Semiconductor device

The semiconductor device with self-aligned electrode layers and low resistance regions in the oxide semiconductor layer addresses the challenges of miniaturization by improving yield and on-state characteristics, enabling high-speed operation with reduced power consumption.

JP2024161624AActive Publication Date: 2024-11-19SEMICON ENERGY LAB CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024150920
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2011-10-13
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2032-10-11

AI Technical Summary

Technical Problem

The challenge lies in achieving faster transistor operation with lower power consumption and higher integration while maintaining a high yield in the manufacturing process, particularly with the miniaturization of transistors, which often leads to decreased yield and the need for improved on-characteristics even when power is on.

Method used

A semiconductor device is designed with an oxide semiconductor layer, a gate insulating layer, and conductive films that are stacked and etched to form self-aligned source and drain electrode layers, reducing resistance through low resistance regions and thickening the source and drain regions, and utilizing a method that avoids digging processes for precise machining.

Benefits of technology

This approach enhances the yield of transistors with fine structures, improves on-state characteristics, and enables high-speed response and drive, addressing the issues of miniaturization and manufacturing variability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161624000001_ABST
    Figure 2024161624000001_ABST
Patent Text Reader

Abstract

To provide a transistor having a microstructure with a high yield, and to provide a semiconductor device that enables high-speed response and high-speed drive by improving ON characteristics of the transistor.SOLUTION: An oxide semiconductor layer, a gate insulating layer, a gate electrode layer, an insulating layer, a conductive film, and an interlayer insulating layer are sequentially laminated. By cutting the conductive film, the conductive film on the gate electrode layer and the insulating layer is removed to form a source electrode layer and a drain electrode layer with self-alignment. Electrode layers are provided so as to be overlapped with regions contacted with the source and drain electrode layers and to be contacted with the oxide semiconductor layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to a semiconductor device and a method for manufacturing the semiconductor device. [Background technology]

[0002] A transistor (thin film transistor) is made using a semiconductor thin film formed on a substrate with an insulating surface. The technology for constructing thin-film transistors (also called thin-film transistors) is attracting attention.

[0003] For example, indium (In), gallium (Ga), and nickel are used as active layers of transistors. A transistor using an amorphous oxide containing lead (Zn) has been disclosed (see Patent Document 1). ). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-165528 A Summary of the Invention [Problem to be solved by the invention]

[0005] By the way, we have achieved high speed operation of transistors, low power consumption, and high integration. In order to achieve this, miniaturization of transistors is essential.

[0006] However, there are concerns that the miniaturization of transistors will lead to a decrease in yield during the manufacturing process. Therefore, an object of the present invention is to provide transistors with fine structures with high yield.

[0007] In addition, as the performance of semiconductor devices including transistors improves, the transistors are becoming smaller. Therefore, even when transistors are miniaturized, it is necessary to improve the on-state characteristics. One object of the present invention is to provide a structure and a method for fabricating the same that realize high-speed response and high-speed driving of a laser. do. [Means for solving the problem]

[0008] A semiconductor device according to one embodiment of the present invention includes an oxide semiconductor layer, a gate insulating layer over the oxide semiconductor layer, and A conductive film, an interlayer insulating film, and a gate electrode layer on the gate insulating layer and an insulating layer on the gate electrode layer are formed on the gate electrode layer. An edge layer is laminated in order, and the conductive film is cut to remove the conductive film on the gate electrode layer and the insulating layer. By removing and dividing the oxide film, the source electrode layer and the drain electrode layer are formed in a self-aligned manner. The semiconductor layer is divided into a low-resistance region where impurity elements are introduced to reduce resistance, and a channel formation region. and the low resistance region is in contact with the source electrode layer and the drain electrode layer. An electrode layer made of a metal, a conductive metal compound, a semiconductor, or the like is provided in contact with the lower part of the substrate.

[0009] In the process of forming the source electrode layer and the drain electrode layer, etching using a resist mask is performed. Since no machining process is used, precise processing can be performed accurately. In the manufacturing process, the yield of transistors with fine structures with small variations in shape and characteristics is increased. It can be produced easily.

[0010] The low-resistance region of the oxide semiconductor layer is in contact with the source electrode layer and the drain electrode layer. The oxide semiconductor layer functions as a drain region. The contact resistance with the electrode layer is reduced. By providing an electrode layer in contact with the lower part of the low resistance region, Thus, the electrode layer also functions as a source region and a drain region. By making the source and drain regions thicker, The resistance of the source and drain regions is reduced, and the electric field in the source and drain electrode layers is relaxed. Thus, a semiconductor device having excellent on-state characteristics can be provided.

[0011] Therefore, one embodiment of the present invention is a pair of electrode layers, a pair of electrodes on the pair of electrode layers, and a pair of electrodes connected to the pair of electrode layers. A pair of low resistance regions each including a channel formation region sandwiched between the pair of low resistance regions is provided. a conductive layer, a gate insulating layer on the oxide semiconductor layer, and a channel forming region on the gate insulating layer; A gate electrode layer overlapping the gate electrode layer, an upper insulating layer on the gate electrode layer, and a side surface and an upper portion of the gate electrode layer A sidewall insulating layer covering a side surface of the insulating layer, an oxide semiconductor layer, a side surface of the gate insulating layer, and the sidewall insulating layer a source electrode layer and a drain electrode layer in contact with the side surfaces of the source electrode layer and the drain electrode layer; The first insulating layer, the upper insulating layer, the sidewall insulating layer, and the source electrode layer and the drain electrode layer The second insulating layer and the source electrode layer are formed through an opening in the first insulating layer and the second insulating layer. and a pair of wiring layers in contact with the source electrode layer and the drain electrode layer. The height of the upper surface of the upper insulating layer is lower than the height of the upper surfaces of the upper insulating layer, the sidewall insulating layer, and the first insulating layer; and The pair of wiring layers are higher than the upper surface of the gate electrode layer and overlap the pair of electrode layers, respectively. It is a semiconductor device.

[0012] In the semiconductor device, the electrode layer is formed in or on the underlying insulating layer below the oxide semiconductor layer. The electrode layer is provided on an insulating layer, and the upper surface of the electrode layer is exposed from the insulating base layer or the upper surface of the insulating base layer is exposed from the insulating base layer. In this case, the height of the film of the electrode layer may be the same as that of the upper surface of the electrode layer. The thickness of the source region and the drain region can be made larger than the thickness of the oxide semiconductor layer. It is possible to increase the thickness of the film.

[0013] In addition, the electrode layer may be formed on a base insulating layer, and an oxide semiconductor layer may be formed on the electrode layer. In this case, the number of steps in manufacturing the semiconductor device can be reduced.

[0014] Further, the first insulating layer includes an aluminum oxide layer in contact with the source electrode layer and the drain electrode layer. It is preferred that the compound contains

[0015] In addition, it is preferable that the surface on which the channel formation region is formed be flat.

[0016] In one embodiment of the present invention, a pair of electrode layers is formed, and an oxide semiconductor layer is formed over the pair of electrode layers. a gate insulating layer is formed on the oxide semiconductor layer, and the oxide semiconductor layer is overlapped on the gate insulating layer. A gate electrode layer and an upper insulating layer are formed, and the gate electrode layer and the upper insulating layer are used as a mask to An impurity element is introduced into the oxide semiconductor layer to form a pair of low-resistance regions and a channel formation region. A sidewall insulating layer is formed on the gate insulating layer to cover the side surface of the gate electrode layer, and an oxide A conductive film is formed on the semiconductor layer, the gate electrode layer, the sidewall insulating layer and the upper insulating layer, and a layer is formed on the conductive film. An interlayer insulating layer is formed, and the interlayer insulating layer and the conductive film are subjected to chemical mechanical polishing until the upper insulating layer is exposed. The conductive film is divided by removing the conductive film by a polishing method, and a source electrode layer and a drain electrode layer are formed. A semiconductor device having an insulating layer, an upper insulating layer, a source electrode layer, and a drain electrode layer, and a second insulating layer formed on the insulating layer, the upper insulating layer, and a source electrode layer. The present invention relates to a method for fabricating a semiconductor device. Also, a source electrode layer and a drain electrode layer are formed on the first insulating layer and the second insulating layer. An opening is formed to reach the drain electrode layer, and the source electrode layer and the drain electrode layer are connected through the opening. A wiring layer may be formed to cover the wiring layer.

[0017] In this specification, the term "above" means that the positional relationship of a component is "directly above." For example, the expression "gate electrode layer on an insulating layer" is not limited to the insulating layer. This does not exclude the inclusion of other components between the layer and the gate electrode layer. It is.

[0018] In addition, in this specification, the terms "electrode layer" and "wiring layer" refer to the functional components of these elements. For example, the "electrode layer" is used as a part of the "wiring layer." In addition, the terms "electrode layer" and "wiring layer" may be used interchangeably. This also includes cases where multiple "electrode layers" or "wiring layers" are formed integrally.

[0019] In addition, the functions of the "source" and "drain" may differ depending on whether transistors of different polarities are used or not. However, they may be swapped when the direction of the current changes during circuit operation. In this specification, the terms "source" and "drain" are used interchangeably. It is assumed that this is possible.

[0020] In this specification, "electrically connected" means "something that has some kind of electrical effect" " includes cases where the device is connected via "anything that has some electrical effect." " is not subject to any particular restriction as long as it enables the transmission and reception of electrical signals between the connection objects.

[0021] For example, "something that has some kind of electrical function" includes electrodes and wiring. Effect of the Invention

[0022] One embodiment of the present invention can provide transistors with a fine structure with high yield. In addition, the on-characteristics of miniaturized transistors can be improved. It is also possible to provide a structure and a manufacturing method thereof that realize high-speed response and high-speed operation of a transistor. can. [Brief description of the drawings]

[0023] [Figure 1] 1A and 1B are a top view and a cross-sectional view of a semiconductor device of one embodiment of the present invention. [Diagram 2] 1A to 1C illustrate a method for manufacturing a semiconductor device of one embodiment of the present invention. [Diagram 3] 1A to 1C illustrate a method for manufacturing a semiconductor device of one embodiment of the present invention. [Figure 4] 1A to 1C illustrate a method for manufacturing a semiconductor device of one embodiment of the present invention. [Diagram 5] FIG. 1 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 6] 1A and 1B are a top view and a cross-sectional view of a semiconductor device of one embodiment of the present invention. [Figure 7] FIG. 1 is a cross-sectional view of a semiconductor device according to one embodiment of the present invention. [Figure 8] 1A to 1C are a cross-sectional view, a top view, and a circuit diagram illustrating one embodiment of a semiconductor device. [Figure 9] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Figure 10] 1A and 1B are a circuit diagram and a perspective view illustrating one embodiment of a semiconductor device. [Figure 11] 1 is a cross-sectional view illustrating one embodiment of a semiconductor device. [Figure 12] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Figure 13] 1A and 1B are a top view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Figure 14] FIG. 1 is a circuit diagram illustrating one embodiment of a semiconductor device. [Figure 15] FIG. 1 is a block diagram illustrating one embodiment of a semiconductor device. [Figure 16] FIG. 1 is a block diagram illustrating one embodiment of a semiconductor device. [Figure 17]FIG. 1 is a block diagram illustrating one embodiment of a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and those skilled in the art will recognize that the modes and details of the present invention may be modified in various ways. It will be easily understood. In addition, the present invention is not limited to the description of the embodiment shown below. It is not something that can be achieved.

[0025] In the embodiments described below, the same reference numerals are used in common between different drawings. In addition, the thickness, width, relative position, etc. of components shown in the drawings, i.e., layers and regions, may be different from those shown in the drawings. In the description of the embodiments, the positional relationship may be exaggerated for clarity. There is a match.

[0026] (Embodiment 1) In this embodiment, a basic structure and a manufacturing method of a semiconductor device according to one embodiment of the present invention will be described. 1 illustrates a semiconductor device according to one embodiment of the present invention.

[0027] FIG. 1A is a top view of a transistor according to one embodiment of the present invention, and FIG. 1(A) is a cross-sectional view taken along dashed line A1-A2 of FIG.

[0028] The semiconductor device including the transistor 420 is formed by forming a base insulating layer 436 and a base insulating film 438 on a substrate 400. An electrode layer 405a provided in the edge layer 436 and having an upper surface exposed from the base insulating layer 436; The electrode layer 405b and the low resistance region 40 4a and low resistance region 404b, and the low resistance region 404a and the low resistance region 404b sandwiched therebetween An oxide semiconductor layer 409 including a channel formation region 403; A gate insulating layer 402, a gate electrode layer 401 on the gate insulating layer 402, and a gate electrode layer 4 The sidewall insulating layer 412a and the sidewall insulating layer 412b cover the side surfaces of the gate electrode layer 401. A sidewall insulating layer is formed on the upper insulating layer 413 covering the upper surface, the base insulating layer 436, and the oxide semiconductor layer 409. The source electrode layer 406a and the drain electrode layer 406b are in contact with the side surfaces of the edge layer 412a and the sidewall insulating layer 412b. The electrode layer 406b and the insulating layer 415 over the source electrode layer 406a and the drain electrode layer 406b The insulating layer 415, the source electrode layer 406a, the drain electrode layer 406b, and the sidewall insulating layer 412 a, the insulating layer 417 on the sidewall insulating layer 412b and the upper insulating layer 413, the insulating layer 415 and the insulating layer The source electrode layer 406a and the drain electrode layer 406 The wiring layers 465a and 465b are in contact with the wiring layers 465a and 465b, respectively.

[0029] The height of the upper surface of the insulating layer 415 is the height of the sidewall insulating layer 412a, the sidewall insulating layer 412b and the upper insulating layer 4 The height of the top surface of the source electrode layer 406a and the drain electrode layer 4 The height of the upper surface of the insulating layer 415, the sidewall insulating layer 412a, and the sidewall insulating layer 412b is The height is lower than the height of the upper surface of the gate electrode layer 401 and is higher than the height of the upper surface of the gate electrode layer 401. , the distance from the top surface of the substrate 400.

[0030] The oxide semiconductor layer 409 has a channel formation region 403 overlapping with the gate electrode layer 401 and an insulator layer 403 . A low resistance region 404a and a low resistance region 404b in which the resistance is reduced by introducing a pure element; The low resistance region 404a and the low resistance region 404b are formed by masking the gate electrode layer 401. By introducing an impurity element into the oxide semiconductor layer 409, the insulating film 404 is formed in a self-aligned manner.

