Siloxane polymer having silanol group, and cross-linked body

By synthesizing a siloxane polymer with silanol groups and crosslinking it, a product with low thermal expansion and high glass transition temperature is achieved, addressing the need for thermal stability in specific applications.

JP2024160023AInactive Publication Date: 2024-11-08JNC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024151686
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polymers do not provide a crosslinked product with a low coefficient of thermal expansion in the temperature range of 50°C to 180°C, which is essential for applications requiring thermal stability and minimal expansion.

Method used

A siloxane polymer with silanol groups is synthesized by reacting a silsesquioxane compound with a chain siloxane structure, and the resulting polymer is crosslinked to achieve a thermal expansion coefficient of less than 200 ppm/K in the specified temperature range.

Benefits of technology

The crosslinked product exhibits a low coefficient of thermal expansion and a high glass transition temperature, making it suitable for applications where thermal stability and minimal expansion are critical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160023000001
    Figure 2024160023000001
  • Figure 2024160023000002
    Figure 2024160023000002
  • Figure 2024160023000003
    Figure 2024160023000003
Patent Text Reader

Abstract

To provide a siloxane polymer capable of providing a cross-linked body having a low thermal expansion coefficient in a temperature range of 50°C to 180°C, and to provide the cross-linked body having the low thermal expansion coefficient in the temperature range of 50°C to 180°C.SOLUTION: A siloxane polymer comprises a repeating unit represented by a formula (1). In the formula, R0 is independently 6-20C aryl or 5-6C cycloalkyl; R1 is independently a hydrogen atom, 6-20C aryl, 5-6C cycloalkyl, 7-40C arylalkyl, or 1-40C alkyl; R2 and R3 are each independently 6-20C aryl, 5-6C cycloalkyl, 7-40C arylalkyl, or 1-40C alkyl; p represents a real number of 1 or more; x represents a real number of 1-30; and y1+y2 represents a real number of 1-30, provided that y2 is 0 or more but less than 30.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a siloxane polymer having a silanol group and a crosslinked product thereof. [Background technology]

[0002] Polymers containing silsesquioxanes having a cage structure have attracted attention in various fields because of their unique structure and the expectation of unique effects due to the structure. As a polymer containing such a silsesquioxane skeleton, a silicon-based polymer containing a silsesquioxane skeleton in the main chain is known (see, for example, Patent Document 1). In addition, a silicone film with excellent heat resistance has been developed by introducing a crosslinkable functional group into a silicon compound containing a silsesquioxane skeleton having a cage structure in the main chain to form a crosslinked polymer (Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2006-33307 A [Patent Document 2] JP 2010-116464 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a siloxane polymer capable of providing a crosslinked product having a low thermal expansion coefficient in a temperature range of 50°C to 180°C, and to provide a crosslinked product having a low thermal expansion coefficient in a temperature range of 50°C to 180°C. [Means for solving the problem]

[0005] The present inventors have succeeded in synthesizing a novel siloxane polymer having a silanol group by reacting a silsesquioxane compound with a compound having a chain siloxane structure to generate a siloxane polymer having a hydroxyl group in the main chain, and converting the hydrosilyl group of the siloxane polymer to a silanol group. Furthermore, they have found that a crosslinked body having a thermal expansion coefficient of less than 200 ppm / K in the temperature range of 50°C to 180°C can be obtained by crosslinking the siloxane polymer having a silanol group, thereby completing the present invention.

[0006] That is, the embodiment of the present invention includes the following configurations. [1] A siloxane polymer comprising a repeating unit represented by formula (1). [ka] In the above formula, R 0 each independently represents an aryl having 6 to 20 carbon atoms or a cycloalkyl having 5 to 6 carbon atoms, and any hydrogen atom in the aryl having 6 to 20 carbon atoms and the cycloalkyl having 5 to 6 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms; R 1 each independently represents a hydrogen atom, an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, In the aryl of the arylalkyl, any hydrogen atom may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, and in the alkylene of the arylalkyl having 7 to 40 carbon atoms, any hydrogen atom may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; R 2 and R 3 each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; p represents a real number greater than or equal to 1; x represents a real number from 1 to 30; y1+y2 represents a real number from 1 to 30, and y2 is equal to or greater than 0 and less than 30.

[0007] [2] A siloxane polymer composition comprising the siloxane polymer according to [1], a crosslinking agent, and a transition metal catalyst. [3] The siloxane polymer composition according to [2], which gives a crosslinked product having a maximum linear expansion coefficient calculated in the range from 50°C to 180°C in 10°C increments of less than 200 ppm / K. [4] The siloxane polymer composition according to [2] or [3], which gives a crosslinked product having a glass transition temperature of 0°C or higher. [5] The crosslink density n calculated by the following formula (α) is 150 mol / m 3 The siloxane polymer composition according to any one of claims [1] to [4], which gives a crosslinked product as described above. n = E' / 3RT (α) n: Crosslink density (mol / m 3 ), E': storage modulus (Pa), R: gas constant ((Pa m 3) / (K mol)), T: temperature (K) [6] A crosslinked body obtained by crosslinking the siloxane polymer composition according to any one of [2] to [5]. [7] The crosslinked body according to [6], having a maximum linear expansion coefficient calculated in the range from 50°C to 180°C in 10°C increments of less than 200 ppm / K. [8] The crosslinked body according to [6] or [7], having a glass transition temperature of 0°C or higher. [9] The crosslink density n calculated by the following formula (α) is 150 mol / m 3 The crosslinked body according to any one of [6] to [8] above. n = E' / 3RT (α) n: Crosslink density (mol / m 3 ), E': storage modulus (Pa), R: gas constant ((Pa m 3 ) / (K mol)), T: temperature (K)

[0008]

[10] A method for producing a siloxane polymer containing a repeating unit represented by formula (1), comprising the step of converting a hydrosilyl group of a siloxane polymer containing a repeating unit represented by formula (1') into a silanol group in the presence of a transition metal catalyst. [ka] In the above formula, R 0 each independently represents an aryl having 6 to 20 carbon atoms or a cycloalkyl having 5 to 6 carbon atoms, and any hydrogen atom in the aryl having 6 to 20 carbon atoms and the cycloalkyl having 5 to 6 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms; R 1each independently represents a hydrogen atom, an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; R 2 and R 3 each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; p represents a real number greater than or equal to 1; x represents a real number from 1 to 30; y1+y2 represents a real number from 1 to 30, and y2 is equal to or greater than 0 and less than 30.

[11] The method for producing a siloxane polymer containing a repeating unit represented by formula (1) according to

[10] , wherein the transition metal catalyst is a palladium catalyst. Effect of the Invention

[0009] According to the present invention, a crosslinked material having a low thermal expansion coefficient in the temperature range of 50°C to 180°C is obtained. The present invention provides a siloxane polymer and a crosslinked product thereof having a low coefficient of thermal expansion in the temperature range of 50°C to 180°C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail, but the following description is an example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents in any way. In addition, the embodiments of the present invention can be appropriately combined. The terms used in this specification are defined as follows. In either case, alkyl and alkylene may be a straight-chain group or a branched group. This means that even if any hydrogen in these groups is replaced with a halogen or a cyclic group, any -CH 2 The same applies when - is replaced by -O-, -CH=CH-, cycloalkylene, cycloalkenylene, phenylene, etc. The term "any" used in the present invention indicates that not only the position but also the number is arbitrary. When the number is plural, each may be replaced by a different group. For example, in an alkyl group, two -CH 2 When - is replaced by -O- and -CH=CH-, it indicates alkoxyalkenyl or alkenyloxyalkyl. In this case, any of the alkoxy, alkenylene, alkenyl and alkylene groups may be linear or branched. However, any -CH 2 When describing that - is replaced by -O-, multiple consecutive -CH 2 - cannot be replaced by -O-. That is, for example, -CH 2 -CH 2- will never be replaced by -OO-.

