Polarizer protective film, polarizing plate, and image display device

A polarizer protective film with controlled water absorption and optical alignment addresses durability and color unevenness issues in humid environments, enhancing the performance of polarizing plates in image display devices.

JP2024159986AInactive Publication Date: 2024-11-08NITTO DENKO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024150812
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-26
Filing Date
2024-09-02
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polarizing plates with colored layers exhibit poor durability in humid environments and suffer from color unevenness on the display screen.

Method used

A polarizer protective film made of a resin containing a dye with a water absorption rate of 3.0% or less, combined with specific optical properties and alignment, is used to enhance durability and reduce color unevenness.

Benefits of technology

The solution provides a polarizing plate with improved durability in humid conditions and reduced color unevenness by using a resin film with controlled water absorption and optical alignment, maintaining high visible light transmission and polarization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159986000001_ABST
    Figure 2024159986000001_ABST
Patent Text Reader

Abstract

To provide a polarizer protective film improved in durability under a humidification environment.SOLUTION: There are provided: a polarizer protective film which is a resin film containing pigment and has a water absorption of 3.0% or less; and polarizing plate which includes a polarizer and the polarizer protective film placed at least on one side of the polarizer, and in which a rate of change of visible light transmission under the environment of 90%RH at 65°C after 96 hours is 10% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizer protective film, and a polarizing plate and an image display device each using the polarizer protective film. [Background technology]

[0002] In a liquid crystal display device, which is one of the representative image display devices, polarizing plates are attached to both sides of a liquid crystal cell due to its image formation method. A polarizing plate usually includes a polarizer and a protective film for protecting the polarizer, and from the viewpoint of improving the viewing angle, it can be used as a polarizing plate with a retardation layer that further includes a retardation layer. In addition, an organic electroluminescence (EL) display device is provided with a circular polarizing plate on the viewing side to prevent problems such as external light reflection and background reflection caused by the high reflectivity of an organic EL cell. A typical circular polarizing plate is known to be one in which a polarizer and a retardation layer (typically a λ / 4 plate) are laminated so that the slow axis of the retardation layer forms an angle of about 45° with respect to the absorption axis of the polarizer.

[0003] It has been proposed to provide a colored layer on the polarizing plate to obtain high polarization characteristics and good reflection characteristics over a wide band (for example, Patent Document 1, Patent Document 2, etc.). However, a polarizing plate provided with a colored layer may have poor durability in a humid environment.

[0004] As described above, it is known that the viewing angle of an image display device can be improved by using a polarizing plate with a retardation layer. However, in such an image display device, differences in color (color unevenness) may be visible on the display screen. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO2018 / 110503 [Patent Document 2] JP 2018-72712 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above-mentioned problems in the prior art, and a main object of the present invention is to provide a polarizing plate having improved durability in a humid environment. Another object of the present invention is to improve color unevenness on a display screen. [Means for solving the problem]

[0007] According to one aspect of the present invention, there is provided a polarizer protective film which is a resin film containing a dye and has a water absorption rate of 3.0% or less. In one embodiment, the polarizer protective film contains at least one resin selected from the group consisting of polyethylene terephthalate-based resins, acrylic-based resins, polycarbonate-based resins, and cycloolefin-based resins. In one embodiment, the polarizer protective film has a front retardation Re(550) of 90 nm to 160 nm or 200 nm to 320 nm. In one embodiment, the polarizer protective film is a stretched resin film. In one embodiment, the polarizer protective film has a slow axis in a direction of 20° to 60° or 110° to 150° clockwise when the longitudinal direction is taken as 0°. In one embodiment, the polarizer protective film has a haze of 3% or less. According to another aspect of the present invention, there is provided a polarizing plate having a polarizer and the above-mentioned polarizer protective film arranged on at least one side of the polarizer, wherein the change in visible light transmittance after 96 hours in an environment of 65°C and 90% RH is 10% or less. In one embodiment, in the polarizing plate, the polarizer and the polarizer protective film are attached to each other via an ultraviolet-curable adhesive. In one embodiment, the polarizing plate has a visible light transmittance of 20% or more. In one embodiment, the polarizer protective film has a front retardation Re(550) of 90 nm to 160 nm, and the angle between the absorption axis direction of the polarizer and the slow axis of the polarizer protective film is 35° to 55° in a clockwise or counterclockwise direction. In one embodiment, the polarizer has a long shape, the polarizer protective film is a long obliquely stretched film, and the polarizer and the polarizer protective film are attached to each other with their longitudinal directions aligned. According to another aspect of the present invention, there is provided an image display device including the above polarizing plate. Effect of the Invention

[0008] According to the present invention, a polarizing plate having improved durability in a humid environment can be obtained by using a polarizer protective film which is a resin film containing a dye and has a water absorption rate of 3.0% or less. Also, by arranging the polarizing plate so that the polarizer protective film is closer to the optical cell than the polarizer, an image display device with improved color unevenness on the display screen can be obtained. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating a polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating a polarizing plate according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view illustrating a polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0011] (Definition of terms and symbols) The terms and symbols used in this specification are defined as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re.

[0012] A. Polarizer protection film The polarizer protective film according to the embodiment of the present invention is a resin film containing a dye and has a water absorption rate of 3.0% or less. Conventional polarizing plates provided with a colored layer are subject to large changes in physical properties due to the environment, and problems such as dye loss can occur in a humid environment. However, by incorporating a dye into the polarizer protective film and setting the water absorption rate to a predetermined value or less, a polarizing plate in which changes in physical properties in a humid environment are suppressed can be obtained.

