Powder coating composition, coating film, and coated body

The powder coating composition addresses separation issues between resin and glitter pigments by using a binder with specific solubility parameters and a high Tg solvent, achieving glossy and recyclable coatings with consistent film appearance and workability.

JP2024161264AInactive Publication Date: 2024-11-15DAI NIPPON TORYO CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024153861
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing powder coating compositions using fluororesins and glitter pigments face issues such as separation between resin powder and glitter pigment during electrostatic coating, leading to deteriorated film design, color tone changes, and difficulty in recycling due to solvent compatibility problems with terpene-based resins and fluoro-based halogen-containing solvents, which affect coating workability and film appearance.

Method used

A powder coating composition is developed using a binder with specific Hansen solubility parameters (δd, δp, δh) = (19.0, 7.0, 5.0) and an interaction distance R, dissolved in a solvent with a Tg of 20°C or higher, allowing for glossy and glittering coatings with improved reusability by bonding various resin-containing powder particles without increasing particle size.

Benefits of technology

The composition forms a glossy coating film with excellent glitter properties and enhances recyclability by preventing resin particle agglomeration, maintaining coating workability, and ensuring consistent film appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161264000001_ABST
    Figure 2024161264000001_ABST
Patent Text Reader

Abstract

To provide a powder coating composition or the like that is capable of forming a coating film having gloss and excellent brilliance and that also has excellent recyclability.SOLUTION: A powder coating composition according to the present invention contains resin-containing powder particles (A), a brilliant pigment (B), and a binder (C), and the binder (C) is a resin that dissolves or disperses in a solvent (D) the interaction distance Ra of which is 20 or more when the center coordinates (δd, δp, δh) are taken to be (19.0, 7.0, 5.0) in a Hansen solubility sphere HSS for determining solubility with mixed solvents, that has a Tg of 30°C or more, and that has a weight-average molecular weight of 1,000-100,000.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder coating composition, a coating film, and a coated body. [Background technology]

[0002] Conventionally, as a powder coating material having weather resistance and adhesion to a substrate, a thermosetting powder coating material containing a fluororesin, a non-fluororesin, and a pigment has been known. When a glittering pigment is used as the pigment in this powder coating material, a coating film having glittering properties can be formed (see, for example, Patent Document 1). For example, an electrostatic powder coating method is used as a method for forming the coating film.

[0003] Generally, the resin powder and the luster pigment (e.g., metal pigment) constituting the powder coating material have a large difference in electrostatic charge rate. Therefore, when electrostatic powder coating is performed using a powder coating material containing a resin powder and a luster pigment, a separation phenomenon is likely to occur between the resin powder and the luster pigment during coating. When this separation phenomenon occurs, there is a problem that the design of the resulting coating film is likely to deteriorate. In addition, when the above-mentioned separation phenomenon occurs, the pigment content of the powder coating material is likely to change before and after coating. When this pigment content changes, the color tone is likely to change between the coating film obtained using the powder coating material after recovery and reuse and the coating film obtained using the powder coating material before reuse, which makes it difficult to recycle (recover and reuse) the powder coating material.

[0004] In response to this, various proposals have been made in the past. For example, Patent Document 2 and Patent Document 3 disclose a method (bonding method) in which the surface of the thermosetting resin powder and the luster pigment are attached with a binder having adhesiveness in order to avoid the separation phenomenon between the thermosetting resin powder and the metal pigment. In addition, the examples of Patent Document 2 and Patent Document 3 disclose the use of a terpene-based resin as a binder.

[0005] Furthermore, Patent Document 4 discloses a bonding method for resin powder, particularly fluororesin powder. Specifically, Patent Document 4 discloses a powder coating material containing resin powder including fluororesin and non-fluororesin, a luster pigment, and a binder, and a method for adhering the surface of a thermosetting resin powder to the luster pigment using a binder made of a surfactant having a melting point of 25° C. or higher. An example of Patent Document 4 discloses the use of a fluoro-based halogen-containing solvent as a solvent for the binder. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2011-12119 A [Patent Document 2] JP 2004-175813 A [Patent Document 3] Patent No. 3926270 [Patent Document 4] Patent No. 6841235 Summary of the Invention [Problem to be solved by the invention]

[0007] When the terpene resin used in the examples of Patent Document 2 and Patent Document 3 is used as a binder with adhesive properties, it is necessary to dissolve the terpene resin in a low-polarity solvent such as n-heptane. However, these low-polarity solvents generally dissolve fluororesin as well, and therefore problems are likely to occur when used with thermosetting resin powder particles containing fluororesin. Specifically, when the above-mentioned low-polarity solvent is used with thermosetting resin powder particles containing fluororesin, a part of the fluororesin dissolves and the thermosetting resin powder particles bond together, which may increase the particle size of the thermosetting resin powder, reduce the ease of painting, or deteriorate the appearance of the coating film.

[0008] In addition, the fluoro-based halogen-containing solvent used in the examples of Patent Document 4 generally dissolves fluororesin. Therefore, when the above-mentioned fluoro-based halogen-containing solvent is used for thermosetting resin powder particles containing fluororesin, there is a risk that the particle size of the thermosetting resin powder increases, the coating workability decreases, and the appearance of the coating film deteriorates, as in the case of using the low-polarity solvents of Patent Documents 2 and 3.

[0009] When the powder coating material contains a resin having a carboxyl group, the use of the binders disclosed in Patent Documents 2 to 4 can cause a problem that the gloss of the coating film appearance is likely to decrease.

[0010] In a powder coating composition for a bonding method containing resin-containing powder particles, a luster pigment, and a binder, it is desired to contain a solvent that dissolves the binder but does not dissolve the resin of the resin-containing powder particles. In contrast, the powder coating compositions disclosed in Patent Documents 2 to 4 can only be used in a bonding method when they relate to a combination of a specific resin and a specific binder. In the industry, from the viewpoint of the degree of freedom in designing a powder coating composition, a bonding method that can be widely applied to various types of resin-containing powder particles is desired.

[0011] The present invention has been made in view of the above problems, and aims to provide a powder coating composition capable of forming a coating film having a gloss and excellent brilliance, and also having excellent recoverability and reusability. Another aim of the present invention is to provide a coating film and a coated body formed using the powder coating composition. [Means for solving the problem]

[0012] The present inventors have determined the Hansen solubility parameter (HSP) (δ d , δ p , δ h ) to form a specific Hansen melting sphere, and the binder is the interaction distance R aThe present inventors have succeeded in developing a powder coating composition that is capable of forming a coating film having a high gloss and excellent brilliance and that is also easily recyclable and reusable, when the resin is soluble or dispersible in 20 or more solvents, and have thus completed the present invention.

[0013] (1) The powder coating composition according to the present invention is a powder coating composition containing resin-containing powder particles (A), a luster pigment (B) and a binder (C), and the binder (C) has a central coordinate (δ) in the Hansen Solubility Sphere (HSS) which determines the solubility of the binder with a solvent to be mixed. d , δ p , δ h ) is (19.0, 7.0, 5.0), the interaction distance R a The resin is characterized in that it is soluble or dispersible in a solvent (D) having a Tg of 30° C. or higher and a weight average molecular weight of 1,000 to 100,000.

[0014] (2) The binder (C) has the interaction distance R a It is preferable that the resin is a resin that dissolves or disperses in a solvent (D) having a molecular weight of 30 or more.

[0015] (3) The binder (C) preferably has a Tg of 40° C. or higher.

