Resin laminated optical body, light source unit, optical unit, light irradiation device, image display device, method of manufacturing resin laminated optical body, and method of manufacturing light source unit

By integrating a resin layer with fine uneven structures onto optical elements, the size of optical devices is reduced, and light emission quality is enhanced through reduced reflections and improved transmittance.

JP2024159937AInactive Publication Date: 2024-11-08DEXERIALS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024147633
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing optical devices face challenges in miniaturization due to separate components like light diffusing plates and light sources, leading to increased size and decreased light transmittance and quality due to interfacial reflections and ghosting effects.

Method used

Integration of a resin layer with a fine uneven structure, such as a moth-eye or light diffusion structure, onto optical elements to reduce interfacial reflections and enhance light transmission and diffusion.

Benefits of technology

The integration of a resin layer with fine uneven structures reduces device size and improves light emission quality by minimizing reflections and enhancing transmittance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159937000001_ABST
    Figure 2024159937000001_ABST
Patent Text Reader

Abstract

To provide a novel and improved resin laminated optical body which allows for miniaturizing optical devices and improving light emission quality, and to provide a light source unit, an optical unit, a light irradiation device, an image display device, and a method of manufacturing the resin laminated optical body.SOLUTION: A resin laminated optical body comprises, according to an aspect of the present invention, an optical base material having a curved surface, and a resin layer formed on the curved surface of the optical base material, the resin layer having a light diffusion structure formed on a surface thereof.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin laminated optical body, a light source unit, an optical unit, a light irradiation device, an image display device, a method for manufacturing a resin laminated optical body, and a method for manufacturing a light source unit. [Background technology]

[0002] In recent years, optical devices (such as various image projection devices and imaging devices) incorporating many optical elements have been developed and spread. There is a strong demand for these optical devices to be small and lightweight from the viewpoint of attachment to the human body and incorporation into various devices or infrastructure such as vehicles. In order to meet such demands, techniques for combining multiple optical elements have been proposed, as disclosed in Patent Documents 1 and 2, for example. Specifically, in Patent Documents 1 and 2, an anti-reflection structure is combined with the surface of an optical lens. According to Patent Documents 1 and 2, it is possible to impart anti-reflection properties to an optical lens. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-256015 A [Patent Document 2] JP 2001-300944 A [Patent Document 3] JP 2017-174542 A Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, as disclosed in Patent Document 3, for example, image projection devices are often provided with a light diffusion plate (defined as a light diffusion sheet in Patent Document 3) from the viewpoint of displaying an image evenly. However, the light diffusion plate is separate from the optical lens. For this reason, a large space is required inside the image projection device to accommodate the light diffusion plate and the optical lens, which makes the image projection device large. Furthermore, when the optical lens and the light diffusion plate are separate, interfacial reflection occurs on the surface of the optical lens or the surface of the light diffusion plate, which may result in a decrease in light transmittance and a decrease in light emission quality such as the occurrence of ghosts due to stray light inside the housing.

[0005] Furthermore, a light source unit in which a light source such as an LED (light emitting diode) or a laser is built into an optical lens may be used as the light source for the image projection device. However, the light source unit and other optical elements are separate. This makes the image projection device large. Furthermore, interfacial reflection may occur on the surface of the light source unit or the surfaces of other optical elements, resulting in a decrease in light transmittance, a decrease in the quality of light emission such as the occurrence of ghosts, etc.

[0006] The above-mentioned light diffusion plate and light source unit may be used in other types of optical devices, and these optical devices may also have problems such as increased size and reduced light emission quality. Thus, there is room for further improvement in optical devices from the viewpoints of miniaturization and improvement of light emission quality.

[0007] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide new and improved resin laminated optical bodies, light source units, optical units, light irradiation devices, image display devices, methods for manufacturing resin laminated optical bodies, and methods for manufacturing light source units, which enable optical equipment to be miniaturized and light emission quality to be improved. [Means for solving the problem]

[0008] In order to solve the above problems, according to one aspect of the present invention, there is provided a resin laminated optical body comprising an optical substrate having a curved surface, and a resin layer provided on the curved surface of the optical substrate, characterized in that a light diffusion structure is formed on the surface of the resin layer.

[0009] Here, the light diffusion structure may include a fine concave-convex structure, and the average distance between the fine concave portions or the average distance between the fine convex portions constituting the fine concave-convex structure may be 1 to 150 μm.

[0010] The difference in height between adjacent fine recesses and fine protrusions may be 0.5 to 50 μm.

[0011] According to another aspect of the present invention, there is provided a light source unit comprising a light source, an optical substrate incorporating the light source, and a resin layer provided on the light-emitting surface of the optical substrate, characterized in that a fine uneven structure is formed on the surface of the resin layer.

[0012] Here, the fine uneven structure may be one or more of a moth-eye structure, a light diffusion structure, a microlens array structure, and a diffraction grating structure.

[0013] The fine unevenness may include a moth-eye structure, and the average interval between the fine recesses or the average interval between the fine protrusions constituting the fine unevenness may be 50 nm to 400 nm, and the height difference between adjacent fine recesses and fine protrusions may be 100 to 500 nm.

[0014] According to another aspect of the present invention, there is provided an optical unit comprising the above-mentioned resin laminated optical body and at least one of the above-mentioned light source units.

[0015] According to another aspect of the present invention, there is provided a light irradiation device comprising the above-mentioned optical unit.

[0016] According to another aspect of the present invention, there is provided an image display device comprising the above-mentioned light irradiation device.

[0017] According to another aspect of the present invention, there is provided a method for manufacturing a resin laminated optical body, comprising: a first step of preparing an optical substrate having a curved surface; a second step of forming an uncured resin layer on the curved surface of the optical substrate; a third step of preparing a flexible master having an inverted structure of a light diffusion structure formed on its surface and having flexibility; a fourth step of bringing the flexible master close to the uncured resin layer; a fifth step of applying a printing pressure to the flexible master to press the inverted structure of the flexible master against the uncured resin layer while deforming the flexible master; and a sixth step of curing the uncured resin layer while pressing the inverted structure of the flexible master against the uncured resin layer, thereby forming a resin layer on the curved surface of the optical substrate.

[0018] Here, the light diffusion structure may include a fine concave-convex structure, and the average distance between the fine concave portions or the average distance between the fine convex portions constituting the fine concave-convex structure may be 1 to 150 μm.

[0019] The difference in height between adjacent fine recesses and fine protrusions may be 0.5 to 50 μm.

[0020] According to another aspect of the present invention, there is provided a method for manufacturing a light source unit, comprising: a first step of preparing an optical substrate having a curved surface and a built-in light source; a second step of forming an uncured resin layer on the curved surface of the optical substrate; a third step of preparing a flexible master having an inverted structure of a fine unevenness structure formed on its surface and having flexibility; a fourth step of bringing the flexible master close to the uncured resin layer; a fifth step of applying a printing pressure to the flexible master to press the inverted structure of the flexible master against the uncured resin layer while deforming the flexible master; and a sixth step of curing the uncured resin layer while pressing the inverted structure of the flexible master against the uncured resin layer, thereby forming a resin layer on the curved surface of the optical substrate.

[0021] According to another aspect of the present invention, there is provided a method for manufacturing a light source unit, comprising: a first step of preparing an optical substrate having a curved surface; a second step of forming an uncured resin layer on the curved surface of the optical substrate; a third step of preparing a flexible master having an inverted structure of a fine unevenness structure formed on its surface and having flexibility; a fourth step of bringing the flexible master close to the uncured resin layer; a fifth step of applying a printing pressure to the flexible master to press the inverted structure of the flexible master against the uncured resin layer while deforming the flexible master; a sixth step of curing the uncured resin layer while pressing the inverted structure of the flexible master against the uncured resin layer, thereby forming a resin layer on the curved surface of the optical substrate; and a seventh step of placing the optical substrate on which the resin layer has been formed on a light source.

[0022] Here, the fine uneven structure may be one or more of a moth-eye structure, a light diffusion structure, a microlens array structure, and a diffraction grating structure.

[0023] The fine unevenness may include a moth-eye structure, and the average interval between the fine recesses or the average interval between the fine protrusions constituting the fine unevenness may be 50 nm to 400 nm.The height difference between adjacent fine recesses and fine protrusions may be 100 to 500 nm. Effect of the Invention

[0024] As described above, according to the present invention, it is possible to reduce the size of an optical device and improve the light emission quality. [Brief description of the drawings]

[0025] [Figure 1] 1 is a cross-sectional view illustrating an example of a resin laminate optical body according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a fine concavo-convex structure formed on a surface of the resin laminated optical body according to the embodiment. [Diagram 3] FIG. 4 is a cross-sectional view showing another example of a resin laminated optical body. [Figure 4] FIG. 4 is a cross-sectional view showing another example of a resin laminated optical body. [Diagram 5] FIG. 4 is a cross-sectional view showing another example of a resin laminated optical body. [Figure 6] FIG. 4 is a cross-sectional view showing another example of a resin laminated optical body. [Figure 7] FIG. 4 is a cross-sectional view showing another example of a resin laminated optical body. [Figure 8] FIG. 4 is a cross-sectional view showing another example of a resin laminated optical body. [Figure 9] FIG. 2 is a cross-sectional view showing an example of a light source unit according to the embodiment of the present invention. [Figure 10] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 11] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 12] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 13] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 14] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 15] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 16] 5A to 5C are cross-sectional views illustrating a method for manufacturing a resin laminated optical body. [Figure 17] FIG. 2 is a perspective view showing an example of the appearance of a master according to the present embodiment. [Figure 18] FIG. 2 is a block diagram showing an example of the configuration of an exposure apparatus. [Figure 19] FIG. 1 is a schematic diagram showing an example of a transfer apparatus for producing a flexible master by roll-to-roll. [Figure 20] 1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. [Figure 21] 1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. [Figure 22] 1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. [Diagram 23]1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. [Figure 24] 1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. [Diagram 25] 1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. [Figure 26] 1A to 1C are explanatory diagrams showing application examples of the resin laminated optical body and the light source unit according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.

[0027] <1. Structure of the resin laminated optical body> First, the configuration of the resin laminated optical body 1 according to the present embodiment will be described with reference to Figs. 1 and 2. As shown in Fig. 1, the resin laminated optical body 1 includes an optical substrate 10 and a resin layer 20. The optical substrate 10 is a convex lens and has a convex curved surface 11. In the example of Fig. 1, the optical substrate 10 is a plano-convex lens (a convex lens with one flat surface), but may be a biconvex lens (a convex lens with both convex surfaces). The optical substrate 10 may be another type of lens, such as a concave lens or a Fresnel lens. The shape of the optical substrate 10 is not limited to the above, and may be, for example, an aspheric shape, a round shape, a square shape, an asymmetric shape, or the like. The optical substrate 10 may be a mirror.

