Method for producing coated film formation composition for lithography
By passing an organic solvent with low water content through ion exchange resins to achieve a dehydration efficiency of 5 or more, the method addresses the inefficiency of batch pretreatments, reducing water content in lithography coating film-forming compositions and preventing defects in semiconductor substrates.
Patent Information
- Application Number
- JP2024137521
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-07-10
AI Technical Summary
Existing methods for producing lithography coating film-forming compositions fail to efficiently reduce water content, leading to defects in semiconductor substrates and reducing production efficiency due to time-consuming batch pretreatments of ion exchange resins.
A method involving the use of an organic solvent with low water content to pass through ion exchange resins, achieving a dehydration efficiency of 5 or more, resulting in a water content of 5% or less in the ion exchange resin, followed by a liquid passage step to produce a coating film-forming composition with a water content of 0.3% or less.
The method effectively reduces water content in the coating film-forming composition, enhancing production efficiency and preventing defects in semiconductor substrates.
Smart Images

Figure 2024161521000001 
Figure 2024161521000002 
Figure 2024161521000003
Abstract
Description
[Technical field]
[0001] The present application relates to a method for producing a coating film-forming composition for lithography (e.g., a resist underlayer film-forming composition) having a reduced water content, which is used in a lithography process in semiconductor manufacturing, and a method for cleaning an ion exchange resin having a reduced water content used in the production of the same. [Background technology]
[0002] In the lithography process of cutting-edge semiconductor manufacturing having wiring of 20 nm or less, there is a demand for an unlimited reduction in the water content of a coating film-forming composition for lithography in order to prevent defects on a semiconductor substrate. Patent Document 1 describes an ion exchange resin characterized by having a water content of 30% or less and a method for purifying the same. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-117781 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the manufacturing process of a coating film-forming composition for lithography, ion exchange purification using an ion exchange resin may be performed for the purpose of reducing metal impurities, but there is a problem that moisture from commercially available ion exchange resins is mixed into the product, and the moisture content of the final product cannot be reduced. In order to reduce the moisture content from the ion exchange resin, a batch-type pretreatment of the ion exchange resin is also performed in which the resin is put into an organic solvent with a low moisture content to replace the solvent, but this treatment method requires time, and therefore there is a problem that the manufacturing efficiency of the coating film-forming composition for lithography is reduced.
[0005] In order to solve the above problems, the present application provides a method for producing a coating film-forming composition for lithography, which is used in the lithography process in semiconductor manufacturing and has a reduced water content, and a method for cleaning an ion exchange resin, which has a reduced water content, used in the production of the same. [Means for solving the problem]
[0006] The present invention encompasses the following:
[0007] [1] A method for producing an ion exchange resin having a water content of 5% by weight or less, comprising the steps of: The method includes a step of passing an organic solvent having a water content of 150 ppm or less through an ion exchange resin precursor having a water content of 40% by weight or more, A method for producing an ion exchange resin having a water content of 5% by weight or less, in which dehydration efficiency=(dehydration rate (%) / (weight of organic solvent used per unit weight of the ion exchange resin precursor (kg / kg)×cleaning time (h))) is 5 or more.
[0008] [2] The flow rate of the organic solvent in the flow step is a space velocity relative to the volume of the ion exchange resin packed bed: 3 (h -1 ) The method for producing an ion exchange resin having a water content of 5% by weight or less according to [1],
[0009] [3] A method for producing a coating film-forming composition for lithography, comprising a step of subjecting a precursor of the coating film-forming composition for lithography to an ion exchange treatment using an ion exchange resin having a water content of 5% by weight or less produced by the production method described in [1] or [2].
[0010] [4] The method for producing a coating film-forming composition for lithography according to [3], wherein the water content of the coating film-forming composition for lithography after the liquid passing step is 0.3 wt % or less.
[0011] [5] The method for producing a coating film-forming composition for lithography according to [3] or [4], wherein the coating film-forming composition for lithography contains a polymer.
[0012] [6] The method for producing a coating film-forming composition for lithography according to any one of [3] to [5], wherein the coating film-forming composition for lithography further contains at least one selected from the group consisting of a crosslinkable compound, a crosslinking catalyst, and a surfactant.
[0013] [7] The method for producing a resist underlayer film forming composition according to any one of [3] to [6], wherein the coating film forming composition for lithography is a resist underlayer film forming composition.
[0014] [8] A method for washing an ion exchange resin, comprising the steps of: The method includes a step of passing an organic solvent having a water content of 150 ppm or less through the ion exchange resin, A method for cleaning an ion exchange resin, in which the (dehydration rate (%) / (weight of organic solvent used per unit weight of the ion exchange resin precursor (kg / kg)×cleaning time (h))) before and after cleaning the ion exchange resin is 5 or more.
[0015] [9] A method for producing a coating film-forming composition for lithography, comprising the step of subjecting a precursor of the coating film-forming composition for lithography to an ion exchange treatment using the ion exchange resin washed by the method of [8].
