Toner

A toner formulation with carbon black, boron nitride, and controlled fumaric acid content addresses adhesion issues in boron nitride particles, ensuring high image quality and preventing development streaks in challenging environments.

JP2024160734APending Publication Date: 2024-11-15CANON KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023075961
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Boron nitride particles in toner exhibit high lubricity, leading to detachment from the toner surface, especially in high-temperature and high-humidity environments, causing charging performance issues and development streaks due to contamination of the developing blade.

Method used

A toner formulation containing carbon black, boron nitride particles, and fumaric acid, with a controlled content ratio of fumaric acid to boron nitride particles (f0/a0) within 0.050 to 5.000, enhances adhesion and maintains high image quality by forming strong bonds between carbon black and boron nitride particles.

Benefits of technology

The toner achieves high image quality and suppresses development streaks even in long-term use under high temperature and high humidity conditions by improving adhesion and reducing contamination of the developing blade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160734000001
    Figure 2024160734000001
  • Figure 2024160734000002
    Figure 2024160734000002
  • Figure 2024160734000003
    Figure 2024160734000003
Patent Text Reader

Abstract

To provide a toner that can achieve both an improvement in image quality and suppression of development streaks even when used for a long period in a high temperature and high humidity environment.SOLUTION: A toner has toner particles containing a binder resin and a coloring agent, and an external additive. The coloring agent contains carbon black. The external additive includes boron nitride particles. The toner contains fumaric acid. When the content ratio of the boron nitride particles in the toner is defined as a0 (mass%), and the content ratio of the fumaric acid in the toner as f0 (mass%), f0 / a0 is 0.050-5.000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners for use in recording methods utilizing electrophotography, electrostatic recording, and toner jet recording. [Background technology]

[0002] 2. Description of the Related Art In recent years, image forming apparatuses such as copiers and printers are being used for increasingly diverse purposes and environments, and there is a demand for them to be smaller, faster, have higher image quality, and be more stable. In order to achieve excellent durability, for example, Patent Document 1 proposes maintaining and improving the transferability, etc. of the toner by using a toner for developing electrostatic latent images that contains boron nitride having a predetermined number average primary particle size. Furthermore, Patent Document 2 proposes that by using a developer containing boron nitride and providing a supplying means for supplying boron nitride particles and a fatty acid metal salt to an image carrier, it is possible to suppress filming and achieve high image quality by improving cleaning properties. In addition, Patent Document 3 proposes that by mixing toner base particles with boron nitride and then performing surface treatment on the toner base particles with hot air, durability can be improved while achieving both storage stability and low-temperature fixability. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-128406 A [Patent Document 2] JP 2012-103493 A [Patent Document 3] JP 2015-125413 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the inventors of the present invention have found that it is difficult to maintain the adhesion of boron nitride particles to the toner particle surface because of their high lubricity. Therefore, they have found that the boron nitride particles are detached from the toner particle surface. In particular, in a high-temperature and high-humidity environment, the detachment of boron nitride particles may cause a decrease in charging property, resulting in insufficient image quality, or the development blade may become contaminated, resulting in significant development streaks, and therefore improvement was necessary. Furthermore, the inventors have realized that if boron nitride particles or fatty acid metal salts are actively supplied as in the configuration described in Patent Document 2, the developing blade may become significantly contaminated during long-term use, resulting in development streaks. In addition, when the surface of the toner base particles is treated with hot air as described in Patent Document 3, the release agent and plasticizer seep out onto the surface of the toner particles, which may contaminate the developing blade. Then, external additives and other substances that migrate from the toner particles may adhere to and grow on the developing blade, becoming fused products and appearing as development streaks.

[0005] The present disclosure provides a toner that solves the above problems and can achieve both high image quality and suppression of development streaks even when used for a long period of time in a high-temperature, high-humidity environment. [Means for solving the problem]

[0006] The present disclosure relates to A toner having toner particles containing a binder resin and a colorant, and an external additive, The colorant contains carbon black, the external additive comprises boron nitride particles; The toner contains fumaric acid, The toner is characterized in that, when the content of the boron nitride particles in the toner is a0 (mass %) and the content of the fumaric acid in the toner is f0 (mass %), f0 / a0 is 0.050 to 5.000. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a toner that can achieve both high image quality and suppression of development streaks even when used for a long period of time in a high-temperature and high-humidity environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. The term "monomer unit" refers to the reacted form of a monomer substance in a polymer. For example, one section of carbon-carbon bond in the main chain of a polymer in which a polymerizable monomer is polymerized is considered to be one unit. The polymerizable monomer can be represented by the following formula (C). [ka]

[0009] In formula (C), R A represents a hydrogen atom or an alkyl group (preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group); R B represents an optional substituent.

[0010] The present disclosure relates to A toner having toner particles containing a binder resin and a colorant, and an external additive, The colorant contains carbon black, the external additive comprises boron nitride particles; The toner contains fumaric acid, The toner is characterized in that, when the content of the boron nitride particles in the toner is a0 (mass %) and the content of the fumaric acid in the toner is f0 (mass %), f0 / a0 is 0.050 to 5.000.

[0011] The present inventors speculate as follows about the reason why the toner of the present disclosure is able to suppress detachment of boron nitride particles and achieve both high image quality and suppression of development streaks. Boron nitride particles have a hexagonal crystal structure in which hexagonal network structures consisting of BN bonds between boron and nitrogen atoms are layered. The (0001) plane of the hexagonal network structure of boron nitride particles is chemically very stable, and therefore exhibits excellent lubricity against other substances. The inventors have found that the (0001) surface of the boron nitride particles has high lubricity even with respect to the surface of toner particles, that is, the (0001) surface of the boron nitride particles has low adhesion to the surface of toner particles. Therefore, during the electrophotographic printing process, the boron nitride particles are detached from the toner surface. In particular, in a high-temperature and high-humidity environment, the particles are caught, accumulated, and fused at the nip between the development blade and the development carrier, resulting in the problem of development streaks.

[0012] On the other hand, boron nitride particles with a hexagonal crystal structure are suitable for use as a carbon black pigment in toner. The structure of boron nitride is very similar to that of carbon black. Specifically, like carbon black, functional groups such as -OH groups (hydroxyl groups) and -NH2 groups (amino groups) are present on the surface of boron nitride particles. The inventors of the present invention thought that if they could take advantage of this similar structure and strengthen the interaction between carbon black and boron nitride, they could increase the adhesion to toner particles while maintaining the lubricity that is a characteristic of boron nitride, thereby solving the above-mentioned problems. As a result of intensive research, the inventors of the present invention found that by making the colorant contained in the toner particles contain carbon black, making the toner contain fumaric acid, and further controlling the content ratio of fumaric acid and boron nitride particles in the toner, it was possible to significantly improve the adhesion of boron nitride particles to toner particles. As a result, it was found that it is possible to achieve both high image quality and suppression of development streaks when used for a long period of time in a high-temperature and high-humidity environment.

[0013] This is because the carboxyl groups in the fumaric acid molecules form hydrogen bonds with the terminal functional groups, such as hydroxyl groups and amino groups, contained in the carbon black and boron nitride particles, respectively, and the carbon black and boron nitride particles are strongly bonded to each other. In other words, the carbon black and boron nitride particles interact with each other via the fumaric acid. As a result, it is believed that the adhesion of the boron nitride particles to the toner particles increases. In addition, fumaric acid has a double bond and a trans-type molecular structure. Therefore, compared to other dicarboxylic acids, it is less likely to cause steric hindrance and does not become anhydride. As a result, we believe that fumaric acid can efficiently and firmly bind boron nitride particles and carbon black.

[0014] The present disclosure will now be described in detail. The toner has toner particles containing a binder resin and a colorant, and an external additive. The colorant contains carbon black. The external additive contains boron nitride particles. The toner contains fumaric acid. When the content of the boron nitride particles in the toner is a0 (mass%) and the content of the fumaric acid in the toner is f0 (mass%), f0 / a0 is 0.050 to 5.000.

[0015] f0 / a0 represents the ratio of the content of fumaric acid in the toner to the content of boron nitride particles in the toner. When f0 / a0 satisfies the above range, the ratio of fumaric acid to boron nitride particles in the toner becomes optimal. As a result, the interaction between the carboxyl group in the fumaric acid molecule and the functional groups contained in the boron nitride particles and carbon black becomes sufficient, improving the adhesion of the boron nitride particles to the toner particles. Furthermore, contamination of the developing blade is suppressed, and it is possible to achieve both high image quality and suppression of development streaks. When f0 / a0 is less than 0.050, there is not enough fumaric acid relative to the boron nitride particles, and the adhesion of the boron nitride particles to the toner particles is not sufficiently improved, and the development streaks may not be sufficiently suppressed. On the other hand, when f0 / a0 is more than 5.000, the interaction between the carboxyl group in the fumaric acid molecule and the functional groups contained in the boron nitride particles and carbon black becomes too large, and the lubricity of the boron nitride particles is reduced. Furthermore, the charging property is reduced, and the development streaks may not be sufficiently suppressed due to contamination of the development blade. f0 / a0 is more preferably 0.100 to 5.000, further preferably 0.200 to 5.000, and particularly preferably 0.250 to 5.000. Within the above range, development streaks can be more effectively suppressed. f0 / a0 is calculated from the values ​​obtained by measuring f0 and a0 by the method described below.