[0028] The material of the optical substrate 10 is not particularly limited, and may be any material used for optical lenses or optical mirrors. Examples of materials for the optical substrate 10 include polycarbonate, acrylate, cycloolefin polymer, cycloolefin copolymer, polypropylene, glass, and the like. The material for the optical substrate 10 may be appropriately selected depending on the application of the resin laminated optical body 1, etc. When the optical substrate 10 is used as an optical mirror, the curved surface 11 may be subjected to mirror finishing (for example, deposition of a metal film or a dielectric material, etc.).

[0029] The curved surface 11 may be subjected to various pretreatments (treatments before laminating the resin layer 20 on the curved surface 11) in order to improve adhesion with the resin layer 20. Examples of such pretreatments include corona treatment, excimer treatment, UV ozone treatment, heat treatment, flame treatment (treatment of applying a flame to the curved surface 11), solvent washing, primer coating treatment, and the like.

[0030] The resin layer 20 is provided on the curved surface 11 of the optical substrate 10. As shown in FIG. 2, a fine uneven structure 50 is formed on the surface 21 of the resin layer 20. The fine uneven structure 50 is composed of a large number of fine convex portions 50a and fine concave portions 50b. The resin layer 20 is given optical properties derived from the fine uneven structure 50. By changing the shape of the fine uneven structure 50, various optical properties can be given to the resin layer 20. In particular, in this embodiment, the fine uneven structure 50 is a light diffusion structure. Specifically, the shape of the fine convex portions 50a or the fine concave portions 50b is adjusted so that the light that has passed through the optical substrate 10 and reached the fine uneven structure 50 is diffused and radiated to the outside. Therefore, the resin layer 20 is given light diffusion properties.

[0031] The average interval between the fine recesses 50b or the fine protrusions 50a is preferably 1 to 150 μm. Furthermore, the height difference between the adjacent fine recesses 50b and fine protrusions 50a is preferably 0.5 to 50 μm. When at least one of these conditions (preferably both) is satisfied, the light diffusion properties are further improved.

[0032] Here, the shape of the fine concave-convex structure 50 is observed using, for example, a scanning electron microscope (SEM) or an atomic force microscope (AFM). Then, based on the observation results, the above-mentioned average interval or height difference is measured. For example, the average interval between the fine concaves 50b is measured by the following method. That is, a cross section (a cross section passing through the optical axis and parallel to the optical axis) of the resin laminated optical body 1 at the center is observed. Then, the distance between the center points (center points of the bottom surfaces) of adjacent fine concaves 50b is measured. Then, several distances between the center points are measured, and the arithmetic average value of these is taken as the average interval between the fine concaves 50b. The average interval between the fine convex portions 50a is also measured by the same method. That is, the distance between the vertices (center points of the upper ends) of adjacent fine convex portions 50a is measured. Then, several distances between the vertices are measured, and the arithmetic average value of these is taken as the average interval between the fine convex portions 50a. The height difference between the adjacent minute recess 50b and minute protrusion 50a is the distance between the center point of the bottom surface of the minute recess 50b and the apex of the minute protrusion 50a (the distance in the thickness direction of the resin layer 20).

[0033] The thickness of the resin layer 20 is not particularly limited, but is preferably, for example, 200 μm or less. If the resin layer 20 is too thick, film stress accumulates due to the curing shrinkage of the resin during light (UV) curing, and there is a possibility that poor adhesion occurs between the optical substrate 10 and the resin layer 20.

[0034] Here, as described above, the surface 21 of the resin layer 20 is not flat because the fine uneven structure 50 is formed on the surface 21. Therefore, the thickness of the resin layer 20 is measured, for example, by the following method. That is, using various three-dimensional measuring devices (for example, a three-dimensional measuring device UA3P manufactured by Panasonic), a cross section (a cross section passing through the optical axis and parallel to the optical axis) at the center of the resin laminated optical body 1 is observed. Then, the curve of the obtained surface 21 is spherically fitted by the least squares method. A cross section (a cross section passing through the optical axis and parallel to the optical axis) at the center of the optical substrate 10 (i.e., before processing) is observed, and the region of the resin layer 20 is identified by comparing the obtained image with the cross section at the center of the resin laminated optical body 1. Then, the distance from the curve of the surface 21 obtained by the above-mentioned spherical fitting to the curve of the curved surface 11 is taken as the thickness of the resin layer 20. In the examples described later, the thickness of the resin layer 20 was measured by this method. The thickness was taken as the arithmetic average value of values ​​measured at several measurement points. For the measurements, a Panasonic three-dimensional measuring device UA3P was used.

[0035] In this manner, in this embodiment, the resin layer 20 having light diffusion properties and the optical substrate 10 are integrated. Therefore, by applying the resin laminated optical body 1 to an optical device, the optical device can be made smaller. Furthermore, compared to a case where the substrate having light diffusion properties and the untreated optical substrate 10 are arranged as separate components, in this embodiment, the components are integrated to reduce the number of interfaces that may cause reflection, improving the light transmittance and suppressing the occurrence of ghosts. That is, the light emission quality is improved.

[0036] Here, a light diffusion property may be imparted to a part of the surface 21 of the resin layer 20, and a different optical property may be imparted to the other part. That is, the type of the fine uneven structure 50 may be different for each region of the surface 21. Examples of the fine uneven structure 50 other than the light diffusion structure include a moth-eye structure, a light diffusion structure, a microlens array structure, and a diffraction grating structure. That is, the surface 21 of the resin layer 20 may contain one or more of these structures in addition to the light diffusion structure.

[0037] When the fine uneven structure 50 has a moth-eye structure, the fine convex portions 50a or the fine concave portions 50b are arranged on the surface 21 at an average period (the average period here is synonymous with the above-mentioned average interval) equal to or less than the visible light wavelength. This suppresses reflection of external light on the surface 21. Furthermore, the average interval between the fine concave portions or the average interval between the fine convex portions constituting the fine uneven structure is preferably 50 nm to 400 nm, and the height difference between the adjacent fine concave portions 50b and fine convex portions 50a is preferably 100 to 500 nm. In this case, reflection of external light is more effectively suppressed. Therefore, when the fine uneven structure 50 has a moth-eye structure, the resin layer 20 is provided with anti-reflection properties.

[0038] When the fine uneven structure 50 is a microlens array structure, the fine convex portion 50a or the fine concave portion 50b is a microlens on the order of microns. When the fine uneven structure 50 is a diffraction grating structure, the fine convex portion 50a or the fine concave portion 50b has a diffraction grating shape. The fine uneven structure 50 other than the light diffusion structure is not limited to the above example. In addition, fine uneven structures 50 adjusted to have different optical characteristics even with the same type of pattern may be mixed or arranged on the surface 21 of the resin layer 20. For example, the fine uneven structure 50 may be designed so that the light diffusion characteristics are different between some regions and other regions among the regions where the light diffusion structure is formed. In this case, the above-mentioned average interval or height difference may be changed for each region.

[0039] The resin layer 20 is composed of a cured product of a curable resin. The cured product of the curable resin is preferably transparent. The curable resin includes a polymerizable compound and a curing initiator. The polymerizable compound is a resin that is cured by a curing initiator. Examples of the polymerizable compound include an epoxy polymerizable compound and an acrylic polymerizable compound. The epoxy polymerizable compound is a monomer, oligomer, or prepolymer having one or more epoxy groups in the molecule. Examples of the epoxy polymerizable compound include various bisphenol type epoxy resins (bisphenol A type, F type, etc.), novolac type epoxy resins, various modified epoxy resins such as rubber and urethane, naphthalene type epoxy resins, biphenyl type epoxy resins, phenol novolac type epoxy resins, stilbene type epoxy resins, triphenol methane type epoxy resins, dicyclopentadiene type epoxy resins, triphenyl methane type epoxy resins, and prepolymers thereof.

[0040] The acrylic polymerizable compound is a monomer, oligomer, or prepolymer having one or more acrylic groups in the molecule. Here, the monomer is further classified into a monofunctional monomer having one acrylic group in the molecule, a bifunctional monomer having two acrylic groups in the molecule, and a polyfunctional monomer having three or more acrylic groups in the molecule.

[0041] Examples of "monofunctional monomers" include carboxylic acids (acrylic acid, etc.), hydroxyls (2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate), alkyl or alicyclic monomers (isobutyl acrylate, t-butyl acrylate, isooctyl acrylate, lauryl acrylate, stearyl acrylate, isobornyl acrylate, cyclohexyl acrylate), and other functional monomers (2-methoxyethyl acrylate, methoxyethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, benzyl acrylate, ethyl carbitol acrylate, phenoxyethyl acrylate, and N,N-dimethylaminoethyl acrylate). , N,N-dimethylaminopropylacrylamide, N,N-dimethylacrylamide, acryloylmorpholine, N-isopropylacrylamide, N,N-diethylacrylamide, N-vinylpyrrolidone, 2-(perfluorooctyl)ethyl acrylate, 3-perfluorohexyl-2-hydroxypropyl acrylate, 3-perfluorooctyl-2-hydroxypropyl acrylate, 2-(perfluorodecyl)ethyl acrylate, 2-(perfluoro-3-methylbutyl)ethyl acrylate), 2,4,6-tribromophenol acrylate, 2,4,6-tribromophenol methacrylate, 2-(2,4,6-tribromophenoxy)ethyl acrylate), 2-ethylhexyl acrylate, and the like.

[0042] Examples of the "bifunctional monomer" include tri(propylene glycol) diacrylate, trimethylolpropane diallyl ether, and urethane acrylate.

[0043] Examples of the "polyfunctional monomer" include trimethylolpropane triacrylate, dipentaerythritol penta- and hexaacrylate, and ditrimethylolpropane tetraacrylate.

[0044] Examples of the acrylic polymerizable compounds other than those listed above include acrylic morpholine, glycerol acrylate, polyether acrylate, N-vinyl formamide, N-vinyl caprolactone, ethoxydiethylene glycol acrylate, methoxytriethylene glycol acrylate, polyethylene glycol acrylate, EO-modified trimethylolpropane triacrylate, EO-modified bisphenol A diacrylate, aliphatic urethane oligomer, and polyester oligomer.

[0045] By adjusting the type and compounding ratio of the constituent units of the curable resin, that is, the monomer, oligomer, or prepolymer, the properties of the resin layer 20, such as the refractive index and viscosity, can be adjusted.

[0046] The curing initiator is a material that cures the curable resin. Examples of the curing initiator include a heat curing initiator and a photocuring initiator. The curing initiator may be one that cures by some energy ray other than heat or light (e.g., an electron beam), etc. When the curing initiator is a heat curing initiator, the curable resin becomes a heat curable resin, and when the curing initiator is a photocuring initiator, the curable resin becomes a photocurable resin.

