Toner

The toner formulation with strontium titanate particles and fumaric acid addresses charging performance and contamination issues across diverse environments, enhancing image stability and longevity.

JP2024160831APending Publication Date: 2024-11-15CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023076244
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing toners face issues with charging performance in varying environments, particularly in low temperature and low humidity conditions leading to contamination of charging members and image quality problems, while toners with strontium titanate particles suffer from long-term durability issues in high temperature and high humidity environments.

Method used

A toner formulation containing strontium titanate particles with fatty acids on their surface and fumaric acid within specific content ratios, which helps in maintaining uniform charge distribution and reducing contamination of charging members across different environmental conditions.

Benefits of technology

The toner achieves improved charging performance in high temperature and high humidity environments and suppresses contamination of charging members in low temperature and low humidity environments, ensuring stable image density and reduced streaking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160831000001
    Figure 2024160831000001
  • Figure 2024160831000002
    Figure 2024160831000002
  • Figure 2024160831000003
    Figure 2024160831000003
Patent Text Reader

Abstract

To provide a toner that can achieve both electrification characteristics when used for a long period in a high temperature and high humidity environment and prevention of contamination of a charging member when used for a long period in a low temperature and low humidity environment.SOLUTION: A toner has toner particles containing a binder resin, and an external additive. The external additive includes strontium titanate particles. The strontium titanate particles have fatty acid in a surface of each of the strontium titanate particles. The toner contains fumaric acid. When the content ratio of the fumaric acid in the toner is defined as f0 (mass%), the f0 is 0.010-0.120 mass%. When the content ratio of the fumaric acid extracted from the toner by using methanol is defined as f1 (mass%), the f1 is 0.0010-0.0100 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners for use in recording methods utilizing electrophotography, electrostatic recording, and toner jet recording. [Background technology]

[0002] In electrophotographic image forming apparatuses, there is a demand for higher speeds and longer life. In addition, as the environments in which they are used are becoming more diverse, there is a demand for them to be able to achieve higher speeds and longer life in a wide range of environments, from high-temperature, high-humidity environments to low-temperature, low-humidity environments. To this end, there is a demand for toners to have even greater improvements in various performances. Specifically, the toner's chargeability can be mentioned. By improving the toner's chargeability, the toner can be sufficiently charged even in a faster development process, which contributes to increasing the speed of an electrophotographic image forming apparatus. In addition, the toner's chargeability can be easily maintained even after long-term use, which also contributes to a longer life.

[0003] As a means for increasing the chargeability of a toner, a method of externally adding strontium titanate particles to toner particles has been proposed (Patent Document 1). On the other hand, Patent Document 2 discloses a toner in which the content of a monomer having a carboxylic acid group in the toner is specified in order to improve the low-temperature fixing property, heat-resistant storage property, charge stability (charge rise property), and contamination resistance of the toner and to suppress the occurrence of toner scattering inside the machine and background scumming. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-045578 A [Patent Document 2] JP 2016-173396 A Summary of the Invention [Problem to be solved by the invention]

[0005] As a result of the inventors' investigation, it was confirmed that the toner described in Patent Document 1 has a certain effect of improving the charging property by adding externally added strontium titanate particles. Specifically, the effect of suppressing the occurrence of fogging when restarting after being left for several days after continuous use in a high-temperature, high-humidity environment was observed. However, the inventors have realized that there is a problem with long-term durability. In particular, when used for a long time in a low-temperature, low-humidity environment, charging members such as charging rollers are contaminated with strontium titanate particles, and streaky image defects may occur when halftone images are output. In addition, the toner described in Patent Document 2 does not contain strontium titanate particles, and therefore has insufficient charging properties. As a result, it has been found that there are problems such as a decrease in image density after continuous use in a high-temperature, high-humidity environment, and fogging when restarting the device after leaving it for several days after continuous use in a high-temperature, high-humidity environment.

[0006] The present disclosure provides a toner that solves the above problems. Specifically, the present disclosure provides a toner that improves the chargeability of the toner and the contamination resistance of a charging member, and that can achieve both good chargeability when used for a long period of time in a high-temperature, high-humidity environment and suppression of contamination of the charging member when used for a long period of time in a low-temperature, low-humidity environment. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors have focused on the chargeability of the toner and the contamination resistance of the charging member. As a result, it was found that a toner containing fumaric acid and strontium titanate particles having fatty acids on the surface thereof can achieve both good chargeability when used for a long period of time in a high-temperature, high-humidity environment and suppression of contamination of the charging member when used for a long period of time in a low-temperature, low-humidity environment.

[0008] That is, the present disclosure: A toner having toner particles containing a binder resin and an external additive, the external additive comprises strontium titanate particles; the strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles, The toner contains fumaric acid, When the content of the fumaric acid in the toner is f0 (mass%), the f0 is 0.010 to 0.120 mass%, When the content of fumaric acid in the toner that is extracted with methanol is defined as f1 (mass %), the toner has a content of f1 of 0.0010 to 0.0100 mass %. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a toner that can achieve both good chargeability when used for a long period of time in a high-temperature, high-humidity environment and suppression of contamination of the charging member when used for a long period of time in a low-temperature, low-humidity environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. The term "monomer unit" refers to the reacted form of a monomer substance in a polymer. For example, one section of carbon-carbon bond in the main chain of a polymer in which a polymerizable monomer is polymerized is considered to be one unit. The polymerizable monomer can be represented by the following formula (C). [ka]

[0011] In formula (C), R A represents a hydrogen atom or an alkyl group (preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group), R B represents an optional substituent.

[0012] The present disclosure provides a toner having toner particles containing a binder resin and an external additive, the external additive comprises strontium titanate particles; the strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles, The toner contains fumaric acid, When the content of the fumaric acid in the toner is f0 (mass%), the f0 is 0.010 to 0.120 mass%, Regarding the toner, when the content of fumaric acid in the toner, which is extracted from the toner by methanol, is f1 (mass %), the f1 is 0.0010 to 0.0100 mass %. do.

[0013] As described above, adding strontium titanate particles to toner particles is an effective means for improving the chargeability of toner. However, when the toner is used for a long time in a low-temperature and low-humidity environment, the strontium titanate particles contaminate the charging member. The present inventors conducted detailed studies on why strontium titanate particles are prone to contaminating charging members. As a result, they discovered the following. That is, when used for a long time in a low-temperature, low-humidity environment, some of the strontium titanate particles become excessively charged particles, and the electrostatic adhesion force with the photoconductor becomes too strong. As a result, the strontium titanate particles cannot be cleaned in the cleaning process, and the charging member is contaminated.

[0014] The reason why the toner is charged by the strontium titanate particles is believed to be that the toner particles are given a negative charge due to the peeling charge with the toner surface. At this time, a positive charge is given to the strontium titanate particles. The amount of charge of the peeling charge varies depending on the composition of the peeling surface and the contact state, so the amount of charge of the strontium titanate particles after peeling varies to a certain extent from particle to particle. As a result, a certain number of strontium titanate particles with a very high amount of charge are produced. Furthermore, particularly in a low-temperature, low-humidity environment, the amount of moisture in the air is small, so the charge generated in the strontium titanate particles by the peeling charge with the toner particles is easily retained. Therefore, when used for a long time in a low-temperature, low-humidity environment, the toner is stirred in the developing device, or rubbed against the developing blade, developing roller, photoconductor, etc., so that the charge is excessively accumulated in the strontium titanate particles. It is believed that the contamination of the charging member occurs due to the excessively charged strontium titanate particles generated in this way.

[0015] The reason why the toner of the present disclosure is able to achieve both good chargeability when used for a long period of time in a high-temperature, high-humidity environment and suppression of contamination of the charging member when used for a long period of time in a low-temperature, low-humidity environment is not entirely clear, but the inventors speculate as follows.

[0016] The toner of the present disclosure has an external additive, and the external additive contains strontium titanate particles, so that the charging property is improved. Furthermore, in the toner of the present disclosure, the strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles. In addition, the content ratio of fumaric acid in the toner is within a predetermined range. Furthermore, the content ratio of fumaric acid extracted from the toner by methanol in the toner is within a predetermined range. As a result, excessive charging of the strontium titanate particles is suppressed, and the electrostatic adhesion force between the photoconductor and the strontium titanate particles is suppressed. For this reason, it is considered that the cleaning property in the cleaning process is improved, and the contamination of the charging member is suppressed.

[0017] It is speculated that the reason why excessive charging of strontium titanate particles is suppressed is that charge uniformization occurs between strontium titanate particles via fatty acid and fumaric acid. Since fumaric acid is a compound with unsaturated bonds and a wide conjugated system, it is thought that it is easy to give and receive electrons with other compounds via the π electrons of the conjugated system. In addition, when excessively charged strontium titanate particles and strontium titanate particles with a small amount of charge coexist, a potential difference occurs between the strontium titanate particles. In this case, it is thought that the presence of fumaric acid between these strontium titanate particles causes charge exchange by the π electrons of fumaric acid, resulting in charge uniformization between the strontium titanate particles. Such charge uniformization occurs when the content of fumaric acid extracted from the toner by methanol is within a predetermined range in the toner, that is, when fumaric acid is present near the surface of the toner. Its presence makes it more likely to occur. In addition, the fatty acid present on the surface of the strontium titanate particles is a carboxylic acid compound having a carboxyl group, just like fumaric acid. Therefore, the fatty acid and fumaric acid interact with each other through hydrogen bonds. As a result, it is considered that the fatty acid and fumaric acid have high affinity and are compounds that easily approach each other. In addition, as described above, fumaric acid is present near the surface of the toner. Therefore, the strontium titanate particles having fatty acids on their surfaces are in close proximity to each other through the fumaric acid, and a network is formed between the strontium titanate particles, the fatty acid, and the fumaric acid. As a result, it is considered that the transfer of charges between the strontium titanate particles described above is promoted, and the contamination of the charging member is suppressed.

[0018] The present disclosure will now be described in detail. The toner has toner particles containing a binder resin and an external additive. The external additive contains strontium titanate particles. The strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles. The toner contains fumaric acid. When the content of fumaric acid in the toner is f0 (mass %), f0 is 0.010 to 0.120 mass %. When the content of fumaric acid in the toner extracted from the toner by methanol is f1 (mass %), f1 is 0.0010 to 0.0100 mass %.

