Coating layer forming method and coated article
A multi-component thermosetting coating composition forms a stain-resistant film with high modulus, addressing the challenge of graffiti removal by providing easy and clean cleaning while maintaining film integrity.
Patent Information
- Application Number
- JP2023077644
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing coating compositions fail to provide effective stain resistance and ease of removal for graffiti, requiring time-consuming and difficult cleaning processes that can erode the paint film.
A multi-component thermosetting coating composition comprising acrylic polyol, polyisocyanate compound, and optional additives like colloidal silica and catalysts, which forms a coating film with a minimum storage modulus of 2.6×10^7 Pa, ensuring stain resistance and easy removal.
The coating film exhibits excellent hardness, stain resistance, and scratch resistance, allowing easy and clean removal of graffiti while maintaining a transparent finish.
Smart Images

Figure 2024162283000001 
Figure 2024162283000002 
Figure 2024162283000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating film forming method and a coated article. [Background technology]
[0002] Artificial graffiti on various building structures, railway cars, large vehicles, etc. is a major social problem because it not only damages the beauty and scenery, but also leads to a deterioration of public order. However, the removal of graffiti drawn on a coated object with spray paint, oil-based pen, etc. is time-consuming and labor-intensive, and is difficult to remove cleanly, and there is a risk of damaging the existing coating film. Therefore, there is a demand for a coating composition that has removable properties that allow graffiti to be easily and cleanly removed.
[0003] Patent Document 1 discloses a coating composition containing a resin (A) having a hydroxyl group and an alkoxysilyl group, a curing agent (B) and an acrylic resin-coated silica particle (C) dispersion, the acrylic resin-coated silica particle (C) dispersion being a reaction product of silica particles (c1) having a polymerizable unsaturated group and a polymerizable unsaturated monomer mixture (c2), and the polymerizable unsaturated monomer mixture (c2) contains, as at least a part of its components, a polymerizable unsaturated monomer (c21) having a polysiloxane structure represented by formula (I) and an alkoxysilyl group-containing polymerizable unsaturated monomer (c22). It is described that the coating composition can form a coating film excellent in stain removability, scratch resistance and transparency. However, there are cases where stain removability is not sufficient. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2021 / 131444 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method for forming a stain-resistant coating film having removable properties that allows graffiti to be easily and cleanly removed. [Means for solving the problem]
[0006] As a result of intensive research into solving the above problems, the inventors have discovered a coating film forming method in which a multi-liquid type thermosetting coating composition containing a base component containing an acrylic polyol (A) and an organic solvent, and a curing agent component containing a polyisocyanate compound (B) and an organic solvent is applied and cured by heating, and the coating film formed has a minimum storage modulus E' in the range of 40 to 200°C. min is 2.6 × 10 7 The present inventors have found that the above-mentioned problems can be solved by a coating film forming method, which provides a stain-resistant coating film having a surface tension of 10 Pa or more, and have completed the present invention.
[0007] That is, the present invention provides the following multi-component thermosetting coating composition, a coating film forming method and coated article using the multi-component thermosetting coating composition, and a stain-resistant coating film. Item 1. A coating film forming method comprising applying a multi-liquid thermosetting coating composition containing a base component containing an acrylic polyol (A) and an organic solvent, and a curing agent component containing a polyisocyanate compound (B) and an organic solvent, and then heat-curing the composition, The minimum storage modulus E' of the coating film formed in the range of 40 to 200°C min is 2.6 × 10 7 The coating film forming method is a stain-resistant coating film having a viscosity of 100 Pa or more. Item 2. The method for forming a coating film according to Item 1, wherein the acrylic polyol (A) contains an alkoxysilyl group. Item 3. The method for forming a coating film according to Item 1 or 2, wherein the polyisocyanate compound (B) contains an isocyanurate trimer. Item 4. The coating film forming method according to any one of Items 1 to 3, wherein the multi-liquid thermosetting coating composition further contains at least one catalyst compound (C) selected from amidine compounds, guanidine compounds, phosphazene compounds, imidazole compounds, phosphate compounds, and phosphite compounds. Item 5. The method for forming a coating film according to any one of Items 1 to 4, wherein the multi-component thermosetting coating composition further contains a silicone (D) modified with a hydroxyl group-containing resin. Item 6. The method for forming a coating film according to any one of Items 1 to 5, wherein the multi-component thermosetting coating composition further contains an organic solvent-dispersed colloidal silica (E). Item 7. An article coated with the coating film forming method according to any one of items 1 to 6. Effect of the Invention
[0008] According to the coating film forming method of the present invention, it is possible to form a stain-resistant coating film from which graffiti can be easily and cleanly removed. The coating film formed using the coating film forming method of the present invention has excellent hardness, stain resistance, a transparent finish, and scratch resistance, and can be widely used in various applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described in detail.
[0010] It should be understood that the present invention is not limited to the following embodiments, but includes various modified examples that are implemented within the scope that does not deviate from the gist of the present invention.
[0011] In this specification, "parts" indicates parts by mass and "%" indicates % by mass.
[0012] Acrylic polyol (A) The multi-liquid thermosetting coating composition used in the coating film forming method of the present invention contains an acrylic polyol (A). The content is preferably 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more based on the resin solid content mass contained in the main component, and is preferably 20 to 80% by mass, preferably 30 to 75% by mass, more preferably 40 to 70% by mass based on the resin solid content mass contained in the entire multi-liquid thermosetting coating composition.
[0013] The acrylic polyol (A) can be produced by copolymerizing a hydroxyl group-containing polymerizable unsaturated monomer (a11) and another copolymerizable polymerizable unsaturated monomer (a13).
[0014] The hydroxyl-containing polymerizable unsaturated monomer (a11) is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated groups in one molecule. In this specification, the polymerizable unsaturated group means an unsaturated group that can undergo radical polymerization. Examples of such polymerizable unsaturated groups include vinyl groups and (meth)acryloyl groups.
[0015] Furthermore, the hydroxyl group based on the hydroxyl group-containing polymerizable unsaturated monomer (a11) can function as a crosslinkable functional group of the resulting acrylic polyol (A).
[0016] Specific examples of the hydroxyl group-containing polymerizable unsaturated monomer (a11) include monoesters of acrylic acid or methacrylic acid with dihydric alcohols having 2 to 10 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, caprolactone-modified hydroxyl group-containing (meth)acrylate, and 4-methylolcyclohexyl (meth)acrylate. Commercially available caprolactone-modified hydroxyl group-containing (meth)acrylates include "Placcel FM" (trade name, manufactured by Daicel Chemical Industries, Ltd.), and commercially available 4-methylolcyclohexyl acrylates include "CHDMMA" (trade name, manufactured by Nippon Kasei Chemical Industries, Ltd.). These hydroxyl group-containing polymerizable unsaturated monomers (a11) can be used alone or in combination of two or more kinds.