[0016] The content ratio f0 (mass %) of fumaric acid in the toner is preferably 0.001 to 0.120 mass %, more preferably 0.005 to 0.120 mass %, and even more preferably 0.010 to 0.120 mass %. By satisfying the above conditions, the content ratio of fumaric acid in the toner becomes more appropriate. Fumaric acid has chargeability and hygroscopicity. Therefore, by making the content ratio of fumaric acid more appropriate, the charge amount and charge standability in a high-temperature and high-humidity environment can be improved. This makes it possible to achieve both high-temperature and high-humidity fogging and suppresses fogging on the drum after the first sheet is printed after being left in a high-temperature, high-humidity environment for two days (hereinafter referred to as durable fogging in an H / H environment), resulting in excellent dot reproducibility in a high-temperature, high-humidity environment. The method for measuring the content ratio f0 of fumaric acid in the toner will be described later. Measuring f0 by the method described later indicates that fumaric acid exists in a free state in the toner. The value of the content ratio f0 of fumaric acid in the toner can be adjusted by changing the amount of fumaric acid added during toner production.

[0017] When the content of fumaric acid in the toner extracted by methanol is f1 (mass%), the f1 is preferably 0.0010 to 0.0100 mass%, more preferably 0.0012 to 0.0090 mass%, and even more preferably 0.0014 to 0.0084 mass%. Methanol hardly dissolves the binder resin in the toner particles, but can dissolve the fumaric acid contained in the surface vicinity of the toner. Therefore, f1 is an index of the content of fumaric acid contained in the surface vicinity of the toner. By setting f1 in the above range, both the chargeability and the hygroscopicity can be effectively achieved at a high level, and the durable fogging in the H / H environment can be significantly suppressed. A method for measuring the content ratio f1 of fumaric acid extracted from the toner with methanol in the toner will be described later. The value of f1 can be adjusted by changing the amount of fumaric acid added during the production of the toner.

[0018] f1 / a0 is preferably 0.005 to 0.350, more preferably 0.005 to 0.250, and even more preferably 0.005 to 0.200. When the above range is satisfied, the ratio of fumaric acid contained in the toner surface vicinity to boron nitride particles in the toner becomes more appropriate. As a result, the interaction between the carboxyl group in the fumaric acid molecule and the functional group contained in the boron nitride particles and carbon black is efficiently performed, and the adhesion of the boron nitride particles to the toner particles is further improved. Furthermore, the charge transfer performance of the toner is improved, and the uniform charging property is further improved. f1 / a0 is calculated from the values ​​obtained by measuring f1 and a0 by the method described later.

[0019] The means for making the toner contain fumaric acid is not particularly limited, and known means can be used. For example, fumaric acid can be made to be contained in the toner particles. That is, it is preferable that the toner particles contain fumaric acid. Specifically, when producing toner particles by a pulverization method, a method can be used in which fumaric acid is incorporated into the raw material resin in advance, or a method can be used in which fumaric acid is added when the raw material is melted and kneaded so that it is incorporated into the toner particles. When toner particles are produced by a wet production method such as a suspension polymerization method or an emulsion aggregation method, a method of incorporating fumaric acid in the raw material or a method of adding fumaric acid via an aqueous medium during the production process can be used. Further, it is also possible to use a method of externally adding fumaric acid to toner particles by using a known external addition method.

[0020] The content a0 (mass %) of boron nitride particles in the toner is preferably from 0.009 to 1.050 mass %, and more preferably from 0.010 to 1.000 mass %. By satisfying the above conditions, the content ratio of boron nitride particles in the toner becomes more appropriate. Boron nitride particles have excellent lubricity. Therefore, by making the content ratio in the toner more appropriate, the slipperiness between the cleaning blade and the photoconductor can be improved in a system that employs a blade cleaning method. As a result, the cleaning ability of the external additive that has migrated from the toner to the photoconductor can be improved. The method for measuring the content ratio a0 of boron nitride particles in the toner will be described later. The value of the content ratio a0 of boron nitride particles in the toner can be determined by changing the amount of boron nitride particles added during toner production. This can be adjusted.

[0021] Next, materials that can be used in the toner of the present disclosure will be described in detail below.

[0022] <Boron nitride> The toner contains an external additive. The external additive contains boron nitride particles. The boron nitride particles have a hexagonal crystal structure. That is, the crystal system of the boron nitride particles is a hexagonal crystal system. One method for producing boron nitride particles is, for example, the reduction and nitridation of molten boric anhydride with ammonia. Reduction and nitridation basically follows the reaction formula B2O3+NH3→2BN+3H2O. Specifically, for example, boric acid, borate salts, molten boric anhydride, etc. are used as raw materials, and are reduced and nitrided by reacting with ammonia in a synthesis furnace. After that, boron nitride particles can be obtained through purification and crystallization treatment. At temperatures of around 450°C, boron oxide softens and becomes glassy, ​​and nitridation stops. For this reason, boric acid, borate salts, molten boric anhydride, etc. are used as raw materials, and urea, dicyandiamide, ammonium chloride, etc. are added to the raw materials, which are then heated to cause reduction and nitridation. The boron nitride particles produced by the above method may contain oxygen atoms as trace impurities. The amount of oxygen atoms can be adjusted by the raw materials, the type of catalyst for promoting the reaction, the amount of catalyst, and the reaction conditions.

[0023] The number-average particle diameter of the primary particles of the boron nitride particles is preferably 300 to 2000 nm, more preferably 450 to 1200 nm, even more preferably 450 to 1000 nm, and particularly preferably 700 to 1000 nm. If it is 300 nm or more, the boron nitride particles effectively act as spacers and can maintain fluidity throughout long-term use. As a result, the charge retention performance is excellent and the image density uniformity is improved. Also, if it is 1200 nm or less, the adhesion area of ​​the boron nitride particles to the toner particles is sufficient, and the interaction between the boron nitride particles and the carbon black via fumaric acid is large. As a result, the adhesion of the boron nitride particles to the toner particles is improved, the detachment of the boron nitride particles is suppressed, and development streaks are suppressed for a long period of time. The number average particle size of the primary particles of the boron nitride particles can be adjusted by the type of catalyst for promoting the reaction and the reaction conditions. It can also be adjusted by pulverizing the produced boron nitride particles using a known wet pulverizer. The method for measuring the number average particle size of the primary particles of the boron nitride particles will be described later.

[0024] The shape of the boron nitride particles is not particularly limited, but the boron nitride particles are preferably flat particles. When the major axis of the boron nitride particles is D (nm) and the thickness is T (nm), D / T is preferably 6 to 20, more preferably 13 to 20. By setting D / T within the above range, the boron nitride particles are easily attached to the surface of the toner particles, and the boron nitride particles and the carbon black are easily interacted with each other via fumaric acid near the surface of the toner particles. As a result, the adhesion of the boron nitride particles to the toner particles is improved, and the detachment of the boron nitride particles is suppressed, thereby suppressing development streaks over a long period of time.

[0025] The major axis D (nm) of the boron nitride particles is not particularly limited, but is preferably 300 to 2000 nm, more preferably 450 to 1200 nm, and even more preferably 700 to 1000 nm. The major axis of the boron nitride particles can be adjusted by the catalyst species and reaction conditions for promoting the reaction. It can also be adjusted by pulverizing the produced boron nitride particles using a known wet pulverizer. The method for measuring the major axis of the boron nitride particles will be described later.

[0026] The thickness T (nm) of the boron nitride particles is not particularly limited, but is preferably from 25 to 230 nm, more preferably from 30 to 205 nm, and even more preferably from 35 to 120 nm. The thickness of the boron nitride particles can be adjusted by the catalyst species and reaction conditions for promoting the reaction. It can also be adjusted by pulverizing the produced boron nitride particles using a known wet pulverizer. The method for measuring the thickness of the boron nitride particles will be described later.

[0027] <Binding resin> The toner includes toner particles, and the toner particles contain a binder resin. The binder resin may be any known binder resin without any particular limitations. Specific examples include polyester resin, vinyl resin, polyurethane resin, polyamide resin, etc. The binder resin preferably contains a polyester resin, and more preferably contains a polyester resin having a monomer unit corresponding to fumaric acid, since this makes it easier to retain fumaric acid in the toner. As the polyester resin, it is preferable to use at least one selected from the group consisting of an amorphous polyester resin and a crystalline polyester resin.

[0028] The polyester resin can be obtained by combining suitable compounds selected from polyvalent carboxylic acids, polyols, hydroxycarboxylic acids, etc., and synthesizing the compounds using a known method such as an ester exchange method or a polycondensation method. Polycarboxylic acids are compounds containing two or more carboxy groups in one molecule. Among them, dicarboxylic acids are compounds containing two carboxy groups in one molecule and are preferably used.

[0029] Examples of dicarboxylic acids include fumaric acid, oxalic acid, succinic acid, glutaric acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-carboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, suberic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylenediacetic acid, m-phenylenediacetic acid, o-phenylenediacetic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracenedicarboxylic acid, and cyclohexanedicarboxylic acid. As described above, it is preferable to contain fumaric acid as the dicarboxylic acid, and it is more preferable to use fumaric acid in combination with an aromatic dicarboxylic acid.

