Method for producing viscous composition

By adding a copolymer to a surfactant and water solution under controlled pH and frequency conditions, the solubility of (meth)acrylic acid-based copolymers is enhanced, addressing poor solubility issues and improving manufacturing efficiency.

JP2024160366APending Publication Date: 2024-11-13SUMITOMO SEIKA CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024138942
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-13

AI Technical Summary

Technical Problem

Copolymers containing (meth)acrylic acid as a constituent unit have poor solubility in water, leading to prolonged dissolution times in the preparation of viscous compositions.

Method used

A method involving the addition of a copolymer to a mixed solution of a surfactant and water, characterized by specific storage modulus conditions, including a pH of 6.5 to 7.5 and a rheometer frequency of 1Hz, to enhance solubility.

Benefits of technology

The method improves the solubility of copolymers in water, reducing dissolution times and enhancing manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160366000004
    Figure 2024160366000004
  • Figure 2024160366000005
    Figure 2024160366000005
  • Figure 2024160366000001
    Figure 2024160366000001
Patent Text Reader

Abstract

To provide a method for producing a viscous composition which can improve solubility of a copolymer containing a (meth)acrylic acid as a constitutional unit to water, and contains the copolymer.SOLUTION: A method for producing a viscous composition contains a copolymer containing a constitutional unit derived from a (meth)acrylic acid, and a surface active agent and water, in which the copolymer is a copolymer having storage elastic modulus (G') at frequency dispersion of 1 rad / s measured under the following condition of 10 Pa or less, and the production method includes a step of adding the copolymer to an aqueous solution of the surface active agent. [Measurement condition: as for 0.5 mass% of a neutralized aqueous solution of a copolymer having a pH of 6.5 to 7.5, strain in subsequent frequency dispersion is determined to be 0.1% or 1% by measurement of storage elastic modulus in strain dispersion at a liquid temperature of 25°C and a frequency of a rheometer of 1 Hz, storage elastic modulus in the frequency dispersion obtained by changing angular frequency from 0.1 rad / s to 300 rad / s is measured under the strain condition, and storage elastic modulus at angular frequency of 1 rad / s is determined.]SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a viscous composition containing a copolymer having (meth)acrylic acid as a constituent unit, a surfactant, and water. [Background technology]

[0002] Viscous compositions containing copolymers having (meth)acrylic acid as a structural unit are widely used as products in various fields, such as cosmetics and topical compositions. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2007 / 055354 Summary of the Invention [Problem to be solved by the invention]

[0004] Copolymers having a specific (meth)acrylic acid as a constituent unit have poor solubility in water, and in the process of preparing a viscous composition containing the copolymer, there was a problem that it took a long time to dissolve the copolymer, so further improvement was desired. [Means for solving the problem]

[0005] The present invention encompasses, for example, the subject matter described in the following paragraphs. Section 1. (a) A copolymer containing structural units derived from (meth)acrylic acid (b) Surfactants (c) water A method for producing a viscous composition comprising: The (a) copolymer has a storage modulus (G') of 10 Pa or less at a frequency dispersion of 1 rad / s measured under the following conditions: The method includes a step of adding the copolymer (a) to a mixed solution of the copolymers (b) and (c), Manufacturing method. [Measurement conditions: For a neutralized aqueous solution of pH 6.5 to 7.5 containing 0.5 mass% of the above (a) copolymer based on the total amount of the neutralized aqueous solution, the storage modulus is measured by strain dispersion at a liquid temperature of 25°C and a rheometer frequency of 1 Hz, and the strain in the subsequent frequency dispersion is determined to be 0.1% or 1%. Under the strain conditions, the storage modulus is measured by frequency dispersion obtained by changing the angular frequency from 0.1 rad / s to 300 rad / s, and the storage modulus (G') at an angular frequency of 1 rad / s is obtained.] Effect of the Invention

[0006] According to the present invention, there can be provided a method for producing a viscous composition containing a copolymer having a specific (meth)acrylic acid as a constituent unit, which can improve the solubility of the copolymer in water. [Brief description of the drawings]