[0011] 1. Siloxane polymer A siloxane polymer according to one embodiment of the present invention (hereinafter also referred to as "the siloxane polymer of the present invention") is characterized by including a repeating unit represented by formula (1). [ka] In the above formula, R 0 each independently represents an aryl having 6 to 20 carbon atoms or a cycloalkyl having 5 to 6 carbon atoms, and any hydrogen atom in the aryl having 6 to 20 carbon atoms and the cycloalkyl having 5 to 6 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms; R 1 each independently represents a hydrogen atom, an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; R 2 and R 3each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; p represents an integer of 1 or greater; x represents an integer from 1 to 30; y1+y2 represents an integer of 1 to 30, and y2 is 0 or more and less than 30.

[0012] (R 0 ) R 0 each independently represents an aryl having 6 to 20 carbon atoms or a cycloalkyl having 5 to 6 carbon atoms. Examples of the aryl having 6 to 20 carbon atoms include phenyl, naphthyl, anthryl, phenanthryl, triphenylenyl, pyrenyl, chrysenyl, naphthacenyl, perylenyl, etc. Among these, phenyl, naphthyl, anthryl, and phenanthryl are preferred, and phenyl, naphthyl, and anthryl are more preferred. Examples of the cycloalkyl having 5 to 6 carbon atoms include cyclopentyl and cyclohexyl. In the aryl having 6 to 20 carbon atoms and the cycloalkyl having 5 to 6 carbon atoms, any hydrogen atom may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms. R 0 is preferably phenyl or cyclohexyl.

[0013] (R 1 ) R 1 each independently represents a hydrogen atom, an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms. Aryl having 6 to 20 carbon atoms and cycloalkyl having 5 to 6 carbon atoms are R 0 Examples of the above-mentioned methods are the same as those described above. Examples of the arylalkyl having 7 to 40 carbon atoms include benzyl, phenethyl, diphenylmethyl, triphenylmethyl, 1-naphthylmethyl, 2-naphthylmethyl, 2,2-diphenylethyl, 3-phenylpropyl, 4-phenylbutyl, and 5-phenylpentyl. Examples of alkyl having 1 to 40 carbon atoms include methyl, ethyl, n-propyl, iso-propyl, n-butyl, sec-butyl, iso-butyl, tert-butyl, n-pentyl, sec-pentyl, iso-pentyl, tert-pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, dodecyl, and octadecyl. In the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms, any hydrogen atom may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, and in the alkylene in the arylalkyl having 7 to 40 carbon atoms, any hydrogen atom may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms. R 1 is preferably selected from a hydrogen atom, phenyl, cyclohexyl, and alkyl having 1 to 5 carbon atoms, and more preferably selected from alkyl having 1 to 5 carbon atoms.

[0014] (R2 , R 3 ) R 2 and R 3 each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms. . Aryl having 6 to 20 carbon atoms and cycloalkyl having 5 to 6 carbon atoms are R 0 Examples of the above-mentioned methods are the same as those described above. As the arylalkyl having 7 to 40 carbon atoms, R 1 Examples of the above-mentioned methods are the same as those described above. As the alkyl having 1 to 40 carbon atoms, R 1 Examples of the above-mentioned methods are the same as those described above. In the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms, any hydrogen atom may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, and in the alkylene in the arylalkyl having 7 to 40 carbon atoms, any hydrogen atom may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms. R 2 is preferably selected from phenyl, cyclohexyl, and alkyl having 1 to 5 carbon atoms, and more preferably selected from alkyl having 1 to 5 carbon atoms. R 3 is preferably selected from phenyl, cyclohexyl, and alkyl having 1 to 5 carbon atoms, and more preferably selected from alkyl having 1 to 5 carbon atoms.

[0015] (p, x, y1, y2) In the repeating unit represented by formula (1), p is a real number of 1 or more; x is a real number of 1 to 30; y1+y2 is a real number of 1 to 30, and y2 is 0 or more and less than 30. By adjusting p, x, y1, and y2, the physical properties of the crosslinked body obtained by crosslinking the siloxane polymer of the present invention can be controlled. p represents a real number of 1 or more. From the viewpoint of production and handling, p is preferably 20 or less, and more preferably 8 or less. From the viewpoint of facilitating production and handling of a crosslinked body obtained by crosslinking a siloxane polymer, p is 1 or more, preferably 4 or less, and more preferably 2 or less. x represents a real number of 1 to 30. From the viewpoint of production and handling, x is preferably 20 or less, more preferably 8 or less. When the glass transition temperature of the crosslinked material obtained by crosslinking the siloxane polymer is to be increased, x is preferably 1 or more, more preferably 2 or more, and is preferably 4 or less, more preferably 3 or less. When the crosslink density is to be increased, x is preferably 2 or more, more preferably 4 or more. y1+y2 represents a real number of 1 to 30, and y2 is 0 or more and less than 30. From the viewpoint of production and handling, y1+y2 is preferably 20 or less, more preferably 8 or less. As described later, the siloxane polymer of the present invention can be produced by converting hydrosilyl groups to silanol groups. Therefore, by adjusting the conversion ratio of hydrosilyl groups to silanol groups, the glass transition temperature, crosslinking density, thermal expansion coefficient, viscoelasticity, mechanical properties, etc. can be controlled. When all hydrosilyl groups are converted to silanol groups, y2=0. When the glass transition temperature and crosslinking density of the crosslinked body obtained by crosslinking the siloxane polymer are to be increased, it is preferable to increase y1, i.e., the ratio of silanol groups, and y1 is preferably 1 or more, more preferably 2 or more. Here, in the siloxane polymer according to one embodiment of the present invention, the repeating unit represented by formula (1) is not limited to one type, and may include a plurality of different repeating units. The synthesis method of the siloxane polymer described below is equilibrium polymerization, and p, x, y1, and y2 are expressed as average values. When p is 1, the values ​​of x and y1+y2 may be expressed as decimals. The ratio of x and y1+y2 can be controlled by the ratio of raw materials charged during polymerization in the production method described later. For example, in the examples described later, compound α can be charged in an increased amount to increase the silsesquioxane units, and D4 or D'4 can be charged in an increased amount to increase the chain siloxane units. In addition, the concentration of the reaction solution, the concentration and type of catalyst, temperature conditions, reaction The ratio of x and y1+y2 can be controlled by time. In addition, an increase in the silsesquioxane units (p) makes the crosslinked body harder, but if there are too many silsesquioxane units, the body becomes brittle. On the other hand, an increase in the linear siloxane units (x, y1, y2) increases the flexibility and gives a flexible crosslinked body. On the other hand, if there are too many linear siloxane units, the surface of the crosslinked body becomes sticky and the strength decreases.