[0030] Examples of polycarboxylic acids other than dicarboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, pyrene tetracarboxylic acid, itaconic acid, glutaconic acid, n-dodecyl succinic acid, n-dodecenyl succinic acid, isododecyl succinic acid, isododecenyl succinic acid, n-octyl succinic acid, and n-octenyl succinic acid. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0031] A polyol is a compound containing two or more hydroxyl groups in one molecule. Among them, a diol is a compound containing two hydroxyl groups in one molecule, and is preferably used. Specifically, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanediol, dipropylene glycol, polyethylene glycol, polypropylene glycol, Examples of suitable bisphenols include ethylene glycol, polytetramethylene ether glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-butenediol, neopentyl glycol, 1,4-cyclohexanediol, polytetramethylene glycol, hydrogenated bisphenol A, bisphenol A, bisphenol F, bisphenol S, and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols are particularly preferred.

[0032] Examples of trivalent or higher polyols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, tetraethylolbenzoguanamine, sorbitol, trisphenol PA, phenol novolac, cresol novolac, and alkylene oxide adducts of the above-mentioned trivalent or higher polyphenols. The polyols may be used alone or in combination of two or more kinds.

[0033] The peak top molecular weight (Mp) of the polyester resin is not particularly limited, but is preferably 5000 to 10000, and more preferably 5000 to 8000. When the peak top molecular weight of the polyester resin is within the above range, the adhesion of boron nitride and toner particles is reduced, and thus it is possible to suppress the occurrence of development streaks. The peak top molecular weight of the polyester resin can be controlled by a known method such as controlling the reaction time. The type of binder resin can be measured by a known method such as NMR.

[0034] The content of the binder resin relative to 100 parts by mass of the toner particles is not particularly limited, but may be 50.0 to 98.0 parts by mass, or 60.0 to 95.0 parts by mass.

[0035] <Release agent> The toner preferably contains a release agent. By containing the release agent, a release agent layer is formed on the image surface, thereby improving the strength of the image surface. As the releasing agent, there are no particular limitations and known waxes, silicone oils, etc. can be used. Among them, it is preferable to use wax. Specific examples of waxes include paraffin wax, microcrystalline wax, petroleum-based hydrocarbon waxes such as petrolatum and derivatives thereof, montan wax and derivatives thereof, and Fischer-Tropsch hydrocarbon waxes and derivatives thereof. monofunctional ester waxes, such as behenyl behenate, stearyl stearate, and palmityl palmitate, typified by esters of monohydric alcohols and aliphatic carboxylic acids, or esters of monohydric carboxylic acids and aliphatic alcohols; bifunctional ester waxes, such as esters of dihydric alcohols and aliphatic carboxylic acids, or esters of dihydric carboxylic acids and aliphatic alcohols, such as ethylene glycol distearate, dibehenyl sebacate, and hexanediol dibehenate; trifunctional ester waxes, such as esters of trihydric alcohols and aliphatic carboxylic acids, such as glycerol tribehenate, or esters of trihydric carboxylic acids and aliphatic alcohols; tetrafunctional ester waxes, such as esters of tetrahydric alcohols and aliphatic carboxylic acids, or esters of tetrahydric carboxylic acids and aliphatic alcohols, such as pentaerythritol tetrastearate and pentaerythritol tetrapalmitate; Esters of hexavalent alcohols and aliphatic carboxylic acids, such as dipentaerythritol hexastearate and dipentaerythritol hexapalmitate, or hexavalent carboxylic acids and hexafunctional ester waxes, represented by esters of fatty alcohols; Esters of polyhydric alcohols and aliphatic carboxylic acids, such as polyglycerol behenate, or esters of polyhydric carboxylic acids and aliphatic alcohols; Natural ester waxes such as carnauba wax and rice wax; Ester waxes, such as Examples of the wax include polyolefin-based hydrocarbon waxes such as polyethylene and polypropylene and their derivatives, and natural waxes such as carnauba wax and candelilla wax and their derivatives. The derivatives include oxides, block copolymers with vinyl monomers, and graft modified products. Other examples include alcohols such as higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid or their acid amides, esters, and ketones, hydrogenated castor oil and its derivatives, vegetable waxes, and animal waxes. These can be used alone or in combination of two or more kinds.

[0036] Among them, at least one selected from the group consisting of hydrocarbon waxes and ester waxes is preferred, and at least one selected from the group consisting of Fischer-Tropsch hydrocarbon waxes, tetrafunctional ester waxes and hexafunctional ester waxes is more preferred. These waxes have high crystallinity and therefore tend to form a uniform release agent layer on the image surface, and are excellent in terms of the effect of increasing the strength of the image surface.

[0037] The content of the release agent is preferably 1.0 to 30.0 parts by mass, and more preferably 5.0 to 20.0 parts by mass, relative to 100.0 parts by mass of the binder resin. The melting point of the release agent is preferably 60 to 120° C., more preferably 70 to 120° C., and even more preferably 80 to 120° C. By using a release agent having a melting point in the above range, the heat resistance of the image is further improved.

[0038] The molecular weight of the release agent is not particularly limited, but may be 500-1,800, and is preferably 700-1,500.

[0039] <Plasticizer> The toner may contain a plasticizer. The plasticizer is not particularly limited, and the waxes listed in the section on release agents can be used.

[0040] <Coloring agent> The toner particles contain a colorant. The colorant contains carbon black. The carbon black is not particularly limited, and examples thereof include furnace black, gas black, thermal black, acetylene black, and lamp black. When the colorant contains carbon black, the carbon black and the boron nitride particles interact with each other via fumaric acid, and therefore the adhesion of the boron nitride particles to the toner particles is increased. The amount of carbon black contained is not particularly limited, but is preferably 2.0 to 12.0 parts by mass, and more preferably 3.0 to 10.0 parts by mass, relative to 100.0 parts by mass of the binder resin. The fact that the colorant contains carbon black is confirmed by the STEM-EDS analysis of the toner described below.

[0041] When the content ratio of carbon black in the toner particles is c0 (mass%), c0 / f0 is preferably 15 to 1400, more preferably 15 to 1200, further preferably 25 to 800, and particularly preferably 50 to 600. c0 / f0 is the ratio of carbon black in the toner particles to fumaric acid in the toner. Shows. Since fumaric acid has a double bond, it is easy for electrons to be transferred to and from carbon black via the π electrons of the conjugated system. Therefore, by controlling the content within this range, the charge transfer performance into the toner is significantly improved, and the dot reproducibility of the image is improved. c0 / f0 is calculated from the values ​​obtained by measuring c0 and f0 using the method described below.

[0042] Furthermore, c0 / a0 is preferably from 2 to 800, more preferably from 3 to 750, and even more preferably from 30 to 500. c0 / a0 represents the abundance ratio of carbon black in the toner particles to boron nitride particles in the toner. By controlling the content within this range, it is easy to balance the lubricity of boron nitride and the strong adhesion of boron nitride particles to toner particles due to the interaction via fumaric acid. Therefore, it is easy to suppress development streaks and maintain chargeability at the same time. c0 / a0 is calculated from the values ​​obtained by measuring c0 and a0 using the method described below.

[0043] The carbon black content c0 (mass%) in the toner particles is not particularly limited, but is preferably 1.0 to 15.0 mass%, more preferably 2.5 to 10.5 mass%, more preferably 3.0 to 10.0 mass%, and particularly preferably 4.0 to 8.0 mass%. When the value of c0 is within the above range, it is easy to adjust c0 / a0 to the above range. A method for measuring the content ratio c0 of carbon black in toner particles will be described later. The value of the content ratio c0 of carbon black in toner particles can be adjusted by changing the amount of carbon black added during the production of the toner particles.

[0044] In order to strengthen the interaction between the boron nitride particles and the carbon black via fumaric acid, it is preferable that the carbon black is present near the surface of the toner particles. The presence of the carbon black near the surface of the toner particles is confirmed by the following method. That is, in cross-sectional observation of the toner with a scanning transmission electron microscope (STEM), it is preferable that the carbon black is present in a region 100 nm deep from the toner surface. The presence of carbon black near the surface of the toner particles is confirmed by observing the cross-section of the toner with a scanning transmission electron microscope (STEM). Specifically, an Os film (5 nm) and a naphthalene film (20 nm) are applied to the toner as a protective film using an osmium plasma coater (OPC80T, Filgen), and the toner is then embedded in a photocurable resin D800 (JEOL). Then, a cross-section of the toner with a film thickness of 60 nm (or 70 nm) is prepared using an ultrasonic ultramicrotome (UC7, Leica) at a cutting speed of 1 mm / s. The obtained cross-section is observed with a STEM (JEM2800, JEOL). If carbon black is present in a region 100 nm deep from the toner surface, it is determined that carbon black is present near the surface of the toner particles. Detailed measurement conditions will be described later.