[0019] As described above, the content ratio f0 of fumaric acid in the toner is 0.010 to 0.120% by mass. f0 indicates the content ratio of fumaric acid in the entire toner. By f0 being in the above range, the fumaric acid inside the toner gradually exudes to the surface of the toner, so that excessive charging of the strontium titanate particles can be suppressed through long-term use. When f0 is less than 0.010% by mass, the amount of fumaric acid in the entire toner is insufficient, so that the gradually released exudation of fumaric acid to the toner surface is insufficient, and excessively charged strontium titanate particles may be generated. As a result, contamination of the charging member in a low-temperature, low-humidity environment may not be sufficiently suppressed, and the in-plane uniformity of the halftone image may decrease. In addition, when f0 exceeds 0.120% by mass, the amount of fumaric acid in the entire toner is too large, so that the resistance of the toner decreases and the charge retention decreases. Therefore, the charging property in a high-temperature, high-humidity environment may be insufficient, and the image density may decrease and the fogging may not be sufficiently suppressed. f0 is preferably 0.050 to 0.110% by mass, and more preferably 0.050 to 0.100% by mass. Within this range, the fumaric acid is more suitably gradually released onto the toner surface, and contamination of the charging member in a low-temperature, low-humidity environment is more easily suppressed. In addition, the toner resistance is more suitable, and the charging property in a high-temperature, high-humidity environment is more improved. The method for measuring the content ratio f0 of fumaric acid in the toner will be described later. Measuring f0 by the method described later indicates that fumaric acid exists in a free state in the toner. The value of the content ratio f0 of fumaric acid in the toner can be adjusted by changing the amount of fumaric acid added during toner production.

[0020] As described above, the content ratio f1 of fumaric acid extracted from the toner by methanol is 0.0010 to 0.0100 mass%. Methanol hardly dissolves the binder resin in the toner particles, but can dissolve the fumaric acid contained in the surface vicinity of the toner. Therefore, f1 is an index of the content of fumaric acid contained in the surface vicinity of the toner. When f1 is in the above range, the amount of fumaric acid in the surface vicinity of the toner is sufficient, and excessive charging of the strontium titanate particles can be suppressed. When f1 is less than 0.0010 mass%, the amount of fumaric acid in the surface vicinity of the toner is insufficient, so that excessively charged strontium titanate particles are generated. As a result, contamination of the charging member may not be sufficiently suppressed. Also, when f1 exceeds 0.0100 mass%, the amount of fumaric acid in the surface vicinity of the toner is too large, so that the resistance of the toner surface decreases and the charge retention decreases. Therefore, the charging property in a high temperature and high humidity environment may be insufficient, and the image density may decrease, or the suppression of fogging may be insufficient. The controls may be insufficient. f1 is preferably 0.0030 to 0.0080 mass %, and more preferably 0.0040 to 0.0070 mass %. A method for measuring the content ratio f1 of fumaric acid extracted from the toner with methanol in the toner will be described later. The value of f1 can be adjusted by changing the amount of fumaric acid added during toner production or by providing a surface cleaning process in the toner particle production process.

[0021] The means for making the toner contain fumaric acid is not particularly limited, and known means can be used. For example, fumaric acid can be made to be contained in the toner particles. That is, it is preferable that the toner particles contain fumaric acid. Specifically, when producing toner particles by a pulverization method, a method can be used in which fumaric acid is incorporated into the raw material resin in advance, or a method can be used in which fumaric acid is added when the raw material is melted and kneaded so that it is incorporated into the toner particles. When toner particles are produced by a wet production method such as a suspension polymerization method or an emulsion aggregation method, a method of incorporating fumaric acid in the raw material or a method of adding fumaric acid via an aqueous medium during the production process can be used. Further, it is also possible to use a method of externally adding fumaric acid to toner particles by using a known external addition method.

[0022] When the content of strontium titanate particles in the toner is a0 (mass%), the a0 may be 0.010 to 8.000 mass%. Moreover, a0 is preferably 0.010 to 5.000 mass%, and more preferably 0.020 to 4.000 mass%. When a0 is in the above range, the content of strontium titanate particles in the toner becomes more appropriate, and it is possible to achieve both high levels of chargeability of the toner in a high-temperature and high-humidity environment and high levels of inhibition of contamination of the charging member in a low-temperature and low-humidity environment. a0 can be adjusted by changing the amount of strontium titanate particles added during toner production.

[0023] When the content ratio of the strontium titanate particles in the toner is a0 (mass%), f0 / a0 is preferably 0.002 to 12.000. When f0 / a0 is in this range, a network of strontium titanate, fatty acid, and fumaric acid is formed in a good state, and the chargeability of the toner in a high-temperature, high-humidity environment and the suppression of the contamination of the charging member in a low-temperature, low-humidity environment can be simultaneously achieved at a high level. f0 / a0 is more preferably 0.050 to 9.000, and even more preferably 0.100 to 5.000. When it is in this range, a network of strontium titanate, fatty acid, and fumaric acid is formed in a better state, and the chargeability of the toner in a high-temperature, high-humidity environment and the suppression of the contamination of the charging member in a low-temperature, low-humidity environment can be simultaneously achieved at a high level. f0 / a0 is calculated from the values ​​obtained by measuring f0 and a0 by the method described below.

[0024] Next, materials that can be used in the toner of the present disclosure will be described in detail below.

[0025] <Strontium titanate particles> The toner has an external additive. The external additive includes strontium titanate particles. The strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles. By including strontium titanate particles having fatty acids on the surfaces, the image density is stable even when the toner is used for a long time under a high temperature and high humidity environment, which is a more severe condition for the chargeability of the toner, and fogging is also suppressed after restarting the toner after being left for several days after long-term use. As described above, the strontium titanate particles have a surface By having a fatty acid on the surface, a network of strontium titanate, fatty acid, and fumaric acid can be formed. As a result, the charged state of the strontium titanate particles is made uniform, and excessive charging of the strontium titanate particles is suppressed. This action suppresses the electrostatic adhesion between the photoreceptor and the strontium titanate particles, and prevents contamination of the charging member in a low-temperature, low-humidity environment. Methods for providing fatty acids on the surfaces of strontium titanate particles include, for example, a wet method in which fatty acids are dissolved and dispersed in a solvent, strontium titanate particles are added thereto, and the solvent is removed while stirring, and a dry method in which fatty acids and strontium titanate particles are directly mixed and treated while stirring.

[0026] The structure of the fatty acid on the surface of strontium titanate is not particularly limited as long as it has a structure in which a hydrocarbon group (R-) and a carboxy group (-COOH) are bonded, and may be a saturated fatty acid or an unsaturated fatty acid, but is preferably a saturated fatty acid. The fatty acid may be linear or branched. From the viewpoint of controlling the hydrophobicity and steric hindrance of the fatty acid, the fatty acid preferably has 10 to 30 carbon atoms. Examples of the fatty acid include at least one selected from the group consisting of capric acid, undecylic acid, lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and montanic acid. At least one selected from the group consisting of lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid is preferable, and stearic acid is more preferable.

[0027] The fatty acid having 10 or more carbon atoms has sufficiently high hydrophobicity, which is preferable because it can improve the chargeability of the toner even when high-density images that consume a lot of toner are continuously output in a high-temperature and high-humidity environment with a high absolute moisture content. On the other hand, since the carbon number of the fatty acid is 30 or less, the steric hindrance of the fatty acid molecule is not too large. In this case, the fatty acid can approach the fumaric acid at a sufficient distance. Therefore, a network of strontium titanate, fatty acid, and fumaric acid can be effectively formed. As a result, excessive charging of the strontium titanate particles can be suppressed, and contamination of the charging member in a low-temperature and low-humidity environment can be suppressed, which is preferable. The number of carbon atoms of the fatty acid is more preferably from 12 to 28, and further preferably from 14 to 22. Within this range, the hydrophobicity and steric hindrance of the fatty acid are well balanced, and the chargeability of the toner in a high-temperature, high-humidity environment and the prevention of contamination of the charging member in a low-temperature, low-humidity environment can be achieved at a higher level. The number of carbon atoms of the fatty acid on the surface of the strontium titanate particles can be adjusted by changing the type of fatty acid used in the above-mentioned method of making the surface of the strontium titanate particles have fatty acids. Also, the type of fatty acid on the surface of the strontium titanate particles can be measured by the method described below. The measurement of fatty acid by the method described below indicates that the fatty acid is present in a free state.

[0028] The content of fatty acid on the surface of the strontium titanate particles is preferably 0.1 to 20.0 parts by mass, more preferably 0.5 to 10.0 parts by mass, even more preferably 0.5 to 5.0 parts by mass, and particularly preferably 0.5 to 2.0 parts by mass, per 100 parts by mass of the strontium titanate particles.

[0029] The number-average particle size of the primary particles of the strontium titanate particles is not particularly limited, but if the number-average particle size of the primary particles is 300 nm or less, the specific surface area becomes large, which increases the chance of peeling off and charging the toner. Therefore, it is preferable because it is easy to improve the charge amount of the toner. Also, if the average particle size of the primary particles is 30 nm or more, the cleaning process is performed with a large amount of cleaning powder. Therefore, contamination of the charging member in a low-temperature, low-humidity environment can be suppressed, which is preferable. That is, the number-average particle size of the primary particles of the strontium titanate particles is preferably 30 to 300 nm, and more preferably 50 to 200 nm. The shape of the strontium titanate particles is not particularly limited, and may be, for example, a rectangular parallelepiped, cubic, or spherical shape. Among these, a rectangular parallelepiped or cubic shape is preferred because it can increase the contact area with the toner compared to spherical particles, and it is easy to improve the chargeability of the toner in a high-temperature and high-humidity environment.

[0030] <Binding resin> The toner includes toner particles, and the toner particles contain a binder resin. The binder resin may be any known binder resin without any particular limitations. Specific examples include polyester resin, vinyl resin, polyurethane resin, polyamide resin, etc. The binder resin preferably contains a polyester resin, and more preferably contains a polyester resin having a monomer unit corresponding to fumaric acid, since this makes it easier to retain fumaric acid in the toner. As the polyester resin, it is preferable to use at least one selected from the group consisting of an amorphous polyester resin and a crystalline polyester resin.