[0017] In this specification, "(meth)acrylate" means "acrylate or methacrylate". "(meth)acrylic acid" means "acrylic acid or methacrylic acid". "(meth)acryloyl" means "acryloyl or methacryloyl". "(meth)acrylamide" means "acrylamide or methacrylamide".
[0018] As the hydroxyl group-containing polymerizable unsaturated monomer (a11), from the viewpoint of preventing the penetration of inks and contaminants, it is preferable to use a polymerizable unsaturated monomer having a hydroxyl group-containing hydrocarbon group having 2 to 20 carbon atoms, specifically, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-methylolcyclohexyl acrylate, etc.
[0019] The other copolymerizable polymerizable unsaturated monomer (a13) is a compound having one or more polymerizable unsaturated groups in one molecule other than the hydroxyl group-containing polymerizable unsaturated monomer (a11), and specific examples thereof are listed in the following (1) to (11). (1) Aromatic polymerizable unsaturated monomers: for example, styrene, α-methylstyrene, vinyltoluene, etc. (2) Polymerizable unsaturated monomers having a branched structure and a hydrocarbon group having 8 or more carbon atoms: For example, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isomyristyl (meth)acrylate, isostearyl (meth)acrylate, etc. Commercially available products include "Isostearyl Acrylate" (trade name, manufactured by Osaka Organic Chemical Industry Co., Ltd.), etc. (3) Polymerizable unsaturated monomers containing an alicyclic hydrocarbon group having 3 to 20 carbon atoms: for example, polymerizable unsaturated monomers containing a bridged alicyclic hydrocarbon group having 10 to 20 carbon atoms, such as isobornyl (meth)acrylate, tricyclodecanyl (meth)acrylate, adamantyl (meth)acrylate, 3,5-dimethyladamantyl (meth)acrylate, and 3-tetracyclododecyl (meth)acrylate; polymerizable unsaturated monomers having an alicyclic hydrocarbon group having 3 to 12 carbon atoms, such as cyclohexyl (meth)acrylate, 4-methylcyclohexylmethyl (meth)acrylate, 4-ethylcyclohexylmethyl (meth)acrylate, 4-methoxycyclohexylmethyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclododecyl (meth)acrylate, and tetrahydrofurfuryl (meth)acrylate. (4) Linear or branched alkyl esters of (meth)acrylic acid having 1 to 7 carbon atoms: methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, and the like. (5) Linear alkyl esters of (meth)acrylic acid having 8 to 22 carbon atoms: for example, lauryl (meth)acrylate, stearyl (meth)acrylate, etc. (6) Epoxy group-containing polymerizable unsaturated monomers: for example, glycidyl (meth)acrylate. (7) Nitrogen-containing polymerizable unsaturated monomers: for example, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, vinylpyridine, vinylimidazole, and the like. (8) Other vinyl compounds: For example, vinyl acetate, vinyl propionate, vinyl chloride, vinylidene chloride, divinyl ether, and versatic acid vinyl esters such as "Veova 9" and "Veova 10" (product names, manufactured by Hexion). (9) Unsaturated group-containing nitrile compounds: for example, (meth)acrylonitrile, etc. (10) Acidic functional group-containing polymerizable unsaturated monomers: for example, carboxyl group-containing unsaturated monomers such as (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, and maleic anhydride; sulfonic acid group-containing unsaturated monomers such as vinyl sulfonic acid and sulfoethyl (meth)acrylate; acidic phosphate ester-based unsaturated monomers such as 2-(meth)acryloyloxyethyl acid phosphate, 2-(meth)acryloyloxypropyl acid phosphate, 2-(meth)acryloyloxy-3-chloropropyl acid phosphate, and 2-(meth)acryloyloxyethylphenyl phosphoric acid. (11) Polymerizable unsaturated monomers having a polydimethylsiloxane structure: for example, commercially available products such as "Silaplane FM-0721", "Silaplane FM-0711", and "Silaplane FM-0725" (all of which are product names manufactured by JNC Corporation), "X-22-174ASX", "X-22-174BX", "KF-2012", "X-22-2426", "X-22-2404", and "X-22-2475" (all of which are product names manufactured by Shin-Etsu Chemical Co., Ltd.), and the like. (12) Alkoxysilyl group-containing polymerizable unsaturated monomer: a compound having one or more alkoxysilyl groups and one or more polymerizable unsaturated groups in one molecule. For example, vinyltrimethoxysilane, vinyltriethoxysilane, acryloxyethyltrimethoxysilane, methacryloxyethyltrimethoxysilane, acryloxypropyltrimethoxysilane, methacryloxypropyltrimethoxysilane, acryloxypropyltriethoxysilane, methacryloxypropyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, etc. can be mentioned. Among these, preferred alkoxysilyl group-containing polymerizable unsaturated monomers include vinyltrimethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, etc.
[0020] The other copolymerizable polymerizable unsaturated monomers (a13) may be used alone or in combination of two or more. Among them, it is preferable to use an acidic functional group-containing polymerizable unsaturated monomer or an alkoxysilyl group-containing polymerizable unsaturated monomer.
[0021] The acrylic polyol (A) can be obtained by copolymerizing a polymerizable unsaturated monomer mixture consisting of the hydroxyl-containing polymerizable unsaturated monomer (a11) and another copolymerizable polymerizable unsaturated monomer (a13). The proportion of the hydroxyl-containing polymerizable unsaturated monomer (a11) used is suitably 15 to 55 mass%, preferably 20 to 50 mass%, based on the total mass of the copolymerizable monomer components constituting the acrylic polyol (A), from the viewpoints of the stain removability, scratch resistance, water resistance, etc. of the resulting coating film.
[0022] Among the other polymerizable unsaturated monomers (a13), acidic functional group-containing polymerizable unsaturated monomers such as carboxyl group-containing unsaturated monomers, sulfonic acid group-containing unsaturated monomers, and acidic phosphate ester-based unsaturated monomers can act as internal catalysts when the obtained acrylic polyol (A) undergoes a crosslinking reaction with a polyisocyanate compound, and the amount of the monomers used is preferably within a range of about 0 to 5 mass%, more preferably within a range of about 0 to 3 mass%, based on the total mass of the copolymerizable monomer components constituting the acrylic polyol (A).
[0023] When using an alkoxysilyl group-containing polymerizable unsaturated monomer, the proportion of the monomer is 5 to 60 mass%, preferably 20 to 50 mass%, based on the total mass of the copolymerizable monomer components constituting the acrylic polyol (A) in terms of the stain removability, scratch resistance, transparency, etc. of the resulting coating film. The copolymerization method for obtaining the acrylic polyol (A) by copolymerizing the above-mentioned monomer mixture is not particularly limited, and a known copolymerization method can be used. Among them, it is preferable to use a solution polymerization method in which polymerization is performed in an organic solvent in the presence of a polymerization initiator.