[0047] Here, from the viewpoint of the processability of the resin layer 20, the curing initiator is preferably an ultraviolet curing initiator. The ultraviolet curing initiator is a type of photocuring initiator. Examples of the ultraviolet curing initiator include 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl phenyl ketone, and 2-hydroxy-2-methyl-1-phenylpropane-1-one. Therefore, the curable resin is preferably an ultraviolet curable resin. From the viewpoint of transparency, the curable resin is more preferably an ultraviolet curable acrylic resin. The above curable resin can be appropriately selected and adjusted according to the optical characteristics of the material constituting the optical substrate 10 and the optical design of the device.

[0048] <2. Various Modifications of the Resin Laminated Optical Body> Next, various modified examples of the resin laminated optical body 1 will be described with reference to Fig. 3 to Fig. 8. In the modified example shown in Fig. 3, the optical substrate 10 is a plano-concave lens (a concave lens having a flat surface on one side). The resin layer 20 is formed on the curved surface 11 of the optical substrate 10. The resin layer 20 has the above-mentioned fine concave-convex structure 50 formed therein.

[0049] In the modified example shown in FIG. 4, a resin layer 20 is formed on both the front and back surfaces of the optical substrate 10 shown in FIG. 1. The above-mentioned fine uneven structure 50 is formed in each resin layer 20. The types of these fine uneven structures 50 may be the same or different. For example, the fine uneven structures 50 on both the front and back surfaces may be light diffusion structures. The fine uneven structure 50 on the front surface (curved surface 11 in this case) may be a light diffusion structure, and the fine uneven structure 50 on the back surface may be a moth-eye structure. Conversely, the fine uneven structure 50 on the front surface side may be a moth-eye structure, and the fine uneven structure 50 on the back surface side may be a moth-eye structure. In other words, the fine uneven structure 50 formed in the resin laminated optical body 1 may include a light diffusion structure. The same applies to each of the following modified examples.

[0050] In the modified example shown in Fig. 5, resin layers 20 are formed on both the front and back sides of the optical substrate 10 shown in Fig. 3. The above-mentioned fine uneven structure 50 is formed in each resin layer 20. The types of the fine uneven structures 50 may be the same or different.

[0051] 6, the optical substrate 10 is a biconvex lens (a lens having convex surfaces on both sides), and resin layers 20 are formed on both sides. The above-mentioned fine concave-convex structures 50 are formed in each resin layer 20. The types of the fine concave-convex structures 50 may be the same or different.

[0052] 7, the optical substrate 10 is a biconcave lens (a lens having concave surfaces on both sides), and resin layers 20 are formed on both sides. The above-mentioned fine concave-convex structures 50 are formed in each resin layer 20. The types of the fine concave-convex structures 50 may be the same or different.

[0053] 8, the optical substrate 10 has a convex front surface and a concave rear surface, and further has resin layers 20 formed on both the front and rear surfaces of the optical substrate 10. The above-mentioned fine uneven structure 50 is formed in each resin layer 20. The types of the fine uneven structures 50 may be the same or different.

[0054] Of course, the resin laminated optical body 1 according to this embodiment is not limited to the example in Fig. 1 and the above-mentioned modified examples. For example, in Figs. 4 to 8, the resin layer 20 on the front side or back side may be omitted.

[0055] <3. Light source unit configuration> Next, the configuration of the light source unit 30 according to this embodiment will be described with reference to Fig. 2 and Fig. 9. As shown in Fig. 9, the light source unit 30 includes a light source 31, an optical base material 32, and a resin layer 40. The light source 31 is a member that emits light. There is no particular limit to the type of light source 31, and it may be, for example, a light-emitting diode (LED) or a laser. Although three light sources 31 are depicted in Fig. 9, the number of light sources 31 included in the light source unit 30 is appropriately adjusted depending on the application of the light source unit 30, etc.

[0056] Here, the light source 31 is built into the optical substrate 32. The light source 31 may be integrated with the optical substrate 32 or may be separate from the optical substrate 32. The light source unit 30 emits light emitted from the light source 31 to the outside from the interface 32a. A curved surface 33 is formed on the interface 32a, and a resin layer 40 is laminated along the curved surface 33. In the example of FIG. 9, the curved surface 33 is a convex surface, but it may be a concave surface. Therefore, the optical substrate 32 functions as a lens for the light source 31. The curved surface 33 may be omitted. The material of the optical substrate 32 is not particularly limited, and may be the same as that of the optical substrate 10, for example.

[0057] The interface 32a may be subjected to various pretreatments (treatments before laminating the resin layer 20 on the light-emitting surface 32a) in order to improve adhesion with the resin layer 40. Examples of such pretreatments include corona treatment, excimer treatment, UV ozone treatment, heat treatment, flame treatment (treatment of applying a flame to the curved surface 11), solvent washing, primer coating treatment, and the like.

[0058] The resin layer 40 is provided on the interface 32a of the optical substrate 32. A fine uneven structure 50 shown in FIG. 2 is formed on the surface 41 of the resin layer 40. The details of the fine uneven structure 50 are as described above. The resin layer 40 is endowed with optical properties derived from the fine uneven structure 50. By changing the shape of the fine uneven structure 50, it is possible to impart various optical properties to the resin layer 40.

[0059] Here, the resin layer 40 is given any optical characteristic. That is, the fine uneven structure 50 may be, for example, a moth-eye structure, a light diffusion structure, a microlens array structure, or a diffraction grating structure. That is, the optical characteristic of the resin layer 40 is not necessarily limited to the light diffusion characteristic. The surface 41 of the resin layer 40 may have one or more of these structures mixed therein. In addition, the shape of the fine uneven structure 50 may be adjusted so that the optical characteristics are different even for the same type of pattern (for example, a light diffusion structure). The material and thickness constituting the resin layer 40 may be the same as those of the resin layer 20. The thickness of the resin layer 40 is measured by the same method as that of the resin layer 20.

[0060] In this manner, in this embodiment, the light source unit 30 and the resin layer 40 having various optical properties are integrated together. Therefore, by applying the light source unit 30 to an optical device, the optical device can be made smaller. Furthermore, for example, by forming a moth-eye structure on the surface of the light source unit 30, reflection at the interface 32a is suppressed, the light transmittance is improved, and the occurrence of ghosts is suppressed. In other words, the light emission quality is improved.

[0061] <4. Method for producing resin laminated optical body> The resin laminated optical body 1 can be produced by a so-called imprinting method. A method for producing the resin laminated optical body 1 will be described in detail below with reference to Fig. 10 to Fig. 14. In the example of Fig. 10 to Fig. 14, the optical substrate 10 is a biconvex lens.

[0062] (4-1. First step) First, the above-mentioned optical substrate 10 is prepared.

[0063] (4-2. Second step) Next, as shown in FIG. 10, the optical substrate 10 is set on the optical substrate fixing jig 600. Next, an uncured curable resin is applied onto the curved surface 11 (here, one convex surface) of the optical substrate 10 using a coating device 700. As a result, an uncured resin layer 20a is formed on the curved surface 11 of the optical substrate 10. The type of coating device 700 is not particularly limited, and may be, for example, a spin coater, a dispenser, an inkjet device, or the like. The type of coating device 700 may be selected according to the properties of the uncured resin layer 20a, etc. In order to adjust the adhesion of the uncured resin layer 20a to the optical substrate 10, the viscosity of the uncured resin layer 20a, etc., the optical substrate 10 may be heated before or during coating. In addition, the uncured resin layer 20a may be subjected to a heat treatment after coating depending on the type of the uncured resin layer 20a. The coating device 700 may be incorporated into a chamber device 500 described later, or may be separate from the chamber device 500.

[0064] (4-3. Third step) In the third step, a flexible master 400 shown in FIG. 11 is prepared. Here, the flexible master 400 is a flexible film, and an inverted structure of the fine concave-convex structure 50 (hereinafter also referred to as "inverted concave-convex structure 430") is formed on the surface of the flexible master 400. The flexible master 400 is sometimes called a soft mold. The inverted concave-convex structure 430 is shown in FIG. 19. A method for manufacturing the flexible master 400 will be described later. The third step may be performed at least before the fourth step described later.

[0065] (4-4. Fourth step) The fourth process consists of the optical substrate / flexible master setting process and the optical substrate approach process.

[0066] (Optical substrate / flexible master setting process) 11, an optical substrate fixing jig 600 and an optical substrate 10 are set in a chamber apparatus 500. Here, the chamber apparatus 500 is a hollow apparatus, and has an upper chamber box 510, a lower chamber box 520, a film fixing jig 530, and a movable table 540. The upper chamber box 510 is a box-shaped member that opens to the bottom, and the lower chamber box 520 is a box-shaped member that opens to the top.

[0067] A vacuum pump or a compressed air pump is connected to the upper chamber box 510 and the lower chamber box 520, and each internal space can be in a negative or positive pressure state. Here, when the space in each chamber box is in a positive pressure state, various fluids are introduced into the space in each chamber box. Here, an example of the fluid is a gas such as air, but it may also be a liquid. The specific value of the pressure in each chamber box and the time for which such pressure is maintained can be arbitrarily adjusted. In addition, an ultraviolet ray irradiation device (not shown) is provided in the upper chamber box 510. The ultraviolet ray irradiation device may be provided in the lower chamber box 520. The intensity of the ultraviolet ray and the irradiation time can be arbitrarily adjusted. Note that, in this example, it is assumed that the uncured resin layer 20a is an ultraviolet ray curable resin, but in the case of another type of curable resin, a device for curing the curable resin may be provided in the upper chamber box 510 or the lower chamber box 520. Also, a heating device may be provided in each chamber box. The film fixing jig 530 is a jig for fixing the flexible master 400 described later to the opening surface of the lower chamber box 520. The movable table 540 is disposed within the lower chamber box 520 and is capable of moving up and down by a drive device (not shown).

[0068] Specifically, the optical substrate 10 is set on the movable table 540 together with the optical substrate fixing jig 600. Next, the flexible master 400 is fixed to the film fixing jig 530. The open surface of the lower chamber box 520 is closed by the flexible master 400. The flexible master 400 is fixed to the film fixing jig 530 such that the inverted uneven structure 430 faces the optical substrate 10.

[0069] (Optical substrate approach process) Next, as shown in FIG. 12, the upper chamber box 510 and the lower chamber box 520 are connected. This seals the space inside the chamber device 500. At this time, the temperature inside the chamber device 500 may be raised. Next, the space inside the chamber device 500 is evacuated. Next, the movable table 540 is raised to bring the flexible master 400 and the optical substrate 10 close to each other. The distance between the flexible master 400 and the optical substrate 10 may be adjusted appropriately depending on the shape of the optical substrate 10, etc. The arrow in FIG. 12 indicates the movement direction of the movable table 540.

