Nonwoven laminate
Patent Information
- Application Number
- JP2024071399
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-25
Smart Images

Figure 2024159650000001 
Figure 2024159650000002
Abstract
Description
[Technical field]
[0001] The present invention relates to nonwoven laminates and shaped articles comprising the nonwoven laminates. [Background technology]
[0002] Nonwoven laminates can be molded into molded articles for a variety of applications, such as automotive applications that require lightweight parts with high stability and durability, such as underbody shields.
[0003] EP 3769954 A1 discloses a nonwoven laminate and a molded article made therefrom that can be used as an underbody shield in an automobile. The nonwoven laminate comprises 3-5 layers of nonwoven fabrics melt-bonded to each other. The structure is characterized in that a needled staple fiber nonwoven layer is enclosed between two outer spunbond nonwoven layers. These layers are essentially formed from polyethylene terephthalate (PET) fibers and copolyester fibers for melt bonding. The molded article produced by molding such a nonwoven laminate has high mechanical stability and provides acoustic insulation.
[0004] US Patent Application Publication No. 2016 / 0288451 discloses a nonwoven composite that is moldable and usable in the manufacture of a vehicle underbody, the nonwoven composite including needled polyester staple fiber layers and spunbond polyester fiber layers that are mechanically bonded to one another by needling.
[0005] US 2018 / 0251924 A1 relates to a nonwoven composite that can be used in a variety of applications. The composite features certain hydrophobic PET fibers and polyalkylsiloxane-based or perfluorinated additives.
[0006] However, such nonwoven composites and the resulting molded articles still need improvement. For use in the automotive industry, they must meet stringent internal standards for mechanical stability and durability, thereby ensuring that the product is suitable for long-term use without degradation or loss of advantageous properties. Automotive structural parts such as underbody shields, wheel arch liners, and engine shields are exposed to mechanical stresses and strains over long periods of time. They must maintain their integrity and properties even after long periods of use under demanding conditions. Vehicle structural parts must also be resistant to stone chipping, which occurs continuously during standard use and causes high mechanical strains.
[0007] The problem underlying the invention The object of the present invention is to provide a new material which at least partially overcomes the drawbacks encountered in the art. It is desirable to provide an improved product suitable for structural parts, particularly for vehicle structural parts. The product should have high mechanical stability and be suitable for long term use. Preferably, the material should have good acoustic properties, recyclability, light weight, low heat shrinkage and also exhibit reduced elephant skin effect.
[0008] One particular challenge is to provide materials, such as nonwoven composites and molded articles, that are highly resistant to stone chipping and are therefore ideally suited for structural components in exterior applications such as underbody shields, wheel arch liners, engine shields, etc., where stone chipping is a problem.
[0009] A further challenge is that the material be capable of being manufactured and shaped in an easy and convenient manner: it is desirable that the material be available at low cost and by standard processing methods.
[0010] Disclosure of the Invention Surprisingly, it has been found that the problem underlying the present invention is solved by the nonwoven laminates and molded articles as claimed in the claims. Further embodiments are outlined throughout the specification.
[0011] The subject of the present invention is a nonwoven laminate, which comprises (A) to (C): - a spunbond nonwoven layer (A) comprising fibers comprising polyethylene terephthalate (PET) and a copolyester; - an optional spunbond nonwoven layer (B) comprising fibers comprising polyethylene terephthalate (PET) and a copolyester, wherein nonwoven layer (B) has a higher copolyester content than nonwoven layer (A); - a needled staple fiber nonwoven layer (C) comprising: Monocomponent polyethylene terephthalate (PET) staple fibers (c1), and Multicomponent staple fibers (c2), comprising at least a polyethylene terephthalate (PET) component and a copolyester component. A nonwoven layer (C) It is structured in the order of Here, all layers are melt bonded to one another and are a nonwoven laminate.
[0012] As used herein, the term nonwoven refers to nonwoven fabrics, which are layers of fibers bound by physical and / or chemical means excluding weaving, knitting or papermaking. In general, nonwoven fabrics are defined in DIN EN ISO 9092:2018.
[0013] Spunbond generally refers to fabrics that contain theoretically infinite fibers drawn from molten fiber feedstock. Spunbond nonwoven layers (A) and (B) are preferably each made of continuous filaments that are calendered together in the form of a sheet. In all embodiments described herein, layer (B) is optional unless otherwise indicated.
[0014] Staple fibers generally refer to fibers of varying lengths. A group of staple fibers has an average length of the fibers within the group, which is called the staple length.
[0015] A needled nonwoven layer generally refers to a layer comprised of a plurality of fibers that are intertwined and bonded with needles.
[0016] Polyethylene terephthalate is a copolymer of terephthalic acid and ethane-1,2-diol (also known as ethylene glycol).
[0017] A copolyester is a copolymer of a first diacid monomer, a first diol monomer, and one or both of at least one second different diacid monomer and at least one second different diol monomer, where diacid monomer preferably refers to a dicarboxylic acid monomer.
[0018] Melt bonding (thermal bonding) generally refers to the technique of joining high molecular weight, usually thermoplastic, materials by the application of heat such that at least one of the materials partially melts or softens, bringing the materials into intimate contact, and then cooling.
[0019] In the nonwoven laminate of the present invention, layers (A) and (C), and if present, intermediate layer (B), are melt bonded to one another. This can be accomplished by forming a stack of layers and melt bonding the stack. By melt bonding all layers to one another, high uniformity in the heat shrink properties of the nonwoven laminate can be obtained. High uniformity in the heat shrink properties can reduce the formation of elephant skin during molding. Reduction in the formation of elephant skin can allow the nonwoven laminate to have an attractive aesthetic and a higher flexural strength after molding. Melt bonding of the layers can also impart high dimensional stability to the nonwoven laminate during heating and molding.
