Base paper for paper cup

A single-layer paper cup base paper with specific properties and a sizing agent composition addresses the issue of liquid penetration, enhancing the structural integrity of paper cups by preventing tearing and peeling.

JP2024160359AActive Publication Date: 2024-11-13HOKUETSU CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024137590
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-13
Estimated Expiration
2041-10-18

Smart Images

  • Figure 2024160359000001
    Figure 2024160359000001
Patent Text Reader

Abstract

To provide base paper for a paper cup, which hardly causes tearing and peeling due to absorption of liquid from an edge, and a method for producing the same.SOLUTION: There is provided single-ply base paper for a paper cup, which is composed of a pulp as a main component, and has a basis weight of less than 350 g / m2, wherein the base paper contains a sizing agent, a water absorbency at an edge is 0.6 g / 1,000 mm2 or less, and a formation index measured by a β-ray formation meter is 1.2 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a paper cup base paper used for paper cups. [Background technology]

[0002] Base paper for paper cups is known (for example, Patent Documents 1 to 3). In general, paper cups can be obtained by using paper with a thin polyethylene laminated surface, printing as necessary, and then molding the paper into a cup with the polyethylene-laminated surface facing inside. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-219381 A [Patent Document 2] JP 2019-65436 A [Patent Document 3] JP 2019-52382 A Summary of the Invention [Problem to be solved by the invention]

[0004] At least one surface of the base paper for paper cups is laminated, but the edge (cross section) is not laminated. Therefore, liquid poured into the cup or condensation on the surface of the cup can penetrate the base paper, causing problems such as tearing or peeling. The object of the present invention is to solve these problems and provide a base paper for paper cups that is less likely to tear or peel due to absorption of liquid from the edge, and a method for manufacturing the same. [Means for solving the problem]

[0005] As a result of extensive research into base paper for paper cups, the inventors have found that the following configuration can solve the problems. That is, the base paper for paper cups according to the present invention is a paper cup base paper mainly composed of pulp and having a basis weight of 350 g / m2 A single-ply paper base paper for paper cups, containing a sizing agent and having a water absorption of less than 0.6g / 1000mm 2 The paper is characterized in that the formation index measured by the total of β-rays is 1.2 or less. In the present invention, it is preferable that the pulp contains 0.1 to 0.8 mass% of a sizing agent relative to 100 mass parts of pulp, and it is preferable that the sizing agent is one or more selected from the group consisting of reinforced rosin sizing agents, neutral rosin sizing agents, neutral rosin emulsion sizing agents, acidic rosin sizing agents, acidic rosin emulsion sizing agents, weakly acidic rosin sizing agents, weakly acidic rosin emulsion sizing agents, AKD (alkyl ketene dimer), and ASA (alkenyl succinic anhydride). Furthermore, the present invention relates to a paper cup made of the paper cup base paper. A paper cup formed using the paper cup base paper of the present invention is a paper cup in which the penetration of liquid from the cross section of the body bonding part is suppressed even after liquid is poured into the cup, and the paper cup is less likely to break or peel off.

[0006] In addition, the basis weight is 350 g / m 2 It has been found that the above-mentioned problems can be solved by a method for producing base paper for single-ply paper cups in which the sizing agent content is less than 0.1 to 0.8 mass% relative to 100 mass parts of pulp, the method being characterized in that a papermaking raw material mainly composed of pulp containing 0.1 to 0.8 mass% of a sizing agent per 100 mass parts of pulp is made by a papermaking machine at an inlet concentration of 0.5 to 1.5 mass%, which is the concentration at the inlet of the papermaking machine. Furthermore, in the production method of the present invention, it is preferable that the sizing agent is one or more selected from the group consisting of reinforced rosin sizing agents, neutral rosin sizing agents, neutral rosin emulsion sizing agents, acidic rosin sizing agents, acidic rosin emulsion sizing agents, weakly acidic rosin sizing agents, weakly acidic rosin emulsion sizing agents, AKD (alkyl ketene dimer), and ASA (alkenyl succinic anhydride). Effect of the Invention

[0007] According to the paper for paper cups and the manufacturing method thereof of the present invention, it is possible to provide a paper cup in which the infiltration of liquid from the cross section of the body joint after molding is suppressed, and which is less likely to tear or peel off. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Next, the present invention will be described in detail with reference to the embodiments, but the present invention is not limited to these descriptions. Various modifications of the embodiments may be made as long as the effects of the present invention are achieved.

