BLUE TO UV UP-CONVERTER COMPRISING LANTHANIDE IONS SUCH AS Pr3+ ACTIVATED AND OPTIONALLY Gd3+ CO-ACTIVATED SILICATES, AND ITS APPLICATION FOR SURFACE DISINFECTION PURPOSES
Silicate-based materials doped with praseodymium and gadolinium ions efficiently convert blue/green light to UV radiation, addressing low efficiency issues in existing upconversion materials, offering effective disinfection and meeting environmental and longevity criteria.
Patent Information
- Application Number
- JP2024135344
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-10-14
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-13
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024160354000001_ABST
Abstract
Description
[Technical field]
[0001] A silicate-based lanthanide ion-doped material for converting electromagnetic radiation energy of long wavelengths less than 530 nm into electromagnetic radiation energy of short wavelengths in the range of 220-425 nm, the material being a crystalline silicate material doped with lanthanide ions selected from praseodymium, gadolinium, erbium, neodymium, and in case of co-doping, at least two of them. Moreover, the silicate-based material is obtained in particular by subjecting a mixture containing a salt and an organic solvent to a specific calcination process and tribological impact to adjust the particle size and increase the crystallinity of the particles. The silicate-based material can be used to inactivate microorganisms or cells under exposure to electromagnetic radiation energy of long wavelengths less than 500 nm. [Background technology]
[0002] With the invention of InN, GaN semiconductor materials (365-500 nm) that efficiently emit blue or ultraviolet A (UV-A) light, inorganic solid-state light sources have surpassed other lighting technologies such as incandescent and discharge lamps, so that indoor and outdoor lighting are dominated by phosphor-converted light-emitting diodes (pcLEDs), which utilize inorganic semiconductor materials (InN, GaN) as the primary radiation source.
[0003] This situation is expected to change over the next few decades, as light sources using blue-emitting InN and GaN LEDs as the primary radiation source will penetrate and become the majority in all types of lighting application areas (e.g., indoor lighting, outdoor lighting, advertising lighting, architectural lighting, decorative lighting, specialty lighting, and street lighting).
[0004] Thus, indoor lighting will utilize semiconductor light sources with an emission band of 400-480 nm, partially converted by inorganic phosphors to other colors to obtain white light, but remaining in the blue spectral range, depending on the color temperature, aimed at about 5-10% of the total power distribution. This radiation will then force the excitation of an illuminated upconverter, obtaining UV radiation at the point of illumination.
[0005] Recently, this incident prompted 2 SiO 5 A dedicated research and development project has been launched with the aim of identifying efficient blue to UV-C upconversion materials such as Pr, Gd, Li, etc. The main challenge with the materials discovered and published so far is the low upconversion efficiency, which is just below the detection level or detection signal-to-noise ratio.
[0006] Furthermore, US Patent No. 5,999,633 discloses a phosphor-containing composition capable of converting initial electromagnetic energy (A) into electromagnetic energy (B) to inactivate or kill microorganisms, although the method described therein does not provide a phosphor with upconversion properties.
[0007] What is truly needed are upconverting materials that can significantly reduce infectious microorganisms within a typical daylight period, i.e., within a few hours, thus providing efficient daily microbial reduction. Furthermore, the material must be environmentally harmless and exhibit a service life of at least 10,000 hours. Finally, to achieve widespread penetration into such surface coatings, the material must be cost-effective and recyclable.
[0008] Furthermore, since only the remaining 5-10% of the LED's overall power distribution remains in the blue spectral range and should be used to force excitation of the illuminated upconverter to obtain UV radiation at the illumination point, the efficiency of the upconversion material must be much better than known materials. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] U.S. Patent Publication No. 2013 / 0052079 Summary of the Invention [Problem to be solved by the invention]
[0010] It is therefore an object of the present invention to provide inorganic materials that efficiently upconvert blue / green to ultraviolet radiation, as well as methods for making said materials. [Means for solving the problem]
[0011] The subject matter is solved by the disclosed novel blue / green to ultraviolet upconverting inorganic silicate-based materials, their preparation methods and their application in coatings, matrix material surfaces, thin films and composite layers. Particularly preferred embodiments are disclosed in the dependent claims and the description. One preferred embodiment of the present invention is a compound having the ideal general formula A 1-x-y-z B* y B 2 SiO 4 :Pr x and Gd as required z Pr represented by 3+ activation and Gd 3+ Co-doped silicate, especially A 1-x-y-z B* y B 2 SiO 4 :Pr x and Gd as required z (Wherein, A=Mg, Ca, Sr, Ba; B=Li, Na, K, Rb, Cs, preferably Li, Na, K, particularly preferably Li; B*=Li, Na, K, Rb, Cs, preferably Na, K). In both formulas, x = 0.0001 to 0.05, preferably 0.001 to 0.05, z = 0 or z = 0.0001 to 0.3, preferably 0.001 to 0.3, y = x + z (wherein y = 0.0001 to 0.35, preferably i) when z = 0, y = x, and ii) when z = 0.001 to 0.3, y = 0.0002 to 0.35), and B* y Pr x and Gd z A preferred example is Ca 0.98 Pr 0.01 Na 0.01 Li 2 SiO 4 or Ca 0.96 Pr 0.01 Gd 0.01 Na 0.02 Li 2 SiO 4 It is.
[0012] Alternatively, the ideal general formula is A 1-2x-2z B* x+z B 2 SiO 4 :Pr x , Gd z (In the formula, x+z in B* is Pr x and Gd z ) may be used.
[0013] Another embodiment of the present invention relates to the incorporation of such Vis and / or UV radiation upconverter materials into a polymer matrix.
[0014] The silica-based material according to the present invention doped with lanthanide ions is capable of reducing the microbial concentration on a surface when illuminated by sunlight or an LED lamp.
[0015] The subject of the present invention is to provide a UV-emitting material, in particular a material capable of emitting electromagnetic radiation energy at wavelengths in the range of 220-425 nm, in particular 240 nm-320 nm, most preferably 250-320 nm. Praseodymium and gadolinium co-doped silicate shows a very strong emission at 311 nm (FIG. 26). Another subject of the present invention is to provide a composition or film comprising at least one photoluminescent inorganic microscale particle for self-disinfection purposes. These particles are capable of converting blue-green (380-550 nm) photons into UV photons, a process known as up-conversion. In particular, the particles have a crystalline content of more than 70%, in particular more than 80%, more than 90%, more preferably more than 95%, more preferably more than 98%, most preferably more than 99%. The degree of crystallinity can be evaluated by methods known to those skilled in the art (crystallographers) using Rietveld analysis (Madsen et al., Description and Survey of Methods for Determining Amorphous Content by X-ray Powder Diffraction, Z. Kristallog 226 (2011) pp. 944-955).
[0016] According to a main aspect of the present invention, the silicate-based lanthanide ion-doped material, which is a UV-emitting material, in particular capable of emitting electromagnetic radiation energy at wavelengths in the range of 220-425 nm, in particular 240-320 nm (short wavelengths), is not harmful to microorganisms even when not irradiated, in particular when irradiated with wavelengths in the range of 450 nm and above, in particular when irradiated with wavelengths in the range of 450-530 nm. Irradiation of the silicate-based lanthanide ion-doped material, which is a UV-emitting material, with wavelengths in the range of 450 nm and above, in particular when irradiated with wavelengths in the range of 450-530 nm, induces the emission of electromagnetic radiation energy at (short) wavelengths in the range of 220-425 nm, in particular 240-320 nm, which is harmful to microorganisms.
