Lead frame and manufacturing method thereof
The lead frame structure with a smooth copper surface and anodic oxide film addresses manufacturing inefficiencies and solvent spread issues, ensuring strong adhesion and cost-effective production of semiconductor packages.
Patent Information
- Application Number
- JP2023076372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-02
AI Technical Summary
Existing lead frame manufacturing methods require additional steps and equipment for forming roughening relaxation regions, increasing costs and reducing efficiency, while also facing issues with solvent spread and adhesion due to capillary action, especially in solder and die attach material connections.
A lead frame structure with a smooth surface area ratio of 1.0 to 1.3 and an anodic oxide film ratio of 1.7 to 2.3, featuring a connection plating layer surrounded by an annular smooth copper surface, formed using a high cyanide silver plating bath to prevent solvent spread and reduce manufacturing complexity.
The solution ensures excellent adhesion with sealing resin, prevents solvent spread, and reduces manufacturing costs and steps, making it suitable for efficient production of semiconductor packages.
Smart Images

Figure 2024160880000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a lead frame for use in a resin-sealed semiconductor package and a method for manufacturing the same. [Background technology]
[0002] In general, a resin-sealed semiconductor package uses a metallic lead frame and sealing resin. A copper alloy material is mainly used as the base material of the lead frame. An epoxy resin is mainly used as the sealing resin. This type of semiconductor package may have problems with adhesion between the surface of the lead frame and the sealing resin. In the case of wire bonding mounting, there is a problem that the solvent of the die attach material, which is a paste for bonding semiconductor elements to connect semiconductor elements, seeps out and the adhesion with the sealing resin is impaired. In the case of flip chip mounting, when electrical connection is made using solder, there is a problem that the solder spreads and causes a short circuit, and the spread solder further deteriorates the adhesion with the sealing resin.
[0003] Therefore, in order to improve adhesion to the sealing resin, it is known that lead frames used in resin-sealed semiconductor packages are subjected to roughening treatments such as forming an anodized film on the entire surface except for areas that require connection for connecting or conducting the semiconductor element.
[0004] For example, the following Patent Document 1 discloses a technology in which a silver plating layer is formed on the electrically joined portions, an anodized film is formed on the entire surface of the lead frame base material on which the silver plating layer is not formed, and then the silver plating layer is peeled off.
[0005] However, when a roughening treatment is applied to the surface of a lead frame, the solvent components contained in the die attach material used to fix a semiconductor element to the lead frame mounting surface tend to wet and spread over the roughened surface formed on the surface of the lead frame due to capillary action, and the wetted and spread solvent components reduce the adhesion between the lead frame and the sealing resin and may hinder wire bonding if wire bonding is performed.
[0006] However, Patent Document 2 discloses a lead frame that forms a roughened surface and then crushes part of the roughened surface to form a roughness-mitigating surface with a high degree of flatness, thereby having two types of roughened surfaces, a roughened region and a roughness-mitigating region that is flatter than the roughened region, thereby suppressing the spreading of solvent components due to capillary action, thereby suppressing a decrease in adhesion to the resin and avoiding wire bonding problems. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2021-019095 [Patent Document 2] JP 2022-103594 A Summary of the Invention [Problem to be solved by the invention]
[0008] The lead frame disclosed in Patent Document 2 is manufactured in such a manner that the lead frame shape is formed from a metal plate, a plating layer that allows for partial wire bonding is formed, a roughening treatment is then performed on the entire surface of the lead frame with the plating layer formed thereon to form a roughened region, and then a mold is used to press part of the roughened region to form a roughening mitigation region. However, the technology disclosed in Patent Document 2 requires a pressing step to form a roughness mitigating region using a mold after forming the roughened region, which increases the number of manufacturing steps and reduces manufacturing efficiency, and also requires manufacturing equipment for the pressing step using a mold, resulting in higher costs.
[0009] In addition, when solder is used for electrical connection, it is known that the joint strength is higher when soldering is performed directly to the copper material than when soldering is performed via a connection plating layer, for example, which is layered in the order of nickel plating, palladium plating, and gold plating. Therefore, there is a demand for a lead frame in which both the connection plating layer and the copper material for electrical connection are exposed at the site where soldering is performed, and which has an anodized film on the other surfaces.
[0010] The present invention has been made in consideration of the above-mentioned conventional problems, and aims to provide a lead frame and a manufacturing method thereof which does not have a roughening mitigation region, is suitable for solder connection or connection using a die attach material at connection sites for connecting or providing conductivity to semiconductor elements, has excellent adhesion to the sealing resin when resin-sealed to manufacture a semiconductor package, and can be manufactured efficiently and at low cost. [Means for solving the problem]
[0011] In order to achieve the above-mentioned object, the lead frame according to the present invention is a lead frame formed using a plate-shaped copper material having at least one side with a smooth surface, and is characterized in that it has a predetermined connection plating layer at a connection site for connecting or providing conductivity to a semiconductor element on the side with the smooth surface of the plate-shaped copper material, and has a ring-shaped exposed area around the connection plating layer, and an anodic oxide film of the copper material at other areas.
[0012] In the lead frame of the present invention, it is preferable that the surface area ratio of the smooth surface of the copper material is 1.0 to 1.3, and the surface area ratio of the anodic oxide film is 1.7 to 2.3.
[0013] In the lead frame of the present invention, the connection plating layer is preferably formed by laminating nickel plating, palladium plating, and gold plating in this order on the plate-like copper material.