[0031] The source electrode layer 406a and the drain electrode layer 406b are formed on the oxide semiconductor layer 409. The insulating layer 412 is provided in contact with the surface of the insulating layer 412 and the sidewall insulating layer 412a or the sidewall insulating layer 412b. The source electrode layer 406a or the drain electrode layer 406b is in contact with the oxide semiconductor layer 409. The distance (shortest distance) between the contact region and the gate electrode layer 401 is determined by the sidewall insulating layer 4 12a or the width of the sidewall insulating layer 412b in the channel length direction, which allows miniaturization to be achieved. The variation in the minimum distance can be controlled in the manufacturing process.

[0032] The low resistance region 404a and the low resistance region 404b of the oxide semiconductor layer 409 are and the source and drain electrode layers 406a and 406b of the transistor 420. The low resistance region 404a and the low resistance region 404b function as an oxide film and a drain region. The nitride semiconductor layer 409 is connected to the source electrode layer 406a and the drain electrode layer 406b. In order to achieve this, the source electrode layer 406a, the drain electrode layer 406b, and the oxide semiconductor layer 409 are The contact resistance is reduced.

[0033] The low resistance region 404a and the low resistance region 404b are formed by ion implantation of an electrode embedded in the base insulating layer 436. The electrode layer 405a and the electrode layer 405b are in contact with each other. The low resistance region 404a and the low resistance region 404b are made of metal, conductive metal compound, semiconductor, etc. Region 404b functions as the source and drain regions of transistor 420. By providing the electrode layer 405a and the electrode layer 405b under the source region and the drain region, The source and drain regions can be thickened, and the resistance of the source and drain regions can be reduced. This can reduce the resistance and improve the on-characteristics of the transistor.

[0034] In addition, the electrode layer 405a and the electrode layer 405b are embedded in a base insulating layer. Even if the thicknesses of the electrode layer 405a and the electrode layer 405b are increased, the thickness of the electrode layer 405a and the electrode layer 40 Therefore, the coverage of the oxide semiconductor layer 409 provided on the electrode layer 405 is not affected. The thicknesses of the electrode layers 405a and 405b are set to the resistance of the source and drain regions of the transistor 420. The thickness of the channel forming region 403 can be increased until the resistance is sufficiently reduced. Since no electrode layer is provided on the lower part, the channel forming region 403 is thinned, and the source region and Only the gate and drain regions can be thickened.

[0035] Next, an example of a method for manufacturing the transistor 420 shown in FIG. 1 will be described with reference to FIGS. explain.

[0036] First, a conductive film that will become the electrode layer 405a and the electrode layer 405b is formed on the substrate 400. A resist mask is formed on the electrode layer 405a and the electrode layer 405b, and selective etching is performed. After forming 405b, the resist mask is removed.

[0037] There are no major limitations to the substrate that can be used, but at least the substrate must be heat-resistant enough to withstand subsequent heat treatment. For example, barium borosilicate glass and aluminoborosilicate glass are Glass substrates such as acid glass, ceramic substrates, quartz substrates, sapphire substrates, etc. can be used. This can be done.

[0038] In addition, single crystal semiconductor substrates such as silicon and silicon carbide, polycrystalline semiconductor substrates, silicon gate Compound semiconductor substrates such as ruthenium, SOI substrates, and semiconductor elements on these substrates The provided one can be used.

[0039] The conductive film that will become the electrode layer 405a and the electrode layer 405b is made of a material that can withstand the subsequent heat treatment. The film is formed by CVD or sputtering to a thickness of 10 nm to 500 nm. For example, a metal film containing an element selected from Al, Cr, Cu, Ta, Ti, Mo, and W, Or a metal nitride film containing the above-mentioned elements (titanium nitride film, molybdenum nitride film, titanium nitride film, etc.) In addition, metals such as Al and Cu can be used. A structure in which a film and a high melting point metal such as Ti, Mo, or W are laminated may be used. High melting point metals such as W are placed either under or over metal films such as Al and Cu, or both. The conductive film may be formed of an oxide semiconductor material. The materials include indium oxide (In2O3), tin oxide (SnO2), and zinc oxide (ZnO ), indium tin oxide (In2O3-SnO2), indium zinc oxide (In 2O3-ZnO) or these metal oxide materials containing silicon oxide are used. It is possible.

[0040] In the case where an oxide semiconductor is used for the conductive film, the conductive film may be made of the same oxide semiconductor material as the oxide semiconductor layer 409. In particular, the conductive film and the oxide semiconductor layer 409 may be made of the same oxide semiconductor material. When a semiconductor material is used, the electrode layers 405a and 405b and the oxide semiconductor layer 409 Since the contact resistance can be further reduced, transistors with good electrical characteristics can be manufactured. For example, In-Ga-Zn oxide (IGZ) can be used as an oxide semiconductor material. In the case where IGZO is used, the electrode layer 405a and the electrode layer 405b are also made of IGZO. It would be good to do so.

[0041] In this embodiment, a conductive film having an atomic ratio of In:Ga:Z is formed by sputtering. After forming a 30 nm IGZO film with n=1:1:1, etching was performed using a resist mask. Then, the electrode layer 405a and the electrode layer 405b are formed.

[0042] Next, a base insulating film 435 is formed so as to cover the substrate 400, the electrode layer 405a, and the electrode layer 405b. The base insulating film 435 is formed by a sputtering method, an MBE method, or a C The VD method, the pulsed laser deposition method, the ALD method, etc. can be appropriately used. When 435 is formed by sputtering, impurity elements such as hydrogen can be reduced. Cut.

[0043] The base insulating film 435 may be formed of silicon oxide, gallium oxide, aluminum oxide, or oxynitride. An insulating oxide layer such as silicon, silicon oxynitride, hafnium oxide, or tantalum oxide It is preferable to use these compounds in a single layer structure or a laminate structure of two or more layers. When forming a laminated structure, for example, C is added to the base insulating layer that contacts the substrate. A silicon oxide film formed by a VD method is used as a base insulating film in contact with the oxide semiconductor layer 409. A silicon oxide film formed by a sputtering method may be used as the oxide layer. By making the insulating layer in contact with the semiconductor layer an oxide insulating layer with a reduced hydrogen concentration, In addition to suppressing the diffusion of hydrogen into the semiconductor layer 409, the oxide semiconductor layer 409 is also provided with an insulating base to prevent oxygen defects. Since oxygen is supplied from the oxide insulating layer that becomes the insulating layer 436, the electrical characteristics of the transistor 420 are improved. It can improve the sex.

[0044] Note that silicon oxynitride here refers to a material whose composition contains more oxygen than nitrogen. For example, oxygen is between 50 atomic % and 70 atomic % and nitrogen is between 0.5 atomic %. % or more and 15 atomic % or less of silicon, and 25 atomic % or more and 35 atomic % or less of silicon. However, the above range is based on the Rutherford Backscattering Spectroscopy (RBS). ackscattering spectrometry and hydrogen forward scattering spectrometry (HFS) : Hydrogen Forward Scattering) The total content of the constituent elements does not exceed 100 atomic percent. .

[0045] Since the base insulating film 435 is in contact with the oxide semiconductor layer 409, at least It is preferable that the amount of oxygen contained in the base insulating film 43 exceeds the stoichiometric composition. When a silicon oxide layer is used as 5, SiO (2+α) (where α>0) do.

[0046] Before the base insulating film 435 is formed, the electrode layer 405a and the electrode layer 405b are subjected to nitrogen plasma treatment. By performing nitrogen plasma treatment, the electrode layer 405a and the electrode layer 40 The contact resistance between the oxide semiconductor layer 409 and the insulating layer 5b can be further reduced. can.

[0047] Next, the base insulating film 435 is polished (for example, chemical mechanical polishing). Mechanical Polishing (CMP) and etching are performed. As a result, the upper surfaces of the electrode layer 405a and the electrode layer 405b are exposed from the base insulating film 435, and the electrodes A base insulating layer 436 is formed so as to be flush with the top surfaces of the layer 405a and the electrode layer 405b. (See FIG. 2(B)). The polishing or etching process may be performed multiple times. When the steps are performed in combination, the order of the steps is not particularly limited. In order to improve the crystallinity of the oxide semiconductor layer provided over the base insulating layer 436, It is preferable to keep the surface as flat as possible.

[0048] In this embodiment, after the electrode layer 405a and the electrode layer 405b are provided, a base insulating layer The method of forming the electrode layer 405a, the electrode layer 405b and the base insulating layer 436 has been described. The method for manufacturing the insulating film 6 is not limited to this. For example, after the insulating base layer 436 is provided on the substrate 400, An opening is formed in the base insulating layer 436 by an etching process or the like, and the opening is filled with a conductive material. By filling the gap, the electrode layer 405a and the electrode layer 405b may be formed.

[0049] In this embodiment, the electrode layer 405a and the electrode layer 405b are embedded in the base insulating layer 436. Therefore, even if the thicknesses of the electrode layers 405a and 405b are increased, the thickness of the oxide film provided later can be increased. Therefore, the electrode layer 405a and the electrode layer 405 The thickness of b may be set to a value sufficient to reduce the resistance of the source and drain regions. For example, The source electrode layer 406a and the drain electrode layer 406b are formed later. The thickness is preferably larger than that of the electrode layer 406b or the oxide semiconductor layer 409.

[0050] Next, an oxide semiconductor film is formed over the base insulating layer 436, the electrode layer 405a, and the electrode layer 405b. The oxide semiconductor film is formed by sputtering, evaporation, pulsed laser deposition (Puls Photoinduced Laser Deposition (PLD), ALD, or MBE, etc. The film can be formed using the following method.

[0051] A resist mask is provided over the oxide semiconductor film, and the oxide semiconductor film is etched into an island shape. The resist mask is then removed, and the oxide semiconductor layer 409 is formed. Alternatively, the oxide semiconductor layer 405 may be formed by completely covering the electrode layer 405a and the electrode layer 405b. The end of 409 overlaps with the electrode layer 405a and the electrode layer 405b. A part of the upper surface of 405b may be exposed.

[0052] When a part of the upper surface of the electrode layer 405a and the electrode layer 405b is exposed, The electrode layer 405b is a layer including a source electrode layer 406a and a drain electrode layer 406b that will be formed later. For example, in FIG. 5A, the electrode layer 405a and the electrode layer 405b are connected to the source 4, the electrode layer 406a and the drain electrode layer 406b are in contact with each other.

[0053] The oxide semiconductor used for the oxide semiconductor layer 409 is at least indium (In), Alternatively, it is preferable that the alloy contains zinc (Zn). In particular, it is preferable that the alloy contains In and Zn. In addition, a stabilizer for reducing variations in electrical characteristics of a transistor including the oxide semiconductor is also provided. It is preferable to have gallium (Ga) in addition to the above as a riser. Other materials that can be used include tin (Sn), hafnium (Hf), and aluminum (Al). It is preferable that

[0054] Other stabilizers include the lanthanides lanthanum (La) and cerium (C e), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium ( Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Hg), Ho, Erbium (Er), Thulium (Tm), Ytterbium (Yb), Ruthenium (Ru) The metal may contain one or more of tungsten (Lu) and zirconium (Zr).

[0055] For example, oxide semiconductors include oxides of single-element metals such as indium oxide, tin oxide, and oxide Zinc oxide, binary metal oxides such as In-Zn oxide, Sn-Zn oxide, Al-Z n-based oxides, Zn-Mg-based oxides, Sn-Mg-based oxides, In-Mg-based oxides, In-G a-type oxides, ternary metal oxides such as In-Ga-Zn-type oxides and In-Al-Zn-type oxides Oxides, In-Sn-Zn oxides, Sn-Ga-Zn oxides, Al-Ga-Zn oxides oxides, Sn-Al-Zn oxides, In-Hf-Zn oxides, In-La-Zn oxides In-Ce-Zn oxides, In-Pr-Zn oxides, In-Nd-Zn oxides , In-Sm-Zn oxide, In-Eu-Zn oxide, In-Gd-Zn oxide, In-Tb-Zn oxide, In-Dy-Zn oxide, In-Ho-Zn oxide, I n-Er-Zn oxide, In-Tm-Zn oxide, In-Yb-Zn oxide, In -Lu-Zn ​​oxides, In-Sn-Ga-Zn oxides, which are oxides of quaternary metals, I n-Hf-Ga-Zn oxide, In-Al-Ga-Zn oxide, In-Sn-Al- Zn-based oxide, In-Sn-Hf-Zn-based oxide, In-Hf-Al-Zn-based oxide are used. There can be.

[0056] In this specification, for example, In-Ga-Zn oxide is an oxide having In, Ga, and Zn as main components. The ratio of In, Ga, and Zn does not matter. Metals other than Ga and Zn may be included.

[0057] In addition, as an oxide semiconductor, InMO3(ZnO) m (m>0 and m is not an integer) In addition, M may be selected from Ga, Fe, Mn, and Co. It indicates one or more metal elements. In2SnO5 (ZnO) n A material expressed as (n>0, and n is an integer) may be used.

[0058] For example, In:Ga:Zn=1:1:1 (=1 / 3:1 / 3:1 / 3) or In:G In-Ga-Zn oxide with an atomic ratio of a:Zn=2:2:1 (=2 / 5:2 / 5:1 / 5) The oxides of In:Sn:Zn=1: 1:1(=1 / 3:1 / 3:1 / 3), In:Sn:Zn=2:1:3(=1 / 3:1 / 6:1 / 2) or In:Sn:Zn=2:1:5(=1 / 4:1 / 8:5 / 8) It is advisable to use an In-Sn-Zn oxide having a molecular ratio or an oxide having a composition close to that.

[0059] For example, the atomic ratio of In, Ga, and Zn is In:Ga:Zn=a:b:c(a+b+ The composition of the oxide with the atomic ratio of In:Ga:Zn=A:B:C (A+B+C = 1), a, b, and c are in the vicinity of the oxide composition (aA)2 +(bB) 2 + (cC) 2 ≦r 2 It means that the following condition is satisfied. For example, r can be set to 0.05. The same is true for other oxides.