[0045] <Charge control agent> The toner may contain a charge control agent. As the charge control agent, any known charge control agent can be used without any particular limitation. Specifically, examples of negative charge control agents include metal compounds of aromatic carboxylic acids such as salicylic acid, alkylsalicylic acid, dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids, or polymers or copolymers having metal compounds of the aromatic carboxylic acids; polymers or copolymers having a sulfonic acid group, a sulfonate salt group, or a sulfonate ester group; metal salts or metal complexes of azo dyes or azo pigments; boron compounds, silicon compounds, and calixarenes. On the other hand, examples of the positive charge control agent include quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains, guanidine compounds, nigrosine compounds, imidazole compounds, and the like. As the polymer or copolymer having a sulfonate group or a sulfonate ester group, there is styrene. Homopolymers of sulfonic acid group-containing vinyl monomers such as styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, and methacrylsulfonic acid, or copolymers of other known vinyl monomers and the above-mentioned sulfonic acid group-containing vinyl monomers can be used. The content of the charge control agent is preferably 0.01 parts by mass or more and 5.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0046] <External additives> The toner has an external additive. The external additive contains boron nitride particles. The external additive may contain an external additive other than the boron nitride particles in addition to the boron nitride particles. As the external additive, any known external additive can be used without any particular limitation. Specific examples include raw silica fine particles such as wet-process silica and dry-process silica, or surface-treated silica fine particles obtained by subjecting such raw silica fine particles to a surface treatment with a treating agent such as a silane coupling agent, a titanium coupling agent, or silicone oil; and resin fine particles such as vinylidene fluoride fine particles and polytetrafluoroethylene fine particles. The content of the external additive is preferably 0.1 to 5.0 parts by mass with respect to 100.0 parts by mass of the toner particles.

[0047] Next, a method for obtaining the toner of the present disclosure will be described in detail below.

[0048] <Method of manufacturing toner particles> The method for producing the toner particles is not particularly limited, and an emulsion aggregation method, a suspension polymerization method, a dissolution suspension method, a pulverization method, or the like can be used. Among these, it is preferable to use the emulsion aggregation method. That is, it is preferable that the toner particles are emulsion aggregation toner particles. In the emulsion aggregation method, a dispersion of fine particles of a binder resin is first prepared, followed by a dispersion of a colorant and, if necessary, a dispersion of each material such as a release agent. The obtained dispersions of each material are dispersed and mixed, with the addition of a dispersion stabilizer if necessary. Then, an aggregating agent is added to aggregate the particles to the desired toner particle size, and then or simultaneously with the aggregation, the resin fine particles are fused together. If necessary, the shape is controlled by heat to form toner particles.

[0049] The method for producing the toner preferably includes the following steps. (1) A dispersion and mixing step of preparing a binder resin particle dispersion liquid (and, if necessary, a colorant particle dispersion liquid, etc.) containing a binder resin and fumaric acid, and mixing them to obtain a mixed dispersion liquid; (2) an aggregation step of aggregating the binder resin fine particles (and colorant fine particles, if necessary) contained in the obtained mixed dispersion to form aggregates; and (3) a fusion step of heating the aggregates to fuse them together to form fused particles; The resulting fused particles can be cooled to obtain toner particles.

[0050] It is preferable to have the following step (4) during the above step (3) or after the above steps (1) to (3). (4) A spheronization step in which the agglomerates are heated at a higher temperature. Furthermore, it is more preferable to have the following steps (5) and (6) in this order after the above step (4). (5) A cooling step of cooling the aggregate at a cooling rate of 0.1° C. / min or more. (6) an annealing step of heating and holding the temperature at or above the crystallization temperature or the glass transition temperature of the binder resin after the cooling step;

[0051] Here, the fine particles of the binder resin may be composite particles formed of two or more layers of resins having different compositions. For example, the fine particles may be formed by emulsion polymerization or mini-emulsion polymerization. The emulsion can be produced by at least one method selected from the group consisting of a phase inversion emulsification method and a phase inversion emulsification method.

[0052] When an internal additive is contained in the toner particles, the internal additive may be contained in the resin fine particles, or a dispersion liquid of internal additive fine particles containing the internal additive may be prepared separately, and the internal additive fine particles may be aggregated together with the resin fine particles when the internal additive fine particles are aggregated. In addition, toner particles having layer structures with different compositions can be produced by adding resin fine particles with different compositions at different times during aggregation and aggregating them. That is, toner particles having a core-shell structure can be produced. After aggregating resin fine particles containing a binder resin to form a core portion, resin fine particles containing a shell resin can be added at different times and aggregating them to form a shell portion. The shell resin may be the same as or different from the binder resin. For example, the shell resin may contain fumaric acid. The resin fine particles containing the shell resin may contain fumaric acid. The amount of the shell resin added (shell content) is preferably 1.0 to 10.0 parts by mass, more preferably 2.0 to 7.0 parts by mass, based on 100 parts by mass of the binder resin contained in the core particles.

[0053] In the case of producing toner particles having a core-shell structure, the method for producing the toner preferably includes the following steps in the following order. (1) A dispersion and mixing step of preparing a dispersion of binder resin particles containing a binder resin and fumaric acid (or a colorant particle dispersion, if necessary) and mixing the mixture to obtain a mixed dispersion; (2) an aggregation step of aggregating the binder resin particles (and, if necessary, colorant particles) contained in the obtained mixed dispersion to form aggregates; (3) a shell formation step of further adding resin fine particles containing a resin for a shell to the dispersion containing the aggregates, and aggregating the resin fine particles to form aggregates having a shell; and (4) a fusion step of heating the aggregates to fuse them together to form fused particles;

[0054] In addition, it is preferable to have the following step (5) during the above step (4) or after the above steps (1) to (4). (5) A spheronization step in which the agglomerates are heated at a higher temperature. It is more preferable to have the following steps (6) and (7) after the above step (5). (6) A cooling step of cooling the aggregate at a cooling rate of 0.1° C. / sec or more. (7) an annealing step of heating and holding the temperature at or above the crystallization temperature or the glass transition temperature of the binder resin after the cooling step;

[0055] The amount of fumaric acid added is not particularly limited, but is preferably 0.006 to 0.500 parts by mass, more preferably 0.006 to 0.400 parts by mass, and even more preferably 0.006 to 0.200 parts by mass, relative to 100 parts by mass of the binder resin. By being in the above range, it becomes easier to suitably adjust the content ratio f0 of fumaric acid in the toner. The amount of boron nitride particles added is not particularly limited, but is preferably 0.005 to 1.200 parts by mass, more preferably 0.010 to 1.000 parts by mass, and even more preferably 0.100 to 1.000 parts by mass, relative to 100 parts by mass of toner particles. By being in the above range, it becomes easy to suitably adjust the content ratio a0 of boron nitride particles in the toner.

[0056] The following can be used as the dispersion stabilizer. As the dispersion stabilizer, a surfactant can be used, including known cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of inorganic dispersion stabilizers include tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Examples of the organic dispersion stabilizer include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch. These can be used alone or in combination of two or more.

[0057] As the flocculant, in addition to a surfactant having a polarity opposite to that of the surfactant used in the above-mentioned dispersion stabilizer, an inorganic salt or a divalent or higher inorganic metal salt can be suitably used. In particular, an inorganic metal salt is preferred because it is easy to control the flocculation property and the toner charge property by ionizing a polyvalent metal element in an aqueous medium. Specific examples of preferred inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, iron chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyiron chloride, polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. Among these, aluminum salts and their polymers are particularly preferred. These can be used alone or in combination of two or more. In general, in order to obtain a sharper particle size distribution, the valence of the inorganic metal salt is preferably divalent rather than monovalent, and more preferably trivalent or more than divalent. Furthermore, even if the valence is the same, an inorganic metal salt polymer is more suitable.

[0058] From the viewpoint of high definition and high resolution of images, the weight average particle size (D4) of the toner particles is preferably 3.0 to 10.0 μm. From the viewpoint of the balance between developing ability and cleaning ability, the average circularity of the toner particles is preferably 0.935 to 0.985, and more preferably 0.940 to 0.980.The average circularity of the toner particles is preferably 0.935 to 0.985, and more preferably 0.940 to 0.980. The average circularity can be controlled by adjusting the production conditions of the toner particles.

[0059] <Toner manufacturing method> The toner particles obtained above can be mixed with an external additive containing boron nitride particles and attached to the surface of the toner particles to produce a toner. That is, the toner manufacturing method includes an external addition step of externally adding an external additive containing boron nitride particles to the toner particles. At this time, an external additive other than the above-mentioned boron nitride particles may be added as necessary. The mixer for adding the external additive to the toner particles is not particularly limited, and any known mixer can be used, regardless of whether it is a dry or wet type. Examples include FM Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (manufactured by Kawata Corporation), Nobilta (manufactured by Hosokawa Micron Corporation), and Hybridizer (manufactured by Nara Machinery Co., Ltd.). In order to control the coating state of the external additive, the toner can be prepared by adjusting the rotation speed, processing time, and water temperature and amount of water in the jacket of the external addition device. In addition, sieving devices used to sift out coarse particles after external addition include Ultrasonic (manufactured by Koei Sangyo Co., Ltd.); Resonaseave, Gyroshifter (Tokuju Kogyo Co., Ltd.); Vibrasonic System (manufactured by Dalton Co., Ltd.); Soniclean (manufactured by Shinto Kogyo Co., Ltd.); Turbo Screener (manufactured by Turbo Kogyo Co., Ltd.); Microshifter (manufactured by Makino Sangyo Co., Ltd.), etc.

