heat treatment temperature was changed to 1750°C, and a three-point bending strength test was performed. The average value of the three-point bending strength was 158 MPa. When SEM-EDS analysis was performed on the cross section, it was confirmed that the average value of the SEM-EDS detection signal of Zr and the average value of the SEM-EDS detection signal of Y in the region mainly containing Zr was larger than that in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si and the average value of the SEM-EDS detection signal of Al in the region mainly containing Si was larger than that in the region mainly containing Zr, and the type of the ceramic molded object was type (II). Figure 5(a) shows EDS element mapping images of Zr, Si, Y, and Al.

[0109] (Examples 3 to 8) In Examples 3 to 8, the powder for molding was composed of elements Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 1.88 g of SiO2 particles and 0.154 g of SiO particles, and mixed uniformly to form an inorganic material powder having the composition ratio shown in Table 1, which was then used to mold an intermediate product that would become a ceramic product. The intermediate product was heat-treated from 1690°C to 1790°C at 20°C intervals, and processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of the test specimens prepared as described above. The average three-point bending strength was 161 MPa for Example 3, 198 MPa for Example 4, 197 MPa for Example 5, 200 MPa for Example 6, 228 MPa for Example 7, and 217 MPa for Example 8. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that in all samples, the average value of the SEM-EDS detection signal of Zr, the average value of the SEM-EDS detection signal of Y, and the average value of the SEM-EDS detection signal of Al were larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si was larger in the region mainly containing Si than in the region mainly containing Zr, and all the ceramic objects were type (III). Figure 5(b) shows the EDS element mapping images of Zr, Si, Y, and Al in Example 8.

[0110] (Examples 9 to 11) In Examples 9 to 11, the powder for molding was composed of elements Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.77 g of SiO2 particles and 0.124 g of SiO particles, and mixed uniformly to form an inorganic material powder having the composition ratio shown in Table 1, which was then used to mold an intermediate product that would become a ceramic product. The intermediate product was heated at 1690°C to 1730°C in 20°C increments, and processed into a bending strength test shape of width 4 mm x thickness 3 mm x total length 38 mm, which was used as a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of each of the test specimens prepared as described above. The average three-point bending strength was 179 MPa for Example 9, 214 MPa for Example 10, and 239 MPa for Example 11. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that in each sample, there were regions with a ceramic object type of type (III) characterized in that the average value of the SEM-EDS detection signal of Zr, the average value of the SEM-EDS detection signal of Y, and the average value of the SEM-EDS detection signal of Al are larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si is larger in the region mainly containing Si, and regions with a ceramic object type of type (II) characterized in that the average value of the SEM-EDS detection signal of Zr and the average value of the SEM-EDS detection signal of Y are larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si and the average value of the SEM-EDS detection signal of Al are larger in the region mainly containing Si. Figure 5 (c) shows the EDS element mapping images of Zr, Si, Y, and Al in Example 11. Figure 5(c) shows the distribution of Zr, Si, Y, and Al when the ceramic object type is type (III).

[0111] (Examples 12 to 14) In Examples 12 to 14, the powder for molding was composed of Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.77 g of SiO2 particles and 0.124 g of SiO particles, and mixed uniformly to form an inorganic material powder having the composition ratio shown in Table 1, which was then used to mold an intermediate product that would become a ceramic product. The intermediate product was heated at 1750°C to 1790°C in 20°C increments, and processed into a bending strength test shape of width 4 mm x thickness 3 mm x total length 38 mm, which was used as a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of each of the test specimens prepared as described above. The average three-point bending strength was 259 MPa for Example 12, 274 MPa for Example 13, and 286 MPa for Example 14. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that the ceramic object type was a type (II) region, characterized in that the average value of the SEM-EDS detection signal of Zr and the average value of the SEM-EDS detection signal of Y in each sample were larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si and the average value of the SEM-EDS detection signal of Al were larger in the region mainly containing Si than in the region mainly containing Zr. Figure 5(d) shows the EDS element mapping images of Zr, Si, Y, and Al in Example 14.