[0009] The base paper for paper cups of the present invention is made of a single-layered base paper mainly composed of pulp. The freeness of the pulp used in the base paper is preferably 200 ml to 500 ml. More preferably, it is 300 ml to 400 ml. If it is less than 200 ml, the base paper becomes too dense and becomes too hard when forming a paper cup, which makes the top curl crack more likely to occur. If it exceeds 500 ml, the interfiber bond becomes weak, the paper strength decreases, and the strength after processing into a container is low, which may cause problems in use. The freeness of the pulp in the present invention is obtained by measuring with a Canadian Standard Type Freeness Tester (based on JIS P 8121:1995 "Testing Method for Freeness of Pulp").

[0010] The pulp used for the base paper may be any known pulp such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), bleached hardwood sulfite pulp (LBSP), bleached softwood sulfite pulp (NBSP), mechanical pulp (GP, TMP, BCTMP), or deinked pulp (DIP). In addition to wood pulp, non-wood pulp, synthetic pulp, synthetic fiber, etc. may be used as needed. In order to obtain whiteness and a clean feeling, it is preferable to use LBKP or NBKP. LBKP is more preferable because shorter pulp fibers are easier to impart smoothness and uniformity. The pulp blend is preferably 90-100% LBKP or 95-100% LBKP in the pulp used, and is particularly preferably 100% LBKP.

[0011] A filler may be blended into the base paper of the paper cup base paper according to this embodiment. Examples of fillers that can be used include light calcium carbonate, heavy calcium carbonate, talc, clay, kaolin, calcined clay, titanium dioxide, and aluminum hydroxide. However, since blending of a filler may reduce the strength of the base paper, the filler blending rate in the base paper is preferably 2% by mass or less, and more preferably 1% by mass or less.

[0012] In the paper base paper for paper cups according to this embodiment, a sizing agent is contained in the base paper. By containing a sizing agent, it is possible to prevent condensation water or liquid poured into the cup from entering through the edge of the base paper. The sizing agent used is not particularly limited, and various known ones such as reinforced rosin sizing agent, neutral rosin sizing agent, neutral rosin emulsion sizing agent, acidic rosin sizing agent, acidic rosin emulsion sizing agent, weak acidic rosin sizing agent, weak acidic rosin emulsion sizing agent, AKD (alkyl ketene dimer), and ASA (alkenyl succinic anhydride) can be used, but acidic rosin emulsion sizing agent is preferred. The content of the sizing agent in the paper base paper for paper cups is not particularly limited, but for example, when an acidic rosin emulsion sizing agent is used, it is preferably 0.1 to 0.8 mass% relative to 100 parts by mass of pulp, and more preferably 0.2 to 0.6 mass%. If it is less than 0.1 mass%, there is a possibility that liquid intrusion through the edge cannot be sufficiently prevented. Furthermore, if the content exceeds 0.8% by mass, the sizing agent may inhibit the entanglement of pulp fibers, leading to a decrease in strength, and may lead to process contamination such as foaming during the papermaking process or circulation of sizing agent that has not been completely fixed, making production virtually impossible.

[0013] In the paper for paper cups according to the present embodiment, known additives for papermaking can be used within a range that does not impair the intended effect of the present invention. For example, it is preferable to add a paper strength enhancer to the papermaking raw material. By adding a paper strength enhancer, sufficient interlayer strength can be ensured and the occurrence of fuzz and creases can be suppressed. The paper strength enhancer is not particularly limited, but is preferably an internal paper strength enhancer such as cationic starch, amphoteric starch, or polyacrylamide. For example, it is preferable that the papermaking raw material contains amphoteric polyacrylamide as a paper strength enhancer in an amount of 0.1 to 1.0% by mass relative to the amount of pulp. Furthermore, various auxiliaries such as aluminum sulfate as a flocculation aid, a retention improver, a drainage improver, a coloring dye, a coloring pigment, a fluorescent brightener, a fluorescent decolorizer, a charge regulator, or a pitch control agent may be blended. For example, it is preferable to contain aluminum sulfate as a flocculation aid in an amount of 0.1 to 1.0% by mass relative to the amount of pulp.