[0016] The terminal of the siloxane polymer containing the repeating unit represented by formula (1) according to the present invention is not particularly limited. In the siloxane polymer of the present invention, the mass % occupied by the repeating unit represented by formula (1) is usually 10% or more, preferably 30% or more, more preferably 50% or more, and particularly preferably 70% or more, and is usually less than 100, preferably 99% or less. In other words, the polymer may contain units other than the repeating unit represented by formula (1) as long as the effects of the present invention are not significantly impaired. Examples of such units include -(CH 2 -CH 2 )-, -(CH=CH)-, -(O-SiMe 2 -C 6 H 4 -SiMe 2 )- are mentioned. The weight average molecular weight (Mw) of the siloxane polymer containing the repeating unit represented by formula (1) according to the present invention is not particularly limited, but is preferably 2,000 or more, more preferably 10,000 or more, and is preferably 10,000,000 or less, more preferably 1,000,000 or less. The weight average molecular weight is determined by calculating a chromatogram obtained by gel permeation chromatography (GPC) using a calibration curve obtained from a molecular weight standard sample, as described in the examples below.

[0017] 2. Method for producing siloxane polymer The siloxane polymer containing a repeating unit represented by formula (1) according to one embodiment of the present invention can be obtained by reacting a silsesquioxane compound with a compound containing a chain siloxane structure to produce a siloxane polymer containing a repeating unit represented by formula (1') containing a hydroxyl group in the main chain, and converting the hydrosilyl group of the siloxane polymer containing the repeating unit represented by formula (1') into a silanol group, for example, in the presence of a transition metal catalyst. [ka] In the above formula (1'), R 0 ~R 3 , p, x, y1, and y2 are R in formula (1), 0 ~R 3 , p, x, y1, y2.

[0018] The method for producing the siloxane polymer represented by formula (1') is not particularly limited, but may be, for example, For example, it can be suitably produced by a production method including the steps of the following method (I) or (II). do. (I): A compound represented by formula (a), a compound represented by formula (b), and a compound represented by formula (c) A step of reacting with a compound. (II): A step of reacting a silicon compound represented by formula (a), a silicon compound represented by formula (b), and a compound having a hydrosilyl group represented by formula (d). In the above step (I) or (II), a compound represented by formula (e) is added to react The ends may be sealed by subjecting the polymer to a In the above step (I) or step (II), tetrahydrofuran, toluene, ethyl acetate, A solvent such as ethanol may be used. It is preferable to carry out the reaction in the presence of an acid such as sulfuric acid. 2 It is preferable to carry out the reaction under an inert atmosphere such as a 200° C. or 500° C. atmosphere. It is also preferable to carry out the reaction with stirring.

[0019] [ka]

[0020] (Compound represented by formula (a)) In the siloxane polymer, the silsesquioxane units are derived from a compound represented by formula (a). [ka] In the above formula, R 0 each independently represents an aryl having 6 to 20 carbon atoms or a cycloalkyl having 5 to 6 carbon atoms, and any hydrogen atom in the aryl having 6 to 20 carbon atoms and the cycloalkyl having 5 to 6 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms; R 1 each independently represents a hydrogen atom, an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2- may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms. Specific R 0 , R 1 is "1. Siloxane polymer" (R 0 ), (R 1 ) are some of the examples described in the section. The compound represented by formula (a) can be synthesized, for example, by referring to the description in JP-A-2006-022207, and the compound shown below is preferred.

[0021] [ka]