[0013] The water absorption rate of the polarizer protective film is typically 3.0% or less, preferably 2.5% or less, more preferably 2.0% or less, and even more preferably 0% to 1.5%. When the water absorption rate of the polarizer protective film is within this range, pigment loss and the like that may occur due to moisture entering and leaving the colored layer (polarizer protective film) is suppressed, and as a result, a polarizing plate in which changes in physical properties in a humid environment are suppressed can be obtained. The water absorption rate of the polarizer protective film can be determined in accordance with JIS K 7209.

[0014] A-1. Resin film As the resin forming the resin film, any suitable resin capable of realizing the desired water absorption rate is used. Specific examples of the resin forming the resin film include polyester-based resins such as polyethylene terephthalate, (meth)acrylic resins, cycloolefin-based resins such as polynorbornene, polycarbonate-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polysulfone-based resins, and the like. Among them, polyethylene terephthalate resins, (meth)acrylic resins, polycarbonate-based resins, and cycloolefin-based resins are preferred because they have excellent stability in a humid environment (in other words, they can suitably achieve a water absorption rate of 3% or less). Note that "(meth)acrylic resins" refers to acrylic resins and / or methacrylic resins.

[0015] As the (meth)acrylic resin, a (meth)acrylic resin having a cyclic structure such as a lactone ring or a glutarimide ring in the main chain is preferably used. (Meth)acrylic resins having a glutarimide ring (hereinafter also referred to as glutarimide resins) are described in, for example, JP 2006-309033 A, JP 2006-317560 A, JP 2006-328329 A, JP 2006-328334 A, JP 2006-337491 A, JP 2006-337492 A, JP 2006-337493 A, JP 2006-337569 A, JP 2007-009182 A, JP 2009-161744 A, and JP 2010-284840 A. These descriptions are incorporated herein by reference.

[0016] As the polycarbonate-based resin, preferably, an aromatic polycarbonate is used. The aromatic polycarbonate can be obtained, typically, by the reaction of a carbonate precursor with an aromatic dihydric phenol compound. Specific examples of the carbonate precursor include phosgene, bischloroformate of dihydric phenols, diphenyl carbonate, di-p-tolyl carbonate, phenyl-p-tolyl carbonate, di-p-chlorophenyl carbonate, dinaphthyl carbonate, etc. Among these, phosgene and diphenyl carbonate are preferred. Specific examples of aromatic dihydric phenol compounds include 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)butane, 2,2-bis(4-hydroxy-3,5-dipropylphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, etc. These may be used alone or in combination of two or more. Preferably, 2,2-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane are used. In particular, it is preferable to use 2,2-bis(4-hydroxyphenyl)propane and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane together.

[0017] The cycloolefin resin is not particularly limited as long as it is a resin having a monomer unit made of a cyclic olefin (cycloolefin), and may be, for example, a cycloolefin polymer (COP) or a cycloolefin copolymer (COC). A cycloolefin copolymer is a non-crystalline cyclic olefin resin that is a copolymer of a cyclic olefin and an olefin such as ethylene.

[0018] The cyclic olefins include polycyclic cyclic olefins and monocyclic cyclic olefins.The polycyclic cyclic olefins include norbornene, methylnorbornene, dimethylnorbornene, ethylnorbornene, ethylidenenorbornene, butylnorbornene, dicyclopentadiene, dihydrodicyclopentadiene, methyldicyclopentadiene, dimethyldicyclopentadiene, tetracyclododecene, methyltetracyclododecene, dimethylcyclotetradodecene, tricyclopentadiene, tetracyclopentadiene, etc.The monocyclic cyclic olefins include cyclobutene, cyclopentene, cyclooctene, cyclooctadiene, cyclooctatriene, cyclododecatriene, etc.

[0019] The cycloolefin resin is also available as a commercially available product, and examples thereof include Topas manufactured by Ticona, Arton manufactured by JSR Corporation, ZEONOR and ZEONEX manufactured by Zeon Corporation, and APEL manufactured by Mitsui Chemicals.

[0020] The resin film may be composed of a single layer or may have a multi-layer structure. The resin film having a multi-layer structure can be obtained by any appropriate production method such as an extrusion method or a lamination method.

[0021] A-2. Pigments Specific examples of the dye include anthraquinone-based, triphenylmethane-based, naphthoquinone-based, thioindigo-based, perinone-based, perylene-based, squarylium-based, cyanine-based, porphyrin-based, azaporphyrin-based, phthalocyanine-based, subphthalocyanine-based, quinizarin-based, polymethine-based, rhodamine-based, oxonol-based, quinone-based, azo-based, xanthene-based, azomethine-based, quinacridone-based, dioxazine-based, diketopyrrolopyrrole-based, anthrapyridone-based, isoindolinone-based, indanthrone-based, indigo-based, thioindigo-based, quinophthalone-based, quinoline-based, triphenylmethane-based dyes, etc. Dyes can be preferably used because they are well compatible with the resin film, which is the matrix.

[0022] In one embodiment, an anthraquinone-based, oxime-based, naphthoquinone-based, quinizarin-based, oxonol-based, azo-based, xanthene-based, or phthalocyanine-based dye is used as the dye. By using these dyes, a polarizer protective film having an absorption maximum wavelength in the wavelength band of 440 nm to 510 nm can be formed.

[0023] In one embodiment, an indigo-based, rhodamine-based, quinacridone-based or porphyrin-based dye is used as the coloring matter. By using these dyes, it is possible to form a polarizer protective film having an absorption maximum wavelength in the wavelength band of 560 nm to 610 nm.