[0112] (Examples 15 and 16) In Examples 15 and 16, the powder for molding was composed of Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.29 g of SiO2 particles and 0.111 g of SiO particles, and mixed uniformly to form an inorganic material powder having the composition ratio shown in Table 1, which was then used to form an intermediate product that would become a ceramic product. The intermediate product was heat-treated at 1770°C and 1790°C, and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm, and used as a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of the test specimens produced in the above manner. The average three-point bending strength was 172 MPa for Example 15 and 260 MPa for Example 16. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that the ceramic object type was a type (II) region, characterized in that the average value of the SEM-EDS detection signal of Zr and the average value of the SEM-EDS detection signal of Y in the region mainly containing Zr were larger than the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si and the average value of the SEM-EDS detection signal of Al were larger in the region mainly containing Si than in the region mainly containing Zr. Figure 5(e) shows the EDS element mapping images of Zr, Si, Y, and Al in Example 16.

[0113] (Examples 17 and 18) In Examples 17 to 18, the powder for molding was composed of Zr, Y, Si, and Al as elements, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.29 g of SiO2 particles and 0.111 g of SiO particles, and mixed uniformly to form an inorganic material powder with the composition ratio shown in Table 1, which was then used to mold an intermediate product that would become a ceramic product. In Examples 17 and 18, the powders were heat-treated at heating temperatures of 1770°C and 1790°C, respectively, and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form test specimens for a three-point bending strength test. A three-point bending strength test was performed on two of each of the test specimens prepared as described above. The average three-point bending strength was 83 MPa for Example 17 and 87 MPa for Example 18. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that the ceramic object type was a type (I) region, characterized in that in all samples, the average value of the SEM-EDS detection signal of Zr was larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si, the average value of the SEM-EDS detection signal of Y, and the average value of the SEM-EDS detection signal of Al were larger in the region mainly containing Si than in the region mainly containing Zr. Figure 5(f) shows EDS element mapping images of Zr, Si, Y, and Al in Example 18.

[0114] (Example 19) In Example 19, the powder for molding was composed of elements Zr, Y, Si, and Al, and was weighed out at a ratio of 10 g of 3YSZ(Al) particles to 0.103 g of SiO particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The cracks in the intermediate product were impregnated with Al of the modifier three times, and the product was heat-treated at a processing temperature of 1750 ° C., and processed into a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two test specimens prepared as described above. The average value of the three-point bending strength was 212 MPa.

[0115] (Example 20) In Example 20, the powder for molding was composed of elements Zr, Y, Si, and Al, and was weighed out at a ratio of 10 g of 3YSZ(Al) particles to 0.103 g of SiO particles, and mixed uniformly to form an intermediate molded object that would become a ceramic molded object as an inorganic material powder with the composition ratio shown in Table 1. The cracks in the intermediate molded object were impregnated with Al of the modifier three times, and the intermediate molded object was heat-treated at a processing temperature of 1770 ° C., and processed into a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two test specimens prepared as described above. The average value of the three-point bending strength was 351 MPa. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that the ceramic object type was a type (I) region, characterized in that in all samples, the average value of the SEM-EDS detection signal of Zr was larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si, the average value of the SEM-EDS detection signal of Y, and the average value of the SEM-EDS detection signal of Al were larger in the region mainly containing Si than in the region mainly containing Zr. Figure 5(g) shows EDS element mapping images of Zr, Si, Y, and Al in Example 20.

[0116] Example 21 In Example 21, an intermediate product similar to that in Example 16 was produced. The cracks in the intermediate product were impregnated with Al of the modifier 0.5 times, and the product was heat-treated at a processing temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. A three-point bending strength test was carried out on two test specimens produced in the above manner. The average value of the three-point bending strength was 280 MPa.

[0117] Example 22 In Example 22, an intermediate product similar to that in Example 17 was produced. The cracks in the intermediate product were impregnated with Al modifier three times, and the product was heat-treated at a processing temperature of 1770°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. A three-point bending strength test was carried out on two test specimens produced in the above manner. The average three-point bending strength was 141 MPa.

[0118] Example 23 In Example 23, an intermediate product similar to that in Example 17 was produced. The cracks in the intermediate product were impregnated with Al modifier three times, and the product was heat-treated at a processing temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. A three-point bending strength test was carried out on two test specimens produced in the above manner. The average three-point bending strength was 173 MPa.

[0119] Example 24 In Example 24, an intermediate product similar to that in Example 16 was produced. The intermediate product was impregnated with LiSi modifier twice into the cracks, and then heated at a heating temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. The two test specimens produced in the above manner were subjected to a three-point bending strength test. The average three-point bending strength was 234 MPa.