[0017] The present invention relates to a method for producing 3+ doped with, and optionally with, Gd 3+ This was achieved by using a host silicate-based material co-doped with - Blue light (wavelengths less than 500 nm) causes Pr3+ Ground state configuration of [Xe]4f 2 of 3 H 4 From level 3 P 0,1,2 Absorption occurs via a transition to an excited state, with photon energies corresponding to photons having wavelengths in the range of 440-490 nm. - In the second step, 3 P 0 After relaxation to the excited state, the blue pump source is again utilized, and the excited state absorption is reduced to the excited state configuration [Xe]4f 1 5d 1 This involves the excited-state absorption that results in the occupation of the excited-state configuration [Xe]4f in the spectral range of 220–250 nm. 1 5d 1 Therefore, suitable luminescent materials must and are claimed to exhibit suitable crystal field splittings in order to obtain 5d excited states in this spectral range. - After excitation, the excited state configuration [Xe]4f 1 5d 1 The lowest crystal field component of returns to the ground state upon emission of a photon, resulting in UV emission.
[0018] Claimed Gd 3+ The co-doping of materials with Pr 3+ and Gd 3+ This results in energy transfer between the two, followed by the main emission at 311 nm.
[0019] Currently, pcLEDs are the most efficient white light source and are therefore widely used in all kinds of general lighting applications. Best practice bluish-white pcLEDs have wall plug efficiencies of nearly 60%, with radiant flux in the range of a few light watts per pcLED. Upconversion methods can achieve efficiencies of around 25%, with at least 500 lm / m for indoor lighting. 2 or 5 W / m 2 It is very interesting that this method uses the blue-green part of the emission spectrum for so-called low-dose disinfection of surfaces, since (for a light source of 100 lm / W) is required.
[0020] According to the present invention, up-conversion means the conversion of electromagnetic radiation energy of longer wavelengths, in particular less than 500 nm, preferably in the range of 365-500 nm, most preferably in the range of 440-490 nm, into electromagnetic radiation energy of shorter wavelengths, in particular in the range of 220-425 nm, preferably in the range of 250-325 nm.
[0021] The subject of the present invention is therefore a silicate-based lanthanide ion-doped material for converting long wavelength electromagnetic radiation energy to short wavelength electromagnetic radiation energy; a crystalline silicate material doped with lanthanide ions, preferably lanthanide ions (III+), selected from praseodymium, gadolinium, erbium, neodymium, and in the case of co-doping, selected from at least two of them, In particular, less than 530 nm, preferably less than 500 nm, for example 365 to 500 nm, in particular The material converts at least one long wavelength electromagnetic radiation energy in the range of 440 to 495 nm, most preferably 440 to 490 nm, into at least one short wavelength electromagnetic radiation energy in the range of 220 to 425 nm, particularly 250 to 350 nm, more preferably 250 to 320 nm. In particular, the crystalline silicate material is doped or co-doped with lanthanide ions, the lanthanide ions being selected from lanthanide ions (III+).
[0022] According to the most preferred embodiment of the invention, the subject of the invention is a silicate-based lanthanide ion-doped material for converting long-wavelength electromagnetic radiation energy into short-wavelength electromagnetic radiation energy, which is a crystalline silicate material doped with lanthanide ions (III+) selected from praseodymium (III+), gadolinium (III+), erbium (III+), neodymium (III+) and, in the case of co-doping, from at least two of these ions (III+).
[0023] According to the most preferred embodiment of the present invention, the lanthanide ion is praseodymium(III+) (Pr 3+ ), Gadolinium(III+)(Gd 3+ ), Erbium(III+)(Er 3+ ) and neodymium(III+)(Nd 3+ ) and in case of co-doping, at least two of them are selected. In a preferred embodiment, the silicate-based lanthanide ion-doped material does not contain lanthanide ions (IV+), in particular due to calcination under a reducing atmosphere.
[0024] Thus, the material according to the present invention, when irradiated with at least one long wavelength electromagnetic radiation energy of less than 530 nm, particularly 440-495 nm, preferably 440 nm-490 nm, emits at least one short wavelength electromagnetic radiation energy in the range of 220-425 nm, particularly 250-350 nm, more preferably 250-320 nm.
[0025] According to Figures 11 and 12, CaLi 2 SiO 4 : Pr, Na (1 mol%) ((Ca 0.98 Pr 0.01 Na 0.01 )Li 2 SiO 4 and CaLi 2 SiO 4 : Pr, Gd (1 mol%), also known as Na (2 mol%), (Ca 0.96 Pr 0.01 Gd 0.01 Na 0.02 )Li 2 SiO 4 The emission spectrum of ) clearly shows a range from 275 to 375 nm, with an intensity of at least 1 × 10 5 Counts / (mm 2 *s) (Excitation laser: 445 nm, 75 mW). When excited with a 488 nm laser and an efficiency of 150 mW (see Figures 11 and 12), CaLi 2 SiO 4: Pr, Na (1 mol%) ((Ca 0.98 Pr 0.01 Na 0.01 )Li 2 SiO 4 and CaLi 2 SiO 4 : Pr, Gd (1 mol%), also known as Na (2 mol%), (Ca 0.96 Pr 0.01 Gd 0.01 Na 0.02 )Li 2 SiO 4 ), which clearly shows an emission spectrum intensity in the range of 225 to 425 nm, with the intensity maximum being at least 1 × 10 in the subrange of 230 to 325 nm, and, if necessary, in the subrange of 365 nm to 425 nm. 5 Counts / (mm 2 *s) is particularly popular. Preferred is an intensity maximum in the range of 275 nm to 320 nm, in particular at least 2 × 10 5 Counts / (mm 2 *s), more preferably 2.5 × 10 5 Counts / (mm 2 When excited with a 488 nm laser and an efficiency of 150 mW, or with a 445 nm laser and an efficiency of 75 mW (see Figure 12), CaLi 2 SiO 4 : Pr, Gd (1 mol%), Na (2 mol%) ((Ca 0.98 Pr 0.01 Gd 0.01 Na 0.02 )Li 2 SiO 4 ) emission spectrum, which clearly shows additional intensity in the range of 300-320 nm, especially at 312 nm, with a maximum intensity of at least 5 × 10 5 Counts / (mm 2 *s), especially at least 6 × 10 5 Counts / (mm 2 *s), more preferably at least 7 × 10 5 Counts / (mm 2 *s). Strong emission at about 312 nm is produced by gadolinium (Gd).
[0026] The intensity of the electromagnetic spectrum emitted in the range of 220-425 nm is at least 5 × 10 4 Counts / (mm 2 *s), preferably at least 1 × 10 5 Counts / (mm 2 *s), more preferably at least 2 × 10 5 Counts / (mm 2 *s). In particular, 220 The intensity of the electromagnetic spectrum emitted in the range of ~330 nm is at least 2 × 10 5 Counts / (mm 2 *s), which is the strong electromagnetic spectrum emitted in the range of 220 to 425 nm. Degrees are at least 2 x 10 5 Counts / (mm 2 The emission spectrum is The laser is excited with a laser, in particular with a laser having an efficiency of 75 mW at 445 nm and / or an efficiency of 150 mW at 488 nm.
[0027] The preferred maximum value of the converted electromagnetic radiation energy is in the range of 250 to 350 nm, particularly 250 to 350 nm, and most preferably 280 to 330 nm.
[0028] A preferred silicate-based material is praseodymium doped and co-doped with gadolinium, particularly a crystalline silicate material is praseodymium doped and co-doped with gadolinium.
[0029] According to one aspect of the invention, silicate-based materials are preferred, and crystalline silicate materials doped with lanthanide ions are, for example, cyclosilicates (e.g., [Si 3 O 9 ] 6- , [Si 4 O 12 ] 8- and / or [Si 6 O18 ] 12- ), pyrosilicates (e.g. [Si 2 O 7 ] 6- ), and inosilicates (so-called chain silicates with an atomic ratio of Si:O=1:3 for single chains and Si:O=4:11 for double chains).