[0014] A method for producing a lead frame according to the present invention includes the steps of: preparing a plate-shaped copper material having at least one side formed of a smooth surface with a surface area ratio of 1.0 to 1.3; forming a plating resist mask on the smooth side of the plate-shaped copper material, the plating resist mask having openings at locations corresponding to locations to be connected for connection and conduction of a semiconductor element as a lead frame; forming a predetermined connection plating layer on the plate-shaped copper material exposed from the openings of the plating resist mask; and covering the upper and side surfaces of the connection plating layer and plating the front and rear surfaces of the plate-shaped copper material with a silver plating bath having a property of penetrating into the interface between the plating resist mask and the connection plating layer and the interface between the plating resist mask and the plate-shaped copper material around the connection plating layer. The method includes the steps of: forming a silver plating layer to cover the plate-shaped copper material under the plating resist mask around the connection plating layer; removing the plating resist mask; forming the plate-shaped copper material with the silver plating layer formed thereon into the lead frame shape; immersing the plate-shaped copper material formed into the lead frame shape in an alkaline solution to remove an oxide film on the surface; immersing the plate-shaped copper material from which the oxide film has been removed into a blackening treatment solution as an anode to form an anodic oxide film having a surface area ratio of 1.7 to 2.3 on the portion of the plate-shaped copper material not covered with the silver plating layer; and peeling off the silver plating layer to expose the smooth surface of the copper material in a ring shape around the connection plating layer.
[0015] In the lead frame manufacturing method of the present invention, the current is 1.5 A / dm 2 It is preferable to form the anodic oxide film at a low current density of 0.1 to 1000 .mu.m or less.
[0016] In the method for producing a lead frame of the present invention, the silver plating bath is preferably a high cyanide bath.
[0017] In the method for producing a lead frame of the present invention, the connection plating layer is preferably formed by laminating nickel plating, palladium plating, and gold plating in this order on the plate-like copper material. Effect of the Invention
[0018] According to the present invention, a lead frame and a manufacturing method thereof are obtained which do not have a roughening mitigation region, are suitable for solder connection or connection using a die attach material for connecting or conducting semiconductor elements, have excellent adhesion to the sealing resin when resin-sealed to produce a semiconductor package, and can be manufactured efficiently and at low cost. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is an explanatory diagram showing an example of a lead frame for flip chip mounting manufactured by a lead frame manufacturing method according to one embodiment of the present invention, from one side, where (a) is a plan view and (b) is a partially enlarged view of (a). [Diagram 2] FIG. 1 is an explanatory diagram showing an example of a lead frame for flip chip mounting manufactured by a lead frame manufacturing method according to one embodiment of the present invention, from the other side, where (a) is a plan view and (b) is a partially enlarged view of (a). [Diagram 3] 1A to 1C are explanatory diagrams showing an example of a manufacturing process of a lead frame for flip chip mounting according to an embodiment of the present invention. [Figure 4] FIG. 1 is an explanatory diagram showing a schematic view of a lead frame for wire bonding as another example of a lead frame manufactured by a lead frame manufacturing method according to one embodiment of the present invention, where (a) is a plan view seen from one side, and (b) is a plan view seen from the other side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Prior to describing the embodiments, the circumstances under which the present invention was derived and the effects of the present invention will be described.
[0021] The technology disclosed in Patent Document 1 is a technology that was filed by the applicant of the present application and derived by inventors other than the inventors of the present application. In this technology, a metal plate is exposed in the areas where connection is required for the connection and conductivity of semiconductor elements, and an oxide film is formed on the entire surface except for the areas where connection is required. Through a process of repeated trial and error, a plating layer was considered that would not peel off the mask even when immersed in a blackening solution that forms an anodic oxide film, and that could reduce manufacturing costs, and it was decided to use a silver plating layer.
[0022] Therefore, the inventors of the present invention conducted the following studies using the technology of Patent Document 1 in order to obtain a lead frame that does not have a roughening mitigation region, is suitable for solder connection or connection using a die attach material at the connection points for connecting or conducting semiconductor elements, and has excellent adhesion to the sealing resin when sealed with resin to manufacture a semiconductor package.
[0023] First, the inventors of the present invention attempted to use the technology of Patent Document 1 to form a silver plating layer of the same size on a connection plating layer formed by stacking nickel plating, palladium plating, and gold plating in that order at a portion requiring connection, and then form an anodized film using the silver plating layer as a mask, and then remove the silver plating layer. However, with such a method, for example, an anodic oxide film comes into close proximity to the periphery of a connection plating layer laminated in a region where connection is required, and this does not solve the problem that the solvent component contained in the die attach material used to fix the semiconductor element to the lead frame mounting surface spreads due to capillary action over the roughened surface formed on the surface of the lead frame, reducing adhesion with the sealing resin. Furthermore, if a silver plating layer of the same size is formed on a connection plating layer laminated in an area where connection is required, copper ions are likely to dissolve in the blackening solution used to subsequently form an anodic oxide film on the exposed surface of the metal plate (plate-shaped copper material), and discolor the sides of the connection plating layer along with the silver plating layer. Even if the silver plating layer is removed, the peripheral edges of the connection plating layer will remain as a lead frame, reducing the suitability of the connection plating layer and significantly reducing its value as a product.