[0020] Both layers include polyethylene terephthalate, also referred to herein as "PET." The polyethylene terephthalate may be virgin polyethylene terephthalate (not recycled), recycled polyethylene terephthalate (also referred to as "r-PET"), or a mixture of virgin and recycled polyethylene terephthalate. Virgin polyethylene terephthalate allows for more precise setting of the mechanical properties of the nonwoven laminate. Recycled polyethylene terephthalate can reduce the cost of the nonwoven laminate.
[0021] Polyethylene terephthalate can provide high uniformity in mechanical properties of the nonwoven laminate. It can increase the uniformity of elongation and tensile strength of the nonwoven laminate. It can easily heat and mold the nonwoven laminate to provide a desired configuration. It can be dimensionally stable when heated and molded. Polyethylene terephthalate can provide a relatively low basis weight for the layers and the entire laminate, respectively.
[0022] Polyethylene terephthalate has a relatively high melting point of about 260° C., which allows the nonwoven laminate to have high heat resistance and flame resistance. In this specification, the melting point is preferably the melting point determined in accordance with DIN ISO 11357-3:2013.
[0023] The polyethylene terephthalate contained in all layers is relatively inexpensive, which can provide cost savings for articles containing the nonwoven laminate.
[0024] Both layers contain a copolyester. The copolyester may be an amorphous copolyester, a crystalline copolyester, or a mixture of amorphous and crystalline copolyesters. When present, optional layer (B) has a higher copolyester content than layer (A). The relatively high copolyester content, respectively, can strengthen the bond between layer (A) and layer (C). Thus, the relatively high copolyester content, respectively, can increase the peel strength of layer (A).
[0025] The nonwoven laminate may be composed of layers (A), (B) and (C), or, most preferably, composed only of layers (A) and (C).
[0026] A nonwoven laminate composed of layers (A) and (C) is preferred. A two-ply laminate is advantageous in terms of manufacturing simplicity and cost efficiency. The production of such a laminate does not require an additional feeder for layer (B). Surprisingly, it has been found that a nonwoven laminate composed only of layers (A) and (C) and / or a molded article obtained therefrom can meet the requirements of structural parts for automotive applications.
[0027] Optionally, layer (B) can be included to function as an adhesive layer. Layer (B) can increase the bond strength between outer layer (A) and outer layer (C). In such a laminate, peeling between layer (A) and layer (C) can be advantageously reduced. From the viewpoint of increasing the peel strength, a nonwoven laminate including layers (A), (B) and (C) may be preferred.
[0028] Preferably, none of the layers (A), (B), (C) are mechanically bonded to any other layer in the nonwoven laminate. It is particularly preferred that none of the layers (A), (B), (C) are needled to any other layer. In other words, there is no intertwining between any two of the layers (A), (B), (C). In particular, none of the fibers contained in the needled staple fiber nonwoven layer (C) extend into either of the layers (A) and (B). More preferably, none of the fibers of the needled staple fiber nonwoven layer (C) penetrate either of the layers (A) and (B). The absence of mechanical bonds can minimize the formation of undesirable elephant skin during heating, thereby achieving an attractive aesthetic. Furthermore, molded articles produced from nonwoven laminates without mechanical bonds are advantageously flat, and in particular do not have wrinkles, wavy structures, etc. Furthermore, their bending strength can be increased.
[0029] The needled staple fiber nonwoven layer (C) is preferably heat shrunk before being combined with layer (A). Preferably, the needled fibers shrink in both the machine and cross directions when exposed to heat. The heat shrink layer (C) prevents undesirable further shrinkage, which avoids the formation of undesirable elephant skin during the subsequent molding process.
[0030] It is preferred that less than 20%, more preferably less than 10%, of the total fibers in the nonwoven laminate are not PET or copolyester. Most preferably, all of the fibers in the nonwoven laminate are composed of PET, copolyester, or mixtures thereof. When all of the fibers in the nonwoven laminate are primarily, and preferably exclusively, composed of PET, copolyester, or mixtures thereof, the nonwoven laminate can be relatively low cost, relatively lightweight, and have relatively high peel strength.
[0031] The nonwoven laminate is preferably free of polyolefins, especially polypropylene, which allows the nonwoven laminate to be recycled more easily; which allows the nonwoven laminate to have improved heat resistance and flame resistance; which allows the nonwoven laminate to have improved uniformity in mechanical properties, especially elongation and tensile strength, which allows the properties of products containing the nonwoven laminate to be more easily tailored;
[0032] The nonwoven laminate is preferably free of silicon and / or fluorine. Thus, the nonwoven laminate is free of silicon compounds and / or fluorine compounds. It has been found that advantageous properties can be achieved without additives such as polyalkylsiloxanes and perfluorinated compounds contained in the composites of US Patent Application Publication No. 2018 / 0251924. This is advantageous for convenient processing, low cost and recycling.
[0033] The nonwoven laminate is preferably free of inorganic reinforcement, particularly glass fibers. The absence of inorganic reinforcement, particularly glass fibers, can facilitate processability. The absence of inorganic reinforcement, particularly glass fibers, can reduce the cost of articles that include the nonwoven laminate.
[0034] The nonwoven laminate preferably does not include a lofting agent. The absence of a lofting agent can improve the dimensional stability of the nonwoven laminate when it is heated and molded. The absence of a lofting agent can reduce the cost of articles that include the nonwoven laminate.