[0060] The methods for measuring the physical properties of the toner and each material will be described below.

[0061] <Method for measuring the content of fumaric acid in toner (% by mass)> Dissolve 0.1 g of toner in 1 ml of chloroform. Add 20 ml of methanol to the resulting sample solution. 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile are added to the resulting sample, which is then heated to 80°C for 1 hour to perform a silylation treatment. The resulting sample is analyzed by GC-MS (gas chromatography mass spectrometry).

[0062] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0063] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is contained. On the other hand, several samples of fumaric acid alone (e.g., 100 ng, 200 ng, and 300 ng) are precisely weighed and prepared, and before measuring the sample obtained from the toner, each sample is measured under the above-mentioned analytical conditions, and then a calibration curve is created from the amount of fumaric acid added and the fumaric acid peak area value. The content ratio f0 (mass %) of fumaric acid in the toner is obtained by converting the area value of the fumaric acid component of the toner based on this calibration curve into the mass of fumaric acid, and then converting it into an amount based on the toner mass.

[0064] <Method for measuring the content f1 (mass%) of fumaric acid in toner, which is extracted from toner with methanol> 0.5 g of toner is placed in 20 ml of methanol and dispersed for 30 minutes. Then, solids are removed by centrifugation (HITACHI himac CR22G, 12000 rpm, 10 minutes). The solvent is removed from the resulting solution by vacuum distillation, and the solution is further dried for 4 hours under reduced pressure in a 60°C atmosphere. 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile are added to the resulting sample, which is then heated at 80°C for 1 hour to perform a silylation treatment. The resulting sample is analyzed by GC-MS (gas chromatography mass spectrometry).

[0065] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0066] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is contained. On the other hand, several samples of fumaric acid alone (e.g., 100 ng, 200 ng, and 300 ng) are precisely weighed and prepared, and before measuring the sample obtained from the toner, each sample is measured under the above-mentioned analytical conditions, and then a calibration curve is created from the amount of fumaric acid added and the fumaric acid peak area value. The content ratio f1 (mass %) of fumaric acid in the toner extracted with methanol is obtained by converting the area value of the fumaric acid component in the toner based on this calibration curve into the mass of fumaric acid, and then converting it into an amount based on the toner mass.

[0067] <Method for measuring the content a0 (mass%) of boron nitride particles in toner> (Method for isolating toner particles and boron nitride particles from a toner) Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. In a centrifuge tube (50 mL capacity), add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries, Ltd.). Add 1.0 g of toner to this and break up the toner clumps with a spatula or the like. Shake the centrifuge tube at 300 strokes per minute (spm) for 20 minutes in a shaker (AS-1N, sold by AS ONE Corporation). After shaking, transfer the solution to a glass tube for a swing rotor (50 mL) and separate it in a centrifuge (H-9R, manufactured by Kokusan Corporation) at 3,500 rpm for 30 minutes. This operation separates the toner particles from the external additives. It is visually confirmed that the toner particles and the aqueous solution are sufficiently separated, and the separated toner particles and external additives are collected with a spatula or the like. When boron nitride particles and external additives other than boron nitride particles are mixed as external additives, the target substances are isolated by further centrifugal separation, taking advantage of the difference in particle size and specific gravity. The isolated toner particles and boron nitride particles are filtered with a reduced pressure filter, and then dried in a vacuum dryer at 40°C under reduced pressure for 24 hours or more to obtain toner particles and boron nitride particles. The above operation is carried out multiple times depending on the required amount of toner particles and boron nitride particles.

[0068] (Method for identifying constituent elements of boron nitride particles) The constituent elements of the boron nitride particles are identified by SEM-EDS analysis of the boron nitride particles isolated by the above method. The constituent elements of boron nitride particles can be identified by combining shape observation with a scanning electron microscope (SEM) and elemental analysis with energy dispersive X-ray analysis (EDS). The isolated boron nitride particles are observed using a scanning electron microscope "Ultra Plus" (product name; manufactured by Carl Zeiss). The boron nitride particles are subjected to EDS analysis, and the boron nitride particles can be identified based on the presence or absence of element peaks. When the boron element peak and the nitrogen element peak constituting the boron nitride particles are observed as element peaks, the observed particles are judged to be boron nitride particles.

[0069] (Method for measuring the content a0 (mass%) of boron nitride particles in toner) The content ratio a0 of boron nitride particles in the toner can be calculated by measuring the toner and the toner particles from which the external additives have been removed by the above-mentioned method using X-ray fluorescence analysis (XRF). The measurement equipment used was a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "Sup The X-ray tube anode is Rh, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. When measuring boron, which is a light element, it is detected with a proportional counter (PC). The measurement sample is prepared by placing 4g of toner in a special aluminum ring for pressing, flattening it, and pressing it at 20MPa for 60 seconds using a tablet press "BRE-32" (Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of 2mm and a diameter of 39mm. The pellet is then used to measure the count rate intensity (unit: cps) of boron element. The acceleration voltage and current value of the X-ray generator are 32kV and 125mA, respectively. In order to calculate the ratio of the boron elemental strength contained in the boron nitride particles to the boron elemental strength of the toner being analyzed, a similar measurement is performed on a sample in which the toner particles isolated by the above-mentioned method are mixed with external additives other than the isolated boron nitride particles to obtain the boron elemental strength after separation of the boron nitride particles. From the boron elemental strength of the toner and the boron elemental strength after separation of the boron nitride particles, the boron elemental strength contained in the boron nitride particles in the toner is calculated according to the following formula: (boron elemental strength ratio contained in boron nitride particles in toner)=(boron elemental strength of toner-boron elemental strength after separation of boron nitride particles) / (boron elemental strength of toner)

[0070] The boron elemental strength of the toner is multiplied by the boron elemental strength ratio contained in the boron nitride particles in the toner to determine the boron elemental strength originating from boron nitride in the toner. The amount of boron nitride contained in the toner is determined as a percentage of the toner weight by comparing the boron elemental strength originating from boron nitride in the toner with a separately prepared calibration curve for boron nitride particles, and this is designated as the content ratio a0 (mass%) of the boron nitride particles contained in the toner.

[0071] <Method of measuring number average particle size and D / T of primary particles of boron nitride particles> The number average particle size of the primary particles of the boron nitride particles is measured using a scanning electron microscope "Ultra Plus" (product name; manufactured by Zeiss). The boron nitride particles are identified by the above-mentioned SEM-EDS analysis. The toner is observed under the following conditions, and the major axis D (nm) and thickness T (nm) of the primary particles are measured for 100 boron nitride particles. The arithmetic mean value of the obtained major axis D is the number-average particle size of the primary particles, and the arithmetic mean value of the ratio of the major axis D to the thickness T measured for each particle is D / T. The observation magnification is adjusted appropriately depending on the size of the fine particles.

[0072] (SEM observation conditions) Sample pretreatment: Toner is fixed to the tip of the conical sample stage with carbon tape and Pt coated. SEM acceleration voltage: 2.0 kV Working distance: 2.8 mm Detector: SE2 Sample tilt angle: -45 degrees to 45 degrees (to observe the thinnest part of the boron nitride particle) Magnification: 5,000 to 50,000 times

[0073] <X-ray diffraction analysis of boron nitride particles> In order to determine whether boron nitride is a hexagonal crystal, an X-ray diffraction analysis of boron nitride sampled from a toner by the method described below is used. The X-ray diffraction measurement is performed using a measuring device "RINT-TTRII" (manufactured by Rigaku Corporation) and the control software and analysis software that come with the device. The measurement conditions are as follows. X-ray:Cu / 50kV / 300mA Goniometer: Rotor horizontal goniometer (TTR-2) Attachment: Standard sample holder Divergence slit: open Divergence vertical limit slit: 10.00mm Scattering slit: open Receiving slit: open Counter: Scintillation counter Scanning mode: Continuous Scan speed: 4.0000° / min Sampling width: 0.0200° Scan axis: 2θ / deg Scanning range: 3.0000°~60.0000° The obtained spectrum is analyzed using software provided with the device, and if the peaks match those detected for boron nitride, which has a hexagonal crystal structure, the crystal structure is determined to be hexagonal.

[0074] <How to check for the presence of carbon black in toner particles> The presence or absence of carbon black in toner particles is determined by EDS mapping measurement of the toner particles using a scanning transmission electron microscope (STEM). In EDS mapping measurement, spectrum data is obtained for each pixel in the analysis area. By using a silicon drift detector with a large detection element area, EDS mapping can be measured with high sensitivity. By performing statistical analysis on the spectral data for each pixel obtained by EDS mapping measurement, it is possible to obtain a principal component mapping that extracts pixels with similar spectra, making it possible to map specific components.

[0075] The observation sample is prepared according to the following procedure. 0.5 g of the toner particles isolated from the toner by the above-mentioned method is weighed out, and placed in a cylindrical mold with a diameter of 8 mm and left to stand for 2 minutes under a load of 40 kN using a Newton press to prepare a cylindrical toner pellet with a diameter of 8 mm and a thickness of approximately 1 mm. A thin section with a thickness of 200 nm is prepared from the toner pellet using an ultramicrotome (Leica, FC7).