[0031] The polyester resin can be obtained by combining suitable compounds selected from polyvalent carboxylic acids, polyols, hydroxycarboxylic acids, etc., and synthesizing the compounds using a known method such as an ester exchange method or a polycondensation method. Polycarboxylic acids are compounds containing two or more carboxy groups in one molecule. Among them, dicarboxylic acids are compounds containing two carboxy groups in one molecule and are preferably used.

[0032] Examples of dicarboxylic acids include fumaric acid, oxalic acid, succinic acid, glutaric acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-carboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, suberic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylenediacetic acid, m-phenylenediacetic acid, o-phenylenediacetic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracenedicarboxylic acid, and cyclohexanedicarboxylic acid. As described above, it is preferable to contain fumaric acid as the dicarboxylic acid, and it is more preferable to use fumaric acid in combination with an aromatic dicarboxylic acid.

[0033] Examples of polycarboxylic acids other than dicarboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, pyrene tetracarboxylic acid, itaconic acid, glutaconic acid, n-dodecyl succinic acid, n-dodecenyl succinic acid, isododecyl succinic acid, isododecenyl succinic acid, n-octyl succinic acid, and n-octenyl succinic acid. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0034] A polyol is a compound containing two or more hydroxyl groups in one molecule. Among them, a diol is a compound containing two hydroxyl groups in one molecule, and is preferably used. Specifically, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,7-heptanediol. , 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanediol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-butenediol, neopentyl glycol, 1,4-cyclohexanediol, polytetramethylene glycol, hydrogenated bisphenol A, bisphenol A, bisphenol F, bisphenol S, and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols are particularly preferred.

[0035] Examples of trivalent or higher polyols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, tetraethylolbenzoguanamine, sorbitol, trisphenol PA, phenol novolac, cresol novolac, and alkylene oxide adducts of the above-mentioned trivalent or higher polyphenols. The polyols may be used alone or in combination of two or more kinds. The type of binder resin can be measured by a known method such as NMR.

[0036] The content of the binder resin relative to 100 parts by mass of the toner particles is not particularly limited, but may be 50.0 to 98.0 parts by mass, or 60.0 to 95.0 parts by mass.

[0037] <Wax> The toner may be made of a known wax. Specific examples include petroleum waxes and derivatives thereof, such as paraffin wax, microcrystalline wax, and petrolatum; montan wax and derivatives thereof; hydrocarbon waxes produced by the Fischer-Tropsch process and derivatives thereof; polyolefin waxes and derivatives thereof, such as polyethylene; natural waxes and derivatives thereof, such as carnauba wax and candelilla wax, and derivatives thereof. Derivatives also include oxides, block copolymers with vinyl monomers, and graft modified products. Other examples include alcohols such as higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid or their acid amides, esters, and ketones, hydrogenated castor oil and its derivatives, vegetable waxes, and animal waxes. These can be used alone or in combination of two or more kinds.

[0038] Among these, polyolefins, Fischer-Tropsch hydrocarbon waxes, and petroleum waxes can be suitably used, with Fischer-Tropsch hydrocarbon waxes being particularly preferred since they tend to improve developability and transferability. From the viewpoint of phase separation with respect to the binder resin or crystallization temperature, preferred examples include higher fatty acid esters such as behenyl behenate and dibehenyl sebacate. An antioxidant may be added to these waxes as long as it does not adversely affect the effects of the toner. The content of the wax is preferably 1.0 to 30.0 parts by mass with respect to 100.0 parts by mass of the binder resin. The melting point of the wax is preferably 30 to 120° C., and more preferably 60 to 100° C. By using a wax having the above-mentioned thermal properties, the release effect is efficiently exerted and a wider fixing area is ensured.

[0039] <Plasticizer> The toner particles may contain a crystalline plasticizer in order to improve the sharp melting property. The plasticizer is not particularly limited, and any of the known plasticizers used in toners such as those described below can be used. Specifically, the esters include esters of monohydric alcohols and aliphatic carboxylic acids, such as behenyl behenate, stearyl stearate, and palmityl palmitate, or esters of monohydric carboxylic acids and aliphatic alcohols; esters of dihydric alcohols and aliphatic carboxylic acids, such as ethylene glycol distearate, dibehenyl sebacate, and hexanediol dibehenate, or esters of dihydric carboxylic acids and aliphatic alcohols; esters of trihydric alcohols and aliphatic carboxylic acids, such as glycerin tribehenate, or esters of trihydric carboxylic acids and aliphatic alcohols; and pentaerythritol tetrastearate. Examples of the ester include esters of tetrahydric alcohols and aliphatic carboxylic acids, such as pentaerythritol tetrapalmitate, or esters of tetrahydric carboxylic acids and aliphatic alcohols; esters of hexahydric alcohols and aliphatic carboxylic acids, such as dipentaerythritol hexastearate and dipentaerythritol hexapalmitate, or esters of hexahydric carboxylic acids and aliphatic alcohols; esters of polyhydric alcohols and aliphatic carboxylic acids, such as polyglycerin behenate, or esters of polyhydric carboxylic acids and aliphatic alcohols; and natural ester waxes, such as carnauba wax and rice wax. These may be used alone or in combination of two or more.

[0040] <Coloring agent> The toner particles may contain a colorant. As the colorant, known pigments and dyes of black, yellow, magenta, cyan, and other colors, magnetic materials, and the like can be used without any particular limitation. Black colorants include black pigments such as carbon black.

[0041] Examples of yellow colorants include yellow pigments and yellow dyes such as monoazo compounds, disazo compounds, condensed azo compounds, isoindolinone compounds, benzimidazolone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include CI Pigment Yellow 74, 93, 95, 109, 111, 128, 155, 174, 180, and 185, and CI Solvent Yellow 162.

[0042] Examples of magenta colorants include magenta pigments and magenta dyes such as monoazo compounds, condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 238, 254, 269, and CI Pigment Violet 19.

[0043] Examples of cyan colorants include cyan pigments and cyan dyes such as copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Specifically, examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66.

[0044] The content of the colorant is preferably 1.0 to 20.0 parts by mass with respect to 100.0 parts by mass of the binder resin.

[0045] It is also possible to make the toner magnetic by incorporating a magnetic material in the toner particles. In this case, the magnetic material can also serve as a colorant. Examples of magnetic materials include iron oxides such as magnetite, hematite, and ferrite; metals such as iron, cobalt, and nickel; and alloys of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, beryllium, bismuth, cadmium, calcium, manganese, selenium, titanium, tungsten, and vanadium, and mixtures thereof. When a magnetic material is used as the colorant, the content of the magnetic material is preferably 20.0 to 120.0 parts by mass with respect to 100.0 parts by mass of the binder resin.

[0046] <Charge control agent> The toner may contain a charge control agent. As the charge control agent, any known charge control agent can be used without any particular limitation. Specifically, examples of negative charge control agents include metal compounds of aromatic carboxylic acids such as salicylic acid, alkylsalicylic acid, dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids, or polymers or copolymers having metal compounds of the aromatic carboxylic acids; polymers or copolymers having a sulfonic acid group, a sulfonate salt group, or a sulfonate ester group; metal salts or metal complexes of azo dyes or azo pigments; boron compounds, silicon compounds, and calixarenes. On the other hand, examples of the positive charge control agent include quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains, guanidine compounds, nigrosine compounds, imidazole compounds, and the like. As the polymer or copolymer having a sulfonate group or a sulfonate ester group, a homopolymer of a sulfonate group-containing vinyl monomer such as styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, or methacrylsulfonic acid, or a copolymer of another known vinyl monomer and the above-mentioned sulfonate group-containing vinyl monomer, can be used. The content of the charge control agent is preferably 0.01 to 5.0 parts by mass with respect to 100.0 parts by mass of the binder resin.

[0047] <External additives> The toner has an external additive. The external additive contains strontium titanate particles. The external additive may contain, in addition to the strontium titanate particles, an external additive other than the strontium titanate particles. As the external additive, any known external additive can be used without any particular limitation. Specific examples include raw silica fine particles such as wet-process silica and dry-process silica, or surface-treated silica fine particles obtained by subjecting such raw silica fine particles to a surface treatment with a treating agent such as a silane coupling agent, a titanium coupling agent, or silicone oil; and resin fine particles such as vinylidene fluoride fine particles and polytetrafluoroethylene fine particles. The content of the external additive is preferably 0.1 to 5.0 parts by mass with respect to 100.0 parts by mass of the toner particles.

[0048] <Dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts> The toner preferably contains at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts. When the toner contains at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts, the dodecylbenzenesulfonic acid or dodecylbenzenesulfonate salts receive charge from excessively negatively charged sites on the toner surface and are adsorbed to excessively positively charged sites, thereby making the charge distribution on the toner surface uniform. This reduces the adhesive force to the photoreceptor surface. This improves the cleaning properties of the toner. Similarly, strontium titanate Even if the strontium titanate particles are excessively positively charged, it is possible to suppress overcharging. As a result, the adhesive force between the strontium titanate particles and the photoconductor is reduced, improving the cleaning ability of the cleaning member. As a result, contamination of the charging member is further suppressed. There is no particular limitation on the method for adding dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts, and they can be added in any step of the method for producing toner particles or the method for producing toner described below. The dodecylbenzenesulfonate is not particularly limited, but examples thereof include sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, and lithium dodecylbenzenesulfonate, and among these, sodium dodecylbenzenesulfonate is preferred.

[0049] The content ratio of at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts in the toner is not particularly limited, but is preferably 10 to 1000 mass ppm, more preferably 20 to 800 mass ppm, relative to the toner. The content ratio can be adjusted by changing the amount of at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts added during toner production.

[0050] Next, a method for obtaining the toner of the present disclosure will be described in detail below.