[0035] Surprisingly, it has been found that the nonwoven laminate, composed of only the two layers (A) and (C), and the molded articles obtained therefrom, are suitable for structural parts in automotive applications. The mechanical stability as well as the sound absorption are able to meet the standard tests for automotive parts prescribed for original equipment manufacturers (OEMs). Such standards are used in the technical field for parts and devices that are provided for use by other manufacturers.
[0036] It is preferred that the copolyester of all layers is a copolymer of polyethylene terephthalate. The copolymer of polyethylene terephthalate comprises the monomers terephthalic acid, ethane-1,2-diol, and at least one additional different dicarboxylic acid monomer and / or at least one additional different diol monomer. A preferred additional dicarboxylic acid monomer is adipic acid. Another preferred additional dicarboxylic acid monomer is isophthalic acid. A preferred additional diol monomer is cyclohexanedimethanol. The copolymer of polyethylene terephthalate can facilitate the recyclability of the nonwoven laminate. The copolymer of polyethylene terephthalate can increase the peel strength within the nonwoven laminate. The copolymer of polyethylene terephthalate can reduce the raw material cost of the nonwoven laminate.
[0037] It is preferred that the copolyester of all layers has a melting point of ≦240° C. It is more preferred that the copolyester has a melting point of ≦220° C., more preferably ≦210° C., even more preferably ≦200° C., even more preferably ≦190° C., especially =180° C. Copolyesters with melting points of ≦240° C. can reduce the energy required for melt bonding of the layers together. Copolyesters with melting points of ≦240° C. can reduce the energy required for the manufacture of the spunbond layers (A), (B). This energy reduction can increase continuously with decreasing melting points of ≦220° C., ≦210° C., ≦200° C., ≦190° C. and =180° C., respectively.
[0038] The copolyester of layer (A) preferably has a melting point higher than the melting point of the copolyester of layer (C), more preferably ≧20° C. higher, even more preferably ≧30° C. higher, and even more preferably ≧35° C. higher, so that a stronger bond between the layers of the nonwoven laminate after melt bonding can be achieved.
[0039] It is particularly preferred that layer (B) does not exist, and in this case, the copolyester of layer (A) preferably has a melting point of 205 to 240° C., more preferably 210 to 230° C., and even more preferably 210 to 225° C. In this case, the copolyester of layer (C) preferably has a melting point of 160 to 200° C., more preferably 170 to 190° C., and even more preferably 175 to 185° C. This can prevent peeling between layer (A) and layer (C).
[0040] It is preferred that the copolyester of all layers has a melting point of ≧100° C. It is more preferred that the copolyester has a melting point of ≧110° C., more preferably ≧140° C., and even more preferably ≧160° C. Copolyesters having a melting point of ≧100° C. can increase the bond strength between layers after melt bonding.
[0041] It is preferred that the copolyester of all layers has a melting point in the range of 100 to 240° C., more preferably in the range of 110 to 240° C., even more preferably in the range of 140 to 230° C., and even more preferably in the range of 160 to 225° C. Copolyesters having melting points within these ranges can reduce the energy required for melt bonding between layers, can reduce the energy required for producing the spunbond layers (A) and (B), and can increase the bond strength between the layers after melt bonding.
[0042] It is preferred that the copolyester of layers (A), (B), in particular layer (A), is essentially neutral, i.e. has a pH value of 6.5 to 7.5, more preferably 6.8 to 7.2, even more preferably 7.0, in order to avoid undesirable chemical interactions between the surface of the nonwoven laminate and the environment.
[0043] The copolyester of layers (A) and (B), especially layer (A), has a viscosity of 1.1 to 1.6 g / cm 3 , more preferably 1.2 to 1.5 g / cm 3 , and even more preferably 1.3 to 1.4 g / cm 3It is preferred that the laminate has a density of 0.1 to 1.0 mm, which is measured in accordance with DIN EN ISO 1183-1:2019-09. Such a density makes it possible to obtain a laminate having an adequate strength while avoiding excessive costs.
[0044] More preferably, the copolyester of all layers is a copolymer of polyethylene terephthalate, which simultaneously has a melting point of ≦240° C. This simultaneously provides improved peel strength, reduced cost, and reduced energy required to produce the melt bonded and spunbonded layers of each layer.
[0045] When layer (B) is present, layer (A) preferably contains 2% to 30% copolyester, more preferably 5% to 25% copolyester. When layer (B) is not present, layer (A) preferably contains at least 30% copolyester, more preferably 30 to 70% copolyester, particularly preferably at least 40% copolyester, at least 50% copolyester, at least 60% copolyester, or at least 70% copolyester. Such a copolyester content can avoid a wavy structure of the laminate. Such a copolyester content can further achieve an improvement in the bending strength of the laminate. Here, % means weight % unless otherwise specified.
[0046] When layer (B) is present and layer (A) contains 2% to 30% of the copolyester, it may be easier to melt-bond layer (A) to layer (B) or layer (C). When layer (A) contains 2% to 30% of the copolyester, the peel strength of layer (A) can be increased. When layer (A) contains 5% to 25% of the copolyester, the ease of melt-bonding and the peel strength of layer (A) can be further increased.
[0047] When layer (A) contains at least 30%, more preferably at least 40%, at least 50%, at least 60%, or at least 70% of the copolyester, the peel strength can be increased by the laminate without layer (B). This can simplify the production of the laminate. When layer (B) is preferably not present, it is particularly preferred that the copolyester of layer (A) has a melting point of 205 to 240°C, more preferably 210 to 230°C, and even more preferably 210 to 225°C. In this case, the copolyester of layer (C) preferably has a melting point of 160 to 200°C, more preferably 170 to 190°C, and even more preferably 175 to 185°C. This can particularly prevent peeling between layer (A) and layer (C).