[0022] (Compound represented by formula (b)) The compound represented by formula (b) can be used to introduce linear siloxane units into a siloxane polymer. [ka] In the above formula, R 2 each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - are each independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, and any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms. a represents an integer of 3 to 30. From the viewpoint of production of the siloxane polymer, a is preferably an integer of 3 to 20, and more preferably 3 to 10. Specific R 2 is "1. Siloxane polymer" (R 2 , R 3 The preferred embodiments are also the same. Examples of the compound represented by formula (b) include 2,2,4,4,6,6-hexamethylcyclotrisiloxane, 2,4,6-triethyl-2,4,6-trimethylcyclotrisiloxane, 2,2,4,4,6,6-hexaethylcyclotrisiloxane, 2,4,6-trimethyl-2,4,6-tripropylcyclotrisiloxane, 2,4,6-triethyl-2,4,6-tripropylcyclotrisiloxane, 2,2,4,4,6,6-hexapropylcyclotrisiloxane, and 2,4,6-trimethyl-2,4,6-tris(1-methylethyl)cyclotrisiloxane. 2,4,6-triethyl-2,4,6-tris(1-methylethyl)cyclotrisiloxane 2,2,4,4,6,6-hexakis(1-methylethyl)cyclotrisiloxane 2,4,6-tributyl-2,4,6-trimethylcyclotrisiloxane 2,4,6-tributyl-2,4,6-triethylcyclotrisiloxane 2,2,4,4,6,6-hexabutylcyclotrisiloxane 2,4,6-trimethyl-2,4,6-tris(1,1-dimethylethyl)cyclotrisiloxane 2,46-triethyl-2,4,6-tris(1,1 -dimethylethyl)cyclotrisiloxane, 2,4,6-tris(1,1-dimethylethyl)-2,4,6-tripropylcyclotrisiloxane, 2,2,4,4,66-hexakis(1,1-dimethylethyl)cyclotrisiloxane, 2,4,6-trimethyl-2,4,6-tris(trifluoromethyl)cyclotrisiloxane, 2,2,4,4,6,6-hexakis(trifluoromethyl)cyclotrisiloxane, 2,2,4,4,6,6-hexakis(1,1,2,2,2-pentafluoroethyl)cyclotrisiloxane, 2,4,6-trimethyl- 2,4,6-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 2,2,4,4,6,6-hexakis(3,3,3-trifluoropropyl)cyclotrisiloxane, 2,4,6-trimethyl-2,4,6-triphenylcyclotrisiloxane, 2,2,4,4,6,6-hexaphenylcyclotrisiloxane, 2,4,6-tricyclohexyl-2,4,6-trimethylcyclotrisiloxane, 2,2,4,4,6,6-hexacyclohexylcyclotrisiloxane, 2,2,4,4,6,6-hexavinylcyclotrisiloxane, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane, 2,2,4,4,6,6,8,8-octamethylcyclotetrasiloxane, 2,4,6,8-tetraethyl-2,4,6,8-tetramethylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-octaethylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetrapropylcyclotetrasiloxane, 2,4,6,8-tetraethyl-2,4,6,8-tetrapropylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-octapropylcyclo Tetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetrakis(1-methylethyl)cyclotetrasiloxane, 2,4,6,8-tetraethyl-2,4,6,8-tetrakis(1-methylethyl)cyclotetrasiloxane, 2,2,4,4,6,6,8,8-octakis(1-methylethyl)cyclotetrasiloxane, 2,4,6,8-tetrabutyl-2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetrabutyl-2,4,6,8-tetraethylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-octakis(1-methylethyl)cyclotetrasiloxane 2,4,6,8-tetramethyl-2,4,6,8-tetrakis(1,1-dimethylethyl)cyclotetrasiloxane, 2,4,6,8-tetraethyl-2,4,6,8-tetrakis(1,1-dimethylethyl)cyclotetrasiloxane, 2,4,6,8-tetrakis(1,1-dimethylethyl)-2,4,6,8-tetrapropylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-octakis(1,1-dimethylethyl)cyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetrakis(1,1-dimethylethyl)cyclotetrasiloxane 2,2,4,4,6,6,8,8-octakis(trifluoromethyl)cyclotetrasiloxane, 2,2,4,4,6,6,8,8-octakis(1,1,2,2,2-pentafluoroethyl)cyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetrakis(3,3,3-trifluoropropyl)cyclotetrasiloxane, 2,2,4,4,6,6,8,8-octakis(3,3,3-trifluoropropyl)cyclotetrasiloxane, 2,4,6,8-tetramethyl-2,4,6,8-Tetraphenylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-Octaphenylcyclotetrasiloxane, 2,4,6,8-Tetracyclohexyl-2,4,6,8-Tetramethylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-Octacyclohexylcyclotetrasiloxane, 2,2,4,4,6,6,8,8-Octavinylcyclotetrasiloxane, 2,4,6,8-Tetramethyl-2,4,6,8-Tetravinylcyclotetrasiloxane, 2,6-Diethynyl-2,4,4,6,8,8-Hexamethylcyclotetrasiloxane Siloxane, 2,2,4,4,6,6,8,8,10,10-decamethylcyclopentasiloxane, 2,4,6,8,10-pentaethyl-2,4,6,8,10-pentamethylcyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-decaethylcyclotrisiloxane, 2,4,6,8.10-pentamethyl-2,4,6,8-pentapropylcyclopentasiloxane, 2,4,6,8,10-pentaethyl-2,4,6,8,10-pentapropylcyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-decapropyl 2,4,6,8,10-pentamethyl-2,4,6,8,10-pentakis(1-methylethyl)cyclopentasiloxane, 2,4,6,8,10-pentaethyl-2,4,6,8,10-pentakis(1-methylethyl)cyclopentasiloxane 2,2,4,4,6,6,8,8,10,10-decakis(1-methylethyl)cyclopentasiloxane, 2,4,6,8,10-pentabutyl-2,4,6,8,10-pentamethylcyclopentasiloxane, 2,4,6,8,10-pentabutyl-2,4,6,8,10-penta 2,2,4,4,6,6,8,8,10,10-decabutylcyclopentasiloxane, 2,4,6,8,10,10-pentamethyl-2,4,6,8,10,10-pentakis(1,1-dimethylethyl)cyclopentasiloxane, 2,4,6,8,10-pentaethyl-2,4,6,8,10-pentakis(1,1-dimethylethyl)cyclopentasiloxane, 2,4,6,8,10-pentakis(1,1-dimethylethyl)-2,4,6,8,10-pentapropylcyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-Deca-kis(1,1-dimethylethyl)cyclopentasiloxane, 2,4,6,8,10-pentamethyl-2,4,6,8-pentakis(trifluoromethyl)cyclopentasiloxane, 2,2,4,4,6,6,8,8,10.10-Deca-kis(trifluoromethyl)cyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-Deca-kis(1,1,2,2,2-pentafluoroethyl)cyclopentasiloxane, 2,4,6,8,10,10-pentamethyl-2,4,6,8-pentakis(3,3,3-trifluoropropyl)cyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-Deca-kis(3,3,3- trifluoropropyl)cyclopentasiloxane, 2,4,6,8,10-pentamethyl-2,4,6,8-pentaphenylcyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-decaphenylcyclopentasiloxane, 2,4,6,8,10-pentacyclohexyl-2,4,6,8,10-pentamethylcyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-decacyclohexylcyclopentasiloxane, 2,2,4,4,6,6,8,8,10,10-decavinylcyclopentasiloxane, 2,4,6,8,10-pentamethyl-2,4,6,8,10-pentavinylcyclopentasiloxane, among which R, 2 is an alkyl group having 1 to 40 carbon atoms, and cyclic siloxanes such as hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), and dodecamethylcyclohexasiloxane (D6) are more preferred, with octamethylcyclotetrasiloxane being particularly preferred from the standpoints of availability, cost, and handling.

[0023] (Compound represented by formula (c)) The compound represented by formula (c) can be used to introduce a hydrosilyl group into the siloxane polymer (1'). [ka] In formula (c), R3 each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; b represents an integer of 1 to 40. R 3 is "1. Siloxane polymer" (R 2 , R 3 The same explanations apply as in the previous section. Examples of the compound represented by formula (c) include 2,4,6-trimethylcyclotrisiloxane, 2,4,6-triethylcyclotrisiloxane, 2,4,6-tris(1-methylethyl)cyclotrisiloxane, tripropylcyclotrisiloxane, 2,4,6-tris(1,1-dimethylethyl)cyclotrisiloxane, 2,4,6-tris(1,1-dimethylethyl)cyclotrisiloxane, 2,4,6,8-tetramethylcyclotetrasiloxane, 2,4,6,8-tetraethylcyclotetrasiloxane, 2,4,6,8,10-pentamethylcyclopentasiloxane, and 2,4,6,8,10-pentaethylcyclopentasiloxane.

[0024] (Compound represented by formula (d)) For example, a hydrosilyl group can be introduced into the siloxane polymer (1') using a compound represented by formula (d). [ka] In formula (d), R 2 , R 3 and R 4 are independently an aryl having 6 to 20 carbon atoms, any hydrogen atom in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms; any hydrogen atom in the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom; any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; c and d each represent an integer of 1 to 40. R 2 , R 3 and R 4 is "1. Siloxane polymer" (R 2 , R 3 The same explanations apply as in the previous section. Examples of the compound represented by formula (d) include 1,1,1,3,5,5,5-heptamethyltrisiloxane, 1,1,1,3,5,5,7,7,7-nonamethyltetrasiloxane, 1,1,1,3,5,5,5-heptaphenyltrisiloxane, 1,1,1,3,5,5,7,7,7-nonaphenyltetrasiloxane, and HMS-031, HMS-071, HMS-151, HMS-301, HMS-501, and HAM-301 manufactured by Gelest; and (when d=1): HMS-991, HMS-992, and HMS-993 manufactured by Gelest.

[0025] (Compound represented by formula (e)) The compound represented by formula (e) can be used to end-cap the siloxane polymer (1). [ka] In formula (e), R 2 and R 4 each independently represents an aryl having 6 to 20 carbon atoms, a cycloalkyl having 5 to 6 carbon atoms, an arylalkyl having 7 to 40 carbon atoms, or an alkyl having 1 to 40 carbon atoms, and any hydrogen atom of the aryl in the aryl having 6 to 20 carbon atoms, the cycloalkyl having 5 to 6 carbon atoms, and the aryl in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom or an alkyl having 1 to 20 carbon atoms, any hydrogen atom of the alkylene in the arylalkyl having 7 to 40 carbon atoms may be independently replaced by a fluorine atom, and any -CH 2 - may be independently replaced by -O-, -CH=CH-, or cycloalkylene having 5 to 20 carbon atoms, any hydrogen atom in the alkyl having 1 to 40 carbon atoms may be independently replaced by a fluorine atom, any -CH 2 - may be independently replaced by -O- or cycloalkylene having 5 to 20 carbon atoms; e represents an integer from 1 to 1000. R 2 and R 4 is "1. Siloxane polymer" (R 2 , R 3 The same explanations apply as in the previous section. Examples of the compound represented by formula (e) include hexamethyldisiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, hexaphenyldisiloxane, octaphenyltrisiloxane, decaphenyltetrasiloxane, and DMA-T07R manufactured by Gelest.