[0016]
[10] The method for producing a coating film-forming composition for lithography according to [9], wherein the water content of the coating film-forming composition for lithography after the step of carrying out the ion exchange treatment is 0.3% by weight or less. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] <Method of manufacturing ion exchange resin and method of cleaning ion exchange resin> The present application relates to a method for producing or washing an ion exchange resin having a water content of 5% by weight or less, The method includes a step of passing an organic solvent having a water content of 150 ppm or less through an ion exchange resin precursor having a water content of 40% by weight or more, This is a method for producing an ion exchange resin having a water content of 5% by weight or less, in which the dehydration efficiency = (dehydration rate (%) / (weight of organic solvent used per unit weight of the ion exchange resin precursor (kg / kg) × washing time (h))) is 5 or more.
[0018] Usually, commercially available ion exchange resins are washed with water at the end, and generally contain 40% by weight or more of water relative to the entire ion exchange resin product. When this ion exchange resin is used as is in the purification process of the coating film forming composition precursor for lithography, the final coating film forming composition for lithography contains, for example, about several % of water due to the moisture contained in the ion exchange resin. In order to reduce the amount of moisture derived from the ion exchange resin, the resin is put into an organic solvent with a low moisture content to replace the solvent, which is called batch processing, but this processing method has a problem of taking time.
[0019] The method for producing an ion exchange resin of the present invention is characterized by including a step of passing an organic solvent having a water content of 150 ppm or less through an ion exchange resin precursor having a water content of 40% by weight or more.
[0020] The lower the water content of the organic solvent, the more preferable, and it is preferably 150 ppm or less, 130 ppm or less, 100 ppm or less, 80 ppm or less, 70 ppm or less, 60 ppm or less, 50 ppm or less, 40 ppm or less, 30 ppm or less, 20 ppm or less, 10 ppm or less, 5 ppm or less, 3 ppm or less, 1 ppm or less, or below the detection limit.
[0021] The water content in the organic solvent can be measured, for example, by a Karl Fischer moisture meter.
[0022] The method for producing an ion exchange resin of the present invention is not a batch method, but involves filling a column with the hydrous ion exchange resin (untreated) of the present invention (i.e., an ion exchange resin precursor) and passing the organic solvent through it, thereby efficiently producing an ion exchange resin with a reduced water content, specifically, an ion exchange resin with a water content of 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, and more preferably 1% by weight or less. One pass through is usually sufficient, but two or more passes through are acceptable if necessary.
[0023] The method for producing an ion exchange resin of the present invention is characterized in that the dehydration efficiency is expressed by the following formula, and this value is 5 or more.
[0024] Dehydration efficiency=(Dehydration rate (%) / (Weight of organic solvent used per unit weight of ion exchange resin precursor (kg / kg)×Cleaning time (h)) For example, in the first embodiment described below, the calculation is as follows:
[0025] Dehydration efficiency = (94(%) / (8(kg / kg)×2(h))=5.875
[0026] <Ion exchange resin> An example of the ion exchange resin of the present application is one in which ion exchange groups are fixed to the surface of a porous carrier made of a copolymer of styrene and divinylbenzene. Resins are classified into strong acid, weak acid, etc., depending on the type of fixed exchange group. Strong acid is exemplified by sulfonic acid. Weak acid is exemplified by carboxyl, phosphonic acid, phosphinic acid, arsenous acid, and phenoxide. In addition, based on the physical properties of the carrier, they are classified into gel type, macro-reticulated (MR [Micro-Reticular]) type in which pores are formed in a gel type resin body and made porous, etc. The ion exchange resin is not particularly limited as long as it has a dehydration efficiency of 5 or more and a water content of 5% by weight or less, and commercially available ion exchange resins can be used.
[0027] <Organic solvent> The organic solvent according to the present invention can be any organic solvent that can wash the ion exchange resin in the liquid passing step, but is preferably an organic solvent that is generally used in semiconductor lithography steps. In particular, since the coating film forming composition for lithography and the coating film forming composition precursor for lithography according to the present invention are used in a homogeneous solution state, it is recommended to use an organic solvent that is generally used in lithography steps, taking into account the coating performance.
[0028] Examples of the organic solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, 4-methyl-2-pentanol, 2-hydroxypropyl ether, butyl ... Examples of the solvent include methyl diisobutyrate, ethyl 2-hydroxyisobutyrate, ethyl ethoxyacetate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide, alcohols such as methanol, ethanol, propanol, and butanol, ether solvents such as tetrahydrofuran and dioxane, and acetone. These solvents can be used alone or in combination of two or more.
[0029] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate, cyclohexanone, etc. are preferred, with propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate being particularly preferred.
[0030] The flow rate of the organic solvent in the flow step is a space velocity relative to the volume of the ion exchange resin packed bed: 3 (h -1 ) is preferably represented as follows:
[0031] The space velocity is calculated by the following formula:
[0032] Space velocity (h -1 ) = (cleaning liquid flow rate (L / h) / resin packed bed volume (L)) For example, in the first embodiment described below, the calculation is as follows:
[0033] Space velocity=105(L / h) / 35(L)=3(h -1 )
[0034] <Method for producing coating film-forming composition for lithography> The method for producing a coating film-forming composition for lithography of the present application includes a step of passing a coating film-forming composition precursor for lithography, which has been washed by the above-mentioned method, through an ion exchange resin having a water content of 5% by weight or less produced by the above-mentioned method. The amount of ion exchange resin used per kg of the coating film-forming composition precursor for lithography is, for example, 0.1 kg or less.