[0048] The needled staple fiber nonwoven layer (C) is preferably composed of 10-90% monocomponent staple fibers (c1) and 10-90% multicomponent staple fibers (c2). More preferably, layer (C) is composed of 20-80% monocomponent staple fibers (c1) and 20-80% multicomponent staple fibers (c2), more preferably 30-70% monocomponent staple fibers (c1) and 30-70% multicomponent staple fibers (c2), even more preferably 40-60% monocomponent staple fibers (c1) and 40-60% multicomponent staple fibers (c2), and most preferably 50% monocomponent staple fibers (c1) and 50% multicomponent staple fibers (c2). When layer (C) is composed of 10-90% monocomponent staple fibers (c1) and 10-90% multicomponent staple fibers (c2), it can be more easily manufactured as a needled layer. When layer (C) is composed of 10-90% monocomponent staple fibers (c1) and 10-90% multicomponent staple fibers (c2), it is mainly composed of polyethylene terephthalate. This can reduce the weight of the nonwoven laminate, improve the heat resistance and flame resistance of the nonwoven laminate, and reduce the cost of the nonwoven laminate. These effects become larger as the ratio of (c1) / (c2) approaches a value of 1; that is, these effects become larger in the following order: 20-80%(c1) / 20-80%(c2), 30-70%(c1) / 30-70%(c2), 40-60%(c1) / 40-60%(c2), 50%(c1) / 50%(c2).
[0049] The staple fibers (c1) are monocomponent fibers, i.e. composed of polyethylene terephthalate. The staple fibers (c2) are multicomponent fibers, i.e. composed of two or more components. The first component of the staple fibers (c2) is polyethylene terephthalate. The second component of the staple fibers (c2) is a copolyester. One or more additional components of the staple fibers (c2) may be present. It is preferred that the staple fibers (c2) are bicomponent fibers, i.e. composed of polyethylene terephthalate and a copolyester. It is preferred that the bicomponent fibers have an islands-in-the-sea filament structure, a pie-segment filament structure, a sheath-core filament structure or a side-by-side filament structure, more preferably a sheath-core filament structure. The copolyester component is generally present on the surface of such bicomponent fibers.
[0050] The staple fibres (c2) preferably have at least one, more preferably two or more and most preferably all of the following properties: - a fineness between 1 and 10 dtex, more preferably between 3 and 6 dtex, even more preferably between 4 and 6 dtex, measured according to DIN EN ISO 1973:2020-05; - a fiber length of 30-100 mm, more preferably 40-60 mm, even more preferably 45-55 mm; - a strength, measured according to DIN EN 13844:2003-04, of 1 to 6 g / de, more preferably 2 to 5 g / de, even more preferably 3 to 4 g / de; - an elongation, measured according to DIN EN ISO 5079:2020-01, of 20 to 60%, more preferably 30 to 50%, even more preferably 35 to 55%; - a crimp number, measured according to JIS L-1074, of 4 to 10 EA / inch, more preferably 5 to 9 EA / inch, and even more preferably 6 to 8 EA / inch; - a heat shrinkage at 75°C for 15 min, measured according to DIN EN 13844:2003-04, of 3 to 7%, more preferably 4 to 6%, even more preferably 3.5 to 4.5%; and A melting point of 160-200°C, more preferably 170-190°C, even more preferably 175-185°C.
[0051] When the staple fibers (c2) have at least one, more preferably two or more, and most preferably all of the above characteristics, the needled staple fiber nonwoven layer (C) can simultaneously impart strength, flexibility and moldability to the nonwoven laminate.
[0052] Layer (C) has a coating strength of ≦2900 g / m according to DIN EN 29073-1:1992-08 2 , more preferably 400 to 2500 g / m 2 In standard passenger car applications, the layer (C) preferably has a weight per unit area of 600 to 1500 g / m 2 , more preferably 700 to 1200 g / m 2 , and most preferably 800 to 1000 g / m 2 It is preferable that the fiber has a basis weight of 1000 g / m2 or more.
[0053] The layer (C) is composed of 10-90% monocomponent staple fibres (c1) and 10-90% multicomponent staple fibres (c2) and at the same time has a strength of ≦2900 g / m according to DIN EN 29073-1:1992-08. 2 , more preferably 600 to 1500 g / m 2 In this way, the nonwoven layer (C) can be more easily manufactured as a needled layer, and the nonwoven laminate can be used widely, particularly as a structural part for a vehicle.
[0054] The spunbond nonwoven layer (A) has a density of 20 to 200 g / m according to DIN EN 29073-1:1992-08. 2 , more preferably 30 to 80 g / m 2When such a relatively light spunbond layer is included, the overall properties can be particularly advantageous.
[0055] The entire nonwoven laminate has a density of 650-1600 g / m according to DIN EN 29073-1:1992-08. 2 It is preferable that the nonwoven laminate has a thickness of 2 to 8 mm.
[0056] If an additional spunbond layer (B) is included, it is preferred that the fibers of the nonwoven layer (B) consist of a copolyester, since then it is easier to melt bond all layers together. The spunbond nonwoven layer (B) can increase the peel strength of layer (A). The spunbond nonwoven layer (B) has a fiber density of 1 to 100 g / m2 according to DIN EN 29073-1:1992-08. 2 , preferably 5 to 50 g / m 2 , more preferably 10 to 20 g / m 2 It is preferable that the laminate has a basis weight of 100% or more. This makes it possible to achieve a good balance between the light weight of the laminate and high abrasion resistance of the laminate.