[0007] [Figure 1] The figure shows the strain dispersion of a neutralized aqueous solution of pH 6.5 to 7.5 containing 0.5 mass% of copolymer (component (a)) based on the total amount of the neutralized aqueous solution, with the liquid temperature set to 25°C and the frequency of the rheometer set to 1 Hz. The horizontal axis is the strain ratio, and the vertical axis is the storage modulus (G'). This figure shows an overview for determining whether to use 0.1% or 1% as the strain value as a condition for measuring the G' value (storage modulus) of the copolymer (component (a)) with a frequency dispersion of 1 rad / s (conceptual diagram unrelated to the examples). It shows that 1% is selected if the linear region obtained in the strain dispersion measurement at 1 Hz includes 1% strain, and 0.1% is selected if the linear region includes 0.1% strain but does not include 1%. [Diagram 2]The frequency dispersion is shown for a neutralized aqueous solution of pH 6.5 to 7.5 containing 0.5% by mass of copolymer (component (a)) based on the total amount of the neutralized aqueous solution, and is obtained by changing the angular frequency from 0.1 rad / s to 300 rad / s under the conditions of a liquid temperature of 25°C, a strain of 0.1% or 1% in strain dispersion with a rheometer frequency set to 1 Hz. The horizontal axis is the angular frequency, and the vertical axis is the storage modulus (G'). Note that this figure is a conceptual diagram unrelated to the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below. The present invention is a method for producing a viscous composition containing a specific copolymer containing a structural unit derived from (meth)acrylic acid, a surfactant, and water, the method comprising the step of adding the copolymer to a mixed solution of the surfactant and water.

[0009] In this specification, "(meth)acrylic" means acrylic and / or methacrylic. As the (meth)acrylic acid, either acrylic acid or methacrylic acid can be used alone, or both of them can be used in combination.

[0010] The (a) copolymer is a copolymer containing (I) a structural unit derived from (meth)acrylic acid, (II) a structural unit derived from a compound having two or more ethylenically unsaturated groups, and (III) a structural unit derived from a (meth)acrylic acid alkyl ester, the alkyl group of which has 10 to 30 carbon atoms.

[0011] The (a) copolymer preferably contains 0.001 to 0.05 parts by mass, more preferably 0.005 to 0.05 parts by mass, and even more preferably 0.005 to 0.03 parts by mass of (II) a structural unit derived from a compound having two or more ethylenically unsaturated groups, per 100 parts by mass of (I) a structural unit derived from (meth)acrylic acid.

[0012] The (a) copolymer preferably contains 0.1 to 10 parts by mass, more preferably 0.2 to 9 parts by mass, still more preferably 0.5 to 7 parts by mass, and particularly preferably 1.0 to 5.0 parts by mass of (III) structural units derived from a (meth)acrylic acid alkyl ester, the alkyl group of which has 10 to 30 carbon atoms, per 100 parts by mass of (I) structural units derived from (meth)acrylic acid.

[0013] The (a) copolymer can be prepared by copolymerizing at least (i) (meth)acrylic acid, (ii) a compound having two or more ethylenically unsaturated groups, and (iii) a (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 10 to 30. By adjusting the amounts of each of (i) to (iii) used when copolymerizing these (i) to (iii), it is possible to adjust the parts by mass of (II) or (III) relative to 100 parts by mass of the above (I).

[0014] (ii) Examples of compounds having two or more ethylenically unsaturated groups include, but are not limited to, di- or more substituted acrylic acid esters of polyols such as ethylene glycol, propylene glycol, polyoxyethylene glycol, polyoxypropylene glycol, glycerin, polyglycerin, trimethylolpropane, pentaerythritol, sucrose, and sorbitol; di- or more substituted allyl ethers of the above polyols; diallyl phthalate, triallyl phosphate, allyl methacrylate, tetraallyloxyethane, triallyl cyanurate, divinyl adipate, vinyl crotonate, 1,5-hexadiene, divinylbenzene, polyallylsucrose, and the like. Among these compounds having two or more ethylenically unsaturated groups, preferred are sucrose allyl ether, pentaerythritol allyl ether (among which pentaerythritol triallyl ether and pentaerythritol tetraallyl ether are preferred), tetraallyloxyethane, triallyl phosphate, and polyallylsaccharose, among which sucrose allyl ether and pentaerythritol allyl ether are more preferred.These compounds having two or more ethylenically unsaturated groups may be used alone or in combination of two or more.