[0035] The precursor of a coating film-forming composition for lithography referred to here is a coating film-forming composition for lithography prior to treatment with an ion exchange resin.
[0036] <Coating film-forming composition for lithography and precursor thereof> The coating film-forming composition for lithography and its precursor used in the present application are, for example, the photoresist composition described below, a resist underlayer film-forming composition (containing an organic compound and / or an inorganic compound), a protective film-forming composition for protecting a substrate from an etching solution during semiconductor substrate processing, an underlayer film-forming composition for a self-assembled film, an overlayer film-forming composition for a self-assembled film, and a resist overlayer film-forming composition, etc., compositions before passing through a filter cartridge as specified above, but are not limited to these.
[0037] The exposure wavelength in the lithography process may be i-line, KrF excimer laser, ArF excimer laser, EUV (extreme ultraviolet) or EB (electron beam).
[0038] Other examples of the composition may include a resist upper layer film forming composition for a resist upper layer film described in WO2014 / 115843, WO2015 / 129486, etc., an underlayer film forming composition for a self-assembled film utilizing a block copolymer self-assembly (DSA, Direct Self Assembly) technology described in WO2013 / 146600, WO2014 / 097993, etc., such as an overlayer film forming composition for the self-assembled film described in WO2018 / 051907, and a coating composition for pattern reversal described in WO2016 / 031563.
[0039] Examples of the precursor include photoresist compositions (positive and negative) for photoresist films known per se, which are formed by applying to a semiconductor wafer preferably by spin coating and baking, resist underlayer film-forming compositions known per se (containing an organic compound and / or an inorganic compound) for resist underlayer films known per se, protective film-forming compositions for semiconductor substrate protective films known per se used when wet etching a semiconductor substrate known per se, resist overlayer film-forming compositions for resist overlayer films known per se, underlayer film-forming compositions for self-assembled films known per se, and overlayer film-forming compositions for self-assembled films known per se, but preferably protective film-forming compositions or resist underlayer film-forming compositions. Preferably resist underlayer film-forming compositions. Preferably resist underlayer film-forming compositions for ArF, EUV, or EB. Preferably underlayer film-forming compositions for self-assembled films. Preferably overlayer film-forming compositions for self-assembled films. Preferably resist overlayer film-forming compositions for EUV. Preferably coating compositions for pattern reversal.
[0040] Examples of the resist underlayer film forming composition include those described in WO2009 / 096340, JP2009-053704A, WO2010 / 147155A, WO2011 / 102470A, WO2013 / 047516A, WO2015 / 030060A, WO2018 / 052130A, and WO2019 / 124 Examples of the protective film-forming composition, the resist underlayer-forming composition, and the silicon-containing resist underlayer film-forming composition are described in Patent Publication No. 474, WO2019 / 124475, WO2019 / 151471, PCT / JP2019 / 042708, PCT / JP2020 / 001627, Japanese Patent Application No. 2019-088345, etc.
[0041] The solid content of the coating film forming composition for lithography and the coating film forming composition precursor for lithography according to the present invention is usually 0.1 to 70% by mass, preferably 0.1 to 60% by mass, and preferably 0.1 to 40% by mass. The solid content is the content of all components excluding the solvent from the coating film forming composition for lithography and its precursor. The proportion of the polymer in the solid content is, for example, 1 to 100% by mass, 2 to 100% by mass, 3 to 100% by mass, 4 to 100% by mass, 5 to 100% by mass, 10 to 100% by mass, 30 to 100% by mass, 50 to 100% by mass, 6 to 100% by mass, 1 to 99.9% by mass, 50 to 99.9% by mass, 50 to 95% by mass, or 50 to 90% by mass.
[0042] <Polymer> The coating film-forming composition for lithography and its precursor used in the present application preferably contain a polymer having a weight average molecular weight of 800 or more and an organic solvent.
[0043] The organic solvent is the same as the <organic solvent> described above. However, since the coating film-forming composition for lithography and the coating film-forming composition precursor for lithography according to the present invention are used in the state of a homogeneous solution, in consideration of their coating performance, it is recommended to use an organic solvent that is generally used in lithography processes.
[0044] An example of a specific structure of the polymer is represented by the following formula (01): [ka] [In the above formula, X represents the following formula (02), formula (03), or formula (04): [ka] (In the above formula, R 1 ~R 5each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, a benzyl group, or a phenyl group, the phenyl group being optionally substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, and an alkylthio group having 1 to 6 carbon atoms; 1 and R 2 , R 3 and R 4 may be bonded to each other to form a ring having 3 to 6 carbon atoms; A 1 ~A 6 each independently represents a hydrogen atom, a methyl group, or an ethyl group; Q 1 represents a divalent group containing a disulfide bond, preferably a divalent group containing an alkylene group having 1 to 6 carbon atoms on each end of the disulfide bond, n is the number of repeating unit structures and represents an integer of 5 to 100. It is preferable that the monomer unit has a unit structure represented by the following formula:
[0045] Examples of the polymer of the present application include, but are not limited to, the polymers described in WO 2009 / 096340 and reaction products of bifunctional or higher compounds having at least one disulfide bond and trifunctional or higher compounds described in WO 2019 / 151471.