[0057] In a preferred embodiment, the laminate comprises: - does not include a spunbond nonwoven layer (B), - the copolyester of layers (A), (C) is a copolymer of polyethylene terephthalate, said copolymer having a melting point between 100 and 240°C; and - the needled staple fiber nonwoven layer (C) is composed of 40-60% monocomponent staple fibers (c1) and 40-60% multicomponent staple fibers (c2);
[0058] Such preferred nonwoven laminates can be easily heated and molded to provide desired configurations. Such nonwoven laminates can be dimensionally stable when heated and molded. Such nonwoven laminates are particularly suitable for structural parts, especially structural parts for exterior applications, preferably structural parts for vehicles. The absence of layer (B) can reduce costs and simplify manufacturing.
[0059] In further embodiments - the copolyester of layers (A), (B), (C) is a copolymer of polyethylene terephthalate, said copolymer having a melting point between 100 and 240°C; - the spunbond nonwoven layer (B) is made of copolyester and has a density of 10 to 20 g / m according to DIN EN 29073-1:1992-08 2 and - the needled staple fiber nonwoven layer (C) is composed of 40-60% monocomponent staple fibers (c1) and 40-60% multicomponent staple fibers (c2);
[0060] Such nonwoven laminates can be easily heated and molded to provide a desired configuration. Such nonwoven laminates can be dimensionally stable when heated and molded. Such nonwoven laminates are suitable for structural parts, particularly structural parts for vehicles. The presence of layer (B) can provide high peel strength and heat resistance.
[0061] The subject of the present invention is also a shaped article comprising the nonwoven laminate of the present invention. The shaped article can be obtained by shaping the nonwoven laminate in a mold ("mold"). Typically, shaping is performed under heat and / or pressure. After or during shaping, the nonwoven laminate is bonded. Typically, the density increases and the porosity decreases, while the mechanical stability increases. The shaped article can be shaped into a given form and shape. Generally, the shaped article is rigid and can be cut. Overall, a mechanically stable and relatively lightweight article can be obtained, which is suitable for automotive applications such as underbody shields. Preferably, the shaped article has the shape of a desired automotive part, such as an underbody shield.
[0062] In a preferred embodiment, the shaped article is obtained by cold forming. In the cold forming process, the nonwoven laminate is preheated for 1-5 minutes, preferably at a temperature range of 180°C to 220°C depending on the basis weight. This is aimed at activating the low melting point copolyester, which acts as a binder. The activation of the binder melts it and forms a kind of adhesive between the virgin PET fibers or recycled PET fibers. It also acts as an adhesive between the staple fiber nonwoven layer and the spunbond nonwoven layer. After activation, the nonwoven laminate is placed in a compression mold. The compression mold can then compress all or part of the nonwoven laminate with a tonnage of 50 tons to 200 tons. The nonwoven laminate is allowed to remain in the mold for a maximum of 60 seconds. The compressed nonwoven laminate is allowed to cool in or outside the mold, allowing the staple fibers and the copolyester fibers of the spunbond structure to cool below their melting points. The nonwoven laminate is then transformed into its final shape. For example, the final thickness of the material can be from 2mm to 6mm depending on the requirements of the intended application. The nonwoven laminate is then trimmed as required, which can be accomplished by mechanical cutting, thermal cutting or water jet cutting.
[0063] The molded articles of the present invention benefit from the advantages of the nonwoven laminates described herein, most notably the reduced formation of elephant skin during molding and the associated benefits.
[0064] The molded article and / or nonwoven laminate preferably have at least one of the following characteristics: - Flexural strength ≥ 330MPa according to ISO 178:2019-04; - Tensile strength of ≥ 780N according to ASTM 5034:2009; and / or - Tear strength ≥ 110 N according to DIN EN 29073-3:1992-08.
[0065] A flexural strength of ≧330 MPa, a tensile strength of ≧780 N, and / or a tear strength of ≧110 N can result in high abrasion resistance for the nonwoven laminate. A flexural strength of ≧330 MPa, a tensile strength of ≧780 N, and / or a tear strength of ≧110 N can result in high sound absorption for the nonwoven laminate.
[0066] More preferably, the nonwoven laminate has a bending strength of ≧370 MPa, more preferably ≧400 MPa, and even more preferably ≧430 MPa. More preferably, the nonwoven laminate has a tensile strength of ≧850 N, more preferably ≧900 N, and even more preferably ≧950 N. More preferably, the nonwoven laminate has a tear strength of ≧125 N, more preferably ≧145 N, and even more preferably ≧165 N. The bending strength, tear strength and tensile strength can be adapted by adjusting parameters such as layer thickness, fiber type, amount of binder copolymer and bonding method. This can further improve the mechanical properties of the nonwoven laminate, such as stone chipping resistance and sound absorption.
[0067] The nonwoven laminates and molded articles can be used in the automotive industry, and thus in vehicles, but also in transportation in general, i.e. land, sea or aerospace applications, such as aircraft, ships or railway parts. The nonwoven laminates and molded articles are particularly suitable for structural parts, especially for vehicles, where high stability is required.
[0068] The nonwoven laminate or molded article is particularly suitable for exterior applications, preferably vehicle applications. Preferred exterior applications are particularly those that are subject to high stresses and strains, such as underbody shields, wheel arch liners, engine shields, etc. Exterior applications benefit from the advantages of the nonwoven laminate and / or molded article described herein. Particularly prominent are the mechanical stability, improved stone chipping and abrasion resistance, high heat resistance, non-flammability and sound absorption effects, and the associated benefits. Preferably, in exterior applications, the molded article is positioned such that layer (C) faces the outside. Layer (C) is a surface layer and is therefore exposed to the outside. Thus, the molded article is positioned such that layer (A) faces the inside.