[0016] (4) The resin (A1) constituting the resin-containing powder particles (A) is preferably a resin obtained by reacting one or more binder resins (A11) selected from the group consisting of fluororesins, polyester resins, and acrylic resins with one or more curing agents (A12) selected from the group consisting of compounds having an epoxy group or polymers thereof, amide compounds, and isocyanate compounds.

[0017] (5) The solvent (D) is preferably one or more solvents selected from the group consisting of water, ethylene glycol, and methanol.

[0018] (6) The solvent (D) is preferably a mixed solvent of water and a water-soluble organic solvent.

[0019] (7) The above-mentioned bright pigment (B) is preferably aluminum flakes.

[0020] (8) The coating film according to the present invention is formed using the powder coating composition.

[0021] (9) The coated body according to the present invention has a substrate and a coating film formed on a surface of the substrate using the powder coating composition. Effect of the Invention

[0022] According to the present invention, it is possible to provide a powder coating composition capable of forming a coating film having a gloss and excellent brilliance, and also having excellent recoverability and reusability. Also, according to the present invention, it is possible to provide a coating film formed using the above powder coating composition, and a coated body having this coating film. [Brief description of the drawings]

[0023] [Figure 1] This is a diagram to explain how to create a Hansen melting sphere with specific center coordinates and specific interaction radius R0 on a Hansen 3D graph using HSP (δd, δp, δh). [Diagram 2] This is a diagram showing a group of solvents that dissolve a resin (hypothetical resin X) used in forming a specific Hansen dissolution sphere, and a group of solvents that do not dissolve the resin (hypothetical resin X). [Diagram 3] This is a diagram showing a group of solvents that dissolve a resin (virtual resin X) used to form a specific Hansen melting sphere, a group of solvents that do not dissolve the resin (virtual resin X), and a solvent located at an interaction distance Ra from the center coordinate (CC) of the specific Hansen melting sphere. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the shape and size of the drawings are appropriately changed for convenience of explanation. Therefore, the present invention is not limited to the shape of the drawings.

[0025] [Powder coating composition] The powder coating composition according to the present invention contains resin-containing powder particles (A), a luster pigment (B) and a binder (C).

[0026] (Resin-containing powder particles (A)) The resin-containing powder particles (A) contain at least a resin (A1). The resin (A1) contains at least a binder resin (A11) and may contain a curing agent (A12) as necessary. Here, the curing agent (A12) is a compound or polymer that reacts with the binder resin (A11). It is preferable that the curing agent (A12) does not react when preparing the resin-containing powder particles (A) but reacts when forming a film using the powder coating composition.

[0027] The resin-containing powder particles (A) are prepared by, for example, melting and kneading a mixture containing at least a binder resin (A11) and, if necessary, a curing agent (A12), followed by cooling and pulverization, so as to contain a resin (A1). The mixture may further contain additives (A2) such as a surface conditioner and a lubricant, a color pigment (A3), etc., if necessary.

[0028] When the mixture further contains an additive (A2), the resulting resin-containing powder particles (A) contain the resin (A1) and a component derived from the additive (A2). Here, the "component derived from the additive (A2)" means the additive (A2) itself or a reaction product of the additive (A2) with another component.

[0029] When the mixture further contains a color pigment (A3), the resulting resin-containing powder particles (A) contain the resin (A1) and the color pigment (A3).

[0030] When the additive (A2) and the color pigment (A3) are further contained, the resulting resin-containing powder particles (A) contain the resin (A1), a component derived from the additive (A2), and the color pigment (A3).

[0031] <Binder resin (A11)> As the binder resin (A11), for example, one or more types selected from the group consisting of fluororesins, polyester resins, and acrylic resins are used, and a combination of multiple types of binders may be used.

[0032] The fluororesin used in the binder resin (A11) is a fluorocopolymer obtained by polymerizing or copolymerizing a fluorine-containing monomer.

[0033] As the fluororesin, for example, a resin that is solid at room temperature and has a softening point of 50 to 150° C. is used.

[0034] Examples of the fluorine-containing monomer that can be used include vinyl fluoride, vinylidene fluoride, trifluoroethylene, tetrafluoroethylene, bromotrifluoroethylene, chlorotrifluoroethylene, pentafluoropropylene, hexafluoropropylene, and (per)fluoroalkyl trifluorovinyl ether (the (per)fluoroalkyl group has 1 to 18 carbon atoms).

[0035] The fluororesin may be a copolymer of a fluorine-containing monomer and a polymerizable monomer other than the fluorine-containing monomer. Examples of the polymerizable monomer include vinyl ethers, olefins, allyl ethers, vinyl esters, allyl esters, (meth)acrylic esters, and crotonates.

[0036] Examples of the polymerizable monomer include alkyl vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, cyclohexyl vinyl ether, and chloroethyl vinyl ether; Olefins such as ethylene, propylene, 1-butene, isobutylene, cyclohexene, vinyl chloride, and vinylidene chloride; Styrenic monomers such as styrene and α-methylstyrene; Alkyl allyl ethers such as methyl allyl ether, ethyl allyl ether, butyl allyl ether, and cyclohexyl allyl ether; fatty acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl isobutyrate, vinyl valerate, vinyl hexanoate, vinyl octanoate, and vinyl versatate; Fatty acid allyl esters such as allyl propionate and allyl acetate; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and cyclohexyl (meth)acrylate; (Meth)acrylic acid amides such as (meth)acrylic acid amide; cyano group-containing monomers such as acrylonitrile and 2,4-dicyanobutene-1; Dienes such as isoprene and butadiene Polymerizable monomers such as the above can be used.

[0037] The fluororesin may have a reactive site that reacts with a curing agent, etc. The fluororesin may also be a copolymer of one or more of the above-mentioned fluorine-containing monomers and polymerizable monomers with a reactive group-containing monomer.

[0038] Examples of the reactive group-containing monomer include Monomers containing functional groups such as hydroxyl groups, carboxyl groups, amide groups, amino groups, nitrile groups, glycidyl groups, isocyanate groups, etc. Examples of reactive group-containing monomers include hydroxyl group-containing monomers, carboxyl group-containing monomers, amino group-containing monomers, amide group-containing monomers, nitrile group-containing monomers, glycidyl group-containing monomers, isocyanate group-containing monomers, etc.

[0039] Examples of the hydroxyl group-containing monomer include Allyl alcohol; hydroxyalkyl vinyl ethers such as 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, and 4-hydroxycyclohexyl vinyl ether; hydroxyalkyl allyl ethers such as 2-hydroxyethyl allyl ether, 3-hydroxypropyl allyl ether, 4-hydroxybutyl allyl ether, and 4-hydroxycyclohexyl allyl ether; Hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate; Esters of hydroxyalkyl carboxylic acids with vinyl alcohol, such as vinyl hydroxyacetate, vinyl hydroxyisobutyrate, vinyl hydroxypropionate, vinyl hydroxybutyrate, vinyl hydroxyvalerate, and vinyl hydroxycyclohexylcarboxylate; Hydroxyalkyl allyl esters such as hydroxyethyl allyl ester, hydroxypropyl allyl ester, hydroxybutyl allyl ester, and hydroxyisobutyl allyl ester etc. are used.

[0040] In addition, as the carboxyl group-containing monomer, (meth)acrylic acid, carboxyalkyl allyl ester, etc. are used. As the amino group-containing monomer, aminoalkyl vinyl ethers, aminoalkyl allyl ethers are used. As the amide group-containing monomer, (meth)acrylamide, N-methyl(meth)acrylamide, etc. are used. As the nitrile group-containing monomer, (meth)acrylonitrile is used. As the glycidyl group-containing monomer, glycidyl allyl ether, glycidyl(meth)acrylate, etc. are used. As the isocyanate group-containing monomer, vinyl isocyanate, isocyanate ethyl acrylate, etc. are used.