[0051] <Method of manufacturing toner particles> The method for producing the toner particles is not particularly limited, and an emulsion aggregation method, a suspension polymerization method, a dissolution suspension method, a pulverization method, or the like can be used. Among these, it is preferable to use the emulsion aggregation method. That is, it is preferable that the toner particles are emulsion aggregation toner particles. In the emulsion aggregation method, a dispersion of fine particles of a binder resin is first prepared, and then dispersions of other materials such as a colorant and a release agent are prepared as necessary. The obtained dispersions of the materials are dispersed and mixed by adding a dispersion stabilizer as necessary. Then, an aggregating agent is added to aggregate the particles to the desired toner particle size, and then or simultaneously with the aggregation, the resin fine particles are fused together. If necessary, the shape is controlled by heat to form toner particles.

[0052] The method for producing the toner preferably includes the following steps. (1) A dispersion and mixing step of preparing a binder resin particle dispersion liquid (and, if necessary, a colorant particle dispersion liquid, etc.) containing a binder resin and fumaric acid, and mixing them to obtain a mixed dispersion liquid; (2) an aggregation step of aggregating the binder resin fine particles (and colorant fine particles, if necessary) contained in the obtained mixed dispersion to form aggregates; and (3) a fusion step of heating the aggregates to fuse them together to form fused particles; The resulting fused particles can be cooled to obtain toner particles.

[0053] It is preferable to have the following step (4) during the above step (3) or after the above steps (1) to (3). (4) A spheronization step in which the agglomerates are heated at a higher temperature. Furthermore, it is more preferable to have the following steps (5) and (6) in this order after the above step (4). (5) A cooling step of cooling the aggregate at a cooling rate of 0.1° C. / min or more. (6) an annealing step of heating and holding the temperature at or above the crystallization temperature or the glass transition temperature of the binder resin after the cooling step;

[0054] It is further preferable to have the following step (7) after the above step (3), (4) or (6). (7) Surface cleaning process for cleaning the surfaces of toner particles In step (7), the surfaces of the toner particles are washed with water such as ion-exchanged water or fumaric acid water. A solution, methanol, etc. can be used. When water is used, impurities contained in the toner particles can be removed. When an aqueous fumaric acid solution is used, the amount of fumaric acid on the surface of the toner particles can be increased while removing impurities contained in the toner particles. When methanol is used, the amount of fumaric acid on the surface of the toner particles can be reduced while removing impurities contained in the toner particles. That is, the value of f1 can be adjusted by cleaning the surface of the toner particles with an aqueous fumaric acid solution or methanol. The concentration of the aqueous fumaric acid solution is not particularly limited, and for example, an aqueous fumaric acid solution in which 0.2 to 0.8 parts by mass of fumaric acid is dissolved in 100 parts by mass of ion-exchanged water can be used.

[0055] Here, the binder resin particles may be composite particles formed of two or more layers of resins having different compositions, and may be produced by at least one method selected from the group consisting of emulsion polymerization, mini-emulsion polymerization, and phase inversion emulsification.

[0056] When an internal additive is contained in the toner particles, the internal additive may be contained in the resin fine particles, or a dispersion liquid of internal additive fine particles containing the internal additive may be prepared separately, and the internal additive fine particles may be aggregated together with the resin fine particles when the internal additive fine particles are aggregated. In addition, toner particles having layer structures with different compositions can be produced by adding resin fine particles with different compositions at different times during aggregation and aggregating them. That is, toner particles having a core-shell structure can be produced. After aggregating resin fine particles containing a binder resin to form a core portion, resin fine particles containing a shell resin can be added at different times and aggregating them to form a shell portion. The shell resin may be the same as or different from the binder resin. For example, the shell resin may contain fumaric acid. It is preferable that the resin fine particles containing the shell resin contain fumaric acid. The amount of the shell resin added (shell content) is preferably 1.0 to 10.0 parts by mass, more preferably 2.0 to 7.0 parts by mass, based on 100 parts by mass of the binder resin contained in the core particles.

[0057] In the case of producing toner particles having a core-shell structure, the method for producing the toner preferably includes the following steps in the following order. (1) A dispersion and mixing step of preparing a dispersion of binder resin particles containing a binder resin and fumaric acid (or a colorant particle dispersion, if necessary) and mixing the mixture to obtain a mixed dispersion; (2) an aggregation step of aggregating the binder resin particles (and, if necessary, colorant particles) contained in the obtained mixed dispersion to form aggregates; (3) a shell formation step of further adding resin fine particles containing a resin for a shell to the dispersion containing the aggregates, and aggregating the resin fine particles to form aggregates having a shell; and (4) a fusion step of heating the aggregates to fuse them together to form fused particles;

[0058] In addition, it is preferable to have the following step (5) during the above step (4) or after the above steps (1) to (4). (5) A spheronization step in which the agglomerates are heated at a higher temperature. It is more preferable to have the following steps (6) and (7) in this order after the above step (5). (6) A cooling step of cooling the aggregate at a cooling rate of 0.1° C. / sec or more. (7) an annealing step of heating and holding the temperature at or above the crystallization temperature or the glass transition temperature of the binder resin after the cooling step;

[0059] It is further preferable to have the following step (8) after the above step (4), (5) or (7). (8) Surface cleaning process for cleaning the surfaces of toner particles The surface cleaning step can be carried out in the same manner as in step (7) above.

[0060] The amount of fumaric acid added is not particularly limited, but is preferably 0.006 to 0.500 parts by mass, more preferably 0.006 to 0.400 parts by mass, and even more preferably 0.006 to 0.200 parts by mass, relative to 100 parts by mass of the binder resin. By being in the above range, it becomes easier to suitably adjust the content ratio f0 of fumaric acid in the toner. The amount of strontium titanate particles added is not particularly limited, but is preferably 0.003 to 10,000 parts by mass, more preferably 0.005 to 8,000 parts by mass, even more preferably 0.010 to 5,000 parts by mass, and particularly preferably 0.020 to 4,000 parts by mass, relative to 100 parts by mass of toner particles. By being within the above range, it becomes easier to suitably adjust the content ratio a0 of strontium titanate particles in the toner.

[0061] The following can be used as the dispersion stabilizer. As the dispersion stabilizer, a surfactant can be used, including known cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of inorganic dispersion stabilizers include tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Examples of the organic dispersion stabilizer include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch. These can be used alone or in combination of two or more.

[0062] As the dispersion stabilizer, it is preferable to use at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts, which are anionic surfactants. At least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts can be effectively retained in the toner. That is, it is preferable to allow the toner to contain at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts, which improves the cleaning properties by a cleaning member.

[0063] As the flocculant, in addition to a surfactant having a polarity opposite to that of the surfactant used in the above-mentioned dispersion stabilizer, an inorganic salt or a divalent or higher inorganic metal salt can be suitably used. In particular, an inorganic metal salt is preferred because it is easy to control the flocculation property and the toner charge property by ionizing a polyvalent metal element in an aqueous medium. Specific examples of preferred inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, iron chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyiron chloride, polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. Among these, aluminum salts and their polymers are particularly preferred. These can be used alone or in combination of two or more. In general, in order to obtain a sharper particle size distribution, the valence of the inorganic metal salt is preferably divalent rather than monovalent, and more preferably trivalent or more than divalent. Furthermore, even if the valence is the same, an inorganic metal salt polymer is more suitable.

[0064] <Average circularity of toner> The toner may have an average circularity of 0.930 to 0.990, and preferably 0.950 to 0.980. By making the average circularity of the toner 0.950 or more, the contact area with the photoconductor is reduced. As a result, the adhesion between the toner and the photoconductor is reduced, and the transferability from the photoconductor is improved. This is preferable because it suppresses the decrease in image density even after continuous use in a high-temperature and high-humidity environment. Furthermore, by making the circularity of the toner 0.980 or less, the transfer residual toner remaining on the photoconductor in the transfer step can be easily cleaned in the cleaning step, which is preferable because it can reduce contamination of the charging member. In order to adjust the circularity of the toner to fall within the above range, it is preferable to employ a production method such as an emulsion aggregation method, a suspension polymerization method, or a suspension granulation method as a production method for the toner. Such production methods are also used for producing chemical toner. When the emulsion aggregation method is used, it is preferable to provide a spheronization step to adjust the circularity of the toner in order to obtain a desired toner surface shape. When the pulverization method is used, the circularity of the toner can be adjusted by subjecting the toner to surface treatment using hot air in a thermal sphering process.

[0065] <Toner manufacturing method> The toner particles obtained above can be mixed with strontium titanate particles and attached to the surface of the toner particles to produce a toner. That is, the toner manufacturing method includes an external addition step of externally adding an external additive containing strontium titanate particles to the toner particles. At this time, an external additive other than the above-mentioned strontium titanate particles may be added as necessary. The mixer for adding the external additive to the toner particles is not particularly limited, and any known mixer can be used, regardless of whether it is a dry or wet type. Examples include FM Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), Super Mixer (manufactured by Kawata Corporation), Nobilta (manufactured by Hosokawa Micron Corporation), and Hybridizer (manufactured by Nara Machinery Co., Ltd.). In order to control the coating state of the external additive, the toner can be prepared by adjusting the rotation speed, processing time, and water temperature and amount of water in the jacket of the external addition device. In addition, sieving devices used to sift out coarse particles after external addition include Ultrasonic (manufactured by Koei Sangyo Co., Ltd.); Resonaseave, Gyroshifter (Tokuju Kogyo Co., Ltd.); Vibrasonic System (manufactured by Dalton Co., Ltd.); Soniclean (manufactured by Shinto Kogyo Co., Ltd.); Turbo Screener (manufactured by Turbo Kogyo Co., Ltd.); Microshifter (manufactured by Makino Sangyo Co., Ltd.), etc.

[0066] The methods for measuring the physical properties of the toner and each material will be described below.

[0067] <Method for measuring the content of fumaric acid in toner (% by mass)> Dissolve 0.1 g of toner in 1 ml of chloroform. Drop 20 ml of methanol into the obtained sample solution to precipitate the resin in the solution, then remove the solid matter by centrifugation (HITACHI himac CR22G, 12000 rpm, 10 minutes). Remove the solvent from the obtained solution by vacuum distillation, and further dry the solution under reduced pressure in a 60°C atmosphere for 4 hours. Add 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile to the obtained sample, The silylation treatment is carried out by heating at 80° C. for 1 hour. The obtained sample is analyzed by GC-MS (gas chromatography-mass spectrometry).