[0076] The STEM-EDS analysis is carried out using the following equipment and conditions. Scanning transmission electron microscope: JEM-2800 manufactured by JEOL Ltd. EDS detector: JED-2300T Dry SD100GV detector (detector area: 100 mm 2 ) EDS analyzer: NORAN, manufactured by Thermo Fisher Scientific System 7

[0077] [Conditions for STEM-EDS] STEM accelerating voltage: 200kV ·Magnification: 20,000x Probe size 1nm STEM image size: 1024 x 1024 pixels (EDS element mapping images are acquired at the same position.) EDS mapping size: 256 x 256 pixels, Dwell Time: 30 μs, Integration count: 100 frames

[0078] The carbon black in the toner particles is identified based on the multivariate analysis as follows. The EDS mapping is obtained by the STEM-EDS analysis device. Next, the collected spectral mapping data is subjected to multivariate analysis using the COMPASS (PCA) mode in the measurement command of the NORAN System 7 described above, and a principal component map image is extracted. In this case, the setting values ​​are as follows: Kernel size: 3×3 Quantitative map setting: High (slow) Filter Fit Type: High Precision (Slow)

[0079] At the same time, this operation calculates the area ratio of each extracted principal component in the EDS measurement field of view. Quantitative analysis is performed on the EDS spectrum of each obtained principal component mapping by the Cliff-Lorimer method. The binder resin portion of the toner particles and the carbon black particles are distinguished from each other based on the above-mentioned quantitative analysis results of the obtained STEM-EDS main component mapping.

[0080] <Method for measuring the carbon black content c0 (mass%) in toner particles> The amount of carbon black in the toner particles is quantified by thermogravimetric analysis (TGA) using the toner particles. Specifically, in the first step, the temperature is raised to 550°C at 10°C / min in a nitrogen atmosphere and held for 10 minutes to decompose the resin components. In the second step, the temperature is cooled to 400°C at 10°C / min, and then air is introduced and the temperature is raised to 800°C at 10°C / min to decompose the carbon black. The carbon black content ratio c0 in the toner particles is calculated from the ratio of the mass loss in the first step to that in the second step.

[0081] <Identification and quantification of binder resin> A pyrolysis gas chromatography mass spectrometer (hereinafter also referred to as "pyrolysis GC / MS") and NMR are used to identify the type and ratio of monomer units in the binder resin. Pyrolysis GC / MS is used to analyze the types of constituent compounds of the resin. The type of monomer unit is identified by analyzing the mass spectrum of the components of the resin decomposition products generated when the resin is pyrolyzed at 550°C to 700°C. The specific measurement conditions are as follows:

[0082] (Measurement conditions for pyrolysis GC / MS) Pyrolysis device: JPS-700 (Japan Analysis Industry) Decomposition temperature: 590℃ GC / MS equipment: Focus GC / ISQ (Thermo Fisher) Column: HP-5MS, length 60 m, inner diameter 0.25 mm, film thickness 0.25 μm Inlet temperature: 200℃ Flow pressure: 100kPa Split: 50mL / min MS ionization: EI Ion source temperature: 200℃ Mass Range 45-650 Next, the ratio of the monomer units of the identified binder resin is 1 The structure was determined using a FT-NMR apparatus JNM-EX400 (manufactured by JEOL Ltd.) 1 H-NMR 400 MHz, CDCl3, room temperature (25 °C)].

[0083] ( 1 H-NMR measurement conditions) Measurement frequency: 400MHz Pulse condition: 5.0μs Frequency range: 10500Hz Number of times of accumulation: 1024 times Measurement temperature: 25℃ Sample: 50 mg of the measurement sample is placed in a sample tube with an inner diameter of 5 mm, deuterated chloroform (CDCl3) is added as a solvent, and this is dissolved in a thermostatic bath at 40°C to prepare the sample. The molar ratio of each monomer unit is determined from the integral value of the obtained spectrum, and the ratio (mass %) of each monomer unit is calculated based on this.

[0084] <Method of measuring peak top molecular weight (Mp)> The peak top molecular weight (Mp) of the polyester resin is measured by gel permeation chromatography (GPC) as follows. First, the sample to be measured is dissolved in tetrahydrofuran (THF) at room temperature. If it is difficult to dissolve, heat it to a temperature of 35°C or less. The obtained solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: High-speed GPC equipment "HLC-8220GPC" [Tosoh Corporation] Column: 2 columns of LF-604 [Showa Denko Co., Ltd.] Eluent:THF Flow rate: 0.6mL / min Oven temperature: 40℃ Sample injection volume: 0.020mL The molecular weight of the sample was calculated using standard polystyrene resin (product name "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40 A molecular weight calibration curve prepared using "A-5000, A-2500, A-1000, A-500" (manufactured by Tosoh Corporation) is used.

[0085] <Method for measuring average circularity> The average circularity of the toner and toner particles is measured and analyzed under the following conditions using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation). The specific measurement method is as follows. First, 20 mL of ion-exchanged water from which solids and other impurities have been removed is placed in a glass container. 0.2 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant. 0.02 g of the measurement sample is then added, and the dispersion is processed for 2 minutes using an ultrasonic disperser to obtain a dispersion for measurement. At this time, the dispersion is appropriately cooled so that the temperature of the dispersion is between 10 and 40°C. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser ("VS-150" (manufactured by Velvoclear)) with an oscillation frequency of 50 kHz and an electrical output of 150 W was used. A predetermined amount of ion-exchanged water was placed in the water tank, and approximately 2 mL of the Contaminon N was added to the water tank. For the measurement, the flow type particle image analyzer equipped with "UPlanApro" (magnification 10x, numerical aperture 0.40) as the objective lens is used, and particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid.

[0086] The dispersion liquid prepared according to the above procedure is introduced into the flow type particle image analyzer, and 3000 toner particles are measured in HPF measurement mode and total count mode.Then, the binarization threshold during particle analysis is set to 85%, and the analyzed particle diameter is limited to a circle equivalent diameter of 1.985 μm or more and less than 39.69 μm, and the average circularity of the toner particles is obtained. Before starting the measurement, automatic focus adjustment is performed using standard latex particles (Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water).

[0087] <Method of measuring weight average particle size (D4)> The weight average particle diameter (D4) of the toner or toner particles (hereinafter, also referred to as toner, etc.) is calculated as follows. The measurement device used was a 100 μm aperture tube equipped with a small hole electrical resistance method. A precision particle size distribution measuring device "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.) is used. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000 channels. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1.0%, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter, Inc.). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0088] The specific measurement method is as follows. (1) Pour 200.0 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "Aperture tube flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Place 30.0 mL of the electrolyte solution in a 100 mL flat-bottom glass beaker. Add 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees and an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank and add 2.0 mL of Contaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is being irradiated with ultrasonic waves, 10 mg of toner or the like is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted so that it is between 10°C and 40°C. (6) Using a pipette, drip the electrolytic solution (5) in which the toner or the like has been dispersed into the round-bottom beaker (1) placed in the sample stand to adjust the measurement concentration to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) Analyze the measurement data using the dedicated software that comes with the device to calculate the weight-average particle size (D4). Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4). EXAMPLES

[0089] The present disclosure will be specifically described with reference to the following examples. However, these are not intended to limit the present disclosure in any way. Unless otherwise specified, "parts" and "%" are all by mass.

[0090] [Production example of polyester resin] <Polyester resin 1> Fumaric acid: 10.6 parts (23 mol%) Terephthalic acid: 8.5 parts (13 mol%) Trimellitic acid: 3.3 parts (4 mol%) Bisphenol A-ethylene oxide 2-mol adduct: 47.6 parts (38 mol%) Bisphenol A-propylene oxide 2-mol adduct: 30.0 parts (22 mol%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted for 1 hour under reduced pressure of 60 to 70 mmHg to obtain amorphous polyester resin 1. In this specification, the reaction rate refers to the value of the amount of reaction water produced (mol) / theoretical amount of water produced (mol)×100. The resulting polyester resin 1 had an acid value of 20.3 mgKOH / g, a peak top molecular weight (Mp) of 6000, and a glass transition temperature of 54.6°C.

[0091] <Polyester resin 2> Terephthalic acid: 22.6 parts (36 mol%) Trimellitic acid: 3.2 parts (4 mol%) Bisphenol A-ethylene oxide 2-mol adduct: 45.5 parts (38 mol%) Bisphenol A-propylene oxide 2-mol adduct: 28.7 parts (22 mol%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted for 1 hour under a reduced pressure of 60 to 70 mmHg to obtain amorphous polyester resin 2. The resulting polyester resin 1 had an acid value of 20.1 mgKOH / g, a peak top molecular weight (Mp) of 6000, and a glass transition temperature of 59.4°C.

[0092] <Polyester resin 3> Amorphous polyester resin 3 was obtained in the same manner as in Production Example of Polyester Resin 1, except that the reaction was continued until the peak top molecular weight reached 12,000. The resulting polyester resin 3 had an acid value of 12.2 mgKOH / g, a peak top molecular weight (Mp) of 12,000, and a glass transition temperature of 55.2°C.