[0024] Pigments may also be used as the coloring matter. Specific examples of pigments include black pigments (carbon black, bone black, graphite, iron black, titanium black, etc.), azo pigments, phthalocyanine pigments, polycyclic pigments (quinacridones, perylenes, perinones, isoindolinones, isoindolines, dioxazines, thioindigo, anthraquinones, quinophthalones, metal complexes, diketopyrrolopyrroles, etc.), dye lake pigments, white extender pigments (titanium oxide, zinc oxide, sulfur, etc.), and the like. Examples of pigments that can be used include zinc oxide, clay, talc, barium sulfate, calcium carbonate, etc.), chromatic pigments (yellow lead, cadmium-based, chrome vermilion, nickel titanium, chrome titanium, yellow iron oxide, red iron oxide, zinc chromate, red lead, ultramarine, Prussian blue, cobalt blue, chrome green, chromium oxide, bismuth vanadate, etc.), lustrous pigments (pearl pigments, aluminum pigments, bronze pigments, etc.), and fluorescent pigments (zinc sulfide, strontium sulfide, strontium aluminate, etc.).

[0025] The content ratio of the dye can be any appropriate ratio depending on the type of dye, the desired light absorption characteristics, etc. The content ratio of the color material is, for example, 0.01 to 5.0 parts by weight, more preferably 0.05 to 2.0 parts by weight, and even more preferably 0.10 to 1.0 parts by weight, relative to 100 parts by weight of the matrix resin (resin film).

[0026] A-3. Optical properties of polarizer protection film In one embodiment, the polarizer protective film selectively absorbs light in a specific wavelength range (i.e., has a maximum absorption wavelength in a specific wavelength band). In another embodiment, the polarizer protective film functions to absorb all wavelengths in the visible light region. Preferably, the polarizer protective film selectively absorbs light in a specific wavelength range. A polarizer protective film that selectively absorbs light in a specific wavelength range can enhance the anti-reflection function while suppressing a decrease in visible light transmittance (i.e., a decrease in brightness). In addition, by adjusting the wavelength of the light to be absorbed, the reflection hue of the polarizing plate described in section B can be made neutral.

[0027] In one embodiment, the polarizer protective film has an absorption maximum wavelength in a wavelength band ranging from 440 nm to 510 nm and / or from 560 nm to 610 nm. A polarizer protective film having two or more absorption maximum wavelengths can be obtained, for example, by containing a plurality of types of dyes.

[0028] The transmittance of the polarizer protective film at the absorption maximum wavelength is preferably from 0% to 80%, and more preferably from 0% to 70%.

[0029] The visible light transmittance of the polarizer protective film is preferably 30% to 90%, and more preferably 30% to 80%.

[0030] The haze of the polarizer protective film is preferably 3% or less, more preferably 2% or less, further preferably 1% or less, and even more preferably 0% to 0.5%. When the haze of the polarizer protective film is within this range, the polarization of light passing through the polarizer protective film is maintained, and a polarizing plate with a high degree of polarization can be obtained.

[0031] In one embodiment, the polarizer protective film is optically anisotropic and can also function as a retardation film. The in-plane retardation Re(550) of the polarizer protective film that can function as a retardation film can be appropriately set according to the purpose. For example, the polarizer protective film can function as a λ / 4 plate or a λ / 2 plate. Hereinafter, the case where the polarizer protective film is a λ / 4 plate or a λ / 2 plate will be described.

[0032] When the polarizer protective film is a λ / 4 plate, its in-plane retardation Re(550) is preferably 90 nm to 160 nm, more preferably 120 nm to 160 nm, and further preferably 135 nm to 155 nm. The λ / 4 plate typically has an index ellipsoid of nx>ny=nz or nx>ny>nz. In this specification, for example, "ny=nz" includes not only strictly equal but also substantially equal. The Nz coefficient is, for example, 0.9 to 2, preferably 1 to 1.5, and more preferably 1 to 1.3.

[0033] The thickness of the polarizer protective film functioning as a λ / 4 plate can be set so that it can function most appropriately as a λ / 4 plate. In other words, the thickness can be set so that a desired in-plane retardation can be obtained. Specifically, the thickness is preferably 10 μm to 80 μm, more preferably 10 μm to 60 μm, and most preferably 30 μm to 50 μm.

[0034] The λ / 4 plate may exhibit a reverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value hardly changes depending on the wavelength of the measurement light. As described above, since the polarizer protective film contains a dye, the hue shift can be suppressed by adjusting the type and amount of the dye, regardless of the wavelength dispersion characteristic.

[0035] The λ / 4 plate is preferably a stretched film of a resin film containing a dye. The stretched direction of the stretched film is not limited, and may be, for example, the longitudinal direction and / or the width direction or the oblique direction. Examples of the stretching method include transverse uniaxial stretching, fixed-end biaxial stretching, and sequential biaxial stretching. A specific example of fixed-end biaxial stretching is a method in which a resin film is stretched in the short direction (width direction) while running in the longitudinal direction. This method may appear as transverse uniaxial stretching. In addition, by employing oblique stretching, a long stretched film having an orientation axis (slow axis) at a predetermined angle with respect to the width direction can be obtained. Specific examples of the oblique stretching method are described in, for example, WO2012 / 053218, WO2016 / 047465, JP2013-97216A, and the like. These descriptions are incorporated herein by reference.

[0036] The λ / 4 plate obtained by oblique stretching has an orientation axis (slow axis) in a direction of preferably 20° to 60°, more preferably 35° to 55°, even more preferably 38° to 52°, even more preferably 40° to 50°, even more preferably 42° to 48°, and particularly preferably 44° to 46° clockwise, or preferably 110° to 150°, more preferably 128° to 142°, even more preferably 130° to 140°, even more preferably 132° to 138°, and particularly preferably 134° to 136°, when the longitudinal direction is taken as 0°.

[0037] When the polarizer protective film is a λ / 2 plate, its in-plane retardation Re(550) is preferably 200 nm to 320 nm, more preferably 210 nm to 280 nm, and most preferably 230 nm to 240 nm. The λ / 2 plate typically has an index ellipsoid of nx>ny=nz. The Nz coefficient of the λ / 2 plate is, for example, 0.9 to 2, preferably 1 to 1.5, and more preferably 1 to 1.3.