[0030] A preferred subject of the present invention is a silicate-based lanthanide ion-doped material for converting long-wavelength electromagnetic radiation energy into short-wavelength electromagnetic radiation energy, the silicate-based material being doped with lanthanide ions (III+) (Ln 3+ ) doped crystalline silicate material, in particular obtained by heating, preferably calcining, said silicate-based lanthanide ion doped material in a reducing atmosphere, in particular to a temperature above 600°C and below the melting point, preferably 50°C to 200°C below the melting point, in a reducing atmosphere. The reduction step after a prior calcination in air is particularly relevant for increasing the amount of lanthanide ions (III+) and thus increasing the upconversion intensity of the material. According to a most preferred embodiment, the crystalline silicate material is doped or co-doped with lanthanide ions, the lanthanide ions being selected from the lanthanide ions (III+).
[0031] According to one aspect of the invention, silicate-based materials are preferred, and the crystalline silicate materials doped with lanthanide ions are selected from silicates that are free of water of crystallization, crystalline solvates with -OH functionality. In particular, lanthanide ions, preferably Ln 3+ , and most preferably more than 95% Ln 3+ and less than 5% Ln 4+ The doped crystalline silicate material is selected from silicates that are free of stoichiometric hydrates and / or solvates.
[0032] Particularly preferred are silicate-based materials, i) where the crystalline silicate material is not a silicate hydrate, in particular the silicate does not contain water of crystallization. Water-free silicates are also preferred. Water adsorbed or on the surface of the silicate-based material is not considered water from silicate hydrate or crystallization. Nevertheless, it is preferred that the silicate-based material does not contain water adsorbed and does not contain water on the surface of the particles of the material.
[0033] It is particularly preferred that the crystallinity of the silicate-based material, in particular the crystallinity of the particles having the particle size distribution disclosed above, is greater than 70%, in particular the crystallinity of the material is 80% or more, more preferably 85% or more, 90% or more, 95% or more, most preferably 98% or more, 99% or more, 99.5% or more, 99.8% or more (analysis example: half of the peak of the long-term XRPD Width grain size measurement and Debye-Scherrer equation; strongest The height of the reflections may also be used (XRPD, Rietveld analysis).
[0034] Furthermore, the silicate-based material is in particular free of amorphous phase, where free of amorphous phase in the silicate-based material means less than 5%, preferably less than 2%, most preferably less than 1%, less than 0.01%, less than 0.001%, less than 0.0001% (analysis see above, XRPD, Rietveld analysis).
[0035] More preferred are silicate-based materials, which are crystalline silicate materials including: i) A crystalline pure phase. In particular, the crystalline material comprises a crystalline phase, in particular one crystalline phase, which comprises 90% by weight of the crystalline material. In particular, the crystalline phase comprises 95% or more by weight of the crystalline material (100% by weight), more preferably 98% or more by weight, most preferably 99%, 99.5% or 99.8% by weight. Alternatively, ii) The silica-based material comprises at least one crystalline phase, in particular one crystalline phase, comprising 90% by weight, in particular at least 95% by weight, more preferably at least 98% by weight, at least 99% by weight, at least 99.5% by weight, at least 99.8% by weight, at least 99.9% by weight of the silica-based material (100% by weight).
[0036] Most preferred are crystalline phase pure (ie, containing no distinct crystalline or amorphous phases) silicate-based materials.
[0037] According to another aspect of the invention, the crystalline silicate material is preferably a solid solution of lanthanide ions doped with at least one alkali ion and at least one earth alkali ion, in particular a silicate doped with praseodymium and optionally co-doped with gadolinium. Particularly preferred are lanthanide doped crystalline silicates selected from praseodymium and optionally gadolinium ions, with at least one alkali ion selected from Li, Na, K, Rb, Cs, preferably Li and optionally Na or K, most preferably Li and optionally Na, and at least one earth alkali ion selected from Mg, Ca, Sr, Ba, preferably Ca. Most preferred are the above crystalline silicates, with a crystallinity of 90% or more, preferably 95% or more, and an average particle size D 50 is in the range of 1 μm to 20 μm, preferably in the range of 5 to 15 μm.
[0038] Preferred crystalline silicate materials doped with lanthanide ions and containing at least one alkali ion and at least one earth alkali ion are water-free silicates or silicates containing no water of crystallization (e.g., cyclosilicates ([Si 3 O 9 ] 6- , [Si 4 O 12 ] 8- , [Si 6 O 18 ] 12- ), pyrosilicate ([Si2 O 7 ] 6- ) and inosilicate (chain silicate, silicate containing no crystal water selected from Si:O=1:3 (single chain), Si:O=4:11 (double chain)).
[0039] A particularly preferred embodiment of the present invention is a silicate- or silica-based material, the crystalline silicate material being selected from the idealized general formula I: A 1-x-y-z B* y B 2 SiO 4 :Ln 1 x,, Ln 2 z, (I) (In the formula, x=0.0001 to 0.05, z=0 or z=0.0001 to 0.3, and y=x+z, A is selected from Mg, Ca, Sr and Ba; B is selected from Li, Na, K, Rb and Cs; B* is selected from Li, Na and K, B is equal to or unequal to B*, preferably B is unequal to B*; Ln 1 is selected from praseodymium (Pr), erbium (Er), and neodymium (Nd); Any Ln 2 is selected from gadolinium (Gd).
[0040] Most preferred are crystalline silicates of formula I above, having a crystallinity of 90% or more, preferably 95% or more, and an average particle size D 50 is in the range of 1 μm to 20 μm, preferably in the range of 5 to 15 μm.
[0041] A further preferred embodiment of the present invention is a silicate- or silica-based material, wherein the crystalline silicate material is selected from the idealized general formula Ia: A 1-x-y-z B* y B 2 SiO 4 :Prx, Gd z, Ia (Wherein A=Mg, Ca, Sr, Ba, and B=Li, Na, K, Rb, Cs, and x=0.0001~0.05, z=0 or z=0.0001~0.3, and y=x+z, B* is selected from Li, Na and K, and K is an element for charge balance of the silicate. It exists for the purpose of B is equal to or unequal to B*, and preferably B is unequal to B*.
[0042] Most preferred are silicate-based materials, where the crystalline silicate material is selected from the idealized general formula II: (Ca 1-a Sr a ) 1-2b Ln b Na b Li 2 SiO 4 II (In the formula, a=0.0001 to 1, preferably 0.0001 to 0.1, b=0.0001 to 1, preferably 0.0001 to 0.1, or a=0 or 0.0001 to 0.1, preferably a=0, b=0.0001 to 0.35, preferably b=0.001 to 0.1; Ln is a lanthanide ion selected from praseodymium, gadolinium, erbium, and neodymium, and in the case of co-doping, is selected from at least two of them, and in particular, praseodymium and, if necessary, gadolinium are preferred.
[0043] The preferred silicate-based lanthanide ion-doped material according to the present invention is 0.9998-0.9 B* 0.0001-0.05 B 2 SiO 4 :Pr 0.0001-0.05 and A 0.9998-0.30 B* 0.0001-0.35 B 2 SiO 4 :Pr 0.0001- 0.05 Gd 0.0001-0.30 where A is selected from Mg, Ca, Sr, Ba, B is selected from Li, Na, K, Rb, Cs, preferably Li, Na, K, more preferably Li, and B* is selected from Na and K.
[0044] Particularly preferred is Ca 0.98 Pr 0.01 Na 0.01 Li 2 SiO 4 , Ca 0.96 Pr 0.01 Gd 0.01 Na 0.02 Li 2 SiO 4 , Sr 0.98 Pr 0.01 Na 0.01 Li 2 SiO 4 , Sr 0.96 P r0.01 Gd 0.01 Na 0.02 Li 2 SiO 4 It is.
