Method for producing nitrogen-containing carbon material in which pyridinic nitrogen is selectively introduced

By heating precursor compounds with pyridine rings under controlled conditions, the method addresses the challenge of producing nitrogen-containing carbon materials with precise structural control and minimal impurities, enabling scalable and efficient production.

JP2024162334AInactive Publication Date: 2024-11-21CHIBA UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023077731
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing nitrogen-containing carbon materials face challenges in precisely controlling their structure, often requiring difficult-to-handle raw materials and harsh conditions, leading to impurities and limited scalability, especially when using metal substrates.

Method used

A method involving the heating of precursor compounds with pyridine rings and aromatic rings under controlled conditions, such as specific temperatures and atmospheres, to introduce nitrogen atoms into the edges of carbon materials, using easily manageable raw materials and avoiding catalytic reactions to produce a nitrogen-containing carbon material with precise structural control.

Benefits of technology

This approach allows for the easy production of nitrogen-containing carbon materials with high pyridinic nitrogen content at the edges, achieving precise structural control and minimal impurities, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162334000001_ABST
    Figure 2024162334000001_ABST
Patent Text Reader

Abstract

To provide a method for simply producing a nitrogen-containing carbon material in which the structure is precisely controlled by introducing nitrogen atoms at an edge, using an easy-to-handle material under mild conditions.SOLUTION: A method for producing a nitrogen-containing carbon material according to an embodiment of the present invention comprises a heating step (I) for heating a precursor compound (A). The precursor compound (A) has a pyridine ring (a) and an aromatic ring (b). The aromatic ring (b) is bonded to the pyridine ring (a) by a single bond. The aromatic ring (b) is at least one selected from the group consisting of a benzene ring and a pyridine ring.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a nitrogen-containing carbon material into which pyridinic nitrogen has been selectively introduced. [Background technology]

[0002] In recent years, carbon materials such as carbon nanotubes, fullerenes, graphite, graphene, graphene oxide, reduced graphene oxide, artificial graphite, and carbon black have been expected to become novel functional materials in various fields due to their characteristic physical properties (e.g., Non-Patent Documents 1 to 6).

[0003] Graphene is a two-dimensional carbon sheet with a structure of six-membered rings of sp2 carbon. Graphite usually refers to a multi-layer structure in which two-dimensional graphene sheets are bonded together by van der Waals forces, but a single layer is called graphene. A material with two to five layers of graphene is called few-layer graphene, and a material with three or more layers of graphene is called multi-layer graphene. In single-layer graphene, the properties and shape of the graphene itself change significantly when functional groups are introduced to the basal plane. In three or more layers, the graphene in the center is less likely to be directly affected by introducing functional groups to the basal plane of graphene. Therefore, in graphene with three or more layers, the number of layers basically increases, and no significant differences in properties are likely to appear other than a decrease in the specific surface area.

[0004] Although the existence of graphene has been known for a long time, a method for extracting a single sheet of graphene from graphite had not been established until recently. In 2004, it was discovered that thin graphene flakes could be extracted by peeling the surface of highly oriented anhydrous graphite with adhesive tape and attaching the peeled piece to a substrate. Since then, with the aim of mass production and low-cost production, methods for producing graphene using gas-phase film formation methods such as CVD (chemical vapor deposition) and methods for producing graphene by reducing graphene oxide (GO) (reduced graphene oxide: RGO) have been investigated.

[0005] However, graphene manufacturing methods using gas phase film formation methods such as CVD (chemical vapor deposition) have problems such as the inability to obtain graphene in any form other than a film (typically, in bulk), the need to use flammable gases, the problem of metal impurities being contained because the film is formed on a metal substrate with catalytic properties such as Cu, and the fact that only the metal surface is produced, making mass production impossible.

[0006] In addition, a method for producing a carbon material by heating a compound that undergoes a condensation reaction between the same molecules and / or different molecules has been disclosed (Patent Document 1). It has been shown that this technology can synthesize a carbon material under mild conditions.

[0007] Industrially produced carbon materials have various functional groups. Therefore, it is difficult to precisely control the structure of the carbon material, and there is a problem that the physical properties vary. In recent years, there is a demand for carbon materials that can reliably exhibit targeted physical properties, and therefore there is a demand for the development of carbon materials with precisely controlled structures.

[0008] Among such carbon materials with precisely controlled structures, if a carbon material with precisely controlled structures can be obtained by introducing atoms other than carbon into the edges, it is expected to be applicable to various uses. In particular, nitrogen-containing carbon materials with precisely controlled structures by introducing nitrogen atoms into the edges may have a wide range of applications.