[0070] (4-5. The fifth process (pressing process)) Next, a fluid is introduced into the upper chamber box 510 to put the space in the upper chamber box 510 into a positive pressure state. This applies printing pressure to the flexible master 400. The arrow in FIG. 13 indicates the direction of the printing pressure. This process presses the inverted uneven structure 430 of the flexible master 400 against the uncured resin layer 20a while deforming the flexible master 400. This causes the uncured resin layer 20a to spread over the entire curved surface 11 (the convex surface on one side), and the uncured resin layer 20a penetrates between the fine convex portions of the inverted uneven structure 430. Here, it is preferable to form as few gaps as possible between the uncured resin layer 20a and the flexible master 400. If gaps remain, there is a possibility that air bubbles may be trapped or the inverted uneven structure 430 may not be sufficiently transferred to the resin layer 20.

[0071] (4-6. Sixth step (hardening step)) Then, in this state, the uncured resin layer 20a is cured. Specifically, the uncured resin layer 20a is irradiated with ultraviolet light. As a result, the uncured resin layer 20a becomes the resin layer 20, and the inverted uneven structure 430 is transferred to the surface of the resin layer 20. That is, an inverted structure of the inverted uneven structure 430, i.e., a fine uneven structure 50, is formed on the surface 21 of the resin layer 20. Through the above steps, the resin laminated optical body 1 is produced.

[0072] (2-7. Peeling process) 14, the movable table 540 is lowered to peel the resin laminated optical body 1 from the flexible master 400. In this step, a peeling assist step may be performed to promote peeling between the flexible master 400 and the resin laminated optical body 1. Examples of such a peeling assist step include inserting a blade between the flexible master 400 and the resin laminated optical body 1, blowing a gas such as air between the flexible master 400 and the resin laminated optical body 1, and the like.

[0073] Thereafter, the space within the chamber device 500 is set to atmospheric pressure, and the upper chamber box 510 is removed. Next, the flexible master 400 and the resin laminated optical body 1 are taken out from the lower chamber box 520. Note that a further ultraviolet irradiation process may be performed to promote the curing of the resin layer 20, and a heat treatment may be performed to relieve stress within the resin layer 20.

[0074] By the above steps, the resin layer 20 can be formed on the curved surface 11 on one side of the optical substrate 10. If necessary, the resin layer 20 may also be formed on the curved surface on the opposite side by the same steps as above.

[0075] In addition, even when the optical substrate 10 is a concave lens, the resin laminate optical body 1 can be produced by the same process as above. The outline of the process is shown in FIG. 15 and FIG. 16. As shown in FIG. 15, an uncured resin layer 20a is formed on the curved surface 11 of the optical substrate 10. Next, the optical substrate 10 and the flexible master 400 are set in a chamber device 500. Next, the flexible master 400 and the optical substrate 10 are brought close to each other. Next, as shown in FIG. 16, printing pressure is applied to the flexible master 400. The arrow in FIG. 16 indicates the direction of printing pressure. Through this process, the flexible master 400 is deformed while the inverted concave-convex structure 430 of the flexible master 400 is pressed against the uncured resin layer 20a. As a result, the uncured resin layer 20a spreads over the entire curved surface 11, and the uncured resin layer 20a penetrates between the fine convex portions of the inverted concave-convex structure 430. Here, it is preferable to form as little gap as possible between the uncured resin layer 20a and the flexible master 400. In this state, the uncured resin layer 20a is cured. Specifically, the uncured resin layer 20a is irradiated with ultraviolet light. As a result, the uncured resin layer 20a becomes the resin layer 20, and the inverted uneven structure 430 is transferred to the surface of the resin layer 20. That is, an inverted structure of the inverted uneven structure 430, i.e., the fine uneven structure 50, is formed on the surface 21 of the resin layer 20. Through the above steps, the resin laminated optical body 1 is produced.

[0076] Next, the resin laminated optical body 1 is peeled off from the flexible master 400 , and the flexible master 400 and the resin laminated optical body 1 are taken out from the chamber device 500 .

[0077] Through the above steps, the resin layer 20 can be formed on the curved surface 11 on one side of the optical substrate 10. If necessary, the resin layer 20 may also be formed on the opposite curved surface through the same steps as above. According to the above-described method for producing the resin laminated optical body 1, the resin layer 20 can be easily formed on the curved surface 11 of the optical substrate 10.

[0078] <5. Manufacturing method of light source unit> Next, a method for manufacturing the light source unit 30 will be described. The light source unit 30 is also manufactured by the same manufacturing method as the resin laminated optical body 1, but is different from the manufacturing method of the resin laminated structure 1 in that a step of incorporating the light source 31 in the light source unit 30 is added. Here, as a method for incorporating the light source 31 in the light source unit 30, for example, a method for incorporating the light source 31 in advance in the optical substrate 32 can be mentioned. In this method, the light source 31 is embedded in the optical substrate 32 by directly filling the resin on the light source 31 by molding or the like. The light source unit 30 is manufactured by carrying out the above-mentioned second step and subsequent steps on this optical substrate 32. As another method for incorporating the light source 31 in the light source unit 30, the following method can be mentioned. That is, the above-mentioned first step to the peeling step are carried out on the optical substrate 32 that is separate from the light source 31, thereby forming the resin layer 40 on the optical substrate 32. Next, the optical substrate 32 on which the resin layer 40 is formed is placed on the light source 31. In this way, the light source unit 30 is manufactured. According to the above-described method for manufacturing the light source unit 30, the resin layer 40 can be easily formed on the curved surface 33 of the optical base material 32.

[0079] <6. Detailed configuration and manufacturing method of flexible master> Next, a detailed configuration and a manufacturing method of the flexible master 400 will be described. As shown in Fig. 19, the flexible master 400 includes a flexible substrate 410 and a resin layer 425 formed on the surface of the flexible substrate 410. The flexible substrate 410 is a flexible, flat substrate. Examples of materials constituting the flexible substrate 410 include acrylic resin (polymethyl methacrylate, etc.), polycarbonate, PET (polyethylene terephthalate. Note that the properties of the PET are not particularly limited, and it may be amorphous or stretched), TAC (triacetyl cellulose), polyethylene, polypropylene, polycarbonate, cycloolefin polymer, cycloolefin copolymer, vinyl chloride, etc.

[0080] The resin layer 425 is made of a curable resin. The type of the curable resin is not particularly limited, and may be, for example, the same curable resin as that constituting the resin layer 20. An inverted uneven structure 430 is formed in the resin layer 425. The inverted uneven structure 430 is made of a large number of fine convex portions 430a and fine concave portions 430b.

[0081] Next, a description will be given of a manufacturing method of the flexible master 400. The manufacturing method of the flexible master 400 includes a first master fabrication step of fabricating a transfer mold having an inverted structure of the inverted concave-convex structure 430, a second master fabrication step of forming an uncured resin layer 420 on the surface of the flexible base material 410, and a third master fabrication step of curing the uncured resin layer 420 and transferring the concave-convex structure of the transfer mold to the cured resin layer 425.

[0082] (6-1. First master production process) The first master fabrication process is a process for fabricating a transfer mold having an inverted structure of the inverted concavo-convex structure 430. The transfer mold is, for example, the master 100 shown in FIG.

[0083] (6-1-1. Master composition) The configuration of the master 100 will now be described. The master 100 has a cylindrical shape. The master 100 may be cylindrical or may have another shape (for example, a flat plate shape). However, when the master 100 has a cylindrical or columnar shape, the concave-convex structure (i.e., master concave-convex structure) 120 of the master 100 can be seamlessly transferred to a resin substrate or the like by a roll-to-roll method. This allows the inverted concave-convex structure 430 to be formed on the surface of the flexible substrate 410 with high production efficiency. From this viewpoint, the shape of the master 100 is preferably cylindrical or columnar.

[0084] The master 100 includes a master substrate 110 and a master uneven structure 120 formed on the peripheral surface of the master substrate 110. The master substrate 110 is, for example, a glass body, and more specifically, is made of quartz glass. However, the master substrate 110 is preferably made of SiO 2As long as it has high purity, it may be formed of fused quartz glass, synthetic quartz glass, or the like, without any particular limitation. The master substrate 110 may be a metal substrate having the above-mentioned materials laminated thereon, or may be a metal substrate (e.g., Cu, Ni, Cr, Al). The master substrate 110 has a cylindrical shape, but may also have a columnar shape or other shapes. However, as described above, the master substrate 110 is preferably cylindrical or columnar. The master concave-convex structure 120 has an inverted structure of the inverted concave-convex structure 430.

[0085] (6-1-2. Manufacturing method of master disc) Next, a method for manufacturing the master 100 will be described. First, a base resist layer is formed (deposited) on the master substrate 110. Here, the resist material constituting the base resist layer is not particularly limited, and may be either an organic resist material or an inorganic resist material. Examples of the organic resist material include novolac-based resists and chemically amplified resists. Examples of the inorganic resist material include metal oxides containing one or more transition metals such as tungsten (W) or molybdenum (Mo). Other examples of the inorganic resist material include Cr, Au, and the like. However, in order to perform thermal reaction lithography, it is preferable that the base resist layer is formed of a thermal reaction resist containing a metal oxide.

[0086] When an organic resist material is used, the substrate resist layer may be formed on the master substrate 110 by using spin coating, slit coating, dip coating, spray coating, screen printing, or the like. When an inorganic resist material is used for the substrate resist layer, the substrate resist layer may be formed by using a sputtering method. The organic resist material and the inorganic resist material may be used in combination.

[0087] Next, a latent image is formed in the substrate resist layer by exposing a portion of the substrate resist layer using an exposure device 200 (see FIG. 18). Specifically, the exposure device 200 modulates a laser beam 200A and irradiates the substrate resist layer with the laser beam 200A. This causes the portion of the substrate resist layer irradiated with the laser beam 200A to denature, so that a latent image corresponding to the master concave-convex structure 120 can be formed in the substrate resist layer.

[0088] Next, a developer is dropped onto the substrate resist layer on which the latent image is formed, thereby developing the substrate resist layer. As a result, a concave-convex structure is formed on the substrate resist layer. Next, the master substrate 110 and the substrate resist layer are etched using the substrate resist layer as a mask, thereby forming a master concave-convex structure 120 on the master substrate 110. Note that the etching method is not particularly limited, but is preferably dry etching having vertical anisotropy, for example, reactive ion etching (RIE). Through the above steps, the master 100 is produced. The etching may be wet etching.

[0089] (6-1-3. Configuration of Exposure Equipment) Next, the configuration of the exposure apparatus 200 will be described with reference to Fig. 18. The exposure apparatus 200 is an apparatus that exposes a substrate resist layer. The exposure apparatus 200 includes a laser light source 201, a first mirror 203, a photodiode (PD) 205, a deflection optical system, a control mechanism 230, a second mirror 213, a movable optical table 220, a spindle motor 225, and a turntable 227. The master substrate 110 is placed on the turntable 227 and is capable of rotating.