[0014] In the paper for paper cups according to the present embodiment, the method of manufacturing the base paper is not particularly limited as long as it is a single-layer papermaking, but for example, it is a single-layer papermaking using a papermaking machine such as a Fourdrinier papermaking machine or a cylinder papermaking machine. In the case of a multi-layer papermaking having two or more layers, when comparing between layers and within layers, the entanglement of fibers between layers is clearly smaller, and as a result, the density of that area is lower. This makes it easier for water to penetrate and there is a possibility of peeling, which is not preferable in the present invention.

[0015] In the paper for paper cups according to this embodiment, a surface sizing liquid may be applied to the surface of the base paper. Examples of surface sizing liquid include known water-soluble polymers such as starch, polyvinyl alcohol, polyacrylamide resin, acrylic resin, and polyamide resin. The amount of the surface sizing liquid is 0.1 to 2.0 g / m2 in solid form per side of the base paper. 2 For example, the oxidized starch is preferably 0.2 to 1.5 g / m2 in solid form per one side of the base paper. 2 The surface strength agent applied as the surface sizing liquid is unlikely to affect the tensile breaking elongation in the lateral direction of the paper, so that a general surface strength agent can also be used as long as it does not impair the intended effect of the present invention.

[0016] The method of applying the surface size liquid can be, but is not particularly limited to, a known applicator such as a type equipped with a pond such as a size press, a film metering type such as a gate roll size press or a shim sizer, a rod coater or an air knife coater.

[0017] In the base paper for paper cups according to this embodiment, a coating layer containing a pigment may be provided on the surface of the base paper. The coating layer may be provided on one side of the base paper or on both sides of the base paper. Pigments used in the coating layer may include kaolin clay, heavy calcium carbonate, light calcium carbonate, titanium oxide, talc, satin white, lithopone, silica, alumina, aluminum hydroxide, zinc oxide, magnesium carbonate, calcined kaolin, and the like. Organic pigments may also be used. These may be used alone or in combination of two or more. When coating layers are provided on both sides of the base paper, the coating layer provided on one side and the coating layer provided on the other side may have the same composition or different compositions.

[0018] In the base paper for paper cups according to this embodiment, the paint for forming the coating layer may contain various commonly used auxiliary agents such as adhesives, dispersants, defoamers, water-resistant agents, coloring dyes, coloring pigments, and thickeners, as necessary.

[0019] In the base paper for paper cups according to this embodiment, a coating layer can be provided by applying a coating material for forming a coating layer to the base paper. The method for applying the coating material for forming a coating layer to the base paper is not particularly limited, and various methods such as a metering size press, various film transfer coaters such as a gate roll or a shim sizer, an air knife coater, a rod coater, a blade coater, a direct fountain coater, a spray coater, and a curtain coater are appropriately used. There is no restriction on the dry coating amount per side of the coating layer as long as it is within a range that does not impair the intended effect of the present invention, but if the coating amount is too high, top curl cracking is likely to occur, so for example, 7 to 30 g / m 2 The range is preferably:

[0020] In this embodiment, the edge absorption capacity of the base paper for the paper cup is 0.6 g / 1000 mm 2 Less than 0.5g / 1000mm 2 Less than 0.4g / 1000mm is preferable. 2 The following is more preferable: 0.6g / 1000mm 2 If the thickness exceeds 100 mm, it may not be possible to prevent liquid from entering through the opening. There is no specific lower limit, but the minimum limit is 0.1 g / 1000 mm. 2 To achieve a water absorption of less than this, a large amount of sizing agent is used, which can result in the inhibition of inter-fiber bonding as described below, and can lead to breakage of the base paper. Here, the water absorption at the edge is the measured amount of water absorbed from the edge. The water absorption at the edge is measured by covering the entire front and back sides of the base paper for paper cups with cellophane tape to prevent pure water from penetrating from the front and back, then immersing the entire base paper in water for one hour and measuring the weight increase per cross-sectional area of ​​the edge (total length of the sample edge x paper thickness). Water absorption at the edge A (g / 1000mm 2 ) = Weight increase (g) x 1000 ÷ Cross-sectional area of ​​the fore edge (paper thickness (mm) x total length of the fore edge (mm)).