[0015] (iii) A (meth)acrylic acid alkyl ester having an alkyl group with 10 to 30 carbon atoms (10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30) is an ester of (meth)acrylic acid and a higher alcohol having an alkyl group with 10 to 30 carbon atoms. The number of carbon atoms in the alkyl group is preferably, for example, 12 to 30, more preferably 14 to 28, further preferably 16 to 26, and particularly preferably 18 to 24. Such an (meth)acrylic acid alkyl ester is not particularly limited, and examples thereof include an ester of (meth)acrylic acid and stearyl alcohol, an ester of (meth)acrylic acid and eicosanol, an ester of (meth)acrylic acid and behenyl alcohol, and an ester of (meth)acrylic acid and tetracosanol. Among these (meth)acrylic acid alkyl esters, stearyl methacrylate, eicosanyl methacrylate, behenyl methacrylate, and tetracosanyl methacrylate are preferred. These (meth)acrylic acid alkyl esters may be used alone or in combination of two or more. In addition, as such (meth)acrylic acid alkyl esters, for example, commercially available products such as Blenmar VMA-70 and Blenmar SMA, manufactured by Nippon Oil & Fats Corporation, may be used.

[0016] In the present invention, the copolymer is a concept that includes a compound in which (meth)acrylic acid and a crosslinking agent (particularly a compound having two or more ethylenically unsaturated groups) are polymerized (in other words, a compound in which (meth)acrylic acid is crosslinked with a crosslinking agent). Therefore, the (a) copolymer includes a compound in which a compound having two or more ethylenically unsaturated groups is also polymerized in addition to (meth)acrylic acid (in other words, a compound in which a (meth)acrylic acid polymer is crosslinked with the compound). In this case, the compound having two or more ethylenically unsaturated groups can be said to function as a crosslinking agent.

[0017] (a) The storage modulus (G') of the copolymer is determined by the following procedure. 1) <Preparation of neutralized aqueous solution for measurement> The (a) copolymer is dispersed in water so that the copolymer concentration is 0.5 mass% based on the total amount of the neutralization aqueous solution, and an alkaline aqueous solution is added while stirring to dissolve the (a) copolymer while adjusting the pH to 6.5 to 7.5, thereby obtaining a neutralization aqueous solution. 2) <Determination of strain by strain distribution> The temperature of the neutralized aqueous solution prepared in 1) above is set to 25°C, and the frequency of a rheometer (e.g., TA Instruments (model number: AR-2000ex)) is set to 1 Hz. Then, the storage modulus (G') is measured while applying strain. When it is confirmed that the storage modulus (G') has decreased, the measurement is stopped (a graph like that shown in Figure 1 is obtained). From the obtained strain dispersion graph, if the storage modulus (G') maintains a constant value up to a strain of 1% but cannot maintain a constant value up to 10%, the strain is set to 1%. If the storage modulus (G') maintains a constant value up to a strain of 0.1% but cannot maintain a constant value up to 1%, the strain is set to 0.1%. 3) <Determination of storage modulus by frequency dispersion> Under the conditions of a liquid temperature of 25°C for the neutralization solution prepared in 1) above and a strain (0.1 or 1%) determined by the above criteria, the angular frequency is changed from 0.1 rad / s to 300 rad / s (a graph like that shown in Figure 2 is obtained). From the measured values, the storage modulus (G') at an angular frequency of 1 rad / s is adopted.

[0018] The storage modulus (G') is preferably 10 Pa or less, more preferably 5 Pa or less, and even more preferably 1 Pa or less. The lower limit is preferably 0.01 Pa or more.

[0019] An example of such a copolymer is AQUPEC SER W-300C (trade name) manufactured by Sumitomo Seika Chemicals Co., Ltd. The storage modulus (G') can be adjusted by changing the amount of crosslinking agent added, and in particular, a low G' can be achieved by setting the amount of crosslinking agent added to a certain amount or less.