[0026] (siloxane polymer containing a repeating unit represented by formula (1')) (Process for converting to an isol group) Another aspect of the present invention is a method for producing a siloxane polymer containing a repeating unit represented by formula (1), which comprises a step of converting a hydrosilyl group of a siloxane polymer containing a repeating unit represented by formula (1') into a silanol group in the presence of a transition metal catalyst. This process converts all or part of the hydrogen atoms of the hydrosilyl groups to hydroxyl groups, and a siloxane polymer containing a repeating unit represented by formula (1) containing a silanol group can be obtained. When all of the hydrosilyl groups are converted to silanol groups, y2=0 in the siloxane polymer containing the repeating unit represented by formula (1). The conversion ratio of hydrosilyl groups to silanol groups can be controlled, for example, by adjusting the time, solution concentration, and catalyst concentration of this process. In this process, for example, the hydrosilyl group of the siloxane polymer containing the repeating unit represented by formula (1') is converted to a silanol group as follows. The siloxane polymer containing the repeating unit represented by formula (1') containing the hydrosilyl group is dissolved in a solvent, and the solution is dropped into a mixture of the solvent, water, and catalyst while stirring. After hydrogen generation is completed, the reaction solution is aged. After that, the catalyst is removed using a filter aid or the like, an organic solvent such as ethyl acetate is added, the solution is separated, and the organic layer is dried with sodium sulfate. Next, the sodium sulfate is removed, the solution is concentrated under reduced pressure, and then reprecipitated with heptane, and the resulting precipitate is vacuum dried to obtain the target product. Examples of the transition metal catalyst include palladium catalyst, platinum catalyst, rhodium catalyst, ruthenium catalyst, copper catalyst, and rhenium catalyst, and preferably palladium catalyst. Examples of the palladium catalyst include palladium hydroxide / carbon catalyst and palladium / carbon catalyst, and preferably palladium hydroxide / carbon catalyst from the viewpoint of reaction efficiency. The amount of catalyst is not particularly limited, but is preferably 1 to 30 mol% relative to the substrate from the viewpoint of reactivity and yield. The reaction solvent used in this step is not particularly limited as long as it is a solvent that does not participate in the reaction, and examples thereof include aromatic hydrocarbon solvents such as toluene and xylene; ester solvents such as methyl acetate and ethyl acetate; and ether solvents such as THF, diethyl ether, and cyclopentyl methyl ether. Among these, solvents that are miscible with water are preferred, and THF is particularly preferred. The amount of the solvent used is not particularly limited, but from the viewpoint of reactivity and workability, it is preferred to use the solvent so that the solid content concentration (solid content concentration = 100 x weight other than solvent / weight of the entire reaction solution) is 1% by mass or more and 50% by mass or less. The amount of water to be added is not particularly limited, but from the viewpoint of miscibility with the solvent, it is preferable to add water in an amount of 1% by mass to 15% by mass relative to the solvent. The reaction time is not particularly limited. However, if the reaction time is too long, condensation between silanol groups (-SiOH) or an exchange reaction between H and OH may occur between a hydrosilyl group (SiH) and a silanol group (SiOH). Therefore, from the viewpoint of ensuring the yield and preventing the increase in molecular weight, the reaction time is preferably 15 minutes to 24 hours. The reaction temperature is not particularly limited, but is preferably 1° C. or higher, more preferably 5° C. or higher, and is preferably 50° C. or lower, more preferably 40° C. or lower. Specifically, in this process, for example, a siloxane polymer containing a repeating unit represented by formula (1') containing a hydrosilyl group is stirred in a mixed solvent of tetrahydrofuran and water using a palladium hydroxide / carbon catalyst under an inert atmosphere, whereby all or a part of the hydrogen atoms in the hydrosilyl group are converted to hydroxyl groups, thereby obtaining a siloxane polymer containing a repeating unit represented by formula (1) containing a silanol group.

[0027] 3.Crosslinked body The crosslinked body according to one embodiment of the present invention is a crosslinked body obtained by crosslinking a siloxane polymer containing a repeating unit represented by the above formula (1) (hereinafter, also referred to as the "crosslinked body of the present invention"). The crosslinked body of the present invention will be described below.

[0028] 3.1 Manufacturing method of crosslinked body A siloxane polymer comprising a repeating unit represented by formula (1) according to one embodiment of the present invention. The method for producing the crosslinked body of the present invention (hereinafter, also referred to as "the method for producing the crosslinked body of the present invention") is not particularly limited as long as it is a method in which the silanol group of the siloxane polymer containing the repeating unit represented by formula (1) is crosslinked to obtain a crosslinked body, but it is preferable to include a heat treatment step. As such a production method, for example, a method in which a siloxane polymer composition containing a siloxane polymer containing a repeating unit represented by formula (1), a crosslinking agent, and a catalyst is prepared, the siloxane polymer composition is applied to a substrate, and the siloxane polymer composition is heated to crosslink the siloxane polymer. More specifically, the siloxane polymer containing the repeating unit represented by formula (1) is dissolved in a solvent such as toluene, a crosslinking agent and a catalyst are added thereto, and the mixture is stirred to prepare a siloxane polymer composition. After degassing, the siloxane polymer composition is applied to a substrate, and heated in an oven at 70°C for 20 minutes, 100°C for 1 hour, and 200°C for 2 hours. After cooling, the film formed on the substrate is peeled off, and the crosslinked body can be obtained as a free-standing film.

[0029] (Siloxane polymer composition) In the method for producing a crosslinked body of the present invention, it is preferable to prepare and use a siloxane polymer composition (hereinafter also referred to as "siloxane polymer composition") containing a siloxane polymer containing a repeating unit represented by formula (1), a crosslinking agent, and a catalyst. The siloxane polymer composition may contain a solvent. The composition may be prepared by mixing a siloxane polymer containing a repeating unit represented by formula (1), a crosslinking agent, and a catalyst. For example, a siloxane polymer containing a repeating unit represented by formula (1) is dissolved in a solvent, a crosslinking agent and a catalyst are added thereto, and the mixture is stirred to obtain a solution that is a siloxane polymer composition. From the viewpoint of uniformity of the obtained crosslinked body, it is preferable to degas the siloxane polymer composition before being subjected to coating.