[0024] Examples of organic solvents used in the solution polymerization method include aromatic solvents such as toluene, xylene, and high-boiling aromatic hydrocarbons; ester solvents such as ethyl acetate, butyl acetate, 3-methoxybutyl acetate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and methyl amyl ketone; glycol ether solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, and propylene glycol monomethyl ether; alcohol organic solvents such as methanol, ethanol, isopropanol, n-butanol, and isobutanol; propyl propionate, butyl propionate, and ethoxyethyl propionate. Commercially available high-boiling aromatic hydrocarbons include, for example, "Swasol 1000" (trade name, manufactured by Cosmo Oil Co., Ltd., high-boiling petroleum solvent).
[0025] These organic solvents can be used alone or in combination of two or more. When the acrylic polyol (A) has a high hydroxyl value, it is preferable to use a high-boiling ester solvent or ketone solvent as the organic solvent from the viewpoint of the solubility of the resin. Furthermore, a high-boiling aromatic solvent can be used in combination with a high-boiling ester solvent or ketone solvent.
[0026] Examples of the polymerization initiator that can be used in the copolymerization of the acrylic polyol (A) include known radical polymerization initiators such as 2,2'-azobisisobutyronitrile, benzoyl peroxide, 2,2-di(t-amylperoxy)butane, di-t-butyl peroxide, di-t-amyl peroxide, t-butyl peroctoate, and 2,2'-azobis(2-methylbutyronitrile).
[0027] The acrylic polyol (A) may be composed of one type of copolymer, or may be composed of two or more types of copolymers.
[0028] From the viewpoint of stain removability, the hydroxyl value of the acrylic polyol (A) is suitably within the range of 120 to 200 mgKOH / g, preferably 130 to 200 mgKOH / g, and more preferably 140 to 200 mgKOH / g.
[0029] The weight average molecular weight of the acrylic polyol (A) is preferably within the range of 5,000 to 30,000, particularly 5,000 to 20,000, and further particularly 6,000 to 15,000, from the viewpoints of stain removability, scratch resistance, transparency, and the like.
[0030] In this specification, the weight average molecular weight and number average molecular weight are values calculated from a chromatogram measured by a gel permeation chromatograph based on the molecular weight of standard polystyrene. The gel permeation chromatograph used was "HLC8120GPC" (manufactured by Tosoh Corporation). Four columns, "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL", and "TSKgel G-2000HXL" (all of which are product names manufactured by Tosoh Corporation), were used, and the measurement was performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 mL / min, and detector: RI.
[0031] The glass transition temperature of the acrylic polyol (A) is preferably within the range of -30°C to 50°C, particularly -10°C to 40°C, from the standpoints of stain removability, scratch resistance, smoothness, and the like.
[0032] In the present invention, the glass transition temperature Tg is a value calculated by the following formula. 1 / Tg(K)=W1 / T1+W2 / T2+...Wn / Tn Tg(℃)=Tg(K)-273 In the formula, W1, W2, ...Wn are the mass fractions of each monomer, and T1, T2...Tn are the glass transition temperatures Tg (K) of the homopolymers of each monomer. The glass transition temperature of the homopolymer of each monomer is a value according to POLYMER HANDBOOK Fourth Edition, edited by J. Brandrup, Eh Immergut, and EA Grulke (1999), and the glass transition temperature of a monomer not described in the literature is a value obtained by synthesizing a homopolymer of the monomer so that the weight-average molecular weight is about 50,000, and measuring the glass transition temperature with a Seiko Electronics DSC220U (differential scanning calorimeter). The measurement was performed by weighing out a predetermined amount of 50 mg of the sample into a dedicated sample dish, drying it at 130°C for 3 hours, and then heating it in an inert gas from -50°C to 150°C at a speed of 10°C / min, and reading the temperature of the inflection point of the obtained heat change curve.
[0033] Polyisocyanate compound (B) The polyisocyanate compound (B) in the present invention is a compound having two or more isocyanate groups in one molecule.
[0034] Examples of the polyisocyanate compound (B) include aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, aromatic polyisocyanates, and derivatives of the polyisocyanates.
[0035] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4 or 2,2,4-trimethylhexamethylene diisocyanate, dimer acid diisocyanate, methyl 2,6-diisocyanatohexanoate (common name: lysine diisocyanate), aliphatic diisocyanates such as 2-isocyanatoethyl 2,6-diisocyanatohexanoate, 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, and 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane.
[0036] Examples of the alicyclic polyisocyanate include 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexylene diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexylene diisocyanate, alicyclic diisocyanates such as 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylylene diisocyanate) or mixtures thereof, methylene bis(4,1-cyclohexanediyl) diisocyanate (common name: hydrogenated MDI), and norbornane diisocyanate; 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane, 2-(3-isocyanatopropyl)- 2,5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 2-(3-isocyanatopropyl)-2,6-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-di(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 6-(2-iso alicyclic triisocyanates such as (2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, and 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane.
[0037] Examples of the aromatic aliphatic polyisocyanate include aromatic aliphatic diisocyanates such as methylenebis(4,1-phenylene)diisocyanate (common name: MDI), 1,3- or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (common name: tetramethylxylylene diisocyanate) or a mixture thereof; and aromatic aliphatic triisocyanates such as 1,3,5-triisocyanatomethylbenzene.
[0038] Examples of the aromatic polyisocyanate include aromatic diisocyanates such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4-tolylene diisocyanate (common name: 2,4-TDI) or 2,6-tolylene diisocyanate (common name: 2,6-TDI) or a mixture thereof, 4,4'-toluidine diisocyanate, 4,4'-diphenyl ether diisocyanate, etc.; aromatic triisocyanates such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, etc.; and aromatic tetraisocyanates such as 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate, etc.
[0039] Furthermore, examples of derivatives of the above polyisocyanates include dimers, trimers, biurets, allophanates, uretdione, uretoimine, isocyanurates, oxadiazinetrione, polymethylene polyphenyl polyisocyanates (crude MDI, polymeric MDI), crude TDI, and the like.
[0040] The above polyisocyanates and derivatives thereof may be used alone or in combination of two or more kinds.
[0041] In the multi-liquid thermosetting coating composition used in the coating film forming method of the present invention, the polyisocyanate compound (B) preferably contains an isocyanurate trimer. When the polyisocyanate compound (B) contains an isocyanurate trimer, the crosslink density of the coating film formed is increased, resulting in good removability.