[0041] The fluororesin used in the present invention preferably has a fluorine content of 10 to 70% by mass.

[0042] When a curing agent that reacts with a hydroxyl group is used as the curing agent component (A12), the hydroxyl value of the fluororesin is preferably from 10 to 100 mgKOH / g, and more preferably from 30 to 70 mgKOH / g.

[0043] When a curing agent that reacts with a carboxyl group is used as the curing agent component (A12), the acid value of the fluororesin is preferably from 1 to 80 mgKOH / g, and more preferably from 10 to 60 mgKOH / g.

[0044] The polyester resin used in the binder resin (A11) is a resin that is solid at room temperature and is obtained by reacting a carboxylic acid with a polyhydric alcohol by a known method. The softening point of the polyester resin is preferably 100 to 150°C.

[0045] Examples of the carboxylic acid component that contains a carboxylic acid include polycarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,2-octadecanedicarboxylic acid, maleic acid, fumaric acid, cyclohexanedicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, trimellitic acid, and pyromellitic acid; lower alkyl esters of these polycarboxylic acids and their anhydrides; and hydroxycarboxylic acids such as malic acid, tartaric acid, 1,2-hydroxystearic acid, and paraoxybenzoic acid.

[0046] Examples of polyhydric alcohols that can be used include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, spiroglycol, 1,4-cyclohexanedimethanol, trimethylolethane, trimethylolpropane, glycerin, and pentaerythritol.

[0047] The polyester resin can be produced by a conventional method for producing polyester resins for powder coatings using the above-mentioned carboxylic acid component and polyhydric alcohol as raw materials. For example, the above-mentioned raw materials can be used in an appropriate combination and mixing ratio, and esterification or transesterification can be carried out at 200 to 280°C according to a conventional method, followed by polycondensation reaction at 230 to 290°C using a catalyst under reduced pressure, and then depolymerization reaction can be carried out with an alcohol component to produce the polyester resin.

[0048] It is preferable for the polyester resin to have a number average molecular weight of 8,000 or less and a weight average molecular weight of 10,000 to 20,000 from the viewpoint of controlling the melt viscosity.

[0049] When a curing agent that reacts with a hydroxyl group is used as the curing agent component (A12), the hydroxyl value of the polyester resin is preferably from 20 to 100 mgKOH / g, more preferably from 30 to 80 mgKOH / g.

[0050] When a curing agent that reacts with a carboxyl group is used as the curing agent component (A12), the acid value of the polyester resin is preferably from 1 to 80 mgKOH / g, more preferably from 10 to 60 mgKOH / g.

[0051] Furthermore, for powder coatings containing fluororesin and polyester resin, if the melt viscosity of the polyester resin used is 3.5 Pa s (190°C) or less, and the melt viscosity is measured with a rheometer at a cooling rate of 10°C / min from 200°C and the slope of the Arrhenius plot of temperature and viscosity at 100-120°C is 15,000 or more, the fluororesin component tends to be unevenly distributed on the surface of the coating film during coating formation. When the fluororesin component is unevenly distributed on the surface of the coating film in this way, the weather resistance of the coating film becomes good.

[0052] The above slope is calculated, for example, by the following method. First, a rheometer ARES manufactured by TA Instruments is used to measure the viscosity under the measurement conditions of parallel plates with a diameter of 40 mm, a gap width of 1.0 mm, a frequency of 9.42 rad / s, and a strain of 1.0%. Next, using the obtained measurement results, the reciprocal 1 / T of the temperature T (K) is plotted on the horizontal axis and the logarithm lnV of the viscosity V is plotted on the vertical axis (Arrhenius plot). Then, the slope of the obtained straight line at 100 to 120°C is obtained, and this value is regarded as the above slope.

[0053] The above gradient is more preferably 16,000 to 20,000 from the viewpoint of facilitating layer separation of the coating film.

[0054] The acrylic resin used in the binder resin (A11) is a solid resin at room temperature, and is a polymer of acrylic acid esters or methacrylic acid esters. As the acrylic resin, for example, a polymer obtained by polymerizing one or more acrylic components selected from acrylic acid, methacrylic acid, and their esters, amides, nitriles, etc. is used. In addition, as the acrylic resin, a polymer obtained by polymerizing an acrylic component and a non-acrylic component such as styrene is also used. From the viewpoint of controlling the melt viscosity, it is preferable that the acrylic resin has a softening point of 100 to 150°C, a number average molecular weight of 8000 or less, and a weight average molecular weight of 10000 to 20000.

[0055] Examples of the acrylic component include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, and the like. Examples of (meth)acrylate monomers that can be used include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl acrylate, 2-aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, 3-aminopropyl (meth)acrylate, 2-butylaminoethyl (meth)acrylate, glycidyl (meth)acrylate, and allyl glycidyl ether.In addition, examples of the acrylic component that can be used include acrylic acid and methacrylic acid; amide monomers such as acrylic acid amide and methacrylic acid amide; and alkoxysilyl group-containing monomers such as γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, β-(meth)acryloxyethyltrimethoxysilane, β-(meth)acryloxyethyltriethoxysilane, γ-(meth)acryloxypropylmethyldimethoxysilane, γ-(meth)acryloxypropylmethyldiethoxysilane, γ-(meth)acryloxypropylmethyldipropoxysilane, γ-(meth)acryloxybutylphenyldimethoxysilane, γ-(meth)acryloxypropyldimethylmethoxysilane, and γ-(meth)acryloxypropyldiethylmethoxysilane.

[0056] The ratio of the acrylic component to all the components constituting the acrylic resin is, for example, 40 to 100% by mass.

[0057] Examples of non-acrylic components that can be used include carboxyl group-containing monomers such as fumaric acid, maleic acid, maleic anhydride, itaconic acid, itaconic anhydride, crotonic acid, and vinyl versatic acid; aromatic monomers such as styrene, methylstyrene, chlorostyrene, methoxystyrene, and vinyltoluene; olefin monomers such as ethylene and propylene; vinyl monomers such as vinyl acetate and vinyl chloride; amide monomers such as maleic acid amide; alkoxysilyl group-containing monomers such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, and vinylmethyldiethoxysilane; dialkyl fumarate, allyl alcohol, vinylpyridine, and butadiene.

[0058] When a curing agent that reacts with a hydroxyl group is used as the curing agent component (A12), the hydroxyl value of the acrylic resin is preferably from 20 to 100 mgKOH / g, more preferably from 30 to 80 mgKOH / g.

[0059] When a hardener that reacts with a carboxyl group is used as the hardener component (A12), the acid value of the acrylic resin is preferably from 1 to 80 mgKOH / g, more preferably from 10 to 60 mgKOH / g.

[0060] <Hardening agent (A12)> As the curing agent (A12), at least one selected from the group consisting of a compound having an epoxy group or a polymer thereof, an amide compound, and an isocyanate compound is used.

[0061] As the compound having an epoxy group, a compound having a plurality of epoxy groups in the molecule is preferable, and a representative example thereof is triglycidyl isocyanurate. Examples of polymers having epoxy groups (hereinafter also referred to as epoxy resins) include bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, novolac type epoxy resins, cyclic aliphatic epoxy resins, glycidylamine type resins, heterocyclic epoxy resins, polyfunctional epoxy resins, etc. These can be used alone or in combination.