[0030] (Crosslinking agent) The crosslinking agent used in the present embodiment is not particularly limited as long as it reacts with a silanol group, but from the viewpoints of ease of handling and availability, a siloxane compound containing an alkoxysilyl group is preferable. Specific examples of the crosslinking agent include methyl silicate, ethyl silicate, a mixture of methyl silicate and ethyl silicate, etc. Methyl silicate is represented by the following formula: [ka] In the above formula, m is 2 to 100, preferably 2 to 50, more preferably 4 to 10, and further preferably 4 to 5. Examples of commercially available products include MKC (registered trademark) Silicate MS51, MS56, MS57, and MS56S (manufactured by Mitsubishi Chemical Corporation); Ethyl Silicate 28, Ethyl Silicate 40, Ethyl Silicate 48, EMS-485, Methyl Silicate 51, and Methyl Silicate 53 (manufactured by Colcoat Co., Ltd.). The crosslinking agent may be used alone or in combination of two or more kinds. The amount of the crosslinking agent added is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and usually 20% by mass or less, preferably 10% by mass or less, and more preferably 5% by mass or less, based on the siloxane polymer. When two or more crosslinking agents are used, the total content is preferably within the above range.

[0031] (catalyst) The catalyst used in this embodiment may be appropriately selected according to the crosslinking agent. For example, when a siloxane compound containing an alkoxysilyl group is used as the crosslinking agent, an organometallic compound containing a metal such as tin, titanium, zirconium, zinc, or bismuth; an acidic compound; or a basic compound may be used. Such metal compounds preferably include organotin catalysts such as dibutyltin dilaurate, dibutyltin maleate, dibutyltin diacetate, dibutyltin dioctanoate, dibutyltin acetylacetonate, dibutyltin oxide, and tin octoate; and alkoxy titaniums such as tetrabutyl titanate, tetrapropyl titanate, tetraisopropyl titanate, and titanium tetraacetylacetonate. Acidic compounds include, for example, phosphoric acid, toluenesulfonic acid, sulfuric acid, nitric acid, acetic acid, and benzoic acid. Examples of basic compounds include triethylamine, tributylamine, 1,4-diazabicyclo[2.2.2]octane, 1,5-diazabicyclo[4.3.0]non-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, N,N-bis(N,N-dimethyl-2-aminoethyl)methylamine, N,N-dimethylcyclohexylamine, N,N-dimethylphenylamine, and N-ethylmorpholinine. The catalyst may be used alone or in combination of two or more. The amount of catalyst added is usually 0.001% by mass or more, preferably 0.005% by mass or more, more preferably 0.01% by mass or more, and usually 10% by mass or less, preferably 5% by mass or less, and more preferably 3% by mass or less, based on the siloxane polymer. When two or more catalysts are used, the total content is preferably within the above range.

[0032] (solvent) The siloxane polymer composition used in the present embodiment may contain a solvent. From the viewpoint of handling of the siloxane polymer composition, it is preferable to adjust the viscosity of the siloxane polymer composition using a solvent. The solvent used in the siloxane polymer composition is not particularly limited as long as it can dissolve the siloxane polymer containing the repeating unit represented by formula (1).Preferred solvents include hydrocarbon solvents such as butane, hexane, heptane, octane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, mesitylene, and anisole; ether solvents such as diethyl ether, diisopropyl ether, 1,2-dimethoxyethane, tetrahydrofuran (THF), and dioxane; halogenated hydrocarbon solvents such as methylene chloride and carbon tetrachloride; ester solvents such as ethyl acetate; glycol ester solvents such as propylene glycol monomethyl ether acetate (PGMEA); nitrogen-containing solvents such as dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), N-methylpyrrolidone (NMP), and pyridine; alcohol solvents such as methanol, ethanol, isopropanol, and butanol; and ketone solvents such as acetone and methyl ethyl ketone. Preferred are toluene, mesitylene, anisole, tetrahydrofuran, cyclopentyl methyl ether, propylene glycol monomethyl ether acetate, and 2-(2-ethoxyethoxy)ethyl acetate, and more preferred are toluene and propylene glycol monomethyl ether acetate (PGMEA). One or more solvents may be used. The solvent may be dehydrated before use. The amount of the solvent used is not particularly limited, but is usually 10% by mass or more, preferably 20% by mass or more, and usually 1000% by mass or less, preferably 500% by mass or less, based on the siloxane polymer containing the repeating unit represented by formula (1).

[0033] (Heating process) A method for crosslinking a siloxane polymer containing a repeating unit represented by formula (1) includes heat treatment. Specifically, the heat treatment step may involve applying the siloxane polymer composition to a substrate and then heating the substrate in an oven or the like. The temperature and time of the heat treatment step are not particularly limited as long as the siloxane polymer containing the repeating unit represented by formula (1) can be crosslinked as desired. The siloxane polymer crosslinked and cured by the heat treatment can be peeled off from the substrate as a film-like crosslinked product after being allowed to cool. The substrate is not particularly limited as long as it can withstand the temperature of the heat treatment step and the crosslinked body formed on the substrate can be peeled off from the substrate to be taken out as a free-standing film. Examples of the substrate that can be used include glass substrates such as quartz, barium borosilicate glass, and aluminoborosilicate glass; calcium fluoride substrates; metal oxide substrates such as ITO (indium tin oxide); ceramic substrates; plastic films such as polycarbonate (PC) film, silicone-based film, polyethylene terephthalate (PET) film, polyethylene naphthalate (PEN) film, cycloolefin polymer (COP) film, polypropylene film, polyethylene film, acrylic polymer film, polyvinyl alcohol film, triacetyl cellulose film, and polyimide (PI) film; fluororesin substrates such as polytetrafluoroethylene (PTFE) and perfluoroalkoxyalkane (PFA); laminate substrates in which a fluororesin is applied to glass or the like; and metal substrates such as SUS and copper can be used.

[0034] 3.2 Physical properties of cross-linked bodies A crosslinked product obtained by crosslinking a siloxane polymer containing a repeating unit represented by formula (1) has a lower thermal expansion coefficient and can achieve a higher crosslink density and a higher glass transition temperature (Tg) than a siloxane polymer not containing a silanol group.

[0035] 3.2.1 Glass transition temperature In dynamic viscoelasticity measurement by DMA, the glass transition temperature is the peak top temperature of the loss modulus (E"). The crosslinked body of the present embodiment preferably has a glass transition temperature of 0°C or higher, and more preferably 30°C or higher. The dynamic viscoelasticity measurement by DMA may be performed, for example, using Hitachi High-Tech Science DMS6100 under the following measurement conditions. 1℃ / min, sample area 10mm×1mm Load: 10mN, measurement frequency: 10 Hz

[0036] 3.2.2 Crosslink density Generally, the storage modulus of the rubber-like plateau region of a crosslinked polymer is observed to be higher as the crosslink density increases. By utilizing this phenomenon, the apparent crosslink density n can be approximated from the storage modulus of the rubber-like plateau region using the following formula. n≒E' / 3RT n: Crosslink density (mol / m 3 ), E': storage modulus (Pa), R: gas constant ((Pa m 3 ) / (K mol)), T: temperature (K) From the viewpoint of heat resistance, a siloxane polymer film with a high crosslink density is required. The crosslinked body of the present embodiment has a crosslink density n calculated from the above formula (α) of 150 mol / m 3 It is preferable that the concentration is 250 mol / m or more. 3 is more preferred.