[0042] As the polyisocyanate compound (B), a blocked polyisocyanate compound in which the isocyanate group of the polyisocyanate compound is blocked may be used. As the blocking agent, for example, phenol compounds, lactam compounds, alcohol compounds, oxime compounds, mercaptan compounds, active methylene compounds such as dimethyl malonate and diethyl malonate, etc. can be suitably used. Blocking can be easily performed by mixing an unblocked polyisocyanate compound with a blocking agent. These polyisocyanate compounds can be used alone or in combination of two or more, and an unblocked polyisocyanate compound and a blocked polyisocyanate compound can also be used in combination.
[0043] From the viewpoints of the stain removability, scratch resistance, curing property, etc. of the resulting coating film, the content of the above polyisocyanate compound (B) in the coating composition is preferably such that the equivalent ratio (NCO / OH) of the isocyanate groups in the polyisocyanate compound (B) to the hydroxyl groups of the hydroxyl-containing resin in the coating composition is usually within the range of 0.5 to 2.0, particularly 0.6 to 1.2.
[0044] From the viewpoints of the contamination removability, scratch resistance, curing property, etc. of the resulting coating film, the content of the polyisocyanate compound (B) in the coating composition is preferably within the range of 0.1 to 50 mass%, more preferably within the range of 5 to 45 mass%, and even more preferably within the range of 10 to 40 mass%, based on the resin solids mass in the coating composition.
[0045] Catalyst compound (C) The multi-component thermosetting coating composition used in the coating film forming method of the present invention preferably contains at least one catalyst compound (C) selected from amidine compounds, guanidine compounds, phosphazene compounds, imidazole compounds, phosphate compounds and phosphite compounds, from the viewpoints of curability and stain resistance.
[0046] Examples of the amidine compound include 1,5-diazabicyclo[4,3,0]-nonene-5 (DBN) and derivatives thereof, 1,5-diazabicyclo[4,4,0]-decene-5 and derivatives thereof, 1,8-diazabicyclo[5,4,0]-undecene-7 (DBU) and derivatives thereof, 5-hydroxypropyl-1,8-diazabicyclo[5,4,0]-undecene-7 and derivatives thereof, and 5-dibutylamino-1,8-diazabicyclo[5,4,0]-undecene-7 and derivatives thereof.
[0047] Examples of the guanidine compound include 1,3-diphenylguanidine, 1,3-dimethylguanidine, and 1,1,3,3-tetramethylguanidine (TMG).
[0048] Examples of phosphazene compounds include tert-butylimino-tris(dimethylamino)phosphorane and its derivatives, tert-butylimino-tri(pyrrolidino)phosphorane and its derivatives, 1-tert-octyl-4,4,4-tris(dimethylamino)-2,2-bis[tris(dimethylamino)phosphoranylideneamino]-2λ5,4λ5-catenadi(phosphazene) and its derivatives, and the like.
[0049] Examples of the imidazole compound include 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-phenylimidazole.
[0050] Examples of the phosphate ester compounds include trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, trihexyl phosphate, tris(2-ethylhexyl)phosphate, trioctyl phosphate, trinonyl phosphate, tridecyl phosphate, trilauryl phosphate, trimyristyl phosphate, tricetyl phosphate, tristearyl phosphate, trioleyl phosphate, tribehenyl phosphate, monomethyl phosphate, dimethyl phosphate, monoethyl phosphate, diethyl phosphate, monopropyl phosphate, dipropyl phosphate, monoisopropyl phosphate, diisopropyl phosphate, monobutyl phosphate, dibutyl phosphate, monopentyl phosphate, phosphate, dipentyl phosphate, monohexyl phosphate, dihexyl phosphate, monooctyl phosphate, dioctyl phosphate, mono 2-ethylhexyl phosphate, di 2-ethylhexyl phosphate, monodecyl phosphate, didecyl phosphate, monoisodecyl phosphate, diisodecyl phosphate, monoundecyl phosphate, diundecyl phosphate, monododecyl phosphate, didodecyl phosphate, monotetradecyl phosphate, ditetradecyl phosphate, monohexadecyl phosphate, dihexadecyl phosphate, monooctadecyl phosphate, dioctadecyl phosphate, monophenyl phosphate, diphenyl phosphate, monobenzyl phosphate, and dibenzyl phosphate.
[0051] Examples of the phosphite ester compound include triphenyl phosphite, diphenyl phosphite, tri-o-tolyl phosphite, di-o-tolyl phosphite, tri-m-tolyl phosphite, di-m-tolyl phosphite, tri-p-tolyl phosphite, di-p-tolyl phosphite, di-o-chlorophenyl phosphite, tri-p-chlorophenyl phosphite, and di-p-chlorophenyl phosphite. These catalyst compounds (C) can be used alone or in combination of two or more. Among them, it is preferable to contain an amidine compound, and particularly preferable to contain 1,8-diazabicyclo[5,4,0]-undecene-7 (DBU) and its derivatives.
[0052] The catalyst compound (C) is suitably contained within the range of 0.01 to 10 mass %, preferably 0.1 to 8 mass %, and more preferably 0.2 to 6 mass %, based on the mass of the resin solid content contained in the main component.
[0053] Silicone modified with hydroxyl-containing resin (D) The multi-liquid thermosetting coating composition used in the coating film forming method of the present invention preferably contains a silicone (D) modified with a hydroxyl-containing resin. A coating film obtained from a coating composition containing a silicone (D) modified with a hydroxyl-containing resin repels ink and makes graffiti less likely to adhere, improving the so-called repellency.
[0054] When the multi-component thermosetting coating composition contains a silicone (D) modified with a hydroxyl group-containing resin, it is suitable to contain it in an amount of 0.01 to 20 mass %, preferably 0.1 to 15 mass %, and more preferably 1 to 10 mass %, based on the mass of the resin solids contained in the main component.
[0055] The hydroxyl value of the silicone (D) modified with a hydroxyl-containing resin in the present invention is preferably from 10 to 200 mgKOH / g, and more preferably from 20 to 150 mgKOH / g.
[0056] The number average molecular weight of the silicone (D) modified with a hydroxyl-containing resin in the present invention is preferably within the range of 1,000 to 100,000, and more preferably 3,000 to 50,000.
[0057] Examples of commercially available silicones (D) modified with hydroxyl-containing resins include X-22-4952 and KF-6123 (manufactured by Shin-Etsu Chemical Co., Ltd.), which contain a polyether structure in the polymer structure; BYK-370, BYK-375, BYK-377, and BYK-SILCLEAN3720 (manufactured by BYK Japan), which contain a polyester structure in the polymer structure; and BYK-SILCLEAN3700 (manufactured by BYK Japan), ZX-028-G (manufactured by T&K TOKA), and SIMAC US-270 (manufactured by Toagosei Co., Ltd.), which contain an acrylic structure in the polymer structure.