[0046] When the polymer is a reaction product of a bifunctional compound (A) having at least one disulfide bond and a bifunctional compound (B) different from the compound (A), the disulfide bond is present in the main chain of the polymer.
[0047] The polymer has the following formula (1): [ka] (In the above formula (1), R1 is an alkyl group having 0 to 1 carbon atoms, n is the number of repeating unit structures and represents an integer of 0 or 1, and m is an integer of 0 or 1.
[0048] In the above formula (1), Z1 represents the following formula (2), formula (3), or formula (2-1): [ka] In the above formula (3), X represents the following formula (4), formula (51), or formula (6).
[0049] [ka] In the above formula (1), R2~R 61 (R2, R3, R4, R 51 and R 61 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 3 to 6 carbon atoms, a benzyl group or a phenyl group, the phenyl group may be substituted with at least one group selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group and an alkylthio group having 1 to 6 carbon atoms, and R2 and R3, and R4 and R5 may be bonded to each other to form a ring having 3 to 6 carbon atoms; A1 to A6 each independently represent a hydrogen atom, a methyl group, or an ethyl group; Q1 represents an alkylene group having 1 to 10 carbon atoms interrupted by a disulfide bond; l is the number of repeating unit structures and represents an integer of 5 to 100. The compound may have a repeating unit structure represented by the following formula:
[0050] Q1 is preferably an alkylene group having 2 to 6 carbon atoms interrupted by a disulfide bond.
[0051] Examples of the "ring having 3 to 6 carbon atoms" include cyclopropane, cyclobutane, cyclopentane, cyclopentadiene, and cyclohexane.
[0052] The above formula (01) is represented by the following formula (5): [ka] [In the above formula (5), X represents a group represented by the above formula (4), formula (51) or formula (6); R 6 and R 7 each independently represents an alkylene group having 1 to 3 carbon atoms or a direct bond, p is the number of repeating unit structures and represents an integer of 5 to 100. It may be expressed as:
[0053] The polymer of the present invention is preferably represented by the following formulas P-6 to P-8.
[0054] [ka] [ka] [ka] The polymer is preferably a reaction product synthesized by reacting a bifunctional or higher functional compound (A) having at least one disulfide bond with a bifunctional or higher functional compound (B) by a method known per se.
[0055] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclopropyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, and a 1-ethyl-n-propyl group. , cyclopentyl, 1-methyl-cyclobutyl, 2-methyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2 -dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-i-propyl-cyclopropyl, 2-i-propyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,Examples of such cyclopropyl groups include 3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl groups.
[0056] Examples of the alkenyl group having 2 to 6 carbon atoms include a vinyl group, an allyl group, a propenyl group, a butenyl group, a hexenyl group, and a cyclohexenyl group.
[0057] Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a t-butoxy group, a cyclopentyloxy group, and a cyclohexyloxy group.
[0058] Examples of the alkylthio group having 1 to 10 carbon atoms include an ethylthio group, a butylthio group, a hexylthio group, and an octylthio group.
[0059] The alkylene group having 1 to 6 carbon atoms is a divalent organic group corresponding to the alkyl group, and examples thereof include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, a cyclopropylene group, an n-butylene group, an isobutylene group, an s-butylene group, a t-butylene group, a cyclobutylene group, a 1-methyl-cyclopropylene group, a 2-methyl-cyclopropylene group, an n-pentylene group, a 1-methyl-n-butylene group, a 2-methyl-n-butylene group, a 3-methyl-n-butylene group, a 1,1-dimethyl-n-propylene group, a 1,2-dimethyl-n-propylene group, a 2,2 -Dimethyl-n-propylene, 1-ethyl-n-propylene, cyclopentylene, 1-methyl-cyclobutylene, 2-methyl-cyclobutylene, 3-methyl-cyclobutylene, 1,2-dimethyl-cyclopropylene, 2,3-dimethyl-cyclopropylene, 1-ethyl-cyclopropylene, 2-ethyl-cyclopropylene, n-hexylene, 1-methyl-n-pentylene, 2-methyl-n-pentylene, 3-methyl-n-pentylene, 4-methyl-n-pentylene, 1,1-dimethyl-n-butylene, 1,2-dimethyl-n -butylene group, 1,3-dimethyl-n-butylene group, 2,2-dimethyl-n-butylene group, 2,3-dimethyl-n-butylene group, 3,3-dimethyl-n-butylene group, 1-ethyl-n-butylene group, 2-ethyl-n-butylene group, 1,1,2-trimethyl-n-propylene group, 1,2,2-trimethyl-n-propylene group, 1-ethyl-1-methyl-n-propylene group, 1-ethyl-2-methyl-n-propylene group, cyclohexylene group, 1-methyl-cyclopentylene group, 2-methyl-cyclopentylene group, 3-methyl-cyclopentylene group, 1-ethyl -cyclobutylene group, 2-ethyl-cyclobutylene group, 3-ethyl-cyclobutylene group, 1,2-dimethyl-cyclobutylene group, 1,3-dimethyl-cyclobutylene group, 2,2-dimethyl-cyclobutylene group, 2,3-dimethyl-cyclobutylene group, 2,4-dimethyl-cyclobutylene group, 3,3-dimethyl-cyclobutylene group, 1-n-propyl-cyclopropylene group, 2-n-propyl-cyclopropylene group, 1-isopropyl-cyclopropylene group, 2-isopropyl-cyclopropylene group, 1,2,2-trimethyl-cyclopropylene group, 1,2,Examples of the cyclopropylene group include a 3-trimethyl-cyclopropylene group, a 2,2,3-trimethyl-cyclopropylene group, a 1-ethyl-2-methyl-cyclopropylene group, a 2-ethyl-1-methyl-cyclopropylene group, a 2-ethyl-2-methyl-cyclopropylene group, and a 2-ethyl-3-methyl-cyclopropylene group.