[0009] In recent years, various carbon materials such as graphene (Non-Patent Document 7), graphene nanoribbons (Non-Patent Documents 8-10), and graphene oxide (Non-Patent Document 11) with nitrogen atoms, i.e., pyridinic nitrogen, introduced to the edge have been reported (Non-Patent Documents 12-15). As for the highly controlled structure of pyridinic nitrogen, it is considered that the control is about 89% for graphene (Non-Patent Document 7), about 75% for graphene nanoribbons (Non-Patent Document 8), and about 80% for graphene oxide (Non-Patent Document 11). However, graphene is prepared at a low temperature of 600°C or less, and copper, which exhibits catalytic action, is used as the metal substrate (Non-Patent Document 7). For this reason, as described above, there are problems that metals are contained as impurities, and that mass production is not possible because only the metal surface is produced. In two of the above three reports on graphene nanoribbons (Non-Patent Documents 8 and 9), a metal substrate is not used. However, in the technology described in Non-Patent Document 8, a brominated raw material having a structure in which two pyridinic nitrogens are introduced at the ortho position is used, and there is a problem that the raw material is not easy to handle. In addition, in Non-Patent Document 9, a graphene nanoribbon in which pyridinic nitrogen is introduced at the para position is reported, but the analysis has not been sufficiently performed, and it has not been examined whether the structure is precisely controlled. Furthermore, the graphene oxide described in Non-Patent Document 11 is not heat-treated, and is considered to have low durability. In addition, in the carbon materials described in Non-Patent Documents 12, 13, 14, and 15, the structural control state of pyridinic nitrogen is not high (45% in the carbon material described in Non-Patent Document 12, 60% to 70% in the carbon material described in Non-Patent Document 13, 70% in the carbon material described in Non-Patent Document 14, and 73% in the carbon material described in Non-Patent Document 15). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2019-085298 A [Non-patent literature]

[0011] [Non-Patent Document 1] Nature, 354, p.56-58 (1991) [Non-Patent Document 2] Science, 306, p.666-669 (2004) [Non-Patent Document 3] H.Nishihara et.al., Adv.Funct.Mater., 26, 6418-6427(2016) [Non-Patent Document 4] Riichiro Saito, "Graphene's cutting-edge technology and expanding applications", Chapter 2. Fundamental properties of graphene, 3. Optoelectronic properties of graphene [Non-Patent Document 5] Dawei Pan et.al., Langmuir, 22, 5872-5876(2006) [Non-Patent Document 6] V. Ruiz et.al., Electrochem. Commun., 24, 35-38(2012) [Non-Patent Document 7] S. Yasuda et.al.,Chem.Commun.,49,9627-9629(2013) [Non-Patent Document 8] THVo et.al.,Chem.Commun.,49,4172-4174(2014) [Non-Patent Document 9] KTKim et.al.,Macromol.Chem.Phys.,214,2768-2773(2013) [Non-Patent Document 10] Y.Zhang et.al.,Appl.Phys.Lett.,105,023101(2014) [Non-Patent Document 11] G.Bang et.al.,ACS Omega,3,5522-5530(2018) [Non-Patent Document 12] W.Ding et.al.,Angew.Chem.Int.Ed.,52,11755-11759(2013) [Non-Patent Document 13] MASHaniff et.al.,ACS Appl.Mater.Interfaces,9,15192-15201(2017) [Non-Patent Document 14] Y.Chen et.al.,Nanoscale Res,Lett.,9,646(2014) [Non-Patent Document 15] T.Khai et.al.,Carbon,50,3799-3806(2012) [Non-Patent Document 16] Y.Yamada et.al.,Carbon,198,411-434(2022) Summary of the Invention [Problem to be solved by the invention]

[0012] An object of the present invention is to provide a method for simply producing a nitrogen-containing carbon material having a precisely controlled structure by introducing nitrogen atoms into the edges, using easily handled raw materials under mild conditions. [Means for solving the problem]

[0013] A method for producing a nitrogen-containing carbonaceous material according to an embodiment of the present invention includes the steps of: A heating step (I) of heating the precursor compound (A), The precursor compound (A) is A pyridine ring (a), and at least one aromatic ring (b) selected from the group consisting of a benzene ring and a pyridine ring, bonded to the pyridine ring (a) via a single bond.

[0014] In one embodiment, the aromatic ring (b) is a pyridine ring.

[0015] In one embodiment, the precursor compound (A) is a polypyridine.

[0016] In one embodiment, the precursor compound (A) contains a halogen element.

[0017] In one embodiment, the precursor compound (A) is at least one selected from the group consisting of the compounds (1) to (4).

[0018] [ka]

[0019] Here, R1 to R4 are each hydrogen or bromine, and n is an integer of 2 to 500.

[0020] In one embodiment, the heating temperature of the precursor compound (A) in the heating step (I) is 300°C to 1000°C. Effect of the Invention

[0021] According to the present invention, it is possible to provide a method for simply producing a nitrogen-containing carbon material having a precisely controlled structure by introducing nitrogen atoms into the edges, using easy-to-handle raw materials under mild conditions. [Brief description of the drawings]