[0020] (a) In producing the copolymer, the method for polymerizing (i), (ii), and (iii) is not particularly limited, and examples thereof include a method in which these are polymerized in a polymerization solvent in the presence of a radical polymerization initiator.

[0021] The radical polymerization initiator is not particularly limited, and examples thereof include α,α'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 2,2'-azobismethylisobutyrate, 2,2'-azobis(2-methylpropionamidine) dihydrochloride, benzoyl peroxide, lauroyl peroxide, cumene hydroperoxide, tertiary butyl hydroperoxide, etc. These radical polymerization initiators may be used alone or in combination of two or more.

[0022] The amount of the radical polymerization initiator used is not particularly limited, but is, for example, preferably 0.01 to 0.45 parts by mass, and more preferably 0.01 to 0.35 parts by mass, relative to 100 parts by mass of (meth)acrylic acid.

[0023] The polymerization solvent is not particularly limited, but is preferably a solvent that dissolves (i), (ii), and (iii) and does not dissolve the copolymer obtained. Such polymerization solvents are preferably aliphatic hydrocarbons, aromatic hydrocarbons, halogenated hydrocarbons, esters, and ketones, and specific examples thereof include normal pentane, normal hexane, normal heptane, normal octane, isooctane, cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane, benzene, toluene, xylene, chlorobenzene, ethylene dichloride, ethyl acetate, isopropyl acetate, ethyl methyl ketone, and isobutyl methyl ketone. Among these polymerization solvents, ethylene dichloride, normal hexane, normal heptane, or ethyl acetate is preferably used from the viewpoint of stable quality and easy availability. These polymerization solvents may be used alone or in combination of two or more.

[0024] The amount of the polymerization solvent used is not particularly limited, but is preferably 200 to 10,000 parts by mass, and more preferably 300 to 2,000 parts by mass, relative to 100 parts by mass of (I) (meth)acrylic acid. By using the polymerization solvent within the above range, even if the polymerization reaction proceeds, aggregation of the copolymer is preferably suppressed, and the copolymer can be stirred uniformly, and the polymerization reaction can proceed more efficiently.

[0025] The atmosphere in which the polymerization reaction is carried out is not particularly limited as long as the polymerization reaction is possible, and examples of the atmosphere include an inert gas atmosphere such as nitrogen gas, argon gas, etc.

[0026] The reaction temperature when carrying out the above polymerization reaction is not particularly limited as long as the polymerization reaction is possible, but is preferably, for example, 50 to 90° C., more preferably 55 to 75° C. By carrying out the polymerization reaction at such a reaction temperature, an increase in the viscosity of the reaction solution can be preferably suppressed, the reaction can be more easily controlled, and the bulk density of the obtained copolymer can be preferably controlled.

[0027] The reaction time for carrying out the above polymerization reaction varies depending on the reaction temperature and cannot be generally determined, but is usually 2 to 10 hours.

[0028] After the reaction is completed, the copolymer can be isolated, for example, by heating the reaction solution to 80 to 130° C. and removing the polymerization solvent. The copolymer thus obtained is usually a white fine powder.

[0029] The (b) surfactant may be a nonionic surfactant, an anionic surfactant, or an amphoteric surfactant. The (b) surfactant may be used alone or in combination of two or more kinds.

[0030] The nonionic surfactant is preferably a nonionic surfactant having a polyoxyethylene chain, a fatty acid alkylolamide obtained by condensation of a fatty acid and ethanolamine, or an alkyl glucoside. The nonionic surfactant having a polyoxyethylene chain is preferably, for example, (b1) polyoxyethylene castor oil, (b2) an ester compound of polyoxyethylene castor oil and a fatty acid, (b3) a block copolymer of a hydroxy fatty acid and ethylene oxide, and (b4) polysorbates, and is preferably at least one selected from the group consisting of (b1) to (b4).