[0024] For this reason, the present inventors considered it necessary to provide a region corresponding to the roughening mitigating region described in Patent Document 2 between the connection plating layer and the anodic oxide film. However, providing a roughening relief region as described in Patent Document 2 requires a step of pressing a portion of the roughening region using a mold, which increases the number of manufacturing steps and reduces manufacturing efficiency, and also requires manufacturing equipment for the pressing step using a mold, resulting in higher costs.
[0025] Therefore, the present inventors have studied a method for preventing the spread of the solvent components contained in the die-attach material to the roughened surface of the anodized film due to capillary action without providing a roughness mitigation region. They have come to the conclusion that by forming a large silver plating layer so as to extend around the connection plating layer, and then removing the silver plating layer after forming the anodized film, a smooth surface of the lead frame base material can be provided between the connection plating layer and the anodized film, and that this smooth surface can prevent the solvent components contained in the die-attach material used for connecting semiconductor elements for connection or conduction from spreading due to capillary action to the roughened surface of the anodized film.
[0026] The present inventors then used the technology of Patent Document 1 and came up with the idea of forming a lead frame by separately forming a plating resist mask for forming the connection plating layer and a plating resist mask for forming the silver plating layer in order to form a large silver plating layer that would extend around the connection plating layer, and performed the following first prototype.
[0027] (First prototype) A copper plate (metal plate) having a thickness of 0.2 mm and smooth surfaces on both sides was prepared for a lead frame having a surface area ratio of 1.3 or less. A first plating resist mask having openings corresponding to the connection plating layer was formed on a plate-shaped copper material as a lead frame, and nickel plating, palladium plating, and gold plating were performed in that order to form the connection plating layer. The first plating resist mask was peeled off, and then a second plating resist mask was formed with an opening 20 μm wider on one side than the periphery of the formed connection plating layer, and a silver plating layer was formed on the plate-shaped copper material up to the top and side surfaces of the previously formed connection plating layer and an area of 20 μm around the connection plating layer, and the second plating resist mask was peeled off. Next, an etching resist mask having an opening in the shape of a predetermined lead frame was formed on the plate-shaped copper material on which the silver plating layer was formed, and etching was performed to form the lead frame shape. Next, the etching resist mask was removed, and the surface of the plate-like copper material formed into the lead frame shape was washed with an alkaline solution in order to promote the growth of the anodic oxide film. Next, the plate-like copper material formed into a lead frame shape was immersed in a blackening treatment solution as an anode, and an anodic oxide film with a surface area ratio of 1.7 to 2.3 was formed on the surface of the plate-like copper material on which the silver plating layer was not formed. Then, by peeling off the silver plating layer, a lead frame was obtained which had a connection plating layer in the areas where connection was required, a ring-shaped area where the smooth surface of the copper material was exposed around the connection plating layer, and an anodized film of the copper material in other areas. When an anodic oxide film is formed using a blackening solution, short needle-like crystals are formed at a high current density, and the surface area ratio is less than 1.5. However, when it is formed at a low current density, the oxide film is a mixture of long and short needle-like crystals, and the surface area ratio is 1.7 or more. In this prototype, the current density was 1.5 A / dm 2 The anodic oxide film was formed at the following current density.
[0028] In the first prototype, it was confirmed that a lead frame could be obtained that could prevent the solvent components contained in the die attach material from spreading due to capillary action to the roughened surface forming the anodized film without providing a roughness mitigation region. However, this requires a process of separately forming the first plating resist mask and the second plating resist mask, and it has been found that adding the process of forming the second plating resist mask increases the manufacturing cost and makes it difficult to adopt this method for mass production.
[0029] Therefore, the present inventors have investigated a method for forming a large silver plating layer so as to extend over the periphery of the connection plating layer without forming a plating resist mask twice. During the course of their investigations, the inventors of the present invention noted that high cyanide silver plating baths generally tend to deteriorate resist masks and are therefore unsuitable for partial plating, and considered that by taking advantage of the property of high cyanide silver plating baths that they tend to deteriorate resist masks when performing partial plating, it might be possible to allow silver plating solution to penetrate into the interface between the plating resist mask and the connection plating layer, and into the interface between the plating resist mask and the plate-like copper material around the connection plating layer. It was thought that if the silver plating solution could seep into the gap between the side of the connection plating layer and the side of the resist mask, and further under the resist mask, the copper material around the connection plating layer could be partially (partially) covered with silver plating, thereby preventing discoloration of the connection plating layer due to contamination by copper ions that dissolve into the blackening solution when forming the anodized film, and obtaining a lead frame that can prevent the solvent components contained in the die attach material from spreading due to capillary action to the roughened surface forming the anodized film.
[0030] (Second prototype) Therefore, as a second prototype, the inventors prepared a plate-shaped copper material similar to that of the first prototype, formed a similar first plating resist mask on the plate-shaped copper material, and plated it in the order of nickel plating, palladium plating, and gold plating to form a connection plating layer, and then formed a silver plating layer using a high cyan silver plating bath without peeling off the first resist mask. After forming the silver plating layer, a lead frame shape was formed in the same manner as in the first prototype, an anodic oxide film was formed, and the silver plating layer was peeled off to obtain a lead frame. The lead frame produced by the second prototype had a connection plating layer in the area where connection was required, and the smooth surface of the copper material was exposed around the connection plating layer in a ring shape, with an anodic oxide film of the copper material formed in other areas. In addition, the peripheral area of the connection plating layer was not contaminated by copper ions, and no discoloration was observed. As a result, the inventors of the present invention have confirmed that if a silver plating layer is formed using a high-cyan silver plating bath while using the same resist mask used to form the connection plating layer, a silver plating layer will be formed over a wider area than the connection plating layer, which is formed as a plating layer below the silver plating layer using the same plating resist mask. This is thought to be a phenomenon in which the silver plating solution penetrates into the interface between the plating resist mask and the connection plating layer, and into the interface between the plating resist mask and the plate-like copper material around the connection plating layer, forming a silver plating layer. In the second prototype, the silver plating layer was formed to a thickness of 1 μm, and the resist mask was made to be 25 μm thick. Furthermore, the copper material exposed around the connecting plating layer had a smooth surface exposed in a ring shape with a width of approximately 5 to 20 μm.
