Coating film layer for detecting crack, method for detecting crack in steel structure, and method for repairing crack
The crack detection coating layer with a conductive coating film and insulating layers addresses the challenges of conventional methods by enabling easy detection and repair of cracks in steel structures, enhancing maintainability and accuracy.
Patent Information
- Application Number
- JP2024075290
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2044-05-07
AI Technical Summary
Conventional crack detection methods require numerous gauges for wide or long-distance detection, are difficult to adjust resistance values, involve complex devices with multiple frequencies, and are challenging to maintain when used for wiring.
A crack detection coating layer comprising a first insulating coating, a conductive coating film, and a second insulating coating with repair points, using silver powder and silver-coated copper powder as conductive pigments, and acrylic or epoxy resin, allowing for easy detection and repair of cracks by monitoring disconnections in the wiring circuit.
Enables accurate crack detection and easy maintenance, reducing construction and management time, and facilitating efficient repair of cracks in steel structures.
Smart Images

Figure 2024161908000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating layer for detecting cracks that occur in steel structures, welds, etc., and to a method for detecting cracks in steel structures and a method for repairing cracks using the coating layer. In the following description, the numerical range "x to y" means not less than x and not more than y, and includes the boundary value. [Background technology]
[0002] Conventional crack detection methods involve attaching a crack detection gauge to the area where a crack has occurred, passing a constant current through it, and detecting the break in the wire from the change in voltage.
[0003] For example, Patent Document 1 discloses a conductive paint, a conductive coating film, and a crack detection paint that have an optimal volume resistivity for detecting the occurrence of cracks, are easy to apply on-site, and can accurately detect the occurrence of cracks. The crack detection coating film is formed by applying a conductive paint containing carbon black and epoxy resin, and a pair of electrodes is arranged on the surface, with the resistance between the electrodes being 200 to 10,000 Ω.
[0004] Patent Document 2 discloses a crack monitoring device and a crack monitoring method that can improve the detection accuracy of crack occurrence without being affected by fluctuations in the opening width of a crack that occurs in a monitored object. This method supplies AC power of multiple different frequencies to a conductive coating film and detects the occurrence of a crack from the AC impedance.
[0005] Patent Document 3 discloses a conductive paint, a conductive coating film, a paint for crack detection, and a coating film for crack detection that have an optimal volume resistivity for detecting crack occurrence, are easy to apply on-site, and can accurately detect the occurrence of cracks. The conductive pigment contains silver powder and silver-coated copper powder, and the organic resin contains urethane resin. By adjusting the pigment composition and form, the volume resistivity can be set within a predetermined range, and for example, a coating film for wiring can be formed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-179501 A [Patent Document 2] JP 2011-174823 A [Patent Document 3] JP 2008-81607 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the above-mentioned conventional techniques have the following problems. In order to detect over a wide range or long distance, it was necessary to attach many foil-type crack detection gauges, which resulted in a lot of maintenance work.
[0008] The technology described in Patent Document 1 detects cracks from resistance changes caused by the progression of the cracks. However, this method has a problem in that it is difficult to adjust the resistance value to be detected when the detection range is wide or long distance.
[0009] The technology described in Patent Document 2 had the problem that the device became complicated because it applied and detected a number of different frequencies.
[0010] The technology described in Patent Document 3 has a problem in that when used for wiring, etc., maintenance is difficult when a break occurs.
[0011] The present invention has been made in consideration of the above circumstances, and aims to provide a technology that is easy to install, highly maintainable, and capable of detecting the occurrence of cracks with high accuracy. [Means for solving the problem]
[0012] The crack detection coating layer of the present invention, which advantageously solves the above-mentioned problems, is a crack detection coating layer comprising a first insulating coating formed on the surface of a steel structure, a conductive coating for crack detection applied to the surface of the first insulating coating, and a second insulating coating applied to protect the conductive coating, and is characterized in that a repair point is provided between the conductive coating and the second insulating coating for peeling off the conductive coating so as to expose it.