[0022] [Figure 1] FIG. 2 is an XPS spectrum diagram in N1s X-ray photoelectron spectroscopy (XPS) of the nitrogen-containing carbon materials (1a), (1b), and (1c) obtained in Example 1, and P25pyr (raw material). [Diagram 2] FIG. 1 shows Raman spectra actually measured in a Raman spectroscopic analysis of the nitrogen-containing carbon materials (1a) and (1b) obtained in Example 1, and Raman spectra calculated for structures related to the nitrogen-containing carbon materials (1a) and (1b). [Diagram 3] FIG. 2 shows XPS spectrum diagrams of N1sXPS analysis of the nitrogen-containing carbon materials (2a), (2b), and (2c) obtained in Example 2, and P35pyr (raw material). [Figure 4]FIG. 1 shows Raman spectra of the nitrogen-containing carbon materials (2a) and (2b) obtained in Example 2 by Raman spectroscopy, and Raman spectra calculated for structures related to the nitrogen-containing carbon materials (2a) and (2b). [Diagram 5] FIG. 2 is an XPS spectrum diagram of the N1sXPS analysis of the nitrogen-containing carbon materials (3a) and (3b) obtained in Example 3. [Figure 6] FIG. 1 shows Raman spectra of the nitrogen-containing carbon materials (3a) and (3b) obtained in Example 3 by Raman spectroscopy, and Raman spectra calculated for structures related to the nitrogen-containing carbon materials (3a) and (3b). [Figure 7] FIG. 1 is an XPS spectrum diagram of the N1sXPS analysis of the nitrogen-containing carbon materials (4a) and (4b) obtained in Example 4. [Figure 8] FIG. 1 shows Raman spectra of the nitrogen-containing carbon materials (4a) and (4b) obtained in Example 4 by Raman spectroscopy, and Raman spectra calculated for structures related to the nitrogen-containing carbon materials (4a) and (4b). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] <<1. Method for producing nitrogen-containing carbon material>> A method for producing a nitrogen-containing carbon material according to an embodiment of the present invention includes a heating step (I) of heating a precursor compound (A). The precursor compound (A) has a pyridine ring (a) and an aromatic ring (b). The aromatic ring (b) is bonded to the pyridine ring (a) by a single bond. In addition, the aromatic ring (b) is at least one selected from the group consisting of a benzene ring and a pyridine ring.

[0024] The precursor compound (A) may be of only one type, or of two or more types.

[0025] The precursor compound (A) may have a halogen element. The halogen element may be directly bonded to the carbon atom constituting the pyridine ring (a) and / or the carbon atom constituting the aromatic ring (b). Examples of the halogen element are fluorine, chlorine, bromine, and iodine. The precursor compound (A) may contain at least one halogen element selected from the group consisting of fluorine, chlorine, bromine, and iodine. The precursor compound (A) preferably contains bromine as the halogen element.

[0026] The pyridine ring (a) and the aromatic ring (b) may have any suitable substituent at any suitable position within a range that does not impair the effects of the present invention. Examples of such substituents include alkyl groups; aryl groups; and substituents having a leaving ability such as tosylate, triflate, and halogen groups. Since the absence of substituents that can become impurities in the carbon material after heating has no adverse effect on the physical properties, etc., a hydrogen group (without a substituent) or a substituent having a leaving ability is preferred. The substituent having a leaving ability is preferably a halogen group, more preferably bromine.

[0027] As described above, the aromatic ring (b) is at least one selected from the group consisting of a benzene ring and a pyridine ring. The aromatic ring (b) is preferably a pyridine ring. When the aromatic ring (b) is a pyridine ring, carbonization proceeds more easily, and the nitrogen-containing carbon material can be easily produced under milder conditions. In addition, when the aromatic ring (b) is a pyridine ring, the amount of pyridinic nitrogen in the obtained carbon material increases, which is preferable.

[0028] The molecular weight of the precursor compound (A) is, for example, 40,000 or less, preferably 50 to 7,000, more preferably 100 to 600, further preferably 150 to 500, and particularly preferably 200 to 400. When the molecular weight of the precursor compound (A) is within the above range, it can be an easy-to-handle raw material.

[0029] The precursor compound (A) may be polypyridine. In this specification, "polypyridine" means a compound in which two or more pyridine rings are bonded by single bonds. The number of pyridine rings contained in the polypyridine is, for example, 500 or less. The polypyridine may have any suitable substituent at any suitable position within a range that does not impair the effects of the present invention. Examples of the substituent are as described above. When the precursor compound (A) is polypyridine, carbonization proceeds more easily, and therefore the nitrogen-containing carbon material can be easily produced under milder conditions.

[0030] Examples of the precursor compound (A) include the following compounds (1) to (4). However, precursor compounds other than the compounds (1) to (4) may also be used as the precursor compound (A) within the scope of the present invention, so long as the effects of the present invention are not impaired.

[0031] [ka]

[0032] In compounds (1) and (2), R1 to R4 are each hydrogen or bromine. n is an integer of 2 to 500. n is preferably an integer of 2 to 100, more preferably an integer of 2 to 50, further preferably an integer of 2 to 10, and particularly preferably an integer of 2 to 5.

[0033] The method for producing a nitrogen-containing carbon material according to an embodiment of the present invention includes a heating step (I) of heating a precursor compound (A). The "heating" in the heating step (I) may be referred to as "calcination".

[0034] In the heating step (I), the precursor compound (A) may be heated. That is, since the precursor compound (A) is heated in the heating step (I), the heating step (I) may be an embodiment in which the "composition containing the precursor compound (A)" is heated.

[0035] In the case where the heating step (I) is an embodiment in which the "composition containing precursor compound (A)" is heated, the content of precursor compound (A) in the "composition containing precursor compound (A)" is preferably 50% by weight to 100% by weight, more preferably 80% by weight to 100% by weight, even more preferably 90% by weight to 100% by weight, particularly preferably 95% by weight to 100% by weight, and most preferably substantially 100% by weight, in order to further exhibit the effects of the present invention. The term "substantially" used here refers to a form in which another component for exhibiting effects other than the effects attributable to precursor compound (A) is actively used in combination with precursor compound (A). For example, impurities that are inevitably mixed in during the manufacturing process or the like are permitted to be contained within a range that does not impair the effects of the present invention.

[0036] The heating temperature in the heating step (I) is preferably 300° C. to 1000° C., more preferably 350° C. to 900° C., further preferably 400° C. to 800° C., and particularly preferably 450° C. to 700° C. By controlling the heating temperature in the heating step (I) within the above range, a nitrogen-containing carbon material having a precisely controlled structure due to nitrogen atoms introduced into the edges can be easily produced under mild conditions.