[0060] A polymer having a weight average molecular weight of 800 or more, for example, 800 to 100,000, 1,500 to 50,000, 2,000 to 30,000, or 3,000 to 20,000, can be used.
[0061] The weight average molecular weight can be determined, for example, under the following conditions.
[0062] Equipment: Tosoh Corporation HLC-8320GPC GPC column: Shodex (registered trademark) Asahipak (registered trademark) (Showa Denko K.K.) Column temperature: 40℃ Flow rate: 0.35mL / min Eluent: tetrahydrofuran (THF) Standard sample: Polystyrene (Tosoh Corporation) The coating film-forming composition for lithography and its precursor, and each component contained in the coating film-forming composition for lithography of the present invention can be prepared by dissolving them in an organic solvent, and used in the form of a homogeneous solution. The organic solvent is as described above.
[0063] <Crosslinkable compound> The coating film forming composition for lithography and its precursor used in the present application preferably contain a crosslinking compound. Examples of the crosslinking compound include melamine-based, substituted urea-based, or polymers thereof, as well as epoxy-based or polymers thereof and blocked isocyanate-based or polymers thereof. A crosslinking compound having at least two crosslink-forming substituents is preferable, and is a compound such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguwanamine, butoxymethylated benzoguwanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, or methoxymethylated thiourea. A specific example is tetramethoxymethylglycoluril. Condensates of these compounds can also be used.
[0064] In addition, a crosslinking agent having high heat resistance can be used as the crosslinkable compound. As the crosslinking agent having high heat resistance, a compound containing a crosslinking substituent having an aromatic ring (e.g., a benzene ring or a naphthalene ring) in the molecule can be used.
[0065] The compound may be a compound having a partial structure of the following formula (5-1), or a polymer or oligomer having a repeating unit of the following formula (5-2).
[0066] [ka] Above R 11 , R 12 , R 13 , and R 14 is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and the alkyl groups mentioned above can be used.
[0067] m1 is 1≦m1≦6-m2, m2 is 1≦m2≦5, m3 is 1≦m3≦4-m2, and m4 is 1≦m4≦3.
[0068] Examples of the compounds, polymers and oligomers of the formula (5-1) and the formula (5-2) are shown below.
[0069] [ka] [ka] The above compounds are available as products of Asahi Yukizai Kogyo Co., Ltd. and Honshu Chemical Industry Co., Ltd. For example, among the above crosslinking agents, the compound of formula (6-22) is available from Asahi Yukizai Kogyo Co., Ltd. under the trade name TMOM-BP.
[0070] The crosslinking agent may also be a compound having at least two epoxy groups. Examples of such compounds include tris(2,3-epoxypropyl)isocyanurate, 1,4-butanediol diglycidyl ether, 1,2-epoxy-4-(epoxyethyl)cyclohexane, glycerol triglycidyl ether, diethylene glycol diglycidyl ether, 2,6-diglycidylphenyl glycidyl ether, 1,1,3-tris[p-(2,3-epoxypropoxy)phenyl]propane, 1,2-cyclohexanedicarboxylic acid diglycidyl ester, 4,4'-methylenebis(N,N-diglycidylaniline), 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, trimethylolethane triglycidyl ether, bisphenol-A diglycidyl ether, and Epolead (registered trademark) GT-401, GT-403, GT-301, and GT-30 manufactured by Daicel Corporation. 2. Celloxide (registered trademark) 2021, 3000, 1001, 1002, 1003, 1004, 1007, 1009, 1010, 828, 807, 152, 154, 180S75, 871, 872 manufactured by Mitsubishi Chemical Corporation, EPPN201, 202, EOCN-102, 103S, 104S, 1020, 1025, 1027 manufactured by Nippon Kayaku Co., Ltd., and Denacol (registered trademark) EX-25 manufactured by Nagase ChemteX Corporation Examples of such products include BASF EX-611, EX-612, EX-614, EX-622, EX-411, EX-512, EX-522, EX-421, EX-313, EX-314, and EX-321 manufactured by BASF Japan Ltd., CY175, CY177, CY179, CY182, CY184, and CY192 manufactured by BASF Japan Ltd., and Epiclon 200, 400, 7015, 835LV, and 850CRP manufactured by DIC Corporation.