[0013] The crack detection coating layer according to the present invention is (a) the material of the repair point is at least one selected from paper, nylon, vinyl, and cellophane; (b) the conductive coating film contains silver powder and silver-coated copper powder as a pigment of a conductive paint, and the conductive coating film contains at least one resin selected from an acrylic resin and an epoxy resin as a resin; This may be a more preferable solution.
[0014] The crack detection method for steel structures of the present invention, which advantageously solves the above-mentioned problem, is characterized in that any of the above-mentioned crack detection coating layers is formed on the surface of a steel structure, an electric current is passed through the wiring circuit of the conductive coating, and a break in the wiring circuit due to a crack in the steel structure is detected.
[0015] The method for repairing cracks in a steel structure of the present invention, which advantageously solves the above-mentioned problems, is characterized by forming any of the above-mentioned crack detection coating layers on the surface of a steel structure, passing an electric current through the wiring circuit of the conductive coating, detecting a break in the wiring circuit due to a crack in the steel structure, peeling off the coating around the detected crack, repairing the crack by welding, forming a first insulating coating on the exposed surface of the steel structure after peeling off the coating, peeling off a repair point close to the crack to expose the conductive coating, forming a wiring circuit made of a conductive coating across the repaired crack, between the exposed repair points or between the exposed repair point and the start point of current flow, and applying a second insulating coating to protect the conductive coating. Effect of the Invention
[0016] According to the crack detection coating layer, the method for detecting cracks in a steel structure, and the method for repairing cracks of the present invention, cracks in a steel structure can be detected by disconnection of the wiring in the conductive coating, and after repairing the cracked portion, the healthy portion can be reused for wiring. Therefore, the construction is easy, the maintenance is easy, it is economically advantageous, and the occurrence of cracks can be detected with high accuracy. [Brief description of the drawings]
[0017] [Figure 1] 1A and 1B are schematic diagrams illustrating a coating layer for detecting cracks according to one embodiment of the present invention, where (a) shows an example of detecting cracks along a weld, and (b) shows an example of detecting cracks in a steel plate in a direction perpendicular to the weld. [Diagram 2] These are cross-sectional views of coating layers on steel sheets, where (a) shows an example of forming a conductive coating on an existing topcoat, (b) shows an example of forming a conductive coating between the primer coat and topcoat coat during new installation, and (c) shows conventional coating. [Diagram 3] Cross-sectional views of repair points, where (a) shows an example of a repair point installed on an existing top coat of paint, (b) shows an example of a repair point as newly installed, and (c) shows an example of a repair point with tabs. [Figure 4] (a) is a conceptual diagram showing an example of a coating layer for crack detection formed on a flat plate portion, (b) is a conceptual diagram showing an example of crack occurrence, and (c) is a conceptual diagram showing the repaired state of the crack. [Diagram 5] This is a cross-sectional view of part A in Figure 4(c), where (a) shows the state after the cracked part has been ground away, (b) shows the state after the primer paint has been applied to the part that does not have a repair point, and (c) shows the state after the primer paint has been applied to the part that has a repair point. [Figure 6] These are cross-sectional views showing how the crack detection coating is regenerated at the repair point, where (d) shows how the repair point peels off, (e) shows how the conductive coating for crack detection exposed at the repair point is connected, and (f) shows how the conductive coating is protected with a top coat of paint. [Figure 7]1A and 1B are schematic cross-sectional views of the vicinity of a welded part showing a suitable application range of a crack detection coating layer in the above embodiment, where (a) shows a case where the heat-affected zone of the weld has been confirmed, and (b) shows a case where the heat-affected zone is unknown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The following is a detailed description of the embodiments of the present invention. The following embodiments are merely examples of configurations and methods for embodying the technical idea of the present invention, and are not intended to limit the configuration to those described below. In other words, the technical idea of the present invention can be modified in various ways within the technical scope described in the claims.