[0031] As a result of this trial and error, the inventors were able to confirm that it is possible to obtain a lead frame that can prevent discoloration due to copper ion contamination of the peripheral edges of the connection plating layer provided in areas where connection is required, without providing a roughening mitigation region or using a second plating resist mask, and that can prevent the solvent components contained in the die attach material used to connect semiconductor elements from spreading due to capillary action to the roughened surface forming the anodized film, and thus derive the lead frame and its manufacturing method of the present invention.
[0032] The lead frame of the present invention is a lead frame formed using a plate-shaped copper material having at least one side with a smooth surface, and has a predetermined connection plating layer at a connection site for connecting or providing electrical continuity to a semiconductor element on the side with the smooth surface of the plate-shaped copper material, and has a ring-shaped exposed area around the connection plating layer, and an anodic oxidation film of the copper material at other areas. If the lead frame of the present invention is configured to have a ring-shaped exposed smooth surface of copper material around a predetermined connection plating layer provided at a portion for connection or conduction of a semiconductor element, and an anodized film of copper material is provided at other portions, the smooth surface between the connection plating layer and the anodized film can prevent the solvent component contained in the die attach material used to connect the connection plating layer and the semiconductor element from penetrating due to the capillary phenomenon of the anodized film, thereby achieving excellent adhesion with the sealing resin when the semiconductor package is manufactured by resin sealing. Furthermore, as in the lead frame of the present invention, if a configuration is adopted in which a smooth surface of the copper material is exposed in a ring shape around a specified connection plating layer provided at a connection portion for connecting or providing electrical continuity to a semiconductor element, the smooth surface of the plate-shaped copper material used to manufacture the lead frame can be used as is, and a pressing process for forming a roughening mitigating region using a mold after forming a roughened surface as in Patent Document 2 is not required. This reduces the number of manufacturing steps, improves manufacturing efficiency, and obviates the need for manufacturing equipment, thereby reducing costs.
[0033] In the lead frame of the present invention, the surface area ratio of the smooth surface of the copper material is preferably 1.0 to 1.3, and the surface area ratio of the anodic oxide film is preferably 1.7 to 2.3. With this configuration, the sealing resin has excellent adhesion, and the solvent components contained in the die attach material used to connect the semiconductor element can be prevented from spreading to the anodized film.
[0034] In the lead frame of the present invention, the connection plating layer is preferably formed by laminating nickel plating, palladium plating, and gold plating in this order on the plate-like copper material. By configuring in this manner, the lead frame of the present invention can be realized in which both the connection plating layer and the copper material for electrical connection are exposed at the site where solder bonding is performed to connect the semiconductor element, and the other surfaces are provided with an anodized film.
[0035] The method for producing a lead frame of the present invention includes the steps of: preparing a plate-shaped copper material having at least one side formed of a smooth surface with a surface area ratio of 1.0 to 1.3; forming a plating resist mask having openings at locations corresponding to locations to be connected for connection and conduction of a semiconductor element as a lead frame on the side formed of the smooth surface of the plate-shaped copper material; forming a predetermined connection plating layer on the plate-shaped copper material exposed from the openings of the plating resist mask; and covering an upper surface and a side surface of the connection plating layer with a silver plating bath having a property of penetrating an interface between the plating resist mask and the connection plating layer and an interface between the plating resist mask and the plate-shaped copper material around the periphery of the connection plating layer. In addition, the method includes the steps of forming a silver plating layer that covers the plate-shaped copper material under the plating resist mask around the connection plating layer, removing the plating resist mask, forming the plate-shaped copper material with the silver plating layer formed thereon into the lead frame shape, immersing the plate-shaped copper material formed into the lead frame shape in an alkaline solution to remove an oxide film on the surface, immersing the plate-shaped copper material from which the oxide film has been removed into a blackening treatment solution as an anode to form an anodic oxide film having a surface area ratio of 1.7 to 2.3 on the portion of the plate-shaped copper material that is not covered with the silver plating layer, and peeling off the silver plating layer to expose the smooth surface of the copper material in a ring shape around the connection plating layer. With this configuration, a smooth surface of the copper material is exposed in a ring shape around the connection plating layer provided in the area where connection is required for connection and conduction of the semiconductor element, and an anodic oxide film of the copper material can be formed in other areas, and discoloration due to contamination by copper ions on the periphery of the connection plating layer can be prevented without providing a roughness mitigation region as in the technology described in Patent Document 2. Furthermore, in the manufacturing process, there is no need to form separate plating resist masks for forming the connection plating layer and the silver plating layer, and the same plating resist mask can be used for both. As a result, it is possible to obtain a lead frame that is suitable for solder connections or connections using die attach materials at connection sites for connecting or providing electrical continuity to semiconductor elements, has excellent adhesion to the sealing resin when resin-sealed to produce a semiconductor package, and can be manufactured efficiently and at low cost.