[0021] Generally, methods for measuring durability against water include Stockigt sizing and Cobb water absorbency. Stockigt sizing involves floating the paper on water while simultaneously dripping a drop of water from above and measuring the time until the two come into contact. Cobb water absorbency involves covering one side of the paper surface with water and measuring the amount of water absorbed. Both methods measure the amount of water absorbed or the absorption time from a large area of ​​the paper surface, but are not suitable for evaluating the amount of water intrusion from the cross section of the cup base paper, which is the subject of the present invention. Therefore, in the present invention, we use the edge water absorbency, which is suitable for evaluating the amount of water intrusion from the cross section of the cup base paper. With this edge water absorbency, the effect of the surface tension of the liquid is accurately reflected in the measured value.

[0022] The base paper for paper cups according to the present embodiment has a formation index of 1.2 or less, measured by the total of the β-rays. The formation index is preferably 1.0 or less, more preferably 0.8 or less. The lower limit of the formation index is not particularly limited, but is preferably 0.3 or more, more preferably 0.5 or more. If the formation index exceeds 1.2, the microscopic variation in basis weight becomes large, resulting in sparseness and density. As described above, the base paper for paper cups according to the present invention contains a sizing agent to prevent liquid from penetrating from the edge of the base paper, but the sizing agent acts in the direction of inhibiting the inter-fiber bonding of pulp fibers, so the paper tends to become bulky. In such bulky paper, if the microscopic variation in basis weight becomes large and sparseness and density occurs (poor formation), liquid is likely to penetrate from the sparse parts, and it is also thought that the paper strength, such as interlayer strength, will decrease significantly after the liquid penetrates. Also, it is thought that it is possible to prevent the liquid poured into the cup from entering through the edge of the base paper by the surface tension of the liquid, but condensed water not only enters through the edge of the base paper, but also appears as moisture in the air contained in the paper as liquid, and if this concentrates in the above-mentioned open areas, there is a possibility that the paper strength will decrease significantly. Therefore, in the present invention, it is necessary to keep the formation index measured by the total β-ray ground below a certain level while containing a sizing agent.

[0023] The ground weight used in measuring the formation index in this embodiment is a β-ray ground weight, that is, a ground weight using a β-ray radiation source, which indicates the distribution of basis weight (sometimes called U.S. basis weight). The widely used ground weight is based on light transmission, but is not suitable for evaluating formation because it is affected by factors such as pulp components, type and amount of filler, hue, whiteness, and degree of beating of the pulp, and is not suitable for evaluating formation. As mentioned above, base paper for paper cups is more susceptible to liquid absorption from the edge of the base paper than areas with sparse and dense basis weights, which can result in tearing, etc. The formation index measured using the β-ray ground weight is an index of the difference in basis weight (referred to as unit basis weight) measured at a diameter of 1 mm of the cup base paper. The β-ray ground weight is 350 g / m 2 The above basis weights lack precision, so in this embodiment, the basis weight of the base paper is 350 g / m 2 This applies to base paper for paper cups that are less than 100g in size.

[0024] As a method for making the formation index measured by the total β-rays less than 1.2, for example, the consistency of the raw material at the inlet of the papermaking machine (hereinafter, sometimes referred to as raw material consistency) can be reduced. 2 In the manufacturing method of the single-layer paper cup base paper, the papermaking raw material mainly composed of pulp is made by a paper machine with an inlet concentration of 0.5 to 1.5 mass%, which is the concentration at the inlet of the paper machine. By lowering the raw material concentration, the formation of the paper cup base paper can be improved, and as a result, the formation index can be reduced. In the case of a fourdrinier paper machine, the inlet concentration of the head box is preferably 1.5 mass% or less, more preferably 1.3 mass% or less, and even better 1.1 mass% or less. If it exceeds 1.5 mass%, the formation index will not be within the desired range, and the variation in density is likely to become large. If the raw material concentration is less than 0.5 mass%, the sheet will be difficult to peel off from the wire and the yield on the wire will also decrease, so 0.5 mass% is the actual lower limit. In addition, if the basis weight of the paper cup base paper is 150 g / m 2 In the above cases, it is preferable to use a shaking device that vibrates the papermaking machine to make the base paper uniform. When using a shaking device to control the formation, for example, the shaking conditions are preferably a shaking width of 10 to 20 mm and a vibration frequency of 2 to 4 times / second. At the same time, it is preferable to set the inlet concentration, which is the concentration at the inlet of the papermaking machine, to 0.7 to 1.5 mass%.