[0037] 3.2.3 Coefficient of linear expansion (CTE) The linear expansion coefficient is measured by thermomechanical analysis (TMA). In the first scan (first temperature rise, temperature rise rate: 5°C / min) in the temperature range of 50°C to 180°C, the crosslinked body of the present embodiment having the repeating unit represented by formula (1) has a maximum linear expansion coefficient calculated in the range from 50°C to 180°C in increments of 10°C (i.e., 50°C to 60°C, 60°C to 70°C, 70°C to 80°C, 80°C to 90°C, 90°C to 100°C, 100°C to 110°C, 110°C to 120°C, 120°C to 130°C, 130°C to 140°C, and 140°C to 150°C) of preferably less than 200 ppm / K, more preferably 190 ppm / K or less. The linear expansion coefficient can be measured by TMA using, for example, Hitachi High-Tech Science SS / TMA6100 under the following measurement conditions. Tensile mode, 5℃ / min, length 20mm, cross-sectional area 0.3mm 2 Load 9.8 mN EXAMPLES

[0038] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these descriptions.

[0039] The reagents used in the examples are shown below. Toluene (special grade): Fujifilm Wako Pure Chemical Industries, Ltd. Toluene (ultra-dehydrated): Fujifilm Wako Pure Chemical Industries, Ltd. Tetrahydrofuran (primary): Fujifilm Wako Pure Chemical Industries, Ltd. D 4 (Octamethylcyclotetrasiloxane): manufactured by Tokyo Chemical Industry Co., Ltd. D' 4 (2,4,6,8-Tetramethylcyclotetrasiloxane): manufactured by Tokyo Chemical Industry Co., Ltd. Kyoward (registered trademark) 500 SN (synthetic hydrotalcite): manufactured by Kyowa Chemical Industry Co., Ltd. Heptane (primary): Fujifilm Wako Pure Chemical Industries, Ltd. Ethyl acetate (ultra-dehydrated): Fujifilm Wako Pure Chemical Industries, Ltd. Sulfuric acid (special grade): Kanto Chemical Co., Ltd. Palladium hydroxide / carbon (approximately 50% water-wet product): manufactured by Tokyo Chemical Industry Co., Ltd. Sodium sulfate (anhydrous): Fujifilm Wako Pure Chemical Industries, Ltd. MKC (registered trademark) Silicate MS51: Manufactured by Mitsubishi Chemical Corporation Dibutyltin dilaurate (DBTL): manufactured by Tokyo Chemical Industry Co., Ltd. PDMS: Gelest DMS-S42 [ka] Compound (α) was synthesized by reacting the following compound (4) with compound (5), followed by hydrolysis (see, for example, paragraph 0032 of JP-A-2006-022207). [ka]

[0040] GPC Gel Permeation Chromatography <Measurement conditions> Column: Showa Denko Co., Ltd. Shodex KF-804L 300 x 8.0 mm Showa Denko KF-805L 300 x 8.0mm 2 pieces in series Mobile phase: THF Flow rate: 1.0ml / min Temperature: 40℃ Detector: RI Molecular weight standard sample: Polymethylmethacrylate resin (PMMA) with known molecular weight

[0041] DMA Dynamic Mechanical Analysis <Measurement conditions> Hitachi High-Tech Science DMS6100 1℃ / min, sample area 10mm×1mm Load: 10mN, measurement frequency: 10 Hz

[0042] TMA thermomechanical analysis <Measurement conditions> Hitachi High-Tech Science SS / TMA6100 Tensile mode, 5℃ / min, length 20mm, cross-sectional area 0.3mm 2 Load 9.8 mN

[0043] [Synthesis Example 1] [ka]

[0044] Compound (α) 50g, D 4 15.6g, D' 4 Add 2.54g of toluene and 104.6g of toluene to a 500 mL four-neck round-bottom flask and equip it with a thermometer, reflux condenser, mechanical stirrer, oil A filter bath was set and nitrogen was allowed to flow. 1.6 g of sulfuric acid was added while stirring. After stirring at reflux temperature for about 1 hour, the mixture was allowed to cool to below 80°C and aged at 80°C for 3 hours. Heating and stirring were stopped, water was added and the reaction solution was washed several times with water, and then treated with Kyoward 500 to remove the acid. After filtration, the filtrate was concentrated at 50°C. The concentrated filtrate was reprecipitated with heptane, and the precipitate was dried in vacuum to obtain 44.6 g of a white solid (A). The molecular weight was measured by GPC, and the weight average molecular weight Mw was 123,000 and the polydispersity Mw / Mn = 3.8. 1 H-NMR analysis of SiH The presence of the group was confirmed, 29 The (x, x') and (y, y') values ​​obtained by Si-NMR measurement were an average of 3.1 and 1.0, respectively. ( 1 H-NMR results) 1 H-NMR (400MHz, CO(CD 3 ) 2 ) δ: 7.18~7.66(Ph), 4.77-4.86(Si-H), 0.28-0.43(O 3 SiMe), -0.02 to 0.13 (O 2 Sim 2 ). ( 29 Si-NMR results) 29 Si-NMR (99MHz, THF-d 8 )δ: 7.35~10.1( Me3 M 1 ), -18.3~-21.9( Me2 D 2 ), -34.8~-36.2( H,Me D 2 ) , -64.0 to -65.2 ( Me T 3 ), -78.7~-79.9( Ph T 3 ).

[0045] [Example 1-1] [ka]

[0046] In a 50 mL three-necked round-bottom flask, add 34 mL of THF, 7 mL of pure water, and palladium hydroxide / charcoal. 69 mg of phosphate was added, a thermometer was set, the mixture was stirred with a magnetic stirrer, and nitrogen was flowed in. A solution of 10 g of polymer (A) in 20 mL of THF was added dropwise, and the mixture was stirred at room temperature overnight. Ethyl acetate was added to the reaction solution, and palladium hydroxide / carbon was filtered using Celite. After separation, the organic layer was dried over sodium sulfate and concentrated under reduced pressure. After reprecipitation with heptane, the precipitate was dried in vacuum to obtain 9.8 g of a white solid (B). The molecular weight was measured by GPC, and the weight average molecular weight Mw was 113,600, and the polydispersity Mw / Mn was 3.5. 1 The appearance of the SiOH group signal by H-NMR, 29 From Si-NMR measurements H,Me D 2 The appearance of a signal (around -35 ppm) was confirmed, and the conversion rate from SiH to SiOH was 25%. ( 1 H-NMR measurement results) 1 H-NMR (400MHz, CO(CD 3 ) 2 ) δ: 7.15-7.64(Ph), 4.73~4.82(Si-H), 6.27(Si-OH, broad), 0.25~0.39(O 3 SiMe), -0.04 to 0.12 (O 2 Sim 2 ). ( 29 Si-NMR measurement results) 29 Si-NMR (99MHz, CO(CD 3 ) 2 )δ: -17.8~-21.6( M e2 D 2 ), -34.3~-35.9( H,Me D 2 ), -55.5~-56.8( Me T 2), -63.5~-64.7( Me T 3 ), -78.4~-79.2( Ph T 3 ).