[0120] (Example 25) In Example 25, an intermediate product similar to that in Example 16 was produced. The cracks in the intermediate product were impregnated with Na modifier twice, and the product was heat-treated at a processing temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. The two test specimens produced in the above manner were subjected to a three-point bending strength test. The average three-point bending strength was 230 MPa.

[0121] (Example 26) In Example 26, an intermediate product similar to that in Example 16 was produced. The intermediate product was impregnated with K modifier twice into the cracks, and then heat-treated at a processing temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. The two test specimens produced in the above manner were subjected to a three-point bending strength test. The average three-point bending strength was 221 MPa.

[0122] Example 27 In Example 27, an intermediate product similar to that in Example 16 was produced. The intermediate product was impregnated with Ca as a modifier twice in the cracks, and then heated at a heating temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. The two test specimens produced in the above manner were subjected to a three-point bending strength test. The average three-point bending strength was 278 MPa.

[0123] (Example 28) In Example 28, an intermediate product similar to that in Example 16 was produced. The intermediate product was impregnated with the modifier Y three times in the cracks, and then heated at a heating temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. Two test specimens produced in the above manner were subjected to a three-point bending strength test. The average three-point bending strength was 239 MPa.

[0124] (Example 29) In Example 29, an intermediate product similar to that in Example 16 was produced. The cracks in the intermediate product were impregnated with the modifier Y twice and with Al once, and the product was heat-treated at a heating temperature of 1790°C. The product was processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to prepare a test specimen for a three-point bending strength test. The two test specimens produced in the above manner were subjected to a three-point bending strength test. The average value of the three-point bending strength was 277 MPa.

[0125] (Examples 30 and 31) In Examples 30 and 31, the powder for molding was composed of Zr, Y, Si, and Al as elements, and 10 g of 3YSZ(Al) particles was weighed out in a ratio of 0.29 g of SiO2 particles, 0.111 g of SiO particles, and 0.44 g of Al2O3 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at 1750°C and 1790°C, and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two test specimens prepared as described above. The average three-point bending strength was 77 MPa for Example 30 and 103 MPa for Example 31.

[0126] (Examples 32 and 33) In Examples 32 and 33, the powder for molding was composed of Zr, Y, Si, and Al as elements, and 10 g of 3YSZ(Al) particles was weighed out in a ratio of 0.87 g of SiO2 particles, 0.144 g of SiO particles, and 1.09 g of Al2O3 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at 1710°C and 1750°C, and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of the test specimens prepared as described above. The average three-point bending strength was 168 MPa for Example 32 and 164 MPa for Example 33.

[0127] (Examples 34 and 35) In Examples 34 and 35, the powder for molding was composed of Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.106 g of SiO particles and 0.23 g of Al2O3 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at 1690°C and 1790°C and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of the test specimens produced in the above manner. The average three-point bending strength was 183 MPa for Example 34 and 316 MPa for Example 35.

[0128] (Examples 36 and 37) In Examples 36 and 37, the powder for molding consisting of elements Zr, Y, Si, and Al was weighed out in a ratio of 0.11 g of SiO particles and 0.42 g of Al2O3 particles to 10 g of 3YSZ(Al) particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at 1690°C and 1790°C and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of the test specimens produced in the above manner. The average three-point bending strength was 196 MPa for Example 36 and 361 MPa for Example 37. SEM-EDS analysis was performed on the cross section of each sample, and it was confirmed that the ceramic object type was a type (I) region, characterized in that in all samples, the average value of the SEM-EDS detection signal of Zr was larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS detection signal of Si, the average value of the SEM-EDS detection signal of Y, and the average value of the SEM-EDS detection signal of Al were larger in the region mainly containing Si than in the region mainly containing Zr. In this example, there is a region mainly containing Al, where the detection signal of Zr and the detection signal of Si are small and the signal of Al is large. When comparing the average value of the SEM-EDS detection signal of Al in the region mainly containing Zr and the region mainly containing Si, it is larger in the region mainly containing Si, so that it can be determined that the ceramic object type is type (I). Figure 5 (h) shows the EDS element mapping images of Zr, Si, Y, and Al in Example 37.

[0129] (Examples 38 and 39) In Examples 38 and 39, the powder for molding was composed of Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.117 g of SiO particles and 0.90 g of Al2O3 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at 1690°C and 1790°C and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two of the test specimens prepared as described above. The average three-point bending strength was 278 MPa for Example 38 and 203 MPa for Example 39.