[0025] In this embodiment, the formation index is calculated, for example, as follows. The basis weight (referred to as unit basis weight) measured at a diameter of 1 mm of the base paper for paper cups is measured at a pitch of 3.5 mm x 3.5 mm over a measurement area of ​​70 mm x 70 mm, and the standard deviation of basis weight and the weighted average basis weight are calculated for the obtained 400 unit basis weight values. The normalized standard deviation of basis weight (nsd) calculated according to the following formula (Equation 1) is regarded as the formation index. (Equation 1) Standard deviation of basis weight (g / m) = Standard deviation of basis weight (g / m 2 ) / weighted average of basis weight (g / m 2 ) 1 / 2

[0026] In the paper for paper cups according to this embodiment, the moisture content is preferably about 6% to 9%, for example, 9% or less. If the moisture content exceeds 9%, the amount of water contained in the paper becomes liquid, which tends to lead to a decrease in paper strength. If the moisture content is less than 6%, the amount of water contained in the paper decreases, but on the other hand the paper becomes hard and brittle, which tends to lead to a decrease in paper strength such as cracking. The moisture content was measured according to JIS P8127:2010 Paper and cardboard - Lot moisture test method - Dryer method. EXAMPLES

[0027] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" refer to "parts by mass" and "% by mass", respectively, unless otherwise specified. The number of parts added is a value calculated as a solid content.

[0028] The base paper for paper cups obtained in each of the Examples and Comparative Examples shown below was evaluated as follows. The evaluation results are shown in Table 1. The evaluation methods are as follows.

[0029] <Edge torn> Both sides of the base paper for paper cups obtained in each Example and Comparative Example were coated with low-density polyethylene (Petrosen DLZ19A, manufactured by Tosoh Corporation) in an amount of 30 g / m using an extrusion coater (melt extruder). 2 A polyethylene laminate was applied so that the paper cups would be formed using a cup forming machine, and the formed paper cups were immersed in pure water for 1 hour to remove excess water. The edge of the cups was then turned over with the fingers, and the degree of peeling was evaluated. ◎: No peeling at all, good condition (passed) ○: Good condition without peeling. (Pass) △: Slight peeling. (Lower limit of use) ×: Large tear due to peeling (failed)

[0030] <Water absorption at the end> The base paper for paper cups obtained in each of the Examples and Comparative Examples was measured according to the following procedures. - Apply 75mm wide cellophane tape to both sides to prevent pure water from penetrating from the front and back. Cut into strips of 50mm length and 125mm width. Then measure the weight a before immersion. -Immerse in pure water for 1 hour. Wipe off excess water and measure the weight b after immersion. ·Water absorption at the end g / 1000mm 2 =(ba)×1000÷(B×D) B: Paper thickness mm, D: Total length of fore-edge mm = 350 mm

[0031] <Formation index> The basis weight (unit basis weight) measured at a diameter of 1 mm for the paper cup base paper is measured by a ground weight calculator at a pitch of 3.5 mm x 3.5 mm for a measurement area of ​​70 mm x 70 mm, and the standard deviation of the basis weight and the weighted average basis weight are calculated for the 400 unit basis weight values ​​obtained. The normalized standard deviation of the basis weight (nsd) calculated according to the following formula (math 1) is used as the formation index. The ground weight calculator was used to measure the basis weight. (Number 1) Basis weight normalized standard deviation (g / m) = Standard deviation of basis weight (g / m 2 ) / weighted average of basis weight (g / m 2 ) 1 / 2

[0032] Example 1 <Preparation of base paper> The pulp was adjusted to 350 ml of CSF consisting of 100% hardwood pulp (L-BKP), and a basis weight of 230 g / m was produced on a fourdrinier papermaking machine equipped with a top wire. 2The base paper was made in a single layer at a speed of 150 m / min. The raw materials for papermaking contained amphoteric polyacrylamide (Polystron 387, manufactured by Arakawa Chemical Industries Co., Ltd.) at 0.5% of the pulp weight as a paper strength enhancer, aluminum sulfate at 0.6% of the pulp weight as a flocculation aid, and acidic rosin emulsion sizing agent (AL-1203, manufactured by Seiko PMC Co., Ltd.) at 0.4% of the pulp weight as a sizing agent. The shaking conditions for the papermaking machine were 3 times / second, amplitude width 12 mm, and inlet concentration 1.1%.