[0047] [Synthesis Example 2] We synthesized siloxane polymers with only terminal SiOH groups, without any OH groups in the side chains. [ka]

[0048] Compound (α) 20g, D 47.5g, and toluene 44.4g were added to a 200mL four-neck round-bottom flask, and a thermometer, reflux tube, mechanical stirrer, and oil bath were set, and nitrogen was flowed. 2.07g of sulfuric acid was added while stirring. After stirring at reflux temperature for 1 hour, it was cooled to 80℃ and aged at 80℃ for 4 hours. Heating and stirring were stopped, water was added, and the reaction solution was washed with water several times, and then treated with Kyoward 500 to remove the acid. After filtration, the filtrate was concentrated at about 50℃. The filtrate was reprecipitated with heptane and dried in vacuum to obtain 10.3g of white solid (C). The molecular weight was measured by GPC, and the weight average molecular weight Mw was 30,000 and the polydispersity Mw / Mn=1.7. 1 H-NMR showed that (x,x') was 3.9 on average. ( 1 H-NMR measurement results) 1 H-NMR (400MHz, CO(CD 3 ) 2 ) δ: 7.11-7.63(Ph), 5.03~5.05(Si-OH), 0.25~0.38(O 3 SiMe), -0.07 to 0.12 (O 2 Sim 2 ). ( 29 Si-NMR measurement results) 29 Si-NMR (99MHz, CO(CD 3 ) 2 )δ: -12.2~-13.7( M e2 D 1 ), -18.1~-21.6( Me2 D 2 ), -55.1( Me T 2 ), -64.2~-64.7( Me T 3 ), -78.6~-79.3( Ph T 3 ).

[0049] [Example 2-1, Comparative Examples 2-1 to 2-2] In the compositions shown in Table 1, polymer B obtained in Example 1-1, polymer C obtained in Synthesis Example 2, and polymer D, a commercially available PDMS, were each dissolved in dehydrated toluene, and MS-51 and dibutyltin dilaurate were added and stirred to prepare the compositions of Example 2-1 and Comparative Examples 2-1 and 2-2. After degassing the obtained siloxane polymer composition, the solution was cast onto a substrate and heated and crosslinked in an oven at 70°C for 20 minutes, 100°C for 1 hour, and 200°C for 2 hours. After cooling, the film was peeled off from the substrate to obtain a crosslinked product.

[0050] The physical properties were determined as follows. Glass transition temperature: The temperature at the top of the peak of the loss modulus (E") in dynamic viscoelasticity measurement by DMA. Apparent crosslink density: The apparent crosslink density was calculated from the storage modulus in the rubber-like plateau region according to the following formula. n=E' / 3RT n: Crosslink density (mol / m 3 ), E': storage modulus (Pa), R: gas constant ((Pa m 3 ) / (K mol)), T: temperature (K) Coefficient of linear expansion (CTE): Measured by TMA. The maximum value of the coefficient of thermal expansion calculated from the TMA results of the first scan (first heating, heating rate: 5°C / min) in the temperature range of 50°C to 180°C in 10°C increments from 50°C to 180°C.

[0051] [Table 1]

[0052] By forming a film from a siloxane polymer with hydroxyl groups at the pendant positions of the polymer using a crosslinking agent, it is possible to increase the glass transition temperature and apparent crosslink density compared to the comparative example, and significantly reduce the coefficient of linear thermal expansion. The coefficient of linear thermal expansion of silicone is usually higher than 200 ppm / K, and a lower coefficient means that expansion is suppressed more than with normal silicone films. Therefore, when used as a substrate with wiring, expansion can be suppressed even if heat is applied during the process, and the wiring can be prevented from breaking. [Industrial Applicability]

[0053] The crosslinked products obtained by crosslinking the siloxane polymer according to the present invention have a low coefficient of linear thermal expansion and a high glass transition temperature, and are particularly suitable for use as electronics components.

Claims

1. A siloxane polymer comprising a repeating unit represented by formula (1) and having a weight average molecular weight of more than 30,000. 【Chemistry 1】 In the above formula, R 0 is independently phenyl or cyclohexyl; R 1 are independently a hydrogen atom, phenyl, cyclohexyl, or alkyl having 1 to 5 carbon atoms; R 2 and R 3 are each independently a hydrogen atom, phenyl, cyclohexyl, or alkyl having 1 to 5 carbon atoms; p is 1; x represents a real number from 1 to 8; y1+y2 represent a real number from 1 to 8, y1 being 0.25 or more, and y2 being 0 or more and less than 8.

2. A siloxane polymer composition comprising the siloxane polymer of claim 1, a crosslinker, and a transition metal catalyst.

3. 3. The siloxane polymer composition according to claim 2, which gives a crosslinked product having a maximum linear expansion coefficient of less than 200 ppm / K, calculated in the range from 50° C. to 180° C. in 10° C. increments.

4. 4. The siloxane polymer composition according to claim 2 or 3, which gives a crosslinked product having a glass transition temperature of 0° C. or higher.

5. The crosslink density n calculated by the following formula (α) is 150 mol / m 3 The siloxane polymer composition according to any one of claims 2 to 4, which gives a crosslinked product having the above properties. n=E' / 3RT...(α) n: crosslinking density (mol / m 3 ), E': storage modulus (Pa), R: gas constant ((Pa m 3 ) / (K mol)), T: temperature (K)

6. A crosslinked product obtained by crosslinking the siloxane polymer composition according to any one of claims 2 to 5.

7. 7. The crosslinked body according to claim 6, having a maximum linear expansion coefficient calculated in the range from 50°C to 180°C in 10°C increments of less than 200 ppm / K.

8. The crosslinked product according to claim 6 or 7, which has a glass transition temperature of 0°C or higher.

9. The crosslink density n calculated by the following formula (α) is 150 mol / m 3 The crosslinked body according to any one of claims 6 to 8, wherein n=E' / 3RT...(α) n: crosslinking density (mol / m 3 ), E': storage modulus (Pa), R: gas constant ((Pa m 3 ) / (K mol)), T: temperature (K)

10. A method for producing a siloxane polymer having a repeating unit represented by formula (1) and a weight average molecular weight of more than 30,000, comprising the step of converting a hydrosilyl group of a siloxane polymer having a repeating unit represented by formula (1') into a silanol group in the presence of a transition metal catalyst. 【Chemistry 2】 In the above formula, R 0 is independently phenyl or cyclohexyl; R 1 are independently a hydrogen atom, phenyl, cyclohexyl, or alkyl having 1 to 5 carbon atoms; R 2 and R 3 are each independently a hydrogen atom, phenyl, cyclohexyl, or alkyl having 1 to 5 carbon atoms; p is 1; x represents a real number from 1 to 8; y1+y2 represent a real number from 1 to 8, y1 being 0.25 or more, and y2 being 0 or more and less than 8.

11. The method for producing a siloxane polymer containing a repeating unit represented by formula (1) according to claim 10, wherein the transition metal catalyst is a palladium catalyst.

Citation Information

Patent Citations

  • MPLS network system and node

    JP2006033307A

  • Crosslinkable silicon compound, method for producing the same, crosslinkable composition, siloxane polymer, silicone membrane, silicon compound used as raw material of the crosslinkable silicon compound, and method for producing the same

    JP2010116464A