[0038] The thickness of the polarizer protective film functioning as a λ / 2 plate can be set so that it can function most appropriately as a λ / 2 plate. In other words, the thickness can be set so that a desired in-plane retardation can be obtained. Specifically, the thickness is preferably 10 μm to 80 μm, more preferably 10 μm to 60 μm, and most preferably 30 μm to 50 μm.

[0039] The λ / 2 plate may exhibit a reverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, may exhibit a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or may exhibit a flat wavelength dispersion characteristic in which the retardation value changes little depending on the wavelength of the measurement light. As described above, since the polarizer protective film contains a dye, the hue shift can be suppressed by adjusting the type and amount of the dye, regardless of the wavelength dispersion characteristic.

[0040] The λ / 2 plate is preferably a stretched film of a resin film containing the above-mentioned dye. As a method for stretching the resin film, the same stretching methods as those exemplified in the case where the polarizer protective film is a λ / 4 plate can be used.

[0041] The λ / 2 plate obtained by oblique stretching has an orientation axis (slow axis) in a clockwise or counterclockwise direction, preferably at an angle of 10° to 20°, more preferably at an angle of 13° to 17°, and particularly preferably at about 15°, when the longitudinal direction is taken as 0°.

[0042] In another embodiment, the polarizer protective film is optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the retardation Rth(550) in the thickness direction is -10 nm to +10 nm. In this embodiment, the polarizer protective film has a thickness of preferably 10 μm to 80 μm, more preferably 15 μm to 60 μm, and further preferably 20 μm to 40 μm.

[0043] B. Polarizing plate A polarizing plate according to an embodiment of the present invention includes a polarizer and the polarizer protective film (hereinafter, colored polarizer protective film) described in Section A arranged on at least one side of the polarizer. The visible light transmittance of the polarizing plate is preferably 20% or more, more preferably 25% or more, and even more preferably 30% to 50%. The polarization degree of the polarizing plate is 99.9% or more, and preferably 99.95% or more.

[0044] The change rate of the visible light transmittance of the polarizing plate after 96 hours in an environment of 65°C and 90% RH is typically 10% or less, preferably 5.0% or less, more preferably 3.0% or less, even more preferably 2.0% or less, and even more preferably 0% to 1.0%. By using a resin film containing a dye and having low water absorption as a polarizer protective film, a polarizing plate having excellent durability in a humid environment can be obtained. The change rate of the visible light transmittance is calculated based on the following formula. Change in visible light transmittance (%) = (visible light transmittance after 96 hours - initial visible light transmittance) / initial visible light transmittance x 100

[0045] 1 and 2 are schematic cross-sectional views of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100a has a polarizer 10 and a colored polarizer protective film 20 arranged on one side thereof. The polarizing plate 100b has a polarizer 10, a colored polarizer protective film 20 arranged on one side thereof, and a second polarizer protective film 30 arranged on the other side thereof. The second polarizer protective film 30 may be a colored polarizer protective film or may be a normal polarizer protective film (a polarizer protective film that does not contain a dye).

[0046] Although not shown, the colored polarizer protective film 20 is typically laminated on the surface of the polarizer 10 via an adhesive layer. The second polarizer protective film 30 is laminated on the surface of the polarizer 10 via an adhesive layer or in close contact without an adhesive layer. As the adhesive layer, any appropriate pressure-sensitive adhesive layer or adhesive layer may be used. The pressure-sensitive adhesive layer is typically formed of an acrylic pressure-sensitive adhesive. The adhesive layer is typically formed of an ultraviolet-curing adhesive or a polyvinyl alcohol adhesive.

[0047] Any suitable polarizer is used as the polarizer 10. For example, a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film is uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye, or a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride. Among these, a polarizer obtained by adsorbing a dichroic substance such as iodine to a polyvinyl alcohol film and uniaxially stretching the film is particularly preferred because it has a high polarization dichroic ratio. The thickness of the polarizer is preferably 0.5 μm to 80 μm.

[0048] A polarizer obtained by uniaxially stretching a polyvinyl alcohol-based film after adsorbing iodine is typically produced by dyeing the polyvinyl alcohol by immersing it in an aqueous solution of iodine and stretching it to 3 to 7 times its original length. Stretching may be performed after dyeing, or may be performed while dyeing, or may be performed after stretching and dyeing. In addition to stretching and dyeing, the polarizer may be produced by performing treatments such as swelling, crosslinking, adjustment, water washing, and drying. For example, by immersing the polyvinyl alcohol-based film in water before dyeing and washing it with water, it is possible to clean the stains and antiblocking agent on the surface of the polyvinyl alcohol-based film, and also to swell the polyvinyl alcohol-based film and prevent uneven dyeing. The polyvinyl alcohol-based film may be a single-layer film (a film formed from a normal film), or may be a polyvinyl alcohol-based resin layer formed by coating on a resin substrate. The technology for producing a polarizer from a single-layer polyvinyl alcohol-based film is well known in the art. A technique for producing a polarizer from a polyvinyl alcohol-based resin layer formed by coating on a resin substrate is described in, for example, JP-A-2009-098653.

[0049] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm.The single transmittance of the polarizer is preferably 38% to 45.5%, and more preferably 40% to 45%.

[0050] The degree of polarization of the polarizer is preferably 99.9% or more, and more preferably 99.95% or more.

[0051] In the case of a polarizer protective film not containing a dye, the second polarizer protective film 30 is formed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.

[0052] When the polarizing plate is applied to an image display device, and the second polarizer protective film is disposed on the opposite side to the optical cell (when the film is an outer protective layer), the thickness of the second polarizer protective film is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. When the film is surface-treated, the thickness of the outer protective layer includes the thickness of the surface treatment layer.