[0062] As the epoxy resin, for example, a solid epoxy resin synthesized from bisphenol A and an epihalohydrin such as epichlorohydrin, a solid epoxy resin obtained by an elongation reaction between bisphenol A and an epoxy resin derived from bisphenol A, a dihydric phenol, and an epihalohydrin, and bisphenol A, and the like can be used.

[0063] Examples of epoxy resins available on the market include jER1004, jER1004F, jER1007, and jER4005P manufactured by Mitsubishi Chemical Corporation, EPICLON3050 and EPICLON4050 manufactured by DIC Corporation, Epotohto YD014D manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and EPONANYANPE S-904 manufactured by Nan'a Plastics Co., Ltd.

[0064] The softening point of the epoxy resin is not particularly limited, but is preferably 60 to 150° C. The epoxy equivalent of the epoxy resin is also not particularly limited, but is preferably 400 to 3,000.

[0065] As the epoxy resin, a mixture of multiple epoxy resins having different epoxy equivalents can be used. When mixing multiple epoxy resins, it is preferable to combine an epoxy resin having an epoxy equivalent of 1000 or less with an epoxy resin having an epoxy equivalent of 1000 or more.

[0066] In addition, the difference in epoxy equivalent between the epoxy resin having the minimum epoxy equivalent (A-min) and the epoxy resin having the maximum epoxy equivalent (A-max) is usually 300 or more, preferably 500 or more, and more preferably 800 or more.

[0067] As the amide compound, for example, β-hydroxyalkylamide is used. From the viewpoint of low-temperature curing property and water resistance of the coating film obtained by coating, the β-hydroxyalkylamide is preferably a β-hydroxyalkylamide having two or more functional groups per molecule. From the viewpoint of low-temperature curing property and water resistance of the coating film obtained by coating, the β-hydroxyalkylamide is more preferably N,N-di(β-hydroxyethyl)acetamide, bis(β-hydroxyethyl)adipamide, bis(β-hydroxypropyl)adipamide, bis[N,N-di(β-hydroxyethyl)]adipamide, or bis[N,N-di(β-hydroxypropyl)]adipamide. In the β-hydroxyalkylamide, the equivalent of the hydroxylamide group relative to the carboxyl group in the resin is preferably 0.5 to 1.5 equivalents.

[0068] As the isocyanate compound, for example, a blocked isocyanate compound is used. The isocyanate compound used is preferably one that is solid at room temperature.

[0069] Blocked isocyanate compounds can be produced, for example, by reacting an aliphatic, aromatic, or araliphatic diisocyanate with a low molecular weight compound having active hydrogen to obtain a polyisocyanate, and then reacting the resulting polyisocyanate with a blocking agent for masking, and therefore are easy to produce.

[0070] As the diisocyanate, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, hexamethylene diisocyanate, 4,4'-methylenebis(cyclohexylisocyanate), methylcyclohexane diisocyanate, bis(isocyanatemethyl)cyclohexane, isophorone diisocyanate, dimer acid diisocyanate, lysine diisocyanate, etc. can be used.

[0071] Examples of low molecular weight compounds having active hydrogen include water, ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, ethylenediamine, ethanolamine, diethanolamine, hexamethylenediamine, and the like, as well as isocyanurate, uretidione, low molecular weight polyesters containing hydroxyl groups, and polycaprolactone.

[0072] Examples of blocking agents that can be used include alcohols such as methanol, ethanol, and benzyl alcohol; phenols such as phenol and cresone; lactams such as caprolactam and butyrolactam; and oximes such as cyclohexanone, oxime, and methyl ethyl ketoxime.

[0073] For example, a specific example of the blocked isocyanate is isophorone diisocyanate blocked with ε-caprolactam (Vestagon B1530 manufactured by Evonik, Crelan UI manufactured by Bayer), etc.

[0074] The softening point of the isocyanate compound is preferably 10 to 120° C., more preferably 40 to 100° C. If the softening point is less than 10° C., the powder coating composition may harden under normal temperature conditions or form granular lumps. On the other hand, if the softening point is more than 120° C., it may be difficult to disperse the isocyanate compound homogeneously in the powder coating composition when producing the powder coating composition by melt kneading, and the performance of the resulting coating film, such as smoothness, strength, and moisture resistance, may be impaired.

[0075] The isocyanate compound has an equivalent of isocyanate group relative to hydroxyl group in the resin of preferably 0.05 to 1.5 equivalents, more preferably 0.8 to 1.2 equivalents. If the isocyanate group is less than 0.05 equivalents, the degree of curing of the powder coating composition may be insufficient, and the coating film performance such as adhesion, coating film hardness, and chemical resistance may be reduced. If the isocyanate group is more than 1.5 equivalents, the coating film may become brittle, and the heat resistance, chemical resistance, moisture resistance, etc. may be deteriorated. Furthermore, since blocked isocyanate is expensive, costs are likely to increase when excessive blocked isocyanate is used.

[0076] The resin (A1) constituting the resin-containing powder particles (A) preferably contains one or more binder resins (A11) selected from the group consisting of fluororesins, polyester resins, and acrylic resins, and one or more curing agents (A12) selected from the group consisting of compounds having an epoxy group or polymers thereof, amide compounds, and isocyanate compounds.

[0077] The resin (A1) constituting the resin-containing powder particles (A) more preferably contains one or more binder resins (A11) selected from the group consisting of fluororesins and polyester resins, and a curing agent (A12) consisting of an isocyanate compound.

[0078] The resin (A1) constituting the resin-containing powder particles (A) more preferably contains a binder resin (A11) made of a polyester resin and a curing agent (A12) made of a compound having an epoxy group or a polymer thereof.

[0079] The resin (A1) constituting the resin-containing powder particles (A) more preferably contains a binder resin (A11) made of a polyester resin and a curing agent (A12) made of an amide compound.

[0080] <Additives (A3)> Examples of the additive (A3) that can be used include general paint additives such as plasticizers, curing accelerators, crosslinking accelerator catalysts, surface conditioners, ultraviolet absorbers, light stabilizers, antioxidants, flow control agents, sagging inhibitors, and defoamers.

[0081] <Color pigments (A4)> Examples of the color pigment (A4) that can be used include inorganic pigments such as titanium oxide, yellow iron oxide, titanium yellow, red iron oxide (red iron oxide), lithopone, and antimony oxide, and organic pigments such as Hansa Yellow 5G, Permanent Yellow FGL, Phthalocyanine Blue, Indanthrene Blue RS, Permanent Red F5RK, and Brilliant Fast Scarlet G.

[0082] The resin-containing powder particles (A) are prepared so as to contain the resin (A1), for example, by melt-kneading a mixture containing at least the binder resin (A11) and the curing agent (A12), followed by cooling and pulverization, as described above.

[0083] The resin-containing powder particles (A) may further contain, in addition to the resin (A1), a component derived from the additive (A2), a color pigment (A3), and the like, if necessary.

[0084] The resin-containing powder particles (A) have a 50% volume average particle size of, for example, 15 to 100 μm, preferably 20 to 70 μm, and more preferably 30 to 50 μm.

[0085] (Luminous pigment (B)) Examples of the luster pigment (B) include aluminum powder pigments, nickel powder pigments, stainless steel powder pigments, copper powder, bronze powder, gold powder, silver powder, mica pigments, graphite pigments, glass flake pigments, flaked plastic pigments, and scaly iron oxide pigments. Examples of the aluminum powder pigment include flake-shaped aluminum pieces. It is preferable that the luster pigment (B) is flake-shaped aluminum pieces because of its high luster.