[0060] However, the present invention is not limited to these, and may be applied depending on the required electrical characteristics (mobility, threshold value, variation, etc.). In addition, in order to obtain the required electrical characteristics, the carrier concentration, impurity element concentration, defect density, atomic ratio of metal elements to oxygen, interatomic distance, density, etc. It is preferable to use an appropriate one.

[0061] For example, high mobility can be obtained relatively easily with In-Sn-Zn oxides. In the case of In-Ga-Zn oxides, the mobility can be increased by reducing the defect density in the bulk. It is possible.

[0062] Note that the oxide semiconductor film may have either an amorphous structure or a crystalline structure. As a preferred embodiment of the oxide semiconductor film, a CAAC oxide semiconductor (CAAC-OS:C Axis Aligned Crystalline Oxide Semicondu CAAC-OS films are neither completely single crystalline nor completely amorphous. The CAAC-OS film has a crystalline-amorphous mixed phase structure with crystalline and amorphous parts in the amorphous phase. Note that the crystal part is contained within a cube with one side being less than 100 nm. Transmission Electron Microscopy (TEM) The CAAC-OS film was observed under a CT microscope. The boundary between the amorphous and crystalline parts is not always clear. No grain boundaries can be seen in the OS film. In the C-OS film, the decrease in mobility caused by grain boundaries is suppressed.

[0063] The crystal parts in the CAAC-OS film have c-axes that are normal vectors to the surface on which the CAAC-OS film is formed. The triangle is aligned parallel to the normal vector of the ab plane and perpendicular to the ab plane. The metal atoms are arranged in a layered or hexagonal shape when viewed perpendicular to the c-axis. Metal atoms and oxygen atoms are arranged in layers. The orientation of the a-axis may be different. In this specification, when it is simply described as vertical, it means 85 This includes the range of -5° to 95°. Note that the range of the oxygen contained in the oxide semiconductor film may also be included. may be substituted with nitrogen.

[0064] In the CAAC-OS film, the distribution of the crystal parts may not be uniform. In the process of forming the C-OS film, when crystal growth is performed from the surface side of the oxide semiconductor film, The proportion of crystalline parts may be higher near the surface than near the growth surface. By adding impurities to the AC-OS film, the crystalline part becomes amorphous in the impurity-added region. It may also be pawned.

[0065] The c-axis of the crystal part in the CAAC-OS film is the normal vector of the surface on which the CAAC-OS film is formed. The CAAC-OS film shape (the shape of the film on which the film is formed) is Depending on the cross-sectional shape of the surface or the cross-sectional shape of the surface, the directions may differ from each other. The direction of the c-axis of the crystal is the normal vector of the surface on which the CAAC-OS film is formed. The direction of the crystal is parallel to the normal vector of the film or surface. is formed by carrying out a crystallization treatment such as a heat treatment after the film formation.

[0066] The electrical characteristics of transistors using CAAC-OS films change when exposed to visible or ultraviolet light. Therefore, the transistor has high reliability.

[0067] In addition, in the case where the oxide semiconductor layer 409 has a stacked structure, the first oxide semiconductor film, the third oxide semiconductor film, and the An oxide semiconductor film having a different crystallinity may be used as the oxide semiconductor film. oxide semiconductor film, polycrystalline oxide semiconductor film, amorphous oxide semiconductor film, or CAAC-OS film In addition, the first oxide semiconductor film, the second oxide semiconductor film, and the third oxide semiconductor film may be formed by appropriately combining them. When an amorphous oxide semiconductor film is used as one of the conductive films, the internal stress of the oxide semiconductor film and This reduces external stress, reduces the variation in transistor characteristics, and This makes it possible to further improve the reliability of the system.

[0068] Note that part of oxygen contained in the oxide semiconductor film may be replaced with nitrogen.

[0069] For example, when the oxide semiconductor layer is formed of an In-Zn based metal oxide, The composition of the target is, in terms of atomic ratio, In / Zn=1 to 100, preferably In / Zn=1 to 20, and more preferably In / Zn=1 to 10. In order to include an excess of oxygen, The atomic ratio of the metal oxide In:Zn:O=X:Y:Z is preferably set to Z>1.5X+Y. I wish.

[0070] When an In-Ga-Zn oxide is formed as an oxide semiconductor layer by a sputtering method, Preferably, the atomic ratio of In:Ga:Zn is 1:1:1, 4:2:3, 3:1:2, or 1:1. :2, 2:1:3, or 3:1:4 In-Ga-Zn-O targets were used. The oxide semiconductor film was formed using an In-Ga-Zn-O target having the above-mentioned atomic ratio. By forming the film, a polycrystalline semiconductor film or a CAAC-OS film is easily formed.

[0071] In addition, when an In-Sn-Zn oxide is formed as an oxide semiconductor layer by a sputtering method, In this case, the atomic ratio of In:Sn:Zn is preferably 1:1:1, 2:1:3, 1:2:2, Or use the In-Sn-Zn-O target shown in 20:45:35. Deposition of an oxide semiconductor layer using an In-Sn-Zn-O target having a molecular ratio Therefore, a polycrystalline semiconductor film or a CAAC-OS film is easily formed.

[0072] Here, the relative density of the target is 90% or more and 100% or less, preferably 95% or more. The target filling rate should be 99.9% or less. By increasing the target filling rate, the oxide formed The semiconductor layer can be made dense.

[0073] Note that metal oxides that can be used for the oxide semiconductor layer have an energy gap of 2e 5 eV or more, preferably 2.5 eV or more, and more preferably 3 eV or more. Thus, the use of metal oxides with a wide band gap reduces the off-state current of transistors. It is possible.

[0074] The amount of alkali metal and alkaline earth metal in the oxide semiconductor layer is preferably small. , these concentrations are preferably 1 x 10 18 atoms / cm 3 More preferably, 2×10 16 atoms / cm 3 Alkali metals and alkaline earth metals are When the junction is bonded to a ferroelectric semiconductor, carriers can be generated, increasing the off-state current of the transistor. This is because it can cause the problem to worsen.

[0075] The oxide semiconductor film may have a structure in which a plurality of oxide semiconductor films are stacked. The oxide semiconductor film is a stack of a first oxide semiconductor film and a second oxide semiconductor film. The oxide semiconductor film and the second oxide semiconductor film may be made of metal oxides having different compositions. For example, one of a binary metal oxide, a quaternary metal oxide, and a second oxide semiconductor film is formed using ... The oxide semiconductor film includes a binary metal oxide or a quaternary metal oxide different from the first oxide semiconductor film. may also be used.

[0076] In addition, the first oxide semiconductor film and the second oxide semiconductor film are made to contain the same elements, and the composition of both films is For example, the atomic ratio of the first oxide semiconductor film may be set to In:Ga:Zn=1. and the second oxide semiconductor film is In:Ga:Zn=3:1:2 or a ratio of about In:Ga:Zn=3:1:2. The atomic ratio of the first oxide semiconductor film may be In:Ga:Zn = 1:3:2 or in the vicinity thereof, and the atomic ratio of the second oxide semiconductor film is In:Ga:Zn =2:1:3 or a vicinity thereof.

[0077] At this time, the gate electrode layer to be provided later is formed between the first oxide semiconductor film and the second oxide semiconductor film. The content ratio of In and Ga in the oxide semiconductor film on the side closer to 401 (channel side) is In>Ga. In addition, the In and G of the oxide semiconductor film on the side farther from the gate electrode (the back channel side) It is preferable that the content of a satisfies In≦Ga.

[0078] In addition, the oxide semiconductor film has a three-layer structure, and the first oxide semiconductor film, the second oxide semiconductor film, and the third oxide semiconductor film are The constituent elements may be the same, but the compositions may be different. For example, the first oxide semiconductor The atomic ratio of the conductor film is In:Ga:Zn=1:3:2, and the atomic ratio of the second oxide semiconductor film is The atomic ratio of the third oxide semiconductor film is In:Ga:Zn=3:1:2. :Zn=1:1:1 may also be used.

[0079] An oxide semiconductor film having a smaller atomic ratio of In than Ga and Zn, typically having an atomic ratio of In: In the first oxide semiconductor film, the atomic ratio of Ga:Zn is 1:3:2, and the number of atoms of In is greater than that of Ga and Zn. The oxide semiconductor film having a large ratio, typically the second oxide semiconductor film, and the oxide semiconductor film having Ga, Zn, and In comparison with an oxide semiconductor film having the same In atomic ratio, typically a third oxide semiconductor film, The first oxide semiconductor has an atomic ratio of In:Ga:Zn=1:3:2. If the film has an amorphous structure, the insulating properties are further improved.

[0080] In addition, since the constituent elements of the first oxide semiconductor film to the third oxide semiconductor film are the same, The first oxide semiconductor film has a small number of trap states at the interface with the second oxide semiconductor film. Therefore, by using the oxide semiconductor film with the above structure, the deterioration of the transistor over time and the optical BT stripping can be prevented. This can reduce the amount of variation in threshold voltage due to the resist test.

[0081] In oxide semiconductors, the s orbitals of heavy metals mainly contribute to carrier conduction, and the In content By increasing the amount of Ga, more s orbitals overlap, resulting in an oxide with a composition of In>Ga. In oxides with a composition of In≦Ga have higher mobility. The formation energy of oxygen vacancies is larger than that of Ga, so oxygen vacancies are less likely to occur. The oxide having the composition In>Ga has stable characteristics as compared with the oxide having the composition In>Ga.

[0082] An oxide semiconductor with a composition of In>Ga is applied to the channel side, and In≦ By using an oxide semiconductor with a Ga composition, the field-effect mobility and signal This makes it possible to further increase reliability.

[0083] The thickness of the oxide semiconductor layer 409 is 1 nm to 100 nm, preferably 1 nm to 20 The transistor 420 includes an oxide semiconductor layer 409, an electrode layer 405a, and an electrode In the overlapping region of the electrode layer 405b, the electrode layer 405b is connected to the wiring layer 465a and the wiring layer 465b, respectively. Therefore, even if the oxide semiconductor layer is thinned by miniaturization of the transistor, the oxide The electrode layer 405a and the electrode layer 405b overlapping with the oxide semiconductor layer 409 In order to ensure electrical connection between the compound semiconductor layer 409 and the wiring layers 465a and 465b, This can be done.

[0084] The oxide semiconductor layer 409 is preferably formed by a sputtering method at a substrate heating temperature of 100° C. 600°C or less, preferably 150°C or more and 550°C or less, more preferably 200°C or less The film is formed in an oxygen gas atmosphere at a temperature of 500°C or less. In addition, the concentration of the impurity element in the oxide semiconductor layer 409 is reduced. The atomic arrangement of the SiO2 is improved and the density is increased, making it easier to form a polycrystalline or CAAC-OS film. .

[0085] Note that when the CAAC-OS film is formed, for example, a polycrystalline oxide semiconductor sputtering The film is formed by a sputtering method using a sputtering target. When ions bombard the sputtering target, the crystalline regions in the target are transformed into a- Sputtering in the form of a flat plate or pellet cleaved from the b-plane and with a surface parallel to the ab-plane In this case, the plate-like sputtered particles may peel off as crystalline particles. By reaching the substrate while maintaining the above state, a CAAC-OS film can be formed.

[0086] In addition, the following conditions are preferably applied to form the CAAC-OS film.

[0087] By reducing the amount of impurities mixed in during film formation, it is possible to prevent the crystal state from being destroyed by impurities. For example, the concentration of impurities (hydrogen, water, carbon dioxide, nitrogen, etc.) present in the film formation chamber In addition, the impurity concentration in the deposition gas may be reduced. A deposition gas having a temperature of −80° C. or lower, preferably −100° C. or lower is used.

[0088] In addition, by increasing the substrate heating temperature during film formation, the migration of sputtered particles after they reach the substrate is reduced. Specifically, the substrate heating temperature is set to 100° C. or higher and 740° C. or lower, preferably The deposition temperature is set to 200°C or higher and 500°C or lower. When a plate-shaped sputtered particle reaches a substrate, migration occurs on the substrate, The flat surface of the sputtered particle adheres to the substrate.

[0089] In addition, by increasing the oxygen ratio in the deposition gas and optimizing the power, plasma damage during deposition is reduced. The oxygen ratio in the deposition gas is preferably 30% by volume or more, and more preferably 100% by volume or more. The product is %.

[0090] As an example of a sputtering target, an In-Ga-Zn oxide target is The following is shown:

[0091] InO X powder, GaO Y Powder and ZnO Z The powders are mixed in a specified number of moles and then pressurized. By heat treatment at a temperature between 1000 and 1500℃, polycrystalline In-Ga -Zn-based oxide target. Note that X, Y, and Z are any positive numbers. Here, The predetermined molar ratio is, for example, InO X powder, GaO Y Powder and ZnO Z Powder, 2: 2:1, 8:4:3, 3:1:1, 1:1:1, 4:2:3 or 3:1:2. The type of powder and the molar ratio of the powder to be mixed should be determined according to the sputtering target to be prepared. The above can be changed as appropriate depending on the case.

[0092] Furthermore, by forming the film in an oxygen gas atmosphere, no extra atoms such as rare gases are included, Therefore, it is easy to form a polycrystalline semiconductor film or a CAAC-OS film. A rare gas mixture atmosphere may be used. In that case, the ratio of oxygen gas is preferably 30% by volume or more. The oxide semiconductor film is contained at 50% by volume or more, and more preferably at 80% by volume or more. It is preferable that the argon and oxygen used in the film formation do not contain water, hydrogen, etc. For example, The purity of argon is 9N (dew point -121℃, water 0.1ppb, hydrogen 0.5ppb), and oxygen The purity is preferably 8N (dew point -112°C, water 1 ppb, hydrogen 1 ppb).

[0093] In this embodiment, sputtering is performed in an atmosphere with an argon / oxygen flow ratio of 2:1. Using the annealing method, a 10 nm thick IGZO film with an atomic ratio of In:Ga:Zn=3:1:2 was formed. do.

[0094] Since it is relatively easy to obtain a flat surface for an amorphous oxide semiconductor, Transistors using this material can reduce the scattering of carriers (electrons) at the interface during operation, and are relatively easy to manufacture. A relatively high mobility can be easily obtained.