[0045] For example, SrLi 2 SiO 4 :Pr 3+ The silicate-based crystalline materials according to the invention based on strontium as an earth alkali ion, such as SrLi, show an emission in the range 254 to 375 nm, with a maximum at 320 nm. 2 SiO 4 :Pr 3+ , Gd 3+ It emits at 254-375 nm, with a maximum at 312 nm.
[0046] In particular, the crystalline silicate material comprises at least two different alkali ions. More preferred crystalline silicate materials comprise at least one earth alkali ion and at least two different alkali ions.
[0047] According to one aspect of the invention, the silicate-based material, the crystalline silicate material of formula 2, has XRPD signals, particularly high intensity signals in the ranges of 23°2Θ to 27°2Θ and 34°2Θ to 39.5°2Θ, particularly in the ranges of 24.4°2Θ to 25.4°2Θ and 36.8°2Θ to 37.8°2Θ. In particular, the signals are measured according to a Bragg-Brentano type geometry using Cu-Kα radiation.
[0048] The subject of the present invention is also silicate-based crystalline materials doped with praseodymium and optionally co-doped with gadolinium selected from the following list: Surprisingly, it has been found that these materials exhibit a fairly efficient blue to ultraviolet upconversion. Mg 1-x-y-z Pr x Gd z B* y Li 2 SiO 4 (x=0.0001~0.05, Preferably 0.001 to 0.05, z=0) and Gd (z=0.0001 to 0.3) as needed Ca 1-x-y-z Pr x Gd z B* y Li 2 SiO 4 (x=0.0001~0.05, Preferably 0.001 to 0.05, z=0) and Gd (z=0.0001 to 0.3) as needed Sr 1-x-y-z Pr x Gd z B* y Li 2 SiO 4 (x=0.0001~0.05, Preferably 0.001 to 0.05, z=0) and Gd (z=0.0001 to 0.3) as needed Ba 1-x-y-z Pr x Gd z B* y Li 2 SiO 4:Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Mg 1-x-y-z Pr x Gd z B* y Na 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Ca 1-x-y-z Pr x Gd z B* y Na 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Sr 1-x-y-z Pr x Gd z B* y Na 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Ba 1-x-y-z Pr x Gd z B* y Na 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Mg 1-x-y-z Pr x Gd z B* y K 2 SiO 4 :Pr(x=0.0001~0.0 5, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Ca 1-x-y-zPr x Gd z B* y K 2 SiO 4 :Pr(x=0.0001~0.0 5, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Sr 1-x-y-z Pr x Gd z B* y K 2 SiO 4 :Pr(x=0.0001~0.0 5, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Ba 1-x-y-z Pr x Gd z B* y K 2 SiO 4 :Pr(x=0.0001~0.0 5, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Mg 1-x-y-z Pr x Gd z B* y Rb 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Ca 1-x-y-z Pr x Gd z B* y Rb 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Sr 1-x-y-z Pr x Gd z B* y Rb 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3) Ba 1-x-y-z Pr x Gd z B* y Rb 2 SiO 4 :Pr(x=0.0001~0. 05, preferably 0.001 to 0.05, z=0) and optionally Gd (z=0.0001 to 0.3), In all formulas, B* is an additional alkali metal selected from Li, Na, K. , may be equal to or different from B. Preferably, B and B* are alkali metals. Selected from the genus, they are different.
[0049] The particle size of the silica-based crystalline material is preferably in the range of 1 μm to 100 μm, more preferably in the range of 1 μm to 50 μm, and more preferably in the range of 1 μm to 20 μm.
[0050] Preferably, the average particle size (D 50 ) is preferably in the range of 1 μm to 100 μm, more preferably in the range of 1 μm to 50 μm, and even more preferably in the range of 1 μm to 20 μm. More preferably, the average particle diameter (D 50 ) is in the range of 2 μm to 20 μm, more preferably in the range of 5 μm to 20 μm, more preferably in the range of 5 μm to 15 μm, in particular about 10 μm ± 5 μm. According to one particularly preferred embodiment, the particle size distribution is 10 = 2 to 7 μm, D 50 = 5 to 15 μm, and D 90 = less than 20 μm, preferably less than 18 μm. Particle size distribution was measured by dynamic laser light scattering using a Horiba LA-950-V2 organic particle size analyzer.
[0051] All silicate-based crystalline materials according to the invention contain at least a trivalent activator Pr 3+ and has the ground state configuration [Xe]4f 2is the excited configuration [Xe]4f 1 5d 1 The 13 lowest crystal field components are located below the S L J By appropriately selecting the host material, Pr 3+ The lowest crystal field component of the excited configuration of is the ground state level belonging to the ground state configuration. 3 H 4 More than 35,000~40,000cm -1 In this way, a two-photon absorption process in a single ion is possible, resulting in the emission of a UV photon.
[0052] In particular, the present invention relates to 3+ Doped silicate-based materials, and materials treaded according to the present invention, provide blue to UV radiation upconverter materials, which , which is far more efficient than anything previously published in patents and peer-reviewed literature.
[0053] According to a further subject matter of the invention, the excited state configuration [Xe]4f located in the spectral range of 220-250 nm 1 5d 1 A silicate-based lanthanide-doped material having a crystal field component of
[0054] According to a further subject matter of the invention, there is provided an excited state configuration [Xe]4f having an emission in the spectral range of 250-320 nm. 1 5d 1 A silicate-based lanthanide-doped material having a crystal field component of
[0055] Particularly preferred silicate-based materials are those that convert electromagnetic radiation energy of long wavelengths less than 500 nm, in particular less than 490 nm to 450 nm, into electromagnetic radiation energy of short wavelengths in the range of 230 nm to 380 nm. In particular, the intensity of the maximal emission of electromagnetic radiation energy of short wavelengths (in particular at least one maximum of the emitted short wavelengths, or two maxima of the emitted short wavelengths) is independently at least 1·103 Counts / (mm 2 *s), especially 1 10 4 Counts / (mm 2 *s), preferably 1·10 5 Counts / (mm 2 *s), most preferably 2·10 5 Counts / (mm 2 According to a preferred embodiment of the present invention, the luminance is greater than 1·103 counts / (mm 2 *s) and two maxima with a maximum intensity of at least 1 10 4 Counts / (mm 2 *s), preferably 1·10 5 Counts / (mm 2 *s), most preferably 2·10 5 Counts / (mm 2 *s) and a second maximum in the range of 275 nm to 380 nm are preferred. In particular, the mentioned lasers 445 nm 75 mW or 488 nm 150 mW are used.
[0056] Certain particle sizes are most favorable for enhanced release, and the disclosed materials are therefore claimed as μ-scale, sub-μ-scale to nano-scale particles in the range of 10 nm to 100 μm.