[0037] The heating time in the heating step (I) is preferably 1 minute to 120 hours, more preferably 10 minutes to 96 hours, further preferably 30 minutes to 72 hours, and particularly preferably 1 hour to 24 hours. By controlling the heating time in the heating step (I) within the above range, a nitrogen-containing carbon material having a precisely controlled structure due to nitrogen atoms introduced into the edges can be easily produced under mild conditions.

[0038] As a method for heating in the heating step (I), a calcination furnace such as a tubular furnace or a box furnace, a heating reaction device using a heat medium, a heating reaction device using microwaves, or the like can be used.

[0039] The pressure conditions for heating in the heating step (I) may be under vacuum, normal pressure, or increased pressure.

[0040] The heating atmosphere in the heating step (I) may be air or an inert gas atmosphere, etc. Examples of the inert gas atmosphere include nitrogen and argon.

[0041] In the heating step (I), the precursor compound (A) is preferably molded in a bulk state or dissolved in a solvent or the like and heated. Heating the precursor compound (A) in a bulk state includes, for example, (i) heating particles (e.g., powder) made of the precursor compound (A), and (ii) molding the particles (e.g., powder) made of the precursor compound (A) into a pellet, film, or fiber shape by compression molding or the like, and then heating the molded body. In addition, dissolving in a solvent or the like and molding means dissolving the precursor compound (A) in a solvent, molding it into a film or fiber shape, drying it, and heating the molded body. When dissolving the precursor compound (A) in a solvent, a method of mixing the powder, coating the precursor compound (A) on the powder, and then heating the molded body can also be mentioned.

[0042] When the precursor compound (A) is heated in the heating step (I), it may be heated in a container, for example. Any suitable container may be used as the container. For example, such a container is preferably made of a material that is not substantially altered by the heating temperature in the heating step (I). In addition, it is preferable that the surface that comes into contact with the precursor compound (A) is made of a material that does not chemically react with the precursor compound (A) when heated. By performing the heating step (I) of heating the precursor compound (A) under preferred conditions, it is possible to obtain a nitrogen-containing carbon material, and in the heating step (I), the precursor compound (A) may melt and become liquid near the melting point of the precursor compound (A). Such a process is also included in "calcining the precursor compound (A) in a bulk state".

[0043] For example, a thin film is formed by the heating step (I). Methods for forming a thin film include chemical vapor deposition (CVD), physical vapor deposition (PVD), thin film deposition heating, etc. A thin film generally means a film thickness in the range of 1 μm or less.

[0044] In the heating step (I), the precursor compound (A) is heated in contact with a metal. Alternatively, the precursor compound (A) may be heated without contacting the metal. When the precursor compound (A) is heated without contacting the metal, the inclusion of the metal as an impurity in the resulting nitrogen-containing carbon material can be suppressed. However, as described above, not contacting the precursor compound (A) means not actively contacting the precursor compound (A) with the metal. Active contacting the precursor compound (A) with the metal means an operation of actively increasing the contact area with the metal, for example, a method of dissolving the precursor compound (A) in a solvent, applying the precursor compound (A) to the metal, forming a film, and heating the precursor compound (A) with the metal to form a thin film.

[0045] In the heating step (I), the precursor compound (A) is preferably heated without using a catalytic reaction. By heating the precursor compound (A) without using a catalytic reaction, it is possible to prevent the reaction catalyst from being present in the nitrogen-containing carbon material and becoming a fatal impurity.

[0046] By heating the precursor compound (A) in the heating step (I), a condensation reaction of the precursor compound (A) occurs to produce a nitrogen-containing carbon material. When there is one type of precursor compound (A), the condensation reaction may be between molecules of the same type. When there are two or more types of precursor compounds (A), the condensation reaction may occur both between molecules of the same type and between molecules of different types.

[0047] As described above, the precursor compound (A) has a structure in which the pyridine ring (a) and the aromatic ring (b) are bonded by a single bond. This allows the precursor compound (A) to have, for example, multiple C-H bonds and / or multiple C-X bonds in one molecule. Here, C in the C-H bond and C-X bond represents a carbon atom constituting the pyridine ring (a) and / or the aromatic ring (b). X represents a halogen element. The precursor compound (A) has multiple C-H bonds and / or multiple C-X bonds in one molecule, which allows carbonization to proceed more easily. As a result, the nitrogen-containing carbon material can be easily produced under milder conditions.

[0048] In the precursor compound (A), it is preferable that a C-H bond and / or a C-X bond is formed on the carbon atom adjacent to the nitrogen atom constituting the pyridine ring. This makes it easier for carbonization to proceed. As a result, the nitrogen-containing carbon material can be easily produced under milder conditions.

[0049] ≪≪2. Nitrogen-containing carbon material≫≫ The nitrogen-containing carbon material obtained by the manufacturing method according to the embodiment of the present invention is a nitrogen-containing carbon material whose structure is precisely controlled by introducing nitrogen atoms into the edges. Such nitrogen atoms present at the edges are called pyridinic nitrogen atoms.