[0068] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0069] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is contained. On the other hand, several samples of fumaric acid alone (e.g., 100 ng, 200 ng, and 300 ng) are precisely weighed and prepared, and before measuring the sample obtained from the toner, each sample is measured under the above-mentioned analytical conditions, and then a calibration curve is created from the amount of fumaric acid added and the fumaric acid peak area value. The content ratio f0 (mass %) of fumaric acid in the toner is obtained by converting the area value of the fumaric acid component of the toner based on this calibration curve into the mass of fumaric acid, and then converting it into an amount based on the toner mass.

[0070] <Method for measuring the content f1 (mass%) of fumaric acid in toner, which is extracted from toner with methanol> 0.5 g of toner is placed in 20 ml of methanol and dispersed for 30 minutes. Then, solids are removed by centrifugation (HITACHI himac CR22G, 12000 rpm, 10 minutes). The solvent is removed from the resulting solution by vacuum distillation, and the solution is further dried for 4 hours under reduced pressure in a 60°C atmosphere. 0.5 mL of BSTFA (N,O-bis(trimethylsilyl)trifluoroacetamide) and 0.5 mL of acetonitrile are added to the resulting sample, which is then heated at 80°C for 1 hour to perform a silylation treatment. The resulting sample is analyzed by GC-MS (gas chromatography mass spectrometry).

[0071] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0072] The profile obtained by the analysis is analyzed, and the peak positions of the measured sample are compared with the peak positions of the profile obtained from a fumaric acid standard. The mass spectrum is then confirmed to determine whether or not fumaric acid is contained. On the other hand, several samples of fumaric acid alone (e.g., 100 ng, 200 ng, and 300 ng) are precisely weighed and prepared, and before measuring the sample obtained from the toner, each sample is measured under the above-mentioned analytical conditions, and then a calibration curve is created from the amount of fumaric acid added and the fumaric acid peak area value. The content ratio f1 (mass %) of fumaric acid in the toner extracted with methanol is obtained by converting the area value of the fumaric acid component in the toner based on this calibration curve into the mass of fumaric acid, and then converting it into an amount based on the toner mass.

[0073] <Method for measuring the content a0 (mass%) of strontium titanate particles in toner> Strontium titanate particles can be said to be titanates containing strontium particles, which are a group 2 element. The amount of strontium titanate particles containing a group 2 element is determined by the standard addition method. Specifically, the quantification is carried out according to the following procedure. The measurement equipment used is a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, the measurement time is 10 seconds, and detection is performed with a scintillation counter (SC). Measurement is performed under these conditions, and the elements are identified based on the peak positions of the obtained X-rays, and their concentrations are calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time. The measurement sample was prepared by placing approximately 4 g of toner in a special aluminum ring for pressing, flattening it, and then pressing it at 20 MPa for 60 seconds using a tablet molding compression machine "BRE-32" (manufactured by Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of approximately 2 mm and a diameter of approximately 39 mm. Measurements are performed under the above conditions, and elements are identified based on the peak positions of the obtained X-rays, and their concentrations are calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time. Strontium titanate fine powder with a primary particle diameter of 100 nm is added to the toner particles so that the amount is 1.00 parts by mass, and the mixture is thoroughly mixed using a coffee mill. Similarly, strontium titanate fine powder is mixed with the toner particles so that the amount is 2.00% by mass and 3.00% by mass, respectively, and these are used as samples for the calibration curve. For each sample, a pellet of the calibration curve sample is prepared as described above using a tablet molding compression machine, and the count rate (unit: cps) of Sr-Kα rays observed at a diffraction angle (2θ) = 35.8 ° when LiF220 is used as the analyzing crystal is measured. In this case, the acceleration voltage and current value of the X-ray generator are 60 kV and 40 mA, respectively. A linear function calibration curve is obtained by taking the count rate of the obtained X-rays as the vertical axis and the amount of strontium titanate added in each calibration curve sample as the horizontal axis. Next, the toner to be analyzed is pelletized as described above using a tablet molding compressor, and the count rate of the Sr-Kα ray is measured. Then, the content ratio a0 (mass%) of strontium titanate particles in the toner is calculated from the above calibration curve.

[0074] <Method for identifying fatty acids contained in strontium titanate> (1) Method for separating strontium titanate particles from the toner surface Add 1.6 kg of sucrose (Kishida Chemical) to 1 L of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Place 31 g of concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries, Ltd.) in a centrifuge tube to prepare a dispersion. Add 10 g of toner to this dispersion and break up any clumps of toner with a spatula or similar. The centrifugation tube is placed in an Iwaki Sangyo KM Shaker (model: V.SX) and shaken for 20 minutes at 350 reciprocations per minute. After shaking, the solution is transferred to a glass tube (50 mL) for a swing rotor and centrifuged at 3,500 rpm for 30 minutes. After centrifugation, the toner particles are present in the top layer in the glass tube, and the inorganic fine particle mixture containing strontium titanate particles is present in the lower aqueous solution. The lower aqueous solution is separated and then dried to obtain the inorganic fine particle mixture. The above centrifugation process is repeated until the amount of the obtained inorganic fine particle mixture is 10 g or more in total. Next, 10 g of the obtained inorganic fine particle mixture is dispersed in a dispersion liquid containing 100 mL of ion-exchanged water and 6 mL of Contaminon N. The obtained dispersion liquid is transferred to a glass tube (50 mL) for a swing rotor, and centrifuged in a centrifuge at 3500 rpm for 30 minutes. After the centrifugation, in the glass tube, strontium titanate particles are present in the bottom layer, and other inorganic fine particles are present in the upper layer on the aqueous solution side. The mixture of inorganic fine particles containing the strontium titanate particles in the bottom layer is collected and, if necessary, The centrifugation operation is repeated until sufficient separation is achieved, and the strontium titanate particles are separated and dried to collect the strontium titanate particles. This process is repeated until the required amount of strontium titanate particles is collected.

[0075] (2) Method for identifying fatty acids Add 1 mL of chloroform to 0.05 g of the obtained strontium titanate particles, and treat the obtained sample solution with an ultrasonic disperser for 10 minutes to extract fatty acids into the chloroform solution. Further, centrifugation (HITACHI himac CR22G, 12000 rpm, 30 minutes) is performed, and solid matter is removed by filtration. The obtained solution is analyzed by GC-MS (gas chromatography mass spectrometry).

[0076] Specifically, the measurement conditions are as follows. GCMS equipment: Trace1310 (Thermo Fisher Scientific), ISQ (Thermo Fisher Scientific) Column: HP-5ms 30m Inlet temperature: 250℃ Injection volume: 1μL Column oven temperature: 40℃→300℃ (15℃ / min) MS ionization mode: EI Ion source temperature: 250℃ Mass range: 35-800 m / z

[0077] The profile obtained by the analysis is analyzed, and the peak positions of the measurement sample are compared with the peak positions of the profile obtained from a standard sample of fatty acid such as stearic acid, and the fatty acid is identified by confirming the mass spectrum. Furthermore, the detection of fatty acid by such an operation indicates that the strontium titanate particles have fatty acid on the surface of the strontium titanate particles.

[0078] <Quantitative Determination of Dodecylbenzenesulfonic Acid or Dodecylbenzenesulfonate in Toner> 0.5 g of toner is placed in 20 ml of methanol and dispersed for 30 minutes. Solids are then removed by centrifugation (HITACHI himac CR22G, 12,000 rpm, 10 minutes). The solvent is removed from the resulting solution under reduced pressure, and the solution is dried for 4 hours under reduced pressure at 60°C. The resulting sample is subjected to LC / MS measurement to quantify the amount of dodecylbenzenesulfonic acid or sodium dodecylbenzenesulfonate. The LC / MS analysis conditions are as follows. A calibration curve is created using sodium dodecylbenzenesulfonate as the standard, and quantification is performed. If the quantification results in an amount of 10 ppm or more by mass, it is determined that dodecylbenzenesulfonic acid or sodium dodecylbenzenesulfonate is present.

[0079] (LC / MS analysis conditions) Model: Agilent 6130Quadropole LC / MS (Agilent Technologies) Eluent: Methanol Column: ZORBAX Eclipse Plus C18 (1.8 μm, 100 × 4.6 mm I.D.) (Agilent Technologies) Flow rate: 1.0 mL / min Column temperature: 30℃

[0080] <Method for measuring average circularity> The average circularity of the toner and toner particles is measured and analyzed under the following conditions using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation). The specific measurement method is as follows. First, 20 mL of ion-exchanged water from which solids and other impurities have been removed is placed in a glass container. 0.2 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant. 0.02 g of the measurement sample is then added, and the dispersion is processed for 2 minutes using an ultrasonic disperser to obtain a dispersion for measurement. At this time, the dispersion is appropriately cooled so that the temperature of the dispersion is between 10 and 40°C. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser ("VS-150" (manufactured by Velvoclear)) with an oscillation frequency of 50 kHz and an electrical output of 150 W was used. A predetermined amount of ion-exchanged water was placed in the water tank, and approximately 2 mL of the Contaminon N was added to the water tank. For the measurement, the flow type particle image analyzer equipped with "UPlanApro" (magnification 10x, numerical aperture 0.40) as the objective lens is used, and particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid.

[0081] The dispersion liquid prepared according to the above procedure is introduced into the flow type particle image analyzer, and 3000 toner particles are measured in HPF measurement mode and total count mode.Then, the binarization threshold during particle analysis is set to 85%, and the analyzed particle diameter is limited to a circle equivalent diameter of 1.985 μm or more and less than 39.69 μm, and the average circularity of the toner particles is obtained. Before starting the measurement, automatic focus adjustment is performed using standard latex particles (Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water).

[0082] <Method of measuring weight average particle size (D4)> The weight average particle diameter (D4) of the toner or toner particles (hereinafter, also referred to as toner, etc.) is calculated as follows. The measuring device used is a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000 channels. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1.0%, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter, Inc.). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0083] The specific measurement method is as follows. (1) Pour 200.0 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, place it on the sample stand, and rotate the stirrer rod counterclockwise. Then, use the "Aperture Tube Flush" function of the dedicated software to remove any dirt and air bubbles from inside the aperture tube. (2) Place 30.0 mL of the electrolyte solution in a 100 mL flat-bottom glass beaker. Add 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees and an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank and add 2.0 mL of Contaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is being irradiated with ultrasonic waves, 10 mg of toner or the like is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted so that it is between 10°C and 40°C. (6) Using a pipette, drip the electrolytic solution (5) in which the toner or the like has been dispersed into the round-bottom beaker (1) placed in the sample stand to adjust the measurement concentration to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).