[0090] The laser light source 201 is a light source that emits a laser beam 200A, and is, for example, a solid-state laser or a semiconductor laser. The wavelength of the laser beam 200A emitted by the laser light source 201 is not particularly limited, and may be, for example, a wavelength in the blue light band of 400 nm to 500 nm. The spot diameter of the laser beam 200A (the diameter of the spot irradiated on the resist layer) may be smaller than the diameter of the opening surface of the recess of the master disc concave-convex structure 120, and may be, for example, about 200 nm. The laser beam 200A emitted from the laser light source 201 is controlled by a control mechanism 230.

[0091] Laser light 200A emitted from a laser light source 201 travels straight as a parallel beam, is reflected by a first mirror 203, and is guided to a deflection optical system.

[0092] The first mirror 203 is composed of a polarizing beam splitter and has a function of reflecting one polarized component and transmitting the other polarized component. The polarized component transmitted through the first mirror 203 is received by a photodiode 205 and photoelectrically converted. The received light signal photoelectrically converted by the photodiode 205 is input to the laser light source 201, and the laser light source 201 performs phase modulation of the laser light 200A based on the input received light signal.

[0093] The deflection optical system includes a condenser lens 207 , an electro-optic deflector (EOD) 209 , and a collimator lens 211 .

[0094] In the deflection optical system, the laser beam 200A is focused on an electro-optic deflection element 209 by a focusing lens 207. The electro-optic deflection element 209 is an element capable of controlling the irradiation position of the laser beam 200A. The exposure apparatus 200 is also capable of changing the irradiation position of the laser beam 200A guided onto the movable optical table 220 by the electro-optic deflection element 209 (so-called Wobble mechanism). After the irradiation position of the laser beam 200A is adjusted by the electro-optic deflection element 209, the laser beam 200A is collimated again by a collimator lens 211. The laser beam 200A emitted from the deflection optical system is reflected by a second mirror 213 and guided horizontally and parallel onto the movable optical table 220.

[0095] The moving optical table 220 includes a beam expander (BEX) 221 and an objective lens 223. The laser light 200A guided to the moving optical table 220 is shaped into a desired beam shape by the beam expander 221, and then irradiated via the objective lens 223 onto the substrate resist layer formed on the master substrate 110. The moving optical table 220 moves by one feed pitch (track pitch) in the direction of arrow R (feed pitch direction) every time the master substrate 110 rotates once. The master substrate 110 is placed on the turntable 227. The spindle motor 225 rotates the turntable 227 to rotate the master substrate 110. This causes the laser light 200A to scan the substrate resist layer. Here, a latent image of the substrate resist layer is formed along the scanning direction of the laser light 200A.

[0096] Moreover, the control mechanism 230 includes a formatter 231 and a driver 233, and controls the irradiation of the laser beam 200A. The formatter 231 generates a modulation signal for controlling the irradiation of the laser beam 200A, and the driver 233 controls the laser light source 201 based on the modulation signal generated by the formatter 231. This controls the irradiation of the laser beam 200A onto the master substrate 110.

[0097] The formatter 231 generates a control signal for irradiating the substrate resist layer with the laser light 200A based on an input image in which an arbitrary pattern to be drawn on the substrate resist layer is drawn. Specifically, the formatter 231 first acquires an input image in which an arbitrary drawing pattern to be drawn on the substrate resist layer is drawn. The input image is an image corresponding to a development of the outer peripheral surface of the substrate resist layer, in which the outer peripheral surface of the substrate resist layer is cut open in the axial direction and stretched into a single plane. In this development, an image corresponding to the peripheral surface shape of the master 100 is drawn. This image shows the inverted structure of the inverted uneven structure 430. Note that a transfer film to which the master uneven structure 120 of the master 100 is transferred may be produced, and the inverted uneven structure 430 may be formed on the flexible substrate 410 using this transfer film as a transfer mold. In this case, the master uneven structure 120 has the same uneven structure as the inverted uneven structure 430.

[0098] Next, the formatter 231 divides the input image into small regions of a predetermined size (for example, into a grid), and judges whether each of the small regions includes a recess drawing pattern (i.e., a pattern corresponding to the recesses of the master 100). Next, the formatter 231 generates a control signal for controlling each small region determined to include a recess drawing pattern to be irradiated with the laser light 200A. This control signal (i.e., exposure signal) is preferably synchronized with the rotation of the spindle motor 225, but does not have to be synchronized. In addition, the control signal and the rotation of the spindle motor 225 may be resynchronized every time the master substrate 110 rotates once. Furthermore, the driver 233 controls the output of the laser light source 201 based on the control signal generated by the formatter 231. This controls the irradiation of the laser light 200A onto the substrate resist layer. The exposure device 200 may perform known exposure control processing such as focus servo, position correction of the irradiation spot of the laser light 200A, and the like. The focus servo may use the wavelength of the laser light 200A, or may use another wavelength for reference.

[0099] In addition, the laser light 200A emitted from the laser light source 201 may be branched into multiple optical systems and then irradiated onto the substrate resist layer. In this case, multiple irradiation spots are formed on the substrate resist layer. In this case, exposure may be terminated when the laser light 200A emitted from one optical system reaches the latent image formed by the other optical system.

[0100] Therefore, according to this embodiment, a latent image corresponding to the drawing pattern of the input image can be formed in the resist layer. Then, the resist layer is developed, and the master substrate 110 and the substrate resist layer are etched using the developed resist layer as a mask, thereby forming a master uneven structure 120 corresponding to the drawing pattern of the input image on the master substrate 110. That is, an arbitrary master uneven structure 120 corresponding to the drawing pattern can be formed. Therefore, if a drawing pattern in which an inverted structure of the inverted uneven structure 430 is drawn is prepared as the drawing pattern, a master uneven structure 120 having an inverted structure of the inverted uneven structure 430 can be formed.

[0101] It should be noted that the exposure apparatus that can be used in this embodiment is not limited to exposure apparatus 200, and any exposure apparatus that has the same functions as exposure apparatus 200 may be used.

[0102] (6-1-4. Method for forming a concave-convex structure using a master) Next, an example of a method for forming an inverted uneven structure 430 using the master 100 will be described with reference to Fig. 19. The inverted uneven structure 430 can be formed on a flexible substrate 410 by a roll-to-roll transfer device 300 using the master 100. In the transfer device 300 shown in Fig. 19, the curable resin constituting the resin layer 425 is a so-called ultraviolet curable resin. The transfer device 300 is used to perform the second and third master fabrication steps described above.

[0103] The transfer device 300 includes the master 100 , a substrate supply roll 301 , a take-up roll 302 , guide rolls 303 and 304 , a nip roll 305 , a peeling roll 306 , a coating device 307 , and a light source 309 .

[0104] The substrate supply roll 301 is a roll on which a long flexible substrate 410 is wound in a roll shape, and the take-up roll 302 is a roll that takes up the flexible master 400. The guide rolls 303 and 304 are rolls that transport the flexible substrate 410. The nip roll 305 is a roll that brings the flexible substrate 410 on which the uncured resin layer 420 is laminated, i.e., the transferred film 450, into close contact with the master 100. The peeling roll 306 is a roll that peels the flexible master 400 from the master 100.

[0105] Coating device 307 includes a coating means such as a coater, and coats uncured curable resin onto flexible substrate 410 to form uncured resin layer 420. Coating device 307 may be, for example, a gravure coater, a wire bar coater, or a die coater. Light source 309 is a light source that emits light with a wavelength capable of curing the uncured resin, and may be, for example, an ultraviolet lamp.

[0106] In the transfer device 300, first, the flexible substrate 410 is continuously fed from the substrate supply roll 301 through the guide roll 303. The substrate supply roll 301 may be replaced with a substrate supply roll 301 of a different lot during the feeding process. The coating device 307 applies an uncured resin to the fed flexible substrate 410, and the uncured resin layer 420 is laminated on the flexible substrate 410. In this way, the transfer film 450 is produced. The transfer film 450 is brought into close contact with the master 100 by the nip roll 305. The light source 309 irradiates the uncured resin layer 420 in close contact with the master 100 with ultraviolet light, thereby curing the uncured resin layer 420. In this way, the uncured resin layer 420 becomes a resin layer 425, and the master concave-convex structure 120 is transferred to the surface of the resin layer 425. That is, an inverted structure of the master uneven structure 120, that is, an inverted uneven structure 430, is formed on the surface of the resin layer 425. Next, the flexible substrate 410 on which the inverted uneven structure 430 is formed is peeled off from the master 100 by the peeling roll 306. Next, the flexible substrate 410 on which the inverted uneven structure 430 is formed is taken up by the take-up roll 302 via the guide roll 304. Note that the master 100 may be placed vertically or horizontally, and a mechanism for correcting the angle and eccentricity during rotation of the master 100 may be separately provided. For example, an eccentric tilt mechanism may be provided in the chucking mechanism. The transfer may be performed by compressed air transfer.

[0107] In this manner, in the transfer device 300, the transfer film 450 is transported in a roll-to-roll manner, while the peripheral surface shape of the master 100 is transferred onto the transfer film 450. As a result, the inverted concavo-convex structure 430 is formed on the flexible substrate 410.

[0108] If the flexible substrate 410 is a thermoplastic resin film, the coating device 307 and the light source 309 are not necessary. In this case, a heating device is disposed upstream of the master 100. The flexible substrate 410 is heated and softened by the heating device, and then the flexible substrate 410 is pressed against the master 100. As a result, the master uneven structure 120 formed on the peripheral surface of the master 100 is transferred to the flexible substrate 410. The flexible substrate 410 may be a film made of a resin other than a thermoplastic resin, and the flexible substrate 410 and the thermoplastic resin film may be laminated. In this case, the laminated film is heated by the heating device and then pressed against the master 100. Therefore, the transfer device 300 can continuously produce a transfer product in which the inverted uneven structure 430 is formed on the flexible substrate 410.

[0109] In addition, a transfer film to which the master uneven structure 120 of the master 100 is transferred may be prepared, and the transfer film may be used as a transfer mold to form the inverted uneven structure 430 on the flexible substrate 410. The transfer film to which the uneven structure of the transfer film is further transferred may be used as the transfer mold. In this case, the master uneven structure 120 is formed so that the fine uneven structure formed in the resin layer 425 becomes an inverted uneven structure. In addition, the master 100 may be duplicated by electroforming or thermal transfer, and the duplicate may be used as the transfer mold. Furthermore, the shape of the master 100 is not limited to a roll shape, and may be a flat master, and various processing methods such as semiconductor exposure using a mask, electron beam drawing, mechanical processing, and anodization can be selected in addition to the method of irradiating the laser light 200A to the resist.