[0069] The subject of the present invention is also a structural part, preferably for a vehicle, preferably for the exterior, which comprises the molded article of the present invention. The exterior part is preferably an underbody shield, a wheel arch liner or an engine shield. The subject of the present invention is also an interior part, preferably for a vehicle, which comprises the molded article of the present invention. The interior part is preferably a panel, a casing, a covering, a reinforcement or a plate. The interior part is preferably for a door, a roof, a trunk or a seat. The subject of the present invention is also a vehicle, which comprises the molded article of the present invention and / or the structural part.
[0070] In further embodiments, the nonwoven laminates and molded articles can be used in interior applications, particularly vehicle interior applications. Preferred interior applications are panels, casings, coverings, reinforcements or boards for doors, roofs, trunks or seats, for example. Interior applications benefit from the advantages of the nonwoven laminates and / or molded articles described herein.
[0071] The nonwoven laminate of the present invention comprises: - producing a needled staple fiber nonwoven layer (C) by needling; - providing layers (A), optionally (B) and (C), in that order; - melt bonding the layers together; The method can be produced by a method comprising the steps of:
[0072] The method of making the nonwoven laminate benefits from the advantages of the nonwoven laminate, most notably the ease of joining of the layers by melt bonding, which can result in improved peel strength and related benefits.
[0073] In a preferred embodiment, layer (c) can be manufactured as outlined below. Prior to the needling step, fibers (c1) and (c2) are opened from a bale, mixed and carded. Then, fibers (c1) and (c2) are cross-lapped and passed through a needling machine. Another fiber preparation method is the air-laid or airlaid method, where the opened fibers are collected on a suction band and needled. The needled nonwoven can be pre-shrunk by applying heat to avoid shrinkage during the subsequent forming step. The staple fibers (c1) and / or (c2) preferably have a staple length in the range of 10 mm to 150 mm, more preferably 40 mm to 100 mm.
[0074] In one embodiment, layer (C) comprises a mixture of 10-70% virgin or recycled PET staple fibers (c1) and 30-90% bicomponent fibers (c2). The bicomponent fibers have a sheath-core structure, where the sheath has a melting point lower than that of the core. The bicomponent fibers preferably have various geometric configurations, such as side-by-side, sheath-core, segmented pie or islands-in-the-sea structures.
[0075] In one embodiment, the binder polymer of the bicomponent fiber (c2) is selected based on its melting point. In a preferred sheath-core configuration, the core is preferably composed of PET and the sheath is preferably composed of a copolyester having a melting point of <200°C. One particularly preferred binder fiber has a sheath-core filament configuration. The core is composed of PET having a melting point of >250°C, i.e. about 260°C, and the sheath comprises a copolyester having a lower melting point in the range of 100°C to 200°C.
[0076] In one embodiment, layer (C) is pre-shrunk to avoid further shrinkage in the subsequent molding step. The pre-shrunk step is performed after the needling step. The needled staple fiber is usually processed through an oven set at a temperature above the melting point of the low melting copolymer. For example, for a bicomponent fiber with a sheath polymer having a melting point of 180°C, the oven temperature setting can be above 180°C.
[0077] In one embodiment, the layer (A) has a thickness of 30 to 150 g / m 2 The nonwoven fabric may be a spunbond nonwoven fabric with a coarse denier of 1000 mm. The spunbond is a PET-based filament with a circular structure that contains a copolyester in an amount of 1-50%. The copolyester melts during the molding process and aids in bonding the adjacent layers. Additionally, the basis weight of layer (A) is significantly lower than the basis weight of layer (C). This may be desirable in situations where it is desired to reduce the overall weight and cost of the final part.
[0078] Layer (B), when included between layers (A) and (C), can be a copolyester-based spunbond nonwoven layer. This copolyester-based spunbond nonwoven layer is used to enhance the bond between layers (A) and (C), i.e., functions as an adhesive layer. Adhesive layer (B) comprises a low melting point copolyester. Its weight is preferably less than 1 g / m 2 ~50g / m 2 In this embodiment, layer (C) may be pre-shrunk to avoid shrinkage during the subsequent molding step.
[0079] The copolyester in all layers melts during molding to promote bonding with adjacent layers. As a result, the fibers of the nonwoven laminate, especially the fibers containing the copolyester, may lose their fibrous structure partially or completely in the laminate after melt bonding. The resulting structure is included in the nonwoven laminate of the present invention. When the adhesive layer (B) is not present, the amount of copolyester in layer (A) is usually increased.
[0080] The entire laminate is formed by establishing a melt bond, rather than a mechanical bond, between all layers. The laminate is then ready to be formed into the desired shape for a particular application. The laminate structure is formed by either a cold or hot forming process.
[0081] Preferably, the multicomponent fiber is a bicomponent fiber. A pie-segment type filament structure is particularly useful for the multicomponent filament. The multicomponent filament is a multicomponent staple fiber (c2) and may be present in the spunbond nonwoven layer (A) and / or (B). Preferably, the multicomponent filament has 8 segments alternating from PET segments and copolyester segments. Alternatively, the multicomponent filament may have a filament structure including 16, 32 or 64 segments alternating from PET segments and copolyester segments. During the molding process, the low melting point copolyester melts and provides stiffness to the material.
[0082] A sheath-core filament structure may be useful for the spunbond nonwoven layers (A) and / or (B) and the multicomponent staple fibers (c2). The bicomponent filament structure may consist of a sheath of a low melting point copolymer and a core of PET, which has a higher melting point. During the molding process, the low melting point copolyester melts and provides stiffness to the material.