[0095] In addition, in a crystalline oxide semiconductor, defects in the bulk can be further reduced, and the surface By improving the flatness of the oxide semiconductor, it is possible to obtain a mobility equal to or higher than that of an oxide semiconductor in an amorphous state. In order to improve the flatness of the surface, it is preferable to form an oxide semiconductor on a flat surface. Specifically, the average surface roughness (Ra) is 1 nm or less, preferably 0.3 nm or less, and more preferably It is preferable to form the surface on a thickness of 0.1 nm or less.

[0096] Note that Ra is defined in JIS B601:2001 (ISO4287:1997). This is a three-dimensional extension of the arithmetic mean roughness, which is currently used, so that it can be applied to curved surfaces. It can be expressed as "the average of the absolute values ​​of the deviation from the specified surface to the target surface" and is defined by the following formula.

[0097]

number

[0098] Here, the specified surface is the surface to be measured for roughness, and has coordinates (x1, y1, f(x1, y 1))(x1,y2,f(x1,y2))(x2,y1,f(x2,y1))(x2,y 2,f(x2,y2)) is a rectangular area represented by four points, and the specified surface is projected onto the xy plane. The area of ​​the rectangle is S0, and the height of the reference plane (average height of the specified plane) is Z0. Can be measured using an atomic force microscope (AFM) It is.

[0099] The reference plane is a plane parallel to the XY plane at the average height of the specified plane. When the average value of the height of the fixed surface is Z0, the height of the reference surface is also expressed as Z0.

[0100] In this way, in the region where the channel of the oxide semiconductor layer is formed, the average surface area of ​​the undercoat insulating layer To reduce the roughness to 0.3 nm or less, a flattening process is required. This may be done before the formation of the conductive film.

[0101] For example, dry etching or the like may be performed as the planarization treatment. Examples of gases include chlorine, boron chloride, silicon chloride, and chlorine-based gases such as carbon tetrachloride, tetrafluoroethylene, and tetrafluoroethylene. Fluorine-based gases such as carbon fluoride, sulfur fluoride, and nitrogen fluoride may be used.

[0102] The amount of hydrogen contained in the oxide semiconductor layer is preferably as small as possible. In addition to atoms, hydrogen may be present as molecules, water, hydroxyl groups, or other hydrides. Therefore, excess hydrogen (including water and a hydroxyl group) contained in the oxide semiconductor layer is removed (dehydrated or It is preferable to carry out a heat treatment for the purpose of hydrogenation or dehydrogenation. The temperature of the heat treatment is 300°C or higher for 7 The temperature must be below 00°C or below the distortion point of the substrate. Heat treatment must be performed under reduced pressure or in a nitrogen atmosphere. The heat treatment can be performed after the oxide semiconductor film is formed and before it is processed into an island shape. Alternatively, it may be carried out after processing into islands. This may be carried out multiple times, or may be combined with other heat treatments.

[0103] The heat treatment is carried out in a reduced pressure or inert atmosphere, and then the temperature is maintained while the heat treatment is carried out in an oxidizing atmosphere. It is preferable to switch the atmosphere to a reduced pressure or inert atmosphere for further heat treatment. When the heat treatment is performed at room temperature, the concentration of impurities (e.g., hydrogen) in the oxide semiconductor layer can be reduced. However, at the same time, oxygen vacancies may occur. This can be reduced by heat treatment in an oxidizing atmosphere.

[0104] By performing heat treatment on the oxide semiconductor layer, the concentration of impurity elements such as hydrogen in the layer can be reduced to an extremely low level. As a result, it is possible to obtain the field effect mobility of the transistor at an ideal field effect mobility. It is possible to increase the mobility to nearly the same level.

[0105] Note that the oxide semiconductor layer 409 preferably contains excess oxygen compared to the stoichiometric composition. When oxygen is excessively contained, the oxide semiconductor layer 409 to be formed may be oxidized due to oxygen vacancies. In order to contain excess oxygen, the amount of oxygen present during film formation must be The oxide semiconductor film may be formed under conditions in which the amount of oxygen contained therein is large, or the oxide semiconductor film may be formed under conditions in which the amount of oxygen contained therein is large. The oxygen is introduced into the film by introducing oxygen radicals, oxygen atoms, or oxygen ions. The oxygen introduction method includes ion implantation, ion doping, and proton implantation. Plasma ion implantation and plasma treatment can be used. Cut.

[0106] Note that in the case where an oxide insulating layer is used as a base insulating layer, an oxide semiconductor layer is formed over the oxide insulating layer. By heating the oxide semiconductor layer in the provided state, oxygen can be supplied to the oxide semiconductor layer. The oxygen defects in the oxide semiconductor layer can be reduced, and the electrical characteristics can be improved. The heating step is performed in a state where the oxide insulating layer and the oxide insulating layer are at least partially in contact with each other. Note that the heat treatment may be performed to heat the oxide semiconductor film into islands. It may be performed before processing or after processing into islands. By performing the heat treatment before the insulating layer is removed, the amount of oxygen released from the insulating layer to the outside is small. Therefore, more oxygen can be supplied to the oxide semiconductor layer, which is preferable.

[0107] Next, a gate insulating film 452 is formed over the oxide semiconductor layer 409 (see FIG. 2C).

[0108] The material of the gate insulating film 452 is hafnium oxide, yttrium oxide, hafnium silicate, etc. (HfSi x O y , x>0, y>0), nitrogen-doped hafnium silicate (H fSi x O y , x>0, y>0), hafnium aluminate (HfAl x O y , x>0, By using high-k materials such as lanthanum oxide, gate leakage current is reduced. In addition, the gate insulating film 452 may have a single-layer structure or a stacked structure. good.

[0109] The thickness of the gate insulating film 452 is set to 1 nm or more and 20 nm or less. The method may be a deposition method, a CVD method, a PLD method, an ALD method, or the like. 52 is a sputtering target surface and a plurality of substrate surfaces are set substantially perpendicular to the sputtering target surface. Alternatively, the film may be formed using a sputtering apparatus which performs film formation in a vacuum state.

[0110] In this embodiment, a silicon oxynitride film is formed to a thickness of 20 nm by CVD.

[0111] The gate insulating film 452 is in contact with the oxide semiconductor layer like the base insulating layer 436; It is preferred that there is at least an amount of oxygen in the layer (bulk) that exceeds the stoichiometric composition. stomach.

[0112] In order to improve coverage of the gate insulating film 452, a gate insulating film 452 is also formed on the top surface of the oxide semiconductor layer 409. In particular, a thin insulating layer is used as the gate insulating film 452. In this case, the surface of the oxide semiconductor layer 409 preferably has good flatness.

[0113] Next, a conductive film and an insulating film are stacked over the gate insulating film 452 and the oxide semiconductor layer 409. The conductive film and the insulating film are then etched to form the electrode layer 405a and the electrode layer 405b. A gate electrode layer 401 and an upper insulating layer 413 are formed in the sandwiched region and the region overlapping the sandwiched region (FIG. (See 2(D)).

[0114] The material of the gate electrode layer 401 is molybdenum, titanium, tantalum, tungsten, aluminum, etc. Metallic materials such as aluminum, copper, chromium, neodymium, scandium, etc., or alloys containing these as their main components The gate electrode layer 401 can be formed using a gold material. Semiconductor films such as element-doped polycrystalline silicon films, nickel silicide, etc. Silicide films containing indium tin oxide and tungsten oxide may also be used. Indium oxide containing tungsten oxide, indium zinc oxide containing titanium oxide Indium oxide, indium tin oxide with titanium oxide, indium zinc oxide, acid Conductive materials such as indium tin oxide doped with silicon dioxide can also be used. Alternatively, the conductive material and the metallic material may be laminated together.

[0115] In addition, a layer of the gate electrode layer 401 in contact with the gate insulating film 452 is made of a metal oxide containing nitrogen. In-Ga-Zn-O films containing nitrogen, In-Sn-O films containing nitrogen, , In-Ga-O films containing nitrogen, In-Zn-O films containing nitrogen, and Sn-O films containing nitrogen A film containing nitrogen, an In-O film, or a metal nitride film (InN, SnN, etc.) can be used. These films have a work function of 5 eV or more, preferably 5.5 eV or more, and are used as the gate electrode. When used as the gate insulating film, the threshold voltage of the electrical characteristics of the transistor can be made positive.

[0116] In this embodiment, a tungsten film having a thickness of 100 nm is formed by sputtering. do.

[0117] The upper insulating layer 413 is typically made of silicon oxide, silicon oxynitride, or aluminum oxide. Aluminum, aluminum oxide nitride, silicon nitride, aluminum nitride, silicon oxide nitride, nitride An inorganic insulating material such as aluminum oxide can be used. The upper insulating layer 413 is The film can be formed by using a CVD method, a sputtering method, or the like.

[0118] In this embodiment, the upper insulating layer 413 is formed by depositing silicon oxynitride at 2000 nm by a CVD method. Then, the upper insulating layer 413 and the gate electrode layer 414 are formed by dry etching. At this time, the gate insulating layer 402 may be etched as well. good.

[0119] Next, the oxide semiconductor layer 40 is formed by using the gate electrode layer 401 and the upper insulating layer 413 as a mask. An impurity element 421 is introduced into the oxide semiconductor layer 409 so as not to overlap with the gate electrode layer 401. The low resistance region 404a and the low resistance region 404b are formed in a self-aligned manner in the region (FIG. 3( Note that the region where the impurity element 421 is not introduced becomes the channel formation region 403. do.

[0120] Therefore, in the oxide semiconductor layer 409, a channel formation region overlapping with the gate electrode layer 401 is formed. The channel formation region 403 is sandwiched between the first region 403 and the second region 404, which has a lower resistance than the channel formation region 403. The low resistance region 404a and the low resistance region 404b are formed. The methods include ion implantation, ion doping, plasma immersion ion implantation, etc. Methods such as the antennary method can be used.

[0121] The impurity elements introduced are phosphorus, boron, nitrogen, arsenic, argon, aluminum, or Molecular ions containing these elements can be used. The dose of these elements is 1×10 13 ~5×10 16 ions / cm2 It is preferable that the impurity element is phosphorus. When introducing, the acceleration voltage is preferably 0.5 to 80 kV.

[0122] In this embodiment mode, phosphorus is introduced as the impurity element.

[0123] Note that the treatment of introducing the impurity element into the oxide semiconductor layer 409 may be performed multiple times. When the process of introducing the impurity element into the compound semiconductor layer 409 is performed multiple times, the impurity element is introduced multiple times. The concentration may be the same for all treatments, or may be changed for each treatment.

[0124] Impurity elements are introduced to form low resistance regions 404a and 404b having reduced resistance. By including the oxide semiconductor layer 409 and the source electrode layer 406a Therefore, the resistance of the source electrode layer 406a and the drain electrode layer 406b is reduced. The electric field in the vicinity of the drain electrode layer 406b is relaxed, and the transistor 420 has high on-state characteristics. A semiconductor device capable of high-speed operation and high-speed response and having excellent electrical characteristics can be obtained.

[0125] Note that the crystal structure of the oxide semiconductor layer may be changed by the introduction of an impurity element. The semiconductor device of the embodiment may include an oxide semiconductor layer having different crystallinity depending on the region. For example, the channel formation region 403 has a higher resistance than the low resistance region 404a and the low resistance region 404b. Specifically, the oxide semiconductor of the channel formation region 403 may be C The electrode layers 405a and 405b are made of an AAC-OS film. The region in contact with the electrode layer 405b may be an amorphous film.

[0126] In addition, when the electrode layer 405a and the electrode layer 405b are formed using an oxide semiconductor material, In this case, when the impurity element is introduced into the oxide semiconductor layer 409, Impurity elements are also introduced into the electrode layer 405b, so that the resistance of the electrode layer 405a and the electrode layer 405b is reduced. In the electrode layer 405a and the electrode layer 405b, the oxide is formed in the low-resistance region. Since the semiconductor layer 409 is in contact with the semiconductor layer 409, the contact resistance is low and the semiconductor device has excellent on-characteristics. It is possible.

[0127] Next, an insulating film is formed on the gate electrode layer 401 and the upper insulating layer 413, and the insulating film is etched. The sidewall insulating layer 412a and the sidewall insulating layer 412b are formed by etching. The gate insulating film 452 is etched using the insulating layer 401 and the sidewall insulating layers 412a and 412b as a mask. Then, a gate insulating layer 402 is formed (see FIG. 3B).

[0128] The sidewall insulating layer 412a and the sidewall insulating layer 412b are formed using the same material and method as the upper insulating layer 413. In this embodiment, a silicon oxynitride film is formed by a CVD method. It is formed to a film thickness of 70 nm.

[0129] Next, the oxide semiconductor layer 409, the gate insulating layer 402, the gate electrode layer 401, and the sidewall insulating layer A source electrode layer and a drain electrode layer are formed on the sidewall insulating layer 412a, the sidewall insulating layer 412b and the upper insulating layer 413. A conductive film that will become the electrode layers (including wiring and the like formed in the same layer) is formed.

[0130] The conductive film can be formed using a material and a method similar to those of the gate electrode layer 401. In this embodiment, a tungsten film having a thickness of 30 nm is formed by sputtering.

[0131] A resist mask is formed on the conductive film by a photolithography process, and selective etching is performed. After forming an island-shaped conductive film 406 by this process, the resist mask is removed (see FIG. 3(C)). In this etching step, the conductive film 406 in a region overlapping with the gate electrode layer 401 is No removal will be performed.

[0132] An insulating layer 415 is formed over the island-shaped conductive film 406 (see FIG. 3D).

[0133] The insulating layer 415 can be formed using the same materials and methods as the upper insulating layer 413. The insulating layer 415 is formed to a thickness that can planarize unevenness caused by the transistor 420. In this embodiment, silicon oxynitride is formed to a thickness of 500 nm by a CVD method.

[0134] The insulating layer 415 may be a single layer or a laminate of different insulating layers. By using the layered structure, as in the transistor 430 shown in FIG. 6a and the drain electrode layer 406b, an insulating layer 415 and an insulating layer 416 are provided over the drain electrode layer 406a and the drain electrode layer 406b. For example, the insulating layer 416 can be an aluminum oxide layer, and the insulating layer 415 can be an oxide layer. The insulating layer may be a silicon nitride layer.

[0135] Next, the insulating layer 415 and the conductive film 406 are subjected to a chemical mechanical polishing process to remove the upper insulating layer 413. The insulating layer 415 and the conductive film 406 are partly removed so as to expose the insulating layer 415 (see FIG. 4A). .