[0086] The bright pigment (B) has a 50% volume average particle size of, for example, 3 to 100 μm, preferably 5 to 80 μm, and more preferably 15 to 60 μm.

[0087] The bright pigment (B) has an aspect ratio of, for example, 2-60, preferably 3-40, and more preferably 5-25.

[0088] (Binder (C)) The binder (C) is a resin that bonds the resin-containing powder particles (A) and the luster pigment (B). The binder (C) is dissolved or dispersed in the solvent (D) to provide fluidity when bonding the resin-containing powder particles (A) and the luster pigment (B).

[0089] The binder (C) constituting the powder coating composition of the present invention is adapted to be used together with a solvent (D) which does not dissolve the resin (A1) constituting the resin-containing powder particles (A) and dissolves or disperses the binder (C) when bonding the resin-containing powder particles (A) and the luster pigment (B).

[0090] Specifically, the binder (C) is a specific center coordinate (δ d , δ p , δ h ) = (19.0, 7.0, 5.0) a is dissolved or dispersed in a solvent (D) having a specific range, and is a resin having a Tg and a weight average molecular weight both of which are within specific ranges.

[0091] More specifically, the binder (C) is a compound having a central coordinate (δ d , δ p , δ h ) is (19.0, 7.0, 5.0), the interaction distance R a The resin is dissolved or dispersed in a solvent (D) having a molecular weight of 20 or more, and has a Tg of 30° C. or more and a weight average molecular weight of 1,000 to 100,000.

[0092] The above Hansen 3D graph, Hansen melting sphere, center coordinates (δ d , δ p , δ h ), and the interaction distance R a is HSP(δ d , δ p , δ h These concepts will now be described with reference to the drawings.

[0093] <Hansen Solubility Parameter (HSP)> Figure 1 shows the HSP(δ d , δ p , δ h This figure explains how to create a Hansen melting sphere with specific center coordinates and a specific interaction radius R0 on a Hansen 3D graph using the .

[0094] Hansen HSP(δ d , δ p , δ h ) is a parameter defined by the following formula (1).

[0095]

number

[0096] In the present invention, a virtual resin X is set as the substance X as a resin applicable to many resins (A1) constituting the resin-containing powder particles (A). Specifically, in the present invention, this virtual resin X is set as a specific central coordinate (δ d , δ p , δ h ) = (19.0, 7.0, 5.0). In the present invention, the central coordinates of the Hansen melting sphere are set to specific central coordinates (δ d , δ p , δ h ) = (19.0, 7.0, 5.0), it becomes possible to bond the glittering pigment to various types of resin-containing powder particles.

[0097] As shown in Figure 1, HSP(δ d , δ p , δ h ) is δ d axis, δ p axis and δ h It is represented on the Hansen 3D graph G with three axes. On the Hansen 3D graph G, HSP(δ d , δ p , δ h ) is represented by point XC in Figure 1.

[0098] In the present invention, the point XC(δ d , δ p , δ h As a specific value of (δ) for the virtual resin X,d , δ p , δ h ) = (19.0, 7.0, 5.0), and this (δ d , δ p , δ h ) = (19.0, 7.0, 5.0) is set as the center coordinate CC of the Hansen Melting Sphere HSS.

[0099] In the present invention, the (δ d , δ p , δ h A Hansen dissolution sphere HSS is created with center coordinates CC at 19.0, 7.0, 5.0. The Hansen dissolution sphere HSS is the smallest sphere that contains only the solvent that dissolves the virtual resin X. The smallest sphere is calculated as the smallest sphere that contains only the solvent that dissolves the virtual resin X when testing or simulating whether the virtual resin X dissolves in various solvents.

[0100] The radius of the Hansen melting sphere HSS is defined as the interaction radius R0. The interaction radius R0 is the distance from the center coordinate CC on the Hansen 3D graph G, which is defined by the following equation (2), and is the interaction distance R a Among them, the Hansen dissolution sphere HSS is the radius of the smallest sphere that contains only the solvent that dissolves the virtual resin X. In the following formula (2), component 1 is the virtual resin X, and component 2 is the solvent. In the present invention, from the results of the above-mentioned "test or simulation of whether or not the virtual resin X dissolves in various solvents", it was found that the interaction radius R0 of the virtual resin X can be set to less than 20 (excluding 0).

[0101]

number

[0102] Generally, Δδ defined by the following formula (3), that is, the solubility parameter HSP (δ) on the Hansen 3D graph G of component 1 (hypothetical resin X) is d,1 , δ p,1 , δ h,1 ) and component 2 (solvent) on Hansen's 3D graph G. d,2 , δ p,2 , δ h,2 ) is an index showing the solubility of component 1 (virtual resin X) and component 2 (solvent). It can be said that the smaller Δδ is, the easier it is for the two components to dissolve, and the larger Δδ is, the more difficult it is for the two components to dissolve.

[0103]

number

[0104] FIG. 2 is a diagram showing a group of solvents that dissolve a resin (hypothetical resin X) used in forming a specific Hansen dissolution sphere, and a group of solvents that do not dissolve the resin (hypothetical resin X).

[0105] In Figure 2, the solvents plotted as "○ (open circle)" are within the Hansen dissolution sphere HSS with center coordinates CC and interaction radius R0, and dissolve the hypothetical resin X. The solvents plotted as "□ (open square)" are outside the Hansen dissolution sphere HSS, and do not dissolve the hypothetical resin X.

[0106] FIG. 3 shows a group of solvents that dissolve a resin (virtual resin X) used in forming a specific Hansen melting sphere, a group of solvents that do not dissolve the resin (virtual resin X), and a group of solvents that are spaced apart by an interaction distance R from the center coordinate CC of the specific Hansen melting sphere. a and a solvent located at

[0107] In FIG. 3, the solvents indicated by the plot ○ are within the Hansen melting sphere HSS with the center coordinate CC and the interaction radius R0, and dissolve the virtual resin X. The solvents indicated by the plot □ are outside the Hansen melting sphere HSS, and do not dissolve the virtual resin X. Furthermore, among the solvents indicated by the plot □, the solvent indicated by the plot DD is outside the Hansen melting sphere HSS, and has an interaction distance R a is considerably larger than the interaction radius R0, it can be said that the virtual resin X will not dissolve.

[0108] The binder (C) has an interaction distance R a It is a resin that dissolves or disperses in a solvent (D) having a molecular weight of 20 or more, preferably a solvent (D) having a molecular weight of 25 or more, and more preferably a solvent (D) having a molecular weight of 30 or more. The solvent (D) will be described later.

[0109] The binder (C) has a Tg of 30° C. or higher, preferably 40° C. or higher, and more preferably 45° C. or higher. If the Tg is lower than 30° C., the binder will remain tacky even after the solvent has evaporated, making it difficult to obtain sufficient binding between the resin-containing powder particles and the bright pigment, and the binder remaining on the powder particle surfaces will cause the resin-containing powder particles (A) to bind together, increasing the particle size of the resin-containing powder particles (A).

[0110] The binder (C) has a weight-average molecular weight of 1000 to 100000, preferably 2000 to 70000. More preferably, it is 2000 to 50000. If the weight-average molecular weight of the binder (C) is less than 1000, it is difficult to obtain sufficient binding between the resin-containing powder particles and the bright pigment. If the weight-average molecular weight of the binder (C) exceeds 100000, the solubility or dispersibility in the solvent tends to deteriorate. In addition, the dispersibility of the binder can be increased by further using an emulsifier, a dispersant, or the like, but in this case, the binding between the resin-containing powder particles and the bright pigment tends to decrease.