[0036] In the lead frame manufacturing method of the present invention, preferably, 2 The anodic oxide film is formed at a low current density as follows: By configuring it in this manner, an oxide coating is formed that is a mixture of long and short needle-shaped crystals, and an anodic oxide film with a surface area ratio of 1.7 or more is obtained, which prevents the anodic oxide film from peeling off and improves adhesion to the sealing resin.
[0037] In the method for producing a lead frame of the present invention, the silver plating bath is preferably a high cyanide bath. By configuring in this manner, it is possible to realize a silver plating bath that has the property of penetrating into the interface between the plating resist mask and the connection plating layer, and into the interface between the plating resist mask and the plate-shaped copper material around the connection plating layer, in the lead frame manufacturing method of the present invention.
[0038] In the method for producing a lead frame of the present invention, the connection plating layer is preferably formed by laminating nickel plating, palladium plating, and gold plating in this order on the plate-like copper material. By configuring in this manner, the manufacturing method of the lead frame of the present invention can be realized in which both the connection plating layer and the copper material are exposed at the areas where solder bonding is performed and where a semiconductor element is mounted, and an anodized film is provided on the other surfaces.
[0039] Therefore, according to the present invention, a lead frame and a manufacturing method thereof can be obtained which do not have a roughening mitigation region, are suitable for solder connection or connection using a die attach material at connection sites for connecting or providing conductivity to semiconductor elements, have excellent adhesion to the sealing resin when resin-sealed to produce a semiconductor package, and can be manufactured efficiently and at low cost. It is preferable to perform soft etching before forming the connection plating layer to obtain an etching depth of less than 5 μm, since this makes it easier to hold the solder during solder reflow.
[0040] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The lead frame according to this embodiment is a lead frame formed of a plate-like copper material having at least one smooth surface, and has a predetermined connection plating layer at a portion of the smooth surface of the plate-like copper material to be connected for connection or conduction of a semiconductor element, and has a ring-shaped portion where the smooth surface of the copper material is exposed around the connection plating layer, and has an anodic oxide film of the copper material at other portions. The present invention can be applied to lead frames having various shapes, and the shape of the lead frame is not particularly limited, but for convenience, the lead frame shape shown in Figures 1 and 2 will be used as an example for explanation.
[0041] The lead frame 1 shown in FIG. 1 and FIG. 2 is made of copper or copper alloy as a strip-shaped metal material, and is formed into a predetermined shape by etching or pressing a plate-like copper material 10 having smooth surfaces on both sides. A connection plating layer 11 is formed on each of a portion electrically connecting to a semiconductor element on the upper surface side of the lead frame base material and a portion connecting to an external device on the lower surface side, in which a nickel plating layer, a palladium plating layer, and a gold plating layer are laminated in this order. The connection plating layer 11 has a portion 10a where the smooth surface of the copper material is exposed in a ring shape around it. In addition, an anodic oxide film 13 of the copper material is formed on the other portions of the connection plating layer 11 and the portion 10a where the smooth surface of the copper material is exposed in a ring shape. The anodic oxide film 13 is made of a single layer film of a mixture of cuprous oxide (Cu2O), cupric oxide (CuO), and cupric hydroxide (Cu(OH)2), and the single layer film is made of a copper oxide coating having a needle-like crystal structure with an average length of 200 nm or more.
[0042] Next, a method for manufacturing the lead frame of this embodiment configured as shown in Figures 1 and 2 will be described with reference to Figure 3. For convenience, a partial view will be used in Figure 3. In the manufacturing method of this embodiment, first, a strip-shaped metal material made of copper or a copper alloy and a plate-shaped copper material 10 having smooth surfaces with a surface area ratio of 1.0 to 1.3 on both sides is prepared as a lead frame material (see FIG. 3(a)). Next, a resist layer R1 such as a dry film resist is formed on both sides of the plate-like copper material 10 (see FIG. 3(b)). Next, a glass mask is used in which a pattern corresponding to an opening as a portion that will be electrically connected to an electrode of a semiconductor element in flip-chip mounting is drawn on the upper resist layer R1, and a pattern corresponding to an opening as a portion that will be electrically connected to an external device is drawn on the lower resist layer R1. The resist layers R1 on both sides are then exposed and developed to form a plating resist mask 30 (see FIG. 3(c)). Next, a connection plating layer 11 is formed by layering nickel plating, palladium plating, and gold plating in that order on the surface of the plate-shaped copper material 10 exposed from the openings in the plating resist mask 30 (see Figures 3(d) and 3(d')). Next, a silver plating bath (e.g., a high cyan plating bath) having the property of penetrating into the interface between the plating resist mask 30 and the connection plating layer 11 and into the interface between the plating resist mask 30 and the plate-like copper material 10 around the connection plating layer 11 is used to form a silver plating layer 12 that covers the upper and side surfaces of the connection plating layer 11 and also covers the plate-like copper material under the plating resist mask 30 around the connection plating layer 11 (see Figures 3(e) and 3(e')).