[0136] By the polishing treatment, the conductive film 406 overlapping with the gate electrode layer 401 is removed, and the conductive film 4 06 becomes a source electrode layer 406a and a drain electrode layer 406b.

[0137] The source electrode layer 406a and the drain electrode layer 406b are provided on the top surface of the oxide semiconductor layer 409 and The sidewall insulating layer 412a and the sidewall insulating layer 412b are in contact with each other. The drain electrode layer 406a and the drain electrode layer 406b are in contact with the oxide semiconductor layer 409 ( The distance (shortest distance) between the gate electrode layer 401 and the sidewall insulating layer 412a is The width of the sidewall insulating layer 412b in the channel length direction is also the width of the sidewall insulating layer 412b. In this process, the variation in the minimum distance can be controlled.

[0138] In this embodiment mode, the insulating layer 415 and the conductive film 406 are removed by a chemical mechanical polishing method. However, other cutting (grinding, polishing) methods may be used. In the process of removing the conductive film 406, a cutting (grinding, polishing) method such as a chemical mechanical polishing method is used. In addition, we also use etching methods (dry etching, wet etching) and plasma processing. For example, a chemical mechanical polishing process may be followed by dry etching. The flatness of the treated surface may be improved by performing a cutting (grinding, polishing) method or a plasma treatment. When the etching method, plasma treatment, etc. are combined with the deposition method, the order of the steps is not particularly limited. First, the thickness and surface roughness of the insulating layer 415 and the conductive film 406 are appropriately determined. It is enough to set it.

[0139] In this embodiment, the source electrode layer 406a and the drain electrode layer 406b are The side surfaces of the sidewall insulating layer 412a and the sidewall insulating layer 412b provided on the side surfaces of the base electrode layer 401 The side walls of the side wall insulating layer 412a and the side wall insulating layer 412b are provided so as to contact the The source electrode layer 406a and the drain electrode layer 40 The shape of 6b varies depending on the conditions of the polishing process for removing the conductive film 406. As shown in FIG. 1, the sidewall insulating layer 412a, the sidewall insulating layer 412b and the upper insulating layer 413 are polished. However, depending on the polishing conditions, In this case, the upper ends of the source electrode layer 406a and the drain electrode layer 406b are approximately aligned with each other. There are also.

[0140] In the step of removing the conductive film 406, for example, as shown in FIG. 5(B), A transistor 440 in which the entire edge layer 413 is removed and the gate electrode layer 401 is exposed. Furthermore, a part of the gate electrode layer 401 may also be removed. The structure of exposing the gate electrode layer 401, like the transistor 440, allows other It can be used in integrated circuits in which wiring and semiconductor elements are stacked.

[0141] Next, the insulating layer 415, the source electrode layer 406a, the drain electrode layer 406b and the upper insulating layer An insulating layer 417 is formed on the upper insulating layer 413 (see FIG. 4B). The insulating layer 417 can be formed using a material and a method similar to those of the insulating layer 13. When a high-quality inorganic insulating layer (typically, an aluminum oxide film or the like) is used, the transistor 420 It functions as a protective insulating film.

[0142] In this embodiment, the insulating layer 417 is formed of oxidized aluminum by a sputtering method. The thickness of the aluminum film is 50 nm and the thickness of the silicon oxynitride film is 350 nm, which is formed by the CVD method. A layered structure is used.

[0143] Furthermore, after the aluminum oxide film is formed, a heat treatment may be performed. The function of preventing water or hydrogen from entering the oxide semiconductor layer and removing oxygen from the oxide semiconductor layer is Therefore, the oxide semiconductor layer 409 or an insulating layer in contact with the oxide semiconductor layer 409 has a function of preventing the oxide semiconductor layer 409 from being peeled off. The oxygen content of the mixture is in a region where the oxygen content exceeds the stoichiometric composition (also called the oxygen excess region). Then, by performing heat treatment with the aluminum oxide film provided, the oxide semiconductor layer At least one oxygen excess region is present in the film or at the interface between the insulating layer and the oxide semiconductor layer. can be provided.

[0144] Next, the insulating layer 41 is formed in the regions overlapping the electrode layer 405a and the electrode layer 405b. 7 and the insulating layer 415 to reach the source electrode layer 406a and the drain electrode layer 406b. The openings 455a and 455b are formed through the openings 455a and 455b (see FIG. 4C). The etching is carried out by selective etching using a wafer. The opening may be formed by hot etching or by a combination of both. The shape of the insulating film is not particularly limited as long as it reaches the source electrode layer 406a and the drain electrode layer 406b. However, by making it tapered as shown in FIG. 4(C), the wiring to be formed later can be easily formed. This is preferable because the layer can be formed without being broken. This creates a larger opening.

[0145] In the process of forming the openings 455a and 455b, the insulating layer 417 and the insulating layer 415 are By etching, the source electrode layer 406a, the drain electrode layer 406b, or the oxide semiconductor The dielectric layer 409 may also be etched, resulting in a decrease in thickness. The openings 455a and 455b are formed in the regions overlapping the electrode layers 405a and 405b. Therefore, even if the thickness is reduced by etching, the oxide semiconductor layer 409 and the wiring Electrical connections to the layers can be achieved.

[0146] Next, a conductive material is used to form the wiring layer 4 on the opening 455a, the opening 455b, and the insulating layer 417. The wiring layers 465a and 465b are formed (see FIG. 4(D)). The same material as that used for the gate electrode layer 401 can be used. The titanium film was 50 nm, the aluminum film was 100 nm, and the titanium film was Then, a 50 nm silicon film is formed.

[0147] Through the above steps, the transistor 420 can be manufactured.

[0148] In the manufacturing process of the transistor described in this embodiment, a gate electrode layer 401 and an upper insulating layer A conductive film 406 provided on the edge layer 413, the sidewall insulating layer 412a, and the sidewall insulating layer 412b. The conductive film 406 is cut by chemical mechanical polishing to remove the conductive film 406. An electrode layer 406a and a drain electrode layer 406b are formed.

[0149] The source electrode layer 406a and the drain electrode layer 406b are formed on the oxide semiconductor layer 409. The insulating layer 412 is provided in contact with the surface of the insulating layer 412 and the sidewall insulating layer 412a or the sidewall insulating layer 412b. In the region where the source electrode layer 406a and the drain electrode layer 406b are in contact with the oxide semiconductor layer 409, The distance (shortest distance) between the contact region and the gate electrode layer 401 is determined by the sidewall insulating layer 41. 2a and the sidewall insulating layer 412b in the channel length direction, which allows further miniaturization to be achieved. The variation in the shortest distance can be controlled in the manufacturing process.

[0150] In this manner, the source electrode layer 406a or the drain electrode layer 406b and the oxide semiconductor layer 40 9 and the gate electrode layer 401. A region in which the electrode layer 406a or the drain electrode layer 406b is in contact with the oxide semiconductor layer 409 and The resistance between the gate electrode layers 401 is reduced, and the on-characteristics of the transistor 420 are improved. can be done.

[0151] In addition, the gate electrode in the step of forming the source electrode layer 406a and the drain electrode layer 406b In the step of removing the conductive film 406 over the layer 401, etching is performed using a resist mask. Since no process is used, precise processing can be performed accurately. In the process, the yield of transistors with fine structures with small variations in shape and characteristics is It can be produced more easily.

[0152] In addition, the semiconductor device described in this embodiment can be obtained by introducing an impurity element into the oxide semiconductor layer. and forming a low resistance region by forming a source electrode layer and a drain electrode layer in contact with the low resistance region. Therefore, the source electrode layer and the drain electrode layer and the oxide semiconductor layer are The contact resistance of the conductor layer can be reduced. By providing the electrode layer 405a and the electrode layer 405b in the lower part, the source region and the drain region This allows for a thicker film, reduces the resistance of the source and drain regions, and The on-state characteristics can be improved.

[0153] Although not shown, an insulating layer may be further provided over the transistor 420. Representative examples of the thin film include a silicon oxide film, a silicon oxynitride film, an aluminum oxide film, and a nitride oxide film. aluminum oxide film, hafnium oxide film, gallium oxide film, silicon nitride film, aluminum nitride film A single layer of an inorganic insulating film such as an aluminum film, a silicon nitride oxide film, or an aluminum nitride oxide film, or Lamination may be used.

[0154] After the insulating layer is formed, a heating step may be further performed. For example, the insulating layer may be heated at 100° C. or higher to 200° C. in air. A heating step may be performed at a temperature of 0.5° C. or less and for 1 hour to 30 hours. You can either hold the heat and heat it, or heat it from room temperature to a temperature between 100°C and 200°C. The heating and cooling from the heating temperature to room temperature may be repeated several times.

[0155] In addition, in order to reduce surface unevenness caused by the transistor 420, a planarizing insulating film may be formed. The planarizing insulating film may be made of a material such as polyimide, acrylic, or benzocyclobutene resin. In addition to the above organic materials, low-k materials can be used. In addition, it is possible to laminate multiple insulating films made of these materials. In this way, a planarization insulating film may be formed.

[0156] This embodiment mode can be combined with other embodiment modes as appropriate.

[0157] (Embodiment 2) In this embodiment, a semiconductor device according to one embodiment of the present invention, which is different from that in Embodiment 1, will be described. In this embodiment, only the differences from the first embodiment will be described. FIG 6A illustrates a top view of a transistor according to one embodiment of the present invention. 6B is a cross-sectional view taken along dashed line B1-B2 in FIG. 6A.

[0158] The semiconductor device including the transistor 520 is formed by forming a base insulating layer 536 and a base insulating film 538 on a substrate 400. Electrode layer 505a and electrode layer 505b on edge layer 536, and electrode layer 505a and electrode layer 505 low resistance region 404a and low resistance region 404b, which are in contact with low resistance region 404a and low resistance region 404b, respectively; and a channel formation region 403 on a base insulating layer 536, which is sandwiched between the low resistance region 404b. a gate insulating layer 402 over the oxide semiconductor layer 409; A gate electrode layer 401 on an insulating layer 402 and a sidewall insulating layer 4 covering the side surface of the gate electrode layer 401 12a and a sidewall insulating layer 412b, and an upper insulating layer 413 covering the upper surface of the gate electrode layer 401. A sidewall insulating layer 412a and a sidewall insulating layer 412b are formed on the base insulating layer 536 and the oxide semiconductor layer 409. The source electrode layer 406a and the drain electrode layer 406b are in contact with the side surfaces of the source electrode 12b. An insulating layer 415 on the layer 406a and the drain electrode layer 406b, and a source electrode layer 406a, drain electrode layer 406b, sidewall insulating layer 412a, sidewall insulating layer 412b, and The insulating layer 417 on the partial insulating layer 413 and the insulating layer 415 and the openings provided in the insulating layer 417 are The wiring layer 46 is in contact with the source electrode layer 406a and the drain electrode layer 406b through the 5a and a wiring layer 465b.

[0159] The low resistance region 404a and the low resistance region 404b are connected to the electrode layer 505a and the electrode layer 505b. The electrode layer 505a and the electrode layer 505b are made of a metal, a metal compound, or a conductive metallization. The low resistance region 404a and the low resistance region 404b are made of a transistor. The source and drain regions of the source and drain regions of the By providing electrode layers 505a and 505b in the lower portion, the source region and the drain region This allows for a thicker film, reduces the resistance of the source and drain regions, and The on-state characteristics can be improved.

[0160] The transistor 520 described in this embodiment has a structure similar to that of the transistor 420 described in Embodiment 1. In comparison, the difference is that the electrode layer 505a and the electrode layer 505b are provided on a base insulating layer. Since the electrode layer 505a and the electrode layer 505b are not embedded in the base insulating layer, The transistor 520 can be fabricated in fewer steps than the transistor 420 .

[0161] A method for manufacturing the transistor 520 will be described.

[0162] First, a base insulating layer 536 is formed on the substrate 400. The base insulating layer 536 is formed as described in the first embodiment. The base insulating layer 436 can be formed using a material and a method similar to those of the base insulating layer 436 described above.

[0163] Next, a conductive film that will become the electrode layer 505a and the electrode layer 505b is formed, and then photolithography is performed. Selective etching is performed in a process to form the electrode layer 505a and the electrode layer 505b.

[0164] The conductive film to be the electrode layer 505a and the electrode layer 505b is the same as the electrode layer 405a shown in Embodiment 1. The insulating layer 405 can be formed using a material and a manufacturing method similar to those of the electrode layer 405b. In consideration of the coverage of the oxide semiconductor layer 409 formed on the electrode layer 505a and the electrode layer 505 It is preferable that both ends of the electrode layer 505a and the electrode layer 50b are tapered. The thickness of the electrode layer 505a and the electrode layer 505b is set so that the oxide semiconductor layer 409 to be formed later is It is preferable that the film thickness is such that b can be sufficiently covered.

[0165] After the conductive film is formed, the conductive film is etched to form island-shaped electrode layers 505a and 505b. Before the deposition, the conductive film may be subjected to a nitrogen plasma treatment. As a result, the electrode layer 505a, the electrode layer 505b, and the oxide semiconductor layer 409 to be formed later are The contact resistance can be reduced.

[0166] Next, an oxide semiconductor film is formed over the base insulating layer 536, the electrode layer 505a, and the electrode layer 505b. The oxide semiconductor film is then processed into an island-shaped oxide semiconductor layer 409 by etching. The oxide semiconductor layer 409 is formed on the electrode layer 505a as in the transistor 520 illustrated in FIG. and electrode layer 505b are not entirely covered, but at least a portion of electrode layer 505a and electrode layer 505b are partially covered. 5b, or as in the transistor 530 shown in FIG. It may be configured to cover the entirety of the electrode layer 505a and the electrode layer 505b.

[0167] The contact area between the oxide semiconductor layer 409 and the electrode layer 505a and the electrode layer 505b is appropriately adjusted. As a result, contact between the oxide semiconductor layer 409 and the electrode layer 505a and the electrode layer 505b is improved. The oxide of the electrode layer 505a and the electrode layer 505b can be appropriately set. The area not covered with the semiconductor layer 409 is a region for forming a source electrode layer 406a and a drain electrode layer 406b. The first and second electrodes 406a and 406b may be in contact with each other.