[0058] Organic solvent-dispersed colloidal silica (E) The multi-liquid thermosetting coating composition used in the coating film forming method of the present invention preferably contains an organic solvent-dispersed colloidal silica (E). By containing the organic solvent-dispersed colloidal silica (E), a phase with a high crosslink density is formed on the coating film surface layer, improving the stain resistance and scratch resistance.
[0059] Organic solvent-dispersed colloidal silica (E) is a stable dispersion of silica particles with a particle size of about 5 to 120 nm in organic solvents such as alcohols, glycols, and ethers. Commercially available products include Snowtex MPA-ST, Snowtex IPA-ST, Snowtex IPA-ST-UP, Snowtex IPA-ST-ZL, Snowtex EG-ST, Snowtex NPC-ST-30, Snowtex DMAC-ST, Snowtex Examples of such compounds include SNOWTEX MEK-ST, SNOWTEX MEK-ST-UP, SNOWTEX MEK-ST-L, SNOWTEX MIBK-ST, SNOWTEX XBA-ST, SNOWTEX PMA-ST, SNOWTEX PGM-ST (all manufactured by Nissan Chemical Industries, Ltd.), NANOBYK-3650, NANOBYK-3651, NANOBYK-3652 (all manufactured by BYK Japan), and the OSCAL series (manufactured by JGC Catalysts and Chemicals).
[0060] For stability in the coating material, it is preferable that the organic solvent-dispersed colloidal silica (E) has a silica surface modified with a resin. Examples of such a modification method include a method of reacting the colloidal silica with 3-methacryloyloxypropyltrimethoxysilane, 3-acryloyloxypropyltrimethoxysilane, 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, 1,1-bis(acryloyloxymethyl)ethyl isocyanate, etc. Among them, colloidal silica coated with an acrylic resin having a polysiloxane structure as described in WO 2021 / 131444 is particularly preferable.
[0061] The colloidal silica may be used alone or in combination of two or more kinds.
[0062] The average primary particle size of the organic solvent-dispersed colloidal silica (E) is preferably 5 to 100 nm, more preferably 5 to 50 nm. If the average primary particle size is less than 5 nm, when the dispersion is mixed with other organic materials, the effect of improving mechanical properties, etc. may be reduced. If the average primary particle size exceeds 100 nm, transparency may be impaired.
[0063] In this specification, the "average primary particle size" refers to the median diameter (d50) of the volume-based particle size distribution, and the volume-based particle size distribution is measured by a laser diffraction / scattering method. In the present invention, the volume-based particle size distribution of the dispersion was measured using a laser diffraction / scattering type particle size distribution measuring device "Microtrac NT3300" (product name, manufactured by Nikkiso Co., Ltd.). At that time, the sample concentration was adjusted to be within a predetermined transmittance range set in the device.
[0064] When the multi-component thermosetting coating composition contains organic solvent-dispersed colloidal silica (E), it is suitable to contain it in an amount of 0.1 to 50 mass%, preferably 0.5 to 40 mass%, more preferably 1 to 30 mass%, based on the mass of the resin solid content contained in the main component.
[0065] Multi-component thermosetting coating composition The multi-liquid thermosetting coating composition used in the coating film forming method of the present invention contains a base component and a curing agent component. The base component contains the above-mentioned acrylic polyol (A) and an organic solvent, and the curing agent component contains the above-mentioned polyisocyanate compound (B) and an organic solvent.
[0066] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; esters such as ethyl acetate, butyl acetate, methyl benzoate, ethyl ethoxypropionate, ethyl propionate, and methyl propionate; ethers such as tetrahydrofuran, dioxane, and dimethoxyethane; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbons, aliphatic hydrocarbons, and the like, and may be used alone or in combination of two or more. In addition, the same organic solvent may be used for the main component and the curing agent component, or different organic solvents may be used.
[0067] The above organic solvents can be used in appropriate combination depending on the purpose, such as adjusting the viscosity or the coatability.
[0068] When the multi-component thermosetting coating composition used in the coating film forming method of the present invention contains the above-mentioned catalyst compound (C), it may be contained in either the base component or the curing agent component, or it may be contained in both, or it may be contained in a third component different from the base component and the curing agent component. However, from the viewpoints of storage stability and workability, it is preferable that it be contained in a third component different from the base component and the curing agent component.
[0069] When the multi-component thermosetting coating composition used in the coating film forming method of the present invention contains the above-mentioned hydroxyl group-containing resin-modified silicone (D), it is preferred from the standpoint of storage stability that it is contained in the main component or in a third component different from the main component and the curing agent component, and from the standpoint of workability that it is contained in the main component.
[0070] When the multi-component thermosetting coating composition used in the coating film forming method of the present invention contains the above-mentioned organic solvent-dispersed colloidal silica (E), it is preferably contained in the main component or a third component different from the main component and the curing agent component from the viewpoint of storage stability, and it is particularly suitable that it is contained in the main component from the viewpoint of workability.
[0071] The multi-component thermosetting coating composition used in the coating film forming method of the present invention may further contain typical coating additives such as resins other than acrylic polyols, pigments, ultraviolet absorbers (e.g., benzotriazole-based absorbers, triazine-based absorbers, salicylic acid derivative-based absorbers, benzophenone-based absorbers, etc.), light stabilizers (e.g., hindered piperidines, etc.), dehydrating agents, thickeners, antifoamers, plasticizers, surface conditioners, anti-settling agents, etc., either alone or in combination of two or more kinds.
[0072] Examples of resins other than the acrylic polyol (A) include acrylic resins (excluding those containing hydroxyl groups), polyester resins, alkyd resins, urethane resins, fluororesins, epoxy resins, silicone resins, polyether resins, acrylic silicone resins, and vinyl acetate-Beova resins.
[0073] When the multi-component thermosetting coating composition used in the coating film forming method of the present invention contains an ultraviolet absorber, the amount of the ultraviolet absorber is preferably within the range of 0.1 to 10 parts by mass, more preferably within the range of 0.2 to 5 parts by mass, and even more preferably within the range of 0.3 to 2 parts by mass, based on 100 parts by mass of the total resin solids in the coating composition.
[0074] When the multi-component thermosetting coating composition used in the coating film forming method of the present invention contains a light stabilizer, the amount of the light stabilizer is preferably within the range of 0.1 to 10 parts by mass, more preferably within the range of 0.2 to 5 parts by mass, and even more preferably within the range of 0.3 to 2 parts by mass, based on 100 parts by mass of the total resin solids in the coating composition.