[0057] The subject of the invention is also a method for producing a silicate-based material, and a crystalline silicate-based material obtained according to said method, said method comprising the following steps: - preparing the following items i) to iii); i) at least one lanthanide salt, in particular one selected from lanthanide nitrates, lanthanide carbonates, lanthanide carboxylates, in particular lanthanide acetates, lanthanide sulfates, lanthanide oxides, in particular Pr 6 O 11 and / or Gd 2 O 3 (The lanthanide ions in the lanthanide oxide or salt are selected from praseodymium, gadolinium, erbium, neodymium, or, in the case of co-doping, from at least two of them.) ii) silicates, in particular the salts of silicates, more particularly the alkali salts of silicates; iii) at least one earth alkali salt selected from lithium salts or any lithium compound and optionally selected from sodium and potassium salts and at least one alkali salt, in particular an alkali silicate. (Preferably, the lithium salt is selected from ii) and is a lithium silicate.) - carrying out a) or b) below, a) mixing i), ii) and iii) by milling to obtain a mixture; b) mixing i), ii) and iii) in an aprotic organic polar or non-polar solvent to obtain a mixture, and calcining the mixture b) at 600°C to 1,000°C (step 1a) to remove the organic components; (In particular, the calcination is carried out at 600°C to 1,000°C under standard atmosphere (air) for at least 1 hour, in particular 2 hours or more, to obtain a calcined mixture.) - calcining the mixture of a) or the calcined mixture of b) at a temperature below the melting temperature of the silica-based material, in particular under air, at which at least partial crystallization occurs; (In the further calcination step (step 1b) for at least 3 hours at a temperature between 50 and 200° C., preferably in air, below the melting temperature of the silica-based material, the preferred temperature is 800 to 900° C., preferably about 850° C., and the crystallization takes place for at least 3 hours, in particular at least 12 hours, preferably in air.) - in a further calcination step in a reducing atmosphere at high temperatures, in particular above 800 °C and 50-200 °C below the melting temperature of the material (e.g. 850 °C), for at least 3 hours, more preferably at least 6 hours, the lanthanides are converted into Ln 3+ reducing the ions; obtaining, in particular after cooling the material, a silicate-based lanthanide ion-doped material.
[0058] The reducing atmosphere is N 2 or Argon and H 2 Another reducing atmosphere may contain an inert gas and may be a forming gas such as a mixture of CO or NH as the reducing component. 3 The gas may include gases such as
[0059] The material is preferably cooled at a rate of 100° C. / hour to 300° C. / hour, and more preferably 200° C. / hour to 300° C. / hour.
[0060] The heating and cooling in the calcination steps 1a and / or 1b are each independently performed at a heating and cooling rate of 100°C / h to 300°C / h, preferably 300°C / h. The heating and cooling in the calcination step 2 is performed at a rate of 100°C / h to 300°C / h, with heating and cooling rates of 200°C / h being preferred. A linear cooling rate is particularly preferred.
[0061] In a preferred embodiment of the invention, the obtained silicate-based lanthanide ion-doped material is ground and subjected to a tribological shock sufficient to increase the crystallinity of the material, in particular the crystallinity of the main crystalline phase of the silicate-based material, in comparison with a material that has not been subjected to the tribological shock. In particular, the amorphous phase is reduced and the crystalline phase is coordinated with the main crystalline phase. Preferably, the main reflection intensity of the silicate-based lanthanide ion-doped material is increased by at least 5%, in particular 10%, more preferably at least 20%. In the case of a silicate according to formula II, the main reflection intensity in the range of 34°2Θ to 39.5°2Θ is increased by at least 5%, more preferably at least 10%.
[0062] Yet another embodiment of the present invention is a method for tribologically impacting the obtained silicate-based material with the milled material at 200 revolutions per minute for 1-6 hours, preferably about 4 hours. The milling is carried out in a planetary ball mill (PM 200, Retsch), with a g-force of up to 37.1 g, beaker / jar: corundum and milling balls (Al 2 O 3 ), 50 mL (9 balls, approx. 4.5 g sample) or 125 mL (24 balls, approx. 20 g sample). The grinding beaker / jar is eccentrically placed on the sun wheel of the planetary ball mill. The direction of movement of the sun wheel is opposite to that of the grinding jar in a ratio of approximately 1:2. The grinding balls in the grinding beaker / jar are subjected to multiple rotational movements, the so-called Coriolis forces. Due to the difference in speed between the balls and the jar, an interaction occurs between frictional and impact forces, which releases high kinetic energy.
[0063] The preferred main reflection intensity of the resulting silicate-based lanthanide ion-doped material may be increased by at least 25%, in particular 30%, more preferably at least 40%, 50%, 60%, 70% or 80% by the milling step. In the case of the silicate according to formula II, the main reflection intensity in the range 34°2Θ to 39.5°2Θ is increased by at least 50%, more preferably at least 60%. Preferably, this milling step is the first milling step in the process to reduce particle size and unwanted phases in the solid.
[0064] The subject of the present invention is also a silicate-based lanthanide ion-doped material for converting long-wavelength electromagnetic radiation energy into short-wavelength electromagnetic radiation energy, obtainable according to the method of the present invention. the silicate-based material is a crystalline silicate material doped with lanthanide ions selected from praseodymium, gadolinium, erbium, neodymium, and in the case of co-doping, from at least two of them; The crystalline silicate-based material doped with lanthanide ions is a solid solution of crystalline silicates with at least one alkali ion, preferably with at least two different alkali ions, the degree of crystallinity of the silicate-based material being greater than 80%, in particular 80% or more, 85% or more, 90% or more, 95% or more, 98% or more, 99% or more, 99.5% or more, 99.8% or more; At least one electromagnetic radiation energy having a long wavelength of less than 530 nm, particularly in the range of 490 to 450 nm, is converted into at least one electromagnetic radiation energy having a short wavelength of less than 530 nm, particularly in the range of 220 to 400 nm, particularly in the range of 250 to 320 nm.
[0065] The long wavelength is, per regulation, always longer than the short wavelength.
[0066] According to further embodiments, compositions, foils or films comprising silicate-based materials are disclosed for self-disinfecting purposes or for reducing microorganisms. The compositions may include optional excipients, and the compositions do not include water or aprotic solvents in an amount greater than 1-15% by weight, in particular greater than 10% by weight.
[0067] The subject of the present invention is also the use of silicate-based lanthanide ion-doped materials in UV sterilization or disinfection applications, in indoor UV sterilization applications, in particular in indoor UV sterilization applications utilizing electromagnetic radiation energy from LEDs, in particular pcLEDs, having a maximum emission in the range of 450-480 nm, under exposure to electromagnetic radiation energy of long wavelengths less than 500 nm, with a maximum emission in the range of 450-480 nm. [Brief description of the drawings]