[0168] The oxide semiconductor layer 409 is formed using a material and a method similar to those described in Embodiment 1. The thickness of the oxide semiconductor layer can be set to be equal to that of the electrode layer 505a and the electrode layer 505b. It is preferable that the thickness is sufficiently large so that no step discontinuities due to the above phenomenon occur.

[0169] In the following description, the gate electrode layer 401, the upper insulating layer 413, the sidewall insulating layer 412a, and the sidewall insulating layer 4 12b, source electrode layer 406a, drain electrode layer 406b, insulating layer 415, insulating layer 417 The method for manufacturing the wiring layer 465a and the wiring layer 465b is the same as that for the transistor described in Embodiment 1. The same manufacturing method is used for manufacturing the semiconductor device, and the description of Embodiment 1 can be referred to for details. The explanation will be omitted.

[0170] In the manufacturing process of the transistor described in this embodiment, a gate electrode layer 401 and an upper insulating layer A conductive film 406 provided on the edge layer 413, the sidewall insulating layer 412a, and the sidewall insulating layer 412b. The conductive film 406 is cut by chemical mechanical polishing to remove the conductive film 406. An electrode layer 406a and a drain electrode layer 406b are formed.

[0171] The source electrode layer 406a and the drain electrode layer 406b are formed on the oxide semiconductor layer 409. The insulating layer 412 is provided in contact with the surface of the insulating layer 412 and the sidewall insulating layer 412a or the sidewall insulating layer 412b. In the region where the source electrode layer 406a and the drain electrode layer 406b are in contact with the oxide semiconductor layer 409, The distance (shortest distance) between the contact region and the gate electrode layer 401 is determined by the sidewall insulating layer 41. 2a and the sidewall insulating layer 412b in the channel length direction, which allows further miniaturization to be achieved. The variation in the shortest distance can be controlled in the manufacturing process.

[0172] In this manner, the source electrode layer 406a or the drain electrode layer 406b and the oxide semiconductor layer 40 9 and the gate electrode layer 401. A region in which the electrode layer 406a or the drain electrode layer 406b is in contact with the oxide semiconductor layer 409 and The resistance between the channel formation regions 403 is reduced, improving the on-characteristics of the transistor 520. It is possible.

[0173] In addition, the gate electrode in the step of forming the source electrode layer 406a and the drain electrode layer 406b In the step of removing the conductive film 406 over the layer 401, etching is performed using a resist mask. Since no process is used, precise processing can be performed accurately. In the process, the yield of transistors with fine structures with small variations in shape and characteristics is It can be produced more easily.

[0174] In addition, in the semiconductor device described in this embodiment, the source and drain regions of the oxide semiconductor layer By providing the electrode layer 405a and the electrode layer 405b under the region, the source region and the drain region are This allows the thickness of the source and drain regions to be increased, reducing the resistance of the source and drain regions. The on-characteristics of the starter can be improved.

[0175] This embodiment mode can be combined with other embodiment modes as appropriate.

[0176] (Embodiment 3) In this embodiment, the transistors described in Embodiments 1 and 2 are used, and A semiconductor that can retain memory contents even when power is not supplied and has no limit on the number of times it can be written to. An example of a semiconductor device according to the present embodiment will be described with reference to the drawings. The transistors described in the first and second embodiments are used as the transistors 162. The transistor 162 can be any of the transistors described in Embodiments 1 and 2. Any of the above structures can be applied.

[0177] FIG. 8 shows an example of the configuration of a semiconductor device. FIG. 8(A) shows a cross-sectional view of the semiconductor device, and FIG. 8(C) shows a circuit diagram of the semiconductor device. Fig. 8(A) corresponds to the cross sections taken along lines C1-C2 and D1-D2 in Fig. 8(B). In FIG. 8B, for the sake of clarity, a part of the configuration of the semiconductor device shown in FIG. The element is omitted.

[0178] The semiconductor device shown in FIG. 8(A) and FIG. 8(B) has a transistor using a first semiconductor material in the lower part. 160 and a transistor 162 made of a second semiconductor material on top. The transistor 162 has the same structure as that described in Embodiments 1 and 2. It can be said that it is completed.

[0179] Here, the first semiconductor material and the second semiconductor material may be materials having different forbidden band widths. For example, the first semiconductor material may be a semiconductor material other than an oxide semiconductor (such as silicon). The second semiconductor material can be an oxide semiconductor. The transistors used in this study can easily operate at high speed. The characteristics of the charge storage capacitor enable it to retain electric charge for a long period of time.

[0180] It should be noted that the above transistors are all n-channel transistors. However, a p-channel transistor can also be used. The essence is that an oxide semiconductor is used for the transistor 162 to store data. The specific configuration of the semiconductor device, such as the materials used in the semiconductor device and the structure of the semiconductor device, is described below. There is no need to be limited to what is shown here.

[0181] The transistor 160 in FIG. 8A includes a semiconductor material (e.g., silicon). A channel forming region 116 is provided on a substrate 185, and a pair of electrodes are provided so as to sandwich the channel forming region 116. and an intermetallic compound region in contact with the impurity element region. 124, a gate insulating layer 108 provided on the channel forming region 116, and a gate insulating layer 108 and a gate electrode layer 110 provided on the gate electrode layer 108. Although there are cases where the source electrode layer and the drain electrode layer are not provided, for convenience, such a state is also included. In this case, the connection relationship of the transistor is explained. Therefore, the source region and the drain region are collectively referred to as the source electrode layer and the drain electrode layer. That is, in this specification, the term "source electrode layer" includes the source region. Ugh.

[0182] An element isolation insulating layer 106 is provided on the substrate 185 so as to surround the transistor 160. An insulating layer 130 is provided to cover the transistor 160. To achieve this, the transistor 160 is provided with a sidewall insulating layer as shown in FIG. On the other hand, when the characteristics of the transistor 160 are important, In this case, a sidewall insulating layer is provided on the side surface of the gate electrode layer 110, and the impurity element concentration is different. The impurity element region 120 may include a region such as the above.

[0183] A transistor 162 illustrated in FIG. 8A is a transistor in which an oxide semiconductor is used for a channel formation region. Here, the oxide semiconductor layer 144 included in the transistor 162 is a high-purity By using a highly purified oxide semiconductor, In this way, the transistor 162 having excellent off-state characteristics can be obtained. The transistors described in Embodiments 1 and 2 can be used.

[0184] Since the off-state current of the transistor 162 is small, the use of the transistor 162 enables long-term recording. The contents of the memory can be retained, i.e., no refresh operation is required, or Therefore, it is possible to realize a semiconductor memory device in which the frequency of refresh operations is extremely low. Power consumption can be reduced sufficiently.

[0185] The transistor 162 is disposed on the insulating layer 130 and has an electrode layer 1 43a, an electrode layer 143b, and an insulating layer in which the electrode layers 143a and 143b are embedded. and layer 145.

[0186] CMP processing for exposing the upper surfaces of the electrode layer 143a and the electrode layer 143b from the insulating layer 145 In this manner, a surface on which the oxide semiconductor layer 144 is to be formed can be planarized. The surface on which the dielectric layer 144 is to be formed is sufficiently planarized (preferably the electrode layer and the base insulating layer). The average surface roughness of the upper surface of the insulating layer is 0.15 nm or less, and an oxide semiconductor layer 144 with excellent crystallinity is formed. This can improve the characteristics of the transistor 162.

[0187] The transistor 162 is formed by forming a gate insulating layer 146, a gate electrode layer 148, A conductive film provided on the upper insulating layer 137, the sidewall insulating layer 136a, and the sidewall insulating layer 136b. is removed by chemical mechanical polishing to form electrode layer 142a and electrode layer 142b. .

[0188] Therefore, the transistor 162 has a transistor functioning as a source electrode layer or a drain electrode layer. The pole layer 142a and the electrode layer 142b are in contact with the oxide semiconductor layer 144 (contact region). Since the distance between the electrode layer 142a and the gate electrode layer 148 can be shortened, A region (contact region) where the pole layer 142b and the oxide semiconductor layer 144 are in contact with each other, and a channel The resistance between the formation regions 144c is reduced, and the on-characteristics of the transistor 162 are improved. It becomes possible.

[0189] The conductive layer overlapping the gate electrode layer 148 in the process of forming the electrode layer 142a and the electrode layer 142b In the process of removing the conductive film, an etching process using a resist mask is not used. Therefore, in the manufacturing process of a semiconductor device, the shape and It is now possible to manufacture transistors with fine structures that have small variations in characteristics with high yields. can.

[0190] An insulating layer 135 and an insulating layer 140 are provided on the electrode layer 142a and the electrode layer 142b. In addition, the source electrode layer is provided through an opening provided in the insulating layer 135 and the insulating layer 140. The electrode layers 142a and 142b functioning as drain and / or gate electrode layers are in contact with each other. The wiring layer 157a and the wiring layer 157b are provided. The electrode layer 157b is provided to overlap with the electrode layer 143a and the electrode layer 143b.

[0191] The oxide semiconductor layer 144 and the source electrode layer overlap with the electrode layer 143a and the electrode layer 143b. Since the electrode layer 142a and the electrode layer 142b functioning as a drain electrode layer are in contact with each other, Therefore, the source and drain regions of the transistor can be made thicker, and the oxide semiconductor The contact resistance between the layer 144 and the source and drain electrode layers can be reduced. Therefore, the on-characteristics of the transistor 162 can be improved.

[0192] In addition, a process for introducing an impurity element is performed on the oxide semiconductor layer 144. A process for introducing an impurity element into the oxide semiconductor layer 144 is performed by using the electrode layer 148 as a mask. As a result, the low resistance region 144a and the low resistance region 144b are formed in a self-aligned manner in the oxide semiconductor layer 144. And a channel forming region 144c is formed.

[0193] The low resistance region 144a and the low resistance region 144b have a higher impurity concentration than the channel formation region 144c. By increasing the concentration of the impurity element, the oxide semiconductor layer 144 The carrier density of the electrode layer 142a and the electrode layer 142b and the oxide semiconductor layer 144 is increased. Since the contact resistance between the gates is low, the on-current and mobility are improved, enabling high-speed response. .

[0194] An insulating layer 150 is provided on the transistor 162. An electrode layer 156 is provided in the area overlapping the line layer 157a. The capacitor element 164 is formed by the transistor 150 and the wiring layer 157a. The wiring layer 157a of the resistor 162 functions as one electrode of the capacitance element 164, and the electrode layer 1 56 functions as the other electrode of the capacitor element 164. Alternatively, the capacitance element 164 may be omitted. It may be provided above the transistor 162.

[0195] In FIG. 8A and FIG. 8B, the transistor 160 and the transistor 162 are The source region of the transistor 160 is provided so as to overlap at least a portion of the It is preferable that the drain region is provided so as to partially overlap the oxide semiconductor layer 144. In addition, the transistor 162 and the capacitor 164 are at least By adopting such a planar layout, This allows the area occupied by the semiconductor device to be reduced, thereby enabling high integration. .

[0196] Next, an example of a circuit configuration corresponding to FIG. 8(A) and FIG. 8(B) is shown in FIG. 8(C).

[0197] In FIG. 8C, the first wiring (1st Line) and the source voltage of the transistor 160 The electrode layer is electrically connected to the second wiring (2nd Line) and the transistor 160. The drain electrode layer is electrically connected to the third wiring (3rd Line). and one of the source electrode layer and the drain electrode layer of the transistor 162 are electrically connected to each other. The fourth wiring (4th Line) and the gate electrode layer of the transistor 162 are electrically connected to each other. The gate electrode layer of the transistor 160 and the gate electrode layer of the transistor 16 The other of the source electrode layer or the drain electrode layer of the second capacitor is electrically connected to one of the electrodes of the capacitor 164. , and the fifth wiring (5th Line) and the other electrode of the capacitor element 164 are electrically is connected to

[0198] In the semiconductor device shown in FIG. 8C, the potential of the gate electrode layer of the transistor 160 can be held. By taking advantage of this feature, it is possible to write, retain, and read information as follows: .

[0199] The writing and holding of data will be described. First, the potential of the fourth wiring is set to the potential of the transistor 1. The transistor 162 is turned on by applying a potential to the transistor 162. The potential of the third wiring is applied to the gate electrode layer of the transistor 160 and the capacitor 164. That is, a predetermined charge is applied to the gate electrode layer of the transistor 160 (write Here, the charges that give two different potential levels (hereafter, low-level charges, H Then, the voltage of the fourth wire is The transistor 162 is turned off by setting the potential at which the transistor 162 is turned off. By this, the charge applied to the gate electrode layer of the transistor 160 is held ( retention).

[0200] Since the off-state current of the transistor 162 is extremely small, the gate electrode layer of the transistor 160 The charge is retained for a long time.

[0201] Next, the reading of information will be explained. A state in which a predetermined potential (constant potential) is applied to the first wiring When an appropriate potential (read potential) is applied to the fifth wiring, the gate of the transistor 160 Depending on the amount of charge held in the electrode layer, the second wiring has a different potential. If the transistor 160 is an n-channel type, a high level is applied to the gate electrode layer of the transistor 160. The apparent threshold voltage V for a given charge th_H The gate of transistor 160 The apparent threshold voltage V when a low-level charge is applied to the gate electrode layer th_L twist Here, the apparent threshold voltage is the voltage at which the transistor 160 is turned on. The term "potential of the fifth wiring" refers to the potential of the fifth wiring required to achieve the "state". The potential of V th_H and V th_L By setting the potential V0 between the For example, in writing, the charge applied to the gate electrode layer of the If a Bell charge is applied, the potential of the fifth wire is V0 (>V th_H ) Then When a low level charge is applied, the transistor 160 is in the "on state." The potential of the fifth wire is V0( <V th_L ), transistor 160 is "off" Therefore, by observing the potential of the second wiring, the stored information It can be read out.

[0202] When memory cells are arranged in an array, only the information in a desired memory cell can be read. In the case of memory cells that do not read information, the state of the gate electrode layer The potential at which transistor 160 is in the “off state” regardless of the state of the th_ H Alternatively, a smaller potential may be applied to the fifth wiring. First, the potential at which transistor 160 is in the "on" state, i.e., V th_L Greater than A potential can be applied to the fifth wiring.