[0110] <7. Application examples of resin laminated optical bodies and light source units> Next, an application example of the resin laminated optical body 1 and the light source unit 30 will be described with reference to Figs. 20 to 26. In the example of Fig. 20, the resin laminated optical body 1 and the light source unit 30 are applied to a projection type image display device (i.e., an image projection device) 1000. The image display device 1000 has a transmission type diffusion screen structure. That is, the image display device 1000 includes a light irradiation device 1010, a liquid crystal panel 1015, mirrors 1020 and 1030, and a display unit 1040. The light irradiated from the light irradiation device 1010 passes through the liquid crystal panel 1015, is reflected by the mirrors 1020, 1030, and the display unit 1040 in sequence, and enters the field of view of the user (person U). That is, the image displayed on the liquid crystal panel 1015 is displayed as a virtual image on the display unit 1040. This allows the user to view the image (virtual image) displayed on the display unit 1040.

[0111] The light irradiation device 1010 has an optical unit 1a shown in FIG. 21. The optical unit 1a has a resin laminated optical body 1 and a light source unit 30. In the example of FIG. 21, the optical substrate 10 is a biconcave lens, and a resin layer 20 is formed on both the front and back sides. The light sources 31 in the light source unit 30 are arranged in a matrix, and each light source 31 emits light in a desired manner, so that a desired image can be displayed on the display unit 1040. The display unit 1040 is, for example, a windshield or a combiner. For example, when the image display device 1000 is mounted on a vehicle, the display unit 1040 is a windshield.

[0112] The configuration of the optical unit 1a is not limited to the example in FIG. 21. For example, the resin laminated optical body 1 may be any of the examples listed in FIGS. 1 to 8. Furthermore, either the resin laminated optical body 1 or the light source unit 30 may be replaced with a conventional configuration. For example, as shown in FIG. 22, the resin layer 40 of the light source unit 30 may be omitted. Furthermore, as shown in FIG. 23, the resin laminated optical body 1 may be replaced with an optical substrate 10 (i.e., a conventional optical lens).

[0113] Furthermore, at least one of the mirrors 1020 and 1030 may be replaced with the resin laminated optical body 1.

[0114] 20, since the optical unit 1a is built into the light irradiation device 1010, the light irradiation device 1010 can be made smaller, and therefore the image display device 1000 can be made smaller. By replacing at least one of the mirrors 1020 and 1030 with the resin laminated optical body 1, the image display device 1000 can be expected to be further made smaller. Furthermore, since interfacial reflection is less likely to occur between the resin layer 20 and the optical substrate 10, or between the resin layer 40 and the optical substrate 32, the light emission quality, specifically the quality of the displayed image, can be improved (for example, reduction in uneven brightness, etc.).

[0115] In the example of FIG. 24, the resin laminated optical body 1 is applied to a projection type image display device (i.e., an image projection device) 2000. The image display device 2000 has a transmission type diffusion screen structure. That is, the image display device 2000 includes a light irradiation device 2010 and a display unit 2020. The light irradiation device 2010 is, for example, a raster scan type laser irradiation device, and light irradiated from the light irradiation device 2010 passes through the resin laminated optical body 1 and enters the display unit 2020. The light that enters the display unit 2020 is reflected by the display unit 2020 and enters the user's field of vision. This allows the user to view the image (virtual image) displayed on the display unit 2020. The display unit 2020 is, for example, a combiner or the like.

[0116] 24, the resin laminated optical body 1 is disposed in the optical path of the light emitted from the light irradiation device 2010. In the example of Fig. 24, the resin laminated optical body 1 shown in Fig. 1 is disposed, but other resin laminated optical bodies 1 listed in Figs. 3 to 8 may also be disposed.

[0117] 24, since the resin laminated optical body 1 is built into the image display device 2000, it is possible to reduce the size of the image display device 1000. Furthermore, since interfacial reflection is unlikely to occur between the resin layer 20 and the optical substrate 10, the light emission quality, specifically, the quality of the displayed image, can be improved (for example, reduction in uneven brightness, etc.).

[0118] In the example of FIG. 25, the resin laminated optical body 1 is applied to a projection type image display device (i.e., an image projection device) 3000. The image display device 3000 has a reflection type diffusion screen structure. That is, the image display device 3000 includes a light irradiation device 3010, a liquid crystal panel 3015, a mirror 3020, and a display unit 3030. The light irradiation device 3010 may be, for example, a laser light source that emits laser light, or an LED light source. The light irradiated from the light irradiation device 3010 passes through the liquid crystal panel 3015, is reflected by the mirror 3020 and the display unit 3030, and enters the user's field of vision. That is, the image displayed on the liquid crystal panel 3015 is displayed as a virtual image on the display unit 3030. This allows the user to view the image (virtual image) displayed on the display unit 3030.

[0119] In the example of Fig. 25, the mirror 3020 is composed of the resin laminated optical body 1. The display unit 3030 is, for example, a windshield or a combiner. The configuration of the resin laminated optical body 1 is not limited to the example of Fig. 25, and may be any of the other resin laminated optical bodies 1 listed in Figs. 1 to 8. Furthermore, the light irradiation device 3010 may be composed of the light irradiation device 1010 described above.

[0120] 25, the mirror 3020 is formed of the resin laminated optical body 1, so that the image display device 3000 can be made compact. Furthermore, since interfacial reflection is less likely to occur between the resin layer 20 and the optical substrate 10, the light emission quality, specifically, the quality of the displayed image can be improved (for example, reduction in uneven brightness, etc.).

[0121] In the example of FIG. 26, the resin laminated optical body 1 is applied to a projection type image display device (i.e., an image projection device) 4000. The image display device 4000 has a reflection type diffusion screen structure. That is, the image display device 4000 includes a light irradiation device 4010, a liquid crystal panel 4015, mirrors 4020 and 4030, and a display unit 4040. The light irradiation device 4010 may be, for example, a laser light source that emits laser light, or an LED light source. The light irradiated from the light irradiation device 4010 passes through the liquid crystal panel 4015, is reflected by the mirrors 4020 and 4030, and the display unit 4040, and enters the user's field of vision. That is, the image displayed on the liquid crystal panel 4015 is displayed as a virtual image on the display unit 4040. This allows the user to view the image (virtual image) displayed on the display unit 4040.

[0122] In the example of Fig. 26, mirrors 4020, 4030 are configured with a resin laminated optical body 1. Display unit 4040 is, for example, a windshield or a combiner. The configuration of resin laminated optical body 1 is not limited to the example of Fig. 26, and may be other resin laminated optical bodies 1 listed in Figs. 1 to 8. At least one of mirrors 4020, 4030 may be configured with a conventional mirror.

[0123] According to the example of FIG. 26, the mirrors 4020 and 4030 are formed of the resin laminated optical body 1, so that the image display device 4000 can be made compact. EXAMPLES

[0124] <1. Example 1> Next, examples of this embodiment will be described. In Examples 1 to 18 and Comparative Example 1, tests were carried out to evaluate the characteristics of the light irradiation device 1010 shown in Fig. 20. The following is a detailed description.

[0125] (1-1. Creation of the master disc) By carrying out the above-mentioned first to third master fabrication steps, a flexible master 400 was fabricated in which the inverted uneven structure 430 was a light diffusion structure or a moth-eye structure. More specifically, a PET film with a thickness of 75 μm was prepared as the flexible substrate 410. Then, a resin layer 425 was formed on one surface of the flexible substrate 410 using a transfer device 300 shown in FIG. 19. Here, an ultraviolet-curable acrylic resin composition SK1120 manufactured by Dexerials Corporation was used as the ultraviolet-curable resin. The average period of the inverted uneven structure 430 constituting the moth-eye structure was 250 nm, and the height difference was 200 nm. In the inverted uneven structure 430 constituting the light diffusion structure, the average interval between the fine recesses and the average interval between the fine protrusions were 48 μm, and the height difference was 1.2 μm.

[0126] (1-2. Preparation of optical substrate) A plano-concave lens was prepared as an optical substrate 10 for a lens (hereinafter also referred to as "optical substrate 10-1"). Here, the diameter (φ) of the optical substrate 10-1 was 50 mm, the material was BK7, and the radius of curvature was 102 mm. The refractive index of the optical substrate 10-1 was 1.52. Here, the radius of curvature was measured using a three-dimensional measuring device UA3P manufactured by Panasonic Corporation, and the refractive index was measured using an Abbe refractometer manufactured by Atago Co., Ltd. The refractive index was measured at a wavelength of 587 nm.

[0127] Furthermore, as a material for the optical substrate 32 for the light source unit 30, a cycloolefin polymer (ZEONEX 480R manufactured by ZEON CORPORATION) was prepared.

[0128] (1-3. Preparation of UV-curable resin) An acrylic ultraviolet-curable resin having the following composition was prepared as the ultraviolet-curable resin constituting the resin layer 20. The viscosity (cP) of the acrylic ultraviolet-curable resin when uncured was 1240 cP, and the refractive index was 1.52. Here, the viscosity was measured using a Brookfield rotational viscometer, and the refractive index was measured after curing using an Atago Abbe refractometer. The refractive index was measured at a wavelength of 587 nm. Monomer: Toagosei Aronix M305: 45 parts by weight Oligomer: Nippon Synthetic Chemical UV-1700: 20 parts by weight Reactive diluent: KJ Chemical DMAA: 30 parts by weight Photopolymerization initiator: Irgacure 184: 5 parts by weight

[0129] (1-4. Preparation of the light source unit) The light source unit 30-1 was produced by carrying out the above-mentioned first to sixth steps and the peeling step. Here, as the flexible master 400, a flexible master 400 (hereinafter also referred to as "flexible master 400-1") in which the inverted uneven structure 430 has a moth-eye structure was used. Furthermore, a white LED was used as the light source 31. Also, the above-mentioned cycloolefin polymer was directly filled on the light source 31 by molding, thereby embedding the light source 31 in the optical base material 32. In this way, the light source unit 30-1 was produced. The thickness of the resin layer 40 was set to 3 μm. In the following examples, the thickness of the resin layer 40 was all the same as in Example 1.

[0130] (1-5. Preparation of light diffusion plate) A light diffusion plate was produced using the flexible master 400 (hereinafter also referred to as "flexible master 400-2") in which the inverted uneven structure 430 is a light diffusion structure and the above-mentioned ultraviolet curing resin. Specifically, the above-mentioned ultraviolet curing resin was applied to an acrylic film with a thickness of 5 μm, and the flexible master 400-2 was attached thereon. In this state, the ultraviolet curing resin was irradiated with ultraviolet light, and the flexible master 400-2 was peeled off to produce a light diffusion plate.