[0075] Examples of the dehydrating agent include metal alkoxides such as aluminum isopropylate, aluminum sec-butylate, tetraisopropyl titanate, tetra normal butyl titanate, zirconium normal butylate, ethyl silicate, and vinyltrimethoxysilane; organic alkoxy compounds such as trimethyl orthoformate, triethyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, triisopropyl orthoacetate, and dimethoxypropane; and monofunctional isocyanates such as "Additive TI" (product name, manufactured by Sumika Bayer Urethane Co., Ltd.). These may be used alone or in combination of two or more kinds.
[0076] When the multi-component thermosetting coating composition used in the coating film forming method of the present invention contains a dehydrating agent, the amount of the dehydrating agent is preferably within the range of 0.01 to 15 parts by mass, and more preferably within the range of 0.1 to 8% by mass, based on 100 parts by mass of the total resin solids in the coating.
[0077] The solid content of the multi-liquid thermosetting coating composition used in the coating film forming method of the present invention is not particularly limited. For example, in terms of smoothness of the cured coating film and shortening of the drying time, it is preferable to appropriately adjust the viscosity by Ford Cup No. 4 at 20°C to the range of 15 to 60 seconds using a solvent such as the organic solvent described above.
[0078] In this specification, the solid content means the residue after removing the volatile components, and the residue may be in a solid or liquid state at room temperature. The solid content mass can be calculated by multiplying the solid content rate, which is the ratio of the amount of the remaining substance when dried to the mass before drying, by the mass of the sample before drying.
[0079] Method for forming stain-resistant coating film The stain-resistant coating film obtained by the coating film forming method of the present invention has a minimum storage modulus E' of 40 to 200°C of the coating film formed by applying the above-mentioned multi-liquid type thermosetting coating composition. min is 2.6 × 10 7Pa or more. The minimum storage modulus E' min is 2.6 × 10 7 When the crosslinking density is 3.6×10 Pa or more, the coating film has a high crosslinking density, so inks used for graffiti are less likely to penetrate and the coating has high removability. 7 Pa or more, and 4.6×10 7 From the viewpoint of crack resistance of the coating film, the coating composition is applied, heat cured at 80° C. for 30 minutes, and allowed to stand for 1 hour to form a coating film having a minimum storage modulus E' in the range of 40 to 200° C. min is 1.0×10 9 It is preferable that the pressure is 0.1 Pa or less.
[0080] In this specification, the method for preparing the coating film used in measuring the storage modulus is as follows. 1. The coating composition is applied onto a polypropylene plate so that the cured film thickness is 40 μm, then dried at 80° C. for 30 minutes and allowed to stand for 1 hour to form a cured coating film. 2. The cured coating film is cut into strips 20 mm long and 5 mm wide, and peeled off from the polypropylene plate to obtain strips of free coating film as samples.
[0081] In this specification, the storage modulus was measured using an FT rheology spectrometer "Rheogel E-400" (manufactured by UBM Co., Ltd.). The free coating film prepared under the above conditions was subjected to dynamic viscoelasticity measurement under conditions of a frequency of 11 Hz, a heating rate of 4°C / min, and a temperature range of room temperature to 200°C, and the minimum storage modulus E' in the range of 40 to 200°C was measured. min is obtained.
[0082] The substrate to which the present coating film forming method is applied is not particularly limited. For example, metal substrates such as cold-rolled steel, galvanized steel, zinc alloy-plated steel, stainless steel, and tin-plated steel, aluminum, and aluminum alloy substrates, and various plastic materials can be mentioned. In addition, automobiles, trucks, motorcycles, buses, railroad vehicles, two-wheeled vehicles, industrial machinery, construction machinery, ship bodies, building materials, and housing equipment and their parts formed by these can be mentioned, and among them, the coating method is particularly suitable for use with railroad vehicles, building materials, and housing equipment. In addition, the substrate may be one in which the metal surface of the metal substrate or vehicle body has been subjected to surface treatment such as phosphate treatment, chromate treatment, and composite oxide treatment. Furthermore, the substrate may be one in which an undercoat coating film such as various electrodeposition paints has been formed on the metal substrate or vehicle body, or one in which the undercoat coating film and intermediate coating film have been formed, or one in which an undercoat coating film, intermediate coating film, and base coat coating film have been formed, or one in which an undercoat coating film, intermediate coating film, base coat coating film, and clear coat coating film have been formed.
[0083] The coating method is not particularly limited, but examples thereof include air spray coating, airless spray coating, rotary atomization coating, curtain coat coating, and the like, and a wet coating film can be formed by these methods. In these coating methods, electrostatic application may be performed as necessary. Among these, air spray coating, airless spray coating, and rotary atomization coating are particularly preferred.
[0084] The amount of coating is usually preferably set to an amount that results in a cured film thickness of about 10 to 100 μm.
[0085] The wet coating film formed by applying a coating material to a substrate is cured by heating. Heat curing can be performed by a known heating means, for example, a drying furnace such as a hot air oven, an electric oven, or an infrared induction heating oven can be used. The heating temperature is not particularly limited, but from the viewpoint of production efficiency and energy saving, it is preferable to heat at 50°C to 120°C, more preferably from 50°C to 100°C, and particularly preferably from 50°C to 80°C. The heating time is not particularly limited, but from the viewpoint of production efficiency and energy saving, it is suitable to be within the range of 10 to 60 minutes, preferably 15 to 30 minutes. In addition, the coating film after heat curing may be additionally cured at room temperature or cured by heat (after curing) as necessary. When after curing is performed, it is preferable to dry at room temperature for one day or more, or at 30 to 50°C for 30 minutes or more, but from the viewpoint of production efficiency and energy saving, it is preferable not to perform after curing.
[0086] The present coating film forming method can be suitably used when forming a top clear topcoat film. EXAMPLES
[0087] The present invention will be described in more detail below with reference to Production Examples, Examples, and Comparative Examples. However, the present invention is not limited thereto. In each example, "parts" and "%" are based on mass unless otherwise specified. Furthermore, the thickness of the coating film is based on the cured coating film.
[0088] Production Example 1 (Production of Alkoxysilyl Group-Containing Acrylic Polyol) In a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube and a dropping device, 30 parts of "Swasol 1000" (trade name, manufactured by Cosmo Oil Co., Ltd., aromatic organic solvent) and 10 parts of n-butanol were charged. The charged liquid was stirred at 125°C while blowing nitrogen gas into the reaction vessel, and a monomer mixture consisting of 30 parts of γ-methacryloxypropyltrimethoxysilane, 35 parts of 2-hydroxypropyl acrylate, 20 parts of styrene, 15 parts of isobutyl methacrylate and 3 parts of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator) was dropped into the reaction vessel at a uniform speed over 4 hours. Next, after aging for 30 minutes at 125°C, a solution consisting of 0.5 parts of 2,2'-azobis(2-methylbutyronitrile) and 5.0 parts of "Swasol 1000" was dropped at a uniform speed over 1 hour. The mixture was then aged at 125°C for 1 hour, cooled, and further diluted with isobutyl acetate to obtain an alkoxysilyl-containing acrylic polyol (A-1) solution with a solid content of 60% by mass. The alkoxysilyl-containing acrylic polyol (A-1) thus obtained had an alkoxysilyl group content of 1.2 mmol / g, a hydroxyl value of 151 mg KOH / g, a weight average molecular weight of 7,000, and a glass transition temperature of 16.6°C.