[0203] In the semiconductor device described in this embodiment, an off-state current is low when an oxide semiconductor is used for a channel formation region. By using extremely small transistors, memory contents can be retained for an extremely long period of time. In other words, the refresh operation is unnecessary or the refresh operation is possible. This allows the frequency of operation to be reduced significantly, resulting in a significant reduction in power consumption. In addition, when there is no power supply (however, it is preferable that the potential is fixed), However, it is possible to retain the stored contents for a long period of time.

[0204] In addition, the semiconductor device described in this embodiment does not require a high voltage for writing data. There is no problem with degradation of the capacitance. For example, unlike conventional non-volatile memory, the floating gate Since there is no need to inject electrons into the floating gate or extract electrons from the floating gate, The problem of deterioration of the gate insulating layer does not occur at all. The device does not have the limit on the number of times it can be rewritten, which is a problem with conventional non-volatile memory, and is reliable. Furthermore, the on and off states of transistors allow the Since writing is performed, high speed operation can be easily achieved.

[0205] 9A and 9B show another example of the structure of a semiconductor device. 9B is a cross-sectional view of the semiconductor device. Here, FIG. 9B is a cross-sectional view of the E1- It should be noted that in FIG. 9(A), for the sake of clarity, the cross section of FIG. Some components of the semiconductor device shown in FIG.

[0206] The semiconductor device illustrated in FIG. 9 includes a transistor 162 in which a channel is formed in an oxide semiconductor layer. A channel is formed in a layer of a semiconductor material other than an oxide semiconductor (e.g., silicon, etc.). The transistor 162 and the capacitor 164 are included. The configuration of the transistor 160 is the same as that of the semiconductor device shown in FIG. 8, so a detailed description thereof will be omitted. Omitted.

[0207] In FIG. 9, the capacitor 164 includes an electrode layer 143b, an oxide semiconductor layer 144, and an insulating layer 173. The conductive layer 174 is formed in the same process as the gate electrode layer 148. The upper surface is covered with an insulating film 176, and the side surfaces are covered with sidewall insulating layers 175a and 175b.

[0208] The oxide semiconductor layer 144 is etched with an impurity source using the gate electrode layer 148 and the conductive layer 174 as masks. By introducing the element, in a region that does not overlap with the gate electrode layer 148 and the conductive layer 174, A low resistance region is formed in a self-aligned manner. The electrode layer 142a and the electrode layer 142b are in contact with the low resistance region of the oxide semiconductor layer 144 and form a transistor. The oxide semiconductor layer 144 and the The contact resistance with the source electrode layer and the drain electrode layer is reduced.

[0209] In addition, an electrode layer 14 is formed in contact with the lower portion of the low resistance region that functions as a source region and a drain region. 3a and electrode layer 143b are provided. Therefore, the source region and the drain region The oxide semiconductor layer 144 is thickened, and the resistance between the oxide semiconductor layer 144 and the source electrode layer and the drain electrode layer is reduced. can be.

[0210] The electrode layer 142b of the transistor 162 is an electrode layer formed on the insulating layer 135 and the insulating layer 150. In the opening that reaches 142b, the electrode layer 156 is electrically connected. A conductive layer 172 is provided under and in contact with a, and the conductive layer 172 is connected to the source electrode layer of the transistor 160. The source or drain electrode layer of the transistor 162 is electrically connected to the source or drain electrode layer of the transistor 163. are electrically connected.

[0211] As shown in FIG. 9, a transistor 160, a transistor 162, and a capacitor 164 are stacked. By densely stacking the layers in this way, the area occupied by the semiconductor device can be further reduced. This allows for high integration.

[0212] In the transistor 162 described in this embodiment, an electrode layer is formed in contact with a lower part of an oxide semiconductor layer. Then, an impurity element is introduced into the oxide semiconductor layer by using the gate electrode layer as a mask. Such a transistor exhibits good electrical characteristics and can sufficiently reduce the off-current. A semiconductor device that can retain memory contents for an extremely long period of time by using a resistor. is obtained.

[0213] The above-mentioned transistors have high on-state characteristics (for example, on-state current), high-speed operation, and high-speed response. In addition, miniaturization can be achieved. It is possible to provide a semiconductor device with high performance and high reliability.

[0214] As described above, the configurations, methods, etc. described in this embodiment may be used in conjunction with the configurations, methods, etc. described in other embodiments. They can be used in any suitable combination.

[0215] (Embodiment 4) In this embodiment, the transistors described in Embodiments 1 and 2 are used. It is possible to retain memory contents even when power is not supplied, and there is no limit to the number of times it can be written. Regarding a semiconductor device having a structure different from that shown in Embodiment 3, FIGS. Note that the semiconductor device of this embodiment uses a transistor 162. In this case, the structure of any of the transistors described in Embodiment 1 and Embodiment 2 can be applied. can.

[0216] FIG. 10A shows an example of a circuit configuration of a semiconductor device, and FIG. 10B shows an example of a semiconductor device. First, the semiconductor device shown in FIG. The semiconductor device shown in FIG. 10B will be described below.

[0217] In the semiconductor device shown in FIG. 10A, the bit line BL and the source voltage of the transistor 162 are The electrode layer or drain electrode layer of the transistor 162 is electrically connected to the word line WL. The gate electrode layer is electrically connected to the source electrode layer or the drain electrode layer of the transistor 162. The electrode layer and a first terminal of the capacitor 254 are electrically connected to each other.

[0218] The transistor 162 including an oxide semiconductor has an extremely low off-state current. For this reason, when the transistor 162 is turned off, the first The potential of the terminal (or the charge stored in the capacitance element 254) is kept constant for an extremely long period of time. It is possible to retain it.

[0219] Next, data is written and stored in the semiconductor device (memory cell 250) shown in FIG. The case where the above is performed will be explained.

[0220] First, the potential of the word line WL is set to a potential at which the transistor 162 is turned on. This causes the potential of the bit line BL to change to the potential of the capacitor 254. The potential of the word line WL is then applied to the first terminal of the transistor 1 By setting the potential at which the transistor 62 is turned off, the transistor 162 is turned off. The potential of the first terminal of the quantum element 254 is held (held).

[0221] Since the off-state current of the transistor 162 is extremely small, the potential of the first terminal of the capacitor 254 (or the charge stored in the capacitive element) can be held for a long period of time.

[0222] Next, the reading of information will be described. When the transistor 162 is turned on, The bit line BL and the capacitance element 254 are electrically connected to each other. As a result, the potential of the bit line BL changes. The amount of change in the potential is determined by the potential of the first terminal of the capacitance element 254 (or the potential stored in the capacitance element 254). It takes on different values ​​depending on the charge.

[0223] For example, the potential of the first terminal of the capacitance element 254 is V, the capacitance of the capacitance element 254 is C, and the bit line The capacitance component of BL (hereinafter also referred to as bit line capacitance) is CB, If the potential of the bit line BL is VB0, the potential of the bit line BL after the charge is redistributed is (CB×VB0+C×V) / (CB+C). Therefore, the state of memory cell 250 is In this case, the potential of the first terminal of the capacitance element 254 is assumed to be in two states, V1 and V0 (V1>V0). Then, the potential of the bit line BL when the potential V1 is held is (=CB×VB0+C×V1) / (CB+C) is the potential of the bit line BL when the potential V0 is held (=CB×VB0 +C×V0) / (CB+C)).

[0224] Then, by comparing the potential of the bit line BL with a predetermined potential, information can be read out. do.

[0225] As described above, in the semiconductor device illustrated in FIG. 10A, the off-state current of the transistor 162 is extremely low. Due to its small size, the charge stored in the capacitance element 254 can be held for a long time. In other words, refresh operations are not required or the frequency of refresh operations can be reduced. Since it is possible to reduce the power consumption to an extremely low level, the power consumption can be reduced sufficiently. In addition, even if there is no power supply, the memory contents can be retained for a long period of time. be.

[0226] Next, the semiconductor device shown in FIG.

[0227] The semiconductor device shown in FIG. 10B has a memory cell shown in FIG. 10A as a memory circuit in the upper portion. The memory cell array 251a and the memory cell array 251b each having a plurality of memory cells 250 are provided. At the bottom, the memory cell array 251 (memory cell array 251a and memory cell array 25 1b) has a peripheral circuit 253 required for operating the memory device. The memory cell array 251 is electrically connected to the memory cell array 251 .

[0228] By using the configuration shown in FIG. 10B, the peripheral circuit 253 is connected to the memory cell array 251. (Memory cell array 251a and memory cell array 251b) Therefore, the semiconductor device can be made smaller.

[0229] The transistors provided in the peripheral circuit 253 are made of a different semiconductor material from the transistor 162. It is more preferable to use silicon, germanium, silicon germanium, etc. Silicon carbide, gallium arsenide, or the like can be used, and a single crystal semiconductor can be used. In addition, organic semiconductor materials may be used. The transistor can operate at a sufficiently high speed. It is possible to realize various circuits (logic circuits, driver circuits, etc.) that require high speed operation. be.

[0230] In the semiconductor device shown in FIG. 10B, two memory cell arrays 251 (memory cell In the illustrated embodiment, a stacked memory cell array 251a and a stacked memory cell array 251b are used. The number of memory cells to be stacked is not limited to this. is also good.

[0231] Next, a specific configuration of the semiconductor device shown in FIG. 10 will be described with reference to FIG.

[0232] FIG. 11 is a cross-sectional view of a semiconductor device. The semiconductor device shown in FIG. The memory cell array 251 includes a plurality of memory cell arrays 251 and a peripheral circuit 253 below the memory cell array. The memory cell 251 and the peripheral circuit 253 are electrically connected to each other. Among the arrays, the memory cell array 251a, the memory cell array 251b, and the peripheral circuit 253 are shown as representative examples.

[0233] The transistor 162a and the capacitor 254a included in the memory cell array 251a The electrode layer 343c of the memory cell array 251a is connected to other memory cells. The transistor 162a is a transistor in which a channel is formed in an oxide semiconductor layer. The transistor 162a may be any of the transistors described in the first and second embodiments. The capacitor 254a can be implemented by using the transistor 162a. The electrode layer 3 is formed using the source electrode layer and an electrode formed in the same layer as the wiring layer. The electrode layer 43c is formed in the same layer as the electrode layer 143a and the electrode layer 143b of the transistor 162a. It is done.

[0234] The transistor 162b and the capacitor 254b included in the memory cell array 251b, The memory cell array 251b is connected to another memory cell through an electrode layer 343b. The electrode layer 343a connecting the transistor 251b and the peripheral circuit 253 is representatively shown. Transistor 162b has a channel formed in an oxide semiconductor layer. 62b is applied with the transistors described in the first and second embodiments. The capacitance element 254b is connected to the source voltage of the transistor 162b. The electrode layer 343b is formed using an electrode layer and an electrode formed in the same layer as the wiring layer. The transistor 162b is formed in the same layer as the wiring layers 157a and 157b. The electrode layer 343a is the same as the electrode layer 143a and the electrode layer 143b included in the transistor 162b. formed in the same layer.

[0235] The peripheral circuit 253 is a transistor using a semiconductor material other than an oxide semiconductor layer as a channel formation region. The transistor 301 is made of a semiconductor material (e.g., silicon, etc.). An element isolation insulating layer is provided on a substrate 300 including the element isolation insulating layer 306, and a transistor is formed in an area surrounded by the element isolation insulating layer 306. A transistor can be obtained by forming a region that becomes a channel.

[0236] The transistor 301 is a semiconductor layer such as a silicon layer formed on an insulating surface, or a SO The transistor may have a channel formed in the silicon layer of the substrate. The configuration of 301 can be a known configuration.

[0237] A wiring layer 310a is formed between the peripheral circuit 253 and the memory cell array 251b. An insulating layer 341a is provided between the peripheral circuit 253 and the wiring layer 310a. An insulating layer 341b is provided between the gate insulating film 10a and the memory cell array 251b. The layer 341a includes a wiring layer 355a that electrically connects the peripheral circuit 253 and the wiring layer 310a. The insulating layer 341b is provided with a wiring layer 310a and a memory cell array 25 1b, and a wiring layer 355b is provided for electrically connecting the wiring layer 355b to the first and second electrodes 355a and 355b.

[0238] The peripheral circuit 253 and the memory cell array 251b are electrically connected via a wiring layer 310a. The peripheral circuit 253 and the memory cell array 251b are connected in this manner. The peripheral circuit 253 and the memory cell array 251b include a transistor 301 and Although the transistor 162b is electrically connected in a region where the transistor 162b does not overlap with the transistor 162b, this is not limited to this. For example, the electrode layers 143a and 143b of the transistor 162b and the surrounding A configuration in which the circuit 253 is in direct contact with the semiconductor device 252 may also be used.

[0239] A wiring layer 310b is provided between the memory cell array 251a and the memory cell array 251b. The wiring layer 310b is formed in the memory cell array 251b. The wiring layer 310b is provided on the layer 341c. An insulating layer 341d is provided. The insulating layer 341c is provided with a wiring layer 310b and a memory cell array. A wiring layer 355c is provided to electrically connect the wiring layer 251b to the insulating layer 341d. The wiring layer 355d electrically connects the wiring layer 310b and the memory cell array 251a. It is provided.

[0240] By adopting the layout shown in FIG. 11, the area occupied by the semiconductor device can be reduced. This allows for high integration.

[0241] 12 and 13 show the structure of a semiconductor device that can be applied to the memory cell 250 shown in FIG. FIG. 12A is a top view of the semiconductor device, and FIG. 12B is a schematic diagram of the semiconductor device. Here, FIG. 12(B) is a cross-sectional view taken along the line F1-F2 in FIG. 12(A). In FIG. 12(A), for the sake of clarity, the semiconductor shown in FIG. Some components of the device are omitted.

[0242] The memory cell illustrated in FIG. 12 includes a transistor 162 having a channel formed in an oxide semiconductor layer. and a capacitor 254. Note that the structure of the transistor 162 is the same as that of the semiconductor device shown in FIG. Since it is similar to the transistor 162 included in the device, detailed description thereof will be omitted.

[0243] In FIG. 12, the capacitor 254 includes an electrode layer 143b, an oxide semiconductor layer 144, and an insulating layer 17. 3, and a conductive layer 174. The conductive layer 174 is formed in the same process as the gate electrode layer 148. The upper surface is made of an insulating film 176, and the side surfaces are made of a sidewall insulating layer 175a and a sidewall insulating layer 175b. It's covered.