[0083] A side-by-side filament structure may be useful for the spunbond nonwoven layers (A) and / or (B) and the multicomponent staple fibers (c2). A side-by-side filament structure is one side made of a low melting point copolymer and the other side made of PET with a higher melting point. During the molding process, the low melting point copolyester melts and provides stiffness to the material.
[0084] Preferably, the monocomponent fibers of the nonwoven laminate, particularly the monocomponent staple fibers of layer (C), are conventional fibers, preferably having a round or substantially round cross section. Such fiber morphology can be obtained by spinning fibers from simple circular or elliptical orifices. Preferably, the nonwoven laminate does not contain monocomponent fibers having unusual shapes such as hollow fibers. It has been found that advantageous properties can be obtained with standard fibers, which has cost and manufacturing advantages.
[0085] The molded articles and nonwoven laminates solve the problem underlying the present invention. The products have high mechanical stability and good acoustic properties, recyclability, light weight and low thermal shrinkage, and show reduced elephant skin effect. Furthermore, the materials have high stone chipping resistance. The nonwoven composites and molded articles are therefore highly suitable for structural parts and / or exterior applications, especially for vehicle applications such as underbody shields, wheel arch liners, engine shields, etc. The materials are available at low cost and can be manufactured and molded in a convenient and easy manner.
[0086] Working Example Example 1 - Preparation of a two-ply nonwoven laminate The following materials were used in making the nonwoven laminate: Staple Fiber (For layer (C)): 50% Monocomponent Staple Fiber (C1): Material: r-PET Staple length: 64mm Fineness: 6.7dtex Weight: 800~1000g / m 2 50% Bicomponent Staple Fiber (C2): Composition: core-sheath type Material: Sheath: PET, Core: Copolyester with melting point of 180℃ Staple length: 51mm Fineness: 5dtex.
[0087] Spunbond (For layer (A)): Material: 90% PET; 10% PET Copolyester (CoPET) Weight: 50g / m 2 Thickness: 0.33~0.59mm Filament diameter: 25~60μm.
[0088] The staple fibres were mixed in a 50:50 weight ratio. The staple fibres were then carded, cross-wrapped and needled. The needles used were Groz-Beckert 36gg fine needles with a total needling strength of 350 needles / cm. 2 The needling depth was set at 10 mm on both sides. The needled material was then passed through a ventilated oven which was heated to 200° C. at a rate of 10° C. / min. Heating the needled material activated the bicomponent fibres. This resulted in a stiff material emerging from the oven. This produced layer (C). This layer (C) was then passed through a set of calendar rolls into which layer (A) was introduced. At a temperature of 200° C., the calendar pressure was set at 25 bar on both sides, which produced a nonwoven laminate in which layers (A) and (C) were melt-bonded to each other. The layers were not mechanically bonded to each other. The two-layer laminate produced was then sheet cut.
[0089] Example 2 - Production of molded articles The sheet cut material of Example 1 was introduced into an oven heated to 210°C for 3 minutes (for ventilated ovens) or 1 minute (for infrared ovens). The heat softened the material. The material was then immediately transferred to a cold press where it was molded under high pressure (50 tons or more). The nonwoven laminate was allowed to remain in the mold for up to 60 seconds. The compressed nonwoven laminate was allowed to cool in or out of the mold so that the staple fibers and the copolyester fibers of the spunbond structure were cooled below their melting points. The nonwoven laminate was then converted into its final shape.
[0090] Example 3 - Acoustic properties The acoustic properties of a sample of the molded article of Example 2 were tested. The test sample was placed on the wall or bottom of the Alpha Cabin with a 2 mm air gap. The absorption coefficient of the sample was then measured by a series of sensors inside the cabin. The results of the Alpha Cabin test for a sample with a molded thickness of 5 mm are shown in Table 1 below.
[0091] [Table 1]
[0092] Sound absorption coefficient α s The higher the value, the better the acoustic performance of the test sample. The results indicate that the molded article obtained from the two-ply nonwoven laminate has high sound absorption. The wavelength range tested is particularly relevant for automotive underbody shielding, where the interior of the vehicle needs to be insulated from underbody noise.
[0093] Furthermore, the comparative examples showed that the sound absorption efficiency of molded articles according to EP 3769954 obtained from a corresponding three-layer nonwoven laminate having an additional spunbond layer on the opposite surface of layer (C) was approximately the same.
[0094] Example 4 – Mechanical properties The flexural strength of the molded article obtained from the two-layer nonwoven laminate was measured, and for comparison, also that of the molded article according to EP 3769954 obtained from the corresponding three-layer nonwoven laminate (see Example 3).
[0095] The pressure required to bend the material 2 mm was measured under the following test conditions: Starting pressure: 0.5N Speed: 10mm / min Distance between sample holders: 64mm Press element radius: 5mm.
[0096] [Table 2]
[0097] As can be seen from Table 2, the molded articles obtained from the two-ply nonwoven laminate have high flexural strength. The flexural strength of the molded articles obtained from the two-ply laminate meets the requirements for underbody shields in automotive applications. The flexural strength is only slightly lower than that of the comparative three-ply laminate.