[0031] As the polyoxyethylene castor oil, those having an added mole number of ethylene oxide of about 2 to 10 are preferable, and those having an added mole number of about 2 to 5 are more preferable. As the polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil is more preferable.

[0032] In (b2) the ester compound of polyoxyethylene castor oil and a fatty acid, the fatty acid is preferably a saturated or unsaturated fatty acid having 14 to 24 carbon atoms (14, 15, 16, 17, 18, 19, 20, 21, 22, 23, or 24), more specifically, preferred examples thereof include isopalmitic acid, isostearic acid, isooleic acid, etc. A particularly preferred example of the ester compound of polyoxyethylene castor oil and a fatty acid is an ester compound of polyoxyethylene hydrogenated castor oil and isostearic acid.

[0033] (b3) Block copolymer of hydroxy fatty acid and ethylene oxide can be said to be a copolymer consisting of a block of polyhydroxy fatty acid and a block of polyoxyethylene. As the hydroxy fatty acid, a hydroxy fatty acid having about 14 to 22 carbon atoms is preferable, and examples of preferable examples include hydroxymyristic acid, hydroxypalmitic acid, and hydroxystearic acid, and hydroxystearic acid is particularly preferable. As the hydroxystearic acid, 12-hydroxystearic acid is particularly preferable. As the polyhydroxy fatty acid, polyhydroxystearic acid is particularly preferable. As the block copolymer of hydroxy fatty acid and ethylene oxide, a block copolymer of 12-hydroxystearic acid and ethylene oxide is particularly preferable. (b4) Polysorbates are polyoxyethylene ethers of sorbitan fatty acid esters. More specifically, they include polysorbate 20, polysorbate 60, polysorbate 65, polysorbate 80, and polysorbate 85, with polysorbate 85 being particularly preferred.

[0034] In the fatty acid alkylolamide, the fatty acid is preferably a saturated or unsaturated fatty acid having 14 to 24 carbon atoms (14, 15, 16, 17, 18, 19, 20, 21, 22, 23, or 24), more specifically, lauric acid, coconut fatty acid, etc. are preferred. Preferred ethanolamines include monoethanolamine, diethanolamine, etc. The amino group may be alkylated. Preferred fatty acid alkylolamides include lauric acid diethanolamide, coconut oil fatty acid monoethanolamide, coconut oil fatty acid N-methylethanolamide, etc.

[0035] In the alkyl glucoside, the number of carbon atoms in the alkyl group is preferably 8 to 16. Specific examples include caprylyl / capryl glucoside, decyl glucoside, lauryl glucoside, cetearyl glucoside, coconut oil alkyl glucoside, and the like, with lauryl glucoside being particularly preferred.

[0036] Examples of the anionic surfactant include higher alkyl sulfates such as sodium lauryl sulfate and potassium lauryl sulfate; polyoxyethylene alkyl ether sulfates such as polyoxyethylene lauryl ether triethanolamine sulfate and sodium polyoxyethylene lauryl ether sulfate; amino acid anionic surfactants such as triethanolamine cocoyl glutamate and potassium cocoyl glycine; N-acylsarcosinates such as sodium lauroyl sarcosine, higher fatty acid amide sulfonates such as sodium N-myristoyl-N-methyl taurine, sodium coconut oil fatty acid methyl taurate and sodium lauryl methyl taurate, phosphate esters such as sodium polyoxyethylene oleyl ether phosphate and polyoxyethylene stearyl ether phosphate; sodium di-2-ethylhexyl sulfosuccinate, monolauroyl monoethanolamide polyoxyethylene sulfosuccinate, sodium lauryl polypropylene sulfonate, sodium lauroyl monoethanolamide polyoxyethylene sulfosuccinate, sodium lauryl polypropylene sulfonate ... Examples of such sulfosuccinates include sodium pyrene glycol sulfosuccinate; alkylbenzene sulfonates such as sodium linear dodecylbenzene sulfonate, triethanolamine linear dodecylbenzene sulfonate, and dodecylbenzene sulfonic acid; N-acyl glutamates such as monosodium N-lauroyl glutamate, disodium N-stearoyl glutamate, and monosodium N-myristoyl-L-glutamate; higher fatty acid ester sulfates such as sodium hydrogenated coconut oil fatty acid glycerin sulfate; polyoxyethylene alkyl ether carboxylic acids; polyoxyethylene alkyl allyl ether carboxylates; α-olefin sulfonates; higher fatty acid ester sulfonates; secondary alcohol sulfates; higher fatty acid alkylolamide sulfates; sodium lauroyl monoethanolamide succinate; ditriethanolamine N-palmitoyl aspartate; and sodium caseinate. Among these, more specific examples include lauryl sulfate, laureth sulfate, lauryl monoglyceride sulfate, lauryl sarcosine or its salt, lauroyl sarcosine or its salt, cocoyl or its salt (more specifically, cocoyl sulfate, cocoyl glutamate, cocoyl glycine salt, cocoyl methylalanine salt, cocoyl aspartate, cocoyl sarcosine salt), tridecylbenzenesulfonate, dodecylbenzenesulfonic acid or its salt, cocoyl isethionate or its salt, etc. Furthermore, examples of these salts include alkali metal salts (particularly sodium salt and potassium salt), ammonium salt, triethylamine salt, mono-, di-, or triethanolamine salt, etc.