[0089] Production Example 2 (Production of acrylic polyol not containing alkoxysilyl groups) In a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube and a dropping device, 30 parts of "Swasol 1000" (trade name, manufactured by Cosmo Oil Co., Ltd., aromatic organic solvent) and 10 parts of n-butanol were charged. The charged liquid was stirred at 125°C while blowing nitrogen gas into the reaction vessel, and a monomer mixture consisting of 35 parts of 2-hydroxypropyl acrylate, 20 parts of styrene, 45 parts of isobutyl methacrylate and 3 parts of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator) was dropped into the reaction vessel at a uniform speed over 4 hours. After that, the mixture was aged for 30 minutes at 125°C, and then a solution consisting of 0.5 parts of 2,2'-azobis(2-methylbutyronitrile) and 5.0 parts of "Swasol 1000" was dropped at a uniform speed over 1 hour. The mixture was then aged at 125°C for 1 hour, cooled, and further diluted with isobutyl acetate to obtain an acrylic polyol (A-2) solution with a solid content of 60% by mass. The resulting hydroxyl-containing acrylic resin (A-2) had a hydroxyl value of 151 mgKOH / g, a weight average molecular weight of 7,000, and a glass transition temperature of 36.4°C.
[0090] Production Example 3 (Production of acrylic resin-coated colloidal silica) In a separable flask equipped with a reflux condenser, a thermometer and a stirrer, 333 parts (100 parts solids) of "PGM-ST" (trade name, manufactured by Nissan Chemical Industries, Ltd., average primary silica particle size: 15 nm, silica concentration: 30 mass%, dispersion medium: propylene glycol monomethyl ether) and 10 parts of deionized water were added, and 10 parts of "KBM-503" (trade name, manufactured by Shin-Etsu Chemical Co., Ltd., γ-methacryloyloxypropyltrimethoxysilane) were added, and a dehydration condensation reaction was carried out while stirring at 80 ° C. for 2 hours, after which 0.03 parts of tetra-n-butylammonium fluoride was added and the reaction was carried out while stirring for another 1 hour. After the reaction was completed, 30 parts of propylene glycol monomethyl ether was added, and then volatile components were distilled off under reduced pressure to obtain a polymerizable unsaturated group-containing colloidal silica dispersion with a solid content of 40% of surface-modified silica particles.
[0091] In a separable flask equipped with a reflux condenser, a thermometer, a stirrer and a nitrogen gas inlet, 104.5 parts of propylene glycol monomethyl ether and 8.5 parts of trimethyl orthoacetate were charged and heated to 100° C. under nitrogen gas aeration. After reaching 100° C., a monomer mixture consisting of 375 parts (150 parts of solid content) of the above polymerizable unsaturated group-containing colloidal silica dispersion, 1 part of “X-22-174ASX” (trade name, manufactured by Shin-Etsu Silicone Co., Ltd.), 30 parts of γ-methacryloxypropyltrimethoxysilane, 35 parts of 2-hydroxypropyl acrylate, 20 parts of styrene, 14 parts of isobutyl methacrylate, 3 parts of 2,2′-azobis(2-methylbutyronitrile) (polymerization initiator) and 23.5 parts of trimethyl orthoacetate was added dropwise over 2 hours. Then, after aging for 1 hour at 100°C, a mixed solution of 1 part of 2,2'-azobis(2-methylbutyronitrile) (polymerization initiator) and 19.5 parts of propylene glycol monomethyl ether was added and aged for another 2 hours. The polymerization rate calculated from the non-volatile content was 99%. Thereafter, propylene glycol monomethyl ether was added, and the solvent was replaced by azeotropic distillation under reduced pressure, to obtain an acrylic resin-coated colloidal silica dispersion (E-1) with a measured non-volatile content of 40%.
[0092] Production Example 4 The main agent was prepared by mixing 100 parts (60 parts solids) of the alkoxysilyl group-containing acrylic polyol (A-1) obtained in Production Example 1, 4.0 parts (1.0 parts solids) of "BYK-SILCLEAN3700" (product name, manufactured by BYK Japan, silicone (D) modified with a hydroxyl group-containing resin, active ingredient 25%), 25 parts (10 parts solids) of the acrylic resin-coated colloidal silica dispersion (E-1) obtained in Production Example 3, 5.0 parts of trimethyl orthoacetate (dehydrating agent), and 32 parts of butyl acetate (organic solvent) until uniform. In a separate container, 35.5 parts of "Sumidur N3300" (product name, manufactured by Sumika Covestro Urethane Co., Ltd., isocyanurate ring adduct of hexamethylene diisocyanate, solid content 100%) and 17.5 parts of diethylene glycol monoethyl ether acetate were blended and mixed until uniform to prepare a curing agent. 166 parts of the base agent, 53 parts of the curing agent, and 1.5 parts of "U-CAT SA102" (product name, manufactured by San-Apro Co., Ltd., curing catalyst, DBU-octylate salt, active ingredient 100%) were mixed, and butyl acetate was added so that the paint solids content was 40%, and the mixture was stirred to obtain a paint composition (X-1).
[0093] Manufacturing Examples 5-14 Coating compositions (X-2) to (X-11) were obtained in the same manner as in Production Example 4, except that the formulations shown in Table 1 were used.
[0094] [Table 1]
[0095] The notes in the table are as follows: "NANOBYK-3652": Product name, manufactured by BYK Japan, organic solvent-dispersed colloidal silica, solid content 31%, silica content 25% "NACURE 4167": Product name, KING INDUSTRIES, triethylamine salt of alkyl phosphate, curing catalyst, active ingredient 25%, "CAT-AC": Product name, manufactured by Shin-Etsu Silicone, aluminum chelate, curing catalyst, 50% active ingredient.
[0096] Example 1 The viscosity of the above-mentioned coating composition (X-1) was adjusted by adding butyl acetate to a viscosity of 25 seconds at 20° C. using a Ford cup No. 4. On a 0.8 mm thick dull steel plate that had been subjected to zinc phosphate conversion treatment, "ELECRON GT-10" (product name, thermosetting epoxy resin-based cationic electrodeposition paint, manufactured by Kansai Paint Co., Ltd.) was electrocoated to a thickness of 20 μm, heated to 170 ° C for 30 minutes to cure, and then a water-based base coat "WBC713T" (product name, acrylic-melamine resin-based automotive top coat base coat paint, white color, manufactured by Kansai Paint Co., Ltd.) was applied thereon to a dry thickness of 15 μm, left at room temperature for 5 minutes, preheated at 80 ° C for 10 minutes, and then heated and cured at 140 ° C for 30 minutes. Then, on the cured base coat coating, each of the coating compositions manufactured and viscosified in the above examples and comparative examples was applied to a thickness of 35 μm, left at room temperature for 10 minutes, and then heated at 80 ° C for 30 minutes to cure, thereby obtaining a coating film (Y-1).