[0098] Example 5 - Stone chipping resistance The stone chipping resistance of the moulded articles obtained from the two-ply laminate and the comparative three-ply laminate described in the previous examples was investigated in a test according to DIN EN ISO 20567-1:2017. This standard is provided for the testing of paints and varnishes, but is also applicable for the testing of moulded articles. This test is therefore applied in the automotive sector as an OEM standard to simulate stone chipping on the surface of car parts such as underbody shields. In this test method, a defined amount of abrasive grains of defined dimensions are sprayed on the probe surface under specific harsh conditions. The performance is evaluated with standardised comparative images. Before each test of chipping, a new chipping material is used and its amount is determined. The test is carried out in 1 kg steps from 0 kg to 8 kg, 0 kg being the initial position. According to the OEM standard, if the surface fringing is less than 4 mm after the entire series of 0 kg to 8 kg of abrasive grains is directed on the surface, the material passes the test. Fringing is the appearance of loose threads protruding from the surface of the test specimen. Nine specimens were tested in this analysis. The tests were carried out using a stone chip tester (VDA, model 508, manufactured by Erichsen) under the following conditions: - Pressure: 2.0 bar (200kPa) - Angle: 30° - Material: High-quality gravel, grain size 5~8mm - Material amount: 1~8kg - Test piece size: 100mm x 100mm - Test field: 80mm x 80mm - Test time: 10 seconds per 500g.
[0099] The molded article of the invention, obtained from a two-layer laminate, was positioned so that stone chipping occurred on the surface corresponding to layer (C). The comparative molded article, obtained from a three-layer laminate, contained two identical surfaces of the spunbond nonwoven layer.
[0100] The comparative molded article failed the test. No holes were observed in the specimens, but fringing was in the range of 4-8 mm and therefore excessively high. Visual inspection after stone chipping showed a significant amount of fibers and fiber bundles protruding from the surface of the specimen. Thus, the fibrous surface disintegrated upon stone chipping.
[0101] In the molded articles obtained from the two-layer material, no holes were observed in the material after stone chipping. Furthermore, the level of fringing was low and clearly below the standard value of 4 mm. Thus, the material of the present invention passed the standardized stone chipping test. On visual inspection, the surface was relatively flat with no fibers or fiber bundles protruding from the surface.
[0102] The results show that the two-ply material has significantly better resistance to the stone chipping test than the comparative three-ply material.The material of the present invention is suitable for exterior applications such as automotive underbody shields, wheel arch liners, engine shields, etc.
Claims
1. A nonwoven laminate, comprising: (A) to (C): a spunbond nonwoven layer (A) comprising fibers comprising polyethylene terephthalate (PET) and a copolyester; an optional spunbond nonwoven layer (B) comprising fibers comprising polyethylene terephthalate (PET) and a copolyester, said nonwoven layer (B) having a higher copolyester content than said nonwoven layer (A); a needled staple fiber nonwoven layer (C) comprising: monocomponent polyethylene terephthalate (PET) staple fibers (c1), and Multicomponent staple fibers (c2), comprising at least a polyethylene terephthalate (PET) component and a copolyester component. A nonwoven layer (C) comprising: It is structured in the order of A nonwoven laminate wherein all layers are melt bonded to one another.
2. 10. The nonwoven laminate of claim 1, wherein layers (A), (B), and (C) are not mechanically bonded to one another.
3. 3. The nonwoven laminate of claim 1 or 2, wherein the needled staple fiber nonwoven layer (C) is heat-shrunk.
4. 4. The nonwoven laminate of any one of claims 1 to 3, which is free of polyolefins, in particular polypropylene.
5. 5. The nonwoven laminate of any one of claims 1 to 4, wherein the copolyester of all layers is a copolymer of polyethylene terephthalate, said copolymer having a melting point of ≦240°C measured according to DIN ISO 11357-3:2013.
6. 6. The nonwoven laminate according to any one of claims 1 to 5, wherein layer (A) comprises 10% to 70% copolyester, in particular at least 30% copolyester.
7. 7. The nonwoven laminate of claim 1, wherein the needled staple fiber nonwoven layer (C) is composed of 10 to 90% monocomponent staple fibers (c1) and 10 to 90% multicomponent staple fibers (c2).
8. The needled staple fiber nonwoven layer (C) has a fiber density of 600 to 1500 g / m2 measured in accordance with DIN EN 29073-1:1992-08. 2 and / or the spunbond nonwoven layer (A) has a basis weight of 20 to 200 g / m as measured in accordance with DIN EN 29073-1:1992-08. 2 The nonwoven laminate of any one of claims 1 to 7, having a basis weight of
9. - said nonwoven laminate is composed of layers (A) and (C), - the copolyester of the layers (A) and (C) is a copolymer of polyethylene terephthalate, the copolymer having a melting point between 100 and 240°C; and - nonwoven laminate according to any one of claims 1 to 8, characterized in that the needled staple fiber nonwoven layer (C) is composed of 40 to 60% monocomponent staple fibers (c1) and 40 to 60% multicomponent staple fibers (c2).
10. A shaped article comprising the nonwoven laminate of any one of claims 1 to 9.
11. 11. A shaped article according to claim 10, obtained by cold-forming or hot-forming the nonwoven laminate of any one of claims 1 to 9.
12. A structural part for a vehicle comprising a molded article according to claim 10 or 11, said structural part being preferably an underbody shield, a wheel arch liner or an engine shield.
13. A vehicle comprising a shaped article and / or a structural part according to any one of claims 10 to 12.
14. 12. Use of a molded article according to claim 10 or 11 as a structural part for a vehicle, said structural part being preferably an underbody shield, a wheel arch liner or an engine shield.
15. 15. The use according to claim 14, wherein the molded article is positioned so that layer (C) is exposed to the outside.
Citation Information
Patent Citations
Nonwoven fabric for sand-protecting sheet and method for producing the same
JP2002013060A
Sound absorbing material
JP2011110773A
moldable composite mat
JP2018518382A
Nonwoven fabric laminate
JP2021037745A
Joint material and manufacturing method thereof
JP2021110148A