[0068] [Figure 1a] Top X-ray powder diffraction (XRPD) of the synthesized Y2SiO5 and top XRPD of the calculated Y2SiO5. [Figure 1b] Figure 1 shows the emission spectra of Y2SiO5:Pr3+ upon laser excitation at 445 nm (75 mW) and 488 nm (150 mW). [Diagram 2]Figure 1 shows the emission spectra of Ca0.98Pr0.01Na0.01Li2SiO4 upon excitation with a laser at 445 nm (75 mW) and 488 nm (150 mW). [Diagram 3] FIG. 1 is an X-ray diffraction pattern of Ca0.98Pr0.01Na0.01Li2SiO4 (Example 1) for Cu-Kα radiation. [Figure 4] 1 is an X-ray diffraction pattern of Ca0.96Pr0.01Gd0.01Na0.02Li2SiO4 (Example 2) for Cu-Kα radiation. [Diagram 5] FIG. 1 is an X-ray diffraction pattern of Sr0.98Pr0.01Na0.01Li2SiO4 (Example 3) for Cu-Kα radiation. [Figure 6] 1 is an X-ray diffraction pattern of Sr0.96Pr0.01Gd0.01Na0.02Li2SiO4 (Example 4) for Cu-Kα radiation. [Figure 7] FIG. 1 is an emission spectrum of Ca0.98Pr0.01Na0.01Li2SiO4 upon excitation at 160 nm (Example 1). [Figure 8] FIG. 1 is an emission spectrum of Ca0.96Pr0.01Gd0.01Na0.02Li2SiO4 upon excitation at 160 nm (Example 2). [Figure 9] FIG. 1 is an emission spectrum of Sr0.98Pr0.01Na0.01Li2SiO4 upon excitation at 160 nm (Example 3). [Figure 10] FIG. 1 is an emission spectrum of Sr0.96Pr0.01Gd0.01Na0.02Li2SiO4 upon excitation at 160 nm (Example 4). [Figure 11] FIG. 1 is an emission spectrum of Ca0.98Pr0.01Na0.01Li2SiO4 upon excitation with a laser at 445 nm (75 mW) and 488 nm (150 mW) (Example 1). [Figure 12] FIG. 1 shows the emission spectra of Ca0.96Pr0.01Gd0.01Na0.02Li2SiO4 upon excitation with a laser at 445 nm (75 mW) and 488 nm (150 mW) (Example 2). [Figure 13]FIG. 13 is an emission spectrum of Sr0.98Pr0.01Na0.01Li2SiO4 upon excitation with a laser at 445 nm (75 mW) and 488 nm (150 mW) (Example 3). [Figure 14] FIG. 13 is an emission spectrum of Sr0.96Pr0.01Gd0.01Na0.02Li2SiO4 upon excitation with a laser at 445 nm (75 mW) and 488 nm (150 mW) (Example 4). [Figure 15] 1 is a reflectance spectrum of Ca0.98Pr0.01Na0.01Li2SiO4 (Example 1). BaSO4 was used as a reference. [Figure 16] 1 is a reflectance spectrum of Ca0.96Pr0.01Gd0.01Na0.02Li2SiO4 (Example 2). BaSO4 was used as a reference. [Figure 17] 1 is a reflectance spectrum of Sr0.98Pr0.01Na0.01Li2SiO4 (Example 3). BaSO4 was used as a reference. [Figure 18] 1 is a reflectance spectrum of Sr0.96Pr0.01Gd0.01Na0.02Li2SiO4 (Example 4). BaSO4 was used as a reference. [Figure 19] FIG. 1 is an excitation spectrum of Ca0.98Pr0.01Na0.01Li2SiO4 monitoring emission at 300 nm (Example 1). [Figure 20] FIG. 1 is an excitation spectrum of Ca0.96Pr0.01Gd0.01Na0.02Li2SiO4 monitoring emission at 312 nm (Example 2). [Figure 21] FIG. 13 is an excitation spectrum of Sr0.98Pr0.01Na0.01Li2SiO4 monitoring emission at 320 nm (Example 3). [Figure 22] 1 is an excitation spectrum of Sr0.96Pr0.01Gd0.01Na0.02Li2SiO4 monitoring emission at 312 nm (Example 4). [Figure 23a] The increase in crystallinity of CaLi2SiO4:Pr3+ by high-energy milling (200 U / min, 4 h) and the decrease in additional phases as impurities are shown. [Figure 23b] The increase in crystallinity of CaLi2SiO4:Pr3+ by high-energy milling (200 U / min, 4 h) and the decrease in additional phases as impurities are shown. [Figure 24a] ) Particle size distribution of CaLi2SiO4:Pr3+ at 100 U / min for 4 h. [Figure 24b] Particle size distribution of CaLi2SiO4:Pr3+ at 200 U / min for 4 hours. [Figure 24c] It is shown that the release increased with increasing phase purity and crystallinity. [Figure 25a] It is shown that the release increased with increasing phase purity and crystallinity. [Figure 25b] This indicates a reduction in additional phases as impurities and an increase in crystallinity. [Figure 25c] Particle size distribution of CaLi2SiO4:Pr3+ at 200 U / min for 4 hours. [Figure 26] Simplified energy level scheme for Pr3+ (ground state configuration [Xe]4f2) and Gd3+ (ground state configuration [Xe]4f7) showing the relevant optical transitions and energy transfer processes involved in the upconversion mechanism leading to UV emission. [Figure 27a] Top is the XRPD of the extract before grinding, bottom is the calculated XRPD of CaLi2SiO4. [Figure 27b] Top is the XRPD of the ground extract and bottom is the calculated XRPD of CaLi2SiO4. [Figure 27c] Top: silicate-based lanthanide ion doped material fired (calcined) at 850°C for 12 hours in air, reflection 2Θ=37.39°, 13357 counts. Bottom: calculated XRPD of CaLi2SiO4. [Fig. 27d] Top: Second heat: 6 h, 850 °C, forming gas (H2(5%) / N2(95%)), reflection 2Θ=37.39°, 15423 counts. Bottom: Calculated XRPD of CaLi2SiO4. [Figure 27e]Top: Further grinding shows less crystallinity: reflection 2Θ=37.39°, reduced to 13576 counts. Bottom: calculated XRPD of CaLi2SiO4. [Figure 28a] Top: kesilicate-based lanthanide ion doped material (CaLi2SiO4:Pr3+,Na+) heated (calcined) at 850°C for 12 hours in air, then placed in a hot reducing atmosphere (H2 / inert gas, 850°C for 6 hours, not crushed). Reflection 2Θ=37.39°, 10964 counts. Bottom: calculated XRPD of CaLi2SiO4. [Figure 28b] Top: milled silicate-based lanthanide ion doped material after tempering in reducing atmosphere, reflection 2Θ=37.39°, 18665 counts (milling: 200 rpm for 4 hours, CaLi2SiO4:Pr3+,Na+). Bottom: calculated XRPD of CaLi2SiO4. EXAMPLES
[0069] Measurement techniques X-ray diffractograms were recorded using a PANalytical X'PertPROMPD diffractometer operating in Bragg-Brentano type geometry using Cu-Kα radiation and a line-scan CCD sensor. Integration times amounted to 20 s with a step width of 0.017°. Emission spectra were recorded on an Edinburgh Instruments FLS920 spectrometer equipped with a Coherent 488 nm continuous wave OBIS laser and a Peltier-cooled (-20°C) single-photon counting photomultiplier tube (Hamamatsu R2658P). Filters were used to suppress excitation due to secondary reflections caused by the monochromator. For grinding, after cooling in the final firing process, the powder was crushed in a planetary ball mill (PM 200, Retsch), beaker / jar: corundum and grinding balls (Al 2 O 3 ), 50 mL (9 balls, approx. 4.5 g sample) or 125 mL (24 balls, approx. 20 g sample), at 200 rpm for 4 hours. 2 / Inert gases, especially H 2 / N 2 is preferred (H 2 (5%) / N 2 (95%).
[0070] Powder sample synthesis Example 1: Ca 0.98 Pr 0.01 Na 0.01 Li 2 SiO 4 In an agate mortar, CaCO 3 3.3349g (33.3200mmol), Li 2 SiO 3 3.0588g (34.0000mmol), Pr(NO 3 ) 3 6H 2 0.1479 g (0.3400 mmol) of O, and 0.1479 g (0.3400 mmol) of Na 2 CO 3 0.0180g (0.1700mmol) was mixed in hexane. 2+ / Pr 3+ Na for charge compensation 2 CO 3 The precursor formulation was calcined in air at 700 °C for 2 h to remove organic residues. Subsequent calcination in air at 850 °C for 12 h gave the product phase. Pr 4+ Pr 3+ A final firing step at 850°C for 6 hours in a reducing atmosphere is required to reduce it to 0.05%.
[0071] Example 2: Ca 0.96 Pr 0.01 Gd 0.01 Na 0.02 Li 2 SiO 4 In an agate mortar, CaCO 3 3.2668g (32.6400mmol), Li 2 SiO 3 3.0588g (34.0000mmol), Pr(NO 3 ) 3 6H 2 O 0.1479g (0.3400mmol), Gd2 O 3 0.0616g (0.1700mmol), and Na 2 CO 3 0.0360g (0.3400mmol) was mixed in hexane. 2+ / Pr 3+ Na for charge compensation 2 CO 3 The precursor formulation was calcined in air at 700 °C for 2 h to remove organic residues. Subsequent calcination in air at 850 °C for 12 h gave the product phase. Pr 4+ Pr 3+ A final firing step at 850°C for 6 hours in a reducing atmosphere is required to reduce it to 0.05%.