[0131] (1-6. Measurement of total light transmittance and diffusion angle) The optical unit 1a was produced by arranging the optical substrate 10-1 and the light diffusion plate in this order on the light emitting surface 32a of the light source unit 30-1. Here, the curved surface 11 of the optical substrate 10-1 was opposed to the light diffusion plate. Hereinafter, the curved surface 11 is referred to as the "front surface" of the optical substrate 10-1, and the surface opposite to the front surface (the surface on the light source unit 30-1 side) is referred to as the "rear surface". Then, the light source 31 was caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that passed through the light diffusion plate were measured. Here, the total light transmittance is the ratio of the emission intensity of the transmitted light to the emission intensity of the light source 31, and the diffusion angle is the angle at which the light intensity is half when the light intensity at each emission angle is normalized by the light intensity of vertical transmission (0°). The total light transmittance was measured using HM-150 manufactured by Murakami Color Research Laboratory. The diffusion angle was measured using EZ-Contrast manufactured by ELDIM. A white collimated light source was used as the light source. The results are summarized in Table 1.

[0132] <2. Example 2> (2-1. Preparation of resin laminated optical body) The flexible master 400-1 was used to perform the above-mentioned first to sixth steps and the peeling step to form a resin layer 20 on the surface of the optical substrate 10-1. In this way, a resin laminated optical body 1-2 was produced. A moth-eye structure was formed as the fine uneven structure 50 on the surface 21 of the resin layer 20. The thickness of the resin layer 20 was set to 5 μm. In the following examples, the thickness of the resin layer 20 was the same as in Example 2.

[0133] (2-2. Measurement of total light transmittance and diffusion angle) An optical unit 1a was produced by arranging a resin laminated optical body 1-2 and a light diffusion plate in this order on the light emitting surface 32a of a light source unit 30-1. The light diffusion plate was the same as that used in Example 1. Then, the light source 31 was caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that passed through the light diffusion plate were measured. The measurement conditions were the same as those in Example 1. The results are summarized in Table 1.

[0134] <3. Example 3> (3-1. Preparation of resin laminated optical body) The flexible master 400-1 was used to perform the above-mentioned first to sixth steps and the peeling step to form a resin layer 20 on the rear surface of the optical substrate 10-1. In this way, a resin laminated optical body 1-3 was produced. A moth-eye structure was formed as the fine uneven structure 50 on the front surface 21 of the resin layer 20.

[0135] (3-2. Measurement of total light transmittance and diffusion angle) An optical unit 1a was produced by arranging a resin laminated optical body 1-3 and a light diffusion plate in this order on the light emitting surface 32a of the light source unit 30-1. The light diffusion plate was the same as that used in Example 1. Then, the light source 31 was caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that passed through the light diffusion plate were measured. The measurement conditions were the same as those in Example 1. The results are summarized in Table 1.

[0136] <4. Example 4> (4-1. Preparation of resin laminated optical body) By carrying out the above-mentioned first to sixth steps and the peeling step using the flexible master 400-1, the resin layer 20 was formed on both the front and back sides of the optical substrate 10-1. In this way, the resin laminated optical body 1-4 was produced. A moth-eye structure was formed as the fine uneven structure 50 on the surface 21 of the resin layer 20.

[0137] (4-2. Measurement of total light transmittance and diffusion angle) An optical unit 1a was produced by arranging a resin laminated optical body 1-4 and a light diffusion plate in this order on the light emitting surface 32a of the light source unit 30-1. The light diffusion plate was the same as that used in Example 1. Then, the light source 31 was caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that passed through the light diffusion plate were measured. The measurement conditions were the same as those in Example 1. The results are summarized in Table 1.

[0138] <5. Comparative Example 1> (5-1. Measurement of total light transmittance and diffusion angle) The light source unit 30-c1 was produced by incorporating the light source 31 in the optical substrate 32. The light source unit 30-c1 is obtained by omitting the resin layer 40 from the light source unit 30-1 of Example 1. The optical substrate 10-1 and the light diffusion plate were arranged in this order on the light emitting surface 32a of the light source unit 30-c1 to produce an optical unit. The light diffusion plate was used in Example 1. Therefore, in the optical unit of Comparative Example 1, the resin layer according to this embodiment is not formed on either the optical substrates 10-1 and 32. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light transmitted through the light diffusion plate were measured. The measurement conditions were the same as those of Example 1. The results are summarized in Table 1.

[0139] [Table 1]

[0140] In Table 1, lenses 1 and 2 refer to the optical substrates 32 and 10-1, respectively. The "separate" diffuser plate means that the optical substrate 10-1 and the light diffuser plate are separate. "No treatment" means that no resin layer is formed. "Anti-reflection" means that a moth-eye structure is formed.

[0141] <6. Example 5> (6-1. Preparation of resin laminated optical body) The flexible master 400-2 was used to perform the above-mentioned first to sixth steps and the peeling step to form a resin layer 20 on the surface of the optical substrate 10-1. In this way, a resin laminated optical body 1-5 was produced. A light diffusion structure was formed as a fine uneven structure 50 on the surface 21 of the resin layer 20.

[0142] (6-2. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-5 was placed on the light emitting surface 32a of the light source unit 30-c1 to produce the optical unit 1a. The light source 31 was then caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that had passed through the resin laminated optical body 1-5 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0143] <7. Example 6> (7-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-5 was placed on the light emitting surface 32a of the light source unit 30-1 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-5 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0144] <8. Example 7> (8-1. Preparation of resin laminated optical body) The flexible master 400-2 was used to perform the above-mentioned first to sixth steps and the peeling step to form a resin layer 20 on the back surface of the optical substrate 10-1. In this way, a resin laminated optical body 1-7 was produced. A light diffusion structure was formed as a fine uneven structure 50 on the front surface 21 of the resin layer 20.

[0145] (8-2. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-7 was placed on the light emitting surface 32a of the light source unit 30-c1 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-7 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0146] <9. Example 8> (9-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-7 was placed on the light emitting surface 32a of the light source unit 30-1 to produce the optical unit 1a. The light source 31 was then caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that had passed through the resin laminated optical body 1-7 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0147] <10. Example 9> (10-1. Preparation of resin laminated optical body) By carrying out the above-mentioned first to sixth steps and the peeling step using the flexible master 400-2, the resin layer 20 was formed on both the front and back sides of the optical substrate 10-1. In this way, the resin laminated optical body 1-9 was produced. A light diffusion structure was formed as a fine uneven structure 50 on the surface 21 of the resin layer 20.

[0148] (10-2. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-9 was placed on the light emitting surface 32a of the light source unit 30-c1 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-9 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0149] <11. Example 10> (11-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-9 was placed on the light emitting surface 32a of the light source unit 30-1 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-9 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0150] <12. Example 11> (12-1. Preparation of resin laminated optical body) The flexible master 400-2 was used to carry out the first to sixth steps and the peeling step described above, thereby forming a resin layer 20 on the surface of the optical substrate 10-1. A light diffusion structure was formed as the fine uneven structure 50 on the surface 21 of this resin layer 20. Furthermore, the flexible master 400-1 was used to carry out the first to sixth steps and the peeling step described above, thereby forming a resin layer 20 on the rear surface of the optical substrate 10-1. A moth-eye structure was formed as the fine uneven structure 50 on the surface 21 of this resin layer 20. In this way, a resin laminated optical body 1-11 was produced.

[0151] (12-2. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-11 was placed on the light emitting surface 32a of the light source unit 30-c1 to produce the optical unit 1a. The light source 31 was then caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that had passed through the resin laminated optical body 1-11 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0152] <13. Example 12> (11-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-11 was placed on the light emitting surface 32a of the light source unit 30-1 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that passed through the resin laminated optical body 1-11 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0153] <14. Example 13> (12-1. Preparation of resin laminated optical body) The flexible master 400-1 was used to carry out the first to sixth steps and the peeling step described above, thereby forming a resin layer 20 on the surface of the optical substrate 10-1. A moth-eye structure was formed as the fine uneven structure 50 on the surface 21 of this resin layer 20. Furthermore, the flexible master 400-2 was used to carry out the first to sixth steps and the peeling step described above, thereby forming a resin layer 20 on the rear surface of the optical substrate 10-1. A light diffusing structure was formed as the fine uneven structure 50 on the surface 21 of this resin layer 20. In this way, a resin laminated optical body 1-13 was produced.

[0154] (12-2. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-13 was placed on the light emitting surface 32a of the light source unit 30-c1 to produce the optical unit 1a. The light source 31 was then caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that had passed through the resin laminated optical body 1-13 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0155] <15. Example 14> (11-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-13 was placed on the light emitting surface 32a of the light source unit 30-1 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-13 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 2.

[0156] [Table 2]

[0157] In Table 2, lenses 1 and 2 refer to optical substrates 32 and 10-1, respectively. The "lens integrated" of the diffusion plate means that a light diffusion structure is integrated with at least one of optical substrates 10-1 and 32 (i.e., a resin layer having a light diffusion structure is formed). "Untreated" means that a resin layer is not formed. "Anti-reflective" means that a moth-eye structure is formed. "Diffusion" means that a light diffusion structure is formed.

[0158] <16. Example 15> (16-1. Preparation of the light source unit) The light source unit 30-15 was manufactured by carrying out the above-mentioned first to seventh steps and the peeling step. Here, the flexible master 400 was used as the flexible master 400. The light source 31 used was the same as that in Example 1. In this way, the light source unit 30-15 was manufactured. A light diffusion structure was formed as the fine uneven structure 50 on the surface 41 of the resin layer 40.

[0159] (16-2. Measurement of total light transmittance and diffusion angle) The optical unit 1a was produced by disposing the optical substrate 10-1 on the light emitting surface 32a of the light source unit 30-15. Then, the light source 31 was caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the optical substrate 10-1 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 3.

[0160] <17. Example 16> (17-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-2 was placed on the light emitting surface 32a of the light source unit 30-15 to produce the optical unit 1a. The light source 31 was then caused to emit light, and the total light transmittance and diffusion angle of the transmitted light that had passed through the resin laminated optical body 1-2 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 3.

[0161] <18. Example 17> (18-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-4 was placed on the light emitting surface 32a of the light source unit 30-15 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that passed through the resin laminated optical body 1-4 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 3.

[0162] <19. Example 18> (19-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-3 was placed on the light emitting surface 32a of the light source unit 30-15 to produce the optical unit 1a. Then, the light source 31 was made to emit light, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-3 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 3.

[0163] [Table 3]

[0164] In Table 3, lenses 1 and 2 refer to optical substrates 32 and 10-1, respectively. The "lens integrated" of the diffusion plate means that a light diffusion structure is integrated with at least one of optical substrates 10-1 and 32 (i.e., a resin layer having a light diffusion structure is formed). "Untreated" means that a resin layer is not formed. "Anti-reflective" means that a moth-eye structure is formed. "Diffusion" means that a light diffusion structure is formed.

[0165] <20. Example 19> In Examples 19 to 22 and Comparative Example 2, tests were carried out to evaluate the optical characteristics of the image display device 2000 (particularly the periphery of the light irradiation device 2010) shown in Fig. 24. This will be described in detail below.