[0019] FIG. 1 is a schematic diagram of a coating layer for crack detection according to one embodiment. A coating layer for crack detection is formed in the vicinity of a welded portion 2 of a steel structure 1. If the conductive coating 4C is formed as a wiring circuit so as to straddle the welded portion 2 as shown in FIG. 1(a), cracks along the welded portion 2, i.e., vertical cracks, can be detected. On the other hand, if the conductive coating 4C is formed as a wiring circuit so as to follow the weld bead as shown in FIG. 1(b), cracks in the steel plate 1 in a direction perpendicular to the welded portion 2, i.e., horizontal cracks, can be detected. An insulating top coat 4D is applied to protect the conductive coating 4C. The wiring circuit of the conductive coating 4C is not limited to this, and can be applied in any shape. FIG. 7 shows a schematic enlarged cross-sectional view of the vicinity of the welded portion 2. When the heat-affected portion 2A of the weld is clear as shown in FIG. 7(a), it is preferable to set the application range 4E of the coating layer for crack detection to be applied by folding back across the welded portion 2 so as to extend outside the range of the heat-affected portion 2A. In addition, as shown in Fig. 7(b), if the heat-affected zone 2A of the weld is unclear, it is highly likely that stress will be transmitted within 45 degrees from the end of the weld bead, causing cracks. Therefore, it is preferable to set the coating range 4E of the crack detection coating layer to be applied back and forth across the weld 2 so that it spreads to the outside of the stress load range 2B. By applying a voltage to a current start point (not shown) and monitoring the change in the current flow, it is possible to detect cracks from breaks in the wiring circuit. In this embodiment, a repair point 5, which will be described later, is provided in the middle of the wiring circuit made of the conductive coating 4C.
[0020] FIG. 2(a) is a cross-sectional view showing an example of a coating layer 4 for crack detection according to this embodiment, which is formed on the surface of an existing coating. The existing coating is an undercoat 4A and a topcoat 4B applied on the surface of the steel sheet 1 as shown in FIG. 2(c). In this embodiment, these constitute a first insulating coating. An intermediate coating may be applied between the undercoat 4A and the topcoat 4B. A conductive coating 4C is formed on this existing coating as a wiring circuit for crack detection. A topcoat 4D is applied on top of this as a second insulating coating to protect the conductive coating 4C.
[0021] Fig. 2(b) is a cross-sectional view showing an example of another crack detection coating layer 4 according to this embodiment, which is formed on the surface of a steel sheet 1 as a new coating. An undercoat 4A is formed on the surface of the steel sheet 1 as a first insulating coating. A conductive coating 4C is formed thereon as a wiring circuit for crack detection. A topcoat 4D is then applied thereon as a second insulating coating to protect the conductive coating 4C. This is preferable in the case of new coating, as it reduces the number of times topcoats are applied.
[0022] The undercoat 4A electrically insulates the steel plate 1 from the conductive coating film 4C for crack detection and forms a coating film to prevent corrosion of the steel plate. The undercoat 4A is, for example, an undercoat paint applied to anticorrosive coating systems for steel structures, such as epoxy resin containing anticorrosive pigments or organic zinc-rich paint.
[0023] The topcoats 4B and 4D are applied to protect and insulate the undercoat 4A and the conductive coating film 4C for crack detection from the effects of natural factors. Epoxy resin paints with excellent environmental barrier properties, and polyurethane resins and fluororesins with excellent UV and chemical resistance can be used. A middle coat may be applied before the topcoat 4D.
[0024] The conductive coating film 4C is formed by applying an organic resin containing a conductive pigment by spraying, brushing, roller, etc. The conductive pigment may be carbon black, graphite, nickel, silver powder, silver-coated copper powder, etc. It is preferable to use a mixture of silver powder and silver-coated copper powder from the viewpoints of reducing the volume resistivity and ease of painting.
[0025] The organic resin used in the conductive coating film 4C is preferably an acrylic resin, an epoxy resin, a polyurethane resin, a phenolic resin, an alkyl silicate resin, etc. In consideration of compatibility with the paint applied to the surface of the steel structure and dispersibility of the conductive pigment, it is more preferable to include at least one selected from an acrylic resin and an epoxy resin.