[0053] When the polarizing plate is applied to an image display device, in the case where the second polarizer protective film is placed on the optical cell side (when it is an inner protective layer), the thickness of the second polarizer protective film is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and even more preferably 10 μm to 60 μm.

[0054] The colored polarizer protective film 20 is the polarizer protective film described in section A as described above. When the colored polarizer protective film is optically anisotropic and also functions as a retardation film, the polarizing plate 100a or 100b is a retardation layer-attached polarizing plate. By disposing such a retardation layer-attached polarizing plate on the viewing side of the optical cell so that the colored polarizer protective film (retardation layer) is closer to the optical cell than the polarizer, the viewing angle can be improved and color unevenness on the screen can be suppressed. This effect is particularly noticeable when the colored polarizer protective film is a wide obliquely stretched film (for example, an obliquely stretched film having a width of 600 mm or more, preferably 800 mm to 2000 mm). Specifically, the obliquely stretched film is usually laminated to a polarizer in a so-called roll-to-roll process to form a long polarizing plate, which is then cut to a desired size and attached to the optical cell. Here, polarizing plates for large screens (for example, for screens of 40 inches or more, preferably 50 inches or more) made using wide obliquely stretched films tend to have large retardation unevenness in the plane, especially in the diagonal corners, and the retardation unevenness can cause color unevenness on the screen. In contrast, with the above polarizing plate, the colored polarizer protective film contains a dye, which enables color control independent of retardation, and as a result, color unevenness on the screen can be suppressed. In this specification, the "roll-to-roll process" refers to a method in which long films are continuously bonded together while being transported by rolls, with their longitudinal directions aligned.

[0055] When the colored polarizer protective film 20 functions as a λ / 4 plate, the polarizing plate 100a or 100b can function as a circular polarizing plate by arranging the film so that the angle between the absorption axis of the polarizer 10 and the slow axis of the colored polarizer protective film 20 is, for example, 35° to 55°, preferably 38° to 52°, more preferably 40° to 50°, even more preferably 42° to 48°, and particularly preferably 44° to 46°, clockwise or counterclockwise.

[0056] The circular polarizing plate can also function as an anti-reflection film by, for example, arranging a colored polarizer protective film functioning as a λ / 4 plate on the viewing side of the optical cell so that it is on the viewing side of the polarizer. Specifically, the circular polarizing plate exhibits excellent anti-reflection function by the colored polarizer protective film absorbing light of a specific wavelength. In addition, the colored polarizer protective film selectively absorbs light in a specific wavelength range, so that the reflection hue can be appropriately adjusted and a polarizing plate that can contribute to a wide color gamut of the image display device can be obtained. For example, by using a colored polarizer protective film having an absorption maximum wavelength in the wavelength bands of 440 nm to 510 nm and 560 nm to 610 nm, the mixture of red light and green light, and green light and blue light can be well prevented, and as a result, the color gamut of the image display device can be widened, and bright and vivid image quality can be obtained.

[0057] FIG. 3 is a schematic cross-sectional view of a polarizing plate according to another embodiment of the present invention. The polarizing plate 100c includes a second polarizer protective film 30, a polarizer 10, a colored polarizer protective film 20, and a retardation film 40, in this order. In this embodiment, the colored polarizer protective film 20 functions as a λ / 2 plate. The retardation film 40 is a retardation film that functions as a λ / 4 plate. In the polarizing plate 100c, the angle between the absorption axis of the polarizer 10 and the slow axis of the retardation film 40 is preferably 65° to 85°, more preferably 72° to 78°, and even more preferably about 75°, clockwise or counterclockwise. Furthermore, the angle between the absorption axis of the polarizer 10 and the slow axis of the colored polarizer protective film 20 is preferably 10° to 20°, more preferably 13° to 17°, and even more preferably about 15°, clockwise or counterclockwise. By arranging the two retardation films at the above-mentioned axial angle, a circular polarizing plate having very good circular polarization properties (as a result, very good antireflection properties) in a wide band can be obtained.

[0058] C. Image display device The polarizing plate described in the above item B can be applied to an image display device having an optical cell. Therefore, the present invention includes an image display device having the above polarizing plate. Representative examples of image display devices include a liquid crystal display device having a liquid crystal cell, an organic electroluminescence (EL) display device having an organic EL cell, and the like. Typically, the polarizing plate is disposed on the viewing side of an optical cell such as a liquid crystal cell or an organic EL cell, and can stably exhibit a viewing angle improving effect and / or an anti-reflection effect over a wide band. In addition, by disposing the polarizing plate so that the colored polarizer protective film is closer to the optical cell than the polarizer, a color unevenness suppressing effect can be obtained in addition to the viewing angle improving effect. Note that the liquid crystal cell and the organic EL cell are not characteristic of the present invention, and configurations well known in the industry can be adopted, so detailed explanations are omitted. EXAMPLES

[0059] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.

[0060] (1) Front phase difference The film to be measured was cut into a length of 4 cm and a width of 4 cm to be used as a measurement sample. The in-plane retardation of the measurement sample was measured using an Axoscan manufactured by Axometrics. The measurement wavelength was 550 nm and the measurement temperature was 23°C. (2)Visible light transmittance The polarizing plates prepared in the examples and comparative examples were measured for visible light transmittance using an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, product name "V7000 series"). Specifically, the transmittance Ts of the polarizing plate at wavelengths of 380 nm to 780 nm was measured using an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, V-7100) to obtain the visible light transmittance Ts. This Ts is a Y value measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for visibility. (3) Water absorption rate The colored layers (colored polarizer protective films or colored adhesive layers) used in the examples and comparative examples were measured in accordance with the "Test method for water absorption and boiling water absorption of plastics" described in JIS K 7209. The size of the test piece was a square flat plate with sides of 50 mm, and the test piece was immersed in water at a temperature of 25°C for 24 hours, and the weight change before and after immersion was measured to determine the value. The unit is %. (4) Hayes The colored layers (colored polarizer protective films or colored adhesive layers) used in the examples and comparative examples were measured by the method defined in JIS 7136 using a haze meter (manufactured by Murakami Color Science Laboratory, product name "HN-150"). (5) Thickness The thickness in the width direction was measured at intervals of 10 mm using a thickness tester, and the average value was calculated as the thickness.