[0111] (Solvent (D)) The solvent (D) is a solvent that dissolves or disperses the binder (C). For example, one or more solvents selected from the group consisting of water, ethylene glycol, and methanol are used as the solvent (D). If the solvent (D) is a mixed solvent of water and a water-soluble organic solvent, it is preferable because the binder can easily wet the surface of the resin-containing powder particles while maintaining sufficient insolubility in the resin-containing powder particles.

[0112] (action) In the powder coating composition of the present invention, a solution or dispersion is prepared by dissolving or dispersing the binder (C) in the solvent (D) in advance, and the solution or dispersion thus obtained is then added to the resin-containing powder particles (A) and thoroughly mixed. Thereafter, the solvent (D) is completely evaporated, thereby bonding the resin-containing powder particles (A) and the luster pigment (B) with the binder (C).

[0113] Here, examples of "a method of adding a solution or dispersion in which the binder (C) is dissolved or dispersed in a solvent (D) to the resin-containing powder particles (A) and thoroughly mixing" include a method of "dropping a solution or dispersion in which the binder (C) is dissolved or dispersed in a solvent (D) little by little at a specific speed while stirring the resin-containing powder particles (A)" and a method of "spraying a mist of a solution or dispersion in which the binder (C) is dissolved or dispersed in a solvent (D) using a spray nozzle or the like while stirring the resin-containing powder particles (A)".

[0114] In addition, as a method for completely volatilizing the solvent (D), a method using vacuum suction is preferable. In addition, the temperature for volatilizing the solvent is preferably 0 to 80° C. When the temperature is within the range of 0 to 80° C., it is easy to obtain a powder coating composition in a good bonding state.

[0115] Although the solvent (D) dissolves or disperses the binder (C), it does not dissolve the resin-containing powder particles (A) or the resin (A1) that constitutes them. Therefore, even if the solvent (D) is added, there is no risk of the resin-containing powder particles (A) bonding to each other, increasing the particle size of the resin-containing powder particles (A), deteriorating the coating workability, or deteriorating the appearance of the coating film.

[0116] Therefore, the powder coating composition according to the present invention is capable of forming a coating film having a high gloss and excellent brilliance, and is also highly recyclable.

[0117] In the powder coating composition according to the present invention, a specific virtual resin X is set as a resin applicable to many resins (A1) constituting the resin-containing powder particles (A) and specific central coordinates CC(δ d , δ p , δ h ) = (19.0, 7.0, 5.0) is set. Therefore, if the solvent (D) present outside this specific Hansen melting sphere is used as the solvent for the binder (C), the binder (C) can be dissolved or dispersed without dissolving many of the resins (A1) present inside the Hansen melting sphere. Therefore, in the present invention, it is possible to bond the glittering pigment to various types of resin-containing powder particles.

[0118] (effect) According to the powder coating composition of the present invention, it is possible to provide a powder coating composition which is capable of forming a coating film having high brilliance and gloss and which has excellent recoverability and reusability.

[0119] [Paint film] The coating film according to the present invention is formed by using the powder coating composition according to the present invention. Examples of the method for forming the coating film include electrostatic powder coating, corona charging, and tribocharging powder coating.

[0120] The thickness of the coating film is not particularly limited, but is preferably 20 to 1000 μm, more preferably 20 to 500 μm, and even more preferably 20 to 300 μm. When the coating film is a coating film for a member for a high-rise building such as an aluminum curtain wall, the thickness of the coating film is preferably 20 to 90 μm. When the coating film is a coating film for a member that requires high weather resistance such as an outdoor unit of an air conditioner installed along the coast, a traffic light pole, or a sign, the thickness of the coating film is preferably 100 to 200 μm.

[0121] The method for forming the coating film is not particularly limited. For example, the coating film may be formed by applying the powder coating composition of the present invention to a substrate, forming a molten film made of a melt of the powder coating composition, and then cooling the molten film to form the coating film.

[0122] The molten film made of the melt of the above-mentioned powder coating composition can be obtained, for example, by a method in which the film is formed simultaneously with the application of the powder coating composition to a substrate, or by a method in which the powder coating composition is adhered to a substrate and then heated and melted on the substrate to form the film.

[0123] In addition, when the powder coating composition contains a curing agent, the curing reaction of the reactive components in the composition may start almost simultaneously when the powder coating composition is heated and melted. In this case, the method of forming the coating film is preferably a method of heating and melting the powder coating composition and attaching it to the substrate almost simultaneously, or a method of attaching the powder coating composition to the substrate and then heating and melting the powder coating composition.

[0124] The heating temperature (hereinafter also referred to as the "baking temperature") and the heating maintenance time (hereinafter also referred to as the "baking time") for heating and melting the powder coating composition and for maintaining this heated and melted state for a predetermined period of time are appropriately set depending on the types and composition of the raw material components of the powder coating composition, the desired thickness of the coating film, etc.

[0125] When the powder coating composition does not contain a curing agent, the baking temperature is preferably 160 to 300° C. When the powder coating composition contains a curing agent, the baking temperature is preferably set according to the reaction temperature of the curing agent. When a curing agent is used, the baking temperature is preferably 120 to 240° C.

[0126] The reaction temperature of the curing agent can be determined by measuring the change in the elastic modulus of the powder coating composition, for example, using a rheometer such as the ARES rheometer manufactured by TA Instruments Japan, Inc.

[0127] The baking time is preferably 2 to 60 minutes. When the powder coating composition does not contain a curing agent, the baking time is more preferably 5 to 60 minutes, and even more preferably 10 to 50 minutes. When the powder coating composition contains a curing agent, the baking time is more preferably 2 to 50 minutes, and even more preferably 5 to 40 minutes.

[0128] The coating method used in the coating film formation method includes electrostatic coating, electrostatic spraying, electrostatic immersion, spraying, fluidized bed immersion, spraying, spraying, thermal spraying, plasma thermal spraying, etc. Among these, electrostatic coating using a powder coating gun is preferred because of the excellent surface smoothness of the molten film. As the powder coating gun, a corona charging type coating gun, a friction charging type coating gun, etc. are used. Here, the corona charging type coating gun means a gun that sprays a powder coating composition after corona discharge treatment. Also, the friction charging type coating gun means a gun that sprays a powder coating composition after friction charging treatment.

[0129] The cooling temperature of the molten film is preferably 20 to 25° C. When the powder coating composition according to the present invention contains a curing agent, the coating film formed is a cured film. The cooling after baking may be either rapid cooling or slow cooling, with slow cooling being preferred since the coating film is less likely to peel off from the substrate.

[0130] (effect) The coating film according to the present invention can be formed using a powder coating composition that is capable of forming a coating film having high brilliance and gloss and that is excellent in terms of recyclability.

[0131] [Painted body] The coated body according to the present invention has a substrate and a coating film formed on the surface of the substrate using the powder coating composition according to the present invention.

[0132] (base material) As the substrate, for example, a substrate made of a metal (iron, stainless steel, aluminum, copper, titanium, brass, aluminum alloy, etc.), steel, cast iron, etc. is preferably used. As the steel, alloy steel, special steel, or carbon steel is used.

[0133] Specific examples of substrates made of aluminum alloys include architectural sashes and architectural panels, etc. Specific examples of substrates made of carbon steel include railway bridges, road bridges, gas tanks, oil tanks, steel towers, springs, etc.

[0134] The coated body according to the present invention can be obtained by using the powder coating composition according to the present invention and carrying out the method for forming the coating film according to the present invention described in the section on the coating film according to the present invention.