[0084] <Method of calculating the number average particle size of primary particles of strontium titanate particles> The number average particle size of the primary particles of strontium titanate particles is calculated using images obtained by backscattered electron image observation with the S-4800. Backscattered electron images have less charge-up of strontium titanate particles than secondary electron images, so particle size can be measured with high accuracy. (1) Measurement preparation Inject liquid nitrogen into the anti-contamination trap attached to the S-4800 housing until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2, and execute it. Check that the emission current due to flushing is 20 to 40 μA. Insert the sample holder into the sample chamber of the S-4800 housing. Press [Origin] on the control panel to move the sample holder to the observation position. Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [0.8kV] and the emission current to [20μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Upper (U)] and [+BSE], and select [LA100] in the selection box to the right of [+BSE] to set the mode to observation with backscattered electron images. In the same [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [3.0mm]. Press the [ON] button in the accelerating voltage display of the control panel to apply the accelerating voltage.

[0085] (2) Focus adjustment Drag within the magnification display area of ​​the control panel to set the magnification to 100000 (100k). 3x. Rotate the focus knob [COARSE] on the operation panel until the image is in focus to a certain extent, then adjust the aperture alignment. Click [Align] on the control panel to display the alignment dialog, and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles. Next, select [Aperture], and rotate the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or adjust it so that it moves as little as possible. Close the aperture dialog, and use autofocus to adjust the focus. Repeat this operation two more times to adjust the focus.

[0086] (3) Image storage The brightness is adjusted in ABC mode, and a photograph is taken at a size of 640 x 480 pixels and saved. This image file is used for the following analysis. One photograph is taken for each strontium titanate particle, and images are obtained for 300 strontium titanate particles. Here, when obtaining images for the 300 strontium titanate particles, images were obtained using different toners.

[0087] (4) Calculation of the number-average particle size of primary particles of strontium titanate particles The particle size of the primary particles of 300 strontium titanate particles is measured to obtain the number average particle size. Here, the maximum diameter of the primary particles of the strontium titanate particles is measured, and the number average particle size of the primary particles of the strontium titanate particles is obtained by arithmetically averaging the maximum diameters obtained. In addition, the shape of the strontium titanate particles can be determined from the observation results. Furthermore, by combining elemental analysis by energy dispersive X-ray analysis (EDS), it is possible to determine whether the particles are strontium titanate particles or not. Specifically, a scanning electron microscope "S-4800" (product name; manufactured by Hitachi) is used to observe the toner in a field of view magnified up to 100,000 times. The focus is adjusted to the surface of the toner particles, and the external additive to be identified is observed. An EDS analysis is performed on the external additive to be identified, and it is possible to determine whether the particles are strontium titanate particles or not from the element peaks. Specifically, when titanium and strontium are detected, it can be determined that the particles are strontium titanate particles. EXAMPLES

[0088] The present disclosure will be specifically described with reference to the following examples. However, these are not intended to limit the present disclosure in any way. Unless otherwise specified, "parts" and "%" are all by mass.

[0089] [Production example of polyester resin] <Polyester resin A> Fumaric acid: 10.6 parts (23 mol%) Terephthalic acid: 8.5 parts (13 mol%) Trimellitic acid: 3.3 parts (4 mol%) Bisphenol A-ethylene oxide 2-mol adduct: 47.6 parts (38 mol%) Bisphenol A-propylene oxide 2-mol adduct: 30.0 parts (22 mol%) Dibutyltin oxide: 0.5 parts Hydroquinone: 0.05 parts The above materials were charged into an autoclave equipped with a pressure reducing device, a water separator, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and reacted at 230°C until the reaction rate reached 90%, and then further reacted for 1 hour under reduced pressure of 60 to 70 mmHg to obtain an amorphous polyester resin A. In this specification, the reaction rate refers to the value of the amount of reaction water produced (mol) / theoretical amount of water produced (mol)×100.

[0090] [Example of resin particle dispersion production] <Resin particle dispersion 1> Polyester resin A 200 parts -500 parts deionized water Fumaric acid 0.250 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to make the pH greater than 7.0. Thereafter, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise, and emulsified and dispersed while stirring at 7800 rpm to obtain resin particle dispersion 1. The solid content concentration of resin particle dispersion 1 was 20%. The particle size distribution of the polyester resin A particles contained in the resin particle dispersion 1 was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.). The number average particle size of the polyester resin A particles was 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0091] <Resin particle dispersion liquid 2~7> Resin particle dispersions 2 to 7 were produced in the same manner as in Production Example of Resin Particle Dispersion 1, except that the resin used and the amount of fumaric acid added were changed to those shown in Table 1. In all cases, no coarse particles exceeding 1 μm were observed. The number average particle diameters of the polyester resin particles in Resin Particle Dispersions 2 to 7 are shown in Table 1. [Table 1]

[0092] <Production Example of Wax Particle Dispersion> -500 parts deionized water Wax (FNP0090 (manufactured by Nippon Seiro Co., Ltd.): Fischer-Tropsch process hydrocarbon wax, melting point 90°C, molecular weight 771) 200 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50), 0.1 mol / L sodium bicarbonate was added to make the pH greater than 7.0. Then, a mixed solution of 5 parts of sodium dodecylbenzenesulfonate and 295 parts of ion-exchanged water was gradually added dropwise, and emulsified and dispersed while stirring at 7800 rpm to obtain a wax particle dispersion. The solids concentration of the wax particle dispersion was 20%. The particle size distribution of the wax particles contained in the wax particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number average particle size of the wax particles was found to be 0.35 μm.

[0093] <Production Example of Colorant Particle Dispersion> Carbon black (Nipex35: Orion Engineered Carbon ns Co., Ltd.) 100 copies Sodium dodecylbenzenesulfonate 5 parts -Ion-exchanged water 400 parts The above materials were mixed and dispersed using a sand grinder mill to obtain a colorant particle dispersion. The solid content of the colorant particle dispersion was 20%. The particle size distribution of the colorant particles contained in this colorant particle dispersion was measured using a particle size measuring device (LA-960V2, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0094] [Toner particle manufacturing example] <Toner particle 1> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion 1, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 1 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.960.

[0095] <Toner particles 2 to 7> Toner particles 2 to 7 were produced in the same manner as in the production example of toner particles 1, except that the resin particle dispersion liquid used in the production example of toner particles 1 was changed to that shown in Table 2. The weight average particle size (D4) of toner particles 2 to 7 was all 6.9 μm.

[0096] <Toner particles 8> ·Resin particle dispersion 2 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion 1, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was separated into solid and liquid in a 10 L pressure filter under a pressure of 0.4 MPa. A toner cake was obtained. Then, methanol was added until the pressure filter was filled, and washing was performed at a pressure of 0.4 MPa. This operation removed a part of the fumaric acid on the surface of the toner particles. Next, ion-exchanged water was added until the pressure filter was filled, and washing was performed at a pressure of 0.4 MPa. Similarly, washing was performed twice more with ion-exchanged water, for a total of three washings. After that, solid-liquid separation was performed under a pressure of 0.4 MPa, and fluidized bed drying was performed at 45°C to obtain toner particles 8 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.960.

[0097] <Toner particles 9> ·Resin particle dispersion 3 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 3, wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Then, an aqueous fumaric acid solution in which 0.5 parts by mass of fumaric acid was dissolved in 100 parts by mass of ion-exchanged water was added to the pressure filter until it was full, and washed under a pressure of 0.4 MPa. Similarly, the mixture was washed twice with the aqueous fumaric acid solution, for a total of three washes. After that, the mixture was subjected to solid-liquid separation under a pressure of 0.4 MPa, and then fluidized bed drying was performed at 45°C to obtain toner particles 9 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.960.

[0098] <Toner particle 10> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion 1, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Then, an aqueous fumaric acid solution in which 0.5 parts by mass of fumaric acid was dissolved in 100 parts by mass of ion-exchanged water was added to the pressure filter until it was full, and washed under a pressure of 0.4 MPa. Similarly, the mixture was washed twice with the aqueous fumaric acid solution, for a total of three washes. After that, the mixture was subjected to solid-liquid separation under a pressure of 0.4 MPa, and then fluidized bed drying was performed at 45°C to obtain toner particles 10 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.960.

[0099] <Toner particles 11> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 30 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Then, methanol was added until the pressure filter was filled, and washing was performed under a pressure of 0.4 MPa. This operation removed a part of the fumaric acid on the surface of the toner particles. Next, ion-exchanged water was added until the pressure filter was filled, and washing was performed under a pressure of 0.4 MPa. Similarly, washing was performed twice more with ion-exchanged water, for a total of three washings. Then, solid-liquid separation was performed under a pressure of 0.4 MPa, followed by fluidized bed drying at 45°C to obtain toner particles 11 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.960.

[0100] <Toner particles 12> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 60 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation in a 10 L pressure filter under a pressure of 0.4 MPa to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 12 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.980.

[0101] <Toner particles 13> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, a colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. The obtained mixed dispersion was stirred while adding sulfuric acid. An aqueous aluminum solution (0.5 parts as solid content) was added dropwise to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 15 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 13 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.950.

[0102] <Toner particles 14> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropping was completed, the system was replaced with nitrogen, and the mixture was kept at 50°C for 1 hour, and then at 55°C for 1 hour. The temperature was then raised and kept at 90°C for 90 minutes. The temperature was then lowered to 63°C and kept at that temperature for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation under a pressure of 0.4 MPa in a 10 L pressure filter to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 14 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.990.