[0061] [Example 1] 1. Preparation of Polarizer A long roll of polyvinyl alcohol (PVA) resin film (manufactured by Kuraray, product name "PE3000") with a thickness of 30 μm was uniaxially stretched in the longitudinal direction to 5.9 times its original size using a roll stretching machine while simultaneously undergoing swelling, dyeing, crosslinking, and washing processes, and finally a drying process to produce a polarizer with a thickness of 12 μm. Specifically, the film was stretched 2.2 times during the swelling treatment in pure water at 20°C. Next, the film was stretched 1.4 times during the dyeing treatment in an aqueous solution at 30°C in which the weight ratio of iodine to potassium iodide was 1:7, and the iodine concentration was adjusted so that the single transmittance of the resulting polarizer was 45.0%. Furthermore, a two-stage crosslinking treatment was adopted, and the film was stretched 1.2 times during the first stage crosslinking treatment in an aqueous solution at 40°C in which boric acid and potassium iodide were dissolved. The aqueous solution in the first stage crosslinking treatment had a boric acid content of 5.0% by weight and a potassium iodide content of 3.0% by weight. The film was stretched 1.6 times during the second stage crosslinking treatment in an aqueous solution at 65°C in which boric acid and potassium iodide were dissolved. The aqueous solution in the second stage crosslinking treatment had a boric acid content of 4.3% by weight and a potassium iodide content of 5.0% by weight. The cleaning treatment was performed with an aqueous potassium iodide solution at 20° C. The aqueous solution used for the cleaning treatment had a potassium iodide content of 2.6% by weight. Finally, the film was dried at 70° C. for 5 minutes to obtain a polarizer.

[0062] 2. Preparation of colored polarizer protective film 81.98 parts by mass of isosorbide (hereinafter sometimes abbreviated as "ISB"), 47.19 parts by mass of tricyclodecane dimethanol (hereinafter sometimes abbreviated as "TCDDM"), 175.1 parts by mass of diphenyl carbonate (hereinafter sometimes abbreviated as "DPC"), and 0.979 parts by mass of cesium carbonate 0.2% by mass aqueous solution as a catalyst were charged into a reaction vessel, and in a nitrogen atmosphere, as the first step of the reaction, the heating tank temperature was heated to 150°C and the raw materials were dissolved while stirring as necessary (about 15 minutes). Next, the pressure was changed from normal pressure to 13.3 kPa, and the heating tank temperature was increased to 190°C over one hour, while the generated phenol was extracted from the reaction vessel. After the entire reaction vessel was kept at 190°C for 15 minutes, in the second step, the pressure inside the reaction vessel was set to 6.67 kPa, the heating tank temperature was raised to 230°C in 15 minutes, and the generated phenol was removed from the reaction vessel. As the stirring torque of the stirrer increased, the temperature was raised to 250°C in 8 minutes, and the pressure inside the reaction vessel was allowed to reach 0.200 kPa or less in order to remove the generated phenol. After the predetermined stirring torque was reached, the reaction was terminated, and the reaction product was extruded into water to obtain polycarbonate resin pellets. The obtained polycarbonate resin was vacuum dried at 80°C for 5 hours, and then 0.29 parts by weight of dye (manufactured by Yamada Chemical Co., Ltd., product name FDG-007) per 100 parts by weight of the resin was added at the same time to produce a colored polycarbonate resin film with a thickness of 70 μm using a film-forming device equipped with a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 300 mm, setting temperature: 250°C), a chill roll (setting temperature: 120-130°C) and a winder. Furthermore, the unstretched polycarbonate resin film was subjected to preheating and simultaneous biaxial stretching using a simultaneous biaxial stretching machine to obtain a colored polarizer protective film that functions as a retardation film. The preheating temperature was 145°C. The stretching temperature was 140°C (Tg+10°C), and the stretching ratio in the longitudinal direction was 1.2 times and the stretching ratio in the transverse direction was 1.9 times. The obtained colored polarizer protective film had a thickness of 30 μm, a front retardation Re(550) of 144 nm, and a maximum absorption wavelength of 590 nm, and the slow axis direction was 135° with respect to the longitudinal direction.

[0063] 3. Preparation of Polarizing Plates A TAC film (manufactured by Fujifilm Corporation, product name "TG60UL", thickness: 60 μm) was bonded to one side of the polarizer using a roll-to-roll method via a UV-curable adhesive, and then the colored polarizer protective film was bonded to the other side of the polarizer using a roll-to-roll method via a UV-curable adhesive, thereby obtaining a long-sized polarizing plate 1 having a configuration of protective film / polarizer / colored polarizer protective film.

[0064] An acrylic adhesive layer was provided on the surface of the polarizing plate 1 facing the colored polarizer protective film, and the polarizing plate 1 was attached to an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 1.

[0065] [Example 2] A colored polarizer protective film was obtained in the same manner as in Example 1, except that 0.3 parts by weight of Yamamoto Chemical Industries' product name "PD-320" was used as the dye and the stretching temperature was 139°C (Tg+9°C). The thickness of the obtained colored polarizer protective film was 30 μm, the front retardation Re(550) was 135 nm, and the absorption maximum wavelength was 590 nm. In addition, the slow axis direction was 135° with respect to the longitudinal direction. A long-sized polarizing plate 2 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0066] An acrylic adhesive layer was provided on the surface of the polarizing plate 2 facing the colored polarizer protective film, and the polarizing plate 2 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 2.