[0166] (20-1. Measurement of total light transmittance and diffusion angle) A raster scan type laser irradiation device was prepared as the light irradiation device 2010. A resin laminated optical body 1-6 was placed on the optical path of this light irradiation device 2010. Here, the surface of the resin laminated optical body 1-6 (the surface of the optical substrate 10-1) was directed toward the display unit 2020. Then, light was emitted from the light irradiation device 2010, and the total light transmittance and diffusion angle of the transmitted light that passed through the resin laminated optical body 1-6 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 4.

[0167] <21. Example 20> (21-1. Measurement of total light transmittance and diffusion angle) A resin laminated optical body 1-9 was placed on the optical path of the light irradiation device 2010. Here, the surface of the resin laminated optical body 1-9 (the surface of the optical substrate 10-1) was directed toward the display unit 2020. Then, light was emitted from the light irradiation device 2010, and the total light transmittance and diffusion angle of the transmitted light that passed through the resin laminated optical body 1-9 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 4.

[0168] <22. Example 21> (22-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-11 was placed on the optical path of the light irradiation device 2010. Here, the surface of the resin laminated optical body 1-11 (the surface of the optical substrate 10-1) was directed toward the display unit 2020. Then, light was emitted from the light irradiation device 2010, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-11 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 4.

[0169] <23. Example 22> (21-1. Measurement of total light transmittance and diffusion angle) The resin laminated optical body 1-13 was placed on the light path of the light irradiation device 2010. Here, the surface of the resin laminated optical body 1-13 (the surface of the optical substrate 10-1) was directed toward the display unit 2020. Then, light was emitted from the light irradiation device 2010, and the total light transmittance and diffusion angle of the transmitted light that was transmitted through the resin laminated optical body 1-13 were measured. The measurement conditions were the same as in Example 1. The results are summarized in Table 4.

[0170] <24. Comparative Example 2> (24-1. Measurement of total light transmittance and diffusion angle) A light diffusion plate and an optical substrate 10-1 were arranged in this order on the light path of the light irradiation device 2010. The light diffusion plate was the same as that used in Example 1. Here, the surface of the optical substrate 10-1 was directed toward the display unit 2020. Then, light was emitted from the light irradiation device 2010, and the total light transmittance and diffusion angle of the transmitted light that had passed through the optical substrate 10-1 were measured. The measurement conditions were the same as those in Example 1. The results are summarized in Table 4.

[0171] [Table 4]

[0172] In Table 4, lens means the optical substrate 10-1. The "lens integrated" of the diffusion plate means that the light diffusion structure is integrated with the optical substrate 10-1 (i.e., a resin layer having a light diffusion structure is formed). "Separately placed" means that the light diffusion plate and the optical substrate 10-1 are separate. "Untreated" means that no resin layer is formed. "Anti-reflective" means that a moth-eye structure is formed. "Diffusion" means that a light diffusion structure is formed.

[0173] <25. Example 23> In Example 23 and Comparative Example 3, a test was carried out to evaluate the optical characteristics of the image display device 3000 shown in Fig. 25. This will be described in detail below.

[0174] (25-1. Preparation of optical substrate) As the optical substrate 10 for a mirror (hereinafter also referred to as "optical substrate 10-2"), an aluminum metal film was formed by vacuum deposition on a cycloolefin polymer (ZEONEX 480R manufactured by ZEON Corporation) substrate.

[0175] (25-2. Preparation of resin laminated optical body) By carrying out the above-mentioned first to sixth steps and the peeling step using the flexible master 400-2, a resin layer 20 was formed on the reflective surface (the surface on which the curved surface 11 was formed) of the optical substrate 10-2. In this way, a resin laminated optical body 1-23 was produced. A light diffusing structure was formed as a fine uneven structure 50 on the surface 21 of the resin layer 20.

[0176] (25-3. Evaluation of luminance unevenness) A white LED was prepared as the light irradiation device 3010. The light irradiation device 3010, the liquid crystal panel 3015, the mirror 3020, and the display unit 3030 were arranged in the image display device 3000. Here, the resin laminated optical body 1-23 was used as the mirror 3020. Then, light was emitted from the light irradiation device 3010, and the reflected light reflected by the resin laminated optical body 1-23 was made to enter the display unit 3030. Thereby, a virtual image was displayed on the display unit 3030. The luminance difference between the central luminance of this virtual image and the luminance of the outer edge was measured. The luminance was measured using a CS-2000 manufactured by Konica Minolta. The luminance of the outer edge was taken as the arithmetic average value of the values ​​measured at a plurality of measurement points. Next, when the luminance difference was 10% or less of the central luminance, the luminance unevenness was judged to be acceptable (low luminance unevenness), and when the luminance difference was more than 10% of the central luminance, the luminance unevenness was judged to be unacceptable (high luminance unevenness). The luminance unevenness was at an acceptable level in Example 23. The results are summarized in Table 5.

[0177] <26. Comparative Example 3> The same test as in Example 23 was carried out except that the resin laminated optical body 1-23 was replaced with the optical substrate 10-2. In Comparative Example 3, the luminance unevenness was at an unacceptable level. The results are summarized in Table 5.

[0178] [Table 5]

[0179] In Table 5, mirror refers to mirror 3020. "No diffusion" means that no light diffusion structure is formed on optical substrate 10-2. "Diffusion" means that a light diffusion structure is formed on optical substrate 10-2. "◯" for brightness unevenness indicates "pass" and "×" indicates "fail."

[0180] <27. Example 24> In Examples 24 to 26 and Comparative Example 4, tests were carried out to evaluate the optical characteristics of the image display device 4000 shown in Fig. 26. The following will explain in detail.

[0181] (27-1. Evaluation of luminance unevenness) A white LED was prepared as the light irradiation device 4010. The light irradiation device 4010, the liquid crystal panel 4015, the mirrors 4020 and 4030, and the display unit 4040 were arranged in the image display device 4000. Here, the resin laminated optical body 1-23 was used as the mirror 4020, and the optical substrate 10-2 was used as the mirror 4030. Then, light was emitted from the light irradiation device 4010, and the reflected light reflected by the resin laminated optical body 1-23 was made to enter the display unit 4040. Thereby, a virtual image was displayed on the display unit 4040. The luminance difference between the central luminance and the luminance of the outer edge of this virtual image was measured. The luminance measurement was performed in the same manner as in Example 23. Next, when the luminance difference was 10% or less of the central luminance, the luminance unevenness was judged to be acceptable (low luminance unevenness), and when the luminance difference was more than 10% of the central luminance, the luminance unevenness was judged to be unacceptable (high luminance unevenness). In Example 24, the luminance unevenness was at an acceptable level. The results are summarized in Table 6.

[0182] <28. Example 25> (28-1. Evaluation of luminance unevenness) The same test as in Example 24 was carried out except that the optical substrate 10-2 was used as the mirror 4020 and the resin laminated optical body 1-23 was used as the mirror 4030. The luminance unevenness was at an acceptable level. The results are summarized in Table 6.

[0183] <29. Example 26> (29-1. Evaluation of luminance unevenness) The same test as in Example 24 was carried out except that the resin laminated optical body 1-23 was used as the mirrors 4020 and 4030. The luminance unevenness was at an acceptable level. The results are summarized in Table 6.

[0184] <30. Comparative Example 4> The same test as in Example 24 was carried out except that the optical substrate 10-2 was used as the mirrors 4020 and 4030. The luminance unevenness was at an unacceptable level. The results are summarized in Table 6.

[0185] [Table 6]

[0186] In Table 6, mirrors 1 and 2 respectively represent mirrors 4020 and 4030. Other notations are the same as in Table 5.

[0187] As is clear from Examples 1 to 26 and Comparative Examples 1 to 4, the light emission quality was improved in Examples 1 to 26 which satisfied the requirements of this embodiment.

[0188] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. [Explanation of symbols]

[0189] 1. Resin laminated optical body 10 Optical substrate 20 Resin layer 30 Light source unit 31 Light source 32 Optical substrate 40 Resin layer 50 Fine uneven structure

Claims

1. An optical substrate; A first resin layer provided on a surface of the optical substrate; A second resin layer provided on the back surface of the optical substrate; A first fine uneven structure formed on the first resin layer; a second microrelief structure formed on the second resin layer; Equipped with The surface of the optical substrate is a curved surface, A resin laminated optical body, wherein the first microrelief structure formed on the first resin layer and the second microrelief structure formed on the second resin layer are different types of microrelief structures.

2. The first microrelief structure is a light diffusion structure, The resin laminated optical body according to claim 1 , wherein the second fine uneven structure is a moth-eye structure.

3. the optical substrate is a plano-convex lens, The resin laminated optical body according to claim 1 , wherein the front surface of the optical substrate is a convex surface, and the back surface of the optical substrate is a flat surface.

4. the optical substrate is a plano-concave lens, The resin laminated optical body according to claim 1 , wherein the front surface of the optical substrate is a concave surface, and the back surface of the optical substrate is a flat surface.

5. The optical substrate is a biconvex lens, The resin laminated optical body according to claim 1 , wherein the front surface of the optical substrate is a convex surface, and the back surface of the optical substrate is a convex surface.

6. the optical substrate is a biconcave lens, The resin laminated optical body according to claim 1 , wherein the front surface of the optical substrate is a concave surface, and the back surface of the optical substrate is a concave surface.

7. The optical substrate is a concave-convex lens, The resin laminated optical body according to claim 1 , wherein the front surface of the optical substrate is a convex surface, and the back surface of the optical substrate is a concave surface.

8. A method for producing the resin laminated optical body according to any one of claims 1 to 7, A first step of preparing an optical substrate having a curved surface; a second step of forming an uncured resin layer on the curved surface of the optical substrate; a third step of preparing a flexible master having a surface on which an inverted structure of the first microrelief structure is formed and having flexibility; a fourth step of bringing the flexible master into proximity with the uncured resin layer; a fifth step of pressing the inverted structure of the flexible master against the uncured resin layer while deforming the flexible master by applying a printing pressure to the flexible master; a sixth step of forming a first resin layer on the curved surface of the optical substrate by curing the uncured resin layer while pressing the inverted structure of the flexible master against the uncured resin layer; A method for producing a resin laminated optical body, comprising:

9. The first microrelief structure is a light diffusion structure, 9. The method for producing a resin laminated optical body according to claim 8, wherein an average interval between fine recesses or an average interval between fine protrusions constituting the first fine uneven structure is 1 to 150 μm.

10. 10. The method for producing a resin laminated optical body according to claim 9, wherein a height difference between adjacent fine recesses and fine protrusions in the first fine concave-convex structure is 0.5 to 50 μm.

Citation Information

Patent Citations

  • Antireflection article

    JP2003215314A

  • Forming method for minute irregularity on curved surface, and optical member

    JP2004155083A

  • Method for forming antireflection film, apparatus for forming antireflection film, antireflection film and optical component

    JP2006039450A

  • Manufacturing method of scratch-resistant resin plate having glare-proof property

    JP2008296428A

  • Optical element and optical system having the same

    JP2010269957A