[0130] (Examples 40 and 41) In Examples 40 and 41, the powder for molding was composed of Zr, Y, Si, and Al, and 10 g of 3YSZ(Al) particles was weighed out at a ratio of 0.055 g of SiO particles and 0.42 g of Al2O3 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at 1690°C and 1790°C and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two test specimens prepared as described above. The average three-point bending strength was 151 MPa for Example 40 and 325 MPa for Example 41.

[0131] Comparative Example 1 In Comparative Example 1, the inorganic material powder composition was the same as in Example 9, but SiO2 (amorphous silica HS207, manufactured by Nippon Steel Chemical & Material) with a median value of 9.5 μm was used as the silica particles. In this inorganic material powder, the particle size was reduced, which deteriorated the powder fluidity, and the powder layer 302 could not be formed flat in the arrangement step, so modeling could not be performed. For this reason, the powder fluidity was determined to be ×. In the comparative examples and examples other than Comparative Example 1, modeling could be performed in the arrangement step, so the powder fluidity was determined to be ○.

[0132] Comparative Example 2 In Comparative Example 2, an inorganic material powder composition was used in which the ratio of SiO, an infrared absorber, was 1 / 4 compared to Example 20. Although there was no problem with the powder fluidity, the low addition ratio of the infrared absorber reduced the shape formability, resulting in a porous, non-uniform intermediate object with many defects, and it was not possible to obtain an intermediate object in a state in which the heat treatment process could be performed. For this reason, the shape formability was determined to be ×. In the comparative examples and examples other than Comparative Examples 1 and 2, intermediate objects in a state in which the heat treatment process could be performed could be obtained, so the shape formability was determined to be ○.

[0133] Comparative Example 3 In Comparative Example 3, the powder for molding, which is composed of elements Si and Al, was weighed out in a ratio of 12.08 g of Al2O3 particles and 0.47 g of SiO2 particles per 10 g of SiO2 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The intermediate product was heat-treated at a processing temperature of 1690°C and processed to a width of 4 mm, thickness of 3 mm, and total length of 38 mm to be used as a test specimen for a three-point bending strength test. Here, the Al2O3 powder used had a median particle size of 20 μm (AS-20S, manufactured by Showa Denko). In addition, the intermediate product was produced under conditions of an infrared laser scanning speed of 130 mm / sec, compared to 160 mm / sec in the example group, to maintain a dense state. A three-point bending strength test was performed on two ceramic products produced in the above manner. The average value of the three-point bending strength was 108 MPa. From the above, it was found that the ceramic objects fabricated using the material system consisting of SiO2, Al2O3 and SiO had a self-repair function for cracks, but their three-point bending strength was less than 150 MPa.

[0134] Comparative Example 4 In Comparative Example 4, the powder for molding consisting of elements Al, Gd, and Tb was weighed out in a ratio of 9.52 g of Gd2O3 particles and 0.86 g of Tb4O7 particles per 10 g of Al2O3 particles, and mixed uniformly to form an intermediate product that would become a ceramic product as an inorganic material powder with the composition ratio shown in Table 1. The cracks in the intermediate product were impregnated with Zr as a modifier once, and after a heat treatment process at 1690°C, the Zr impregnation process and the heat treatment process were further performed twice, for a total of three impregnation processes and heat treatment processes to repair the cracks. The product was then processed to a width of 4 mm, a thickness of 3 mm, and a total length of 38 mm to form a test specimen for a three-point bending strength test. A three-point bending strength test was performed on two test specimens. It was confirmed that the average value of the three-point bending strength was 140 MPa. In this comparative example, the Al2O3 powder used had a median particle size of 24 μm (CB-A20S, manufactured by Showa Denko). In addition, the infrared laser scanning speed for the intermediate object was set to 130 mm / sec, compared to 160 mm / sec in the example group, to maintain a dense state.

[0135] From the above, the ceramic shaped object made of the material system consisting of Al2O3, Gd2O3, and Tb4O7 was subjected to Zr impregnation and crack repair by heat treatment, but the three-point bending strength was less than 150 MPa. Among Examples 1 to 29, except for Examples 17 and 18, a three-point bending strength exceeding that of Comparative Example 4 was achieved. [Industrial Applicability]

[0136] According to this embodiment, by using a direct manufacturing method (powder bed fusion or infrared laser melting), it is possible to provide a ceramic object containing zirconium oxide having a mechanical strength of 150 MPa or more, or even 200 MPa or more, and having the ability to repair fine cracks.