[0093] [Example of resin particle dispersion production] <Resin particle dispersion 1> 1,200 parts polyester resin -Ion-exchanged water 500 parts Fumaric acid 0.250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise, and emulsified and dispersed while stirring at 7800 rpm to obtain resin particle dispersion 1. The solid content concentration of resin particle dispersion 1 was 20%. The particle size distribution of the polyester resin 1 particles contained in the resin particle dispersion 1 was measured using a particle size measuring device ( When measured using HORIBA, Ltd.'s LA-960V2), the number average particle size of the particles of polyester resin 1 was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0094] <Resin particle dispersion 2~13> Resin particle dispersions 2 to 13 were produced in the same manner as in the production example of resin particle dispersion 1, except that the resin used and the amount of fumaric acid added were changed to those shown in Table 1. However, in resin particle dispersion 11, fumaric acid was not added, and maleic acid was added in the amount shown in Table 1. In any case, coarse particles exceeding 1 μm were not observed. The number average particle size of the polyester resin particles in resin particle dispersions 2 to 13 is also shown in Table 1.

[0095] <Resin particle dispersion 14> A resin particle dispersion 14 in which the vinyl resin 1 was dispersed was produced by the emulsion aggregation method as described below. 78.0 parts of styrene and 22.0 parts of butyl acrylate were placed in a stainless steel container and mixed. An aqueous solution of 4.0 parts of sodium dodecylbenzenesulfonate mixed with 150 parts of ion-exchanged water was added to this solution and dispersed. An aqueous solution of 0.3 parts of potassium persulfate mixed with 10 parts of ion-exchanged water was added while slowly stirring for 10 minutes. After the stainless steel container was replaced with nitrogen, emulsion polymerization was performed at 70°C for 6 hours. After the polymerization was completed, the reaction solution was cooled to room temperature and ion-exchanged water was added to adjust the solid content concentration to 20.0% by mass. The particle size distribution of resin particle dispersion 14 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the particles of vinyl resin 1 was 0.25 μm, and no coarse particles exceeding 1 μm were observed. When vinyl resin 1 was separated from resin particle dispersion 14 and each physical property of vinyl resin 1 was measured, the acid value was 0.0 (mgKOH / g), the weight average molecular weight was 35,000, and the glass transition temperature was 54.0° C. [Table 1] In the table, (maleic acid) indicates that no fumaric acid was added, but maleic acid was added in the amount shown in the table.

[0096] [Example of wax particle dispersion production] <Wax particle dispersion 1> -Ion-exchanged water 500 parts Wax (FNP0090 (manufactured by Nippon Seiro Co., Ltd.): Fischer-Tropsch process hydrocarbon wax, melting point 90°C, molecular weight 771) 200 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath and melted, and 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. Thereafter, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 295 parts of ion-exchanged water was gradually added dropwise, and emulsified and dispersed while stirring at 7800 rpm to obtain wax particle dispersion 1. The solids concentration of wax particle dispersion 1 was 20%. The particle size distribution of the wax particles contained in the wax particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the wax particles was 0.35 μm, and no coarse particles exceeding 1 μm were observed. The melting point was 90° C. and the molecular weight was 771.

[0097] <Production Example of Colorant Particle Dispersion 1> Carbon black (Nipex35: Orion Engineered Carbons) 100 parts Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above materials were mixed and dispersed using a sand grinder mill to obtain a colorant particle dispersion. The solid content concentration of colorant particle dispersion 1 was 20%. When the particle size distribution of the colorant particles contained in this colorant particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0098] <Production Examples of Colorant Dispersions 2 to 4> Colorant dispersion liquid 1 was produced in the same manner as in the production example of colorant dispersion liquid 1, except that the pigment used was changed as shown in Table 2. [Table 2]

[0099] [Toner particle manufacturing example] <Toner particle 1> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 1 35 parts Wax particle dispersion 1 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion 1, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion 1 was uniformly mixed in a 500 mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was dropped into the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation in a 10 L pressure filter under a pressure of 0.4 MPa to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 1 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.96.

[0100] <Toner particles 2-17, 19-21> Toner particles 2 to 17 and 19 to 21 were produced in the same manner as in the production example of toner particle 1, except that the resin particle dispersion and colorant particle dispersion used in the production example of toner particle 1 were changed to those shown in Table 3, the amount of colorant dispersion was changed so that the colorant content ratio became the value shown in Table 3, and the heating temperature holding time during fused particle formation was changed.

[0101] <Production Example of Polyester Resin A> Fumaric acid: 10.6 parts (23 mol%) Terephthalic acid: 8.5 parts (13 mol%) Trimellitic acid: 3.3 parts (4 mol%) Bisphenol A-ethylene oxide 2-mol adduct: 47.6 parts (38 mol%) Bisphenol A-propylene oxide 2-mol adduct: 30.0 parts (22 mol%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted for 1 hour under reduced pressure of 60 to 70 mmHg to obtain an amorphous polyester resin A. In this specification, the reaction rate refers to the value of the amount of reaction water produced (mol) / theoretical amount of water produced (mol)×100.

[0102] <Production Example of Toner Particle 18> Polyester resin A 100 parts Fumaric acid 0.025 parts Carbon black (Nipex35: Orion Engineered Carbons) 5 parts Wax (behenyl behenate, melting point 73°C) 1 part The above materials were premixed in an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.), and then melt-kneaded using a twin-screw kneading extruder (manufactured by Ikegai Iron Works Co., Ltd., PCM-30 type). The resulting kneaded material was cooled, coarsely pulverized using a hammer mill, and then pulverized using a mechanical pulverizer (manufactured by Turbo Kogyo Co., Ltd., T-250). The resulting finely pulverized powder was classified using a multi-division classifier utilizing the Coanda effect, and toner particles 18 with a weight-average particle size (D4) of 6.9 μm and an average circularity of 0.935 were obtained. [Table 3] In the table, the unit of the colorant content is parts, and the elevated temperature holding time indicates the holding time at 90° C. when forming fused particles.

[0103] <Example of manufacturing boron nitride particles> Boric acid, borate salts, or molten boric anhydride are used as raw materials, and are reduced and nitridized by reacting with ammonia in a synthesis furnace, followed by purification and crystallization to obtain boron nitride particles. Various boron nitride particles were prepared by adjusting the mixture ratio of boric acid and ammonia, catalyst type, reaction temperature, and reaction time. Table 4 shows the number average particle size of the primary particles of each boron nitride particle, and the ratio D / T of the major axis D (nm) to the thickness T (nm) of each particle. [Table 4]

[0104] <Toner manufacturing example> <Toner 1> Toner particles 1 100.0 parts Boron nitride particles 1 0.2 parts Silica particles (RX200: primary average particle size 12 nm, HMDS treatment, Nippon Aerosil Co., Ltd.) 1.5 parts The above materials were mixed by external addition using FM10C (manufactured by Nippon Coke & Engineering Co., Ltd.). The external addition conditions were as follows: the lower blade was set to A0 blade, the distance to the deflector wall was set to 20 mm, the amount of toner particles charged was 2.0 kg, and the rotation speed was 66.6 s. -1The external addition was performed for 10 minutes with cooling water at a temperature of 20° C. and a flow rate of 10 L / min. Thereafter, the mixture was sieved through a mesh having an opening of 37 μm to obtain Toner 1. The physical properties of Toner 1 thus obtained are shown in Table 6.

[0105] <Toner 2-33> Toners 2 to 33 were produced in the same manner as in Production Example of Toner 1, except that in Production Example of Toner 1, the toner particles and boron nitride particles were changed to those shown in Table 5, and the amount of boron nitride particles was changed as shown in Table 5. The physical properties of the obtained Toners 2 to 33 are shown in Table 6. [Table 5] [Table 6] In the table, f0 indicates the fumaric acid content (mass %) in the toner, a0 indicates the boron nitride particle content (mass %) in the toner, f1 indicates the fumaric acid content (mass %) in the toner that is extracted from the toner by methanol, c0 indicates the carbon black content (mass %) in the toner particles, PES contained indicates the presence or absence of polyester resin in the toner particles, Y indicates that the toner particles contain polyester resin, and N indicates that the toner particles do not contain polyester resin.

[0106] [Examples 1 to 29, Comparative Examples 1 to 4] The following evaluations were carried out using the above toners 1 to 33. The evaluation results are shown in Table 7.

[0107] The evaluation methods and evaluation criteria of the present disclosure are described below. A modified Canon LBP9950Ci laser beam printer was used. The modifications were to change the gear and software of the evaluation machine to set the rotation speed of the developing roller to twice the peripheral speed of the drum, and to change the process speed to 330 mm / sec. The toner in the toner cartridge of the LBP9950Ci was removed, the inside was cleaned with an air blower, and then 210 g of the toner to be evaluated was loaded. The toner cartridge was then left in a high temperature and high humidity H / H (32.5°C / 80%RH) environment for 5 days. The toner cartridge after being left in the high temperature and high humidity H / H environment for 5 days was attached to the cyan station of the LBP9950Ci, and 30,000 sheets of images with a print ratio of 1.0% were printed out. The development streaks and image density uniformity were checked at the initial stage and after 30,000 sheets were printed (after durability). The fertility (H / H) was evaluated.