[0037] Examples of the amphoteric surfactant include alkylamine oxide, alkylbetaine, alkylamidobetaine, alkylsulfobetaine, alkylglycine salt, alkylcarboxyglycine salt, alkylamphopropionate, alkylamphoglycine salt, alkylamidopropylhydroxysultaine, etc. Here, the alkyl group has 5 to 22 (5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, or 22), preferably 7 to 19, carbon atoms. More specifically, for example, the following formula:

[0038] [ka]

[0039] In the formula, R1 represents a linear or branched alkyl group having 5 to 22 carbon atoms (5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, or 22). The betaine may be a mixture of betaines having different R1, and preferably includes, for example, betaines in which R1CO- is a cocoyl group. In addition, n represents 1 to 6 (1, 2, 3, 4, 5, or 6), and is particularly preferably 3.

[0040] More specifically, examples of the betaine include coconut oil fatty acid amidopropyl betaine (that is, cocamidopropyl betaine: CAPB), lauric acid amidopropyl betaine, and the like.

[0041] Also, for example, the following formula:

[0042] [ka]

[0043] In the formula, R2 represents a linear or branched alkyl group having 1 to 22 carbon atoms (1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, or 22).

[0044] More specifically, examples of the alkyl betaine include trimethylaminoacetic acid betaine (trimethylglycine), lauryldimethylacetic acid betaine, and tetradecyldimethylaminoacetic acid betaine.

[0045] The content of the (b) surfactant is preferably 0.1 to 10.0 mass %, more preferably 0.5 to 8.0 mass %, and particularly preferably 1.0 to 7.0 mass %, based on the total amount of the viscous composition.

[0046] The viscous composition of the present invention may contain minerals, other thickeners, alcohols, pH adjusters, moisturizers, salts, chelating agents, preservatives, antioxidants, UV absorbers, colorants, fragrances, etc., as necessary.

[0047] The viscosity of the viscous composition of the present invention is not particularly limited as long as the viscous composition can be stirred uniformly, but is preferably 10 to 80,000 mPa·s at 25°C.

[0048] The viscous composition of the present invention is used in the fields of, for example, cosmetics, medicines (particularly skin external preparations), toiletries, household products, water-soluble paints, and the like.

[0049] When the viscous composition of the present disclosure is used as a cosmetic, the formulation is not particularly limited, and examples thereof include lotion, milky lotion, beauty essence, cream, cream pack, massage cream, hair setting gel, sunscreen, styling gel, eyeliner, mascara, lipstick, foundation, etc. When the viscous composition of the present disclosure is used as a toiletry product, the formulation is not particularly limited, and examples thereof include cleansing cream, cleansing gel, facial cleanser, hair wash, body wash, rinse, etc.

[0050] The present invention includes all subject matter consisting of any and all combinations of each of the possible combinations of features described herein. EXAMPLES

[0051] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples, but the embodiments of the present invention are not limited to the following examples.