[0137] The present disclosure includes the following embodiments. (Configuration 1) A ceramic modeling powder composed of oxide particles for use in an additive modeling method in which modeling is performed by irradiating a laser beam, the oxide particles include a plurality of elements including at least Zr, Y, Si, and optionally Al, and include at least particles of silicon monoxide; A powder for ceramic molding in which, when the Zr content is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, and when the mass of ZrO2 is defined as α (mass%), the mass of Y2O3 is defined as β (mass%), and the mass of SiO2 is defined as γ (mass%) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3, α, β, and γ satisfy the following: 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29 (Configuration 2) 2. The powder for ceramic forming according to claim 1, wherein the oxide particles include silicon dioxide particles. (Configuration 3) 3. The powder for ceramic shaping according to claim 1 or 2, wherein the oxide particles include yttria-stabilized zirconia particles. (Configuration 4) A powder for ceramic forming according to any one of configurations 1 to 3, wherein when the silicon monoxide particles do not contain any region other than the silicon monoxide, the average particle size of the oxide particles other than the silicon monoxide particles is 10 μm or more and 200 μm or less and is equal to or greater than the average particle size of the silicon monoxide particles. (Configuration 5) A powder for ceramic shaping according to any one of configurations 1 to 4, wherein when the silicon monoxide particles do not contain any region other than the silicon monoxide, the average particle size of the silicon monoxide particles is 1 μm or more and 10 μm or less, and is 1 / 5 or less of the average particle size of the oxide particles other than the silicon monoxide particles. (Configuration 6) 4. The powder for ceramic shaping according to any one of configurations 1 to 3, wherein when the silicon monoxide particles contain regions other than the silicon monoxide, the average particle size of the silicon monoxide particles is 5 μm or more and 200 μm or less. (Configuration 7) 7. The powder for ceramic shaping according to any one of configurations 1 to 6, wherein the oxide particles include particles of yttria-stabilized zirconia to which alumina has been added. (Configuration 8) The oxide particles contain the Al, The powder for ceramic molding according to any one of configurations 1 to 7, in which δ (mass%) is the mass of Al2O3 relative to the total mass of ZrO2, Y2O3, SiO2, and Al2O3, and δ satisfies the following: 0.21≦δ≦9.17 (Configuration 9) 9. The powder for forming ceramics according to any one of configurations 1 to 8, wherein the content of the silicon monoxide particles in the oxide particles is 0.5 volume % or more and 53 volume % or less. (Configuration 10) 10. The powder for ceramic shaping according to any one of configurations 1 to 9, having a fluidity index of 40 (sec / 50 g) or less. (Configuration 11) 11. The powder for ceramic shaping according to any one of configurations 1 to 10, which does not contain a resin binder. (Configuration 12) 12. The powder for ceramic shaping according to any one of configurations 1 to 11, which does not contain simple carbon. (Method 1) a step of disposing oxide particles on a base; an irradiation step of irradiating a part or all of the oxide particles with laser light to melt and solidify the oxide particles at the places irradiated with the laser light, thereby obtaining an intermediate object; a heating step of heat-treating the intermediate object; A method for producing a ceramic shaped object, comprising: The oxide particles contain a plurality of elements including at least Zr, Y, Si, and optionally Al, and contain at least silicon monoxide particles, and when the Zr content is converted into the mass of ZrO2, the Y content is converted into the mass of Y2O3, the Si content is converted into the mass of SiO2, and the Al content is converted into the mass of Al2O3, when the mass of ZrO2 is defined as α (mass%), the mass of Y2O3 is defined as β (mass%), and the mass of SiO2 is defined as γ (mass%) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3, α, β, and γ satisfy the following: 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29 (Method 2) The method for producing a ceramic object according to method 1, further comprising an impregnation step of impregnating the intermediate object with a liquid containing a metal component after the irradiation step and before the heating step. (Method 3) The method for producing a ceramic shaped article according to Method 2, wherein the metal component-containing liquid contains at least one metal component selected from the group consisting of Li, Na, K, Ca, Y, Al, Zr and Si. (Method 4) The method for producing a ceramic shaped article according to Method 3, wherein the metal component is Al. (Method 5) 5. The