[0103] <Toner particles 15> ·Resin particle dispersion 1 500 parts Colorant particle dispersion 50 parts Wax particle dispersion 50 parts Sodium dodecylbenzenesulfonate 5 parts Resin particle dispersion 1, wax particle dispersion, and sodium dodecylbenzenesulfonate were charged into a reactor (1-liter flask, baffled anchor blade) and mixed uniformly. Meanwhile, colorant particle dispersion was mixed uniformly in a 500-mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise to the obtained mixed dispersion while stirring to form aggregated particles. After the dropwise addition was completed, the system was purged with nitrogen, and the mixture was maintained at 50° C. for 1 hour, and then at 55° C. for 1 hour. The temperature was then raised and maintained at 63° C. for 3 hours to form fused particles. After the fused particles were formed, the mixture was cooled to room temperature at a temperature decreasing rate of 0.5° C. per minute. After cooling, the reaction product was subjected to solid-liquid separation in a 10 L pressure filter under a pressure of 0.4 MPa to obtain a toner cake. Thereafter, ion-exchanged water was added until the pressure filter was filled with water, and the mixture was washed under a pressure of 0.4 MPa. The mixture was washed two more times in the same manner, for a total of three times. After solid-liquid separation under a pressure of 0.4 MPa, the mixture was subjected to fluidized bed drying at 45°C to obtain toner particles 15 having a weight average particle size (D4) of 6.9 μm and an average circularity of 0.930.

[0104] <Toner particles 16> Polyester resin A 100 parts Fumaric acid 0.125 parts Carbon black (Nipex35: Orion Engineered Carbons) 10 parts Wax (FNP0090 (Nippon Seiro Co., Ltd.): Fischer-Tropsch process hydrocarbon wax, melting point 90°C, molecular weight 771) 1 part The above materials were premixed in an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.), and then melt-kneaded using a twin-screw kneading extruder (manufactured by Ikegai Iron Works Co., Ltd., PCM-30 type). The resulting kneaded material was cooled, coarsely pulverized using a hammer mill, and then pulverized using a mechanical pulverizer (manufactured by Turbo Kogyo Co., Ltd., T-250). The resulting finely pulverized powder was classified using a multi-division classifier utilizing the Coanda effect, and toner particles 16 with a weight-average particle size (D4) of 6.9 μm and an average circularity of 0.930 were obtained. [Table 2]

[0105] [Example of manufacturing strontium titanate particles] <Strontium titanate particles 1 (T-1)> The titanium oxide hydrous slurry obtained by hydrolysis of the titanyl sulfate aqueous solution was washed with an alkaline aqueous solution. Next, hydrochloric acid was added to the titanium oxide hydrous slurry to adjust the pH to 0.65 to obtain a titania sol dispersion. NaOH was added to the titania sol dispersion to adjust the pH of the dispersion to 4.5, and washing with ion-exchanged water was repeated until the electrical conductivity of the supernatant liquid reached 70 μS / cm. Add 0.97 times the molar amount of Sr(OH)2·8H2O to hydrous titanium oxide to obtain SU The mixture was placed in an S reactor and purged with nitrogen gas. Distilled water was then added to make a slurry of 0.5 mol / L in terms of SrTiO3. The obtained slurry was heated to 83°C at a rate of 6.5°C / hour in a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature, the supernatant was removed, and the mixture was repeatedly washed with ion-exchanged water. The slurry containing the obtained precipitate was adjusted to 40°C, and hydrochloric acid was added to adjust the pH to 2.5. Then, 1.2 parts by mass of stearic acid was added per 100 parts by mass of solid content, and stirring was continued for 10 hours. A 5 mol / L sodium hydroxide solution was added to adjust the pH to 6.5, and stirring was continued for 1 hour. Then, filtration and washing were performed, and the mixture was dried in the air at 120°C for 8 hours to obtain strontium titanate particles 1 (T-1). The number average particle size of the primary particles of the obtained strontium titanate particles 1 (T-1) was 100 nm, and the particle shape was rectangular or cubic.

[0106] <Strontium titanate particles 2 (T-2)> The titanium oxide hydrous slurry obtained by hydrolysis of the titanyl sulfate aqueous solution was washed with an alkaline aqueous solution. Next, hydrochloric acid was added to the titanium oxide hydrous slurry to adjust the pH to 0.5, and a titania sol dispersion was obtained. NaOH was added to the titania sol dispersion to adjust the pH of the dispersion to 4.0, and washing with ion-exchanged water was repeated until the electrical conductivity of the supernatant liquid reached 70 μS / cm. To the titanium oxide hydroxide, 0.93 times the molar amount of Sr(OH)2·8H2O was added, placed in a stainless steel reaction vessel, and purged with nitrogen gas. Distilled water was then added to make a slurry of 0.7 mol / L in terms of SrTiO3. The obtained slurry was heated to 70° C. at a rate of 8.5° C. / hour in a nitrogen atmosphere, and reacted for 5 hours after the temperature reached 70° C. After the reaction, it was cooled to room temperature, the supernatant liquid was removed, and then washing with ion-exchanged water was repeated. The slurry containing the obtained precipitate was adjusted to 40°C, and hydrochloric acid was added to adjust the pH to 2.5. Then, 1.2 parts by mass of stearic acid was added per 100 parts by mass of solid content, and stirring was continued for 10 hours. A 5 mol / L sodium hydroxide solution was added to adjust the pH to 6.5, and stirring was continued for 1 hour. Then, filtration and washing were performed, and the mixture was dried in the air at 120°C for 8 hours to obtain strontium titanate particles 2 (T-2). The number average particle size of the primary particles of the obtained strontium titanate particles 2 (T-2) was 30 nm, and the particle shape was rectangular or cubic.

[0107] <Strontium titanate particles 3 (T-3)> The titanium oxide hydrous slurry obtained by hydrolysis of the titanyl sulfate aqueous solution was washed with an alkaline aqueous solution. Next, hydrochloric acid was added to the titanium oxide hydrous slurry to adjust the pH to 0.7, and a titania sol dispersion was obtained. NaOH was added to the titania sol dispersion to adjust the pH of the dispersion to 5.3, and washing with ion-exchanged water was repeated until the electrical conductivity of the supernatant liquid reached 70 μS / cm. To the titanium oxide hydroxide, 0.93 times the molar amount of Sr(OH)2·8H2O was added, placed in a stainless steel reaction vessel, and purged with nitrogen gas. Distilled water was then added to make a slurry of 0.7 mol / L in terms of SrTiO3. The obtained slurry was heated to 70° C. at a rate of 8.5° C. / hour in a nitrogen atmosphere, and reacted for 5 hours after the temperature reached 70° C. After the reaction, it was cooled to room temperature, the supernatant liquid was removed, and then washing with ion-exchanged water was repeated. The slurry containing the obtained precipitate was adjusted to 40°C, and hydrochloric acid was added to adjust the pH to 2.5. Then, 1.2 parts by mass of stearic acid was added per 100 parts by mass of solid content, and stirring was continued for 10 hours. A 5 mol / L sodium hydroxide solution was added to adjust the pH to 6.5, and stirring was continued for 1 hour. Then, filtration and washing were performed, and the mixture was dried in the air at 120°C for 8 hours to obtain strontium titanate particles 3 (T-3). The number average particle size of the primary particles of the obtained strontium titanate particles 3 (T-3) was 190 nm, and the particle shape was rectangular or cubic.

[0108] <Strontium titanate particles 4 (T-4)> The titanium oxide hydrous slurry obtained by hydrolysis of the titanyl sulfate aqueous solution was washed with an alkaline aqueous solution. Next, hydrochloric acid was added to the titanium oxide hydrous slurry to adjust the pH to 1.4, and a titania sol dispersion was obtained. NaOH was added to the titania sol dispersion to adjust the pH of the dispersion to 5.3, and washing with ion-exchanged water was repeated until the electrical conductivity of the supernatant liquid reached 100 μS / cm. To the titanium oxide hydroxide, 1.07 times the molar amount of Sr(OH)2·8H2O was added, placed in a SUS reactor, and purged with nitrogen gas. Distilled water was then added to make a slurry of 0.3 mol / L in terms of SrTiO3. The obtained slurry was heated to 87° C. at a rate of 70° C. / hour in a nitrogen atmosphere, and reacted for 5 hours after the temperature reached 87° C. After the reaction, it was cooled to room temperature, the supernatant liquid was removed, and then washing with ion-exchanged water was repeated. The slurry containing the obtained precipitate was adjusted to 40°C, and hydrochloric acid was added to adjust the pH to 2.5. Then, 1.2 parts by mass of stearic acid was added per 100 parts by mass of solid content, and stirring was continued for 10 hours. A 5 mol / L sodium hydroxide solution was added to adjust the pH to 6.5, and stirring was continued for 1 hour. Then, filtration and washing were performed, and the mixture was dried in the air at 120°C for 8 hours to obtain strontium titanate particles 4 (T-4). The number average particle size of the primary particles of the obtained strontium titanate particles 4 (T-4) was 300 nm, and the particle shape was rectangular or cubic.

[0109] <Strontium titanate particles 5-8 (T-5-T-8)> Strontium titanate particles 5 to 8 (T-5 to T-8) were produced in the same manner as in the production example of strontium titanate particles 1, except that the fatty acids shown in Table 3 were used instead of stearic acid in the production example of strontium titanate particles 1.

[0110] <Strontium titanate particles 9 (T-9)> Strontium carbonate (SrCO3) equivalent to Ti was dissolved in 300 mL of titanium chloride 100 g / L (TiCl4) aqueous solution. In addition, potassium hydroxide (KOH) equivalent to the amount of chloride ions in the solution was added under a nitrogen atmosphere. The mixture was then stirred and heated at 150°C for 3 hours in an autoclave. After the reaction, the product was cooled to room temperature, the supernatant liquid was removed, and the mixture was repeatedly washed with ion-exchanged water. The slurry containing the obtained precipitate was adjusted to 40°C, and hydrochloric acid was added to adjust the pH to 2.5. Then, 1.2 parts by mass of stearic acid was added per 100 parts by mass of solid content, and stirring was continued for 10 hours. A 5 mol / L sodium hydroxide solution was added to adjust the pH to 6.5, and stirring was continued for 1 hour. Then, filtration and washing were performed, and the mixture was dried in the air at 120°C for 8 hours to obtain strontium titanate particles 9 (T-9). The number average particle size of the primary particles of the obtained strontium titanate particles 9 (T-9) was 300 nm, and the particle shape was spherical.