[0067] [Example 3] A colored polarizer protective film was obtained in the same manner as in Example 1, except that the amount of dye added was 0.18 parts by weight and the stretching temperature was 142°C (Tg+12°C). The thickness of the obtained colored polarizer protective film was 20 μm, the front retardation Re(550) was 100 nm, and the absorption maximum wavelength was 590 nm. In addition, the slow axis direction was 135° with respect to the longitudinal direction. A long polarizing plate 3 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0068] An acrylic adhesive layer was provided on the protective film (TAC film) side surface of the polarizing plate 3, and the polarizing plate 3 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 3.

[0069] [Example 4] A colored polarizer protective film was obtained in the same manner as in Example 1, except that a norbornene-based polymer (made by JSR Corporation, product name ARTON) was used, the amount of dye added was 0.2 parts by weight, and the stretching temperature was Tg+12 degrees. The thickness of the obtained colored polarizer protective film was 25 μm, the front retardation Re(550) was 100 nm, and the absorption maximum wavelength was 590 nm. In addition, the slow axis direction was 135° with respect to the longitudinal direction. A long polarizing plate 4 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0070] An acrylic adhesive layer was provided on the surface of the protective film (TAC film) side of the polarizing plate 4, and the polarizing plate 4 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 4.

[0071] [Example 5] A colored polarizer protective film was obtained in the same manner as in Example 4, except that the amount of dye added was 0.37 parts by weight and the stretching temperature was Tg+10 degrees. The thickness of the obtained colored polarizer protective film was 40 μm, the front retardation Re(550) was 140 nm, and the absorption maximum wavelength was 590 nm. In addition, the slow axis direction was 135° with respect to the longitudinal direction. A long polarizing plate 5 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0072] An acrylic adhesive layer was provided on the surface of the polarizing plate 5 facing the colored polarizer protective film, and the polarizing plate 5 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 5.

[0073] [Example 6] A colored polarizer protective film was obtained in the same manner as in Example 1, except that the amount of the dye added was 0.36 parts by weight and the stretching temperature was Tg+5 degrees. The thickness of the obtained colored polarizer protective film was 40 μm, the front retardation Re(550) was 270 nm, and the absorption maximum wavelength was 590 nm. In addition, the slow axis direction was 135° with respect to the longitudinal direction. A long polarizing plate 6 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0074] An acrylic adhesive layer was provided on the surface of the protective film (TAC film) side of the polarizing plate 6, and the polarizing plate 6 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 6.

[0075] [Example 7] A colored polarizer protective film was obtained in the same manner as in Example 1, except that an acrylic resin (trade name HTX, manufactured by Kaneka Corporation) was used, and 0.39 parts by weight of a dye manufactured by Yamamoto Chemical Industry Co., Ltd., product name "PD-320" was used. The thickness of the obtained colored polarizer protective film was 40 μm, the front retardation Re(550) was 0 nm, and the absorption maximum wavelength was 590 nm. A long polarizing plate 7 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0076] An acrylic adhesive layer was provided on the surface of the protective film (TAC film) side of the polarizing plate 7, and the polarizing plate 7 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 7.

[0077] [Example 8] A colored polarizer protective film was obtained in the same manner as in Example 1, except that a PET resin was used and 0.18 parts by weight of a dye manufactured by Yamamoto Chemical Industry Co., Ltd., product name "PD-320" was used. The thickness of the obtained colored polarizer protective film was 20 μm, the front retardation Re(550) was 350 nm, and the absorption maximum wavelength was 590 nm. A long polarizing plate 8 having a structure of protective film / polarizer / colored polarizer protective film was obtained in the same manner as in Example 1, except that the above-mentioned colored polarizer protective film was used.

[0078] An acrylic adhesive layer was provided on the surface of the protective film (TAC film) side of the polarizing plate 8, and the polarizing plate 8 was attached to one side of an organic EL panel of 55 inches or more via the acrylic adhesive layer to obtain a laminate 8.

[0079] [Comparative Example 1] 1. Preparation of Polarizer A polarizer was produced in the same manner as in Example 1. 2. Preparation of Retardation Film A retardation film was obtained in the same manner as in the preparation of the colored polarizer protective film of Example 1, except that no dye was added. The thickness of the obtained retardation film was 30 μm, and the front retardation Re(550) was 144 nm. The slow axis direction was 135° with respect to the longitudinal direction. 3. Preparation of colored adhesive layer A colored adhesive was prepared by mixing 100 parts by weight of an acrylic polymer obtained by copolymerizing n-butyl acrylate and a hydroxyl group-containing monomer with 0.3 parts by weight of a radical generator (benzoyl peroxide, manufactured by NOF Corporation, trade name "Niper BMT"), 1 part by weight of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, trade name "Coronate L"), 0.3 parts by weight of a dye (manufactured by Yamada Chemical Co., Ltd., trade name "FDG-007"), and 0.2 parts by weight of a phenol-based antioxidant (manufactured by BASF Japan, trade name "IRGANOX1010"). The above adhesive was coated to a thickness of 20 μm on a PET substrate (manufactured by Mitsubishi Plastics, trade name "MRF38CK") that had been treated to facilitate the peeling of the adhesive, and dried at 155° C. for 2 minutes to obtain a colored adhesive layer. The thickness of the obtained colored adhesive layer was 23 μm, and it had an absorption maximum wavelength at 590 nm. 4. Preparation of Polarizing Plates A TAC film (manufactured by Fujifilm Corporation, product name "TG60UL", thickness: 60 μm) was bonded to one side of the polarizer via a UV-curable adhesive by roll-to-roll method, and then the above-mentioned retardation film was bonded to the other side of the polarizer via a UV-curable adhesive by roll-to-roll method, thereby obtaining a long-sized polarizing plate C1 having a structure of protective film / polarizer / retardation film (also serving as protective film).