[0050] Here, "edge" means the "edge" that is normally used in the field of carbon materials, and in a layer structure of one or more layers such as graphite, the flat side is called the "basal plane", and the plane substantially perpendicular to the basal plane (the plane where the cross section of the layer appears) is called the "edge plane" or "edge". In other words, in a carbon material having a hollow structure (a structure in which part of the basal plane is punched out) when viewed from the flat side of the basal plane, for example, the cross section exposed in the hollow part is also called an "edge".

[0051] The nitrogen-containing carbon material obtained by the production method according to the embodiment of the present invention is a nitrogen-containing carbon material obtained by a unique production method, and therefore can be a novel carbon material different from conventionally known carbon materials, such as carbon nanotubes, fullerenes, graphite films, graphene, graphene oxide, reduced graphene oxide, artificial graphite, and carbon black.

[0052] The nitrogen-containing carbonaceous material obtained by the manufacturing method according to the embodiment of the present invention is characterized in that, in N1sXPS analysis, all nitrogen atoms (tertiary nitrogen atoms, pyridinium atoms present at the edge) in the nitrogen-containing carbonaceous material are The ratio of the peak of the pyridinic nitrogen atom to the peak of all nitrogen atoms (the sum of the peaks of pyridinic nitrogen atoms and other nitrogen atoms) is 30% or more, preferably 35% or more, more preferably 40% or more, even more preferably 50% or more, particularly preferably 60% or more, and most preferably 70% or more. The upper limit of the above ratio is preferably 100% or less. In a nitrogen-containing carbon material, if the ratio of the peak of the pyridinic nitrogen atom to the peak of all nitrogen atoms by N1sXPS analysis is within the above range, the structure of the edge nitrogen atoms is precisely controlled in the nitrogen-containing carbon material, and the nitrogen-containing carbon material can have various physical properties and can be widely applied to various uses.

[0053] As described above, the nitrogen-containing carbon material obtained by the production method according to the embodiment of the present invention is found by N1sXPS analysis to have a high proportion of pyridinic nitrogen atoms.

[0054] When the precursor compound (A) contains a benzene ring as the aromatic ring (b), the nitrogen-containing carbon material obtained by the production method according to the embodiment of the present invention preferably has a honeycomb structure (graphene structure) derived from the benzene ring in its structure. The presence or absence of the graphene structure can be confirmed by Raman spectroscopy (Non-Patent Document 4).

[0055] The nitrogen-containing carbon material preferably has a total content of metal components as impurities of 0.1 atomic % or less, more preferably 0.01 atomic % or less, and particularly preferably substantially zero, based on 100 atomic % of carbon atoms. These can be confirmed by analyzing the nitrogen-containing carbon material using elemental analysis by a combustion method, XPS, inductively coupled plasma (ICP) optical emission spectrometry, X-ray fluorescence elemental analysis (XRF), or the like.

[0056] The nitrogen-containing carbonaceous material essentially contains carbon and nitrogen as its constituent elements, and may contain elements other than carbon and nitrogen. The elements other than carbon and nitrogen are preferably at least one element selected from oxygen, hydrogen, sulfur, fluorine, chlorine, bromine, and iodine, more preferably at least one element selected from oxygen, hydrogen, fluorine, chlorine, bromine, iodine, and sulfur, and even more preferably at least one element selected from oxygen, hydrogen, and bromine. When the total amount of elements other than hydrogen among the elements constituting the nitrogen-containing carbonaceous material is taken as 100 atomic %, the sum of carbon and nitrogen is preferably 60 atomic % or more, more preferably 70 atomic % or more, and even more preferably 75 atomic % or more. In addition, the elements other than carbon, nitrogen, and hydrogen are preferably 10 atomic % or less. When the ratio of each element falls within this range, it becomes possible to express a high structural control rate even though it is a nitrogen-containing carbonaceous material. These can be confirmed by quantifying the nitrogen-containing carbonaceous material by XPS.

[0057] The nitrogen-containing carbon material preferably has at least one aspect selected from the group consisting of the following (i) to (iv) as determined by Raman spectroscopic analysis:

[0058] The nitrogen-containing carbon material is preferably a material that exhibits a G band (generally 1550 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~1650cm -1 Therefore, the nitrogen-containing carbon material shows a peak in the G band (generally 1550 cm ) in the Raman spectrum obtained by Raman spectroscopy. -1 ~1650cm -1The presence of a peak at 1490 cm means that the nitrogen-containing carbon material has a graphene structure or a structure similar to the graphene structure. The higher the intensity and the sharper the G band, the cleaner the graphene structure or the structure similar to the graphene structure. -1 ~1575cm -1 In the range of 1490 cm, the peak due to the C-N bond appears, so the inclusion of pyridinic nitrogen causes the peak due to the C-N bond to appear in this range. In other words, the G band is at 1490 cm -1 ~1575cm -1 The extension to the range of 100 nm indicates the presence of a C-N bond.

[0059] The nitrogen-containing carbon material is preferably a material that exhibits a D band (generally around 1300 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~1400cm -1 Nitrogen-containing carbon materials having a structure derived from defects in the graphene structure show a peak in the D band (generally in the range of 1300 cm ) in the Raman spectrum obtained by Raman spectroscopy. -1 ~1400cm -1 Therefore, the nitrogen-containing carbon material exhibits a peak in the D band (generally in the range of 1300 cm ) in the Raman spectrum obtained by Raman spectroscopy. -1 ~1400cm -1 The presence of a peak in the range of 0.1 to 1.0 mm indicates that the nitrogen-containing carbon material contains a functional group or has a structure derived from defects in the graphene structure or a structure similar to a structure derived from defects in the graphene structure. The lower the intensity of the D band, the cleaner the graphene structure or the similar structure to the graphene structure.