[0072] Example 3: Sr 0.98 Pr 0.01 Na 0.01 Li 2 SiO 4 In an agate mortar, SrCO 3 3.6169g (24.5000mmol), Li 2 SiO 3 2.2491g (25.0000mmol), Pr(NO 3 ) 3 6H 2 0.1088 g (0.2500 mmol) of O, and Na 2 CO 3 0.0132g (0.1250mmol) was mixed in hexane. 2+ / Pr 3+ Na for charge compensation 2 CO 3 The precursor formulation was calcined in air at 700 °C for 2 h to remove organic residues. Subsequent calcination in air at 850 °C for 12 h gave the product phase. Pr 4+ Pr 3+ A final firing step at 850°C for 6 hours in a reducing atmosphere is required to reduce it to 0.05%.
[0073] Example 4: Sr 0.96 Pr 0.01 Gd 0.01 Na 0.02 Li2 SiO 4 In an agate mortar, SrCO 3 4.8186g (32.6400mmol), Li 2 SiO 3 3.0588g (34.0000mmol), Pr(NO 3 ) 3 6H 2 O 0.1479g (0.3400mmol), Gd 2 O 3 0.0616g (0.1700mmol), and Na 2 CO 3 0.0360g (0.3400mmol) was mixed in hexane. 2+ / Pr 3+ Na for charge compensation 2 CO 3 The precursor formulation was calcined in air at 700 °C for 2 h to remove organic residues. Subsequent calcination in air at 850 °C for 12 h gave the product phase. Pr 4+ Pr 3+ A final firing step at 850°C for 6 hours in a reducing atmosphere is required to reduce it to 0.05%.
[0074] Comparative Example 1 As comparative examples, other lanthanide-doped silicate systems disclosed in the following publications were prepared and measured under the same conditions (Lu 7 O 6 F 9 :Pr 3+ and Y 2 SiO 5 :Pr 3+ Ceramic visible to UVC upconversion efficiency and mechanism, Cates, Ezra L.; Wilkinson, Angus P.; Kim, Jae-Hong, Journal of Luminescence 160 (2015) pp. 202-209). Abstract: Pr 3+ Visible to UVC upconversion (UC) by doped materials is a promising candidate for applications in sustainable disinfection technologies such as photoactivated antibacterial surfaces and solar water treatment. In this study, Lu 7 O 6 F9 :Pr 3+ Using ceramics to detect Pr in oxyfluoride host systems 3+ This is the first time that we have studied the upconversion of Y 2 SiO 5 :Pr 3+ Compared to the reference material, the oxyfluoride host exhibited a 5-fold increase in the lifetime of the intermediate state, likely due to a lower maximum phonon energy. However, only a 60% increase in the UC intensity was observed. To explain this discrepancy, the emission spectral distributions and decay kinetics were studied for both phosphor systems. 3+ The energy distribution of the 4f5d band was found to play a key role by allowing or forbidding the occurrence of a yet to be elucidated UC mechanism, which had a significant impact on the overall efficiency.
[0075] Lu 7 O 6 F 9 :Pr 3+ was not obtained at the disclosed temperatures. Synthesis at high temperatures and pressures of 350 MPa was not possible due to the modest press used.
[0076] Y 2 SiO 5 :Pr 3+ was synthesized in the same pure phase according to the publication.
[0077] Comparative Example 2 As another comparative example, lanthanide-doped silicates are prepared under the conditions disclosed in U.S. Patent Publication No. 2013 / 502079 with respect to calcination temperature. In an agate mortar, CaCO 3 3.3349g (33.3200mmol), Li 2 CO 3 2.5123g (34.0000mmol), Pr(NO 3 ) 3 6H 2 0.1479 g (0.3400 mmol) of O, and Na 2 CO 30.0180g (0.1700mmol) was mixed in hexane. 2+ / Pr 3+ Na for charge compensation 2 CO 3 The precursor formulation was calcined in air at 700 °C for 2 hours to remove organic residues. Subsequent calcination in air at 1,100 °C (and above) for 12 hours produces an amorphous, glassy product that adheres to the crucible. The amorphous product is then dissolved in Al 2 O 3 It was not possible to separate it from the crucible.
[0078] Crushing Attempts A planetary ball mill PM200 manufactured by Retsch was also used for the following grinding. The inner wall of the grinding bowl and the grinding balls were made of corundum (Al 2 O 3 ). Two different grinding bowls were used: 50 mL and 125 mL. Depending on the size, 9 or 24 grinding balls were used. Depending on their size, the bowls were also loaded with 4.5 g or 20 g of sample. The speed of the grinding bowl is 200 rpm. The grinding time is 4 hours. Working principle: The grinding bowl is placed eccentrically on the sun wheel of the planetary ball mill. The rotational motion of the sun wheel counter-rotates with that of the grinding bowl in a ratio of approximately 1:2. The grinding balls in the grinding bowl are subjected to a multiple rotational motion, the so-called Coriolis force. Due to the speed difference between the balls and the grinding bowl, frictional and impact forces interact and release high kinetic energy. The interaction of these forces results in the advanced and highly effective grinding of the planetary ball mill.
[0079] First, the raw extract (CaCO 3 , Li 2 CO 3 ,Pr 6 O 11 , Na 2 CO 3 , and SiO 2) was recorded (Figure 27a). The extract mixture was then treated in a planetary ball mill as described above (200 rpm for 4 h, Figure 27b: XRPD). The powder diffraction pattern shows that the target phase is absent (Figure 27b). It can therefore be said that the energy input during milling is not sufficient to synthesize the target phase. The exact value of the energy input cannot be calculated. The powder was then sintered in air at 850°C for 12 h.
[0080] After this step, the reactant mixture reacted with the target phase. The strongest reflection at 2Θ=37.39° has an intensity of 13357 counts (Figure 27c). After this sintering process, Pr 3+ In addition to Pr 4+ The powder has a brown color due to the presence of forming gas (H 2 (5%) / N 2 (95%)) needs to be reduced in a second sintering step (850°C for 6 hours).
[0081] After this step, see Figure 27d, the strongest reflection has an intensity of 15423 counts. Thus, the crystallinity can be increased by this sintering step. If it is freshly ground, the crystallinity decreases (see Figure 27e). The number of counts of the reflection decreases to 13576.
[0082] In a second series of experiments, we used conventional synthesis to synthesize CaLi 2 SiO 4 : Pr, Na were provided. For this purpose, the starting material was mixed with acetone in an agate mortar and then sintered in air at 850 °C for 12 h. A second sintering step was then carried out under forming gas (Figure 28a: XRPD). The strongest reflection has an intensity of 10964 counts. The powder sample was then ground as described above.
[0083] Specifically, after 4 hours of grinding at 200 rpm, the intensity of the observed reflections increased to 18665 counts, see FIG. 28b. As a result, the crystallinity can be significantly increased by subsequent grinding. Furthermore, it can be observed that various heterophase reflections also disappear during grinding.
[0084] Pre-milling the extract does not result in a higher crystallinity of the target phase than subsequent milling.In addition, if the starting material is milled before sintering, out-of-phase reflections may be observed even after the sintering step.
Claims
1. a silicate-based lanthanide ion-doped material for converting long wavelength electromagnetic radiation energy to short wavelength electromagnetic radiation energy; said silicate-based material being a crystalline silicate material doped with lanthanide ions selected from praseodymium, gadolinium, erbium, neodymium, or in the case of co-doping, at least two of them; A material that converts at least one long wavelength electromagnetic radiation energy less than 530 nm into at least one shorter wavelength electromagnetic radiation energy in the range of 220-425 nm.
2. 2. The silicate-based material of claim 1, wherein the crystalline silicate material doped with the lanthanide ions is selected from cyclosilicates, pyrosilicates, and inosilicates.
3. i) A silicate-based material according to claim 1 or claim 2, wherein the crystalline silicate material is not a silicate hydrate, in particular the silicate does not contain water of crystallization.