[0080] The polarizing plate C1 was attached to one side of an organic EL panel of 55 inches or more via the colored adhesive layer to obtain a laminate C1. At this time, the polarizing plate C1 was laminated so that the retardation film side faced the organic EL panel.

[0081] [Comparative Example 2] 1. Preparation of Polarizer A polarizer was produced in the same manner as in Example 1. 2. Preparation of Retardation Film A retardation film was obtained in the same manner as in the preparation of the colored polarizer protective film of Example 4, except that no dye was added. The thickness of the obtained retardation film was 25 μm, and the front retardation Re(550) was 100 nm. The slow axis direction was 135° with respect to the longitudinal direction. 3. Preparation of colored adhesive layer Except for changing the amount of the dye to 0.29 parts by weight, a colored adhesive layer was obtained in the same manner as in Comparative Example 1. The obtained colored adhesive layer had a thickness of 23 μm and a maximum absorption wavelength at 590 nm. 4. Preparation of Polarizing Plates A TAC film (manufactured by Fujifilm Corporation, product name "TG60UL", thickness: 60 μm) was bonded to one side of the polarizer via a UV-curable adhesive by roll-to-roll technique, and then the above-mentioned retardation film was bonded to the other side of the polarizer via a UV-curable adhesive by roll-to-roll technique, thereby obtaining a long-sized polarizing plate C2 having a structure of protective film / polarizer / retardation film (also serving as protective film).

[0082] The polarizing plate C2 was attached to one side of an organic EL panel of 55 inches or more via the colored adhesive layer to obtain a laminate C2. At this time, the polarizing plate C2 was laminated so that the protective film (TAC film) side faced the organic EL panel.

[0083] [Comparative Example 3] 1. Preparation of Polarizer A polarizer was produced in the same manner as in Example 1. 2. Preparation of Retardation Film A retardation film was obtained in the same manner as in the preparation of the colored polarizer protective film of Example 5, except that no dye was added. The thickness of the obtained retardation film was 40 μm, and the front retardation Re(550) was 140 nm. The slow axis direction was 135° with respect to the longitudinal direction. 3. Preparation of colored adhesive layer A colored adhesive layer was obtained in the same manner as in Comparative Example 1, except that 0.33 parts by weight of a dye manufactured by Yamamoto Chemical Industry Co., Ltd. under the trade name "PD-320" was added. The thickness of the obtained colored adhesive layer was 23 μm, and it had an absorption maximum wavelength at 590 nm. 4. Preparation of Polarizing Plates A TAC film (manufactured by Fujifilm Corporation, product name "TG60UL", thickness: 60 μm) was bonded to one side of the polarizer via a UV-curable adhesive by roll-to-roll technique, and then the above-mentioned retardation film was bonded to the other side of the polarizer via a UV-curable adhesive by roll-to-roll technique, thereby obtaining a long-sized polarizing plate C3 having a structure of protective film / polarizer / retardation film (also serving as protective film).

[0084] The polarizing plate C3 was attached to an organic EL panel of 55 inches or more via the colored adhesive layer to obtain a laminate C3. At this time, the retardation film side of the polarizing plate C3 was laminated so as to face the organic EL panel.

[0085] [Reference example 1] 1. Preparation of Polarizer A polarizer was produced in the same manner as in Example 1. 2. Preparation of Retardation Film A retardation film was obtained in the same manner as in the preparation of the colored polarizer protective film of Example 2, except that no dye was added. The thickness of the obtained retardation film was 30 μm, and the front retardation Re(550) was 135 nm. The slow axis direction was 135° with respect to the longitudinal direction. 3. Preparation of Polarizing Plates A TAC film (manufactured by Fujifilm Corporation, product name "TG60UL", thickness: 60 μm) was bonded to one side of the polarizer via a UV-curable adhesive by roll-to-roll technique, and then the above-mentioned retardation film was bonded to the other side of the polarizer via a UV-curable adhesive by roll-to-roll technique, thereby obtaining a long polarizing plate R1 having a structure of protective film / polarizer / retardation film (also serving as protective film).

[0086] The polarizing plate R1 was attached to one side of an organic EL panel of 55 inches or more via an acrylic adhesive layer to obtain a laminate R1. At this time, the polarizing plate R1 was laminated so that the retardation film side faced the organic EL panel.

[0087] <Reliability Test> The polarizing plates obtained in the examples and comparative examples were placed in an oven at 65°C and 90% RH, and after 96 hours they were removed and the visible light transmittance was measured to determine the rate of change from the initial visible light transmittance (before being placed in the oven).

[0088] <Color unevenness evaluation> The laminates obtained in the examples and comparative examples were visually inspected for in-plane unevenness in the off and on states. A level that was not problematic for practical use was rated as "good," and a level that was visible as an in-plane change in hue was rated as "poor."

[0089] [Table 1]

[0090] As shown in Table 1, the polarizing plate using the colored polarizer protective film of the example has a small change in transmittance in a humid environment and is excellent in stability. In addition, it is found that color unevenness is suppressed by disposing the colored polarizer protective film of the example on the optical cell side of the polarizer. [Industrial Applicability]

[0091] The polarizer protective film of the present invention can be suitably used in the production of a polarizing plate, a circular polarizing plate, or the like. [Explanation of symbols]

[0092] 10 Polarizer 20 Colored polarizer protection film 30 Second polarizer protection film 100 Polarizing Plate

Claims

[Claim 1] A resin film containing a dye, A polarizer protective film having a water absorption rate of 3.0% or less.

Citation Information

Patent Citations