[0033] <Size press> A sizing solution of 5% aqueous solution of oxidized starch (MS3800 manufactured by Nippon Shokuhin Kako Co., Ltd.) was applied to the base paper using a pond-type size press until the amount of adhesion per side was 1.0 g / m2 in terms of solid content. 2 The mixture was applied to both sides so as to obtain the above-mentioned result, and then dried.

[0034] <Smoothing processing> The dried base paper was subjected to a calendering treatment at a linear pressure of 50 kg / cm to obtain a paper cup base paper, which had a moisture content of 7.2%.

[0035] Example 2 A base paper for a paper cup was obtained in the same manner as in Example 1, except that the inlet concentration was changed from 1.1% to 0.9%.

[0036] Example 3 A base paper for a paper cup was obtained in the same manner as in Example 1, except that the inlet concentration was changed from 1.1% to 1.3%.

[0037] Example 4 A base paper for a paper cup was obtained in the same manner as in Example 1, except that the content of the acidic rosin emulsion sizing agent was changed from 0.4% to 0.2%.

[0038] Example 5 A base paper for a paper cup was obtained in the same manner as in Example 1, except that the content of the acidic rosin emulsion sizing agent was changed from 0.4% to 0.6%.

[0039] Comparative Example 1 A base paper for paper cups was obtained in the same manner as in Example 1, except that the content of the acidic rosin emulsion sizing agent was changed from 0.4% to no addition.

[0040] Comparative Example 2 A base paper for a paper cup was obtained in the same manner as in Example 1, except that the inlet concentration was changed from 1.1% to 1.6%.

[0041] [Table 1]

[0042] As is clear from Table 1, the base papers for paper cups obtained in Examples 1 to 5 all absorbed little liquid from the edge and almost no edge tears occurred.

[0043] On the other hand, the base papers for paper cups obtained in Comparative Examples 1 and 2, in which no sizing agent was added to the base paper, absorbed a large amount of liquid from the edge, causing tears at the edge and making them unusable.

Claims

1. Pulp-based basis weight 350 g / m 2 A single-ply paper base paper for paper cups, containing a sizing agent and having a water absorption of less than 0.6 g / 1000 mm 2 and a formation index measured by a total of β-rays is 1.2 or less.

2. The paper base paper for paper cups according to claim 1, further comprising 0.1 to 0.8% by mass of a sizing agent relative to 100 parts by mass of pulp.

3. The paper base paper for paper cups according to claim 1 or 2, characterized in that the sizing agent is one or more selected from the group consisting of fortified rosin sizing agents, neutral rosin sizing agents, neutral rosin emulsion sizing agents, acidic rosin sizing agents, acidic rosin emulsion sizing agents, weak acidic rosin sizing agents, weak acidic rosin emulsion sizing agents, AKD (alkyl ketene dimer), and ASA (alkenyl succinic anhydride).

4. A paper cup made of the base paper for paper cups according to any one of claims 1 to 3.

5. Basis weight 350g / m 2 A method for producing a single-layer paper base for a paper cup, the method comprising the steps of: The method is characterized in that a papermaking raw material mainly composed of pulp containing 0.1 to 0.8 mass% of a sizing agent per 100 mass parts of pulp is made into paper by a papermaking machine at an inlet concentration of 0.5 to 1.5 mass%, which is the concentration at the inlet of the papermaking machine.

6. The method for manufacturing base paper for paper cups according to claim 5, characterized in that the sizing agent is one or more selected from the group consisting of fortified rosin sizing agents, neutral rosin sizing agents, neutral rosin emulsion sizing agents, acidic rosin sizing agents, acidic rosin emulsion sizing agents, weak acidic rosin sizing agents, weak acidic rosin emulsion sizing agents, AKD (alkyl ketene dimer), and ASA (alkenyl succinic anhydride).

Citation Information

Patent Citations

  • Base paper for acidic food cup

    JP2003155700A

  • Base paper for liquid container

    JP2006219775A

  • Base paper for paper vessel

    JP2009243009A

  • Base paper for paper cup

    JP2021046636A

  • Carrier tape mount for chip-shaped electronic components and manufacturing method thereof

    JP2021079998A