[0043] Next, the plating resist mask 30 is removed (see FIG. 3(f)). Next, a resist layer R2 such as a dry film resist is formed on both sides of the plate-like copper material 10 on which the connection plating layer 11 and the silver plating layer 12 have been formed (see FIG. 3(g)). Next, the resist layers R2 on both sides are exposed and developed using a glass mask on which a pattern of a predetermined lead frame shape is drawn, to form an etching resist mask 31 (see FIG. 3(h)). Next, an etching process is performed using an etching solution, and the plate-like copper material 10 on which the silver plating layer 12 is partially formed is formed into a predetermined lead frame shape (see FIG. 3(i)). Next, the etching resist mask 31 is removed (see FIG. 3(j)). As a result, on the top surface of the plate-shaped copper material 10, a connection plating layer 11 is formed in the area electrically connecting to the electrode of the semiconductor element, and a silver plating layer 12 is formed on the top and side surfaces of the connection plating layer 11 and around the connection plating layer 11, while on the bottom surface, a connection plating layer 11 is formed in the area electrically connecting to an external device, and a silver plating layer 12 is formed on the top and side surfaces of the connection plating layer 11 and around the connection plating layer 11, and a smooth surface is exposed over the entire surface of the other areas.
[0044] Next, a plate-shaped copper material (lead frame substrate) 10 partially formed with a silver plating layer 12 is immersed in a blackening treatment solution, and an electric current is passed through the lead frame substrate 10 using the metal plate as the anode, thereby forming an anodic oxide film 13 with a surface area ratio of 1.7 to 2.3 on the entire surface of the lead frame substrate 10 except for the area where the silver plating layer 12 covering the connection plating layer 11 is formed (see Figures 3(k) and 3(k')). Next, the silver plating layer 12 is peeled off to expose the smooth surface of the copper material 10 in an annular shape around the connection plating layer 11 (see FIG. 3(l) and FIG. 3(l')). This results in a lead frame having a connection plating layer 11 at portion 10, which is connected for connecting and providing electrical continuity to the semiconductor element, as shown in Figures 1 and 2, and having a ring-shaped portion 10a where the smooth surface of the copper material is exposed around the portion having connection plating layer 11, and having an anodic oxide film 13 formed on the entire other surface.
[0045] The lead frame of this embodiment can be applied to the lead frame 1 for flip chip mounting shown in FIG. 1 and FIG. 2, as well as the lead frame 1 for wire bonding connection as shown in FIG. 4. The lead frame 1 shown in FIG. 4 has a connection plating layer 11 formed by laminating a nickel plating layer, a palladium plating layer, and a gold plating layer in this order at a portion of the pad portion located at the center of the upper surface side of the lead frame base material, which is connected to a semiconductor element via a die attachment material, a portion of the lead portion located around the pad portion, which is electrically connected to an electrode of the semiconductor element by wire bonding, and a portion of the lower surface side, which is connected to an external device. The connection plating layer 11 in the pad portion has a portion 10a where the smooth surface of the copper material is exposed in a ring shape around it. An anodic oxide film 13 of copper material is formed on the other portions of the connection plating layer 11 and the portion 10a where the smooth surface of the copper material is exposed in a ring shape on the upper surface side of the pad portion, and on the entire back surface side of the pad portion. The other configurations are substantially the same as those of the lead frame 1 for flip chip mounting shown in FIG. 1 and FIG. 2.
[0046] According to the lead frame 1 of this embodiment, the connection plating layer 11 is provided at the portion to be connected for connection and conduction of the semiconductor element, and the smooth surface of the copper material 10 is exposed in a ring shape at the periphery of the portion provided with the connection plating layer 11 at the portion provided with the connection plating layer 11 at the portion provided with the anodized film 13 of the copper material 10. Therefore, the smooth surface between the connection plating layer 11 and the anodized film 13 improves the bonding strength of the solder used for electrical connection with the connection plating layer 11, and can prevent the solvent component contained in the die attach material used for mounting the semiconductor element from penetrating due to the capillary phenomenon of the anodized film 13. This can provide excellent adhesion to the sealing resin when the semiconductor package is manufactured by resin sealing.
[0047] Furthermore, according to the lead frame 1 of this embodiment, the smooth surface of the copper material 10 is exposed in a ring shape around the portion having the connection plating layer 11 provided at the portion to be connected for connection and conductivity of the semiconductor element. Therefore, the smooth surface of the plate-shaped copper material 10 used to manufacture the lead frame can be used as is, and a pressing process for forming a roughening mitigating region using a mold after forming a roughened surface as in Patent Document 2 is not required. As a result, the manufacturing process is reduced, improving manufacturing efficiency, and manufacturing equipment is not required, thereby reducing costs.
[0048] Furthermore, according to the lead frame 1 of this embodiment, the surface area ratio of the smooth surface of the copper material 10 is 1.0 to 1.3, and the surface area ratio of the anodized film 13 is 1.7 to 2.3, which provides excellent adhesion to the sealing resin, improves the bonding strength of the solder used in the electrical connection parts, and prevents the solvent components contained in the die attach material used to mount the semiconductor element from spreading to the anodized film.
[0049] Furthermore, according to the lead frame 1 of this embodiment, the connection plating layer 11 is configured to be composed of a plating layer formed by laminating nickel plating, palladium plating, and gold plating in that order on the plate-shaped copper material 10, so that a lead frame can be realized in which both the connection plating layer and the copper material are exposed at the site where solder bonding or bonding with a die attach material is performed, and which has an anodized film on the other surfaces.