[0071] As the compound having at least two epoxy groups, a polymer having an epoxy group can also be used. As the polymer, any polymer having an epoxy group can be used without any particular limitation. Such a polymer can be produced by addition polymerization using an addition polymerizable monomer having an epoxy group, or by reaction of a polymer compound having a hydroxyl group with a compound having an epoxy group such as epichlorohydrin or glycidyl tosylate. For example, addition polymerization polymers such as polyglycidyl acrylate, copolymers of glycidyl methacrylate and ethyl methacrylate, copolymers of glycidyl methacrylate, styrene and 2-hydroxyethyl methacrylate, and condensation polymerization polymers such as epoxy novolac can be mentioned. The weight average molecular weight of the polymer is, for example, 300 to 200,000. The weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using polystyrene as a standard sample.
[0072] The compound having at least two epoxy groups may also be an epoxy resin having an amino group, such as YH-434 or YH-434L (manufactured by Shin-Nikka Epoxy Manufacturing Co., Ltd. (formerly Tohto Kasei Co., Ltd.)).
[0073] The crosslinking agent may also be a compound having at least two blocked isocyanate groups. Examples of such compounds include Takenate (registered trademark) B-830 and Takenate (registered trademark) B-870N manufactured by Mitsui Chemicals, Inc., and VESTANAT (registered trademark)-B1358 / 100 manufactured by Evonik Degussa. These crosslinking agents may be used alone or in combination of two or more.
[0074] The amount of the crosslinking compound to be added varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is usually 0.001 to 80% by weight, preferably 0.01 to 50% by weight, and more preferably 0.1 to 40% by weight, based on the total solid content of the coating film-forming composition for lithography and the coating film-forming composition for lithography and its precursor. These crosslinking compounds may cause a crosslinking reaction by self-condensation, but when crosslinking substituents are present in the above-mentioned polymer of the present invention, they can cause a crosslinking reaction with the crosslinking substituents.
[0075] <Crosslinking catalyst> The coating film-forming composition for lithography and the coating film-forming composition precursor for lithography of the present invention may contain a crosslinking catalyst as an optional component in order to promote the crosslinking reaction. As the crosslinking catalyst, in addition to an acidic compound (crosslinking acid catalyst), a compound that generates an acid or a base by heat can be used. As the acidic compound, a sulfonic acid compound or a carboxylic acid compound can be used, and as a compound that generates an acid by heat, a thermal acid generator can be used. Among these, it is preferable to use a crosslinking acid catalyst.
[0076] Examples of sulfonic acid compounds or carboxylic acid compounds include ammonium trifluoroacetate, p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium trifluoromethanesulfonate, pyridinium-p-toluenesulfonate, pyridinium-4-hydroxybenzenesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, pyridinium-4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, 4-nitrobenzenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid.
[0077] Examples of thermal acid generators include K-PURE (registered trademark) CXC-1612, CXC-1614, TAG-2172, TAG-2179, TAG-2678, and TAG2689 (all manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (all manufactured by Sanshin Chemical Industry Co., Ltd.).
[0078] These crosslinking catalysts can be used alone or in combination of two or more.
[0079] When the coating film-forming composition for lithography and its precursor contain a crosslinking catalyst, the content thereof is usually 0.0001 to 20% by weight, preferably 0.01 to 15% by weight, and more preferably 0.1 to 10% by mass, based on the total solid content of the coating film-forming composition for lithography and its precursor.
[0080] <Surfactant> The coating film-forming composition for lithography and its precursor used in the present invention may contain a surfactant as an optional component to improve the coating property on a semiconductor substrate. Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkylaryl ethers such as polyoxyethylene octylphenyl ether and polyoxyethylene nonylphenyl ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, and polyoxyethylene sorbitan monostearate. nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan trioleate and polyoxyethylene sorbitan tristearate; fluorosurfactants such as F-TOP (registered trademark) EF301, EF303, and EF352 (manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Megafac (registered trademark) F171, F173, R-30, R-30N, R-40, and R-40-LM (manufactured by DIC Corporation), Fluorad FC430 and FC431 (manufactured by Sumitomo 3M Limited), Asahiguard (registered trademark) AG710, Surflon (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants can be used alone or in combination of two or more. When the coating film-forming composition for lithography and its precursor contain a surfactant, the content of the surfactant is usually 0.0001 to 10% by weight, preferably 0.01 to 5% by weight, based on the total solid content of the coating film-forming composition for lithography and its precursor.
[0081] <Other ingredients> The coating film forming composition for lithography and its precursor of the present invention may contain a light absorbing agent, a rheology control agent, an adhesion promoter, etc. The rheology control agent is effective in improving the flowability of the coating film forming composition for lithography and its precursor. The adhesion promoter is effective in improving the adhesion between the semiconductor substrate or resist and the underlayer film.