[0026] As shown in FIG. 1, the wiring circuit for crack detection using the conductive coating film 4C has a total length of more than 10 m. The film thickness is preferably 10 μm to 100 μm. Below the lower limit, there is a risk that a continuous coating film cannot be obtained when applied on site. Above the upper limit, many coating defects such as sagging occur when applied, and if the viscosity of the paint is increased as a countermeasure, there is a risk that workability will be sacrificed. More preferably, 30 to 60 μm is preferable. For example, when considering a conductive coating film 4C that has an electrical resistance of about 100 Ω for a wiring with a width of 20 mm and a total length of 10 m, the volume resistivity is 0.5 to 5.0 × 10 -3 It is preferable to adjust the conductive pigment so that the resistivity satisfies the Ω·cm range.
[0027] The repair point 5 used in this embodiment can be configured as shown in Figures 3(a) to (c). Figure 3(a) shows a cross-sectional view of an example of the repair point 5 of the conductive coating film 4C installed on the existing top coat 4B. Figure 3(b) shows a cross-sectional view of an example of the repair point 5 of the conductive coating film 4C in the case of a new installation. The repair point 5 is provided so that when the wiring circuit of the conductive coating film 4C is disconnected due to a crack or the like, the top coat 4D is peeled off to expose the conductive coating film 4C, so that a new wiring circuit can be formed. The repair point 5 is made of at least one material selected from paper, nylon, vinyl, and cellophane, and is disposed between the conductive coating film 4C and the top coat 4D. For example, the material for the repair point 5 can be attached on the conductive coating film 4C as a tape such as an easily peelable adhesive, and the top coat 4D can be applied thereon. If the adhesiveness is too high, the conductive coating film 4C will also peel off at the same time, so it is preferable to have an appropriate adhesiveness. The repair point 5 is provided with a tab 5A as shown in FIG. 3(c) to make the repair point 5 easier to see after the topcoat 4D. In addition, the repair point 5 can be easily peeled off using the tab 5A. The shape of the repair point 5 can also be circular, elliptical or rectangular. It is preferable that the repair point 5 covers a range of the diameter, short diameter and short side that is equal to or longer than the wiring width of the conductive coating film 4C.
[0028] Next, a crack detection method and a crack repair method using the crack detection coating layer according to this embodiment will be described. In the crack detection method according to this embodiment, a wiring circuit is formed using the above-mentioned crack detection coating layer as shown in Fig. 1, and a voltage is applied to a current flow start point (not shown) to monitor the current flowing through the wiring circuit. When the coating is damaged due to a crack in the steel structure or an external impact, causing a break in the wiring circuit, the current value decreases or the current stops flowing. The steel structure at the break point is visually observed to determine whether or not there is a crack.
[0029] FIG. 4(a) is a schematic diagram showing an example of forming a coating layer for crack detection on a flat plate. In this example, a wiring circuit of a conductive coating 4C is formed on an existing top coat 4B. Normally, the top coat 4D contains a pigment, so the presence of the conductive coating 4C for crack detection cannot be observed. By making the top coat 4D a transparent or translucent coating such as a clear coat, the state of the conductive coating 4C for crack detection can be confirmed. Even if the crack cannot be seen from the outside, the crack occurrence position can be identified by peeling off the repair point 5 and checking the conduction between the exposed conductive coating 4C or between the exposed conductive coating 4C and the start point of current flow.
[0030] Fig. 4(b) is a schematic diagram showing a state in which the crack detection coating has been torn by a crack. As shown in Fig. 4(c), the area around the crack is ground and the coating is peeled off to expose the surface of the steel sheet 1. The cracked area of the steel sheet 1 revealed by the surface grinding area 7 is repaired by welding. The crack detection coating layer 4 is also ground down to part A by the above grinding.
[0031] Fig. 5(a) is an enlarged cross-sectional view of part A in Fig. 4(c). The exposed conductive coating film 4C is sandwiched between, for example, a top coat 4B as a first insulating coating film and a top coat 4D as a second insulating coating film. The exposed area of the conductive coating film 4C is the wiring width x coating film thickness, and since the coating film thickness is about 10 to 100 µm, it is difficult to connect this conductive coating film 4D as a new wiring.