[0050] Furthermore, according to the manufacturing method of the lead frame 1 of this embodiment, the steps include the steps of: preparing a plate-shaped copper material 10 having smooth surfaces on both sides with a surface area ratio of 1.0 to 1.3; forming a plating resist mask 30 having openings on the smooth surfaces of the plate-shaped copper material 10 in areas corresponding to areas to be electrically connected as a lead frame; forming a connection plating layer 11 on the plate-shaped copper material 10 exposed from the openings of the plating resist mask 30; and forming a silver plating layer 12 that covers the upper and side surfaces of the connection plating layer 11 and covers the plate-shaped copper material 10 under the plating resist mask 30 around the connection plating layer 11 using a high cyan silver plating bath having a property of penetrating into the interface between the plating resist mask 30 and the connection plating layer 11 and the interface between the plating resist mask 30 and the plate-shaped copper material 10 around the connection plating layer 11. The method includes the steps of removing the plating resist mask 30, forming the plate-shaped copper material 10 having the silver plating layer 12 formed thereon into a lead frame shape, immersing the plate-shaped copper material 10 formed into the lead frame shape in an alkaline solution to remove the oxide film on the surface, immersing the plate-shaped copper material 10 formed into the lead frame shape from which the oxide film has been removed into a blackening treatment solution as an anode to form an anodic oxide film 13 having a surface area ratio of 1.7 to 2.3 in the areas of the plate-shaped copper material 10 formed into the lead frame shape that are not covered by the silver plating layer 12, and peeling off the silver plating layer 12 to expose the smooth surface of the copper material 10 in a ring shape around the connection plating layer 11. This makes it possible to prevent discoloration of the peripheral area of the connection plating layer provided in the area where connection is required due to contamination with copper ions, without providing a roughening mitigation area as in the technology described in Patent Document 2. Furthermore, in the manufacturing process, it is not necessary to form separate plating resist masks for forming the connection plating layer and the silver plating layer, and the same plating resist mask can be used for both. As a result, it is possible to obtain a lead frame that is suitable for solder connection or connection using die attach material, has excellent adhesion to the sealing resin when resin-sealed to produce a semiconductor package, and can be manufactured efficiently and at low cost.
[0051] In addition, according to the manufacturing method of the lead frame 1 of this embodiment, 2The anodized film is formed at a low current density of 1.7 or less, resulting in an oxide coating that is a mixture of long and short needle-shaped crystals, and an anodized film with a surface area ratio of 1.7 or more is obtained. As a result, the anodized film does not peel off, and the adhesion to the sealing resin can be improved.
[0052] Furthermore, according to the manufacturing method of the lead frame 1 of this embodiment, a high cyanide bath is used for the silver plating bath, so that it is possible to realize a silver plating bath that has the property of penetrating into the interface between the plating resist mask 30 and the connection plating layer 11, and into the interface between the plating resist mask 30 and the plate-shaped copper material 10 around the connection plating layer 11.
[0053] Furthermore, according to the manufacturing method of the lead frame 1 of this embodiment, the connection plating layer 11 is formed by layering nickel plating, palladium plating, and gold plating in that order on the plate-shaped copper material 10, thereby realizing a manufacturing method of a lead frame in which both the connection plating layer and the copper material are exposed at the site where the semiconductor element is connected or soldered, for electrical connection, and the other surfaces are provided with an anodized film.
[0054] Therefore, according to this embodiment, a lead frame and a manufacturing method thereof can be obtained which do not have a roughening mitigation region, are suitable for solder connection or connection using a die attach material at connection sites for connecting or providing conductivity to semiconductor elements, have excellent adhesion to the sealing resin when resin-sealed to manufacture a semiconductor package, and can be manufactured efficiently and at low cost.
[0055] Example 1 A copper material (Furukawa Electric: EFTEC64T) with a thickness of 0.2 mm was prepared as the metal plate for the lead frame. The surface area ratio of the metal plate was 1.1. (Olympus short wavelength laser microscope OLS-4100) A dry film resist having a thickness of 25 μm was laminated on the surface of the prepared metal plate to form a resist layer. Next, a glass mask was used on the upper resist layer, on which a pattern corresponding to an opening of approximately φ0.1 mm as the portion corresponding to the portion to be electrically connected to the electrode of the semiconductor element was drawn, and on the lower resist layer, on which a pattern corresponding to an opening of approximately φ0.3 mm as the portion corresponding to the portion to be electrically connected to an external device was drawn.The resist layers on both sides were then exposed and developed to form a resist mask for plating. Next, a 1 μm thick nickel plating layer was formed on the metal plate exposed through the openings in the plating resist mask, followed by a 0.03 μm thick palladium plating layer and finally a 0.003 μm thick gold plating layer to form a plating layer for electrical connection. Next, using a high-cyanide silver plating bath containing silver cyanide and potassium cyanide as its main components, a silver plating layer of approximately 1 μm was formed by electrolytic plating on the metal plate exposed from the openings in the plating resist mask, and the plating resist mask was then removed. Next, the same dry film resist was laminated on both sides of the metal plate on which the silver plating layer was formed to form a resist layer. Next, the resist layers on both sides were exposed and developed using a glass mask on which a pattern of a predetermined lead frame shape was drawn, to form a resist mask for etching. Next, spray etching was carried out using a ferric chloride solution, and the metal plate on which the silver plating layer was partially formed was formed into a predetermined lead frame shape, and the etching resist mask was then removed. Next, the metal plate formed into a predetermined lead frame shape was immersed in a commercially available blackening treatment solution, which is an alkaline solution, with the concentration set to 90 ml / l, the solution temperature set to room temperature, and the treatment time set to 60 seconds. Next, using the same commercially available blackening solution, the concentration was 90 ml / l, the solution temperature was 70°C, the treatment time was 2.5 minutes, and the current density was 0.5 A / dm 2 The metal plate was used as the anode and an anodic oxide film was formed on the entire surface by immersion treatment under the settings of 1. Next, the silver plating layer contaminated by copper ions in the blackening treatment solution was stripped using a commercially available stripping solution. The silver plating layer was peeled off to obtain a lead frame in which a nickel plating layer, a palladium plating layer, and a gold plating layer were laminated as connection plating layers, with the metal plate exposed in an area of approximately 5 to 20 μm around it, and an anodized film formed on the entire surface of the metal plate formed into the remaining specified lead frame shape. The surface area ratio of the formed anodic oxide film was 1.7 to 2.3. In addition, no discoloration due to contamination by copper ions in the blackening solution used in the process of forming the anodic oxide film was observed in the peripheral portion of the connection plating layer, confirming that it was a good quality product. The current density for forming the anodic oxide film used in Example 1 was 0.3 to 1.5 A / dm 2 An immersion time of 1 to 5 minutes is considered to be suitable.