[0060] The nitrogen-containing carbon material is preferably a material that exhibits a G band (generally 1550 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~1650cm -1(ii) a peak in the D band (generally in the range of 1300 cm ) in a Raman spectrum obtained by Raman spectroscopy; -1 ~1400cm -1 The peak is within the range of .

[0061] The nitrogen-containing carbon material is preferably a material that exhibits a G′ band (generally at 2650 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~2750cm -1 Therefore, the nitrogen-containing carbon material shows a peak in the G′ band (generally in the range of 2650 cm ) in the Raman spectrum obtained by Raman spectroscopy. -1 ~2750cm -1 The presence of a peak in the G′ band (range) means that the nitrogen-containing carbon material has a graphene structure or a structure similar to the graphene structure. The intensity of the G′ band is strongest when the graphene structure is one layer, and gradually decreases as the number of stacked graphene structures increases. However, even if the intensity of the G′ band gradually decreases as the number of stacked graphene structures increases, the peak can still be observed. Therefore, the presence of a peak in the G′ band means that the nitrogen-containing carbon material has a graphene structure or a structure similar to the graphene structure. The G′ band is sometimes called the 2D band.

[0062] The nitrogen-containing carbon material is preferably a material that exhibits a G band (generally 1550 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~1650cm -1 (ii) a peak in the D band (generally in the range of 1300 cm ) in a Raman spectrum obtained by Raman spectroscopy; -1 ~1400cm -1 (iii) a peak in the G′ band (generally 2650 cm ) in the Raman spectrum obtained by Raman spectroscopy; -1 ~2750cm -1 The peak is within the range of .

[0063] The nitrogen-containing carbon material is preferably a material that exhibits a D+D′ band (generally around 2800 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~3000cm -1 Nitrogen-containing carbon materials that have a structure derived from defects in the graphene structure show a peak in the D+D′ band (generally in the range of 2800 cm ) in the Raman spectrum obtained by Raman spectroscopy. -1 ~3000cm -1 Therefore, nitrogen-containing carbon materials show a peak in the D+D′ band (generally in the range of 2800 cm ) in the Raman spectrum obtained by Raman spectroscopy. -1 ~3000cm -1 The presence of a peak within the range of 1000 nm indicates that the nitrogen-containing carbon material contains a functional group or has a structure derived from defects in the graphene structure or a structure similar to a structure derived from defects in the graphene structure. If the D+D′ band has a low intensity, it can be said to have a cleaner graphene structure or a structure similar to a graphene structure. The D+D′ band is sometimes called the D+G band.

[0064] The nitrogen-containing carbon material is preferably a material that exhibits a G band (generally 1550 cm ) in a Raman spectrum obtained by Raman spectroscopy. -1 ~1650cm -1 (ii) a peak in the D band in the Raman spectrum obtained by Raman spectroscopy; (generally 1300cm -1 ~1400cm -1 (iii) a peak in the G′ band (generally 2650 cm ) in the Raman spectrum obtained by Raman spectroscopy; -1 ~2750cm -1 (iv) a peak in the D+D′ band (generally in the range of 2800 cm ) in the Raman spectrum obtained by Raman spectroscopy; -1 ~3000cm -1 The peak is within the range of .

[0065] According to elemental analysis, the nitrogen atom content ratio of the nitrogen-containing carbon material is preferably 0.5 atom% to 20 atom%, more preferably 0.7 atom% to 15 atom%, still more preferably 1 atom% to 13 atom%, and particularly preferably 1.5 atom% to 12 atom%.

Examples

[0066] Hereinafter, the present invention will be specifically described with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". In this specification, "mass" may be read as "weight". However, the % in the part related to N1s XPS in this specification means atom%.

[0067] The compounds used in the examples and their abbreviations are as follows. Poly(2,5-pyridine): P25pyr Poly(3,5-pyridine): P35pyr 5-Bromo-2-(4-bromophenyl)pyridine: Brphenpyr 5,5'-Dibromo-2,2'-bipyridine: Brbipyr

[0068] <N1s XPS Analysis> The N1s XPS measurement was carried out using JPS9030 of JEOL under the following conditions. Source: MgKα Measurement range: N1s: 394 eV to 406 eV Number of integrations: 40 times Analysis conditions: The peak of N1s was taken as pyridinic nitrogen (397.0 to 398.4 eV), tertiary nitrogen (tertiary nitrogen surrounded by two benzene rings is T2, and tertiary nitrogen surrounded by three benzene rings is T3) (399.8 to 401.1 eV), and others (398.7 to 399.7 eV), and peak separation was performed based on the peak position of the raw material, calculation results, and past reports (Non-Patent Document 16).