[0097] Examples 2 to 15, Comparative Examples 1 to 5 The coating films (Y-2) to (Y-20) were obtained in the same manner as in Example 1, except that the coating materials and drying conditions shown in Tables 2 and 3 were used.
[0098] [Table 2]
[0099] [Table 3]
[0100] Measurement of storage modulus Each of the coating compositions shown in Tables 2 and 3 was applied onto a polypropylene plate so that the cured film thickness was 40 μm, and each cured coating film was formed by drying under the drying conditions shown in Tables 2 and 3. The cured coating film was cut into a strip of 20 mm in length and 5 mm in width, and peeled off from the polypropylene plate to obtain a strip-shaped free coating film, which was used as a sample.
[0101] The storage modulus was measured using an FT rheology spectrometer "Rheogel E-400" (manufactured by UBM Co., Ltd.). The free coating film prepared under the above conditions was subjected to dynamic viscoelasticity measurement under conditions of a frequency of 11 Hz, a heating rate of 4°C / min, and a temperature range of room temperature to 200°C, and the minimum storage modulus E' in the range of 40 to 200°C was obtained. min obtained.
[0102] Evaluation Test The coating films (Y-1) to (Y-20) thus produced were subjected to the following evaluation tests. The results are shown in Tables 2 and 3.
[0103] Removable (marker) Each test plate was stained by drawing a 10 mm x 10 mm square with an oil-based marker. Six types of oil-based markers were used for staining: "edding 850 permanent marker-red" (product name, Edding Co., Ltd., red marker), "edding 750 paint marker-black" (product name, Edding Co., Ltd., black marker), "Camlin Kokuyo Permanent Marker blue" (product name, Camlin Co., Ltd., blue marker), "Camlin Kokuyo Permanent Marker red" (product name, Camlin Co., Ltd., red marker), "Magic Ink Extra Thick Red" (product name, Teranishi Chemical Industry Co., Ltd., red marker), and "Magic Ink Extra Thick Black" (product name, Teranishi Chemical Industry Co., Ltd., black marker). After staining with each marker, the plate was left to stand for 5 minutes, and then "Strong Graffiti Remover Spray" (product name, Asahipen Co., Ltd., graffiti remover) was sprayed evenly, and the stained area was wiped off with a dry Kimwipe (product name). This process constituted one cycle, and the same process was repeated two more times on the same area contaminated in the first cycle. After completing the three cycles, the incubation time after contamination with the marker was increased to 24 hours, and one similar cycle was carried out. After carrying out the above-mentioned contamination / removal work (three 5-minute standing cycles and one 24-hour standing cycle), the contaminated / removed areas were observed and evaluated according to the following criteria. A and B are acceptable levels. A: No color residue, B: Slight color retention is observed. C: Significant color retention is observed or the coating is dissolved by the graffiti remover.
[0104] Removable (except for markers) A calcined Kanto loam product (JIS test powder 17 types) specified in JIS Z8910 and gear oil were mixed in a weight ratio of 1:1 to obtain a simulated contaminated liquid. Red can curry powder (manufactured by S&B Foods Co., Ltd.) and Nisshin canola oil (edible rapeseed oil, manufactured by Nisshin Oillio Group Ltd.) were mixed in a weight ratio of 1:1 to obtain a curry-contaminated liquid. Nescafe Gold Blend (regular soluble coffee powder, manufactured by Nestle Japan) and water were mixed in a weight ratio of 1:5 to obtain a coffee-contaminated solution.
[0105] Three pieces of cotton cut into 30mm squares were placed on the test plate, and 5ml of each staining liquid was dropped onto each piece of cotton, allowing the cotton to come into full contact with the coating surface of the test plate. The entire contact surface was then covered with a 60mm diameter polypropylene lid and secured in place with masking tape to prevent the staining liquid from evaporating. After leaving the surface to stand at 50°C for 24 hours, the cotton was removed and the test surface was thoroughly washed with tap water and new cotton. The staining resistance to the staining liquid was evaluated on a three-level scale based on the appearance of the coating surface after washing. A and B are pass levels. A: No color residue, B: Slight color retention is observed. C: Significant color retention is observed.
[0106] (Reference test) Repellency Each test plate was stained by drawing a 10 mm x 10 mm square with "edding 850 permanent marker-red" (product name, red marker, manufactured by Edding Co.), and the ink repellency was evaluated. A and B are pass levels. A: The painted surface repels ink and more than 50% of the painted surface is visible. B: The coating surface repels ink slightly, and 10-50% of the coating surface is visible. C: Ink is not repelled and the painted surface is almost invisible.
Claims
1. A coating film forming method comprising applying a multi-liquid thermosetting coating composition comprising a base component containing an acrylic polyol (A) and an organic solvent, and a curing agent component containing a polyisocyanate compound (B) and an organic solvent, and then heat-curing the composition, The minimum storage modulus E' of the coating film formed in the range of 40 to 200°C min is 2.6 x 10 7 The coating film forming method according to the present invention is a stain-resistant coating film having a viscosity of 100 Pa or more.
2. The method for forming a coating film according to claim 1 , wherein the acrylic polyol (A) contains an alkoxysilyl group.
3. The method for forming a coating film according to claim 1 , wherein the polyisocyanate compound (B) contains an isocyanurate trimer.
4. The coating film forming method according to claim 1, wherein the multi-liquid thermosetting coating composition further contains at least one catalyst compound (C) selected from the group consisting of amidine compounds, guanidine compounds, phosphazene compounds, imidazole compounds, phosphate compounds, and phosphite compounds.
5. 2. The method for forming a coating film according to claim 1, wherein the multi-liquid type thermosetting coating composition further contains a silicone (D) modified with a hydroxyl group-containing resin.
6. 2. The method for forming a coating film according to claim 1, wherein the multi-component thermosetting coating composition further contains an organic solvent-dispersed colloidal silica (E).
7. An article coated by the coating film forming method according to any one of claims 1 to 6.
Citation Information
Patent Citations
A coating agent with high scratch resistance and weather resistance.
JP2010513617A
Thermosetting coating agent, cured product, and film
JP2020007540A
Coating material composition and coating film formation method
JP2021091744A
Coating composition and method for forming multilayer coating film
WO2021131444A1