[0056] Comparative Example 1 A lead frame of Comparative Example 1 was obtained using the same materials and manufacturing procedures as in Example 1, except that a low-cyan silver plating bath was used as the plating bath for forming the silver plating layer. The lead frame of Comparative Example 1 was found to have discoloration due to contamination by the blackening solution on the peripheral portion of the connection plating layer, and was therefore confirmed to be unsuitable for use as a product. In addition, an anodic oxide film was formed in close proximity to the connection plating layer, and no area where the smooth surface of the metal plate was exposed was formed around the connection plating layer, as in the lead frame of Example 1, and it was found that the connection plating layer was not suitable for solder connection or mounting of semiconductor elements. [Industrial Applicability]
[0057] The lead frame of the present invention is useful in fields requiring lead frames used in the manufacture of semiconductors sealed with sealing resin, and is useful not only for lead frames in which the connection sites for connecting or conducting semiconductor elements are provided with a plating layer, but also for lead frames in which a metal plate such as a plate-shaped copper material constitutes a site for electrical connection as is. [Explanation of symbols]
[0058] 1 Lead Frame 10 Lead frame substrate (metal plate, copper plate) 10a: A circular area where the smooth surface of the copper material is exposed 11 Connection plating layer 12 Silver plating layer 13 Anodic oxide film 30 Plating resist mask 31 Etching resist mask R1, R2 resist layer
Claims
1. A lead frame formed using a plate-shaped copper material having at least one side with a smooth surface, characterized in that the lead frame has a predetermined connection plating layer at a connection site for connecting or providing electrical continuity to a semiconductor element on the side with the smooth surface of the plate-shaped copper material, a ring-shaped area where the smooth surface of the copper material is exposed around the connection plating layer, and an anodic oxide film of the copper material at other areas.
2. 2. The lead frame according to claim 1, wherein the surface area ratio of the smooth surface of the copper material is 1.0 to 1.3, and the surface area ratio of the anodic oxide film is 1.7 to 2.
3.
3. 3. The lead frame according to claim 1, wherein the connection plating layer is formed by laminating nickel plating, palladium plating, and gold plating in this order on the copper plate.
4. A step of preparing a plate-shaped copper material having at least one side formed of a smooth surface with a surface area ratio of 1.0 to 1.3; forming a plating resist mask on the smooth surface of the plate-like copper material, the plating resist mask having openings at locations corresponding to locations for connection or conduction of a semiconductor element as a lead frame; forming a predetermined connection plating layer on the plate-like copper material exposed through the openings of the plating resist mask; forming a silver plating layer that covers an upper surface and a side surface of the connection plating layer and covers the plate-like copper material under the plating resist mask around the connection plating layer, using a silver plating bath having a property of penetrating into an interface between the plating resist mask and the connection plating layer and an interface between the plating resist mask and the plate-like copper material around the connection plating layer; removing the plating resist mask; forming the plate-shaped copper material having the silver plating layer formed thereon into the lead frame shape; a step of immersing the plate-like copper material formed into the lead frame shape in an alkaline solution to remove an oxide film on the surface; a step of immersing the plate-shaped copper material from which the oxide film has been removed in a blackening treatment solution as an anode to form an anodic oxide film having a surface area ratio of 1.7 to 2.3 on the portion of the plate-shaped copper material that is not covered with the silver plating layer; peeling off the silver plating layer to expose the smooth surface of the copper material in an annular shape around the connection plating layer; A method for manufacturing a lead frame comprising the steps of:
5. 1.5A / dm 2 5. The method of claim 4, wherein the anodic oxide film is formed at a current density as low as or less than 100 .mu.m.
6. 5. The method for producing a lead frame according to claim 4, wherein the silver plating bath is a high cyanide bath.
7. 5. The method for producing a lead frame according to claim 4, wherein the connection plating layer is formed by laminating nickel plating, palladium plating, and gold plating in this order on the plate-like copper material.
Citation Information
Patent Citations
Manufacturing method of lead frame
JP2016105432A
Manufacturing method of multi-row lead frame
JP2021019095A
Lead frame, lead frame manufacturing method, and semiconductor device