[0111] <Strontium titanate particles 10 (T-10)> Strontium carbonate (SrCO3) equivalent to Ti was dissolved in 300 mL of titanium chloride 100 g / l (TiCl4) aqueous solution. In addition, potassium hydroxide (KOH) equivalent to the amount of chloride ions in the solution was added under a nitrogen atmosphere. The mixture was then stirred and heated at 150°C for 3 hours in an autoclave. After the reaction, the product was cooled to room temperature, the supernatant liquid was removed, and the mixture was repeatedly washed with ion-exchanged water. The slurry containing the obtained precipitate was adjusted to 40°C, and hydrochloric acid was added to adjust the pH to 2.5. Then, 4.0 parts by mass of n-octyltriethoxysilane was added per 100 parts by mass of solid content, and stirring was continued for 10 hours. A 5 mol / L sodium hydroxide solution was added to adjust the pH to 6.5, and stirring was continued for 1 hour. Then, filtration and washing were performed, and the mixture was dried in the air at 120°C for 8 hours to obtain strontium titanate particles 10 (T-10). The number average particle size of the primary particles of the obtained strontium titanate particles 10 (T-10) was 300 nm, and the particle The shape was spherical. [Table 3] In the table, the number average particle size indicates the number average particle size of primary particles, and the fatty acid content indicates the content (parts by mass) of fatty acid on the surface of strontium titanate particles per 100 parts by mass of strontium titanate particles.

[0112] <Toner manufacturing example> <Toner 1> Toner particles 1 100.0 parts Strontium titanate particles 1 (T-1) 0.3 parts Silica particles (RX200: primary average particle size 12 nm, HMDS treatment, Nippon Aerosil Co., Ltd.) 1.5 parts The above materials were mixed by external addition using FM10C (manufactured by Nippon Coke and Engineering Co., Ltd.) The conditions for external addition were as follows: the lower blade was set to A0 blade, the gap between the deflector wall was set to 20 mm, the amount of toner particles charged was 2.0 kg, the rotation speed was 66.6 s-1, the external addition time was 10 minutes, and the cooling water temperature was 20°C and the flow rate was 10 L / min. Thereafter, the mixture was sieved through a mesh having an opening of 37 μm to obtain toner 1. The physical properties of toner 1 thus obtained are shown in Table 5.

[0113] <Toner 2-36> Toners 2 to 36 were produced in the same manner as in Production Example of Toner 1, except that in Production Example of Toner 1, the toner particles and strontium titanate particles were changed to those shown in Table 4, and the amount of strontium titanate particles added was changed to the amount shown in Table 4. The physical properties of the obtained Toners 2 to 36 are shown in Table 5.

[0114] <Toner 37> Toner 37 was produced in the same manner as in Production Example of Toner 1, except that strontium titanate particles were not added in Production Example of Toner 1. The physical properties of the obtained Toner 37 are shown in Table 5. [Table 4] [Table 5] In the table, f0 indicates the content (mass %) of fumaric acid in the toner, f1 indicates the content (mass %) of fumaric acid in the toner extracted from the toner by methanol, a0 indicates the content (mass %) of strontium titanate particles in the toner, *1 indicates the presence or absence of at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts, and *2 indicates the content (mass ppm) of at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts in the toner.

[0115] [Examples 1 to 32, Comparative Examples 1 to 5] The following evaluations were carried out using the above toners 1 to 37. The evaluation results are shown in Table 6.

[0116] The evaluation methods and evaluation criteria of the present disclosure are described below. The image forming devices used were a commercially available laser printer, LBP-712Ci (Canon), modified to have a process speed of 200 mm / sec, and a commercially available process card. The toner cartridge used was a 040H (black) (manufactured by Canon). The product toner was removed from inside the cartridge, and after cleaning with an air blower, 165 g of the toner to be evaluated was filled in. The product toner was removed from each of the yellow, magenta, and cyan stations, and the evaluation was performed by inserting a yellow cartridge, a magenta cartridge, and a cyan cartridge with the toner remaining amount detection mechanism disabled.

[0117] (Evaluation of Contamination of Electrostatically Charged Members in a Low-Temperature, Low-Humidity Environment) The image forming apparatus was left in a low-temperature, low-humidity environment (15°C / 10% RH) for 24 hours. After that, the image was printed on Canon color laser copier paper (A4: 81.4 g / m 2 ) was printed on 5,000 sheets of a horizontal line image with a print rate of 1%. Then, a toner load of 0.20 g / cm 2 Halftone images are printed on Canon Color Laser Copier Paper (A4: 81.4g / m 2 After that, the cartridge was disassembled and the surface of the charging member was observed. [Evaluation Criteria] A: No streaks are observed on the charged member or on the image. B: Slight streaks are visible on the charged member, but no streaks are visible on the image. C: Streaks are visible on the charged member, and slight streaks are also visible on the image. D: Streaks are clearly visible on the image.

[0118] (Image density evaluation in a high temperature and high humidity environment) The image forming apparatus was left in a high-temperature, high-humidity environment (30°C / 80% RH) for 24 hours. After that, the image was printed on Canon color laser copier paper (A4: 81.4 g / m 2 ) with a toner load of 0.50g / cm 2 A solid black image with a print rate of 1% was output on one sheet, which was used as an initial image sample. Then, 5,000 sheets of horizontal line images with a print rate of 1% were output continuously. Then, immediately after the 5,000 sheets were output continuously, and after the 5,000 sheets were output continuously and left for 72 hours, the toner amount was measured. 2Solid black image printed on Canon Color Laser Copier Paper (A4: 81.4g / m 2 ) one sheet was printed on each sheet. The density of the obtained images was measured, and the rate of change in density was confirmed for each sample compared to the initial image sample. The sample with the largest rate of change between the sample immediately after 5,000 continuous prints and the sample left stationary for 72 hours after 5,000 continuous prints was regarded as the image density change rate of the sample, and was evaluated according to the following criteria. [Evaluation Criteria] A: Image density change is less than 3% B: Image density change is 3% or more but less than 5% C: Image density change is 5% or more but less than 10% D: Image density change is 10% or more

[0119] <Evaluation of fogging after restarting the printer after being left for several days after long-term use in a high-temperature, high-humidity environment> The evaluation of fog was carried out as follows. As in the evaluation of image density in the high temperature and high humidity environment described above, 5,000 sheets of horizontal line images with a print rate of 1% were output continuously. After that, the power to the main unit was turned off and the unit was left in a high temperature and high humidity environment for 72 hours. After leaving it, the main unit was restarted and the unit was printed with Canon color laser copier paper (A4: 81.4 g / m 2 A piece of paper with a 5 cm x 5 cm sticky note attached was placed in the centre of the printing surface of a paper feed tray, and a solid white image was output. After the sticky note was removed, a white light meter TC-6DX (Tokyo Denshoku Co., Ltd.) was used to measure the reflectance (%) of the area where the sticky note was attached and the reflectance (%) of the area where the sticky note was not attached, and the difference between the two was calculated. This was taken as fogging (%) and was evaluated according to the following criteria. The smaller the value, the more effectively the occurrence of fogging was suppressed. The evaluation criteria are as follows: [Evaluation Criteria] A: Less than 0.5% B: 0.5% or more but less than 1.5% C: 1.5% or more and less than 3.0% D: 3.0% or more [Table 6]

[0120] The present disclosure relates to the following configurations. (Configuration 1) A toner having toner particles containing a binder resin and an external additive, the external additive comprises strontium titanate particles; the strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles, The toner contains fumaric acid, When the content of the fumaric acid in the toner is f0 (mass%), the f0 is 0.010 to 0.120 mass%, The toner, wherein when a content ratio of fumaric acid in the toner that is extracted from the toner with methanol is defined as f1 (mass %), f1 is 0.0010 to 0.0100 mass %. (Configuration 2) The toner according to configuration 1, wherein a0 (mass %) of the strontium titanate particles in the toner is 0.010 to 5,000 mass %. (Configuration 3) 3. The toner according to claim 1 or 2, wherein the fatty acid is a fatty acid having 10 to 30 carbon atoms. (Configuration 4) The toner according to any one of configurations 1 to 3, wherein the fatty acid is stearic acid. (Configuration 5) 5. The toner according to any one of configurations 1 to 4, wherein when the content of the strontium titanate particles in the toner is a0 (mass %), f0 / a0 is 0.002 to 12,000. (Configuration 6) 6. The toner according to any one of configurations 1 to 5, wherein the toner has an average circularity of 0.950 to 0.980. (Configuration 7) The toner according to any one of configurations 1 to 6, wherein the toner contains at least one selected from the group consisting of dodecylbenzenesulfonic acid and dodecylbenzenesulfonate salts.

Claims

1. A toner having toner particles containing a binder resin and an external additive, the external additive comprises strontium titanate particles; the strontium titanate particles have fatty acids on the surfaces of the strontium titanate particles, The toner contains fumaric acid, When the content of the fumaric acid in the toner is f0 (mass%), the f0 is 0.010 to 0.120 mass%, The toner is characterized in that, when a content ratio of fumaric acid in the toner that is extracted from the toner with methanol is defined as f1 (mass %), f1 is 0.0010 to 0.0100 mass %.

2. 2. The toner according to claim 1, wherein a content ratio of the strontium titanate particles in the toner is a0 (mass %), the a0 being 0.010 to 5.000 mass %.

3. 3. The toner according to claim 1, wherein the fatty acid has 10 to 30 carbon atoms.

4. 3. The toner according to claim 1, wherein the fatty acid is stearic acid.

5. 3. The toner according to claim 1, wherein when a content ratio of the strontium titanate particles in the toner is a0 (mass %), f0 / a0 is 0.002 to 12,000.

6. 3. The toner according to claim 1, wherein the toner has an average circularity of 0.950 to 0.

980.

7. 3. The toner according to claim 1, wherein the toner contains at least one selected from the group consisting of dodecylbenzenesulfonic acid and salts of dodecylbenzenesulfonic acid.

Citation Information

Patent Citations

  • Toner, developer, process cartridge, and image forming apparatus

    JP2016173396A

  • Toner

    JP2019045578A