method for producing a ceramic shaped article according to any one of Methods 1 to 4, wherein the heating step comprises carrying out a heat treatment at 1690° C. or higher and 1790° C. or lower. (Method 6) A method for producing a ceramic shaped article according to any one of methods 1 to 5, wherein the oxide particles contain the Al, and when the mass of the Al2O3 relative to the total mass of the ZrO2, the mass of the Y2O3, the mass of the SiO2, and the mass of the Al2O3 is δ (mass%), δ satisfies the following: 0.21≦δ≦9.17 (Configuration 13) A ceramic shaped object containing multiple elements including Zr and Si, A region mainly containing Zr and a region mainly containing Si, In an SEM image of a cross section near the center of the ceramic shaped object, at least the region mainly containing Si has a first region and a second region, The first regions have a length to average width ratio of less than 10 and are each 78.5 μm 2 A planar portion having an area of ​​at least The second region is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more, and is in contact with the first region of the ceramic shaped article. (Configuration 14) 14. The ceramic shaped article of claim 13, further comprising Y and optionally Al. (Configuration 15) 15. The ceramic shaped article according to configuration 14, wherein when the Zr content is converted into the mass of ZrO2, the Si content is converted into the mass of SiO2, the Y content is converted into the mass of Y2O3, and the Al content is converted into the mass of Al2O3, and when the mass of ZrO2 is defined as α' (mass%), the mass of Y2O3 is defined as β' (mass%), and the mass of SiO2 is defined as γ' (mass%) relative to the total amount of the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3, α', β', and γ' satisfy the following: 77.6≦α'≦93.5 4.4≦β'≦6.5 0.4≦γ'≦17.3 (Configuration 16) 16. The ceramic shaped article according to claim 14 or 15, comprising Al. (Configuration 17) 17. The ceramic shaped article according to claim 16, wherein when the mass of Al2O3 relative to the total mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 is δ' (mass%), δ' satisfies the following: 0.2≦δ'≦8.3 (Configuration 18) A ceramic object according to any one of configurations 13 to 17, wherein, in the cross section, the average value of the SEM-EDS output signal of the Zr, the average value of the SEM-EDS output signal of the Y, and the average value of the SEM-EDS output signal of the Al are each larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of the Si is larger in the region mainly containing Si than in the region mainly containing Zr. (Configuration 19) A ceramic object according to any one of configurations 13 to 17, wherein, in the cross section, the average value of the SEM-EDS output signal of the Zr and the average value of the SEM-EDS output signal of the Y are each larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of the Si and the average value of the SEM-EDS output signal of the Al are each larger in the region mainly containing Si than in the region mainly containing Zr. (Configuration 20) A ceramic object according to any one of configurations 13 to 17, wherein, in the cross section, the average value of the SEM-EDS output signal of Zr is larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of Si, the average value of the SEM-EDS output signal of Y, and the average value of the SEM-EDS output signal of Al are each larger in the region mainly containing Si than in the region mainly containing Zr. (Configuration 21) A ceramic shaped object containing a plurality of elements including Zr, Si, and Al, A region mainly containing Zr, a region mainly containing Si, and a region mainly containing Al, the average value of the Zr SEM-EDS output signal is larger in the region mainly containing Zr than in the region mainly containing Si; A ceramic object in which the average value of the SEM-EDS output signal of the Si, the average value of the SEM-EDS output signal of the Y, and the average value of the SEM-EDS output signal of the Al are each larger in the region mainly containing Si than in the region mainly containing Zr. (Configuration 22) 22. The ceramic shaped article according to claim 21, wherein when the Zr content is converted into the mass of ZrO2, the Si content is converted into the mass of SiO2, the Y content is converted into the mass of Y2O3, and the Al content is converted into the mass of Al2O3, and the mass of ZrO2, the mass of Y2O3, the mass of SiO2, and the mass of Al2O3 is expressed as α' (mass%), β' (mass%), γ' (mass%), and δ' (mass%) relative to the total mass of ZrO2, Y2O3, SiO2, and Al2O3, α', β', γ', and δ' satisfy the following: 77.6≦α'≦93.5 4.4≦β'≦6.5 0.4≦γ'≦17.3 0.2≦δ'≦8.3 (Configuration 23) A ceramic shaped article according to any one of configurations 13 to 22, An apparatus comprising at least one of an electrical component, an optical component, a metal component, and a resin component. [Explanation of symbols]