[0135] (effect) According to the coated body of the present invention, it is possible to form a coating film that is glossy and has excellent brilliance, and furthermore, it can be formed using a powder coating composition that is also highly recyclable and reusable. EXAMPLES

[0136] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the descriptions of the examples and comparative examples, "parts" and "%" are based on mass.

[0137] In the examples and comparative examples shown below, the following raw materials were used.

[0138] <1. Raw materials for powder coating composition> (1) Raw material for resin-containing powder particles (A) (1-1) Binder resin (A11) Fluorine resin 1: Lumiflon LF710F, a hydroxyl group-containing fluororesin (hydroxyl value: 46 mgKOH / g, manufactured by AGC Inc.) Polyester resin 1: U-PICA Coat GV560, hydroxyl-containing polyester resin (hydroxyl value: 50 mg KOH / g, acid value: 5 mg KOH / g, softening point: 125°C, manufactured by Japan U-PICA Corporation) Polyester resin 2: Krylcoat 1683-0, carboxylic acid-containing polyester resin (acid value: 50 mg KOH / g, manufactured by Daicel-Allnex Corporation) Polyester resin 3: Krylcoat 2630-2, carboxylic acid-containing polyester resin (acid value: 33 mg KOH / g, manufactured by Daicel-Allnex Corporation)

[0139] (1-2) Hardener (A12) Hardener 1: ε-caprolactam blocked isocyanate (manufactured by Evonik Degussa Co., Ltd., product name: VESTAGON B1530) Hardener 2: Bis-A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name: jER (registered trademark) 1004) Hardener 3: β-hydroxyl alkylamide (manufactured by M-Chemie Corporation, product name) : Primid XL-552)

[0140] (1-3) Additives (A3) Additive 1: Silica-based surface conditioner (manufactured by Big Chemie Co., Ltd., product name: BYK360P) Lubricant 1: Amorphous silicon dioxide (manufactured by Fuji Silysia Ltd., product name: SYLYSIA 358)

[0141] (2) Luminescent pigment (B) Aluminum flake 1: PCF7620A (manufactured by Toyo Aluminum Co., Ltd.)

[0142] (3) Binder (C) Binder 1: Joncryl JDX-C3000 (BASF, acrylic resin, active ingredient 100% by mass, Tg 57°C, weight average molecular weight 10,000) Binder 2: Pluscoat Z-730 (manufactured by GOO Chemical Industry Co., Ltd., polyester resin aqueous solution, active ingredient 25% by mass, Tg 46°C, weight average molecular weight 3000) Binder 3: BURNOCK WD-551P (DIC Corporation, water-based hydroxyl-containing acrylic resin dispersion, active ingredient 40% by mass, Tg 40°C, weight average molecular weight 28,000) Binder 4: WATERSOL EFD-5580 (DIC Corporation, water-based acrylic resin dispersion, active ingredient 40% by mass, Tg 15°C, weight average molecular weight 70,000) Binder 5: JER 1001 (manufactured by Mitsubishi Chemical Corporation, epoxy resin, active ingredient 100% by mass, Tg 64°C, weight average molecular weight 3000) Binder 6: HA 3509 (Resonac Holdings, Inc., acrylic resin solution, active ingredient 55% by mass, Tg 50°C, weight average molecular weight 7500) Binder 7: YS Polystar TH130 (manufactured by Yasuhara Chemical Co., Ltd., terpene-phenol resin, active ingredient 100% by mass, Tg 130°C, weight average molecular weight 1500)

[0143] (4) Solvent (D) Solvent 1: Ion-exchanged water Solvent 2: A mixture of 75 wt% ion-exchanged water and 25 wt% methanol (Kanto Chemical Co., Ltd.) Solvent 3: A mixture of 50 wt% ion-exchanged water and 50 wt% methanol (Kanto Chemical Co., Ltd.) Solvent 4: A mixture of 25 wt% ion-exchanged water and 75 wt% methanol (Kanto Chemical Co., Ltd.) Solvent 5: Methanol (Kanto Chemical Co., Ltd.) Solvent 6: Ethylene glycol (Kanto Chemical Co., Ltd.) Solvent 7: Xylene (Kanto Chemical Co., Ltd.) Solvent 8: n-heptane (Kanto Chemical Co., Ltd.) Solvent 9: Perfluoromethylcyclohexane (Fujifilm Wako Pure Chemical Industries, Ltd.)

[0144] Table 2 shows the NV (%), which is the ratio of the mass of the dried coating material to the mass of the coating material before drying, the glass transition temperature Tg (° C.), and the weight average molecular weight Mw of the binder (C).

[0145] [Test Example 1] Using Hansen Solubility Parameters in Practice (HSPiP), the HSP (δ d , δ p , δ h The HSP of the solvent (D) was calculated using the formula (δ) in the above formulas (2) and (3). d,2 , δ p,2 , δ h,2 ), but in the Test Examples and the following Examples and Comparative Examples, it is simply referred to as (δ d , δ p , δ h ) will be written as In addition, for each solvent (D), (δ d , δ p , δ h ) = (19.0, 7.0, 5.0) a was calculated. HSP(δ d , δ p , δ h ) and the interaction distance R a are shown in Table 2.

[0146] [Table 1]

[0147] [Table 2]

[0148] [Test Example 2] (Solubility evaluation test) Each of the binders 1, 2, and 5 to 7 was adjusted to 100% solid content in a reduced pressure environment of 25°C and 760 mmHg (gauge pressure), and 0.01 g was then measured out. Next, each of the measured binders 1, 2, and 5 to 7 was mixed with 10 ml of each of the solvents 1 to 9 and stirred at 25°C for 30 minutes. After stirring, the mixture was left for 24 hours, and the state of the obtained product was visually evaluated. The evaluation results are shown in Table 3. The evaluation criteria are as follows. Note that binders 3 and 4 are in a state where the resin component is dispersed in water (solvent 1), and if the solid content is 100%, a film will be formed, making it impossible to determine the inherent solubility of the resin. For this reason, 0.04 g (solid content 0.01 g) of binder 3 was measured, and methanol was added so that the water / methanol mixture ratio was equivalent to that of solvents 2 and 3, and the dispersion state was evaluated. For binder 4, 0.018 g (solid content 0.01 g) was measured, and methanol was added so that the water / methanol mixture ratio was equivalent to that of solvents 2 and 3, and the dispersion state was evaluated.

[0149] <Evaluation> The evaluation was as follows: ◎ (Excellent): The liquid is transparent and dissolved. ◯ (Good): The liquid is cloudy and in a dispersed state (no precipitate is formed). × (bad): A precipitate was generated from the time of stirring. -: Dispersion evaluation not performed.

[0150] [Table 3]

[0151] [Examples 1 to 36, Comparative Examples 1 to 15] (1. Preparation of Powder Coating Composition) <1-1: Preparation of resin-containing powder particles (A)> (1) 1-1-1: Preparation of powder particles containing fluororesin and polyester resin The raw materials shown in Tables 1 and 2 were used, and each component was mixed to the blending ratio shown in Tables 4 and 5 to obtain powder particles (A) containing fluororesin and polyester resin. Specifically, the fluororesin, polyester resin, curing agent (blocked isocyanate), additives, and lubricant were charged into a high-speed mixer and mixed for 1 minute. Then, kneading was performed using a single-shaft kneader (manufactured by BUSS) whose temperature was adjusted to 120°C, and the discharged kneaded product was cold-rolled with a cooling roll. Thereafter, the powder particles (A) (50% volume average particle size: about 35 μm) that are raw materials for the powder coating compositions (coatings 1 to 17) were obtained.