[0244] The oxide semiconductor layer 144 is etched with an impurity source using the gate electrode layer 148 and the conductive layer 174 as masks. By introducing the element, in a region that does not overlap with the gate electrode layer 148 and the conductive layer 174, A low resistance region is formed in a self-aligned manner. The electrode layer 142a and the electrode layer 142b are in contact with the low resistance region of the oxide semiconductor layer 144 and form a transistor. The oxide semiconductor layer 144 and the The contact resistance with the source electrode layer and the drain electrode layer is reduced.

[0245] The electrode layer 142b of the transistor 162 is an electrode layer formed on the insulating layer 135 and the insulating layer 150. In the opening that reaches 142b, electrical connection is made to wiring 260.

[0246] FIG. 13A is a top view of the semiconductor device, and FIG. 13B is a cross-sectional view of the semiconductor device. FIG. 13B corresponds to a cross section taken along line G1-G2 in FIG. 13A. In (A), for clarity of the drawing, some components of the semiconductor device shown in FIG. has been omitted.

[0247] The memory cell illustrated in FIG. 13 includes a transistor 162 having a channel formed in an oxide semiconductor layer. and a capacitor 254. Note that the structure of the transistor 162 is the same as that of the transistor shown in FIG. Since it is similar to the starter 162, a detailed description will be omitted.

[0248] 13A and 13B, the capacitance element 254 includes a conductive layer 192, an insulating layer 193, a conductive The insulating layer 193 is made of a layer 194 and is formed in an insulating film 196. It is preferable to use a highly insulating material. Electrode layer 1 of transistor 162 formed on layer 135, insulating layer 150, and insulating layer 195. They are electrically connected via a conductive layer 191 provided in an opening that reaches 42b.

[0249] The oxide semiconductor layer 144 is doped with an impurity element by using the gate electrode layer 148 as a mask. Then, in the region not overlapping with the gate electrode layer 148, a low resistance region is formed in a self-aligned manner. The electrode layer 142a and the electrode layer 142b functioning as a source electrode layer and a drain electrode layer are The source and drain regions of the transistor 162 are in contact with the low-resistance region of the oxide semiconductor layer 144. The oxide semiconductor layer 144 and the source and drain electrode layers function as a gate region. The contact resistance is reduced.

[0250] As shown in FIG. 12 and FIG. 13, the transistor 162 and the capacitor 254 are densely arranged so as to overlap each other. By stacking the layers, the area occupied by the semiconductor device can be further reduced. Integration can be achieved.

[0251] As described above, the memory cells formed in multiple layers on the upper portion are transistors using oxide semiconductors. The transistor is made of a highly purified and intrinsic oxide semiconductor. Since the off-current of a transistor is small, the memory contents can be maintained for a long period of time by using the transistor. In other words, the frequency of refresh operations can be reduced significantly. Therefore, the power consumption can be sufficiently reduced.

[0252] In this way, transistors using materials other than oxide semiconductors (in other words, transistors that operate at sufficiently high speed) The peripheral circuits are made of transistors that can be operated with a semiconductor oxide. In a broader sense, the off-state current of the transistor is sufficiently small. This makes it possible to realize a semiconductor device having unprecedented features. By forming the gate and the memory circuit in a stacked structure, the integration of the semiconductor device can be promoted.

[0253] In the transistor 162 described in this embodiment, an electrode layer is formed in contact with a lower part of an oxide semiconductor layer. Then, an impurity element is introduced into the oxide semiconductor layer by using the gate electrode layer as a mask. Such a transistor exhibits good electrical characteristics and can sufficiently reduce the off-current. A semiconductor device that can retain memory contents for an extremely long period of time by using a resistor. is obtained.

[0254] The above-mentioned transistors have high on-state characteristics (for example, on-state current), high-speed operation, and high-speed response. In addition, miniaturization can be achieved. It is possible to provide a semiconductor device with high performance and high reliability.

[0255] This embodiment mode can be implemented in appropriate combination with the configurations described in other embodiments. It is.

[0256] (Embodiment 5) In this embodiment mode, the semiconductor device described in the above embodiment mode is applied to a mobile phone, a smartphone, An example of application to a portable device such as a child book will be described with reference to FIGS.

[0257] In mobile devices such as mobile phones, smartphones, and e-books, image data is temporarily stored. SRAM or DRAM is used in the following. SRAM or DRAM is used The reason is that flash memory has a slow response time and is not suitable for image processing. On the other hand, when SRAM or DRAM is used for temporary storage of image data, the following characteristics are observed: do.

[0258] In a normal SRAM, as shown in FIG. 14(A), one memory cell is made up of transistors 801 to It is composed of six transistors, 806, which are connected to the X decoder 807 and the Y decoder 808. The transistor 803 and the transistor 805 are driven by the transistor 808. 04 and transistor 806 form an inverter, enabling high-speed operation. Since each memory cell is composed of six transistors, the cell area is large. When the minimum dimension of the design rule is F, the area of ​​the SRAM memory cell is usually 10 0~150F 2 For this reason, SRAM has a high cost per bit.

[0259] On the other hand, in a DRAM, the memory cell is made up of a transistor 811, as shown in FIG. The storage capacitor 812 is connected to the X decoder 813 and the Y decoder 814. Each cell is composed of one transistor and one capacitance, and has a small area. The memory cell area of ​​a DRAM is usually 10F 2 However, DRAM is always refreshed. It requires flash memory and consumes power even if it is not being rewritten.

[0260] However, the memory cell area of ​​the semiconductor device described in the above embodiment is 10F 2 Before and after and frequent refresh is not required. Therefore, the memory cell area is reduced, and Power consumption can be reduced.

[0261] A block diagram of the portable device is shown in FIG. 15. The portable device shown in FIG. 15 includes an RF circuit 901, an analog A digital baseband circuit 902, a digital baseband circuit 903, a battery 904, and a power supply Circuit 905, application processor 906, flash memory 910, display A controller 911, a memory circuit 912, a display 913, a touch sensor 919, The display 913 is a display. The image display device is configured with an application section 914, a source driver 915, and a gate driver 916. The application processor 906 is a CPU 907, a DSP 908, and an interface (IF Generally, the memory circuit 912 is composed of an SRAM or a DRAM. By adopting the semiconductor device described in the previous embodiment for this portion, High speed writing and reading, long-term memory retention, and low power consumption It is possible to provide a portable device having such a configuration.

[0262] FIG. 16 shows a display memory circuit 950 using the semiconductor device described in the previous embodiment. The memory circuit 950 shown in FIG. The memory controller 951 is also configured with a switch 954, a switch 955, and a memory controller 951. The memory circuit 950 receives image data (input image data) input from a signal line, and stores the image data in the memory 9 52 and the data (stored image data) stored in the memory 953 are read out and controlled. A display controller 956 that controls the display A display 957 for displaying the image is connected.

[0263] First, certain image data is generated by an application processor (not shown). The input image data A is input to the memory 952 via the switch 954. The image data stored in the memory 952 (stored image data A) is then The image is sent to a display 957 via a switch 955 and a display controller 956. , will be displayed.

[0264] When there is no change in the input image data A, the stored image data A usually has a frequency of about 30 to 60 Hz. The display controller 956 reads the data from the memory 952 via the switch 955. It is revealed.

[0265] Next, for example, when the user rewrites the screen (i.e., input image data A If there is a change in the input image data, the application processor The input image data B is stored in the memory 953 via the switch 954. During this time, the stored image data A is periodically read out from the memory 952 via the switch 955. When the new image data (stored image data B) has been stored in the memory 953, From the next frame of the display 957, the stored image data B is read out, and the switch 95 5, and the stored image data is displayed on the display 957 via the display controller 956. Data B is sent and displayed. This readout is followed by the next new image data being stored in the memory. This continues until the data is stored in the memory 952.

[0266] In this way, the memory 952 and the memory 953 alternately write image data and receive image data. The display 957 is displayed by reading out the data from the memory 9 The memory 52 and the memory 953 are not limited to being separate memories, but may be one memory divided and used. The semiconductor device described in the above embodiment may be used as the memory 952 and the memory 953. By adopting this technology, information can be written and read at high speeds and memory can be retained for long periods of time. Moreover, power consumption can be sufficiently reduced.

[0267] FIG. 17 shows a block diagram of an electronic book. FIG. 17 shows a battery 1001, a power supply circuit 1002, , microprocessor 1003, flash memory 1004, audio circuit 1005, keyboard A code 1006, a memory circuit 1007, a touch panel 1008, a display 1009, The display controller 1010 is configured as a display controller.

[0268] Here, the semiconductor device described in the previous embodiment is used for the memory circuit 1007 in FIG. The memory circuit 1007 has a function of temporarily storing the contents of a book. For example, when the user uses the highlight function, the memory circuit 1007 stores the The highlight function is a function that allows users to highlight the parts of an e-book that they have read. When you are reading, you can mark a specific part by, for example, changing the color of the display or underlining. Marking by drawing lines, making letters thicker, or changing the font of letters to differentiate them from the surroundings The memory circuit 1007 is used for short-term information storage and long-term information storage. The data held in the memory circuit 1007 is copied to the flash memory 1004. Even in such a case, the semiconductor device described in the above embodiment may be adopted. This allows information to be written and read at high speed, and to be stored for a long period of time. Moreover, power consumption can be sufficiently reduced.

[0269] As described above, the portable device shown in this embodiment mode is equipped with the semiconductor device according to the above embodiment. This allows for high-speed readout, long-term memory retention, and low power consumption. Thus, a portable device with reduced noise is realized.

[0270] The structures, methods, and the like described in this embodiment may be combined as appropriate with the structures, methods, and the like described in other embodiments. They can be used in combination. [Explanation of symbols]

[0271] 106 Element isolation insulating layer 108 Gate Insulation Layer 110 Gate electrode layer 116 Channel formation region 120 Impurity element area 124 Intermetallic compound area 130 Insulating layer 135 Insulating Layer 136a Sidewall insulating layer 136b Sidewall insulating layer 137 Upper insulating layer 140 Insulating layer 142a Electrode layer 142b Electrode layer 143a Electrode layer 143b Electrode layer 144 Oxide semiconductor layer 144a Low resistance area 144b Low resistance region 144c Channel forming region 145 Insulating Layer 146 Gate Insulation Layer 148 Gate electrode layer 150 Insulating layer 156 Electrode layer 157a wiring layer 157b Wiring layer 160 Transistors 162 Transistor 162a Transistor 162b Transistor 164 Capacitive element 172 Conductive Layer 173 Insulating Layer 174 Conductive Layer 175a Sidewall insulating layer 175b Sidewall insulating layer 176 Insulating Film 185 Substrate 191 Conductive Layer 192 Conductive Layer 193 Insulating Layer 194 Conductive Layer 195 Insulating Layer 196 Insulating Film 250 memory cells 251 Memory Cell Array 251a Memory Cell Array 251b Memory Cell Array 253 Peripheral Circuits 254 Capacitive element 254a Capacitive element 254b Capacitive element 260 Wiring 300 Substrates 301 Transistor 306 Element isolation insulating layer 310a wiring layer 310b wiring layer 341a Insulating layer 341b Insulating layer 341c Insulating layer 341d Insulating layer 343a Electrode layer 343b Electrode layer 343c electrode layer 355a wiring layer 355b wiring layer 355c wiring layer 355d wiring layer 400 Substrates 401 Gate electrode layer 402 Gate insulating layer 403 Channel formation region 404a Low resistance area 404b Low resistance region 405a Electrode layer 405b Electrode layer 406 Conductive Film 406a Source electrode layer 406b Drain electrode layer 409 Oxide Semiconductor Layer 412a Sidewall insulating layer 412b Sidewall insulating layer 413 Upper insulation layer 415 Insulating layer 416 Insulating Layer 417 Insulating Layer 420 Transistor 421 Impurity elements 430 Transistor 435 Undercoat insulating film 436 Undercoat insulation layer 440 Transistor 452 Gate insulating film 455a aperture 455b aperture 465a Wiring layer 465b Wiring layer 505a Electrode layer 505b Electrode layer 520 Transistor 530 Transistor 536 Undercoat insulation layer 801 Transistors 803 Transistor 804 Transistor 805 Transistor 806 Transistor 807 X Decoder 808 Y Decoder 811 Transistor 812 holding capacity 813X Decoder 814 Y decoder 901 RF circuit 902 Analog Baseband Circuit 903 Digital Baseband Circuit 904 Battery 905 Power supply circuit 906 Application Processor 907 CPU 908 DSP 910 Flash Memory 911 Display Controller 912 Memory Circuit 913 Display 914 Display section 915 Source Driver 916 Gate Driver 917 Voice Circuit 918 Keyboard 919 Touch Sensor 950 Memory Circuit 951 Memory Controller 952 Memory 953 Memory 954 Switch 955 Switch 956 Display Controller 957 Display 1001 Battery 1002 Power supply circuit 1003 Microprocessor 1004 Flash Memory 1005 Audio Circuit 1006 Keyboard 1007 Memory Circuit 1008 Touch Panel 1009 Display 1010 Display Controller

Claims

[Claim 1] A pair of electrode layers; an oxide semiconductor layer including a pair of low-resistance regions over the pair of electrode layers and in contact with the pair of electrode layers, and a channel formation region sandwiched between the pair of low-resistance regions; a gate insulating layer on the oxide semiconductor layer; a gate electrode layer on the gate insulating layer and overlapping a channel formation region; an upper insulating layer on the gate electrode layer; a sidewall insulating layer covering a side surface of the gate electrode layer and a side surface of the upper insulating layer; a source electrode layer and a drain electrode layer in contact with the oxide semiconductor layer, a side surface of the gate insulating layer, and a side surface of the sidewall insulating layer; a first insulating layer on the source electrode layer and the drain electrode layer; a second insulating layer on the top insulating layer, the sidewall insulating layer, the source electrode layer, and the drain electrode layer; a pair of wiring layers in contact with the source electrode layer or the drain electrode layer through openings provided in the first insulating layer and the second insulating layer; the height of the upper surfaces of the source electrode layer and the drain electrode layer is lower than the heights of the upper surfaces of the upper insulating layer, the sidewall insulating layer, and the first insulating layer, and is higher than the height of the upper surface of the gate electrode layer; The pair of wiring layers overlap the pair of electrode layers.

Citation Information

Patent Citations

  • Image display

    JP2006165528A