[0052] The storage modulus (G') of the copolymers used in the examples and comparative examples was measured as follows. [Method for measuring storage modulus (G')] 1) <Preparation of neutralized aqueous solution for measurement> 288.8 g of ion-exchanged water was placed in a 500 mL beaker, and 1.5 g of copolymer was added while stirring at 500 rpm using a stirrer with four paddles of φ (diameter) 7 cm. After stirring for 60 minutes, 9.7 g of 6% aqueous sodium hydroxide solution was added to adjust the pH to 6.5 to 7.5, and further stirred for 15 minutes at 300 rpm to prepare a 0.5 mass% neutralized aqueous solution of the copolymer. The pH was measured at 25°C using a pH meter (manufactured by Horiba, Ltd., model number: D-51). 2) <Determination of strain by strain distribution> The temperature of the neutralized aqueous solution obtained in 1) above was set to 25°C, the frequency of a rheometer [manufactured by TA Instruments (model number: AR-2000ex)] was set to 1Hz, and the storage modulus (G') was measured while increasing the strain, and the measurement was terminated when a decrease in the storage modulus (G') was observed. From the obtained strain dispersion graph, if the storage modulus (G') maintained a constant value up to a strain of 1% but could not be maintained up to 10%, the strain in the measurement conditions in 3) below was determined to be 1%, and if the storage modulus (G') maintained a constant value up to a strain of 0.1% but did not maintain a constant value up to 1%, the strain in the measurement conditions in 3) below was determined to be 0.1%. 3) <Determination of storage modulus (G') by frequency dispersion> The temperature of the neutralized aqueous solution obtained in 1) above was set to 25°C, and the angular frequency was changed from 0.1 rad / s to 300 rad / s using a rheometer (TA Instruments, model number: AR-2000ex) under the strain conditions of 0.1% or 1% determined in 2) above. From the measured values, the storage modulus (G') at an angular frequency of 1 rad / s was adopted.

[0053] Preparation of copolymers In a 500 mL four-neck flask equipped with a stirrer, a thermometer, a nitrogen blowing tube, and a cooling tube, 45 g of acrylic acid, 1.35 g of Blenmar VMA70 (manufactured by Nippon Oil & Fats Co., Ltd.: a mixture of 10 to 20 parts by mass of stearyl methacrylate, 10 to 20 parts by mass of eicosanyl methacrylate, 59 to 80 parts by mass of behenyl methacrylate, and 1 part by mass or less of tetracosanyl methacrylate), 0.005 g of pentaerythritol tetraallyl ether, 150 g of normal hexane, and 0.081 g of 2,2'-azobismethyl isobutyrate were charged. After the solution was stirred to mix uniformly, nitrogen gas was blown into the solution to remove oxygen present in the upper space of the reaction vessel (four-neck flask), the raw materials, and the solvent. Then, the mixture was reacted for 4 hours at 55 to 65°C under a nitrogen atmosphere. After the reaction was completed, the resulting slurry was heated to 90°C to remove normal hexane, and then dried under reduced pressure at 110°C and 10 mmHg for 8 hours to obtain 43 g of a white fine powder of an alkyl-modified, carboxyl-containing water-soluble copolymer. The storage modulus of the copolymer was measured by the above-mentioned method and found to be 0.42 Pa.