[0138] Region containing mainly 101 Zr Region containing mainly 102 Si 103 Second Area 104 First Area 105 Island area 106 Oceanic region Region containing mainly 107 Al 201 Crack 202 Width of the second area 203 Width of the first area 301 Powder 302 Powder layer 303 Unconsolidated powder 310 Sculptures 330 Foundations 351 Stage 352 Roller 380 Laser Light Source 381 Scanner section 401 Cladding Nozzle 402 Powder supply hole 403 Laser Light

Claims

1. A ceramic modeling powder composed of oxide particles for use in an additive modeling method in which modeling is performed by irradiating a laser beam, The oxide particles include a plurality of elements including at least Zr, Y, Si, and optionally Al, and include at least particles of silicon monoxide; The content of Zr is ZrO 2 The content of Y is calculated as Y 2 O 3 The Si content is converted to SiO 2 The content of Al is converted to the mass of Al 2 O 3 The mass of the ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The total mass of ZrO 2 The mass of Y is α (mass%). 2 O 3 The mass of the SiO 2 A powder for ceramic molding, in which α, β, and γ satisfy the following, where γ is the mass of the powder. 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29

2. The ceramic shaping powder according to claim 1 , wherein the oxide particles include silicon dioxide particles.

3. 2. The ceramic shaping powder according to claim 1, wherein the oxide particles include yttria-stabilized zirconia particles.

4. The powder for ceramic forming according to claim 1, wherein when the silicon monoxide particles do not contain any regions other than the silicon monoxide, the average particle size of the oxide particles other than the silicon monoxide particles is 10 μm or more and 200 μm or less and is larger than the average particle size of the silicon monoxide particles.

5. The powder for ceramic forming according to claim 1, wherein when the silicon monoxide particles do not contain any regions other than the silicon monoxide, the average particle size of the silicon monoxide particles is 1 μm or more and 10 μm or less and is 1 / 5 or less of the average particle size of the particles of the oxide particles other than the silicon monoxide particles.

6. The ceramic shaping powder according to claim 1, wherein when the silicon monoxide particles contain regions other than the silicon monoxide, the average particle size of the silicon monoxide particles is 5 μm or more and 200 μm or less.

7. 2. The ceramic shaping powder according to claim 1, wherein the oxide particles include particles of yttria-stabilized zirconia to which alumina has been added.

8. The oxide particles contain the Al, The ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The Al relative to the total mass of 2 O 3 The powder for ceramic shaping according to claim 1, wherein δ (mass%) satisfies the following: 0.21≦δ≦9.17

9. 2. The powder for ceramic shaping according to claim 1, wherein the content of the silicon monoxide particles in the oxide particles is 0.5 volume % or more and 53 volume % or less.

10. 2. The powder for ceramic shaping according to claim 1, having a fluidity index of 40 (sec / 50 g) or less.

11. 2. The ceramic shaping powder according to claim 1, which does not contain a resin binder.

12. 2. The ceramic shaping powder according to claim 1, which does not contain elemental carbon.

13. a step of disposing oxide particles on a base; an irradiation step of irradiating a part or all of the oxide particles with laser light to melt and solidify the oxide particles at the places irradiated with the laser light, thereby obtaining an intermediate object; a heating step of heat-treating the intermediate object; A method for producing a ceramic shaped object, comprising: The oxide particles contain a plurality of elements including at least Zr, Y, Si, and optionally Al, and contain at least silicon monoxide particles, and the content of Zr is ZrO 2 The content of Y is calculated as Y 2 O 3 The Si content is converted to SiO 2 The mass of Al is converted to Al 2 O 3 When converted into mass of ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The total mass of ZrO 2 The mass of Y is α (mass%). 2 O 3 The mass of the SiO 2 A method for manufacturing a ceramic shaped object, wherein α, β, and γ satisfy the following, where γ is the mass of the above-mentioned material (mass%). 77.64≦α≦93.06 4.42≦β≦6.49 0.72≦γ≦17.29

14. The method for producing a ceramic shaped product according to claim 13, further comprising an impregnation step of impregnating the intermediate product with a liquid containing a metal component, after the irradiation step and before the heating step.

15. 15. The method for producing a ceramic shaped article according to claim 14, wherein the metal component-containing liquid contains at least one metal component selected from the group consisting of Li, Na, K, Ca, Y, Al, Zr and Si.