[0032] In addition, the ground surface 7 of the steel plate 1 exposed by grinding is coated with a primer 4A for rust protection. This is shown in the cross-sectional view of Figure 5(b). Figure 5(b) shows a cross-section without any repair points. When this happens, the conductive coating 4C is completely hidden, making connection impossible.
[0033] Therefore, as shown in Fig. 5(c), a repair point 5 is placed near the ground surface 7. The procedure requires that the undercoat 4A be completed before peeling off the repair point 5. This is to prevent the conductive coating 4C exposed by peeling off the repair point 5 from being covered. Fig. 6(d) is a cross-sectional view showing the state in which the repair point 5 has been peeled off as a peeled piece 5B after the undercoat has been applied. This exposes the conductive coating 4C, allowing wiring connection.
[0034] 6(e) is a cross-sectional view showing a state where a wiring circuit is regenerated from the conductive coating film 4C exposed by peeling off the repair point 5 toward the ground surface part 7 that has been undercoated. The regenerated wiring circuit is wired across the repaired cracked part to the repair point 5 on the opposite side or the start point of current flow. It is preferable to place the repair point 5 at the position of the peeled off repair point 5 or in the middle of the new wiring.
[0035] FIG. 6(f) is a cross-sectional view showing the state where a top coat 5D is applied to further protect the conductive coating 4C. The crack detection coating layer that was ground off to repair the crack is regenerated. The remaining wiring circuit uses the wiring circuit of the healthy part as it is, so the crack detection coating layer can be easily maintained. If the repair point 5 is not used, it is necessary to redraw all the wiring circuits. Therefore, this embodiment contributes to a significant reduction in work. [Explanation of symbols]
[0036] 1 Steel structures (steel plates) 2. Welding 2A heat affected zone 2B Stress load range 4. Crack detection coating layer 4A Primer coating (first insulating coating) 4B Topcoat (first insulating coating) 4C Conductive coating (wiring circuit for crack detection) 4D Topcoat (Second insulating coating) 4E Coating area (for crack detection coating layer) 5 Repair points (masking material) 5A Tab 5B Peeling off piece (from repair point) 6. Crack 7 Surface grinding section
Claims
1. A crack detection coating layer comprising a first insulating coating formed on a surface of a steel structure, a conductive coating for crack detection applied to the surface of the first insulating coating, and a second insulating coating applied to protect the conductive coating, A crack detection coating layer having a repair point between the conductive coating and the second insulating coating for peeling the conductive coating to expose it.
2. 2. The coating layer for detecting cracks according to claim 1, wherein the material of the repair point is at least one selected from the group consisting of paper, nylon, vinyl and cellophane.
3. The conductive coating contains silver powder and silver-coated copper powder as pigments of a conductive paint, The crack detection coating layer according to claim 1 , wherein the conductive coating contains at least one resin selected from an acrylic resin and an epoxy resin.
4. A coating layer for detecting cracks according to any one of claims 1 to 3 is formed on a surface of a steel structure, A method for detecting cracks in a steel structure, comprising: passing an electric current through a wiring circuit of the conductive coating film and detecting a break in the wiring circuit due to a crack in the steel structure.
5. A coating layer for detecting cracks according to any one of claims 1 to 3 is formed on a surface of a steel structure, A current is passed through the wiring circuit of the conductive coating film, and a break in the wiring circuit due to a crack in the steel structure is detected; After removing the paint film around the detected crack, the crack is repaired by welding. forming a first insulating coating film on the surface of the steel structure exposed by peeling off the coating film; Peeling off the repair point near the crack to expose the conductive coating; A wiring circuit is formed by a conductive coating film across the repaired crack, between the exposed repair points, or between the exposed repair points and the current flow start point; A method for repairing cracks in a steel structure, comprising applying a second insulating coating to protect the conductive coating.
Citation Information
Patent Citations
Structure maintenance support system
JP2001201477A
Crack detecting tape, and crack detection system
JP2005091167A
Crack-sensing material, method for manufacturing the same, crack-sensing system and crack sensing method
JP2005172809A
Crack detecting electric circuit, its manufacturing method, crack detecting system and crack detecting method
JP2006317350A
State change detection method for concrete structure using conductive coating material protective tape
JP2016024139A