4. The silicate-based material according to any one of claims 1 to 3, having a crystallinity of more than 70%.
5. i) a silicate-based material according to any one of claims 1 to 4, which is a crystalline silicate material consisting of a crystalline pure phase, in particular the crystalline material consisting of one crystalline phase comprising 90% by weight of the crystalline material, in particular the crystalline phase comprising more than 95% by weight, more preferably more than 98% by weight (100% by weight) of the crystalline material, or ii) The material according to any one of claims 1 to 4, which is a crystalline silicate material consisting of a silica-based material, the silica-based material consisting of at least one crystalline phase comprising at least 90% by weight of the silica-based material, in particular the crystalline phase comprising 95% by weight or more (100% by weight) of the silica-based material.
6. The crystalline silicate material has the ideal general formula I: A 1-x-y-z B* y B 2 SiO 4 : Ln 1 x,, Ln 2 z, I (Wherein, x=0.0001 to 0.05, z=0 or z=0.0001 to 0.3, and y=x+z; A is selected from Mg, Ca, Sr and Ba; B is selected from Li, Na, K, Rb and Cs; B* is selected from Li, Na and K, B is equal to or unequal to B*, preferably B is unequal to B*; Ln 1 is selected from praseodymium (Pr), erbium (Er), and neodymium (Nd); Any Ln 2 is selected from gadolinium (Gd). The silicate-based material according to any one of claims 1 to 5, wherein the silicate-based material is selected from the group consisting of:
7. The silicate-based material of any one of claims 1 to 6, wherein the crystalline silicate material is doped with praseodymium.
8. The silicate-based material of any one of claims 1 to 7, wherein the crystalline silicate material is doped with praseodymium and co-doped with gadolinium.
9. The crystalline silicate material comprises one or more crystalline silicates doped with lanthanide ions, including at least one alkali ion and at least one earth alkali ion. It is a solid solution of tetrahydrofuran and tetrahydrofuran. A silicate-based material according to any one of claims 1 to 8, in particular wherein the crystalline silicate is doped with praseodymium and optionally co-doped with gadolinium.
10. The crystalline silicate material has the ideal general formula Ia: A 1-x-y-z B* y B 2 SiO 4 :Pr x , Gd z Ia (Wherein, A=Mg, Ca, Sr, Ba, and B=Li, Na, K, Rb, Cs, and x=0.0001 to 0.05, z=0 or z=0.0001 to 0.3, and y=x+z; B* is selected from Li, Na and K, and K is selected for charge balance of the silicate. It exists for the purpose of B is equal to or unequal to B*, and preferably B is unequal to B*. The silicate-based material according to any one of claims 1 to 9, selected from the group consisting of:
11. The crystalline silicate material has the general formula II: (Ca 1-a Sr a ) 1-2b Ln b Na b Li 2 SiO 4 II (Wherein, a=0.0001 to 1, preferably 0.0001 to 0.1, b=0.0001 to 1, preferably 0.0001 to 0.1; Ln is a lanthanide ion selected from praseodymium, gadolinium, erbium, neodymium, or, in the case of co-doping, selected from at least two of them, particularly praseodymium and, if necessary, gadolinium. The silicate-based material according to any one of claims 1 to 9, selected from the group consisting of:
12. Converting electromagnetic radiation energy of a long wavelength less than 500 nm, particularly less than 500 nm to 400 nm, into electromagnetic radiation energy of a short wavelength in the range of 230 nm to 380 nm; In particular, the maximum radiation intensity of said short-wavelength electromagnetic radiation energy is at least 1.10 3 Counts / (mm 2 *s), especially 1.10 4 Counts / (mm 2 *s), preferably 1.10 5 Counts / (mm 2 The method according to any one of claims 1 to 11, wherein the Lithium-ion-containing materials.
13. 13. The silicate-based material of any one of claims 1 to 12, wherein the crystalline silicate material of formula II has XRPD signals in the ranges of 23° 2Θ to 27° 2Θ, and 34° 2Θ to 39.5° 2Θ.
14. -below: i) at least one lanthanide salt, in particular one selected from lanthanide nitrates, lanthanide carbonates, lanthanide carboxylates, in particular lanthanide acetates, lanthanide sulfates, and / or lanthanide oxides, ii) silicates, iii) at least one earth alkali salt and at least one alkali salt selected from lithium salts or any lithium compound, and optionally selected from sodium salts and potassium salts; and preparing -below: a) mixing said i), said ii) and said iii) by milling to obtain a mixture; or b) mixing said i), said ii) and said iii) in an aprotic organic polar or non-polar solvent to obtain a mixture, and baking said mixture b) at 600°C to 1,000°C. and removing organic components, in particular said calcination is carried out at 600° C. to 1,000° C. under standard atmosphere (air) for at least 1 hour (2 hours) to obtain a calcined mixture. and - calcining the mixture of a) or the calcined mixture of b) in a calcination step at a temperature below the melting temperature of the silica-based material, resulting in at least partial crystallization; In a further calcination step under a reducing atmosphere, the lanthanide is converted to Ln 3+ ions; - obtaining a silicate-based lanthanide ion-doped material, having In the step i), the lanthanide ions in the lanthanide oxide and / or the lanthanide salt are selected from praseodymium, gadolinium, erbium, and neodymium, or in the case of co-doping, from at least two of them; In the above ii), preferably, the lithium salt is selected from the above ii) and is lithium silicate; A method for producing silicate-based materials.
15. 15. The method of claim 14, further comprising milling the obtained silicate-based lanthanide ion doped material, in particular subjecting said material to a sufficient amount of tribological bombardment to improve its crystallinity compared to said material not subjected to tribological bombardment.
16. 16. The method according to claim 15, wherein the silicate-based material obtained is subjected to tribological impacts using corundum as grinding material at 100 to 500 rpm for 1 to 6 hours, in particular at 200 rpm for 2 to 5 hours.
17. A silicate-based lanthanide ion-doped material for converting long wavelength electromagnetic radiation energy into short wavelength electromagnetic radiation energy, obtainable by the method according to any one of claims 14 to 16, a crystalline silicate material doped with lanthanide ions selected from praseodymium, gadolinium, erbium, neodymium, and in the case of co-doping, at least two of them; the lanthanide ion doped crystalline silicate-based material is a solid solution of one or more crystalline silicates containing at least one alkali ion and at least one earth alkali ion; The crystallinity is more than 80%. Optionally, a silicate-based material that converts at least one long wavelength electromagnetic radiation energy less than 530 nm into at least one short wavelength electromagnetic radiation energy in the range of 220-400 nm.
18. A composition, foil or film made of the silicate-based material according to any one of claims 1 to 17 for self-disinfecting or microbial reduction applications.
19. UV sterilization applications, indoor UV sterilization applications, particularly indoor UV sterilization applications utilizing electromagnetic radiation energy from LEDs, particularly pcLEDs, with maximum emission in the range of 450-480 nm; As an additive to a coating on a surface or an additive to a material that provides a surface or coating that can inactivate microorganisms that cover the surface or coating under exposure to electromagnetic radiation energy of long wavelengths less than 500 nm, in particular electromagnetic radiation energy of long wavelengths less than 500 nm with a maximum emission in the range of 450 to 480 nm; Use of the silicate-based lanthanide ion-doped material according to any one of claims 1 to 17.
Citation Information
Patent Citations
Praseodymium and ytterbium double-doped yttrium silicate up-conversion luminescent material and preparation method and application thereof
CN103421504A
Luminescent alkaline earth metal orthosilicate, luminescent screen provided with such silicate, and low pressure mercury lamp provided with such screen
JP1990247279A
Apparatus for generating images and / or projections
JP2005536736A
radiation generator
JP2005536843A
Antimicrobial ultraviolet up-conversion composition
JP2010270117A