16. The method for producing a ceramic shaped article according to claim 15, wherein the metal component is Al.

17. The method for producing a ceramic shaped article according to claim 13, wherein the heating step comprises heat treatment at 1690°C or higher and 1790°C or lower.

18. The oxide particles contain the Al, and the ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The Al relative to the total mass of 2 O 3 The method for producing a ceramic shaped article according to claim 13, wherein δ (mass%) satisfies the following: 0.21≦δ≦9.17

19. A ceramic shaped object containing a plurality of elements including Zr and Si, A region mainly containing Zr and a region mainly containing Si, In an SEM image of a cross section near the center of the ceramic shaped object, at least the region mainly containing Si has a first region and a second region, The first regions have a length to average width ratio of less than 10 and are each 78.5 μm 2 A planar portion having an area of ​​at least The second region is a linear portion having an average width of 1 μm or more and a ratio of length to average width of 10 or more, and is in contact with the first region.

20. The ceramic shaped article according to claim 19 , which contains Y and optionally Al.

21. The content of Zr is ZrO 2 The Si content is converted to SiO 2 The content of Y is calculated as Y 2 O 3 The content of Al is converted to the mass of Al 2 O 3 The mass of the ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The total mass of ZrO 2 The mass of Y is α' (mass%). 2 O 3 The mass of the SiO 2 The ceramic shaped object according to claim 20, wherein α', β', and γ' satisfy the following, where γ' (mass%) is the mass of the ceramic shaped object. 77.6≦α’≦93.5 4.4≦β’≦6.5 0.4≦γ′≦17.3

22. The ceramic shaped article according to claim 20 or 21, which contains Al.

23. The ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The Al relative to the total mass of 2 O 3 The ceramic shaped object according to claim 22, wherein δ' (mass%) satisfies the following: 0.2≦δ′≦8.3

24. The ceramic object according to claim 22, wherein, in the cross section, the average value of the SEM-EDS output signal of the Zr, the average value of the SEM-EDS output signal of the Y, and the average value of the SEM-EDS output signal of the Al are each larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of the Si is larger in the region mainly containing Si than in the region mainly containing Zr.

25. The ceramic object according to claim 22, wherein, in the cross section, the average value of the SEM-EDS output signal of the Zr and the average value of the SEM-EDS output signal of the Y are each larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of the Si and the average value of the SEM-EDS output signal of the Al are each larger in the region mainly containing Si than in the region mainly containing Zr.

26. The ceramic object according to claim 22, wherein, in the cross section, the average value of the SEM-EDS output signal of Zr is larger in the region mainly containing Zr than in the region mainly containing Si, and the average value of the SEM-EDS output signal of Si, the average value of the SEM-EDS output signal of Y, and the average value of the SEM-EDS output signal of Al are each larger in the region mainly containing Si than in the region mainly containing Zr.

27. A ceramic shaped object containing a plurality of elements including Zr, Si, and Al, A region mainly containing Zr, a region mainly containing Si, and a region mainly containing Al, the average value of the SEM-EDS output signal of the Zr is larger in the region mainly containing Zr than in the region mainly containing Si; A ceramic object in which the average value of the SEM-EDS output signal of Si, the average value of the SEM-EDS output signal of Y, and the average value of the SEM-EDS output signal of Al are each larger in the region mainly containing Si than in the region mainly containing Zr.

28. The content of Zr is ZrO 2 The Si content is converted to SiO 2 The content of Y is calculated as Y 2 O 3 The content of Al is converted to the mass of Al 2 O 3 The mass of the ZrO 2 The mass of and the Y 2 O 3 The mass of the SiO 2 The mass of Al 2 O 3 The total mass of ZrO 2 The mass of Y is α' (mass%). 2 O 3 The mass of the SiO 2 The mass of the Al is γ' (mass%). 2 O 3 The ceramic shaped article according to claim 27, wherein α', β', γ', and δ' satisfy the following, where δ' (mass%) is the mass of the ceramic shaped article. 77.6≦α’≦93.5 4.4≦β’≦6.5 0.4≦γ′≦17.3 0.2≦δ′≦8.3

29. The ceramic shaped article according to claim 19 or 27, An apparatus comprising at least one of an electrical component, an optical component, a metal component, and a resin component.

Citation Information

Patent Citations

  • Powder for ceramic shaping, ceramic shaped article, and method for manufacturing the same