[0069] <Raman Spectroscopic Analysis> The Raman spectroscopic analysis was carried out using the following apparatus and conditions. Measurement equipment: Raman microscope (JASCO NRS-4500) Measurement conditions: 532.23 nm laser used

[0070] Example 1 Poly(2,5-pyridine) (P25pyr) (corresponding to compound (1) described in the specification) (manufactured by Sigma-Aldrich): 40 mg was vacuum sealed in an ampoule (P25pyr was placed in a glass tube and heated to 423 K (150° C.) at a heating rate of 5 K / min, then evacuated at 423 K for 1 hour and sealed with a gas burner), and then heated to a predetermined temperature at a heating rate of 10 K / min in an electric furnace and heated at the predetermined temperature for 1 hour. The specified temperatures were 873K (600°C), 773K (500°C), and 673K ​​(400°C). After heating, the samples were scraped out of each ampoule with a spatula and transferred to separate glass tubes. The tubes were then heated to 573 K (300 °C) at a heating rate of 5 K / min and evacuated at 573 K (300 °C) for 1 hour to obtain nitrogen-containing carbon materials (1a), (1b), and (1c). Nitrogen-containing carbon materials (1a), (1b), and (1c) are the nitrogen-containing carbon materials at the predetermined temperatures of 873 K (600°C), 773 K (500°C), and 673 K (400°C), respectively. The obtained nitrogen-containing carbon materials (1a), (1b), and (1c) were subjected to N1sXPS analysis and Raman spectroscopic analysis. The XPS spectrum of the N1sXPS analysis is shown in Figure 1. In Figure 1, the XPS spectrum of "P25pyr" shows the XPS spectrum of the raw material P25pyr. The Raman spectrum obtained by Raman spectroscopy is shown in FIG. As shown in Figure 1, in the obtained nitrogen-containing carbon material, the ratios of the peak of pyridinic nitrogen atoms to the peak of all nitrogen atoms in the nitrogen-containing carbon material (the sum of tertiary nitrogen atoms and pyridinic nitrogen atoms present on the edges) in the N1sXPS analysis were 81.5%, 100%, and 100%, respectively, regardless of whether the predetermined temperature was 873 K (600°C), 773 K (500°C), or 673 K (400°C), indicating that a nitrogen-containing carbon material in which nitrogen atoms are introduced to the edges and whose structure is precisely controlled can be easily produced under mild conditions. According to the Raman spectrum in FIG. 2, the obtained nitrogen-containing carbon material had peaks in the G band and the D band at both the predetermined temperatures of 873 K (600° C.) and 773 K (500° C.), which indicates that a nitrogen-containing carbon material having a graphene structure and a structure in which the graphene structures are stacked can be easily produced under mild conditions.

[0071] Example 2 Poly(3,5-pyridine) (P35pyr) (corresponding to compound (2) described in the specification) (manufactured by Sigma-Aldrich): 40 mg was vacuum sealed in an ampoule (P35pyr was placed in a glass tube and heated to 423 K (150° C.) at a heating rate of 5 K / min, then evacuated at 423 K for 1 hour and sealed with a gas burner), and then heated to a predetermined temperature at a heating rate of 10 K / min in an electric furnace and heated at the predetermined temperature for 1 hour. The specified temperatures were 873K (600°C), 773K (500°C), and 673K ​​(400°C). After heating, the samples were scraped out of each ampule with a spatula and transferred to separate glass tubes, then heated to 573 K (300 ° C) at a heating rate of 5 K / min, and evacuated at 573 K (300 ° C) for 1 hour to obtain nitrogen-containing carbon materials (2a), (2b), and (2c). Nitrogen-containing carbon materials (2a), (2b), and (2c) indicate the nitrogen-containing carbon materials at the predetermined temperatures of 873 K (600 ° C), 773 K (500 ° C), and 673 K (400 ° C), respectively. The obtained nitrogen-containing carbon materials (2a), (2b), and (2c) were subjected to N1s XPS analysis and Raman spectroscopy analysis. The XPS spectrum of the N1sXPS analysis is shown in Figure 3. In Figure 3, the XPS spectrum of "P35pyr" shows the XPS spectrum of the raw material P35pyr. The Raman spectrum of the Raman spectroscopy is shown in Figure 4. In Figure 4, the Raman spectrum of "P35pyr" shows the Raman spectrum of the raw material P35pyr. As shown in Figure 3, in the obtained nitrogen-containing carbon material, the ratios of the peak of pyridinic nitrogen atoms to the peak of all nitrogen atoms in the nitrogen-containing carbon material (the sum of tertiary nitrogen atoms, pyridinic nitrogen atoms present on the edges, and other nitrogen atoms) in the N1sXPS analysis were 73.9%, 84.9%, and 85.7%, respectively, regardless of whether the predetermined temperature was 873 K (600°C), 773 K (500°C), or 673 K (400°C), indicating that a nitrogen-containing carbon material in which nitrogen atoms are introduced to the edges and whose structure is precisely controlled can be easily produced under mild conditions. According to the Raman spectrum in FIG. 4, the obtained nitrogen-containing carbon material had peaks in the G band and the D band at both the predetermined temperatures of 873 K (600° C.) and 773 K (500° C.). This shows that the nitrogen-containing carbon material having a graphene structure and a structure in which the graphene structures are stacked can be easily produced under mild conditions.