[0082] The water content of the coating film-forming composition for lithography after the liquid passing step is 0.3% by weight or less. The lower the water content of the coating film-forming composition for lithography, the more preferable, and it is preferably 0.2% by weight or less, 0.15% by weight or less, 0.1% by weight or less, 0.05% by weight or less, or below the detection limit.
[0083] The water content of the coating film-forming composition for lithography can be measured, for example, by a Karl Fischer moisture meter. EXAMPLES
[0084] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these.
[0085] <Conditions for analyzing water content of ion exchange resin> The water content of the ion exchange resins shown in the examples below was measured using a Karl Fischer moisture meter, and the measurement conditions were as follows:
[0086] Equipment: Coulometric Karl Fischer moisture meter CA-200 (Mitsubishi Chemical Analytical Co., Ltd.) Evaporation device: Moisture vaporization device VA-200 (Mitsubishi Chemical Analytical Co., Ltd.) <Explanation of abbreviations> (Organic solvent) PGME: Propylene glycol monomethyl ether The actual moisture content of the PGME used in the examples: 50 to 150 ppm <Cleaning of ion exchange resin>
[0087] [Example 1] A 50-L column was packed with 35 L of Muromac XSC-1115-H (product name) strong acid cation exchange resin with a gel-type structure manufactured by Muromachi Chemical Co., Ltd. in a wet state, and PGME was passed through the top of the column. The passing rate was the space velocity (SV [h -1 The flow rate was adjusted so that the flow rate (space velocity) was 3, and the operation was carried out at room temperature. The total amount of PGME passed through was 8 times the weight of the packed resin on a wet basis. After passing through the resin, the PGME remaining in the system was blown out by nitrogen and the moisture content of the resulting ion exchange resin was measured. The results are shown in Table 1.
[0088] [Comparative Example 1] Batch washing was performed on the same resin as in Example 1. A 10 L container was filled with 1 kg of ion exchange resin based on wet weight, and PGME was added to the container in an amount equal to the weight of the filled resin and stirred. The stirring time was 4 hours, and the operation was performed at room temperature. After stirring, the washing liquid was decanted out of the container. The above operation was performed a total of three times, and the water content of the obtained ion exchange resin was measured, and the results are shown in Table 2. However, the stirring time was set to 8 hours or more only in the second operation.
[0089] [Comparative Example 2] Batch washing was performed on the same resin as in Example 1. A 10 L container was filled with 1 kg of ion exchange resin based on wet weight, and PGME was added to the container in an amount twice the weight of the filled resin and stirred. The stirring time was 2 hours, and the operation was performed at room temperature. After stirring, the washing liquid was decanted out of the container. The above operation was performed a total of 5 times, and the results of measuring the water content of the obtained ion exchange resin are shown in Table 3. However, the stirring time was 8 hours or more only in the third operation.
[0090] [Example 2] A strongly acidic cation exchange resin having an MR type structure, AMBERLYST 15JWET (product name) manufactured by Organo Corporation, was washed in the same manner as in Example 1, and the moisture content of the resulting ion exchange resin was measured. The results are shown in Table 1.
[0091] [Comparative Example 3] The same resin as in Example 2 was washed in the same manner as in Comparative Example 2, and the water content of the resulting ion exchange resin was measured. The results are shown in Table 2.
[0092] [Comparative Example 4] The same resin as in Example 2 was washed in the same manner as in Comparative Example 3, and the water content of the resulting ion exchange resin was measured. The results are shown in Table 3.
[0093] [Example 3] A strongly basic anion exchange resin having a gel-type structure, AMBERJET ESG4002(OH) (product name), manufactured by Organo Corporation, was washed in the same manner as in Example 1, and the moisture content of the resulting ion exchange resin was measured. The results are shown in Table 1.
[0094] [Comparative Example 5] The same resin as in Example 3 was washed in the same manner as in Comparative Example 1, and the water content of the resulting ion exchange resin was measured. The results are shown in Table 2.
[0095] [Comparative Example 6] The same resin as in Example 3 was washed in the same manner as in Comparative Example 3, and the moisture content of the resulting ion exchange resin was measured. The results are shown in Table 3. [Table 1] [Table 2] [Table 3] As shown in Tables 1, 2, and 3, when flow-through cleaning was used in Examples 1 to 3, the moisture content of the ion exchange resin could be efficiently reduced, whereas when the batch-type cleaning was used in Comparative Examples 1 to 6, the cleaning efficiency was poor and a large amount of moisture remained, making it impractical. In batch-type cleaning, the cleaning liquid with a high moisture content remains in the container because it is discharged outside the system by decantation, whereas in flow-through cleaning, new cleaning liquid is always supplied to the resin layer, and this is presumably why the cleaning efficiency is high.