[0054] Preparation and evaluation of viscous compositions [Example 1] (1) 79.00 g of ion-exchanged water and 20.00 g of a 25% aqueous solution of sodium polyoxyethylene lauryl ether sulfate (manufactured by Kao Corporation, product name: EMAL 20C) were weighed out into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.00 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0055] [Example 2] (1) 82.3 g of ion-exchanged water and 16.7 g of a 30% aqueous solution of sodium coconut oil fatty acid methyl taurate (manufactured by Nikko Chemicals Co., Ltd., product name: NIKKOL CMT-30) were weighed into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0056] [Example 3] (1) 93.1 g of ion-exchanged water and 5.9 g of sodium lauryl sulfate (purity 85%) (manufactured by Kanto Chemical Co., Ltd., product name: sodium lauryl sulfate) were weighed out into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0057] [Example 4] (1) 94.0 g of ion-exchanged water and 5.0 g of polyoxyethylene hydrogenated castor oil (Kao Corporation, product name: Emanon CH-25) were weighed into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0058] [Example 5] (1) 94.0 g of ion-exchanged water and 5.0 g of polysorbate 85 (Kao Corporation, product name: Rheodol TW-0320V) were weighed into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0059] [Example 6] (1) 82.3 g of ion-exchanged water and 16.7 g of a 30% aqueous solution of cocamidopropyl betaine (manufactured by Kawaken Fine Chemicals Co., Ltd., product name: Softazoline CPB-R) were weighed out into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0060] [Example 7] (1) 94.0 g of ion-exchanged water and 5.0 g of cocamide diethanolamide (manufactured by Miyoshi Oil Co., Ltd., product name: Amycol CDE-1) were weighed out into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0061] [Example 8] (1) 94.0 g of ion-exchanged water and 5.0 g of coconut oil fatty acid N-methylethanolamide (manufactured by Kao Corporation, product name: Aminone C-11S) were weighed into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0062] [Example 9] (1) 86.5 g of ion-exchanged water and 12.5 g of a 40% aqueous solution of lauryl glucoside (manufactured by Kao Corporation, product name: Mydol 12) were weighed out into a 200 ml beaker, and this was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0063] [Example 10] (1) 82.3 g of ion-exchanged water and 16.7 g of a 30% aqueous solution of triethanolamine cocoyl glutamate (manufactured by Ajinomoto Co., Inc., product name: Amisoft CT-12S) were weighed out into a 200 ml beaker, and the mixture was stirred at 300 rpm for 5 minutes using a stirrer with four φ5 cm paddles. (2) 1.0 g of the copolymer was weighed out and added to the aqueous solution of (1), and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0064] [Comparative Example 1] (1) 99.0 g of ion-exchanged water and 1.0 g of the copolymer were weighed out into a 200 ml beaker, and the mixture was stirred at 300 rpm using a stirrer having four paddles with a diameter of 5 cm until the copolymer was completely dissolved, thereby obtaining a 1% aqueous solution of the copolymer.

[0065] [Measurement of dissolution time] The time until the copolymer in a 1% aqueous solution was completely dissolved in the aqueous solution was evaluated as the dissolution time. The time until the copolymer is completely dissolved in the aqueous solution means the time when the copolymer powder and gel lumps disappear by visual inspection. Since the dissolution times of Examples 1 to 10 are shorter than those of Comparative Example 1, it can be said that the solubility is improved. The results are shown in Table 1.

[0066] [Table 1] [Industrial Applicability]

[0067] According to the present invention, there is provided a method for producing a viscous composition containing a copolymer having a specific (meth)acrylic acid as a constituent unit, which can improve the solubility of the copolymer in water. Therefore, it is believed that the production efficiency can be improved and the environmental load can be reduced.

Claims

[Claim 1] (a) A copolymer containing a structural unit derived from (meth)acrylic acid (b) Surfactant (c) water A method for producing a viscous composition comprising: The (a) copolymer has a storage modulus (G') of 10 Pa or less at a frequency dispersion of 1 rad / s measured under the following conditions: The method includes a step of adding the copolymer (a) to a mixed solution of the copolymers (b) and (c), Manufacturing method. [Measurement conditions: for a neutralized aqueous solution of pH 6.5 to 7.5 containing 0.5% by mass of the above (a) copolymer based on the total amount of the neutralized aqueous solution, the storage modulus is measured in strain dispersion at a liquid temperature of 25° C. and a rheometer frequency of 1 Hz, and the strain in the subsequent frequency dispersion is determined to be 0.1% or 1%, and under the strain conditions, the storage modulus is measured in frequency dispersion obtained by changing the angular frequency from 0.1 rad / s to 300 rad / s, to determine the storage modulus (G') at an angular frequency of 1 rad / s.]

Citation Information

Patent Citations

  • Water-soluble copolymer having alkyl-modified carboxyl group

    WO2007055354A1