[0072] Example 3 40 mg of 5-bromo-2-(4-bromophenyl)pyridine (Brphenpyr) (corresponding to compound (3) described in the specification) (manufactured by BLD Pharmatech Ltd.) was vacuum sealed in an ampoule (Brphenpyr was placed in a glass tube, heated to 343 K (70° C.) at a heating rate of 5 K / min, evacuated at 343 K for 1 hour, and sealed with a gas burner), then heated to a predetermined temperature at a heating rate of 10 K / min in an electric furnace, and heated at the predetermined temperature for 1 hour. The specified temperatures were 873K (600°C) and 823K (550°C). After heating, the samples were scraped out of each ampule with a spatula and transferred to separate glass tubes, then the temperature was increased to 443 K (170°C) at a rate of 5 K / min, and the tubes were then evacuated at 443 K (170°C) for 1 hour to obtain nitrogen-containing carbon materials (3a) and (3b). Nitrogen-containing carbon materials (3a) and (3b) indicate the nitrogen-containing carbon materials at the predetermined temperatures of 873 K (600°C) and 823 K (550°C), respectively. The obtained nitrogen-containing carbon materials (3a) and (3b) were subjected to N1sXPS analysis and Raman spectroscopy analysis. The XPS spectrum of the N1sXPS analysis is shown in FIG. The Raman spectrum of the Raman spectroscopy is shown in FIG. As shown in Figure 5, in the obtained nitrogen-containing carbon material, the ratio of the peak of pyridinic nitrogen atoms to the peak of all nitrogen atoms in the nitrogen-containing carbon material (the sum of tertiary nitrogen atoms, pyridinic nitrogen atoms present on the edges, and other nitrogen atoms) in the N1sXPS analysis was 69.3% and 88.2%, respectively, regardless of whether the specified temperature was 873 K (600°C) or 823 K (550°C), indicating that a nitrogen-containing carbon material in which nitrogen atoms are introduced to the edges and whose structure is precisely controlled can be easily produced under mild conditions. According to the Raman spectrum in FIG. 6, the obtained nitrogen-containing carbon material has peaks in the G band and the D band when the predetermined temperature is 873 K (600° C.), which shows that the nitrogen-containing carbon material having a graphene structure and a structure in which the graphene structures are stacked can be easily produced under mild conditions.

[0073] Example 4 40 mg of 5,5'-dibromo-2,2'-bipyridine (Brbipyr) (corresponding to compound (4) described in the specification) (manufactured by BLD Pharmatech Ltd.) was vacuum sealed in an ampoule (Brbipyr was placed in a glass tube, heated to 453 K (180°C) at a heating rate of 5 K / min, evacuated at 453 K for 1 hour, and sealed with a gas burner), then heated to a predetermined temperature at a heating rate of 10 K / min in an electric furnace, and heated at the predetermined temperature for 1 hour. The specified temperatures were 873K (600°C), 823K (550°C), and 773K (500°C). After heating, the samples were scraped out of each ampule with a spatula and transferred to separate glass tubes, then the temperature was increased to 553 K (280°C) at a rate of 5 K / min, and the tubes were then evacuated at 553 K (280°C) for 1 hour to obtain nitrogen-containing carbon materials (4a) and (4b). Nitrogen-containing carbon materials (4a) and (4b) indicate the nitrogen-containing carbon materials at the predetermined temperatures of 873 K (600°C) and 823 K (550°C), respectively. The obtained nitrogen-containing carbon materials (4a) and (4b) were subjected to N1sXPS analysis and Raman spectroscopy analysis. The XPS spectrum of the N1sXPS analysis is shown in Figure 7. In Figure 7, the XPS spectrum of "Brbipyr" shows the XPS spectrum of the raw material Brbipyr. The Raman spectrum of the Raman spectroscopy is shown in FIG. As shown in Figure 7, in the obtained nitrogen-containing carbon material, the ratio of the peak of pyridinic nitrogen atoms to the peak of all nitrogen atoms in the nitrogen-containing carbon material (the sum of tertiary nitrogen atoms, pyridinic nitrogen atoms present on the edges, and other nitrogen atoms) in the N1sXPS analysis was 72.0% and 70.8%, respectively, regardless of whether the specified temperature was 873 K (600°C) or 823 K (550°C), indicating that a nitrogen-containing carbon material in which nitrogen atoms are introduced to the edges and whose structure is precisely controlled can be easily produced under mild conditions. According to the Raman spectrum in FIG. 8, the obtained nitrogen-containing carbon material had peaks in the G band and the D band at both the predetermined temperatures of 873 K (600° C.) and 823 K (550° C.). This shows that a nitrogen-containing carbon material having a graphene structure and a structure in which the graphene structures are stacked can be easily produced under mild conditions. [Industrial Applicability]

[0074] The nitrogen-containing carbon material of the present invention has a precisely controlled structure due to the introduction of nitrogen atoms at the edges, and can be deployed in a variety of applications.

Claims

1. A heating step (I) of heating the precursor compound (A), The precursor compound (A) is A pyridine ring (a), and at least one aromatic ring (b) selected from the group consisting of a benzene ring and a pyridine ring, which is bonded to the pyridine ring (a) via a single bond. A method for producing a nitrogen-containing carbon material.

2. The method for producing a nitrogen-containing carbon material according to claim 1 , wherein the aromatic ring (b) is a pyridine ring.

3. The method for producing a nitrogen-containing carbon material according to claim 1 , wherein the precursor compound (A) is a polypyridine.

4. The method for producing a nitrogen-containing carbon material according to claim 1 , wherein the precursor compound (A) contains a halogen element.

5. 2. The method for producing a nitrogen-containing carbon material according to claim 1, wherein the precursor compound (A) is at least one selected from the group consisting of compounds (1) to (4). [Formula 1] Here, R 1 ~R 4 are each hydrogen or bromine, and n is an integer from 2 to 500.

6. 2. The method for producing a nitrogen-containing carbon material according to claim 1, wherein the heating temperature of the precursor compound (A) in the heating step (I) is 300° C. to 1000° C.