[0108] Evaluation of streaks caused by development in H / H environment After printing 30,000 sheets, one halftone image was printed out. The printed halftone image was evaluated according to the following criteria. C or above was judged as good. [Evaluation Criteria] A: There are 0 to 1 streaks on the halftone image. B: There are 2 to 4 streaks on the halftone image. C: There are 5 to 9 streaks on the halftone image. D: There are 10 or more streaks on the halftone image.

[0109] <Initial fogging evaluation after 2 days of exposure to H / H environment (initial fogging during HH durability)> The fog was measured using a REFLECTMETER MODEL TC-6DS manufactured by Tokyo Denshoku Co., Ltd. A green filter was used. After printing 30,000 sheets as described above, the printer was turned off and left for two days. Then, one solid white image was printed. The solid white image was taped on the drum before transfer with Mylar tape, and the Macbeth density of the Mylar tape on unused paper was subtracted from the reflectance of the Mylar tape on the paper to determine the fog on the drum after white. A grade of C or above was judged to be good. Fog (reflectance) (%) = reflectance on standard paper (%) - reflectance of non-image area of ​​sample (%) [Evaluation Criteria] A: Less than 5.0% B: 5.0% or more and less than 10.0% C: 10.0% or more and less than 20.0% D: 20.0% or more

[0110] (Durable image density uniformity in H / H environment) For the evaluation of image density uniformity, rough paper FOX RIVER BOND paper (110 g / m 2 After printing 30,000 sheets as described above, an image was output having 5 mm x 5 mm solid black patch images in a total of nine locations, three at the left, right, and center, with a 5 mm leading margin and 5 mm left and right margins, and three more at 30 mm intervals in the longitudinal direction. The image density of the nine solid black patch images was measured, and the difference between the maximum and minimum image density values ​​was determined for the nine solid black patch images. Image density was measured using a Macbeth densitometer (manufactured by Macbeth) which is a reflection densitometer, using an SPI filter. The smaller the difference between the maximum and minimum values, the better the image density uniformity. A grade of B or higher was judged to be good. [Evaluation Criteria] A: The difference between the maximum and minimum image density values ​​is 0.05 or less. B: The difference between the maximum and minimum image density values ​​is 0.06 or more and 0.10 or less. C: The difference between the maximum and minimum image density values ​​is 0.11 or more.

[0111] <Evaluation of dot reproducibility> For the evaluation of dot reproducibility, high white paper GF-C081 (81.4 g / m 2 A printer (Canon Marketing Japan Inc.) was used. After printing 30,000 sheets as described above, one halftone (30H) image was formed, and the dot reproducibility of this image was evaluated based on the following criteria. A 30H image is a halftone image in which 256 gradations are expressed in hexadecimal, with 00H being solid white (non-image) and FFH being a solid image (full image). The obtained halftone image was measured using a digital microscope VHX-500 (lens wide range zoom lens VH-Z100 manufactured by Keyence Corporation) at a resolution of 1000 dots. The area of ​​each was measured. The number average of dot area (S) and the standard deviation of dot area (σ) were calculated, and the dot reproducibility index (I) was calculated using the following formula. The dot reproducibility of the halftone image was evaluated using the dot reproducibility index (I). The smaller the value of the dot reproducibility index (I), the better the dot reproducibility. Dot reproducibility index (I) = σ / S × 100 Ranks A to C were judged to be good dot reproducibility. [Evaluation Criteria] A:I is less than 3.0 B: I is 3.0 or more and less than 5.0 C:I is 5.0 or more and less than 8.0 D:I is 8.0 or higher

[0112] Contamination of electrostatically charged parts in an L / L environment The image forming apparatus was left in a low temperature and low humidity environment (15°C / 10% RH, hereinafter also referred to as L / L environment) for 24 hours. After that, in the L / L environment, Canon color laser copier paper (A4: 81.4 g / m 2 ), a horizontal line image with a print rate of 1% was printed on 30,000 sheets in succession. Then, Canon Color Laser Copier Paper (A4: 81.4 g / m 2 ) with a toner load of 0.20 g / cm 2 After that, the cartridge was disassembled and the surface of the charging roller (charging member) was observed. [Evaluation Criteria] A: No streaks are visible on the charged member. B: Slight streaks are visible on the charged member, but no streaks are visible on the image. C: Streaks are visible on the charged member, and slight streaks are also visible on the image. D: Streaks are clearly visible on the image. [Table 7]

[0113] The present disclosure relates to the following configurations. (Configuration 1) A toner having toner particles containing a binder resin and a colorant, and an external additive, The colorant contains carbon black, the external additive comprises boron nitride particles; The toner contains fumaric acid, The toner is characterized in that, when the content of the boron nitride particles in the toner is a0 (mass%) and the content of the fumaric acid in the toner is f0 (mass%), f0 / a0 is 0.050 to 5.000. (Configuration 2) 2. The toner according to claim 1, wherein a0 is 0.010 to 1.000 mass %. (Configuration 3) 3. The toner according to configuration 1 or 2, wherein f0 is 0.001 to 0.120% by mass. (Configuration 4) The toner according to configuration 3, wherein f0 is 0.010 to 0.120% by mass. (Configuration 5) When the content ratio of the carbon black in the toner particles is c0 (mass%), The toner according to any one of configurations 1 to 4, wherein c0 / f0 is 15 to 1,200. (Configuration 6) The toner according to configuration 5, wherein the c0 / f0 is 50 to 600. (Configuration 7) The toner according to any one of configurations 1 to 6, wherein c0 / a0 is from 2 to 800, where c0 (mass %) is the content of the carbon black in the toner particles. (Configuration 8) 8. The toner according to claim 7, wherein c0 / a0 is 30 to 500. (Configuration 9) 9. The toner according to any one of configurations 1 to 8, wherein the number average particle size of the primary particles of the boron nitride particles is 300 to 2000 nm. (Configuration 10) The boron nitride particles are flat particles, 10. The toner according to any one of configurations 1 to 9, wherein D / T is 6 to 20, where D (nm) is the major axis of the boron nitride particles and T (nm) is the thickness of the boron nitride particles. (Configuration 11) 11. The toner according to any one of configurations 1 to 10, wherein the toner has an average circularity of 0.940 to 0.980. (Configuration 12) 12. The toner according to any one of configurations 1 to 11, wherein the binder resin contains a polyester resin. (Configuration 13) 13. The toner according to embodiment 12, wherein the polyester resin has a peak top molecular weight (Mp) of 5,000 to 10,000. (Configuration 14) 14. The toner according to any one of configurations 1 to 13, wherein when a content of fumaric acid in the toner that is extracted from the toner with methanol is defined as f1 (mass %), f1 is 0.0010 to 0.0100 mass %. (Configuration 15) 15. The toner according to any one of configurations 1 to 14, wherein, in cross-sectional observation of the toner with a scanning transmission electron microscope (STEM), the carbon black is present in a region at a depth of 100 nm from the toner surface.

Claims

1. A toner having toner particles containing a binder resin and a colorant, and an external additive, The colorant contains carbon black, the external additive comprises boron nitride particles; The toner contains fumaric acid, The toner is characterized in that, when a0 (mass%) is a content ratio of the boron nitride particles in the toner, and f0 (mass%) is a content ratio of the fumaric acid in the toner, f0 / a0 is 0.050 to 5.

000.

2. 2. The toner according to claim 1, wherein a0 is 0.010 to 1.000% by mass.

3. 3. The toner according to claim 1, wherein the f0 is from 0.001 to 0.120% by mass.

4. The toner according to claim 3, wherein the f0 is 0.010 to 0.120% by mass.

5. When the content ratio of the carbon black in the toner particles is c0 (mass%), 3. The toner according to claim 1, wherein c0 / f0 is from 15 to 1,200.

6. 6. The toner according to claim 5, wherein the c0 / f0 is from 50 to 600.

7. 3. The toner according to claim 1, wherein when a content ratio of the carbon black in the toner particles is c0 (mass %), c0 / a0 is from 2 to 800.

8. 8. The toner according to claim 7, wherein the c0 / a0 is 30 to 500.

9. 3. The toner according to claim 1, wherein the number average particle size of the primary particles of the boron nitride particles is 300 to 2000 nm.

10. The boron nitride particles are flat particles, 3. The toner according to claim 1, wherein the boron nitride particles have a major axis D (nm) and a thickness T (nm), and the ratio D / T is from 6 to 20.

11. 3. The toner according to claim 1, wherein the toner has an average circularity of 0.940 to 0.

980.

12. The toner according to claim 1 or 2, wherein the binder resin contains a polyester resin.

13. 13. The toner according to claim 12, wherein the polyester resin has a peak top molecular weight (Mp) of 5,000 to 10,000.

14. 3. The toner according to claim 1, wherein when a content of fumaric acid in the toner that is extracted with methanol is defined as f1 (mass %), f1 is 0.0010 to 0.0100 mass %.

15. 3. The toner according to claim 1, wherein, in cross-sectional observation of the toner with a scanning transmission electron microscope (STEM), the carbon black is present in a region at a depth of 100 nm from the toner surface.

Citation Information

Patent Citations

  • Toner for electrostatic latent image development and image forming method

    JP2011128406A

  • Image forming apparatus, image forming method, and process cartridge

    JP2012103493A

  • toner

    JP2015125413A