[0096] <Synthesis Example 1> 800g of monoallyl diglycidyl isocyanuric acid (manufactured by Shikoku Chemical Industry Co., Ltd.), 608g of 3,3'-dithiodipropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., trade name: DTDPA), and 53g of triphenyl monoethyl phosphonium bromide, a quaternary phosphonium salt, as a catalyst, were dissolved in 2191g of propylene glycol monomethyl ether, and stirred for 4 hours under a nitrogen atmosphere while heating and maintaining the temperature at 120°C. The obtained reaction product was diluted with 3652g of propylene glycol monomethyl ether to obtain a varnish solution, and the GPC analysis showed that the weight average molecular weight was about 7800 in terms of standard polystyrene. This reaction product contains a polymer compound having a structural unit represented by the following formula (A-1).
[0097] [ka]
[0098] <Preparation Example 1> To 3575 g of a solution containing 715 g of the polymer compound obtained in Synthesis Example 1, 179 g of tetramethoxymethylglycoluril [POWDERLINK (registered trademark) 1174, manufactured by Nippon Cytec Industries Co., Ltd.], 18 g of 4-hydroxybenzenesulfonic acid (PSA), 11 g of bisphenol S, 7 g of a surfactant (R-30N, manufactured by DIC Corporation), 86.3 kg of propylene glycol monomethyl ether, and 9.9 kg of propylene glycol monomethyl ether acetate were added to prepare a resist underlayer film forming composition.
[0099] <Conditions for moisture analysis of ion exchange treatment solution> The water content of the ion exchange treatment solution shown in the examples described later was measured using a Karl Fischer moisture meter, and the measurement conditions were as follows:
[0100] Equipment: Coulometric Karl Fischer moisture meter CA-200 (Mitsubishi Chemical Analytical Co., Ltd.)
[0101] [Example 4] To 500 g of the resist underlayer film forming composition obtained in Preparation Example 1, 25 g of the ion exchange resin obtained in Example 1 was added, and the mixture was stirred at room temperature for 2 hours, and then the resin was removed by decantation to obtain a treatment solution (purified solution). The water content of the obtained treatment solution was measured, and the results are shown in Table 4.
[0102] [Comparative Example 7] The same operation as in Example 4 was carried out using the ion exchange resin obtained in Comparative Example 1, and the water content of the resulting treated liquid was measured. The results are shown in Table 4.
[0103] [Table 4] [Industrial Applicability]
[0104] According to the method of the present application, it is possible to provide a method for producing a coating film-forming composition for lithography having a reduced water content, and a method for cleaning an ion exchange resin having a reduced water content for producing the same.
Claims
1. A method for producing an ion exchange resin having a water content of 5% by weight or less, comprising the steps of: The method includes the step of passing an organic solvent having a water content of 150 ppm or less through an ion exchange resin precursor having a water content of 40% by weight or more, A method for producing an ion exchange resin having a water content of 5% by weight or less, wherein the dehydration efficiency=(dehydration rate (%) / (weight of organic solvent used per unit weight of the ion exchange resin precursor (kg / kg)×cleaning time (h))) is 5 or more.
2. The flow rate of the organic solvent in the flow step is a space velocity relative to the volume of the ion exchange resin packed bed: 3 (h -1 2. The method for producing an ion exchange resin having a water content of 5% by weight or less according to claim 1, wherein the water content is expressed as follows:
3. A method for producing a coating film-forming composition for lithography, comprising a step of subjecting a precursor of the coating film-forming composition for lithography to an ion exchange treatment using an ion exchange resin having a water content of 5% by weight or less produced by the production method according to claim 1 or 2.
4. 4. The method for producing a coating film-forming composition for lithography according to claim 3, wherein the water content of the coating film-forming composition for lithography after the liquid passing step is 0.3% by weight or less.
5. The method for producing a coating film-forming composition for lithography according to claim 3 or 4, wherein the coating film-forming composition for lithography contains a polymer.
6. The method for producing a coating film-forming composition for lithography according to any one of claims 3 to 5, wherein the coating film-forming composition for lithography further comprises at least one selected from the group consisting of a crosslinkable compound, a crosslinking catalyst, and a surfactant.
7. The method for producing a resist underlayer film forming composition according to any one of claims 3 to 6, wherein the coating film forming composition for lithography is a resist underlayer film forming composition.
8. A method for washing an ion exchange resin, comprising the steps of: The method includes a step of passing an organic solvent having a water content of 150 ppm or less through the ion exchange resin, A method for washing an ion exchange resin, wherein the (dehydration rate (%) / (weight of organic solvent used per unit weight of the ion exchange resin precursor (kg / kg)×washing time (h))) before and after washing the ion exchange resin is 5 or more.
9. A method for producing a coating film-forming composition for lithography, comprising the step of subjecting a precursor of a coating film-forming composition for lithography to an ion exchange treatment using an ion exchange resin washed by the method of claim 8.
10. 10. The method for producing a coating film-forming composition for lithography according to claim 9, wherein the water content of the coating film-forming composition for lithography after the step of carrying out the ion exchange treatment is 0.3% by weight or less.
Citation Information
Patent Citations
Metal ion reduction in novolak resin solutions using anion exchange resins
JP1998504599A
Method for recycling photoresist
JP1999133619A
Method for refining non-aqueous liquid material
JP2004181351A
Preparation method of silanization agent chemical liquid and surface treatment method
JP2016180055A
Process for producing cycloalkyl alkyl ether
WO2007058251A1