[0152] (2) 1-1-2: Preparation of powder particles containing polyester resin and epoxy resin The raw materials shown in Tables 1 and 2 were used, and each component was mixed to the blending ratio shown in Tables 6 and 7 to obtain powder particles (A) containing polyester resin and epoxy resin. Specifically, the polyester resin, epoxy resin, and additives were put into a high-speed mixer and mixed for 1 minute. Then, kneading was performed using a single-axis kneader (manufactured by BUSS Co., Ltd.) whose temperature was adjusted to 120°C, and the discharged kneaded product was cold-rolled with a cooling roll. Thereafter, the powder particles (A) (50% volume average particle size: about 35 μm) that are raw materials for the powder coating compositions (coatings 18 to 34) were obtained.

[0153] (3) 1-1-3: Preparation of powder particles containing polyester resin and amide compound The raw materials shown in Tables 1 and 2 were used, and each component was mixed to the blending ratio shown in Tables 8 and 9 to obtain powder particles (A) containing a polyester resin and an amide compound. Specifically, the polyester resin, the amide compound, the additive, and the lubricant were put into a high-speed mixer and mixed for 1 minute. Then, kneading was performed using a single-shaft kneader (manufactured by BUSS Co., Ltd.) whose temperature was adjusted to 120°C, and the discharged kneaded product was cold-rolled with a cooling roll. Thereafter, the powder particles (A) (50% volume average particle size: about 35 μm) that are raw materials for the powder coating compositions (coatings 35 to 51) were obtained.

[0154] <1-2: Preparation of binder liquid> The binder and binder solvent were mixed in the blending ratios shown in Tables 4 to 9 to prepare binder liquids for use in producing powder coating compositions (Coatings 1 to 51).

[0155] <1-3: Preparation of powder coating compositions (coatings 1 to 51)> A luster pigment (manufactured by Toyo Aluminum Co., Ltd., PCF7620A, average particle size 21 μm, resin-coated aluminum powder) was added to the powder particles (A) obtained by the method described above in the blending ratio shown in Tables 4 to 9, and mixed with a spoon until uniform. Next, the binder liquid obtained by the above method was added, and the mixture was kneaded and naturally dried for 1 hour. The mixture was filled into a 1-liter measuring flask, and the mixture was vacuum-dried at room temperature for 20 minutes using an evaporator while rotating and mixing for 30 minutes. The powder thus obtained was classified using a mesh with 100 μm openings to obtain powder coating compositions (coatings 1 to 51).

[0156] (2. Characterization) The properties of the obtained powder coating compositions (Coat 1 to 51) were evaluated. The results of each evaluation test are shown in Tables 4 to 9. In the evaluation tests for luster and surface smoothness, test pieces prepared as follows were used.

[0157] <2-1: How to prepare test specimens> Each powder coating material was electrostatically coated on one side of a chromate-treated aluminum plate (substrate) using an electrostatic coating machine (manufactured by Onoda Cement Co., Ltd., product name: GX3600C) equipped with a powder coating gun, and the coated aluminum plate was held in an atmosphere at 200°C for 20 minutes. The coated aluminum plate was then left to cool to room temperature, yielding an aluminum plate (test piece) with a coating film (cured film) having a thickness of 55 to 65 μm.

[0158] <2-2: Evaluation> The layer separation property, luster, surface smoothness, and recovery and reusability were measured and evaluated as follows.

[0159] (1) Layer separation property The cross sections of the coating films of Examples 1 to 12 and Comparative Examples 1 to 5 were observed using a microscope (Keyence Corporation) to evaluate whether the inside of the coating film was separated into upper and lower layers. The cross sections of the coating films were also observed using a scanning electron microscope (Hitachi High-Technologies Corporation ultra-high resolution analytical scanning electron microscope SU-70) to confirm the distribution of fluorine elements (fluororesin) in the cross sections of the coating films by elemental analysis.

[0160] The evaluation was as follows: ◯ (Good): Fluorine element was unevenly distributed on the surface layer of the coating film. × (bad): No uneven distribution of elemental fluorine on the surface of the coating film was observed.

[0161] (2) Brightness The evaluation was as follows: For each test piece, the coating film was visually inspected for color unevenness and evaluated according to the following criteria. ○ (Good): Color unevenness is 20% or less of the total area of ​​the test piece. × (Fail): Color unevenness occurs in more than 20% of the total area of ​​the test piece.

[0162] (3) Surface smoothness The evaluation was as follows: After the test panels were prepared, the condition of the coating surface was evaluated visually. ◎ (Excellent): No abnormalities ○(Good): Yuzu skin ×(Bad): Rough skin

[0163] (4) Recyclability The evaluation was as follows: Any paint that did not adhere during the first coat was repainted, and each test piece was visually inspected for uneven coloring of the coating and evaluated according to the following criteria. ○ (Good): Color unevenness is 20% or less of the total area of ​​the test piece. × (Fail): Color unevenness occurs in more than 20% of the total area of ​​the test piece.

[0164] The results are shown in Tables 4 to 9.

[0165] [Table 4]

[0166] [Table 5]

[0167] [Table 6]

[0168] [Table 7]

[0169] [Table 8]

[0170] [Table 9]

[0171] From the examples and comparative examples, it was found that the powder coating compositions of the examples were excellent in all respects of luster, surface smoothness, and recovery and reusability. [Explanation of symbols]

[0172] CC center coordinates G Hansen 3D Graph HSS Hansen's Melting Ball R0 interaction radius R a interaction distance

Claims

1. A powder coating composition comprising resin-containing powder particles (A), a glittering pigment (B) and a binder (C), The binder (C) is The central coordinates (δ d , δ p , δ h ) is (19.0, 7.0, 5.0), the interaction distance R a 20 or more, and is characterized in that the powder coating composition is a resin having a Tg of 30° C. or more and a weight average molecular weight of 1,000 to 100,000.

2. The binder (C) is a 2. The powder coating composition according to claim 1, wherein the resin is soluble or dispersible in a solvent (D) having a molecular weight of 30 or more.

3. 2. The powder coating composition according to claim 1, wherein the binder (C) has a Tg of 40° C. or higher.

4. The powder coating composition according to claim 1, characterized in that the resin (A1) constituting the resin-containing powder particles (A) is a resin obtained by reacting one or more binder resins (A11) selected from the group consisting of fluororesins, polyester resins, and acrylic resins with one or more curing agents (A12) selected from the group consisting of compounds having an epoxy group or their polymers, amide compounds, and isocyanate compounds.

5. 2. The powder coating composition according to claim 1, wherein the solvent (D) is one or more solvents selected from the group consisting of water, ethylene glycol, and methanol.

6. 2. The powder coating composition according to claim 1, wherein the solvent (D) is a mixed solvent of water and a water-soluble organic solvent.

7. 2. The powder coating composition according to claim 1, wherein the bright pigment (B) is a flake-like aluminum piece.

8. A coating film formed by using the powder coating composition according to any one of claims 1 to 7.

9. A substrate; A coated body having a coating film formed on a surface of the substrate using the powder coating composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Binder for powder coating material

    JP1994184467A

  • Thermosetting metallic powder coating composition and forming method of metallic powder coating film

    JP2005187543A

  • Powder coating composition, process for producing the same, and coating film made from the same

    WO2002094950A1

  • Composite powder coating material, process for production thereof and method for the color matching of powder coating material

    WO2006057241A1

  • Powder coating composition

    JP2004175813A